Sulfur-chlorine-resistant CeO2-Mo-MnO2 catalyst, preparation method thereof and application of sulfur-chlorine-resistant CeO2-Mo-MnO2 catalyst in catalytic oxidation of VOCs
By doping Mo into the MnO2 catalyst and attaching CeO2 nanoparticles to construct dissociation and sacrificial sites, the problem of easy poisoning of the MnOx catalyst during the catalytic oxidation of VOCs was solved, and an efficient and stable catalytic oxidation effect was achieved.
Patent Information
- Application Number
- CN202510582402.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-07
- Publication Date
- 2025-09-12
AI Technical Summary
Existing MnOx catalysts are easily affected by SO2 and Cl during the catalytic oxidation of VOCs, resulting in catalyst poisoning and deactivation, making it difficult to achieve stable and efficient catalytic oxidation.
By doping Mo element into the MnO2 catalyst to regulate the acidic sites and attaching CeO2 nanoparticles on the Mo-MnO2 surface, dissociation sites and sacrificial sites are constructed to improve the resistance to sulfur and chlorine.
The catalyst achieved high stability in sulfur- and chlorine-containing VOCs. The toluene conversion rate of the catalyst reached 100% at 300°C and there was no attenuation within 1000 hours, significantly improving its resistance to sulfur and chlorine poisoning.
Smart Images

Figure CN120618456A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of waste gas treatment, and in particular to a sulfur-chlorine-resistant CeO2@Mo-MnO2 catalyst, a preparation method thereof, and application in catalytic oxidation of VOCs. Background Art
[0002] Volatile organic compounds (VOCs) are an important type of pollutants. They not only form ozone and fine particulate matter (PM 2.5 ), and is also toxic and even carcinogenic. VOCs come from a wide range of sources, including petrochemicals, fuel combustion, transportation, building decoration and other fields. Chlorinated volatile organic compounds (CVOCs), such as chlorobenzene (CB), are more stable and toxic than VOCs, which makes them more difficult to degrade in organisms, leading to the accumulation of pollutants in biological systems. A variety of end-of-pipe treatment technologies have been developed, among which catalytic oxidation is considered to be the most promising and cost-effective method. However, the low-temperature catalytic unit is usually located downstream of the desulfurization unit, and the catalyst is easily affected by SO2.
[0003] Manganese oxide (MnO x ) is considered to be one of the most promising candidate catalysts for the catalytic oxidation of VOCs due to its low price, flexible structure, good stability and environmental friendliness. x Insufficient catalytic efficiency and toxicity resistance limit their further application. Doping and interactions between transition metal oxides can increase the concentration of oxygen vacancies on the material surface and increase the number of acidic sites on the catalyst surface, promoting the removal of chlorine adsorbed on the catalyst surface as HCl and inhibiting the accumulation of Cl at active sites (CN119588348A). However, acidic sites often affect the catalyst's deep oxidation ability, exposing it to the risk of carbon deposition. Therefore, the development of efficient and stable catalysts that are resistant to sulfur and chlorine deserves further research. Summary of the Invention
[0004] In order to solve the above technical problems, the present invention provides a sulfur- and chlorine-resistant CeO2@Mo-MnO2 catalyst, its preparation method, and its application in the catalytic oxidation of VOCs. The catalyst of the present invention is based on MnO2. First, by doping the Mo element to regulate the acidic sites, the dissociation sites of chlorobenzene are constructed, which can significantly improve the catalyst's resistance to chlorine poisoning; secondly, by attaching a layer of CeO2 nanoparticles in a lattice shape on the Mo-MnO2 surface to construct sacrificial sites, the adsorption of SO2 on the catalyst surface is inhibited, which can significantly improve the catalyst's resistance to sulfur poisoning. The catalyst of the present invention is applied to the catalytic oxidation of sulfur- and chlorine-containing VOCs. It is not easy to be poisoned and deactivated, and has very excellent stability.
[0005] The specific technical solutions of the present invention are: In a first aspect, the present invention provides a sulfur- and chlorine-resistant CeO2@Mo-MnO2 catalyst comprising: Mo-doped MnO2 nanorods and CeO2 nanoparticles attached to the surfaces of the Mo-doped MnO2 nanorods in a lattice pattern. The average valence of Mn is 3.50-3.55.
[0006] The catalyst of the present invention is based on MnO2 nanorods. First, by doping with Mo ions, the acidic sites are regulated to create dissociation sites for chlorobenzene, significantly improving the catalyst's resistance to chlorine poisoning. Second, by attaching a layer of CeO2 nanoparticles in a lattice pattern to the Mo-MnO2 surface, sacrificial sites are created to inhibit the adsorption of SO2 on the catalyst surface, significantly improving the catalyst's resistance to sulfur poisoning. Therefore, when applied to the catalytic oxidation of sulfur- and chlorine-containing VOCs, the catalyst is not susceptible to poisoning and deactivation, and exhibits exceptional stability.
[0007] The mass ratio of Mo to Mn is 0.1-1:1, more preferably 0.2-0.6:1; the mass ratio of CeO2 to Mo-doped MnO (Mo-MnO2) is 0.01-0.5:1, more preferably 0.05-0.3:1.
