Solid-state fluorescence-emitting carbonized polymer point as well as preparation method and application thereof

By microwave heating a mixed solution of polyethyleneimine and small molecule acid, solid-state fluorescent carbonized polymer dots were prepared, which solved the problem of easy aggregation and quenching of solid-state fluorescent carbonized polymer dots and achieved stable fluorescent emission performance, making it suitable for a variety of application scenarios.

CN120718647APending Publication Date: 2025-09-30QUANZHOU NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510801741.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-16
Publication Date
2025-09-30

AI Technical Summary

Technical Problem

In the prior art, fluorescent carbonized polymer dots are easily aggregated after being prepared into a solid state, resulting in fluorescence quenching, making it difficult to maintain fluorescence emission.

Method used

Polyethyleneimine is used as a carbon source, mixed with a small molecule acid and then treated with microwave heating to form molecular fluorescent centers, avoiding fluorescence quenching caused by aggregation, and preparing solid-state fluorescent carbonized polymer dots.

Benefits of technology

The fluorescence emission performance of solid-state carbonized polymer dots was achieved, with stable luminescence intensity and good excitation wavelength independence, and is suitable for luminescent materials, biomedicine, optoelectronic devices and sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120718647A_ABST
    Figure CN120718647A_ABST
Patent Text Reader

Abstract

The invention provides a solid-state fluorescence-emitting carbonized polymer dot as well as a preparation method and application thereof, and belongs to the technical field of luminescent polymer nano materials. The preparation method provided by the invention comprises the following steps: (1) mixing polyethyleneimine, small molecular acid and water to obtain a mixed solution; the small molecular acid comprises one or more of citric acid, tartaric acid, EDTA (Ethylene Diamine Tetraacetic Acid), sulfuric acid, acetic acid and phosphoric acid; and (2) carrying out microwave heating treatment on the mixed solution obtained in the step (1), and then drying to obtain the solid-state fluorescence-emitting carbonized polymer point. According to the preparation method, polyethyleneimine is adopted as a carbon source, small molecular acid is added as an auxiliary agent, the solid carbonized polymer point is obtained through microwave heating treatment, and the prepared solid carbonized polymer point has fluorescence emission property. Results of the embodiment show that the solid carbonized polymer dots prepared by the method present a blue or green fluorescence emission phenomenon under an ultraviolet lamp.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of luminescent polymer nanomaterials, and in particular relates to a solid-state fluorescent carbonized polymer dot and a preparation method and application thereof. Background Art

[0002] Fluorescent carbonized polymer dots (CPDs), a unique carbon nanomaterial with the advantages of tunable luminescence and particle size, have attracted widespread attention in recent years in areas such as room-temperature phosphorescence (RTP). Existing techniques primarily use polymers as raw materials to produce fluorescent CPD aqueous solutions through hydrothermal reactions. However, drying these aqueous solutions results in solid CPDs that aggregate and quench fluorescence. Therefore, the preparation of fluorescent solid CPDs remains a challenge in this field. Summary of the Invention

[0003] The purpose of the present invention is to provide a solid-state fluorescent carbonized polymer dot and its preparation method and application. The preparation method provided by the present invention can be used to prepare solid-state fluorescent carbonized polymer dots.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing solid-state fluorescent carbonized polymer dots, comprising the following steps:

[0006] (1) mixing polyethyleneimine, a small molecule acid, and water to obtain a mixed solution; the small molecule acid comprises one or more of citric acid, tartaric acid, EDTA, sulfuric acid, acetic acid, and phosphoric acid;

[0007] (2) The mixed solution obtained in step (1) is subjected to microwave heating treatment and then dried to obtain solid-state fluorescent carbonized polymer dots.

[0008] Preferably, the weight average molecular weight of the polyethyleneimine in step (1) is 600 to 70,000.

[0009] Preferably, in step (1), when the small molecule acid is one or more of citric acid, tartaric acid and EDTA, the mass ratio of polyethyleneimine to the small molecule acid is 1:(0.5-4).

[0010] Preferably, in step (1), the volume ratio of polyethyleneimine to water is 1 g: (15-50) mL.

[0011] Preferably, the pH value of the mixed solution in step (1) is 0-9.

[0012] Preferably, in step (2), the power of the microwave heating treatment is 80-800 W, the temperature of the microwave heating treatment is 150-160° C., and the time of the microwave heating treatment is 1-10 min.

[0013] Preferably, the pressure of the microwave heating treatment in step (2) is 140-160 PSI.

[0014] The present invention also provides solid-state fluorescent carbonized polymer dots prepared by the preparation method described in the above technical solution.

[0015] The present invention also provides the use of the solid-state fluorescent carbonized polymer dots described in the above technical solution in the preparation of luminescent materials, biomedicine, optoelectronic devices and sensors.

[0016] Preferably, the luminescent material comprises a carbonized polymer dot-boron oxide composite material or a carbonized polymer dot-polymer composite film.

[0017] The present invention provides a method for preparing solid-state fluorescent carbonized polymer dots, comprising the following steps: (1) mixing polyethyleneimine, a small molecule acid, and water to obtain a mixed solution; the small molecule acid comprises one or more of citric acid, tartaric acid, EDTA, sulfuric acid, acetic acid, and phosphoric acid; and (2) subjecting the mixed solution obtained in step (1) to microwave heating and drying to obtain solid-state fluorescent carbonized polymer dots. The present invention uses polyethyleneimine as a carbon source and adds a small molecule acid as an auxiliary agent, and microwave heating is performed to obtain solid-state fluorescent carbonized polymer dots. The amino groups of the polyethyleneimine and the small molecule acid undergo oxidative cross-linking to form molecular fluorescent centers. During the rapid microwave heating process, the fluorescent centers adhere and disperse on the polymer chains, avoiding fluorescence quenching due to aggregation, thereby making the prepared solid-state fluorescent carbonized polymer dots fluorescent. The results of the examples show that the solid-state carbonized polymer dots prepared by the present invention exhibit blue or green fluorescence emission under ultraviolet light. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Fluorescence spectra of an aqueous solution of solid-state fluorescent carbonized polymer dots prepared in Example 1 and an aqueous solution of carbon dots prepared in Comparative Example 1;

