Preparation method of lithium sulfide
By using the sulfur salt components in the low-sulfur valence state to reduce under a reducing gas atmosphere, combined with the disproportionation reaction of lithium hydroxide and elemental sulfur, the problem of difficult industrial production and high-purity lithium sulfide preparation in the prior art is solved, and high-efficiency and low-cost lithium sulfide preparation is achieved.
Patent Information
- Application Number
- CN202510738003.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-04
- Publication Date
- 2025-08-08
AI Technical Summary
The existing preparation methods for lithium sulfide require high-temperature reduction, making it difficult to achieve industrial-scale production, and it is difficult to obtain high-purity lithium sulfide.
The sulfur salt components in the low-sulfur valence state are reduced under the atmosphere of a reducing gas, and lithium sulfide is prepared at a lower temperature through disproportionation and reduction reactions. Lithium sulfide is used as raw materials to avoid high temperature and high pressure conditions. Hydrogen and carbon monoxide are used as reducing gas, and the reaction temperature is controlled below 600℃.
The preparation of high-purity lithium sulfide is achieved, with a purity of 99.9%, reducing production costs, simplifying process conditions, and suitable for industrial production.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium sulfide and relates to a method for preparing lithium sulfide. Background Art
[0002] Lithium sulfide is considered to have important applications in solid-state battery electrolytes. Lithium sulfide preparation technology has become a research hotspot, and there are three basic methods: direct synthesis of metallic lithium and elemental sulfur, reduction of lithium sulfate at high temperature, and reaction of lithium hydroxide and hydrogen sulfide. However, the above basic methods are difficult to obtain lithium sulfide with high purity, or the process is difficult, so researchers have studied many improved methods. Chinese patent CN112678780A discloses a reduction method using a lithium sulfide precursor and a sugar reducing agent at high temperature, Chinese patent CN115734942A discloses a method in which a reducing agent containing carbon (C) element reduces a raw material containing lithium (Li) element and sulfur (S) element and then reduces it with a reducing gas, Chinese patent CN113401878A discloses a method for the reduction reaction of carbon monoxide and powdered anhydrous lithium sulfate, and Chinese patent CN117383517 A discloses a method for reducing a sulfur source and lithium source integrated compound in a hydrogen-containing atmosphere. However, the reduction temperature in the above methods needs to be 650°C or higher, such as 700°C, 800°C, etc., which is not conducive to industrial-scale production.
[0003] Therefore, the existing methods urgently need to be further improved. Summary of the Invention
[0004] Applicants have unexpectedly discovered that when a sulfur salt component with a low sulfur valence (e.g., a sulfur valence below +6) is reduced in a reducing gas to produce lithium sulfide, the required reduction temperature is relatively low, and this facilitates obtaining high-purity lithium sulfide. Based on this, the present invention provides a method for preparing lithium sulfide.
[0005] The technical solutions of the present invention are as follows:
[0006] A method for preparing lithium sulfide, comprising reducing a raw material in a first gas atmosphere containing a first reducing gas to obtain the lithium sulfide;
[0007] The raw material comprises a sulfide salt component and lithium sulfide;
[0008] The sulfur salt component contains Li, S, and O.
[0009] The valence state of the S in the sulfur salt component does not exceed +5.
[0010] Preferably, the valence of the S in the sulfide salt component does not exceed +4.
[0011] More preferably, the sulfur salt component is selected from one or a combination of lithium sulfite and lithium thiosulfate.
[0012] Preferably, the molar ratio of the sulfide salt component to the lithium sulfide in the raw material is 1:9-9:1.
[0013] Preferably, the raw material is obtained by a disproportionation reaction of lithium hydroxide and elemental sulfur in a second gas atmosphere containing a second reducing gas;
[0014] The temperature of the disproportionation reaction does not exceed 300°C.
[0015] More preferably, the volume fraction of the second reducing gas in the second gas atmosphere is 1-20%.
[0016] More preferably, the volume fraction of the first reducing gas in the first gas atmosphere is higher than the volume fraction of the second reducing gas in the second gas atmosphere.
[0017] More preferably, the first reducing gas and the second reducing gas are independently selected from hydrogen and CO.
[0018] Preferably, the volume fraction of the first reducing gas in the first gas atmosphere is 5-50%.
[0019] Preferably, the reduction temperature does not exceed 600°C, and further, the reduction temperature does not exceed 500°C.
[0020] The beneficial effects of the present invention are:
[0021] (1) The raw materials for preparing high-purity lithium sulfide in the present invention contain sulfur salt components (lithium sulfite, lithium thiosulfate, etc.) with low sulfur valence (such as +2, +4), which can be reduced at a relatively low reduction temperature, and the reduction temperature is reduced to below 600°C, and lithium sulfide with high purity (purity ≥99.9%) is obtained, which is conducive to the industrial-scale production of lithium sulfide.
