Multi-element titanium-based oxynitride with tubular structure as well as preparation method and application of multi-element titanium-based oxynitride
By adding anhydrous ethanol to a multi-component titanium-based oxynitride precursor solution through electrospinning and heat treatment, a multi-component titanium-based oxynitride with a tubular structure was prepared, solving the problem of morphology control and improving photocatalytic performance.
Patent Information
- Application Number
- CN202511337601.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-18
- Publication Date
- 2025-12-26
AI Technical Summary
Existing technologies have difficulty effectively controlling the morphology of perovskite-type oxynitrides, which limits their performance in the field of photocatalysis.
Anhydrous ethanol was added to the electrospinning precursor solution of multi-component titanium-based oxynitrides using electrospinning technology, and combined with heat treatment process to prepare multi-component titanium-based oxynitride materials with tubular morphology. The micromorphology of the material was controlled by optimizing the content of anhydrous ethanol.
It significantly increases the specific surface area of multi-component titanium-based nitrogen oxides, increases the catalytic active sites and light absorption area, and reduces the carrier transport distance, thereby improving photocatalytic performance.
Smart Images

Figure CN121198336A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The application belongs to the technical field of photo(electro)catalytic materials, and particularly relates to a multi-element titanium-based oxynitride with a tubular structure and a preparation method and application thereof. BACKGROUND
[0002] Hydrogen energy is a clean and efficient energy source that does not produce greenhouse gases and has important strategic significance. Among the many methods of hydrogen production, using solar energy to perform photocatalytic decomposition of water to produce hydrogen is an ideal method. Compared with other methods, solar hydrogen production has significant advantages. Solar energy is renewable and abundant, and through semiconductor photocatalytic technology, solar energy can be used to perform photocatalytic decomposition of water to produce hydrogen, which is an ideal method. However, low-cost and efficient photocatalysts are needed to achieve this goal. Semiconductor materials are the key to semiconductor photocatalytic technology, and perovskite titanium-based oxynitride RTiO2N (=La, Ce, Pr, Nd) has an ideal energy band structure for solar water splitting (with a band gap of about 2.0 eV, and the valence band and conduction band positions are suitable for water splitting), which has attracted widespread attention.
[0003] Materials with tubular morphology have many unique advantages in the field of photocatalysis, which help to improve the performance of photocatalysts and promote the continuous development of this field. First, one of the characteristics of tubular morphology is multiple light scattering, which means that light can be reflected and scattered multiple times inside the tubular morphology, increasing the propagation path of light and facilitating the absorption and utilization of light. This multiple scattering effect improves the utilization efficiency of light energy by the photocatalyst, thereby enhancing the activity of the catalytic reaction. Second, the advantage of thin-walled tubular morphology is to reduce the transmission distance of carriers. In photocatalytic reactions, light energy excites carriers, and these carriers need to be transported in the catalyst and participate in the reaction. Thin-walled tubular morphology can separate carriers closer, reducing the possibility of recombination, thereby improving the effective use of carriers and increasing the reaction rate. In addition, tubular morphology has a high specific surface area, which means that there are more active sites in a unit volume. This provides a larger reaction interface for the photocatalyst, increasing the contact opportunities between reactants and catalysts, thereby improving the reaction rate and efficiency. Furthermore, tubular morphology has the ability to achieve spatial separation of redox reactions. In some photocatalytic reactions, oxidation and reduction reactions need to be carried out separately to avoid recombination reactions. Tubular morphology can provide different reaction spaces to enable oxidation and reduction reactions to be effectively separated and carried out, which helps to improve reaction selectivity and efficiency. In summary, materials with tubular morphology make full use of their multiple scattering, carrier separation, high specific surface area, and reaction space separation advantages, and have great potential in photocatalysis, which is expected to provide more efficient solutions for clean energy production and environmental protection.
[0004] Currently, perovskite oxynitrides are usually prepared by one-step and two-step methods. In the one-step method, metal elements are used as metal element sources, urea, melamine, etc. are used as nitrogen sources, or metal nitrides and metal oxides are directly mixed and then calcined under a protective atmosphere to obtain the oxynitride. In the two-step method, an oxide precursor containing multiple metal ions is prepared by solid-phase sintering, coprecipitation, hydrothermal method, sol-gel method, etc., and then an ammonolysis reaction is carried out in an ammonia atmosphere to obtain the oxynitride. However, during the preparation process, little attention is paid to the control of the material morphology, and the obtained oxynitride is usually in the form of nano- or micro-particles.