[0008] The influence of element ratio on catalyst performance mainly comes from the regulation of active site distribution, electronic structure and synergistic effect. When the Mo / Mn ratio is too high, excess Mo may occupy the surface sites of the Mn active center, resulting in a decrease in the number of active sites and reduced catalytic reaction efficiency; while when the Mo ratio is too low, it is difficult to effectively regulate the electronic state of the catalyst surface, weakening the active oxygen species (such as O - or O2 - ) formation and migration capacity, thereby affecting the kinetics of redox reactions. For Ce / Mn systems, when the Ce ratio is too low, the oxygen storage capacity and surface oxygen vacancy concentration of CeO2 are insufficient, failing to fully inhibit the adsorption and poisoning of sulfide molecules on active sites. Conversely, excessive CeO2 coverage hinders direct contact between Mn active centers and reactants, potentially forming an inert interface layer, weakening the electronic synergy between Mn and Ce, and leading to decreased catalytic activity. Therefore, optimizing the Mo / Mn and Ce / Mn ratios is key to achieving a balance between active site density, oxygen activation capacity, and anti-poisoning performance.
[0009] Preferably, the width of the Mo-doped MnO2 nanorods is 15-50 nm.
[0010] In a second aspect, the present invention provides a method for preparing a sulfur-chlorine-resistant CeO2@Mo-MnO2 catalyst, which comprises the following steps: 1) KMnO4, (NH4)2C2O4 and ammonium molybdate are used as raw materials for a hydrothermal reaction. The obtained product is filtered, washed, dried and aerobic calcined to obtain Mo-MnO2.
[0011] Under acidic hydrothermal conditions, KMnO4 (Mn 7+ ) is oxalate (C2O4 2- , reducing agent) is gradually reduced to Mn 4+ , generating MnO2 nuclei, while C2O4 2- Oxidized to CO2. The reaction can be simplified as follows: ammonium molybdate (containing Mo 6+ ) as a doping source, Mo 6+ The partial substitution of Mo into the MnO2 lattice forms Mo-doped MnO2 (Mo-MnO2). Subsequent oxygen calcination further promotes the improvement of crystallinity and stabilizes the chemical bonding between Mo and Mn.
[0012] The product is a nanorod structure, and its formation mechanism is related to the coordination and guiding effect of oxalate during the hydrothermal process. 4+ The complexation of can induce the crystal to grow preferentially along a specific crystal plane. The present invention selects ammonium molybdate ((NH4)6Mo7O 24 4H2O) as the source of Mo is that ammonium molybdate easily dissociates into MoO4 in water. 2- and NH 4+ ions. MoO4 2- The stable existence of Mo in the hydrothermal reaction can ensure 6+ The continuous supply of MnO2 precursors (such as Mn 4+ ) are uniformly mixed in the liquid phase, promoting Mo atoms to enter the MnO2 lattice through substitution or interstitial doping, forming a stable Mo-O-Mn bond. MoO4 in ammonium molybdate 2- With other anions in the reaction system (such as MnO4 - 、C2O4 2- ) has charge and size compatibility, avoiding the introduction of other competing ligands (such as Cl - 、NO3 - Complexation interference or side reactions caused by
[0013] 2) Urea and hexamethylenetetramine were dissolved in an ethanol-water mixture, and Mo-MnO2 and Ce salt were added to react. The resulting product was filtered, washed, dried, and aerobic calcined to obtain a sulfur- and chlorine-resistant CeO2@Mo-MnO2 catalyst.
[0014] Urea decomposes into NH3 and CO2 when heated in ethanol-water mixed solution, gradually increasing the pH value of the solution to form a weak alkaline environment. NH3 can react with Ce as a ligand. 3+Complexation, slowing down the generation rate of Ce(OH)3 precipitation, and promoting uniform nucleation. Hydrolysis at high temperature releases NH3, further adjusting the pH value of the system. At the same time, its decomposition products can act as soft templates to guide the directional attachment of CeO2 nanoparticles on the Mo-MnO2 surface, avoiding agglomeration. The low surface tension of ethanol is conducive to the dispersion of Mo-MnO2 nanorods, while regulating the reaction kinetics, inhibiting the excessive growth of CeO2 particles, and achieving size uniformity. The reaction product is Mo-MnO2 nanorods modified with CeO2 nanoparticles. After calcination, it is mainly (CeO2), and there may be a small amount of Ce on the surface. 3+ (caused by oxygen vacancies), enhancing oxygen storage capacity and redox activity.
[0015] In addition, the present invention also found that in the MnO2 catalyst, the modification order of Mo and CeO2 has an important influence on the catalyst's ultimate sulfur and chlorine resistance. The present invention chooses to dope Mo first and then surface-modify CeO2, which can enable molybdenum atoms to be doped into the MnO2 lattice first, thereby effectively changing the electronic structure and acid site distribution of the material. Molybdenum doping can regulate the acid strength and density of the catalyst surface by replacing manganese sites or forming a solid solution, thereby enhancing the adsorption and decomposition ability of sulfur and chlorine poisoning species; at the same time, lattice doping can also optimize the stability of active sites and reduce the irreversible adsorption of poisoning substances on the surface. If CeO2 is modified first and then loaded with molybdenum oxide, molybdenum only exists in the form of surface oxide, and it is impossible to deeply regulate the bulk properties of MnO2, resulting in insufficient modification of acid sites, and the surface molybdenum is easily covered by sulfur and chlorine or deactivated by the reaction. In addition, although the surface modification of CeO2 can provide oxygen storage capacity, its synergistic effect with lattice doped molybdenum is missing, making it difficult to form an efficient anti-poisoning composite interface. Therefore, lattice doping of molybdenum is the key to improving anti-sulfur and anti-chlorine properties, while simple surface modification is difficult to achieve similar structural and functional optimization.
