Manufacturing process of micro supercapacitor based on femtosecond laser 4D printing
By combining femtosecond laser 4D printing technology with multi-layer stacking and multi-path scanning, a porous structure is constructed and the deformed state is solidified, which solves the problems of insufficient precision and lack of material versatility in the manufacture of micro-supercapacitors and realizes high-performance and long-life micro-capacitors.
Patent Information
- Application Number
- CN202511273856.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-08
- Publication Date
- 2025-10-21
AI Technical Summary
Existing technologies make it difficult to simultaneously ensure high-precision microstructure processing and multifunctional integration in the manufacture of micro-supercapacitors, resulting in uneven electrode structure, affecting energy storage performance and cycle life.
Femtosecond laser 4D printing technology is combined with multi-layer stacking and multi-path scanning strategies to prepare a micro supercapacitor with an interdigitated electrode structure by constructing a porous structure in the composite material layer and using infrared laser to solidify the deformation state.
A high-precision micro-capacitor structure is achieved, which improves energy storage capacity and cycle stability, meeting the application requirements of miniaturization, high efficiency and long life.
Smart Images

Figure CN120824134A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of energy storage device manufacturing, and specifically to a manufacturing process of micro supercapacitors based on femtosecond laser 4D printing. Background Art
[0002] With the rapid development of portable electronic devices, wearable technology and the Internet of Things, the demand for miniaturized and high-performance energy storage devices is increasing. Supercapacitors have attracted widespread attention due to their high power density and long cycle life, and have gradually become an important direction in the field of micro-energy. Existing research mainly uses methods such as photolithography, electrodeposition and inkjet printing to manufacture micro supercapacitors, which can achieve miniaturization and diversification of devices to a certain extent. Femtosecond laser processing technology has demonstrated unique advantages in the field of micro-nano manufacturing due to its ultra-high temporal and spatial resolution, non-contact processing methods and wide material applicability. Femtosecond laser 4D printing technology introduces the time dimension on the basis of three-dimensional structure construction, which can achieve dynamic structural response and controllable deformation, providing a new solution for the preparation of high-performance and flexible micro supercapacitors.
[0003] However, existing research still has a core flaw, that is, it is difficult to simultaneously ensure high-precision microstructure processing and multifunctional integration during the manufacturing process. Traditional methods are often constrained by the contradiction between resolution and efficiency at the micron and nanoscale, resulting in uneven electrode structure, which in turn affects energy storage performance. When applied to flexible electronics or complex microsystems, the unevenness will amplify the performance differences of the device, resulting in insufficient specific capacitance and shortened cycle life. Although femtosecond laser 4D printing has the potential for high resolution and dynamic structural design, it has not yet made a complete breakthrough in material selection optimization, printing parameter stability, and deformation controllability, especially in the realization of integrated manufacturing of complex functional structures. Therefore, how to balance the precision of the micro-nanoscale and the complexity of device integration has become a key issue restricting the further development of micro supercapacitors. Summary of the Invention
[0004] In response to the shortcomings of the existing technology, the present invention provides a manufacturing process for micro supercapacitors based on femtosecond laser 4D printing. The technical problem to be solved by this invention is: how to use femtosecond laser 4D printing technology, combined with multi-layer stacking and multi-path scanning strategies, to solve the problems of insufficient precision, lack of material versatility and low processing efficiency in the manufacturing of micro supercapacitors.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions: A manufacturing process for micro supercapacitors based on femtosecond laser 4D printing, comprising: S1. Providing a substrate, wherein the substrate is glass, silicon wafer, polymer film or metal foil, pretreating the surface of the substrate, and coating the pretreated substrate with carbon quantum dots and shape memory epoxy resin to form a composite material layer; S2. Performing optofluidic printing on the composite material layer using femtosecond laser technology, wherein the optofluidic printing includes multi-layer stacking and relative rotation scanning, and wherein a multi-path scanning strategy is combined with the optofluidic printing process to construct a porous structure in the composite material layer; S3. The composite material layer is deformed by infrared laser irradiation, and the deformed state of the deformed composite material layer is fixed by cooling and curing; S4. Preparing an electrode material, preparing an electrode layer on the surface of the deformed composite material layer, wherein the electrode material is a polypyrrole and molybdenum disulfide heterojunction prepared by chemical vapor deposition; S5. Constructing an interdigitated electrode structure on the electrode layer to form a micro supercapacitor.