[0019] Figure 2 Fluorescence spectra of aqueous solutions of solid-state fluorescent carbonized polymer dots prepared in Examples 1 to 4;

[0020] Figure 3 Fluorescence spectra of aqueous solutions of solid-state fluorescent carbonized polymer dots prepared in Examples 5 to 9;

[0021] Figure 4Fluorescence spectra of aqueous solutions of solid-state fluorescent carbonized polymer dots prepared in Examples 6 and 10-12;

[0022] Figure 5 Fluorescence spectra of aqueous solutions of solid-state fluorescent carbonized polymer dots prepared in Examples 1 and 13 to 18;

[0023] Figure 6 Fluorescence spectra of aqueous solutions of solid-state fluorescent carbonized polymer dots prepared in Examples 19 to 25;

[0024] Figure 7 Fluorescence spectra of solid-state fluorescent carbonized polymer dots prepared in Example 6, Example 26, and Examples 31 to 34;

[0025] Figure 8 These are pictures of the solid-state fluorescent carbonized polymer dots prepared in Examples 6, 26, and 31 to 34 under sunlight and ultraviolet light;

[0026] Figure 9 These are pictures of the solid-state fluorescent carbonized polymer dots prepared in Example 6 and Examples 27 to 30 under sunlight and ultraviolet light;

[0027] Figure 10 Fluorescence spectra of solid-state fluorescent carbonized polymer dots prepared in Examples 6 and 28 to 30;

[0028] Figure 11 This is a fluorescence spectrum of an aqueous solution of solid-state fluorescent carbonized polymer dots prepared in Example 6;

[0029] Figure 12 The differential scanning calorimetry curves of the solid-state fluorescent carbonized polymer dots prepared in Examples 6 and 26 to 28 are shown;

[0030] Figure 13 This is a transmission scanning electron micrograph of the solid-state fluorescent carbonized polymer dots prepared in Example 6;

[0031] Figure 14 This is the particle size distribution diagram of the solid-state fluorescent carbonized polymer dots prepared in Example 6;

[0032] Figure 15 Fluorescence spectra of an aqueous solution of solid-state fluorescent carbonized polymer dots prepared in Example 6 at different excitation wavelengths;

[0033] Figure 16 The emission wavelength and fluorescence intensity change curves of the aqueous solution of solid-state fluorescent carbonized polymer dots prepared in Example 6 after irradiation at 365 nm for different time periods;

[0034] Figure 17 Fluorescence spectra of an aqueous solution of solid-state fluorescent carbonized polymer dots prepared in Example 6 under different pH conditions;

[0035] Figure 18 This is a curve showing the change in emission wavelength and intensity of an aqueous solution of solid-state fluorescent carbonized polymer dots prepared in Example 6 under different pH conditions;

[0036] Figure 19 The fluorescence spectra of the carbonized polymer dot-polymer composite films prepared in Application Examples 1 to 5 are shown;

[0037] Figure 20 Fluorescence photographs of carbonized polymer dot-polymer composite films prepared in Application Examples 1 to 5 under sunlight and 365 nm ultraviolet light;

[0038] Figure 21 These are photos of the carbonized polymer dot-polymer composite film prepared in Application Example 4 under sunlight and 365nm UV light;

[0039] Figure 22 This is an afterglow image of the amorphous glassy carbonized polymer dot boron oxide composite powder obtained in Application Example 6, irradiated under a 365nm UV lamp for 2 minutes, and then turned off the light at 0 seconds;

[0040] Figure 23 The amorphous glassy carbonized polymer dot boron oxide composite powder obtained in Application Example 6 was irradiated with sunlight, 254nm and 365nm UV lamps for 2 seconds, and then the afterglow images were taken at different light-off times after the light was turned off.

[0041] Figure 24 The phosphorescence spectra of the amorphous glassy carbonized polymer dot boron oxide composite materials in Application Examples 6 to 10 are shown;

[0042] Figure 25 The phosphorescence spectra of the amorphous glassy carbonized polymer dot boron oxide composite materials in Application Examples 6 and 11-14 are shown;

[0043] Figure 26 The phosphorescence spectra of the amorphous glassy carbonized polymer dot boron oxide composite materials in Application Examples 6 and 15-18 are shown. DETAILED DESCRIPTION

[0044] The present invention provides a method for preparing solid-state fluorescent carbonized polymer dots, comprising the following steps:

[0045] (1) mixing polyethyleneimine, a small molecule acid, and water to obtain a mixed solution; the small molecule acid comprises one or more of citric acid, tartaric acid, EDTA, sulfuric acid, acetic acid, and phosphoric acid;

[0046] (2) The mixed solution obtained in step (1) is subjected to microwave heating treatment and then dried to obtain solid-state fluorescent carbonized polymer dots.

[0047] Unless otherwise specified, the present invention has no particular limitation on the sources of the raw materials, and commercially available products known to those skilled in the art may be used.

[0048] The invention mixes polyethyleneimine, small molecule acid and water to obtain a mixed solution.

[0049] In the present invention, the weight-average molecular weight of the polyethyleneimine is preferably 600 to 70,000. In one embodiment, the weight-average molecular weight of the polyethyleneimine can be 600, 1,800, 10,000, or 70,000. By controlling the weight-average molecular weight of the polyethyleneimine within the above range, the luminescence intensity of the solid-state fluorescent carbonized polymer dots can be further enhanced.

[0050] In the present invention, the small molecule acid includes one or more of citric acid, tartaric acid, EDTA, sulfuric acid, acetic acid and phosphoric acid.

[0051] In the present invention, the concentration of the phosphoric acid is preferably 0.2-0.3 mol / L, more preferably 0.24 mol / L; the concentration of the sulfuric acid is preferably 0.5-1.5 mol / L, more preferably 1 mol / L; the concentration of the acetic acid is preferably 17-18 mol / L, more preferably 17.5 mol / L.

[0052] In the present invention, when the small molecule acid is one or more of citric acid, tartaric acid, and EDTA, the mass ratio of the polyethyleneimine to the small molecule acid is preferably 1:(0.5-4). As an embodiment, the mass ratio of the polyethyleneimine to the small molecule acid can be specifically 1:0.5, 1:1, 1:2, 1:3, or 1:4.