[0005] For example, the Chinese patent application with the publication number CN114835150A discloses a method for preparing LaTiO2N oxynitride using a single precursor. The method focuses on obtaining a double-metal element precursor with precise stoichiometric ratio by using the coprecipitation method, but cannot effectively control the material morphology. The Chinese patent with the publication number CN109331853B discloses a nitrogen oxide nanoparticle photocatalyst and its application. The method prepares a metal oxide precursor by coprecipitation, then calcines the metal oxide precursor to prepare a perovskite nitrogen oxide, and finally treats the perovskite nitrogen oxide with aqua regia to obtain nitrogen oxide nanoparticles. However, this method cannot further control the morphology of the nitrogen oxide, such as obtaining linear or tubular morphology. The Chinese patent with the publication number CN112371159B discloses the nitridation synthesis of a nitrogen oxide material SmTiO2N and its application in the field of photocatalysis. The method uses a composite metal alkali salt as a nitridation precursor to synthesize a perovskite structure nitrogen oxide material of samarium and titanium elements. The composite double-metal alkali salt used in this method synthesizes a new composition of SmTiO2N nitrogen oxide material for the first time. The SmTiO2N nanoparticles synthesized by this method have a porous structure, but the morphology of the oxynitride cannot be further regulated. SUMMARY
[0006] To overcome the above-mentioned shortcomings of the prior art, the purpose of the present application is to provide a multi-element titanium-based oxynitride with a tubular structure, a preparation method thereof, and an application thereof. Anhydrous ethanol is added to the electrospinning precursor solution of the multi-element titanium-based oxynitride by using the electrospinning technology, and a heat treatment process is combined to prepare a multi-element titanium-based nitrogen oxide material with a tubular morphology. The micro-morphology of the multi-element titanium-based nitrogen oxide is controlled by optimizing the content of anhydrous ethanol, and a tubular structure with a large specific surface area is finally obtained. This can increase the catalytic active sites on the surface of the material, increase the light absorption area, reduce the carrier transport distance, and thus improve the photocatalytic performance of the material.
[0007] To achieve the above-mentioned purpose, the technical scheme adopted by the present application is as follows:
[0008] A method for preparing a multi-element titanium-based oxynitride with a tubular structure, comprising the following steps:
[0009] Step 1, configuring an electrostatic spinning precursor solution of a multi-element titanium-based oxynitride RTiO2N (R = La, Ce, Pr, Nd);
[0010] Tetrabutyl titanate is sequentially mixed with acetic acid, DMF, acetylacetone, anhydrous ethanol and a metal nitrate compound, stirred uniformly, then PVP is added and stirred until a viscous transparent solution appears, to obtain the electrostatic spinning precursor solution;
[0011] According to the mass ratio, the tetrabutyl titanate: acetic acid: DMF: acetylacetone: anhydrous ethanol: PVP = 1.23: (0.13-0.23): (4.20-7.80): (0.35-0.65): (1.70-2.40): (0.87-1.21); according to the molar ratio, the tetrabutyl titanate: metal nitrate compound = 1:1;
[0012] Step 2, electrostatic spinning of the electrostatic spinning precursor solution by using an electrostatic spinning process, and obtaining a fiber membrane after drying;
[0013] Step 3, oxidative sintering of the fiber membrane obtained in Step 2, nitrogenization reaction after cooling to room temperature, to obtain a multi-element titanium-based oxynitride with a tubular structure.
[0014] In Step 1, according to the mass ratio, the tetrabutyl titanate: acetic acid: DMF: acetylacetone: anhydrous ethanol: PVP = 1.23: 0.18: 6.00: 0.50: 2.00: 1.00.
[0015] In Step 1, the metal nitrate compound is one of lanthanum nitrate hexahydrate, cerium nitrate hexahydrate, praseodymium nitrate hexahydrate and neodymium nitrate hexahydrate.