[0016] Preferably, in step 1), the mass ratio of KMnO4 to (NH4)2C2O4 is 2:1-4:1; and the content of (NH4)2C2O4 in the reaction system of the hydrothermal reaction is 0.015-0.025 g / mL.
[0017] The present invention found that in the process of preparing Mo-MnO2 by hydrothermal reaction, the mass ratio of KMnO4 and (NH4)2C2O4 is very important. If the mass ratio is too low (such as <2:1), C2O4 2- Excessive amount will lead to over-reduction (forming Mn 2+ or Mn 3+ ), destroying the stability of the MO2 lattice; if it is too high (such as >4:1), C2O4 2- Insufficient reaction leads to incomplete reaction and residual MnO4 - Introducing impurity phases (such as K2MnO4).
[0018] Furthermore, the present invention also found that in the process of preparing Mo-MnO2 by hydrothermal reaction, the concentration of (NH4)2C2O4 has an important influence on the morphology and performance of Mo-MnO2. At the above-mentioned appropriate concentration, (NH4)2C2O4 can fully play the role of reducing permanganate, adjusting pH, complexing and regulating crystallization, and inhibiting side reactions, thereby improving the purity, crystallinity and morphology controllability of the product; the obtained Mo-MnO2 appears as nanorods with a width of 15-50 nm and a relatively ideal crystallinity. If the content of (NH4)2C2O4 is lower than 0.015 g / mL, the reduction ability of Mn2 will be insufficient. 7+ →Mn 4+ The conversion rate is low, and the residual high-valent manganese species (such as MnO4 - ) interferes with the crystallization process; if the content of (NH4)2C2O4 is higher than 0.025 g / mL, the excessive reducing property will trigger side reactions (such as the formation of Mn 3+ ), resulting in lattice distortion, excess C2O4 2- With MoO4 2- Competitive coordination inhibits the effective doping of Mo and reduces the catalytic activity.
[0019] Preferably, in step 1), the temperature of the hydrothermal reaction is 120-260° C., most preferably 160° C., and the time is 6-36 hours, most preferably 16 hours.
[0020] If the reaction temperature is lower than 120 ℃, the reaction kinetics is slow and Mn 7+ The reduction is incomplete, the product is mainly amorphous MnO2, and the nanorod structure is difficult to form; if the reaction temperature is higher than 260℃, the crystal growth rate is too fast in the environment, resulting in the nanorod diameter being too large (>50 nm) or melting and agglomeration, and high temperature accelerates the decomposition of oxalic acid (C2O4 2- →CO2), disrupting the coordination equilibrium. Too short a time (<6 h): Insufficient nucleation, insufficient nanorod length (<0.5 μm), and numerous surface defects. Too long a time (>36 h): Significant Ostwald ripening, coarsening or breakage of the nanorods, and a decrease in specific surface area.
[0021] Preferably, in step 1), the drying temperature is 50-110°C, most preferably 80°C.
[0022] Preferably, in step 1), the calcination temperature is 280-500° C., most preferably 350° C., and the calcination time is 2-10 hours, most preferably 6 hours.
[0023] If the calcination temperature is too low (<280 ℃): Mo doping is mainly physical adsorption, no stable Mo-O-Mn bond is formed, and the doping efficiency is low; the crystallinity is insufficient (XRD peak intensity is weak). On the contrary, if the calcination temperature is too high (>500 ℃): MnO2 undergoes phase transition (α→β phase), and the nanorod structure collapses; Mo 6+ They may migrate to the surface to form MoO3 aggregates, blocking active sites. Too short a time (<2 h): insufficient lattice rearrangement and low oxygen vacancy concentration; too long a time (>10 h): nanorods sinter and densify, resulting in a sharp decrease in specific surface area.
[0024] Preferably, in step 2), the mass ratio of urea to hexamethylenetetramine is 1:1-3:1; and the content of urea in the reaction system is 0.006-0.018 g / mL.
[0025] In the present invention, if the urea ratio is too high (>3:1), NH3 is released too slowly, Ce 3+ The hydrolysis rate lags, resulting in uneven Ce(OH)3 precipitation (large particle agglomeration). Conversely, if the hexamethylenetetramine ratio is too high (<1:1), NH3 is released too quickly, the local pH rises suddenly, Ce(OH)3 nucleates instantly, and the loaded particles are uneven in size.
[0026] Preferably, in step 2), the reaction temperature is 50-150°C, preferably 100°C, and the reaction time is 1-8 hours, most preferably 6 hours.
[0027] The reaction temperature regulates the decomposition rate of urea and hexamethylenetetramine, thereby affecting the kinetics of NH3 release and Ce 3+ Hydrolysis-precipitation behavior.
[0028] Preferably, in step 2), the calcination temperature is 280-480° C., preferably 300° C., and the calcination time is 2-10 hours, most preferably 3 hours.
[0029] Calcination temperature and time affect the morphology and structure of the catalyst.
[0030] In a third aspect, the present invention provides an application of a CeO2@Mo-MnO2 catalyst in the catalytic oxidation of sulfur-containing and chlorine-containing VOCs, specifically comprising: adding a sulfur- and chlorine-resistant CeO2@Mo-MnO2 catalyst to a fixed-bed reactor, introducing sulfur- and chlorine-containing VOCs, and conducting a catalytic oxidation reaction.
