High-temperature-resistant insulated copper wire and preparation method thereof
By coating the surface of the copper wire with a polysilazane mixed filler layer to form a dense organic-inorganic hybrid coating layer, the problems of decreased mechanical strength and poor insulation stability of traditional copper wire at high temperatures are solved, achieving the needs of high-frequency performance and miniaturized inductor materials.
Patent Information
- Application Number
- CN202511010046.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-22
- Publication Date
- 2025-09-12
AI Technical Summary
Traditional copper wires experience decreased mechanical strength, increased surface oxidation corrosion, deteriorated electrical conductivity, and poor insulation layer stability in high-temperature environments, making them unable to meet the high-frequency performance and miniaturization requirements of modern electronic equipment.
A polysilazane mixed filler layer is used, including a matrix resin, inorganic fillers, functional fillers, auxiliary components, etc., to form a dense organic-inorganic hybrid coating layer through coating and curing to improve insulation performance and thermal stability.
It maintains good mechanical and insulation properties at high temperatures, ensures stable electrical conductivity, and is suitable for electronic equipment in high-temperature environments.
Smart Images

Figure CN120636905A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of insulated copper wires, and in particular to a high-temperature resistant insulated copper wire and a preparation method thereof. Background Art
[0002] With the continuous miniaturization and advancement of high-performance electronic devices, the requirements for inductor components are also increasing. Traditional inductor materials are increasingly unable to meet the demands of modern electronic devices in terms of high-frequency characteristics and miniaturization. In the early days of tube radios, inductors were primarily used in tuning circuits, with relatively low requirements for precision and high-frequency performance. However, the advent of transistors and integrated circuits has significantly increased the operating frequency and signal transmission speed of electronic devices, significantly raising the requirements for high-frequency performance and miniaturization of inductors. For example, modern communications equipment, such as 5G mobile phones, operates in the millimeter-wave band. In such high-frequency environments, inductors must be able to efficiently transmit signals and have good electromagnetic compatibility. Enameled copper wire, with its excellent insulation properties and low high-frequency losses, is an ideal material for high-performance inductors. On the one hand, copper, as an excellent conductive material, has high electrical conductivity (second only to silver) and good thermal conductivity, which effectively reduces energy loss during transmission. On the other hand, the development of insulating varnish technology is key to enameled copper wire technology. Early insulating varnishes were mainly simple organic varnishes. With the development of the chemical industry, a variety of high-performance insulating varnishes have emerged. These insulating varnishes provide improved insulation performance and can withstand higher voltages and temperatures. This type of enameled copper wire is widely used in high-power inductive devices such as industrial motors and transformers. Existing conventional copper wire (such as bare copper wire and standard polyimide enameled wire) is susceptible to the following problems when subjected to long-term service in oxidizing or humid, corrosive, high-temperature environments at or above 400°C: 1. A significant decrease in mechanical strength (e.g., grain growth leading to reduced plasticity); 2. Intensified surface oxidation corrosion (formation of a thick Cu2O / CuO oxide film); and 3. Deterioration in electrical conductivity (the oxide film increases contact resistance). Furthermore, the surface insulation layer or bare copper surface becomes less stable due to high temperatures, and in severe cases, the outer insulation layer may deform. Simultaneously, the high temperature is transferred to the copper wire core, causing the core temperature to rise and increasing resistance, which in turn negatively impacts the copper wire's transmission efficiency.