[0016] In Step 2, the electrostatic spinning process is: electrostatic spinning of the electrostatic spinning precursor solution under the conditions of a positive voltage of 18-20 kV, a negative voltage of 3 kV, a liquid pushing speed of 0.6-0.8 ml / h and a receiving distance of 15-20 cm.
[0017] In Step 2, the drying temperature is 50-70℃, and the time is 2-5h.
[0018] In Step 3, the oxidative sintering process is: oxidative sintering at 780-1000℃ for 3-7h under an air atmosphere with a temperature rising rate of 3-10℃ / min.
[0019] In Step 3, the nitrogenization reaction process is: calcination at 900-1050℃ for 4-10h under an ammonia gas atmosphere with a flow rate of 200-500 ml / min.
[0020] A multi-element titanium-based oxynitride with a tubular structure, the chemical general formula of the multi-element titanium-based oxynitride is RTiO2N, wherein R = La, Ce, Pr, Nd; the multi-element titanium-based oxynitride has a tubular structure, the outer diameter is 800 nm to 2.0 microns, and the wall thickness is 50 nm to 300 nm.
[0021] The application also provides application of the multi-element titanium-based oxynitride prepared by the preparation method in the field of photocatalytic decomposition of water to produce hydrogen or photocatalytic fixation of carbon dioxide as a photocatalyst.
[0022] The application also provides application of the multi-element titanium-based oxynitride prepared by the preparation method in the field of photoelectrocatalytic decomposition of water as a photoelectrocatalytic electrode material for preparing a photoanode.
[0023] Compared with the prior art, the application has the following beneficial effects:
[0024] 1. The multi-element titanium-based oxynitride material with a tubular morphology is successfully prepared by adding anhydrous ethanol into the electrospinning precursor solution of the multi-element titanium-based oxynitride through electrospinning, and then sequentially going through drying, oxidation sintering and nitriding, and the specific surface area is significantly improved from 13.810 m 2 / g to 69.411 m 2 / g, and the significant improvement of the specific surface area provides a basis for the later application of the oxynitride material (such as increasing the catalytic reaction active site).
[0025] 2. The micro-morphology of the multi-element titanium-based oxynitride is controlled by optimizing the content of anhydrous ethanol, and finally the tubular structure with a large specific surface area is obtained; and the tubular structure of the multi-element titanium-based oxynitride material as a photocatalyst increases the active site on the surface of the photocatalyst, increases the light absorption area, reduces the carrier transport distance, effectively improves the light absorption characteristics, and thus improves the performance of the photocatalyst.
[0026] 3. By taking advantage of the characteristic that anhydrous ethanol is more likely to separate from the electrospinning precursor system as the temperature rises, as the amount of anhydrous ethanol increases, the number of small molecules that can be combined by the long chain of PVP approaches saturation, and the excess anhydrous ethanol makes the oxynitride spinning precursor system contain more free ethanol small molecule monomers. In the oxidation sintering process of step 3, the free ethanol and the ethanol molecules combined with the long chain of PVP are the first to separate from the oxynitride spinning precursor system, forming "hollows" in the fiber, and gradually diffusing R elements and Ti elements to the edge of the fiber, and finally forming a tubular structure.
[0027] In summary, the present application adopts electrospinning technology to add anhydrous ethanol in the electrospinning precursor solution of the multi-titanium-based oxynitride, and combines a heat treatment process to prepare the multi-titanium-based oxynitride material with a tubular morphology, which has the characteristics of simple process, controllable morphology and low cost; and the present application optimizes the content of anhydrous ethanol to control the micro-morphology of the multi-titanium-based oxynitride, and finally obtains the tubular structure with a larger specific surface area, increases the catalytic active sites on the material surface, increases the light absorption area, reduces the carrier transmission distance, and thus improves the photocatalytic performance of the material. BRIEF DESCRIPTION OF DRAWINGS
[0028] Figure 1 The formation mechanism diagram of LaTiO2N with a tubular morphology provided by the present application is shown.
[0029] Figure 2 The SEM diagram of LaTiO2N provided for Example 1 and Comparative Examples 1-4 is shown, wherein, Figure 2 (a) is Comparative Example 1, Figure 2 (b) is Comparative Example 2, Figure 2 (c) is Comparative Example 3, Figure 2 (d) is Comparative Example 4, Figure 2 (e) is Example 1.