[0031] Preferably, the VOCs is toluene, the content of chlorobenzene is ≥50 ppm, and the content of SO2 is ≥50 ppm.
[0032] Compared with the prior art, the present invention has the following beneficial effects: (1) The catalyst of the present invention is based on MnO2. First, the acidic sites are regulated by doping Mo element to construct the dissociation sites of chlorobenzene, thereby significantly improving the catalyst's resistance to chlorine poisoning; secondly, a layer of CeO2 nanoparticles is attached to the Mo-MnO2 surface in a lattice shape to construct sacrificial sites, which inhibits the adsorption of SO2 on the catalyst surface, thereby significantly improving the catalyst's resistance to sulfur poisoning.
[0033] (2) The catalyst of the present invention is applied to the catalytic oxidation of sulfur- and chlorine-containing VOCs. It is not easily poisoned and deactivated and has excellent stability. Evaluation shows that the catalyst has a 100% conversion rate for toluene under the conditions of 1000 ppm toluene, 50 ppm chlorobenzene, 50 ppm SO2, 5 vol% H2O, and a reaction temperature of 300°C. Under these conditions, the catalyst can operate stably for 1000 hours without any attenuation. Therefore, the catalyst has good application prospects in the catalytic oxidation of sulfur- and chlorine-containing VOCs. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 Transmission electron microscopy (TEM) images of MnO2 (ac) and Mo-MnO2 (df).
[0035] Figure 2 TEM and EDS mapping images of CeO2 modified Mo-MnO2.
[0036] Figure 3 This is a diagram showing the catalytic oxidation performance of Mo-MnO2 modified with MnO2, Mo-MnO2 and CeO2.
[0037] Figure 4 The stability of Mo-MnO2 catalysts modified with MnO2, Mo-MnO2 and CeO2.
[0038] Figure 5 XPS of Mo-MnO2 catalysts modified with MnO2, Mo-MnO2 and CeO2; (a) O 1s, (b) Mn 3s, (c) NH3-TPD.
[0039] Figure 6 (a) MnO2 catalysts with different Mo doping amounts and (b) Mo with different CeO2 modification amounts 0.4 Catalytic oxidation activity of sulfur-containing chlorotoluene over MnO2 catalyst.
[0040] Figure 7 Effect of (NH4)2C2O4 concentration on the morphology of Mo-MnO2 catalyst.
[0041] Figure 8This is the transmission electron microscopy (TEM) image of the CeO2@Mo-MnO2 catalyst obtained when the urea concentration is low. DETAILED DESCRIPTION
[0042] The present invention will be further described below with reference to the embodiments.
[0043] Overall embodiment In the first aspect, a sulfur- and chlorine-resistant CeO2@Mo-MnO2 catalyst is described, comprising: Mo-doped MnO2 nanorods and CeO2 nanoparticles attached to the surfaces of the Mo-doped MnO2 nanorods in a lattice pattern. The mass ratio of Mo to Mn is 0.1-1:1, and the mass ratio of CeO2 to Mo-MnO2 is 0.05-0.5:1. The average valence of Mn is 3.50-3.55.
[0044] In some preferred implementation cases, the mass ratio of Mo to Mn is 0.2-0.6:1; the mass ratio of CeO2 to Mo-MnO2 is 0.05-0.3:1.
[0045] In some preferred embodiments, the width of the Mo-doped MnO2 nanorods is 15-50 nm.
[0046] In a second aspect, a method for preparing a sulfur-chlorine-resistant CeO2@Mo-MnO2 catalyst comprises the following steps: 1) KMnO4, (NH4)2C2O4 and ammonium molybdate are used as raw materials for a hydrothermal reaction. The obtained product is filtered, washed, dried and aerobic calcined to obtain Mo-MnO2.
[0047] In some preferred implementation cases, in step 1), the mass ratio of KMnO4 and (NH4)2C2O4 is 2:1-4:1; and the content of (NH4)2C2O4 in the reaction system of the hydrothermal reaction is 0.015-0.025 g / mL.
[0048] In some preferred embodiments, in step 1), the temperature of the hydrothermal reaction is 120-260° C., most preferably 160° C., and the time is 6-36 hours, most preferably 16 hours.
[0049] In some preferred embodiments, in step 1), the drying temperature is 50-110°C, most preferably 80°C.
[0050] In some preferred embodiments, in step 1), the calcination temperature is 280-500° C., most preferably 350° C., and the calcination time is 2-10 hours, most preferably 6 hours.
[0051] 2) Urea and hexamethylenetetramine were dissolved in an ethanol aqueous solution, and Mo-MnO2 and Ce salt were added to react. The resulting product was filtered, washed, dried, and aerobic calcined to obtain a sulfur- and chlorine-resistant CeO2@Mo-MnO2 catalyst.
[0052] In some preferred implementation cases, in step 2), the mass ratio of urea to hexamethylenetetramine is 1:1-3:1; and the content of urea in the reaction system is 0.006-0.018 g / mL.
[0053] In some preferred embodiments, in step 2), the reaction temperature is 50-150°C, preferably 100°C, and the reaction time is 1-8 hours, most preferably 6 hours.
[0054] In some preferred implementation cases, in step 2), the calcination temperature is 280-480° C., preferably 300° C., and the calcination time is 2-10 hours, most preferably 3 hours.