[0053] In the present invention, when the small molecule acid is one or more of phosphoric acid, acetic acid, and sulfuric acid, the volume ratio of polyethyleneimine to the small molecule acid is preferably 1 g: (0.1-6) mL. By using these small molecule acids and controlling their dosage, the carbonized polymer dots prepared in the present invention retain fluorescence emission properties in the solid state, and exhibit higher luminescence intensity.

[0054] In the present invention, the water is preferably ultrapure water.

[0055] In the present invention, the mass ratio of the polyethyleneimine to the volume of water is preferably 1g:(15-50)mL. As an embodiment, the mass ratio of the polyethyleneimine to the volume of water can be specifically 1g:15mL, 1g:16mL, 1g:18mL, 1g:20mL, 1g:25mL, 1g:30mL, 1g:35mL, 1g:40mL, 1g:45mL or 1g:50mL. In the present invention, the mass ratio of the polyethyleneimine to the volume of water is controlled within the above range, so that the raw materials can be fully dissolved.

[0056] The present invention does not specifically limit the mixing process of the polyethyleneimine, small molecule acid, and water; a mixing technique well known to those skilled in the art may be employed to ensure uniform mixing of the raw materials. In one embodiment, the mixing is performed under ultrasonic conditions. The present invention does not specifically limit the power or duration of the ultrasonication; the raw materials may be fully dissolved and uniformly mixed.

[0057] In the present invention, the pH value of the mixed solution is preferably 0 to 9. As an embodiment, the pH value of the mixed solution can be specifically 0, 1, 2, 3, 4, 5, 6, 7, 8 or 9. By controlling the pH value of the mixed solution within the above range, the luminescence intensity of the solid-state fluorescent carbonized polymer dots can be further improved.

[0058] When the pH of the mixed solution is outside the above range, the present invention preferably adds an acid and / or base to adjust the pH of the mixed solution. In one embodiment, the acid is hydrochloric acid, and the base is aqueous sodium hydroxide solution. The present invention does not specifically limit the concentration and amount of the acid and base, as long as the pH of the mixed solution is within the desired range.

[0059] After obtaining the mixed solution, the present invention performs microwave heating on the mixed solution and then dries it to obtain solid-state fluorescent carbonized polymer dots.

[0060] In the present invention, the power of the microwave heating treatment is preferably 80 to 800 W. As an embodiment, the power of the microwave heating treatment can be specifically 80 W, 100 W, 150 W, 200 W, 400 W, 500 W or 700 W.

[0061] In the present invention, the temperature of the microwave heating treatment is preferably 150-160° C. As an embodiment, the temperature of the microwave heating treatment can be specifically 150° C., 151° C., 152° C., 153° C., 154° C., 155° C., 156° C., 157° C., 158° C., 159° C. or 160° C.

[0062] In the present invention, the microwave heating time is preferably 1 to 10 minutes. As an embodiment, the microwave heating time can be specifically 1 minute, 1 minute 30 seconds (90 seconds), 1 minute 50 seconds (110 seconds), 2 minutes, 2 minutes 10 seconds (130 seconds), 2 minutes 20 seconds (140 seconds), 2 minutes 30 seconds (150 seconds), 2 minutes 40 seconds (160 seconds), 2 minutes 50 seconds (170 seconds), 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes.

[0063] In the present invention, the pressure of the microwave heating treatment is preferably 140-160 PSI. As an embodiment, the pressure of the microwave heating treatment can be specifically 140 PSI, 150 PSI or 160 PSI.

[0064] The present invention controls the parameters of the microwave heating process within the above ranges, which can further improve the luminescence intensity of the solid-state fluorescent carbonized polymer dots.

[0065] In one embodiment, the microwave heating treatment is performed in a microwave oven or under single-mode microwave heating conditions. The carbonized polymer dots prepared by microwave heating in the present invention exhibit fluorescent emission properties in the solid state and are prepared in a short time, enabling the rapid preparation of gram-level carbonized polymer dots in a short period of time.

[0066] The present invention has no particular limitation on the drying operation, and drying to a constant weight may be performed using a drying technique well known to those skilled in the art.

[0067] In one embodiment, the drying is vacuum drying at a temperature of 70° C. and for 24 hours. The present invention has no particular limitation on the vacuum degree of the vacuum drying, and any vacuum degree familiar to those skilled in the art can be used.

[0068] After drying, the dried product is preferably ground to obtain solid-state fluorescent carbonized polymer dots.

[0069] The present invention has no particular limitation on the grinding operation, and the powder can be obtained by using a grinding technique well known to those skilled in the art.

[0070] The present invention uses polyethyleneimine as a carbon source, adds a small molecule acid as an auxiliary agent, and obtains solid carbonized polymer dots through microwave heating. The prepared solid carbonized polymer dots have fluorescence emission properties. At the same time, various process parameters are controlled to improve the luminescence intensity of the solid carbonized polymer dots.

[0071] The present invention also provides solid-state fluorescent carbonized polymer dots prepared by the preparation method described in the above technical solution.

[0072] In the present invention, when the small molecule acid is citric acid, the prepared solid-state fluorescent carbonized polymer dots have a glass transition temperature of 7.07°C, are soluble in water, insoluble in DMF and ethyl acetate, have a positive surface charge, a zeta potential of 22.5 mV, a hydrated particle size of 59.16 nm in aqueous solution, and are spherically dispersed with an average particle size of 6.20 nm. When excited at a wavelength of 320 nm, the carbonized polymer dot aqueous solution has a blue-green fluorescence emission signal at 450 nm, a Stokes shift of up to 130 nm, and a fluorescence quantum yield of 18.84%. The carbonized polymer dot solid has an obvious fluorescence emission signal at 462 nm.

[0073] The solid-state fluorescent carbonized polymer dots prepared by the present invention have stable luminescence performance, both fluorescent and phosphorescent properties, and good excitation wavelength independence and spectral stability.

[0074] The present invention also provides the use of the solid-state fluorescent carbonized polymer dots described in the above technical solution in the preparation of luminescent materials, biomedicine, optoelectronic devices and sensors.