[0003] Polysilazane contains silicon-nitrogen (Si-N) bonds in its molecular structure. This chemical bond has a high bond energy, which makes polysilazane have good thermal stability. Compared with traditional organic polymers, it can maintain structural integrity at higher temperatures. For example, polysilazane resins containing aromatic / alkyl substitutions (such as PSZ-101) that have been pre-cured at 150-200°C and cross-linked at high temperatures above 400°C can still maintain good thermal stability (weight loss rate ≤3% at 500°C), mechanical properties (tensile strength ≥10MPa, elongation at break ≥2%) and electrical insulation properties (dielectric constant 3.0-3.5, breakdown strength ≥20kV / mm, volume resistivity ≥10) when they are used for a long time (≥100 hours) in an inert atmosphere (nitrogen / argon) or a low oxygen content (≤5%) at a high temperature of 400-500°C. 13 Ω·m), providing viable technical support for its use as a base material for high-temperature enamel coatings in the preparation of enameled copper wire with long-term operating temperatures of 400-500°C (e.g., electromagnetic winding components in the aerospace and power electronics sectors). Polysilazane forms a uniform, dense SiO2 protective film on the surface of copper wire under high-temperature conditions. This film not only provides excellent insulation properties but also resists cracking or detaching at high temperatures. The film formation process can be achieved through simple thermal or chemical curing, facilitating industrial production. Summary of the Invention
[0004] To solve the problems in the above-mentioned background technology, the present invention provides a high-temperature resistant insulated copper wire and a preparation method thereof. The high-temperature resistant insulated copper wire includes a copper wire body and a polysilazane mixed filler layer uniformly coated on the surface of the copper wire body.
[0005] The thickness of the polysilazane mixed filler layer is 5 μm to 30 μm, and the thickness deviation is ≤±1 μm.
[0006] The polysilazane mixed filler layer is composed of the following components in parts by weight: Base resin (polysilazane) 20-30 parts; Inorganic fillers: 10-20 parts of aluminum oxide, 8-12 parts of titanium oxide, 4-6 parts of aluminum silicate; Functional filler: 5-10 parts of color filler; 5-10 parts of high temperature resistant filler; Auxiliary components: 10-20 parts of organic modified silicone resin; 5-10 parts of curing agent; 5-10 parts of diluent; 5-10 parts of binder; 5-10 parts of auxiliary agent.
[0007] As a further improvement of the above solution, the aluminum oxide is nano-scale aluminum oxide powder.
[0008] As a further improvement of the above solution, the titanium oxide is nano-scale titanium dioxide powder.
[0009] As a further improvement of the above solution, the high temperature resistant filler is a mixture of ceramic powder and silicate, wherein the mixing ratio is 5:5; As a further improvement of the above solution, the diluent is xylene; the color filler is selected from one of iron oxide and copper oxide; As a further improvement of the above solution, the curing agent is polyamide.
[0010] As a further improvement of the above solution, the binder is a polyurethane aqueous dispersion; As a further improvement of the above solution, the auxiliary agent is a phosphate stabilizer.
[0011] A method for preparing a high-temperature resistant insulated copper wire comprises the following steps: applying a uniformly mixed polysilazane mixed filler layer on the surface of the copper wire body, and after baking and curing, converting the polysilazane mixed filler layer into a dense organic-inorganic mixed coating layer, thereby finally forming a high-temperature resistant insulated flat copper wire.
[0012] Specifically, the following steps are included: S1. Measuring step: According to the pre-set formula, accurately measure polysilazane, aluminum oxide, titanium oxide, aluminum silicate, color filler, high temperature resistant filler, organic modified silicone resin, curing agent, diluent, binder and additives to ensure that the measurement accuracy of each raw material meets the preparation requirements; S2, premixing step: adding the measured polysilazane, aluminum oxide, titanium oxide, aluminum silicate, color filler and high-temperature resistant filler into the premixer, starting the premixing operation, and preliminarily mixing the components; S3, homogenization step: After completing the high-speed mixing process, add the organic modified silicone resin, curing agent, diluent, binder and additives into the homogenizer and perform homogenization to obtain a uniform mixture with a viscosity of 1500-2000 mPa·s (25°C); S4, cleaning step: placing the copper wire body (1) in an ultrasonic cleaner, cleaning the surface of the copper wire body with an alcohol solution and an acetone solution, and then baking and drying the copper wire body to obtain a copper wire body with a smooth surface; S5, coating step: evenly coating the mixed material of step S3 on the surface of the copper wire. Different methods can be used for copper wires of different shapes to control the coating thickness; Flat wire dip coating process (felt coating method): using felt as a coating tool, fully dipping the felt into the polysilazane mixed filler, and then gradually laminating the filled felt onto the surface of the copper wire to achieve the operation steps of evenly coating the polysilazane mixed filler on the copper wire; Dip coating process for round wire: A vertical dip coating machine is used to immerse the copper wire into the mixed paint at a speed of 0.3m / min. The coating thickness is controlled by a squeeze roller (with a gap of 0.25mm) to ensure that the insulation layer evenly covers the surface of the round wire. S6. Curing step: Curing is performed in a vacuum oven at 150°C-200°C (vacuum degree -0.09MPa) according to the following steps: "maintaining at 150°C for 30 minutes (pre-curing), heating to 200°C and maintaining for 60 minutes (complete curing)".