[0055] The third aspect is the application of CeO2@Mo-MnO2 catalyst in the catalytic oxidation of sulfur-containing and chlorine-containing VOCs, which specifically includes: adding the sulfur-chlorine-resistant CeO2@Mo-MnO2 catalyst to a fixed bed reactor, introducing sulfur-containing and chlorine-containing VOCs, and carrying out catalytic oxidation reaction.
[0056] In some preferred implementation cases, the VOCs is toluene, the content of chlorobenzene is ≥50 ppm, and the content of SO2 is ≥50 ppm.
[0057] Specific Examples and Comparative Examples (1) Comparison of different catalyst types Example 1 (CeO2@Mo-MnO2 catalyst) (1) Preparation of molybdenum-doped manganese dioxide Mo-MnO2 catalyst, the specific steps are as follows: 4.5g KMnO4 and 1.5g (NH4)2C2O4 were added to 80mL ultrapure water, and 1.0g (NH4)6Mo7O 24 4H2O to control the Mo / Mn mass ratio to 0.35:1. Once fully dissolved, the mixture was transferred to a hydrothermal reactor and reacted at 160°C for 16 hours. After the reaction, the product was filtered and repeatedly washed with ultrapure water and ethanol. It was then dried in an 80°C oven for 24 hours. Finally, the dried powder was calcined in a muffle furnace at 350°C for 6 hours to obtain the molybdenum-doped manganese dioxide (Mo-MnO2) catalyst.
[0058] (2) Preparation of CeO2@Mo-MnO2 catalyst. The specific steps are as follows: 1 g of urea and 0.5 g of hexamethylenetetramine were added to 100 mL of a mixture of aqueous ethanol and ultrapure water (volume ratio of 1:1). After sufficient dissolution, 1.0 g of Mo-MnO2 was added and evenly dispersed. Subsequently, 0.75 g of Ce(NO3)3·6H2O was added and reacted at 100°C for 6 hours. After completion of the reaction, the mixture was filtered, washed with ultrapure water and ethanol, and then dried in a forced air drying oven at 80°C. Finally, the dried sample was calcined in a muffle furnace at 300°C for 3 hours to obtain the CeO2@Mo-MnO2 catalyst.
[0059] Comparative Example 1 (MnO2 catalyst) The preparation of MnO2 catalyst, the specific steps are as follows: 4.5 g of KMnO₄ and 1.5 g of (NH₄)₂C₂O₄ were added to 80 mL of ultrapure water. Once fully dissolved, the mixture was transferred to a hydrothermal reactor and reacted at 160°C for 16 hours. After the reaction, the product was filtered and repeatedly washed with ultrapure water and ethanol. It was then dried in an 80°C oven for 24 hours. Finally, the dried powder was calcined in a muffle furnace at 350°C for 6 hours to obtain the MnO₂ catalyst.
[0060] Comparative Example 2 (Mo-MnO2 catalyst) The preparation of molybdenum-doped manganese dioxide Mo-MnO2 catalyst, the specific steps are as follows: 4.5 g KMnO4 and 1.5 g (NH4)2C2O4 were added to 80 mL ultrapure water, and 1.0 g (NH4)6Mo7O 24 4H2O was added to control the Mo / Mn mass ratio to 0.35:1. Once fully dissolved, the mixture was transferred to a hydrothermal reactor and reacted at 160°C for 16 hours. After completion of the reaction, the product was filtered and repeatedly washed with ultrapure water and ethanol. It was then dried in an 80°C oven for 24 hours. Finally, the dried powder was calcined in a muffle furnace at 350°C for 6 hours to obtain the molybdenum-doped manganese dioxide (Mo-MnO2) catalyst.
[0061] Performance Testing (1) Morphology observation: Figure 1 (ac) are TEM images of the MnO2 catalyst prepared in Comparative Example 1. Figure 1 (df) are TEM images of the Mo-MnO2 catalyst prepared in Comparative Example 2. It can be seen from the figure that defects appear in the lattice fringes of the catalyst after molybdenum doping, indicating the formation of oxygen vacancies in the catalyst. Figure 2TEM image and EDS mapping image of the CeO2@Mo-MnO2 catalyst prepared in Example 1. It can be seen from the figure that CeO2 is uniformly attached to the surface of the Mo-MnO2 material in a lattice shape.
[0062] (2) The synthesized catalyst is applied to the catalytic oxidation of VOCs containing sulfur, chlorine, and water vapor. The specific steps are as follows: 170 mg of the catalyst was added to the reaction tube of the fixed-bed reactor and pretreated at 300 °C for 12 h in a nitrogen atmosphere (100 ml / min). Then, the reaction gas was introduced: 1000 ppm toluene, 50 ppm chlorobenzene, 50 ppm SO2, and 5 vol% H2O. The space velocity (WHSV) was controlled at 36000 mL g -1 h -1 The reaction temperature was controlled by electric heating, and the conversion rate at different temperatures (80~400 ℃) was determined by programmed temperature increase. The reaction exhaust gas was analyzed by gas chromatography equipped with FID and TCD detectors.
[0063] Figure 3 is the relationship between the reaction temperature and conversion rate of the catalytic oxidation of toluene by the catalysts of Example 1 and Comparative Examples 1-2, Figure 4 The long-term stability data for the catalyst can be analyzed based on the experimental results: Mo doping can adjust the local environment of oxygen vacancies and acidic sites on manganese dioxide, further construct a core-shell structure modified with CeO2 nanoparticles, create sacrificial sites, inhibit SO2 adsorption on the catalyst surface, and thus improve the catalyst's sulfur resistance.
