Method for evaluating tensile strength of brittle solid material soaked in rainwater
By measuring and analyzing the tensile stress-strain curves and microcracks of brittle solid materials after being soaked in rainwater, and combining this with fracture damage mechanics theory, a relational equation was established, which solved the problem of evaluating the tensile strength of brittle materials after being soaked in rainwater and improved the safety assessment of engineering structures.
Patent Information
- Application Number
- CN202511614238.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-06
- Publication Date
- 2025-12-26
AI Technical Summary
Existing technologies lack effective methods to evaluate the tensile strength of brittle solid materials after being soaked in rainwater, making it difficult to assess the safety of engineering structures in environments with heavy rainfall caused by climate change.
By measuring the tensile stress and strain curves of brittle solid materials at different water saturation levels, and combining this with CT scans to determine the proportion of microcracks, the fracture toughness is measured using a three-point bending test. Based on the theory of fracture damage mechanics, a relationship equation between water saturation, tensile stress, and tensile strain is established to characterize the tensile strength of the material.
This invention provides a method to predict and evaluate the tensile strength of brittle solid materials after immersion in rainwater, helping to assess their fracture failure time under external loads and improving the safety and stability assessment of engineering structures.
Smart Images

Figure CN121207709A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of materials mechanics engineering technology, and in particular to a method for evaluating the tensile strength of brittle solid materials after being soaked in rainwater. Background Technology
[0002] With the continuous changes in the Earth's environment in recent years, the greenhouse effect has intensified, leading to increased heavy rainfall and rising sea levels. These factors have resulted in human-built engineering structures such as houses, roads, slopes, bridges, and tunnels facing greater erosion from rainwater. Brittle solid materials, such as cement, gypsum, concrete, and rock, are crucial materials used in the construction of these structures. Increased heavy rainfall and rising sea levels mean these brittle solid materials are exposed to rainwater for longer periods, potentially corroding their structures, reducing their strength, and posing greater risks to human life and property. Therefore, effectively predicting and evaluating the tensile strength of brittle solid materials after rainwater immersion is essential for safer and more stable engineering structure design and construction. A method for evaluating the tensile strength of brittle solid materials after rainwater immersion is needed. Summary of the Invention
[0003] The purpose of this invention is to provide a method for evaluating the tensile strength of brittle solid materials after being soaked in rainwater, in order to solve the problems of the prior art.
[0004] To achieve the above objectives, the present invention adopts the following technical solution: This invention includes the following steps: Includes the following steps: A. Two types of samples were processed from brittle solid materials to obtain a first cuboid sample and a second cuboid sample. The water saturation of the brittle solid materials under different soaking times was measured. B obtains the tensile stress of the first cuboid sample with different water saturation levels through tensile loading tests. With strain Curve, determine tensile strength value ; C determined the proportion of microcracks inside the first cuboid sample at different water saturation levels using CT scanning, and thus determined the initial damage value of the material under different water saturation levels. Based on the initial damage values with different water saturation levels, the relationship between initial damage and water saturation was fitted. D. Using a three-point bending test apparatus, the fracture toughness values of the second cuboid specimens with different water saturation levels were measured. Based on the fracture toughness values at different water saturation levels, the relationship between fracture toughness and water saturation is fitted. Based on fracture damage mechanics theory, an equation describing the relationship between water saturation, tensile stress, and tensile strain is established. The maximum stress value of the stress-strain curves for materials at different water saturation levels is also determined. The formula for characterizing the tensile strength of a water-saturated material is as follows:
[0005] In the formula,
[0006] In the formula: , , It is a material constant, a dimensionless parameter; This is the initial crack length, in meters (m). It is the initial crack angle. , Determined based on test results at a specific water saturation level; parameters The strain value is determined based on the maximum stress value in the stress-strain curve of the material measured by a tensile testing instrument.
[0007] Furthermore, parameters , , , By comparing and analyzing the stress and strain curves calculated theoretically and measured experimentally, when the two curves are basically similar, then at this point... , , The value is a fixed value, and its range is 0 < < 3, 0< < 1 , 0< < 0.004m, 0< < 90.
[0008] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention establishes a relationship equation between stress, strain, and water saturation based on fracture damage mechanics. The maximum stress value of the material under different water saturation levels is used to characterize the tensile strength of the material.
[0009] This invention establishes a method for analyzing brittle solid materials after rainwater immersion. When subjected to external tensile loads, it can further evaluate and predict the fracture failure time of brittle solid materials under different materials, different axial compressive loads, or different immersion rates, providing an important reference for the safety and stability assessment of brittle solid material engineering structures under heavy rainfall caused by climate warming. Attached Figure Description
[0010] Figure 1 This is a schematic diagram showing the tensile strength values of marble at different water saturation levels obtained from experimental tests. Figure 2 A schematic diagram illustrating the tensile strength values of marble at different water saturation levels obtained through theoretical calculations. Figure 3 This is a schematic diagram comparing the theoretical and experimental results of the tensile strength of marble under different water saturation levels. Detailed Implementation
[0011] Reference Figure 1-3 The following example of brittle solid granite is used to verify the reliability of the theoretical equations in this invention.
[0012] To achieve the above objectives, the present invention includes the following steps: 1. Select a brittle solid material and, according to the requirements of the testing instrument, process two types of samples: 10cm*5cm*5cm and 8cm*3cm*1cm rectangular brittle solid material samples. Then, immerse the material in rainwater for different soaking times: 1, 12, and 24 hours (this time can be adjusted according to actual conditions). After each soaking time, remove the samples and measure their mass. Subtract the mass of the sample before soaking from the mass after soaking. The ratio of this difference to the mass before soaking is the water saturation of the sample. .