[0006] Preferably, the pretreatment includes plasma treatment, chemical etching and ultraviolet light irradiation, the content of the carbon quantum dots is 0.1wt%-0.3wt%, the particle size is 3nm-5nm, the mass percentage of the carbon quantum dots is 0.1%-0.3%, and the mass percentage of the shape memory epoxy resin is 99.9%-99.7%.
[0007] Preferably, the wavelength of the femtosecond laser technology is 1030 nm, the pulse width is 200 fs, and the power is 80 mW ± 5 mW. The photofluidic printing scanning speed is 10 mm / s ± 0.5 mm / s. The rotation angle of the relative rotation scanning is 67° ± 1°. The number of layers of the multi-layer stack is ≥ 10, and the thickness of each layer is 1 μm-2 μm.
[0008] Preferably, a UV pre-curing treatment is performed during the photofluidic printing process, and the UV pre-curing treatment has a pre-curing time of 5s-10s and a power of 10mW / cm²-20mW / cm².
[0009] Preferably, the infrared laser irradiation adopts a pulsed irradiation mode, and the pulsed irradiation mode has a wavelength of 808nm, a power of 1W-5W, and an irradiation time of 1s-10s.
[0010] Preferably, the molybdenum disulfide in the molybdenum disulfide heterojunction is 1T phase, the molybdenum disulfide content is ≥80wt%, the electrode layer thickness is 1μm-5μm, the reaction temperature of the chemical vapor deposition method is 500℃-800℃, the carrier gas is argon, and the gas flow rate is 50sccm-200sccm.
[0011] Preferably, the interdigitated electrode structure is arranged in a staggered manner, and the interdigitated width of the interdigitated electrode structure is 10 μm±0.5 μm and the spacing is 5 μm±0.2 μm.
[0012] Preferably, the size of the micro supercapacitor is ≤1 cm², the surface of the micro supercapacitor is covered with an encapsulation layer, the thickness of the encapsulation layer is 5 μm-20 μm, and the material of the encapsulation layer is polyimide, polyethylene terephthalate or polyurethane.
[0013] The present invention provides a manufacturing process for micro supercapacitors based on femtosecond laser 4D printing. It has the following beneficial effects: This femtosecond laser 4D printing micro-supercapacitor manufacturing process uses femtosecond laser technology combined with optofluidic printing and infrared laser irradiation to precisely construct a porous structure within the composite material layer. This process then uses infrared laser curing to fix the deformed state, providing a novel method for manufacturing micro-supercapacitors. This process can achieve high-precision micro-capacitor structures, effectively improving the capacitor's energy storage capacity and cycling stability.
[0014] The manufacturing process uses a variety of advanced technologies such as chemical vapor deposition, femtosecond laser printing and shape memory materials, which enables the micro-supercapacitor to have better morphological stability and efficient electrode structure while maintaining high performance. It can meet the application requirements of miniaturization, high efficiency and long life, and greatly improve the market application potential of micro-capacitors. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a general flow chart of the process for realizing the invention; Figure 2 is a flow chart of substrate preparation and coating treatment for implementing the invention; Figure 3 It is a femtosecond laser optofluidic printing flow chart for realizing the invention; Figure 4 It is a dynamic structure programming flow chart for implementing the invention; Figure 5 The present invention is a flow chart for preparing electrode materials. DETAILED DESCRIPTION
[0016] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0017] Example 1 like Figure 1-5 As shown, an embodiment of the present invention provides a manufacturing process for a micro supercapacitor based on femtosecond laser 4D printing, comprising: S1. Providing a substrate, which is glass, silicon wafer, polymer film or metal foil, pre-treating the surface of the substrate, and coating the pre-treated substrate with carbon quantum dots and shape memory epoxy resin to form a composite material layer. The pre-treatment includes plasma treatment, chemical etching and ultraviolet light irradiation. The carbon quantum dots have a content of 0.3wt%, a particle size of 5nm, a mass percentage of 0.3% for the carbon quantum dots, and a mass percentage of 99.7% for the shape memory epoxy resin.