[0064] (3) X-ray photoelectron spectroscopy (XPS) was used to investigate the elemental composition, valence state, and content of the catalyst surface. The data obtained by the instrument were charge-corrected according to C 1s (284.8 eV) and processed and analyzed using Avantage software. Figure 5 (ab) For the O1s spectrum, the peak at 529.7-530.1 eV is the characteristic peak of surface lattice oxygen, and the peak at 531.4-531.9 eV is the characteristic peak of surface adsorbed oxygen. After molybdenum doping and CeO2 surface modification, O ads / O latt The ratio of Figure 5(a)), indicating that the number of oxygen species on the catalyst surface has increased. Since it is difficult to judge the subtle changes in the valence state of the Mn element on the surface of the manganese-based catalyst by the peak of Mn2p, the average valence state of the Mn element on the surface is generally calculated by the splitting energy level difference of Mn 3s to judge the change in the valence state of the Mn element on the surface. The calculation results show that the average valence state of Mn on the surface of the three samples of MnO2, Mo-MnO2, and CeO2@Mo-MnO2 are 3.74, 3.64, and 3.53 respectively. Figure 5 (b) The average valence of Mn on the catalyst surface is reduced by Mo doping and CeO2 surface modification, indicating that Mn on the catalyst surface 3+ The content increased.
[0065] (4) Ammonia temperature-programmed desorption (NH3-TPD) was used to investigate the surface acidity of the catalyst. The experimental conditions were as follows: 50 mg of catalyst was placed in a chemical adsorption instrument, heated to 300 °C at a rate of 10 °C / min, and kept in a He atmosphere for 60 minutes for pretreatment. After the pretreatment, 10% NH3 / He was introduced and adsorbed for 60 minutes. After the adsorption, the remaining gas in the tube was purged with helium, and the temperature was programmed to 800 °C at 10 °C / min for desorption experiments and TCD was used to record the experimental data. The surface acidity of the catalyst is an important factor affecting the catalyst's resistance to sulfur and chlorine. The acidic sites on the catalyst surface were analyzed by NH3-TPD. Figure 5As shown in Figure c, the NH3-TPD can be divided into weak acids (50-250°C), medium-strong acids (50-250°C), and strong acids (>450°C). Molybdenum doping and CeO2 surface modification increase the desorption temperature of NH3 in weak acids, and a new NH3 desorption peak appears at 300°C in CeO2@Mo-MnO2, likely due to the appearance of new acid sites on the MnO2 catalyst surface. Because the stability of hydroxyl groups decreases with increasing temperature, the acid sites in the low-temperature region of NH3-TPD are generally considered to be Brønsted acid sites, while those in the high-temperature region are Lewis acid sites. Brønsted acids not only donate H protons, allowing the dissociated Cl species of chlorobenzene to desorb as HCl, but also convert chlorobenzene to phenols through nucleophilic substitution, promoting the ring-opening reaction. Furthermore, Lewis acids, as the primary active sites for C-C bond reactions, can promote the deep oxidation of dechlorination intermediates. Due to the CeO2 modification layer, CeO2 has excellent oxygen storage capacity, and oxygen vacancies are easily formed on its surface. When CeO2 covers the surface of MnO2, oxygen vacancies can serve as active sites, promoting the migration or release of oxygen in MnO2. After MnO2 loses oxygen atoms, the valence state of Mn decreases from +4 to +3 to maintain charge balance, thereby reducing the valence state of Mn and improving its redox performance, thereby increasing its stability in catalytic combustion of VOCs. The CeO2 modified layer has a strong ability to preferentially bind to SO2, protecting the Mo-MnO2 core from SO2 poisoning. The preferential adsorption of SO2 on the CeO2 modified layer is due to its strong covalent bonding with SO2. SO2 is oxidized and solidified by lattice oxygen, leaving the gas phase and avoiding further attack on the active center Mn.
[0066] (2) Effects of different element ratios on catalysts Test Example 1 (different Mo / Mn mass ratios) (1) Preparation of molybdenum-doped manganese dioxide Mo-MnO2 catalyst, the specific steps are as follows: 4.5 g KMnO4 and 1.5 g (NH4)2C2O4 were added to 80 mL ultrapure water, and 0.61, 1.15, and 1.71 g (NH4)6Mo7O 24 4H2O was added to adjust the Mo / Mn mass ratio to 0.2:1, 0.4:1, and 0.6:1, respectively. Once fully dissolved, the mixture was transferred to a hydrothermal reactor and reacted at 160°C for 16 hours. After completion of the reaction, the product was filtered and repeatedly washed with ultrapure water and ethanol. It was then dried in an 80°C oven for 24 hours. Finally, the dried powder was calcined in a muffle furnace at 350°C for 6 hours to obtain the molybdenum-doped manganese dioxide (Mo-MnO2) catalyst.