[0013] Alternatively, cure according to the procedure of "pre-curing at 120°C for 20 minutes (removing the diluent) → heating to 180°C for 40 minutes (forming a semi-cured self-adhesive layer) → heating to 220°C for final curing for 30 minutes (complete cross-linking)". During the curing process, nitrogen protection (flow rate 0.5m³ / h) is introduced to prevent oxidation of the insulating layer. Inspection steps: After S6 solidifies, randomly cut 10cm copper wire, cut the cross section with a microcutting machine, observe the insulation layer structure with a metallographic microscope, and measure the thickness at 10 points with a micro thickness gauge to confirm the insulation layer thickness deviation range (deviation ≤ ± 0.3μm). Use a pinhole detector to inspect the 10m copper wire and check the number of pinholes. If the number of pinholes = 0, it means there are no bubbles or coating leaks. Check whether the coating is uniform and dense and whether there are obvious pores.
[0014] S7, standing step: After the above steps, the solidified copper wire is naturally cooled to room temperature (25°C), and finally an inorganic-organic combined coated insulated copper wire with a uniform and smooth surface is obtained.
[0015] Optionally, in step S6, the outer surface of the copper wire body of the polysilazane mixed filler layer is cut to detect the thickness and uniformity of the polysilazane mixed filler layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic diagram of the structure of high temperature resistant insulated round copper wire and flat copper wire; Figure 2 The microstructure of the coating of polysilazane-coated insulated rectangular copper wire; Figure 3 Micrograph of polysilazane-coated insulated round copper wire. DETAILED DESCRIPTION
[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Figure 1 The specific structure of the high temperature resistant insulated copper wire according to the embodiment of the present invention is described. Figure 1As shown, this embodiment provides a high-temperature resistant insulated copper wire, including a copper wire body 1 and a polysilazane filler layer 2 , wherein the polysilazane filler layer is coated on the surface of the copper wire body 1 .
[0018] It should be noted that the polysilazane filler layer 2 is coated on the surface of the copper wire body 1 to form an organic-inorganic combined insulated copper wire that is resistant to high temperature, high pressure, high hardness and quality, and uniformly coated, and has strong stability and reliability, good density and wear resistance, and meets the application temperature in the use environment and component manufacturing process.
[0019] Optionally, the polysilazane filler layer 2 has a uniform thickness within the range of 10-20 μm. This uniformity ensures that the insulated copper wire is more evenly heated and heat-resistant. Because there are no localized thinner areas, adverse effects on key properties of the high-temperature-resistant insulated copper wire, such as its high-temperature resistance, high-voltage resistance, and high hardness, are effectively avoided. This ensures more reliable and stable overall product performance, significantly improving the adaptability and durability of the high-temperature-resistant insulated copper wire in practical applications and providing a solid guarantee for its stable operation under various complex operating conditions.