[0013] 2. Place 10cm*5cm*5cm rectangular solid material specimens with different water saturation levels from step 1 into a tensile loading testing apparatus and measure the tensile stress of the materials with different water saturation levels. With strain Curve, and determine tensile strength value Its unit is Pa.
[0014] 3. Using a CT scanner, measure the proportion of microcracks inside 10cm*5cm*5cm rectangular solid material samples with different water saturation levels from step 1, and then determine the initial damage value of the material under different water saturation levels. Based on the initial damage values with different water saturation levels, an equation relating the initial damage to the water saturation level can be fitted. .
[0015] 4. Using a three-point bending test apparatus, measure the fracture toughness of brittle solid 8cm*3cm*1cm rectangular specimens with different water saturation levels from step 1. Its unit is Pa·m 1 / 2 Then, based on the fracture toughness values at different water saturation levels, a relationship equation between fracture toughness and water saturation was fitted. .
[0016] 5. Based on the theory of fracture damage mechanics, establish a relational equation that can describe the relationship between water saturation, tensile stress, and tensile strain. This equation can be used to plot the stress-strain relationship curves of materials at different water saturation levels, and these curves exhibit a stress maximum value. This maximum value represents the tensile strength of the material at this water saturation level.
[0017]
[0018] In the formula,
[0019] In the formula above: , , It is a material constant, a dimensionless parameter; This is the initial crack length, in meters (m). It is the initial crack angle.
[0020] 6. In the formula of step 5 , It can then be determined based on the test results at a specific water saturation level in steps 3 and 4.
[0021] 7. Parameters in the formula of step 5 The strain value can be determined based on the stress-strain curve of the material measured by the tensile testing instrument in step 2, where the strain value corresponds to the maximum stress value.
[0022] 8. Parameters in the formula of step 5 , , , The stress and strain curves obtained from the theoretical calculations in step 5 and the experimental measurements in step 2 can be repeatedly compared and analyzed. When the two curves are basically similar, then... , , The value is a fixed value, and its range is 0 < <3, 0< < 1 , 0< < 0.004m, 0< < 90.
[0023] 9. After determining all model parameters in step 5 based on the above process, and verifying the rationality of the formula in step 5 through the experimental results in step 2, the tensile strength of brittle solid materials under different water saturation levels can be further predicted and analyzed based on the formula in step 5, thereby providing support for engineering construction.
[0024] The following section takes brittle solid marble as an example to calculate and analyze the theoretical tensile strength of marble under different water saturation levels, and compares and analyzes the results with the experimental results to verify the rationality of the proposed method.
[0025] The following are the specific parameter values for marble materials: =89 0 , =0.003m =1、 =0.12、 =1 / 350.
[0026]
[0027]
[0028] .
[0029] Figure 1 Test results of tensile strength for marble with different water saturation levels are presented. Figure 2 The present invention provides the tensile strength results of marble with different water saturation levels obtained by theoretical calculation. Figure 3 The experimental and theoretical results are compared. The trends of the theoretical and experimental results are consistent and their magnitudes are similar, verifying the rationality of the proposed method for evaluating the tensile strength of brittle solid materials after rainwater immersion.
[0030] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A method for evaluating the tensile strength of a brittle solid material after rainwater immersion, characterized by, The method comprises the following steps: A. selecting a brittle solid material to process two types of samples to obtain a first cuboid sample and a second cuboid sample, and measuring the water saturation of the brittle solid material under different bubble times; B the tensile stress of the material of the first cuboid sample at different water saturations is obtained by the tensile loading test with strain curve, the tensile strength value is determined ; C determining the proportion of micro-cracks inside the first cuboid sample with different water saturation by CT scanning, and determining the initial damage value of the material under different water saturation , fitting the relationship between initial damage and water saturation according to the initial damage value under different water saturation D using a three-point bending test instrument, measure the fracture toughness value of the second cuboid sample with different water saturation , according to the fracture toughness value of different water saturation, fit the relationship between fracture toughness and water saturation; E Based on the fracture damage mechanics theory, the relationship equation describing the water saturation, tensile stress, tensile strain is established, and the maximum stress of the stress-strain relationship curve of the material under different water saturation The tensile strength of the material with water saturation is characterized, and the formula is as follows: ; In the formula, In the formula, ; wherein: , , is a material constant, is a dimensionless parameter; is the initial crack length, in meters; is the initial crack angle, , is determined from the test results at a specific water saturation; parameter is determined from the stress-strain curve of the material measured by the tensile testing instrument, at the strain value corresponding to the maximum stress.
2. A method for evaluating the tensile strength of a brittle solid material after rainwater immersion according to claim 1, characterized in that, Parameters , , , Comparative analysis of the stress and strain curves calculated theoretically and measured by experiments, when the two curves are basically similar, the value of the parameter at this time is determined , , The value is a determined value, and the value range is 0 < 3, 0 < 1 , 0 < 0.004m, 0 < 90.
Citation Information
Patent Citations
Method for testing fracture toughness of rattan canes based on three-point bending mode
CN104568605A
Method for evaluating long-term service life of directly-stretched brittle solid material
CN116399694A
Method for evaluating fracture mechanical property of water-soaked fragile solid material
CN117030452A
Calibration method for finite-discrete element input parameters of water-containing rock
CN120741769A
Method for dynamically assessing slope safety
US20250035816A1