[0018] S2. Optofluidic printing was performed on the composite material layer using femtosecond laser technology. Optofluidic printing included multi-layer stacking and relative rotational scanning. A multi-path scanning strategy was used during the optofluidic printing process to construct a porous structure within the composite material layer. The wavelength of the femtosecond laser technology was 1030 nm, the pulse width was 200 fs, and the power was 85 mW. The optofluidic printing scan speed was 10.5 mm / s, the relative rotational scanning angle was 68°, the number of layers in the multi-layer stack was ≥10, and the thickness of each layer was 2 μm. UV pre-curing was performed during the optofluidic printing process, with a pre-curing time of 10 seconds and a power of 20 mW / cm².
[0019] S3. Deform the composite material layer by infrared laser irradiation, and fix the deformed state by cooling and curing to obtain a deformed composite material layer. The infrared laser irradiation is performed in a pulsed manner, with a wavelength of 808 nm, a power of 5 W, and an irradiation time of 10 seconds.
[0020] S4. Prepare electrode materials and form an electrode layer on the surface of the deformable composite material layer. The electrode material is a polypyrrole and molybdenum disulfide heterojunction prepared by chemical vapor deposition. The molybdenum disulfide in the molybdenum disulfide heterojunction is in the 1T phase, with a molybdenum disulfide content of ≥80wt%. The electrode layer thickness is 5μm. The chemical vapor deposition reaction temperature is 800°C, the carrier gas is argon, and the gas flow rate is 200sccm.
[0021] S5. Construct an interdigitated electrode structure on the electrode layer to form a micro-supercapacitor. The interdigitated electrode structure is arranged in a staggered manner, with interdigits having a width of 10.5 μm and a pitch of 5.2 μm. The micro-supercapacitor has a size of ≤1 cm² and is covered with an encapsulation layer having a thickness of 20 μm and made of polyimide, polyethylene terephthalate, or polyurethane.
[0022] This embodiment achieves high capacitance performance and mechanical strength in a shorter time through higher laser power and faster printing speeds, while also improving production efficiency. However, higher laser power and material concentration may lead to the risk of overheating or over-processing, thereby affecting the integrity and performance of the material. Therefore, this embodiment is suitable for applications with high requirements for electrical performance and production efficiency, but strict parameter control is required during the production process to prevent material damage or performance degradation.
[0023] Example 2 An embodiment of the present invention provides a manufacturing process for a micro-supercapacitor based on femtosecond laser 4D printing, comprising: S1. Providing a substrate, which may be glass, a silicon wafer, a polymer film, or a metal foil; pretreating the surface of the substrate; and coating the pretreated substrate with carbon quantum dots and a shape-memory epoxy resin to form a composite material layer. The pretreatment includes plasma treatment, chemical etching, and ultraviolet light irradiation. The carbon quantum dots have a content of 0.2wt%, a particle size of 4nm, a mass percentage of 0.2%, and a mass percentage of 99.8%.
[0024] S2. Optofluidic printing was performed on the composite material layer using femtosecond laser technology. Optofluidic printing included multi-layer stacking and relative rotational scanning. A multi-path scanning strategy was used during the optofluidic printing process to construct a porous structure within the composite material layer. The wavelength of the femtosecond laser technology was 1030 nm, the pulse width was 200 fs, and the power was 80 mW. The optofluidic printing scan speed was 10 mm / s, the relative rotational scanning angle was 67°, the number of layers in the multi-layer stack was ≥10, and the thickness of each layer was 1.5 μm. UV pre-curing was performed during the optofluidic printing process, with a pre-curing time of 7.5 seconds and a power of 15 mW / cm².