[0075] In the present invention, the luminescent material preferably includes a carbonized polymer dot-boron oxide composite material or a carbonized polymer dot-polymer composite film.

[0076] The present invention has no particular limitation on the preparation method of the carbonized polymer dot-boron oxide composite material or the carbonized polymer dot-polymer composite film, and the technical solutions well known to those skilled in the art can be used.

[0077] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the embodiments described are only some of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0078] Example 1

[0079] A method for preparing solid-state fluorescent carbonized polymer dots comprises the following steps: (1) mixing 0.5 g of polyethyleneimine (weight-average molecular weight 70,000), 0.5 g of citric acid, and 10 mL of ultrapure water (the mass ratio of polyethyleneimine to citric acid is 1:1, and the volume ratio of polyethyleneimine to water is 1 g:20 mL), ultrasonically dissolving the mixture until the mixture is completely dissolved, and adjusting the pH to 5 to obtain a mixed solution;

[0080] (2) The mixed solution in step (1) was transferred and sealed in a quartz beaker, placed in a 700 W microwave oven, and heated in a single mode for 150 s at a temperature of 155° C. and a pressure of 150 PSI. After the reaction was completed, the mixture was vacuum dried at 70° C. for 24 h, cooled, and ground to obtain solid-state fluorescent carbonized polymer dots.

[0081] Comparative Example 1

[0082] A method for preparing a carbon dot solution is as follows: (1) 0.5 g of polyethyleneimine (weight average molecular weight 70,000), 0.5 g of citric acid, and 10 mL of ultrapure water are mixed (the mass ratio of polyethyleneimine to citric acid is 1:1, and the mass ratio of polyethyleneimine to water is 1 g:20 mL), ultrasonically treated until completely dissolved, and then the pH value is adjusted to 5 to obtain a mixed solution;

[0083] (2) The mixed solution in step (1) was transferred to a polytetrafluoroethylene-lined autoclave, subjected to a hydrothermal reaction at 180° C. for 4 h, and naturally cooled to room temperature. The product was filtered through a 0.22 μm microporous membrane to obtain a yellow, clear carbon dot solution.

[0084] 0.01 g of the solid-state fluorescent carbonized polymer dots prepared in Example 1 was diluted to 10 mL with ultrapure water, and 1 mL was taken to dilute 100 times and scan the fluorescence spectrum. After the carbon dot solution prepared in Comparative Example 1 was dried, 0.01 g was taken to dilute to 10 mL with ultrapure water, and 1 mL was taken to dilute 100 times and scan the fluorescence spectrum. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that the luminescence intensity of carbonized polymer dots synthesized by microwave is significantly higher than that of carbon dots synthesized by hydrothermal method.

[0085] Example 2

[0086] The weight average molecular weight of polyethyleneimine in step (1) of Example 1 was replaced with 600, and the other parameters were the same as those in Example 1.

[0087] Example 3

[0088] The weight average molecular weight of polyethyleneimine in step (1) of Example 1 was replaced by 1800, and the other parameters were the same as those in Example 1.

[0089] Example 4

[0090] The weight average molecular weight of polyethyleneimine in step (1) of Example 1 was replaced by 10,000, and the other parameters were the same as those in Example 1.

[0091] 0.01 g of solid-state fluorescent carbonized polymer dots prepared in Examples 1 to 4 were diluted to 10 mL with ultrapure water, and 1 mL was taken to dilute 100 times and then scanned for fluorescence spectra. The results were as follows: Figure 2 As shown. Figure 2 It can be seen that when the weight-average molecular weight of polyethyleneimine is 70,000, the excitation emission spectrum shows good mirror symmetry and the luminescence performance is stable. When the weight-average molecular weight of polyethyleneimine is 600, 1800 or 10,000, the excitation spectrum shows a double peak, indicating that the structure of the formed carbonized polymer dots may be unstable. The optimal weight-average molecular weight of polyethyleneimine is 70,000.

[0092] Example 5

[0093] A method for preparing solid-state fluorescent carbonized polymer dots is as follows: (1) 1 g of polyethyleneimine (weight-average molecular weight 70,000), 0.5 g of citric acid, and 20 mL of ultrapure water are mixed (the mass ratio of polyethyleneimine to citric acid is 2:1, and the volume ratio of polyethyleneimine to water is 1 g:20 mL), ultrasonically dissolved until completely dissolved, and then the pH value is adjusted to 5 to obtain a mixed solution;

[0094] (2) The mixed solution in step (1) was transferred and sealed in a quartz beaker, placed in a 700 W microwave oven, and heated in a single mode for 150 s at a temperature of 155° C. and a pressure of 150 PSI. After the reaction was completed, the mixture was vacuum dried at 70° C. for 24 h, cooled, and ground to obtain solid-state fluorescent carbonized polymer dots.

[0095] Example 6

[0096] The amount of citric acid in step (1) of Example 5 was replaced with 1 g. At this time, the mass ratio of polyethyleneimine to citric acid was 1:1. Other parameters were the same as those in Example 5.

[0097] Example 7

[0098] The amount of citric acid in step (1) of Example 5 was replaced with 2 g. At this time, the mass ratio of polyethyleneimine to citric acid was 1:2. Other parameters were the same as those in Example 5.

[0099] Example 8

[0100] The amount of citric acid in step (1) of Example 5 was replaced with 3 g. At this time, the mass ratio of polyethyleneimine to citric acid was 1:3. Other parameters were the same as those in Example 5.

[0101] Example 9

[0102] The amount of citric acid in step (1) of Example 5 was replaced with 4 g. At this time, the mass ratio of polyethyleneimine to citric acid was 1:4. Other parameters were the same as those in Example 5.

[0103] 0.01 g of solid-state fluorescent carbonized polymer dots prepared in Examples 5 to 9 were diluted to 10 mL with ultrapure water, and 1 mL was taken to dilute 100 times and then scanned for fluorescence spectra. The results were as follows: Figure 3 As shown. Figure 3 It can be seen that when the dosage of citric acid is 1 g, that is, the mass ratio of polyethyleneimine to citric acid is 1:1, the luminescence intensity is the highest.