[0030] Figure 3 The XRD diagram of LaTiO2N provided for Example 1 and Comparative Examples 1-4 is shown.
[0031] Figure 4 The BET adsorption and desorption isotherm of LaTiO2N provided for Example 1 and Comparative Examples 1-4 is shown, wherein, Figure 4 (a) is Comparative Example 1, Figure 4 (b) is Comparative Example 2, Figure 4 (c) is Comparative Example 3, Figure 4 (d) is Comparative Example 4, Figure 4 (e) is Example 1, Figure 4 (f) is the BET specific surface area comparison diagram of LaTiO2N with different anhydrous ethanol contents.
[0032] Figure 5 The UV-vis absorption curve of LaTiO2N provided for Example 1 and Comparative Examples 1-4 is shown.
[0033] Figure 6 The SEM diagram of CeTiO2N, PrTiO2N and NdTiO2N provided for Example 4 is shown, wherein, Figure 6 a is CeTiO2N, Figure 6 b is PrTiO2N, Figure 6 c is NdTiO2N.
[0034] Figure 7 XRD patterns of CeTiO2N, PrTiO2N, NdTiO2N provided for Example 4. DETAILED DESCRIPTION
[0035] The application will be further described below in conjunction with examples and drawings.
[0036] A multi-element titanium-based oxynitride with a tubular structure, chemical general formula is RTiO2N, wherein R = La, Ce, Pr, Nd; the titanium-based oxynitride has a tubular structure, the outer diameter is 800 nm to 2 μm, and the tube wall thickness is 50 nm to 300 nm.
[0037] A preparation method of a multi-element titanium-based oxynitride with a tubular structure, comprising the following steps:
[0038] Step 1, configuring an RTiO2N (R = La, Ce, Pr, Nd) electrostatic spinning precursor solution;
[0039] Tetrabutyl titanate, acetic acid, N, N-dimethylformamide (DMF), acetylacetone, anhydrous ethanol and a metal nitrate compound are sequentially mixed, stirred uniformly, and then polyvinylpyrrolidone (PVP) is added for continuous stirring until a viscous transparent solution is obtained, so as to obtain an RTiO2N electrostatic spinning precursor solution; according to the mass ratio, the tetrabutyl titanate: acetic acid: DMF: acetylacetone: anhydrous ethanol: PVP = 1.23: (0.13-0.23): (4.20-7.80): (0.35-0.65): (1.70-2.40): (0.87-1.21), and preferably 1.23:0.18:6.00:0.50:2.00:1.00; according to the molar ratio, the tetrabutyl titanate: metal nitrate compound = 1:1; the metal nitrate compound is one of lanthanum nitrate hexahydrate, cerium nitrate hexahydrate, praseodymium nitrate hexahydrate and neodymium nitrate hexahydrate, and the chemical general formula is R (NO3) 3·6H2O (R = La, Ce, Pr, Nd);
[0040] Step 2, electrostatic spinning of the RTiO2N electrostatic spinning precursor solution is carried out by using an electrostatic spinning process, and RTiO2N fiber membranes are obtained after drying; DMF, acetic acid, acetylacetone and ethanol in the fiber membranes are removed in the drying stage;
[0041] The electrostatic spinning process is that the electrostatic spinning precursor solution is electrostatically spun under the conditions of a positive voltage of 18-20 kV, a negative voltage of 3 kV, a liquid pushing speed of 0.6-0.8 ml / h and a receiving distance of 15-20 cm; the drying temperature is 50-70 ℃, and the time is 2-5 h;
[0042] Step 3: The RTiO2N fiber film obtained in Step 2 is heated from room temperature to 550-600°C at a heating rate of 3-10°C / min in an air atmosphere, and after forming a tubular morphology, it is further heated to 780-1000°C for 3-7h for oxidation sintering, and then cooled to room temperature to obtain a multi-component titanium-based oxynitride precursor with a tubular structure, with a general chemical formula of R2Ti2O7(R=La, Ce, Pr, Nd); in the oxidation sintering stage, the PVP, inorganic salt, etc. are decomposed by oxidation in air to obtain metal oxides, and a tubular morphology is obtained at the same time;
[0043] Step 4: The multi-component titanium-based oxynitride precursor obtained in Step 3 is calcined at 900-1050°C for 4-10h in an ammonia gas atmosphere with a flow rate of 200-500ml / min for nitriding reaction, and after cooling to room temperature, a multi-component titanium-based oxynitride with a tubular structure is obtained, with a general chemical formula of RTiO2N(R=La, Ce, Pr, Nd); in the nitriding stage, the titanium-based oxynitride precursor is nitrided to obtain a pure-phase multi-component titanium-based oxynitride.