[0067] (2) Preparation of CeO2@Mo-MnO2 catalyst. The specific steps are as follows: 1 g of urea and 0.5 g of hexamethylenetetramine were added to 100 mL of a mixture of anhydrous ethanol and ultrapure water (volume ratio of 1:1). After sufficient dissolution, 1.0 g of Mo-MnO2 was added and evenly dispersed. Subsequently, 0.5 g of Ce(NO3)3·6H2O was added and the mixture was reacted at 100°C for 6 hours. After completion of the reaction, the mixture was filtered, washed with ultrapure water and ethanol, and then dried in a forced air drying oven at 80°C. Finally, the dried sample was calcined in a muffle furnace at 300°C for 3 hours to obtain the CeO2@Mo-MnO2 catalyst.
[0068] Test Example 2 (different CeO2 / Mo-MnO2 mass ratios) (1) Preparation of molybdenum-doped manganese dioxide Mo-MnO2 catalyst, the specific steps are as follows: 4.5 g KMnO4 and 1.5 g (NH4)2C2O4 were added to 80 mL ultrapure water, and 1.15 g (NH4)6Mo7O 24 4H2O to control the Mo / Mn mass ratio to 0.4:1. Once fully dissolved, the mixture was transferred to a hydrothermal reactor and reacted at 160°C for 16 hours. After the reaction, the product was filtered and repeatedly washed with ultrapure water and ethanol. It was then dried in an 80°C oven for 24 hours. Finally, the dried powder was calcined in a muffle furnace at 350°C for 6 hours to obtain the molybdenum-doped manganese dioxide (Mo-MnO2) catalyst.
[0069] (2) Preparation of CeO2@Mo-MnO2 catalyst. The specific steps are as follows: 1 g of urea and 0.5 g of hexamethylenetetramine were added to 100 mL of a mixture of anhydrous ethanol and ultrapure water (volume ratio of 1:1). After sufficient dissolution, 1.0 g of Mo-MnO2 was added and uniformly dispersed. Subsequently, 0.25, 0.50, and 0.75 g of Ce(NO3)3·6H2O were added, respectively, and the mixture was reacted at 100°C for 6 hours. After the reaction, the mixture was filtered, washed with ultrapure water and ethanol, and then dried in a forced air drying oven at 80°C. Finally, the dried samples were calcined in a muffle furnace at 300°C for 3 hours to obtain CeO2@Mo-MnO2 catalysts with different CeO2:Mo-MnO2 mass ratios (0.1:1, 0.2:1, and 0.3:1).
[0070] Performance Testing The catalytic oxidation performance of different molybdenum-doped MnO2 ratios on sulfur-containing and chlorotoluene was investigated. The experimental results are as follows: Figure 6As shown in (a), when the mass ratio of Mo / Mn is 0.4:1, the catalytic performance of the catalyst is the best, and the temperature when toluene is completely converted into water and carbon dioxide is 300 ℃. When the molybdenum doping amount is lower than 0.4:1, the Mo 0.2 The catalytic performance of MnO2 catalyst is significantly lower than that of Mo 0.4 MnO2, this is because the manganese-based catalyst constructed with lower molybdenum doping has fewer active sites, while excessive molybdenum doping also inhibits the catalytic activity, which may be because higher molybdenum content occupies more manganese active centers, resulting in decreased activity. Then, the performance of manganese-based catalysts with different amounts of CeO2 modified on the surface was tested. Figure 6 (b) Ce 0.20 Mo 0.4 The MnO2 catalyst can achieve a toluene conversion rate of 99.99% at 280°C. When the mass ratio of CeO2 to Mo-MnO2 is 0.2:1, the catalyst achieves an optimal balance between redox ability and oxygen vacancy density, thus exhibiting the highest toluene oxidation activity.
[0071] (III) Effects of different preparation process parameters on catalysts Test Example 3 (Effect of (NH4)2C2O4 Concentration on Catalyst Morphology) (1) Preparation of molybdenum-doped manganese dioxide Mo-MnO2 catalyst, the specific steps are as follows: Add 4.5 g KMnO4 and 1.5 g (NH4)2C2O4 to appropriate amounts of ultrapure water (75 mL and 150 mL, respectively), and add 1.5 g (NH4)6Mo7O 24 4H2O; the mass ratio of Mo to Mn was controlled at 0.4:1. Once fully dissolved, the mixture was transferred to a hydrothermal reactor and reacted at 160°C for 16 hours. After the reaction, the product was filtered and repeatedly washed with ultrapure water and ethanol. It was then dried in an 80°C oven for 24 hours. Finally, the dried powder was calcined in a muffle furnace at 350°C for 6 hours to obtain the molybdenum-doped manganese dioxide (Mo-MnO2) catalyst.
[0072] like Figure 7 As shown, when the amount of ultrapure water is controlled at 75 mL, the obtained Mo-MnO2 catalyst appears as nanorods with a width of 15-50 nm ( Figure 7(a)), the crystallinity is relatively ideal; however, when the amount of ultrapure water is increased (75mL), the size of the nanorods becomes smaller and narrower, and the crystallinity deteriorates. The reason for the above differences is that when preparing the Mo-MnO2 catalyst, the amount of ultrapure water directly determines the concentration of (NH4)2C2O4 in the hydrothermal reaction system. (NH4)2C2O4 plays a key role in the hydrothermal preparation of manganese dioxide. It can reduce permanganate, adjust pH, complex and regulate crystallization, and inhibit side reactions. By optimizing its concentration, the purity, crystallinity and morphology controllability of the product can be improved, thereby improving the performance of the catalyst.