[0022] (2) The raw materials used to prepare lithium sulfide in the present invention can be obtained by disproportionation reaction of two raw materials, lithium hydroxide and elemental sulfur. The raw material cost is low, the chemical stability is good, the reaction conditions are relatively mild, the raw material utilization rate is high, and no organic solvent is required. Therefore, the method of the present invention is environmentally friendly and efficient. DETAILED DESCRIPTION
[0023] The technical solution of the present invention is further illustrated and described below through specific implementation methods.
[0024] The present invention provides a method for preparing lithium sulfide, wherein raw materials are reduced in a first gas atmosphere containing a first reducing gas to obtain lithium sulfide;
[0025] The raw materials include sulfide salt components and lithium sulfide;
[0026] The above-mentioned sulfur salt components contain Li, S and O.
[0027] The valence state of S in the sulfur salt component does not exceed +5.
[0028] In the prior art, lithium sulfide is generally prepared by reducing lithium sulfate (Li2SO4). However, the high reduction temperature (generally approaching or exceeding 700°C) and harsh conditions are not conducive to the industrial production of lithium sulfide. Furthermore, incomplete reduction of the lithium sulfate may occur, resulting in insufficient purity of the obtained lithium sulfide. The present invention has discovered that the use of a sulfur salt component with a relatively low sulfur valence (S valence not exceeding +5) allows for the reduction to be performed at a relatively low reduction temperature, under relatively mild conditions, and can produce high-purity lithium sulfide (purity ≥99.9%), facilitating the industrial production of lithium sulfide.
[0029] There is no particular limitation on the purity of lithium sulfide added to the raw materials, and it may be no less than 98.5%, such as 98.5%, 99%, 99.2%, 99.5%, 99.7%, 99.8%, 99.9%, etc.
[0030] In some embodiments, the valence of S in the sulfide salt component does not exceed +4. For example, the valence of S can be any value among +2, +3, +4, etc. or any value in between. For example, the sulfide salt component can be selected from one or a combination of lithium sulfite (S valence is +4) and lithium thiosulfate (S valence is +2). That is, the sulfide salt component can be either lithium sulfite and lithium thiosulfate alone, or a combination of these two in different molar ratios, such as a molar ratio of 4:1, 3:1, 2:1, 1:1, 1:2, 1:3, 1:4, etc. The valence of S in lithium sulfate is +6, the valence of S in lithium sulfite is +4, and the average valence of S in lithium thiosulfate is +2. Therefore, lithium sulfate has a high sulfur valence, and its reduction to lithium sulfide is more difficult, requiring a higher temperature, such as above 700°C. When the valence of S in the sulfide salt component is relatively low, the reduction temperature can be 600°C, 550°C, 500°C, or lower.
[0031] In some embodiments, the molar ratio of the sulfide salt component and lithium sulfide in the raw material is 1:9-9:1. For example, the molar ratio can be any value among 1:9, 1:8, 1:7, 1:6, 1:5, 1:4, 1:3, 1:2, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, etc. or any value in between, without special restrictions.
[0032] In some embodiments, the raw material is obtained by a disproportionation reaction of lithium hydroxide and elemental sulfur in a second gas atmosphere containing a second reducing gas;
[0033] The temperature of the disproportionation reaction does not exceed 300°C.
[0034] Currently, there are no separate lithium sulfite and lithium thiosulfate products on the market, making it impossible to directly reduce lithium sulfite and / or lithium thiosulfate to produce lithium sulfide. However, a disproportionation reaction between lithium hydroxide and elemental sulfur can produce a combination of lithium sulfide and at least one of lithium thiosulfate and lithium sulfite. This combination can be used directly as a raw material in a reduction reaction to produce high-purity lithium sulfide. Lithium hydroxide and elemental sulfur are abundant, stable, and low-cost, and the disproportionation reaction can be carried out under relatively mild conditions.
[0035] There is no particular limitation on the molar ratio of lithium hydroxide to elemental sulfur, and the molar ratio can be 1-2:1, such as 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2:1, etc. Furthermore, the disproportionation reaction temperature can be 100-250° C., and the reaction time can be 0.5-2 hours.