[0044] Example 1
[0045] A method for preparing LaTiO2N with a tubular structure, comprising the following steps:
[0046] Step 1: 1.23g of tetrabutyl titanate, 0.18g of acetic acid, 6.00g of DMF, 0.50g of acetylacetone, 2.00g of anhydrous ethanol, and 1.56g of lanthanum nitrate hexahydrate are weighed in sequence, stirred well, then 1.00g of PVP is added, and then placed on a magnetic stirrer for continuous stirring until a clear, transparent and viscous yellow solution, i.e. an electrospinning precursor solution of LaTiO2N, is obtained;
[0047] Step 2: The electrospinning precursor solution of LaTiO2N is poured into a syringe and placed in a spinning machine for electrospinning. Aluminum foil paper is pasted on the receiving plate and stacked with several protrusions for timed sample collection, and placed in an oven for drying at 60°C for 4h to obtain a LaTiO2N fiber film; the receiving plate is connected to the negative electrode of the power supply to apply a negative voltage of 3kV, the needle is connected to the positive electrode of the power supply to apply a positive voltage of 18kV, and the distance between the receiving plate and the needle tip is about 20cm, and the liquid pushing speed is 0.72ml / h;
[0048] Step 3: The LaTiO2N fiber film obtained in Step 2 is uniformly placed on a corundum sheet, which is placed in a muffle furnace and heated to 600°C at a rate of 10°C / min in an air atmosphere, at which point a tubular morphology is formed, and the temperature is further increased to 900°C for 5h for oxidation sintering, and then cooled to room temperature to obtain La2Ti2O7 with a tubular morphology;
[0049] Step 4: Put La2Ti2O7 with tubular morphology into a quartz boat, and place the quartz boat into a tube furnace for nitridation in an ammonia atmosphere with a flow rate of 250 mL / min; the nitridation temperature is 1000℃, and the holding time is 10h; after the temperature drops to room temperature, the nitridation is completed, and LaTiO2N with tubular structure is obtained.
[0050] As shown in Figure 1 Example 1, when configuring the electrospinning precursor solution of LaTiO2N, adding anhydrous ethanol in the raw material realizes the complexation of lanthanum nitrate in the electrospinning precursor, effectively increases the diameter of the electrospinning precursor, and with the increase of the oxidation sintering temperature, the residual solvent, PVP and inorganic salt in the obtained electrospinning are successively volatilized and decomposed, and the nanowire precursor first forms a cavity, and then the cavity gradually increases, and finally the cavities merge to form a through hole; by optimizing the amount of anhydrous ethanol, the control of tubular morphology is effectively realized.
[0051] Example 2
[0052] A preparation method of LaTiO2N with tubular structure, comprising the following steps:
[0053] Step 1: weigh 1.23g of tetrabutyl titanate, 0.18g of acetic acid, 6.00g of DMF, 0.50g of acetylacetone, 1.70g of anhydrous ethanol, and 1.56g of lanthanum nitrate hexahydrate in sequence, stir well, then add 1.00g of polyvinylpyrrolidone, and then place on a magnetic stirrer for continuous stirring until a clear, transparent and viscous yellow solution, i.e. the electrospinning precursor solution of LaTiO2N, is obtained;
[0054] Step 2: pour the electrospinning precursor solution of LaTiO2N into a syringe and place it in a spinning machine for electrospinning; aluminum foil paper is pasted on the receiving plate and stacked with several protrusions for timing collection of the sample, and placed in an oven for drying at 60℃ for 4h to obtain a LaTiO2N fiber membrane; the receiving plate is connected to the negative electrode of the power supply to apply a negative voltage of 3kV, the needle is connected to the positive electrode of the power supply to apply a positive voltage of 18kV, and the distance between the receiving plate and the needle tip is about 20cm; the liquid pushing speed is 0.72ml / h;
[0055] Step 3: evenly place the LaTiO2N fiber membrane obtained in step 2 on a corundum sheet, and place the corundum sheet in a muffle furnace under an air atmosphere, and heat at a rate of 10℃ / min to 580℃, at which point the tubular morphology is formed, and continue to heat to 900℃ for oxidation sintering for 5h; after cooling to room temperature, La2Ti2O7 with tubular morphology is obtained;
[0056] Step 4: Put La2Ti2O7 with tubular morphology into a quartz boat, and place the quartz boat into a tube furnace for nitridation in an ammonia atmosphere with a flow rate of 350 mL / min; the nitridation temperature is 1000℃, and the temperature is kept for 5h; when the temperature drops to room temperature, the nitridation is completed, and LaTiO2N with tubular morphology is obtained.