[0104] Example 10

[0105] The pH value of the mixed solution in step (1) of Example 6 was replaced with 3, and the other parameters were the same as those in Example 6.

[0106] Example 11

[0107] The pH value of the mixed solution in step (1) of Example 6 was replaced with 7, and the other parameters were the same as those in Example 6.

[0108] Example 12

[0109] The pH value of the mixed solution in step (1) of Example 6 was replaced with 9, and the other parameters were the same as those in Example 6.

[0110] 0.01 g of solid-state fluorescent carbonized polymer dots prepared in Examples 6 and 10 to 12 were diluted to 10 mL with ultrapure water, and 1 mL was taken to dilute 100 times and then scanned for fluorescence spectra. The results were as follows: Figure 4 As shown. Figure 4 It can be seen that the luminescence intensity is highest when the pH value of the mixed solution is 5.

[0111] Example 13

[0112] The microwave heating time in step (2) of Example 1 was replaced with 90 s, and the other parameters were the same as those in Example 1.

[0113] Example 14

[0114] The microwave heating time in step (2) of Example 1 was replaced with 110 s, and the other parameters were the same as those in Example 1.

[0115] Example 15

[0116] The microwave heating time in step (2) of Example 1 was replaced with 130 s, and the other parameters were the same as those in Example 1.

[0117] Example 16

[0118] The microwave heating time in step (2) of Example 1 was replaced with 140 s, and the other parameters were the same as those in Example 1.

[0119] Example 17

[0120] The microwave heating time in step (2) of Example 1 was replaced with 160 s, and the other parameters were the same as those in Example 1.

[0121] Example 18

[0122] The microwave heating time in step (2) of Example 1 was replaced with 170 s, and the other parameters were the same as those in Example 1.

[0123] 0.01 g of solid-state fluorescent carbonized polymer dots prepared in Examples 1 and 13 to 18 were diluted to 10 mL with ultrapure water, and 1 mL was taken to dilute 100 times and then scanned for fluorescence spectra. The results were as follows: Figure 5 As shown. Figure 5 It can be seen from the figure that when the microwave power is 700W and the microwave heating time is 150s, the luminous intensity is the highest.

[0124] Example 19

[0125] A method for preparing solid-state fluorescent carbonized polymer dots comprises the following steps: (1) mixing 0.5 g of polyethyleneimine (weight-average molecular weight 70,000), 0.5 g of citric acid, and 10 mL of ultrapure water (the mass ratio of polyethyleneimine to citric acid is 1:1, and the volume ratio of polyethyleneimine to water is 1 g:20 mL), ultrasonically dissolving the mixture until the mixture is completely dissolved, and adjusting the pH to 5 to obtain a mixed solution;

[0126] (2) The mixed solution in step (1) was transferred and sealed in a quartz beaker, placed in a 200 W microwave oven, and heated in a single mode for 8 min at a temperature of 155° C. and a pressure of 150 PSI. After the reaction was completed, the mixture was vacuum dried at 70° C. for 24 h, cooled, and ground to obtain solid-state fluorescent carbonized polymer dots.

[0127] Example 20

[0128] The microwave heating time in step (2) of Example 19 was replaced with 4 min, and the other parameters were the same as those in Example 19.

[0129] Example 21

[0130] The microwave heating time in step (2) of Example 19 was replaced with 5 min, and the other parameters were the same as those in Example 19.

[0131] Example 22

[0132] The microwave heating time in step (2) of Example 19 was replaced with 6 min, and the other parameters were the same as those in Example 19.

[0133] Example 23

[0134] The microwave heating time in step (2) of Example 19 was replaced with 7 min, and the other parameters were the same as those in Example 19.

[0135] Example 24

[0136] The microwave heating time in step (2) of Example 19 was replaced with 9 min, and the other parameters were the same as those in Example 19.

[0137] Example 25

[0138] The microwave heating time in step (2) of Example 19 was replaced with 10 min, and the other parameters were the same as those in Example 19.

[0139] 0.01 g of solid-state fluorescent carbonized polymer dots prepared in Examples 19 to 25 were diluted to 10 mL with ultrapure water, and 1 mL was taken to dilute 100 times and then scanned for fluorescence spectra. The results were as follows: Figure 6 As shown. Figure 6 It can be seen that when the microwave power is 200W and the microwave heating time is 8min, the luminous intensity is the highest.

[0140] Example 26

[0141] The citric acid in step (1) of Example 6 was replaced by tartaric acid, and the other parameters were the same as those of Example 6.

[0142] Example 27

[0143] The citric acid in step (1) of Example 6 was replaced by EDTA (ethylenediaminetetraacetic acid), and the other parameters were the same as those in Example 6.

[0144] Example 28

[0145] A method for preparing solid-state fluorescent carbonized polymer dots comprises the following steps: (1) mixing 1 g of polyethyleneimine (weight-average molecular weight 70,000) with 15 mL of ultrapure water (the mass ratio of polyethyleneimine to water is 1 g:15 mL), ultrasonicating the mixture until completely dissolved, and then adding 5 mL of 0.24 mol / L phosphoric acid (the mass ratio of polyethyleneimine to phosphoric acid is 1 g:5 mL) to obtain a mixed solution;

[0146] (2) The mixed solution in step (1) was transferred and sealed in a quartz beaker, placed in a 700 W microwave oven, and heated in a single mode for 150 s at a temperature of 155° C. and a pressure of 150 PSI. After the reaction was completed, the mixture was vacuum dried at 70° C. for 24 h, cooled, and ground to obtain solid-state fluorescent carbonized polymer dots.

[0147] Example 29

[0148] A method for preparing solid-state fluorescent carbonized polymer dots comprises the following steps: (1) mixing 1 g of polyethyleneimine (weight-average molecular weight 70,000) with 15 mL of ultrapure water (the mass ratio of polyethyleneimine to water is 1 g:15 mL), ultrasonicating the mixture until completely dissolved, and then adding 5 mL of 1 mol / L sulfuric acid (the mass ratio of polyethyleneimine to sulfuric acid is 1 g:5 mL) to obtain a mixed solution;

[0149] (2) The mixed solution in step (1) was transferred and sealed in a quartz beaker, placed in a 700 W microwave oven, and heated in a single mode for 150 s at a temperature of 155° C. and a pressure of 150 PSI. After the reaction was completed, the mixture was vacuum dried at 70° C. for 24 h, cooled, and ground to obtain solid-state fluorescent carbonized polymer dots.