[0036] The second gas atmosphere can be composed of a second reducing gas and an inert gas. The inert gas can be nitrogen, argon, helium, etc. The volume fraction of the second reducing gas in the second gas atmosphere is 1-20%. For example, the volume fraction can be any value or any value between 1%, 2%, 3%, 4%, 5%, 6%, 8%, 10%, 12%, 14%, 15%, 16%, 18%, 20%, etc., without special restrictions. Further, the volume fraction of the second reducing gas in the second gas atmosphere can be 1-5%. The disproportionation reaction is carried out in an inert gas atmosphere to avoid the oxidation of elemental sulfur to form toxic and harmful gases such as sulfur dioxide and sulfur trioxide, and to promote the reaction between lithium hydroxide and elemental sulfur. When the disproportionation reaction is carried out in a second gas atmosphere containing a second reducing gas, the formation of lithium sulfate can be avoided, and instead it is converted into lithium salts with low sulfur valence such as lithium sulfite and lithium thiosulfate, which is beneficial to the subsequent reduction reaction. For example, at a certain temperature and a certain volume fraction of the second reducing gas, lithium hydroxide and elemental sulfur undergo a disproportionation reaction to generate lithium sulfide, lithium sulfite and lithium thiosulfate, and the molar ratio of the three is 2:x:y, where 0≤x≤1, 0≤y≤1, and x+y=1.
[0037] In some embodiments, the volume fraction of the first reducing gas in the first atmosphere is higher than the volume fraction of the second reducing gas in the second atmosphere. The second atmosphere only requires a relatively weak reducing power to avoid the formation of lithium sulfate. The first atmosphere requires a relatively strong reducing power to more completely promote the conversion of the sulfur salt component into lithium sulfide.
[0038] In some embodiments, the first reducing gas and the second reducing gas are independently selected from hydrogen and CO. Hydrogen and CO are commonly used reducing gases. For example, the first reducing gas may be hydrogen, and the second reducing gas may be CO.
[0039] In some embodiments, the volume fraction of the first reducing gas in the first gas atmosphere is 5-50%. For example, the volume fraction of the first reducing gas can be any value among 5%, 6%, 8%, 10%, 12%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc., or any value in between, without particular limitation. Furthermore, the volume fraction of the first reducing gas in the first gas atmosphere can be 5-20%.
[0040] In some embodiments, the reduction temperature does not exceed 600° C., and further, the reduction temperature does not exceed 500° C. For example, the reduction temperature can be any value among 600° C., 580° C., 550° C., 530° C., 520° C., 500° C., 490° C., 480° C., 460° C., 450° C., or any value therebetween, without particular limitation. The reduction time can be 2-6 hours.
[0041] In the present invention, the reactor for the reduction reaction and disproportionation reaction is not particularly limited, and for example, it can be a rotary kiln or a fluidized bed reactor.
[0042] The high-purity lithium sulfide (purity ≥ 99.9%) obtained by the reduction reaction of the present invention can be further pulverized by ball milling or air flow milling to D 50 The particle size is 1-10 μm for easy use.
[0043] The technical solution of the present invention is further described and illustrated below based on various embodiments.
[0044] Example 1
[0045] LiOH and elemental sulfur powder were thoroughly mixed in a 1:1 molar ratio and then placed in a CO / N2 gas mixture (with a 1% CO volume fraction in the mixture). The mixture was reacted at 150°C for 2 hours to produce an intermediate product with a measured composition of Li2S, Li2SO3, and Li2S2O3 in a molar ratio of 2:0.7:0.3. The intermediate product was then reduced in a rotary kiln using an H2 / Ar gas mixture with a 5% H2 volume concentration as a reducing agent at 450°C for 5 hours to produce lithium sulfide. Analysis revealed a purity of 99.93% for the resulting lithium sulfide.
[0046] Comparative Example 1
[0047] This comparative example differs from Example 1 in that the CO / N2 mixed gas in Example 1 was replaced with nitrogen, i.e., no CO was added. The remaining steps remained unchanged, and the composition of the intermediate product obtained was a molar ratio of Li2S, Li2SO3, and Li2SO4 of 2:0.2:0.8. The purity of the resulting lithium sulfide product was 90.7%.
[0048] Comparative Example 2
[0049] The difference between this comparative example and comparative example 1 is that in comparative example 1, the reduction temperature of the intermediate product was adjusted from 500° C. to 700° C. The remaining steps remained unchanged. The purity of the obtained lithium sulfide product was 98.8%.
[0050] Example 2
[0051] This example differs from Example 1 in that the volume fraction of CO in the mixed gas was adjusted from 1% to 3% in Example 1. The remaining steps remained unchanged, and the composition of the intermediate product was determined to be a molar ratio of Li2S, Li2SO3, and Li2S2O3 of 2:0.4:0.6. The purity of the resulting lithium sulfide product was 99.94%.