[0073] Test Example 4 (Effect of Urea Concentration on Catalyst Structure) (1) Preparation of molybdenum-doped manganese dioxide Mo-MnO2 catalyst, the specific steps are as follows: 4.5 g KMnO4 and 1.5 g (NH4)2C2O4 were added to 75 mL ultrapure water, and 1.5 g (NH4)6Mo7O 24 4H2O was added to control the Mo / Mn mass ratio to 0.4:1. Once fully dissolved, the mixture was transferred to a hydrothermal reactor and reacted at 160°C for 16 hours. After the reaction, the product was filtered and repeatedly washed with ultrapure water and ethanol. It was then dried in an 80°C oven for 24 hours. Finally, the dried powder was calcined in a muffle furnace at 350°C for 6 hours to obtain the molybdenum-doped manganese dioxide (Mo-MnO2) catalyst.
[0074] (2) Preparation of CeO2@Mo-MnO2 catalyst. The specific steps are as follows: 1 g of urea and 0.5 g of hexamethylenetetramine were added to appropriate amounts (80 mL, 160 mL, and 240 mL, respectively) of a mixture of anhydrous ethanol and ultrapure water (volume ratio of 1:1). Once fully dissolved, 1.0 g of Mo-MnO2 was added and evenly dispersed. Subsequently, 0.5 g of Ce(NO3)3·6H2O was added and reacted at 100°C for 6 hours. After completion of the reaction, the mixture was filtered, washed with ultrapure water and ethanol, and then dried in a forced air drying oven at 80°C. Finally, the dried sample was calcined in a muffle furnace at 300°C for 3 hours to obtain the CeO2@Mo-MnO2 catalyst.
[0075] like Figure 8 As shown in the figure, when the urea concentration is low (0.006 g / mL, the amount of mixed solution used is 160 mL), it can be seen from the electron microscope image of the CeO2@Mo-MnO2 catalyst that the cerium oxide nanoparticles are not uniformly dispersed on the surface of the Mo-MnO2 nanorods. This is because the concentration of the precipitant is low, which cannot fully precipitate the cerium nitrate in the solution.
[0076] Unless otherwise specified, the raw materials and equipment used in the present invention are commonly used in the art; the methods used in the present invention are conventional methods in the art unless otherwise specified.
[0077] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still fall within the scope of protection of the technical solution of the present invention.
Claims
1. A sulfur-chlorine-resistant CeO2@Mo-MnO2 catalyst, characterized in that include: Mo-doped MnO2 nanorods and CeO2 nanoparticles attached to the surface of Mo-doped MnO2 nanorods in a lattice pattern; The mass ratio of Mo to Mn is 0.1-1:1; The mass ratio of CeO2 and Mo-doped MnO2 is 0.01-0.5:1; The average valence of Mn is 3.50-3.
55.
2. The catalyst according to claim 1, characterized in that: The mass ratio of Mo to Mn is 0.2-0.6:1; The mass ratio of CeO2 and Mo-doped MnO2 is 0.05-0.3:1; The width of the Mo-doped MnO2 nanorods is 15-50 nm.
3. A method for preparing the catalyst according to claim 1 or 2, characterized in that include: 1) KMnO4, (NH4)2C2O4 and ammonium molybdate are subjected to a hydrothermal reaction, and the resulting product is filtered, washed, dried and calcined in an aerobic atmosphere to obtain Mo-MnO2; 2) Urea and hexamethylenetetramine were dissolved in an ethanol aqueous solution, and Mo-MnO2 and Ce salt were added to react. The resulting product was filtered, washed, dried, and aerobic calcined to obtain a sulfur- and chlorine-resistant CeO2@Mo-MnO2 catalyst.
4. The preparation method according to claim 3, wherein: In step 1), The mass ratio of KMnO4 and (NH4)2C2O4 is 2:1-4:1; The content of (NH4)2C2O4 in the reaction system of the hydrothermal reaction is 0.015-0.025 g / mL.
5. The preparation method according to claim 3 or 4, characterized in that: In step 1), The hydrothermal reaction temperature is 120-260°C and the time is 6-36 hours; The drying temperature is 50-110°C; The calcination temperature is 280-500° C. and the calcination time is 2-10 hours.
6. The preparation method according to claim 3, wherein: In step 2), The mass ratio of urea to hexamethylenetetramine is 1:1-3:1; The content of urea in the reaction system is 0.006-0.018 g / mL.
7. The preparation method according to claim 3 or 6, characterized in that: In step 2), The reaction temperature is 50-150°C and the reaction time is 1-8 hours; The calcination temperature is 280-480° C. and the calcination time is 2-10 hours.
8. Use of the catalyst according to claim 1 or 2 or the catalyst obtained by the preparation method according to any one of claims 3 to 8 in the catalytic oxidation of sulfur-containing and chlorine-containing VOCs.
9. The use according to claim 8, characterized in that include: The sulfur- and chlorine-resistant CeO2@Mo-MnO2 catalyst is added to a fixed-bed reactor, and sulfur- and chlorine-containing VOCs are introduced to carry out catalytic oxidation reactions.
10. The use according to claim 9, characterized in that: The VOCs are toluene, chlorobenzene content ≥ 50 ppm, and SO2 content ≥ 50 ppm.
Citation Information
Patent Citations
Preparation method of ruthenium molybdenum manganese composite electrocatalyst for purifying chlorine-containing organic waste gas
CN119588348A
Cited By
Modified catalyst for resisting chloride ion poisoning and preparation method thereof
CN120827865A