[0025] S3. Deform the composite material layer using infrared laser irradiation, and fix the deformed state by cooling and curing to obtain a deformed composite material layer. The infrared laser irradiation is performed in a pulsed manner, with a wavelength of 808 nm, a power of 3 W, and an irradiation time of 5.5 seconds.
[0026] S4. Prepare electrode materials. Deposit an electrode layer on the surface of the deformable composite material layer. The electrode material is a polypyrrole and molybdenum disulfide heterojunction prepared by chemical vapor deposition. The molybdenum disulfide in the molybdenum disulfide heterojunction is in the 1T phase, with a molybdenum disulfide content ≥ 80 wt%. The electrode layer thickness is 3 μm. The chemical vapor deposition reaction temperature is 650°C, the carrier gas is argon, and the gas flow rate is 125 sccm.
[0027] S5. Construct an interdigitated electrode structure on the electrode layer to form a micro-supercapacitor. The interdigitated electrode structure is arranged in a staggered manner, with interdigits having a width of 10 μm and a pitch of 5 μm. The micro-supercapacitor has a size of ≤1 cm² and is covered with an encapsulation layer having a thickness of 12.5 μm and made of polyimide, polyethylene terephthalate, or polyurethane.
[0028] This embodiment achieves a good balance between performance and material stability through rational parameter settings. This provides strong stability and consistency, making it suitable for large-scale production. By avoiding extreme processing conditions, this embodiment effectively reduces the risk of material damage caused by excessive processing, making it suitable for applications requiring high product quality consistency and stability.
[0029] Example 3 An embodiment of the present invention provides a manufacturing process for a micro-supercapacitor based on femtosecond laser 4D printing, comprising: S1. Providing a substrate, the substrate being glass, silicon wafer, polymer film, or metal foil; pretreating the surface of the substrate; and coating the pretreated substrate with carbon quantum dots and shape memory epoxy resin to form a composite material layer. The pretreatment includes plasma treatment, chemical etching, and ultraviolet light irradiation. The carbon quantum dots have a content of 0.1 wt%, a particle size of 3 nm, a mass percentage of 0.1%, and a mass percentage of 99.9% of the shape memory epoxy resin.
[0030] S2. Optofluidic printing was performed on the composite material layer using femtosecond laser technology. Optofluidic printing included multi-layer stacking and relative rotational scanning. A multi-path scanning strategy was used during the printing process to construct a porous structure within the composite material layer. The femtosecond laser technology had a wavelength of 1030 nm, a pulse width of 200 fs, and a power of 75 mW. The optofluidic printing scan speed was 9.5 mm / s, and the relative rotational scanning angle was 66°. The multi-layer stack had ≥10 layers, each with a thickness of 1 μm. UV pre-curing was performed during the printing process, with a pre-curing time of 5 seconds and a power of 10 mW / cm².
[0031] S3. Deform the composite material layer by infrared laser irradiation, and fix the deformed state by cooling and curing to obtain a deformed composite material layer. The infrared laser irradiation is performed in a pulsed manner, with a wavelength of 808 nm, a power of 1 W, and an irradiation time of 1 second.
[0032] S4. Prepare electrode materials. Deposit an electrode layer on the surface of the deformable composite material layer. The electrode material is a polypyrrole and molybdenum disulfide heterojunction prepared by chemical vapor deposition. The molybdenum disulfide in the molybdenum disulfide heterojunction is in the 1T phase, with a molybdenum disulfide content ≥ 80 wt%. The electrode layer thickness is 1 μm. The chemical vapor deposition reaction temperature is 500°C, the carrier gas is argon, and the gas flow rate is 50 sccm.