[0150] Example 30

[0151] A method for preparing solid-state fluorescent carbonized polymer dots comprises the following steps: (1) mixing 1 g of polyethyleneimine (weight-average molecular weight 70,000) with 15 mL of ultrapure water (the mass ratio of polyethyleneimine to water is 1 g:15 mL), ultrasonicating the mixture until completely dissolved, and then adding 0.298 mL of 17.5 mol / L acetic acid (the mass ratio of polyethyleneimine to acetic acid is 1 g:0.298 mL) to obtain a mixed solution;

[0152] (2) The mixed solution in step (1) was transferred and sealed in a quartz beaker, placed in a 700 W microwave oven, and heated in a single mode for 150 s at a temperature of 155° C. and a pressure of 150 PSI. After the reaction was completed, the mixture was vacuum dried at 70° C. for 24 h, cooled, and ground to obtain solid-state fluorescent carbonized polymer dots.

[0153] Example 31

[0154] The microwave power in step (2) of Example 6 was replaced with 200 W, and the microwave heating time was replaced with 8 min. Other parameters were the same as those in Example 6.

[0155] Example 32

[0156] The microwave power in step (2) of Example 26 was replaced with 200 W, and the microwave heating time was replaced with 8 min. Other parameters were the same as those in Example 26.

[0157] Example 33

[0158] The microwave power in step (2) of Example 27 was replaced with 200 W, and the microwave heating time was replaced with 8 min. Other parameters were the same as those in Example 27.

[0159] Example 34

[0160] The microwave power in step (2) of Example 28 was replaced with 200 W, and the microwave heating time was replaced with 8 min. Other parameters were the same as those in Example 28.

[0161] The solid-state fluorescent carbonized polymer dots prepared in Examples 6, 26, and 31 to 34 were scanned for fluorescence spectra. The results are as follows: Figure 7 shown. Figure 7 Among them, PEI-CAH SSE represents Example 6, PEI-CA SSE represents Example 31, PEI-TAH SSE represents Example 26, PEI-TA SSE represents Example 32, PEI-EDTA SSE represents Example 33, and PEI-PASSE represents Example 34.

[0162] The solid-state fluorescent carbonized polymer dots prepared in Examples 6, 26, and 31 to 34 were photographed under sunlight and ultraviolet light. The results are as follows: Figure 8 shown. Figure 8 From left to right are Example 6, Example 26, Example 32, Example 31, Example 33, and Example 34. Figures 7-8 It can be seen that the solid-state carbonized polymer dots all have solid-state fluorescence excitation emission signals, showing different fluorescence emission phenomena from blue to green. The solid-state fluorescent carbonized polymer dots synthesized using high microwave power (700W) have stronger luminescence performance than the solid-state fluorescent carbonized polymer dots synthesized using low power (200W).

[0163] The solid-state fluorescent carbonized polymer dots prepared in Example 6 and Examples 27 to 30 were photographed under sunlight and ultraviolet light. The results are as follows: Figure 9 shown. Figure 9 From left to right are Example 6, Examples 37 to 30. Figure 9 It can be seen from the figure that all solid-state carbonized polymer dots have solid-state fluorescence excitation emission signals.

[0164] The solid-state fluorescent carbonized polymer dots prepared in Examples 6 and 28 to 30 were scanned for fluorescence spectra. The results are as follows: Figure 10 shown. Figure 10 Among them, PEI-CA SSE represents Example 6, PEI-sulfuric acid SSE represents Example 29, PEI-phosphoric acid SSE represents Example 28, and PEI-acetic acid SSE represents Example 30. Figure 10 It can be seen that the carbonized polymer dot solid powder has obvious fluorescence emission at 430-450nm under the excitation of 360nm wavelength light source, and the fluorescence spectrum shows good mirror symmetry.

[0165] The solid-state fluorescent carbonized polymer dots prepared in Example 6 were dissolved in purified water to obtain a 1 g / L solution. The solution was diluted 100 times with ultrapure water and then scanned for fluorescence spectra. The solution was photographed under sunlight and 365 nm ultraviolet light. The results are shown in FIG. Figure 11 As shown. Figure 11 It can be seen that the solid-state fluorescent carbonized polymer dot aqueous solution has a stable blue fluorescence emission signal at 450nm under the excitation of 320nm wavelength.

[0166] The solid-state fluorescent carbonized polymer dots prepared in Examples 6 and 26-28 were dried at 80° C. in vacuum for 24 h, and then measured using a differential scanning calorimeter (TA Discovery DSC 25, USA). The results are shown in FIG. Figure 12 As shown, PEI-TA represents Example 26, PEI-EDTA represents Example 27, PEI-PA represents Example 28, and PEI-CA represents Example 6. Figure 12 It can be seen from the figure that the glass transition temperatures of solid-state fluorescent carbonized polymer dots are significantly different, and PEI-CA has the lowest transition temperature, which is significantly lower than room temperature.

[0167] The solid-state fluorescent carbonized polymer dots prepared in Example 6 were prepared into a 1 g / L aqueous solution, and then dialyzed for 1 day using a dialysis bag with a molecular weight of 500 Da. The solution was then dropped onto a copper mesh with a holey carbon film and allowed to dry naturally. The morphology and structure of the solution were characterized using a field emission transmission electron microscope. The transmission scanning electron microscope image obtained is shown in FIG. Figure 13 As shown in the particle size distribution diagram Figure 14 As shown. Figure 13 and 14 It can be seen that the solid-state fluorescent carbonized polymer dots in the solid-state fluorescent carbonized polymer dot aqueous solution prepared in Example 6 are uniform in size and highly dispersed, with an average particle size of 6.20±1.54 nm.

[0168] The hydrated particle size of the solid-state fluorescent carbonized polymer dots in the solid-state fluorescent carbonized polymer dot aqueous solution prepared in Example 6 obtained by laser particle size analyzer testing was 59.16 nm, and the zeta potential was 22.5 mV, indicating that the solid-state fluorescent carbonized polymer dots prepared in Example 6 had relatively stable hydrophilicity.