[0057] Example 3
[0058] A method for preparing LaTiO2N with tubular structure, comprising the following steps:
[0059] Step 1: Weigh 1.23g of tetrabutyl titanate, 0.18g of acetic acid, 6.00g of DMF, 0.50g of acetylacetone, 2.40g of anhydrous ethanol, and 1.56g of lanthanum nitrate hexahydrate in sequence, stir well, then add 1.00g of polyvinylpyrrolidone, and continue to stir on a magnetic stirrer until a clear, transparent and viscous yellow solution, i.e. the electrospinning precursor solution of LaTiO2N, is obtained;
[0060] Step 2: Pour the electrospinning precursor solution of LaTiO2N into a syringe and place it in a spinning machine for electrospinning; paste aluminum foil on the receiving plate and stack several protrusions for timing sample collection, and place it in an oven for drying to obtain a LaTiO2N fiber membrane; apply a negative voltage of 3kV to the negative electrode of the power supply on the receiving plate, and apply a positive voltage of 18kV to the positive electrode of the power supply on the needle; the distance between the receiving plate and the needle tip is about 20cm, and the liquid pushing speed is 0.72ml / h;
[0061] Step 3: Place the LaTiO2N fiber membrane obtained in step 2 evenly on a corundum sheet, and place the corundum sheet in a muffle furnace; heat to 550℃ at a rate of 10℃ / min in an air atmosphere, at which point the tubular morphology is formed; continue to heat to 800℃ and sinter for 5h; after cooling to room temperature, La2Ti2O7 with tubular morphology is obtained;
[0062] Step 4: Put La2Ti2O7 with tubular morphology into a quartz boat, and place the quartz boat into a tube furnace for nitridation in an ammonia atmosphere with a flow rate of 250 mL / min; the nitridation temperature is 900℃, and the temperature is kept for 5h; when the temperature drops to room temperature, the nitridation is completed, and LaTiO2N with tubular morphology is obtained.
[0063] Example 4
[0064] This example 4 and the steps of example 1 are the same, and the difference is that the raw material La(NO3)3·6H2O is replaced by equal molar amount of Ce(NO3)3·6H2O, Pr(NO3)3·6H2O, Nd(NO3)3·6H2O, and CeTiO2N, PrTiO2N, NdTiO2N with tubular morphology are prepared.
[0065] Comparative Example 1
[0066] Comparative Example 1 is the same as Example 1 in steps and raw materials, except that no anhydrous ethanol is added.
[0067] Comparative Example 2
[0068] Comparative Example 2 is the same as Example 1 in steps and raw materials, except that 0.5 g of anhydrous ethanol is added after the addition of acetylacetone.
[0069] Comparative Example 3
[0070] Comparative Example 3 is the same as Example 1 in steps and raw materials, except that 1.0 g of anhydrous ethanol is added after the addition of acetylacetone.
[0071] Comparative Example 4
[0072] Comparative Example 5 is the same as Example 1 in steps and raw materials, except that 1.5 g of anhydrous ethanol is added after the addition of acetylacetone.