[0033] S5. Construct an interdigitated electrode structure on the electrode layer to form a micro-supercapacitor. The interdigitated electrode structure is arranged in a staggered manner, with interdigits having a width of 9.5 μm and a pitch of 4.8 μm. The micro-supercapacitor has a size of ≤1 cm² and is covered with an encapsulation layer having a thickness of 5 μm and made of polyimide, polyethylene terephthalate, or polyurethane.
[0034] In summary, lower laser power and reduced material concentration ensure high material stability and reduce the risk of thermal damage and over-processing. However, the resulting low capacitance performance and slow production speed make it difficult to meet the requirements of applications with high performance and high production efficiency. This embodiment is suitable for applications with high requirements for material integrity and stability, but its performance in terms of electrical performance and production efficiency is relatively limited.
[0035] Example 4 This example is based on the manufacturing process of femtosecond laser 4D printing micro supercapacitors. By comparing the effects of different parameters on the performance of micro supercapacitors, the optimal process conditions are explored. The specific implementation is as follows: 1. Experiment A Substrate selection and pretreatment: Select glass substrates and perform plasma treatment, chemical etching, and UV irradiation to ensure the substrate surface is clean and enhance adhesion.
[0036] Composite coating: A composite material containing 0.3wt% carbon quantum dots (5nm in size) and shape memory epoxy resin was applied to the substrate surface. The mass percentage of carbon quantum dots was 0.3% and the mass percentage of epoxy resin was 99.7%.
[0037] Femtosecond laser optofluidic printing: Laser parameters: wavelength 1030 nm, pulse width 200 fs, power 80 mW, scanning speed 10 mm / s, rotation angle 67°.
[0038] Multilayer stacking technology is used, with each layer having a thickness of 2 μm and the number of stacked layers ≥ 10 to construct a porous structure.
[0039] During the printing process, UV pre-curing is performed with a pre-curing power of 20mW / cm² and a curing time of 10 seconds.
[0040] Infrared laser irradiation: The laser wavelength is 808nm, the power is 5W, the irradiation time is 10 seconds, and a pulsed irradiation method is used to cause the composite material layer to deform. The deformation state is fixed after cooling and solidification.
[0041] Electrode materials and preparation: Polypyrrole and molybdenum disulfide heterojunction materials are used, with a molybdenum disulfide content of ≥80wt% and a reaction temperature of 800°C. The electrode layer thickness is 5μm.
[0042] Interdigitated electrode structure and packaging: The interdigital width is 10μm, the spacing is 5μm, and they are staggered. The size of the micro supercapacitor is ≤1cm. 2 The thickness of the encapsulation layer is 20 μm, and the encapsulation material is polyimide.
[0043] 2. Experiment B Substrate selection and pretreatment: Silicon wafer substrates are selected, the surface is plasma treated, and then cleaned by UV irradiation.
[0044] Composite material coating: A composite material containing 0.2 wt% carbon quantum dots with a particle size of 4 nm and shape memory epoxy resin is coated on the substrate, with the mass percentage of carbon quantum dots being 0.2% and epoxy resin being 99.8%.
[0045] Femtosecond laser optofluidic printing: Laser parameters: wavelength 1030 nm, pulse width 200 fs, power 80 mW, scanning speed 10 mm / s, rotation angle 67°.
[0046] A multi-layer stacking technology is used, with each layer having a thickness of 1.5 μm and the number of stacked layers being ≥10, to construct a porous structure.
[0047] UV pre-curing is performed during the printing process, and the pre-curing power is 15mW / cm 2 , the curing time is 7 seconds.
[0048] Infrared laser irradiation: The laser wavelength is 808nm, the power is 3W, and the irradiation time is 7 seconds. Pulsed irradiation is used to deform the composite material layer, and the deformation state is fixed after cooling and solidification.