[0169] The solid-state fluorescent carbonized polymer dots prepared in Example 6 were dissolved in ultrapure water to prepare a 1 g / L aqueous solution. After diluting it 100 times with ultrapure water, the fluorescence spectrum was scanned. The fluorescence spectra at different excitation wavelengths (260 nm, 270 nm, 280 nm, 290 nm, 300 nm, 310 nm, 320 nm, 330 nm, 340 nm, and 350 nm) were as follows: Figure 15 As shown. Figure 15 It can be seen that the solid-state fluorescent carbonized polymer dot aqueous solution exhibits stable fluorescence emission under different excitation wavelengths, and the emission peak position falls at 450nm.

[0170] The solid-state fluorescent carbonized polymer dots prepared in Example 6 were dissolved in ultrapure water to prepare a 1 g / L aqueous solution, diluted 100 times with ultrapure water, and then irradiated at 365 nm. The optimal excitation wavelength and the optimal emission wavelength were scanned every 5 minutes for 1 hour. The emission wavelength and fluorescence intensity at different times were shown in FIG. Figure 16 As shown. Figure 16 It can be seen that the solid-state fluorescent carbonized polymer dot aqueous solution is resistant to photobleaching.

[0171] The solid-state fluorescent carbonized polymer dots prepared in Example 6 were dissolved in ultrapure water to prepare a 1 g / L aqueous solution. 400 μL of the solution was added to each of 12 10 mL centrifuge tubes. 1.2 mL of BR buffer with different pH values ​​(pH values ​​were 1.81, 2.87, 3.78, 4.78, 5.72, 6.80, 7.96, 8.95, 9.91, 10.88, and 11.82) was then added to each centrifuge tube. The fluorescence spectrum was scanned. The results are shown in FIG. Figure 17 As shown, Figure 17 The corresponding emission wavelength and intensity change curves are as follows Figure 18 As shown. Figure 17 and 18 It can be seen that with the increase of pH value, the fluorescence intensity remains basically unchanged, and the position of the fluorescence emission peak undergoes an obvious blue shift.

[0172] Application Example 1

[0173] Mix 6 mL of PVA (type 1795) aqueous solution (30 mg / mL) with 5 mL of solid-state fluorescent carbonized polymer dot aqueous solution (80 mg / mL) prepared in Example 6, make the volume to 15 mL with ultrapure water, and mix evenly under ultrasonication for 2 hours until the bubbles disappear. Pour the mixture onto a film-forming glass plate and prepare a film with a thickness of 0.1 mm using an adjustable film-forming device. Place the film-forming glass plate in an oven and dry it at 50°C for 2 hours, then cool it to form a carbonized polymer dot-polymer composite film.

[0174] Application Example 2

[0175] Mix 7 mL of PVA (type 1795) aqueous solution (30 mg / mL) with 5 mL of an aqueous solution of solid-state fluorescent carbonized polymer dots prepared in Example 6 (80 mg / mL), dilute to 15 mL with ultrapure water, and mix evenly under ultrasonication for 2 hours until the bubbles disappear. Pour the mixture onto a film-forming glass plate and prepare a film with a thickness of 0.1 mm using an adjustable film-forming device. Place the film-forming glass plate in an oven and dry it at 50°C for 2 hours, then cool it to form a carbonized polymer dot-polymer composite film.

[0176] Application Example 3

[0177] Mix 8 mL of PVA (type 1795) aqueous solution (30 mg / mL) with 5 mL of an aqueous solution of solid-state fluorescent carbonized polymer dots prepared in Example 6 (80 mg / mL), dilute to 15 mL with ultrapure water, and mix evenly under ultrasonication for 2 hours until the bubbles disappear. Pour the mixture onto a film-forming glass plate and prepare a film with a thickness of 0.1 mm using an adjustable film-forming device. Place the film-forming glass plate in an oven and dry it at 50°C for 2 hours, then cool it to form a carbonized polymer dot-polymer composite film.

[0178] Application Example 4

[0179] Mix 9 mL of PVA (type 1795) aqueous solution (30 mg / mL) with 5 mL of solid-state fluorescent carbonized polymer dot aqueous solution (80 mg / mL) prepared in Example 6, make the volume to 15 mL with ultrapure water, and mix evenly under ultrasonication for 2 hours until the bubbles disappear. Pour the mixture onto a film-forming glass plate and prepare a film with a thickness of 0.1 mm using an adjustable film-forming device. Place the film-forming glass plate in an oven and dry it at 50°C for 2 hours, then cool it to form a carbonized polymer dot-polymer composite film.

[0180] Application Example 5

[0181] Mix 10 mL of PVA (type 1795) aqueous solution (30 mg / mL) with 5 mL of solid-state fluorescent carbonized polymer dot aqueous solution (80 mg / mL) prepared in Example 6, mix evenly under ultrasonication for 2 hours until the bubbles disappear, pour it onto a film-forming glass plate, and use an adjustable film-forming device to prepare a film with a thickness of 0.1 mm. Place the film-forming glass plate in an oven and dry it at 50°C for 2 hours, then cool it to form a carbonized polymer dot-polymer composite film.

[0182] The fluorescence spectra of the carbonized polymer dot polymer composite films prepared in Application Examples 1 to 5 are shown in FIG. Figure 19 shown.

[0183] The carbonized polymer dot-polymer composite films prepared in Application Examples 1 to 5 were cut into 1.5*2 mm strips and fluorescent photographs were taken under sunlight and 365 nm UV light. The results are as follows: Figure 20As shown (from left to right are application examples 1 to 5). Figure 20 It can be seen that the carbonized polymer dot-polymer composite film shows blue fluorescence under ultraviolet light.

[0184] The photos of the carbonized polymer dot polymer composite film prepared in Application Example 4 under sunlight and 365nm ultraviolet light are as follows: Figure 21 shown.

[0185] The carbonized polymer dot-polymer composite film prepared in Application Example 4 has a maximum tensile stress of 15.9438 N, an elongation at break of 2.6359%, a tensile stress at break of 14.5312 N, and a tensile elastic modulus of 1636.9262 MPa.