[0073] Figure 2 SEM images of LaTiO2N samples with different amounts of anhydrous ethanol, wherein, Figure 2 (a) is an SEM image of a sample without the addition of anhydrous ethanol, Figure 2 (b)- Figure 2 (e) are SEM images of samples with the addition of 0.5 g, 1.0 g, 1.5 g, and 2.0 g of anhydrous ethanol, respectively. Figure 2 As can be seen in (e), the surface morphology of the prepared LaTiO2N is uniform and dense, and the crystallinity is good; as can be seen in Figure 2 As can be seen in (a), the morphology of the sample without the addition of anhydrous ethanol is a solid line, and the cross-sectional diameter is small, about 600-700 nm. As the amount of added anhydrous ethanol gradually increases, the morphology of the sample gradually changes from Figure 2 the line in (a), through Figure 2 (b), Figure 2 (c), Figure 2 (d), and finally to Figure 2 (e) tubular, and the cross-sectional diameter of the sample with the addition of anhydrous ethanol is larger than that of the fiber material, the outer diameter of the obtained nanotube is about 2.0 μm, and the tube wall thickness is 300 nm.
[0074] Figure 3 XRD images of LaTiO2N samples with different amounts of anhydrous ethanol, wherein, Figure 3It can be seen that the XRD results are completely consistent with the standard card JCPDS NO. 48-1230 of LaTiO2N phase. In addition, the X-ray diffraction characteristic peaks of the samples with different anhydrous ethanol contents are almost completely consistent. It can be seen from the comparison with the standard card that the prepared sample matches well with the standard peak, and no impurity peak appears. This indicates that the LaTiO2N material prepared in Example 1 is a pure phase and has good crystallinity. It can be known from the preparation process that the addition of anhydrous ethanol has no effect on the phase of the LaTiO2N material, but only changes the structure of the material.
[0075] Figure 4 (a)- Figure 4 (e) is the BET adsorption and desorption isotherm spectrum of the LaTiO2N sample with 0 g, 0.5 g, 1.0 g, 1.5 g, and 2.0 g of anhydrous ethanol content, respectively, Figure 4 (f) is the BET specific surface area comparison result of the samples prepared by adding different anhydrous ethanol contents in the electrospinning precursor solution, combined with Figure 2 the SEM image of 2 / g, while the LaTiO2N material with 2.0 g of anhydrous ethanol has a tubular morphology, and the specific surface area is the largest, which is 69.411 m 2 / g, which is about 5.02 times the specific surface area of the linear LaTiO2N material. This indicates that the tubular LaTiO2N material prepared by adding anhydrous ethanol can significantly increase the specific surface area of the LaTiO2N material. Especially when the content of anhydrous ethanol is 2.0 g, the specific surface area of the prepared LaTiO2N material is the largest, thereby increasing the active sites on the surface of the photocatalytic material and increasing the light absorption area to achieve higher photocatalytic performance.
[0076] Figure 5 is the UV-vis absorption curve absorption spectrum of the LaTiO2N samples with different anhydrous ethanol contents, and the test range is 350 nm-800 nm to characterize the light absorption capacity of the samples with different anhydrous ethanol contents. From Figure 5 it can be seen that: the light absorption range of all samples is between 400 nm and 540 nm, and the light absorption capacity also increases with the increase of the anhydrous ethanol content. With the increase of the anhydrous ethanol content, the specific surface area of the prepared sample becomes larger and larger, which is beneficial to the absorption of light. On the other hand, the tubular structure is beneficial to the scattering of light inside the material, which greatly enhances the light absorption property of the material.
[0077] Figure 6 is the SEM image of the CeTiO2N, PrTiO2N, and NdTiO2N with tubular morphology prepared in Example 4; from Figure 6As can be seen from the preparation method of the present application, the CeTiO2N, PrTiO2N and NdTiO2N prepared by the preparation method of the present application all have a tubular morphology, the outer diameter is 800nm-2μm, and the wall thickness is 50nm-300nm.
[0078] Figure 7 The XRD pattern of the CeTiO2N, PrTiO2N and NdTiO2N material with a tubular morphology prepared by the preparation method of the present application is shown in the following table: Figure 7 As can be seen from the preparation method of the present application, the CeTiO2N, PrTiO2N and NdTiO2N prepared by the preparation method of the present application all have a tubular morphology, the outer diameter is 800nm-2μm, and the wall thickness is 50nm-300nm.
[0079] The above content is a further detailed description of the present application in combination with specific preferred embodiments, and cannot be deemed as limiting the specific implementation of the present application to these descriptions. For ordinary skilled in the art to which the present application belongs, several simple deductions or substitutions can be made without departing from the concept of the present application, and all of them shall be deemed as falling within the protection scope of the present application.