[0049] Electrode materials and preparation: A polypyrrole and molybdenum disulfide heterojunction material is used, with a molybdenum disulfide content of ≥80wt% and a reaction temperature of 650°C. The electrode layer thickness is 4μm.
[0050] Interdigitated electrode structure and packaging: The interdigital width is 10 μm, the spacing is 5 μm, and they are staggered. The thickness of the encapsulation layer is 15 μm, and the encapsulation material is polyethylene terephthalate.
[0051] 3. Experiment C Substrate selection and pretreatment: Select polymer film substrate, perform chemical etching, and use UV light irradiation for surface treatment.
[0052] Composite material coating: A composite material containing 0.1wt% carbon quantum dots with a particle size of 3nm and shape memory epoxy resin is coated on the substrate, with the mass percentage of carbon quantum dots being 0.1% and epoxy resin being 99.9%.
[0053] Femtosecond laser optofluidic printing: Laser parameters: wavelength 1030 nm, pulse width 200 fs, power 80 mW, scanning speed 10 mm / s, rotation angle 67°.
[0054] Multilayer stacking technology is used, with each layer having a thickness of 1 μm and the number of stacked layers ≥ 10 to construct a porous structure.
[0055] UV pre-curing is performed during the printing process, and the pre-curing power is 10mW / cm 2 , curing time is 5 seconds.
[0056] Infrared laser irradiation: The laser wavelength is 808nm, the power is 1W, and the irradiation time is 5 seconds. The composite material layer is deformed by pulsed irradiation, and the deformation state is fixed after cooling and solidification.
[0057] Electrode materials and preparation: Polypyrrole and molybdenum disulfide heterojunction materials are used, with a molybdenum disulfide content of ≥80wt% and a reaction temperature of 500°C. The electrode layer thickness is 1μm.
[0058] Interdigitated electrode structure and packaging: The interdigital width is 10μm, the spacing is 5μm, and they are staggered. The size of the micro supercapacitor is ≤1cm. 2 The thickness of the encapsulation layer is 5μm, and the encapsulation material is polyurethane.
[0059] Comparative analysis: Effect of carbon quantum dot content: Experiment A used a higher content of carbon quantum dots, which helped improve the conductivity and stability of the composite material, thereby enhancing the performance of the capacitor. In contrast, Experiment C used a lower content of carbon quantum dots, which is expected to have weaker conductivity and may affect the energy storage performance of the capacitor.
[0060] Laser printing layer thickness and number of stacked layers: In Experiment A, each layer was thicker, and the composite material was constructed by stacking more layers, which contributed to a higher porosity and potentially improved energy storage performance. Experiments B and C had layer thicknesses of 1.5 μm and 1 μm, respectively, with the same number of layers, which may have affected porosity and energy storage capacity.
[0061] Differences in infrared laser irradiation power: Experiment A used a 5W infrared laser power, which more effectively induced deformation and potentially achieved higher capacitive energy storage capacity, but excessive power could also cause overheating. Experiment C used a lower power of 1W, which may result in less effective deformation but reduces the risk of overheating.
[0062] Electrode material and reaction temperature: The higher reaction temperature used in Experiment A facilitated the crystallization of molybdenum disulfide and enhanced the conductivity of the electrode. The lower reaction temperature used in Experiment C may have affected the crystallization quality of the electrode material, thereby reducing the performance of the electrode.
[0063] Influence of encapsulation layer thickness: The thickness of the encapsulation layer is 20 μm, 15 μm, and 5 μm in experiments A, B, and C, respectively. A thicker encapsulation layer can provide better protection, but it may also increase the size of the capacitor and affect its response speed under high power operating conditions.
[0064] Through the above comparative experiments, it can be concluded that Experiment A has higher settings in carbon quantum dot content, laser power and number of stacking layers, and is expected to provide the best capacitor energy storage performance. However, excessively high parameters may bring the risk of thermal damage. Experiment B has achieved a better balance between performance and process cost, and is suitable for situations where there are certain performance requirements but cost control is more important. Experiment C, due to its lower carbon quantum dot content and infrared laser power, may result in relatively weak capacitor energy storage capacity, but its process is simple and the cost is low, which is suitable for application scenarios that require low cost and simple process.