[0020] Example 1 A method for preparing a high-temperature resistant insulated flat copper wire comprises the following steps: applying a uniformly mixed polysilazane filler layer on the surface of a copper wire body (1); and after baking and curing, converting the polysilazane filler layer into a dense organic-inorganic hybrid coating layer, thereby finally forming a high-temperature resistant insulated flat copper wire. During high-temperature use, the polysilazane is further converted into inorganic silicon dioxide to form a uniform and dense ceramic coating layer, further increasing the heat resistance temperature.
[0021] Optionally, a method for preparing a high-temperature resistant insulated copper wire comprises the following steps: S1. Measuring step: According to the above formula, use an electronic balance (accuracy 0.01g) to accurately measure each raw material. The nano-scale powder needs to be passed through a 200-mesh sieve to remove agglomerates to ensure the dispersion of the raw materials; According to the pre-set formula, polysilazane, aluminum oxide, titanium oxide, aluminum silicate, color filler, high temperature resistant filler, diluent, binder and additives are accurately measured to ensure that the measurement accuracy of each raw material meets the preparation requirements; The polysilazane mixed filler layer is composed of the following components in parts by weight: Base resin: 25 parts of polysilazane (in the range of 20-30 parts, preferably 25 parts); Inorganic fillers: 15 parts (10-20 parts, preferably 15 parts) of nano-aluminum oxide (particle size 10-20nm), 10 parts (8-12 parts, preferably 10 parts) of nano-titanium dioxide (particle size 5-10nm), 5 parts of aluminum silicate (fiber length ≤ 5μm); Functional fillers: color filler (iron oxide red, particle size ≤ 1 μm) 8 parts (5-10 parts, preferably 8 parts), high temperature resistant filler (ceramic powder (boron nitride): silicate (mica powder) = 5:5) 8 parts (5-10 parts, preferably 8 parts); Auxiliary components: organic modified silicone resin 15 parts (10-20 parts, preferably 15 parts), curing agent (polyamide) 7 parts (5-10 parts, preferably 7 parts), diluent (xylene, analytical grade) 8 parts (5-10 parts, preferably 8 parts), binder (polyurethane aqueous dispersion, solid content 30%) 7 parts (5-10 parts, preferably 7 parts), auxiliary agent (phosphate stabilizer, antioxidant) 6 parts (5-10 parts, preferably 6 parts); Recipe Instructions: 1. Nano-alumina / titanium dioxide: Filled in the polysilazane network, it reduces the porosity of the insulation layer and improves thermal stability (weight loss rate ≤3% at 500°C) and electrical insulation performance. 2. Polysilazane: It combines flexibility and high-temperature resistance. After curing, it forms an organic-inorganic hybrid structure, avoiding the brittleness of pure inorganic materials. 3. Ceramic powder / mica powder mixture: It has a flaky structure, delays oxygen diffusion at high temperatures, and enhances the thermal shock resistance of the insulation layer. 4. Organically modified silicone resin and polyurethane binder: It alleviates the brittleness of inorganic fillers and improves the bonding strength between the insulation layer and the copper wire body.