Claims
1. A method for producing a multi-component titanium-based oxynitride having a tubular structure, characterized by, The method comprises the following steps: Step 1, configuring an electrostatic spinning precursor solution of multi-element titanium-based oxynitride RTiO2N (R = La, Ce, Pr, Nd); Tetrabutyl titanate, acetic acid, DMF, acetylacetone, anhydrous ethanol and a metal nitrate compound are sequentially mixed, stirred uniformly, then PVP is added and stirred until a viscous transparent solution is obtained, thereby obtaining the electrostatic spinning precursor solution; In terms of mass ratio, the tetrabutyl titanate: acetic acid: DMF: acetylacetone: anhydrous ethanol: PVP = 1.23: (0.13-0.23): (4.20-7.80): (0.35-0.65): (1.70-2.40): (0.87-1.21); in terms of molar ratio, the tetrabutyl titanate: metal nitrate compound = 1:1; Step 2, electrostatic spinning of the electrostatic spinning precursor solution by using an electrostatic spinning process, and obtaining a fiber membrane after drying; Step 3, oxidation sintering of the fiber membrane obtained in Step 2, nitrogenization reaction after cooling to room temperature, and obtaining a multi-element titanium-based oxynitride with a tubular structure.
2. The method for preparing a multi-component titanium-based oxynitride with a tubular structure according to claim 1, characterized in that, In Step 1, in terms of mass ratio, the tetrabutyl titanate: acetic acid: DMF: acetylacetone: anhydrous ethanol: PVP = 1.23: 0.18: 6.00: 0.50: 2.00: 1.
00.
3. The method for preparing a multi-component titanium-based oxynitride with a tubular structure according to claim 1, characterized in that, In Step 1, the metal nitrate compound is one of lanthanum nitrate hexahydrate, cerium nitrate hexahydrate, praseodymium nitrate hexahydrate and neodymium nitrate hexahydrate.
4. The method for preparing a multi-component titanium-based oxynitride with a tubular structure according to claim 1, characterized in that, In Step 2, the electrostatic spinning process is that the electrostatic spinning precursor solution is electrostatically spun under the conditions of a positive voltage of 18-20 kV, a negative voltage of 3 kV, a liquid pushing speed of 0.6-0.8 ml / h and a receiving distance of 15-20 cm.
5. The method for preparing a multi-component titanium-based oxynitride with a tubular structure according to claim 1, characterized in that, In Step 2, the drying temperature is 50-70℃ and the time is 2-5 h.
6. The method for preparing a multi-component titanium-based oxynitride with a tubular structure according to claim 1, characterized in that, In Step 3, the oxidation sintering process is that the temperature is raised to 780-1000℃ at a temperature raising rate of 3-10℃ / min in an air atmosphere and then sintered for 3-7 h.
7. The method for preparing a multi-component titanium-based oxynitride with a tubular structure according to claim 1, characterized in that, In Step 3, the nitrogenization reaction process is that the calcination is carried out at 900-1050℃ for 4-10 h in an ammonia gas atmosphere with a flow rate of 200-500 ml / min.
8. A multi-component titanium-based oxynitride having a tubular structure, characterized by: The chemical general formula of the multi-element titanium-based oxynitride is RTiO2N, wherein R = La, Ce, Pr, Nd; the multi-element titanium-based oxynitride has a tubular structure, the outer diameter is 800 nm-2 μm and the tube wall thickness is 50 nm-300 nm.
9. Application of the multi-element titanium-based oxynitride prepared by the preparation method of any one of claims 1-7 as a photocatalyst in photocatalytic decomposition of water to produce hydrogen or photocatalytic fixation of carbon dioxide.
10. Application of the multi-element titanium-based oxynitride prepared by the preparation method of any one of claims 1-7 as a photoelectrocatalytic electrode material in preparation of a photoelectrocatalytic photoanode.
Citation Information
Patent Citations
A nitrogen oxide nanoparticle photocatalyst and its application
CN109331853B
Nitriding Synthesis of Nitrogen Oxide Material SmTiO2N and Its Application in Photocatalysis
CN112371159B
Method for preparing LaTiO2N oxynitride from single precursor
CN114835150A