[0065] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.
Claims
1. A manufacturing process for micro supercapacitors based on femtosecond laser 4D printing, characterized in that: include: S1. Providing a substrate, wherein the substrate is glass, silicon wafer, polymer film or metal foil, pretreating the surface of the substrate, and coating the pretreated substrate with carbon quantum dots and shape memory epoxy resin to form a composite material layer; S2. Performing optofluidic printing on the composite material layer using femtosecond laser technology, wherein the optofluidic printing includes multi-layer stacking and relative rotation scanning, and wherein a multi-path scanning strategy is combined with the optofluidic printing process to construct a porous structure in the composite material layer; S3. The composite material layer is deformed by infrared laser irradiation, and the deformed state of the deformed composite material layer is fixed by cooling and curing; S4. Preparing an electrode material, preparing an electrode layer on the surface of the deformed composite material layer, wherein the electrode material is a polypyrrole and molybdenum disulfide heterojunction prepared by chemical vapor deposition; S5. Constructing an interdigitated electrode structure on the electrode layer to form a micro supercapacitor.
2. The manufacturing process of a micro supercapacitor based on femtosecond laser 4D printing according to claim 1, characterized in that: The pretreatment includes plasma treatment, chemical etching and ultraviolet light irradiation. The content of the carbon quantum dots is 0.1wt%-0.3wt%, the particle size is 3nm-5nm, the mass percentage of the carbon quantum dots is 0.1%-0.3%, and the mass percentage of the shape memory epoxy resin is 99.9%-99.7%.
3. The manufacturing process of a micro supercapacitor based on femtosecond laser 4D printing according to claim 1, characterized in that: The wavelength of the femtosecond laser technology is 1030nm, the pulse width is 200fs, and the power is 80mW±5mW. The optical fluidic printing scanning speed is 10mm / s±0.5mm / s. The rotation angle of the relative rotation scanning is 67°±1°. The number of layers of the multi-layer stack is ≥10, and the thickness of each layer is 1μm-2μm.
4. The manufacturing process of a micro supercapacitor based on femtosecond laser 4D printing according to claim 1, characterized in that: During the photofluidic printing process, UV pre-curing treatment is performed, and the pre-curing time of the UV pre-curing treatment is 5s-10s and the power is 10mW / cm²-20mW / cm².
5. The manufacturing process of a micro supercapacitor based on femtosecond laser 4D printing according to claim 1, characterized in that: The infrared laser irradiation adopts a pulsed irradiation mode, wherein the wavelength of the pulsed irradiation mode is 808nm, the power is 1W-5W, and the irradiation time is 1s-10s.
6. The manufacturing process of a micro supercapacitor based on femtosecond laser 4D printing according to claim 1, characterized in that: The molybdenum disulfide in the molybdenum disulfide heterojunction is a 1T phase, the molybdenum disulfide content is ≥80wt%, the thickness of the electrode layer is 1μm-5μm, the reaction temperature of the chemical vapor deposition method is 500℃-800℃, the carrier gas is argon, and the gas flow rate is 50sccm-200sccm.
7. The manufacturing process of a micro supercapacitor based on femtosecond laser 4D printing according to claim 1, characterized in that: The interdigital electrode structure is arranged in a staggered manner. The interdigital width of the interdigital electrode structure is 10 μm±0.5 μm and the spacing is 5 μm±0.2 μm.
8. The manufacturing process of a micro supercapacitor based on femtosecond laser 4D printing according to claim 1, characterized in that: The size of the micro supercapacitor is ≤1cm², the surface of the micro supercapacitor is covered with an encapsulation layer, the thickness of the encapsulation layer is 5μm-20μm, and the material of the encapsulation layer is polyimide, polyethylene terephthalate or polyurethane.