[0022] Preparation steps (adapted to the dipping process of flat wire) S2, premixing step: polysilazane, nano-alumina, nano-titanium dioxide, aluminum silicate, red iron oxide, ceramic powder-mica powder mixture is put into a high-speed premixer (speed 1500r / min, time 15min) to preliminarily mix the inorganic filler and the resin; S3, homogenization step: adding the organic modified silicone resin, polyamide curing agent, xylene diluent, polyurethane binder and phosphate stabilizer to the premix, transferring the mixture to a planetary homogenizer (speed 2500 r / min, time 30 min) to obtain a uniform mixture with a viscosity of 1500-2000 mPa·s (25°C); S4. Copper wire pretreatment: A flat copper wire (T2 copper, 2.0 mm × 5.0 mm) was placed in an ultrasonic cleaner (frequency 40 kHz). Surface oil was removed using a 75% alcohol solution (cleaning for 10 min) and then an acetone solution (cleaning for 5 min). The wire was then dried in a vacuum oven at 120°C (vacuum degree -0.09 MPa) for 30 min to obtain a smooth surface (contact angle ≤ 10°, as measured by a contact angle meter). S5, coating step: using the felt coating method (felt thickness 5mm, compression rate 30%), the mixture is evenly coated on the surface of the copper wire at a coating speed of 0.5m / min to ensure a uniform coating thickness; S6. Curing step: Place the coated copper wire in a vacuum oven (vacuum degree -0.09 MPa) and cure it according to the procedure of "maintaining at 150°C for 30 minutes (pre-curing), heating to 200°C for 60 minutes (complete curing)" to obtain a semi-cured insulated copper wire; Optional inspection steps: After S6 solidification, randomly cut 10cm copper wires, cut cross sections with a micro-cutting machine, observe the insulation layer structure with a metallographic microscope, and measure the thickness at 10 points with a micro-thickness gauge. The results show that the insulation layer thickness is 10.2μm, with a thickness deviation of ≤±0.5μm. The coating is uniform and dense, with no obvious pores. S7, post-processing step: The solidified copper wire is naturally cooled to room temperature (25°C), and is wound by a wire take-up machine (tension 10N), and finally an inorganic-organic combined coated high-temperature resistant insulated flat copper wire with a uniform and smooth surface is obtained.
[0023] Case 1 test results: Uniform thickness of the insulation layer (deviation ≤ ±0.3μm): thanks to the good dispersion of the nanofiller (homogenizer speed 2500r / min) and precise control of the felt coating method (coating speed 0.5m / min); Excellent high-temperature insulation performance (breakdown voltage 2723V at 200°C): attributed to the organic-inorganic hybrid structure (containing Si-N and Si-O bonds) formed after polysilazane curing, and the reduction of porosity by nano-alumina / titanium dioxide filling; Good mechanical properties (elongation 24.57%): The addition of organic modified silicone resin and polyurethane binder alleviates the brittleness of inorganic fillers, ensuring good bonding between the insulation layer and the copper wire body (peel strength 0.65N / mm); Outstanding thermal stability (weight loss rate of 2.8% at 500℃): Polysilazane further cross-links at high temperature to form a silicon dioxide ceramic layer (Si-O-Si network), which effectively blocks the contact between oxygen and copper wire and avoids oxidation of copper wire. Figure 2 As shown in the SEM photo of the surface of the insulating layer after heating at 500℃, there are no obvious cracks, the wrapping is uniform, and there are no pores.
[0024] The high-temperature-resistant insulated flat copper wire prepared in this example achieves the combined performance of high insulation (2723V breakdown voltage at 200°C), good mechanical properties (24.57% elongation), and excellent thermal stability (2.8% weight loss at 500°C) by optimizing the polysilazane mixed filler formula (nanoscale inorganic filler, aromatic substituted resin) and precisely controlling the preparation process (premixing-homogenization-curing). This meets the demand for high-temperature-resistant insulated copper wire for long-term operation below 400°C in fields such as aerospace and power electronics.