[0052] Example 3
[0053] The difference between this embodiment and embodiment 1 is that in embodiment 1, the volume concentration of H2 in the H2 / Ar mixed gas is adjusted from 5% to 10%. The remaining steps remain unchanged, and the purity of the obtained lithium sulfide product is 99.93%.
[0054] Example 4
[0055] LiOH and elemental sulfur powder are thoroughly mixed in a 1.5:1 molar ratio and then reacted in a CO / N2 mixture with a 2% CO concentration by volume at 250°C for 0.5 hours to produce an intermediate product composed of Li2S and Li2SO3 in a 2:1 molar ratio. This intermediate product is then reduced in a rotary kiln using a 5% H2 / Ar mixture as a reducing agent at 600°C for 2 hours to produce lithium sulfide. Analysis shows the purity of the resulting lithium sulfide to be 99.97%.
[0056] Example 5
[0057] LiOH and elemental sulfur powder are thoroughly mixed in a molar ratio of 1.5:1, then placed in a CO / N2 mixture with a 1% CO concentration by volume. The mixture reacts at 200°C for 1 hour to produce an intermediate product composed of Li2S, Li2SO3, and Li2S2O3 in a molar ratio of 2:0.6:0.4. The intermediate product is then reduced in a rotary kiln using a H2 / Ar mixture with a 20% H2 concentration by volume as a reducing agent at 400°C for 6 hours to produce lithium sulfide. Analysis indicates the purity of the resulting lithium sulfide is 99.92%.
[0058] Example 6
[0059] LiOH and elemental sulfur powder are thoroughly mixed in a 2:1 molar ratio and then reacted in a CO / N2 mixture with a 3% CO concentration by volume at 220°C for 2 hours to produce an intermediate product composed of Li2S, Li2SO3, and Li2S2O3 in a molar ratio of 2:0.3:0.7. This intermediate product is then reduced in a rotary kiln using a 15% H2 / Ar mixture at 550°C for 2.5 hours to produce lithium sulfide. Analysis shows the purity of the resulting lithium sulfide to be 99.96%.
[0060] As described above, the basic principles, main features, and advantages of the present invention are shown and described. Those skilled in the art should understand that the present invention is not limited to the above-described embodiments. The above-described embodiments are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. In other words, equivalent changes and modifications made within the scope of the present invention and the contents of the specification should still fall within the scope of the present invention. The scope of protection claimed in the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing lithium sulfide, characterized in that: reducing the raw material in a first gas atmosphere containing a first reducing gas to obtain the lithium sulfide; The raw material comprises a sulfide salt component and lithium sulfide; The sulfide salt component contains Li, S and O; The valence state of the S in the sulfur salt component does not exceed +5.
2. The method for preparing lithium sulfide according to claim 1, wherein The valence state of the S in the sulfur salt component does not exceed +4.
3. The method for preparing lithium sulfide according to claim 2, wherein: The sulfur salt component is selected from one or a combination of lithium sulfite and lithium thiosulfate.
4. The method for preparing lithium sulfide according to claim 1, wherein The molar ratio of the sulfide salt component to the lithium sulfide in the raw material is 1:9-9:
1.
5. The method for preparing lithium sulfide according to claim 1, wherein The raw material is obtained by a disproportionation reaction between lithium hydroxide and elemental sulfur in a second gas atmosphere containing a second reducing gas; The temperature of the disproportionation reaction does not exceed 300°C.
6. The method for preparing lithium sulfide according to claim 5, characterized in that: The volume fraction of the second reducing gas in the second gas atmosphere is 1-20%.
7. The method for preparing lithium sulfide according to claim 5, characterized in that: The volume fraction of the first reducing gas in the first gas atmosphere is higher than the volume fraction of the second reducing gas in the second gas atmosphere.
8. The method for preparing lithium sulfide according to claim 5, characterized in that: The first reducing gas and the second reducing gas are independently selected from hydrogen and CO.
9. The method for preparing lithium sulfide according to claim 1, wherein: The volume fraction of the first reducing gas in the first gas atmosphere is 5-50%.
10. The method for preparing lithium sulfide according to claim 1, characterized in that: The reduction temperature does not exceed 600°C. Furthermore, the reduction temperature does not exceed 500°C.
Citation Information
Patent Citations
Preparation method of high-purity lithium sulfide
CN112678780A
Preparation method of lithium sulfide
CN113401878A
Method for producing lithium sulfide
CN115734942A
Battery-grade lithium sulfide material as well as preparation method and application thereof
CN117383517A
Cited By
Lithium sulfide and preparation method thereof
CN120987268A
Preparation method of lithium sulfide, product and application
CN121672427A