[0186] Application Example 6

[0187] 2.0 g of boric acid was dissolved in 40 mL of ultrapure water, and then 2 mL of a 50 mg / mL aqueous solution of solid-state fluorescent carbonized polymer dots prepared in Example 6 was added. The mixture was ultrasonically mixed for 10 min, the mouth of the beaker was covered with aluminum foil, and the mixture was placed in an oven at 180°C and heated for 5 h. The mixture was naturally cooled to room temperature to obtain an amorphous glassy carbonized polymer dot boron oxide composite material.

[0188] The amorphous glassy carbonized polymer dot boron oxide composite material obtained in Application Example 6 was ground into powder and irradiated under a 365nm ultraviolet lamp for 2 minutes. The afterglow image at 0 seconds after the light was turned off was as shown in FIG. Figure 22 shown.

[0189] The amorphous glassy carbonized polymer dot boron oxide composite material obtained in Application Example 6 was ground into powder and irradiated under sunlight, 254nm and 365nm UV lamps for 2s respectively. After that, the light was turned off and afterglow pictures were taken at different light-off times. The results are as follows: Figure 23 As shown. Figure 23 It can be seen that the amorphous glassy carbonized polymer dot boron oxide composite material has a room temperature afterglow performance of up to 5s.

[0190] Application Example 7

[0191] The reaction temperature in Application Example 6 was replaced with 120° C., and the other parameters were the same as those in Application Example 6.

[0192] Application Example 8

[0193] The reaction temperature in Application Example 6 was replaced with 140° C., and the other parameters were the same as those in Application Example 6.

[0194] Application Example 9

[0195] The reaction temperature in Application Example 6 was replaced with 160° C., and the other parameters were the same as those in Application Example 6.

[0196] Application Example 10

[0197] The reaction temperature in Application Example 6 was replaced with 200° C., and the other parameters were the same as those in Application Example 6.

[0198] The phosphorescence spectra of the amorphous glassy carbonized polymer dot boron oxide composite materials in Application Examples 6 to 10 are shown in FIG. Figure 24 shown.

[0199] Application Example 11

[0200] The reaction time in Application Example 6 was replaced with 3 h, and the other parameters were the same as those in Application Example 6.

[0201] Application Example 12

[0202] The reaction time in Application Example 6 was replaced with 4 h, and the other parameters were the same as those in Application Example 6.

[0203] Application Example 13

[0204] The reaction time in Application Example 6 was replaced with 6 h, and the other parameters were the same as those in Application Example 6.

[0205] Application Example 14

[0206] The reaction time in Application Example 6 was replaced with 7 h, and the other parameters were the same as those in Application Example 6.

[0207] The phosphorescence spectra of the amorphous glassy carbonized polymer dot boron oxide composite materials in Application Examples 6, 11 to 14 are shown in FIG. Figure 25 shown.

[0208] Application Example 15

[0209] The amount of the aqueous solution of solid-state fluorescent carbonized polymer dots prepared in Example 6 in Application Example 6 was replaced with 0.5 mL, and the other parameters were the same as those in Application Example 6.

[0210] Application Example 16

[0211] The amount of the aqueous solution of solid-state fluorescent carbonized polymer dots prepared in Example 6 in Application Example 6 was replaced with 1.0 mL, and the other parameters were the same as those in Application Example 6.

[0212] Application Example 17

[0213] The amount of the aqueous solution of solid-state fluorescent carbonized polymer dots prepared in Example 6 in Application Example 6 was replaced with 3.0 mL, and the other parameters were the same as those in Application Example 6.

[0214] Application Example 18

[0215] The amount of the aqueous solution of solid-state fluorescent carbonized polymer dots prepared in Example 6 in Application Example 6 was replaced with 4.0 mL, and the other parameters were the same as those in Application Example 6.

[0216] The phosphorescence spectra of the amorphous glassy carbonized polymer dot boron oxide composite materials in Application Examples 6, 15-18 are shown in FIG. Figure 26 shown.

[0217] from Figures 22-26 It can be seen that when the amount of the solid-state fluorescent carbonized polymer dot aqueous solution is 2 mL, the reaction temperature is 180°C, and the reaction time is 5 h, the amorphous glassy carbonized polymer dot boron oxide composite material has the best phosphorescence performance.

[0218] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for preparing solid-state fluorescent carbonized polymer dots, comprising the following steps: (1) mixing polyethyleneimine, a small molecule acid, and water to obtain a mixed solution; the small molecule acid comprises one or more of citric acid, tartaric acid, EDTA, sulfuric acid, acetic acid, and phosphoric acid; (2) The mixed solution obtained in step (1) is subjected to microwave heating treatment and then dried to obtain solid-state fluorescent carbonized polymer dots.

2. The preparation method according to claim 1, characterized in that The weight average molecular weight of the polyethyleneimine in the step (1) is 600 to 70,000.

3. The preparation method according to claim 1, characterized in that In the step (1), when the small molecule acid is one or more of citric acid, tartaric acid and EDTA, the mass ratio of polyethyleneimine to the small molecule acid is 1:(0.5-4).

4. The preparation method according to claim 1, characterized in that In the step (1), the volume ratio of polyethyleneimine to water is 1 g: (15-50) mL.

5. The preparation method according to claim 1, characterized in that The pH value of the mixed solution in step (1) is 0-9.

6. The preparation method according to claim 1, characterized in that In the step (2), the power of the microwave heating treatment is 80 to 800 W, the temperature of the microwave heating treatment is 150 to 160° C., and the time of the microwave heating treatment is 1 to 10 minutes.

7. The preparation method according to claim 1 or 6, characterized in that The pressure of the microwave heating treatment in step (2) is 140-160 PSI.

8. Solid-state fluorescent carbonized polymer dots prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the solid-state fluorescent carbonized polymer dots according to claim 8 in the preparation of luminescent materials, biomedicine, optoelectronic devices and sensors.

10. The use according to claim 9, characterized in that The luminescent material includes a carbonized polymer dot-boron oxide composite material or a carbonized polymer dot-polymer composite film.