[0025] Example 2 This example addresses the high-temperature insulation requirements for 0.2mm diameter round copper wire. A polysilazane-modified lacquer with a self-adhesive layer was designed, with a focus on optimizing self-adhesion, coating uniformity, and high-temperature crack resistance. The polysilazane mixed insulation layer (by parts by weight) consists of the following components: Base resin: 28 parts of hydroxy-terminated polysilazane (containing methyl / vinyl substitution) (in the range of 20-30 parts, preferably 28 parts, to improve self-adhesion and flexibility); Inorganic fillers: nano-silicon dioxide (particle size 5-10nm) 12 parts (10-15 parts, preferably 12 parts, to reduce the porosity of the insulating layer and improve thermal stability), micron-sized mica powder (particle size 1-3μm) 8 parts (5-10 parts, preferably 8 parts, to enhance thermal shock resistance); Self-adhesive component: 18 parts of hydroxyl-terminated polysiloxane (solid content 40%) (15-20 parts, preferably 18 parts, to give the insulating layer self-adhesive properties); Auxiliary components: curing agent (polyetheramine) 6 parts (5-10 parts, preferably 6 parts, low-temperature flexible curing), diluent (ethyl acetate, analytical grade) 10 parts (8-12 parts, preferably 10 parts, to adjust the viscosity to adapt to dipping), binder (acrylate emulsion, solid content 35%) 7 parts (5-10 parts, preferably 7 parts, to improve the bonding strength between the insulation layer and the copper wire), auxiliary agent (polydimethylsiloxane, defoaming agent) 5 parts (3-7 parts, preferably 5 parts, to eliminate bubbles during the coating process).
[0026] Hydroxyl-terminated polysilazane (containing methyl / vinyl substitution): The vinyl group enhances compatibility with the self-adhesive component (hydroxyl-terminated polysiloxane). After curing, it forms an organic-inorganic hybrid network (containing Si-N, Si-O, and C-C bonds), balancing high temperature resistance (weight loss ≤ 4% at 500°C) and flexibility (elongation at break ≥ 5%). Nano-silica + mica powder: Nano-silica fills the gaps in the resin to reduce pinholes; mica powder has a flaky structure, which delays oxygen diffusion at high temperatures and improves resistance to thermal cracking; Hydroxyl-terminated polysiloxane (KH-550 modified, solid content 40%): As a self-adhesive component, it forms reversible hydrogen bonds by cross-linking with the hydroxyl groups in polysilazane. When heated (120-150°C), the hydrogen bonds break, making the insulation layer self-adhesive and facilitating the self-adhesive molding of the winding coil.
[0027] Preparation steps (adapted to the dipping process of round wire) S1. Measuring step: According to the above formula, use an electronic balance (accuracy 0.01g) to accurately measure each raw material. Nano-silicon dioxide needs to be ultrasonically dispersed (frequency 20kHz, time 20min) to remove agglomerates and ensure dispersion; S2, premixing step: put the hydroxyl-terminated polysilazane, nano-silica, and mica powder into a high-speed premixer (speed 1200 r / min, time 10 min) to preliminarily mix the inorganic filler and the resin; S3, homogenization step: Add hydroxyl-terminated polysiloxane, polyetheramine curing agent, ethyl acetate diluent, acrylate binder and polydimethylsiloxane defoamer to the premix, transfer to a high shear homogenizer (speed 3000 r / min, time 40 min), and obtain a uniform mixed paint with a viscosity of 800-1200 mPa·s (25°C) (the viscosity is measured by a rotational viscometer to meet the requirements of dipping); S4. Copper wire pretreatment: Place T2 copper round wire (diameter 0.2 mm, surface finish Ra ≤ 0.6 μm) in an ultrasonic cleaner (frequency 40 kHz) and clean it with 75% alcohol solution for 15 minutes to remove surface oil stains. Then, dry it in a 100°C forced air oven for 20 minutes to obtain a copper wire body with no impurities on the surface. S5, Dipping step: Using a vertical dipping machine, immerse the copper wire in the mixed paint at a speed of 0.3m / min. The coating thickness is controlled by a squeezing roller (gap 0.25mm) to ensure that the insulation layer evenly covers the surface of the round wire; S6. Curing step: Place the dip-coated copper wire in a tunnel-type curing oven and perform curing according to the procedure of "pre-curing at 120°C for 20 minutes (removing the diluent) → heating to 180°C for 40 minutes (forming a semi-cured self-adhesive layer) → heating to 220°C for final curing for 30 minutes (complete cross-linking)". During the curing process, nitrogen protection (flow rate 0.5m³ / h) is introduced to prevent oxidation of the insulating layer. Optional testing steps: After S6 is finally cured, randomly cut 5cm of copper wire and measure the insulation thickness at 10 points using a microscopic thickness gauge. The results show an average thickness of 12.6μm and a thickness deviation of ≤±0.8μm (the round wire diameter is small, and the insulation layer ensures insulation performance). Use a pinhole detector to test 10m of copper wire, and the number of pinholes = 0 (no bubbles or missing coating). S7, post-processing step: The solidified copper wire is naturally cooled to room temperature (25°C), and is wound by a wire take-up machine (tension 5N) to finally obtain a high-temperature resistant insulated round copper wire with a self-adhesive layer.
[0028] Case 2 test results: Excellent self-adhesive properties: The cross-linked structure of hydroxyl-terminated polysiloxane and polysilazane gives the insulation layer excellent self-adhesive properties (peel strength 0.72N / mm) when heated at 120°C, meeting the "self-adhesive molding" requirements of the winding coil; Outstanding high temperature crack resistance: Nano-silicon dioxide filling reduces the internal pores of the insulation layer, and the flaky structure of the mica powder delays the diffusion of oxygen at high temperatures. After sintering at 500℃ for 2 hours, the insulation layer has no cracking or falling off (such as Figure 3As shown in Figure 2, the micrograph of the surface of the insulating layer after sintering shows no obvious cracks); Figure 3 In the figure, the cross-sectional diameter of the copper in the round copper wire is 0.198 mm. From this, it can be seen that even if it is coated with ultra-fine copper wire, the coating is uniform.
[0029] Insulation performance meets small diameter requirements: The 12.6μm insulation thickness (deviation ≤±0.6μm) ensures a breakdown voltage of 1757V at 200°C (much higher than the standard requirement of 1000V), suitable for precision winding applications of round copper wire with a small diameter of 0.2mm. Mechanical properties remain good: the elongation of the copper wire body is 28.5% (much higher than the standard 15%), indicating that the coating and curing of the insulation layer have no negative impact on the mechanical properties of the copper wire.
[0030] This example addresses the high-temperature insulation requirements for small-diameter 0.2mm round copper wire. By optimizing the PSZ modified lacquer formula (adding hydroxyl-terminated polysiloxane to enhance self-adhesion and nano-silica and mica powder to enhance high-temperature stability) and employing a dip-coating process to ensure uniform coating of the round wire, a high-temperature-resistant insulated round copper wire with a self-adhesive layer was produced. This product combines excellent self-adhesion (peel strength of 0.72 N / mm), high-temperature cracking resistance (no cracking after sintering at 500°C), and excellent insulation performance (breakdown voltage of 1757V at 200°C). It is suitable for small-diameter windings (such as micromotors and sensor windings) in electronic equipment, precision instruments, aerospace, and other fields. It addresses the issues of poor self-adhesion and high-temperature cracking associated with traditional round copper wire insulation.
Claims
1. A high temperature resistant insulated copper wire, characterized in that: The high-temperature resistant insulated copper wire comprises a copper wire body and a polysilazane mixed filler layer uniformly coated on the surface of the copper wire body. The thickness of the polysilazane mixed filler layer is 5 μm to 30 μm.
2. The high temperature resistant insulated copper wire according to claim 1, characterized in that: The polysilazane mixed filler layer is composed of the following components in parts by weight: Base resin: 20-30 parts of polysilazane; Inorganic fillers: 10-20 parts of aluminum oxide, 8-12 parts of titanium oxide, 4-6 parts of aluminum silicate; Functional filler: 5-10 parts of color filler, 5-10 parts of high temperature resistant filler; Auxiliary components: 10-20 parts of organic modified silicone resin, 5-10 parts of curing agent, 5-10 parts of diluent, 5-10 parts of binder, and 5-10 parts of additives.
3. The high temperature resistant insulated copper wire according to claim 2, characterized in that: The aluminum oxide is nano aluminum oxide powder; or The titanium oxide is nano-sized titanium dioxide powder; or The high temperature resistant filler is a mixture of ceramic powder and silicate, wherein the mixing ratio is 5:5; or The diluent is xylene; or The color filler is one of iron oxide and copper oxide; or The curing agent is polyamide; or The binder is a polyurethane aqueous dispersion; or The auxiliary agent is a phosphate stabilizer.
4. The method for preparing the high temperature resistant insulated copper wire according to claim 2, characterized in that: The preparation method comprises the following steps: S1. Measuring step: measuring polysilazane, aluminum oxide, titanium oxide, aluminum silicate, color filler, high temperature resistant filler, organic modified silicone resin, curing agent, diluent, binder and additives; S2, premixing step: polysilazane, aluminum oxide, titanium oxide, aluminum silicate, color filler and high temperature resistant filler are placed in a premixer, and the premixing operation is started to preliminarily mix the ingredients; S3, homogenization step: after completing the high-speed mixing process, adding the organic modified silicone resin, curing agent, diluent, binder and additives into the homogenizer and performing homogenization to obtain a uniform mixed material with a viscosity of 1500-2000 mPa·s; S4, cleaning step: cleaning the surface of the copper wire body, and then baking and drying it to obtain a copper wire body with a smooth surface; S5, coating step: evenly coating the mixed material of step S3 on the surface of the copper wire, controlling the coating thickness; S6, curing step: curing the coating layer on the surface of the copper wire by pre-curing-curing method, preventing oxidation during the curing process; S7, standing step: After the above steps, the solidified copper wire is naturally cooled to room temperature, and finally an inorganic-organic combined coated insulated copper wire with a uniform and smooth surface is obtained.
5. The method for preparing the high temperature resistant insulated copper wire according to claim 4, characterized in that: In step S4, the surface of the copper wire body is cleaned using an alcohol solution and an acetone solution in sequence.
6. The method for preparing the high temperature resistant insulated copper wire according to claim 4, characterized in that: In step S5, a felt coating method is adopted: using a felt as a coating tool, the felt is fully dipped in the polysilazane mixed filler, and then the felt dipped in the filler is gradually attached to the surface of the copper wire to achieve an operation step of uniformly coating the polysilazane mixed filler on the copper wire; or A vertical dip coating machine was used to immerse the copper wire into the mixed paint at a speed of 0.3 m / min, and the coating thickness was controlled by a squeeze roller.
7. The method for preparing the high temperature resistant insulated copper wire according to claim 4, characterized in that: In step S5, a vertical dip coating machine is used to immerse the copper wire in the mixed paint at a speed of 0.3 m / min. The coating thickness is controlled by a squeezing roller to ensure that the insulating layer evenly covers the surface of the round wire.
8. The method for preparing the high temperature resistant insulated copper wire according to claim 4, characterized in that: Step S6: Curing is as follows: pre-curing in a vacuum oven at 150°C-200°C for 30 minutes, then heating to 200°C for 60 minutes to fully cure.
9. The method for preparing the high temperature resistant insulated copper wire according to claim 4, characterized in that: Step S6: curing steps are as follows: pre-curing at 120°C for 20 minutes → heating to 180°C for curing for 40 minutes → heating to 220°C for final curing for 30 minutes, with nitrogen protection being introduced during the curing process.
10. The method for preparing the high temperature resistant insulated copper wire according to claim 4, characterized in that: Add an additional inspection step after S6 solidification: randomly cut a section of copper wire, cut the cross section with a micro-cutting machine, observe the insulation layer structure with a metallographic microscope, and measure the thickness at 10 points with a micro-thickness gauge to confirm the insulation layer thickness deviation range; and Use a pinhole detector to check for pinholes.
Citation Information
Cited By
Stator bar end 3D transposition insulation filling forming process
CN120915074A
Co-fired TLVR coupled inductor, preparation method and application thereof
CN122455533A