Environment-friendly high-strength salt film and preparation method thereof

By using grafted PVC, environmentally friendly plasticizers, and degradation promoters in salt films, combined with a microbial-triggered degradation mechanism, the problems of salt films being brittle and difficult to degrade have been solved, resulting in high-strength, environmentally friendly, and biodegradable salt films that extend service life and degrade efficiently after disposal.

CN121249068APending Publication Date: 2026-01-02SHANDONG SEA EAGLE PLASTIC TECH CO LTD

Patent Information

Application Number
CN202511644077.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-11-11
Publication Date
2026-01-02

AI Technical Summary

Technical Problem

Existing salt films suffer from problems such as easy embrittlement, short service life, plasticizer migration and brine contamination, and difficulty in disposal after disposal. Furthermore, existing improvement measures have failed to effectively resolve the contradiction between environmental protection and biodegradability and weather resistance.

Method used

Grafted PVC is used as the film-forming matrix, and environmentally friendly plasticizers and degradation promoters are added. Through the synergistic effect of UV absorbers, light stabilizers and antioxidants, compatibility is enhanced and aging resistance is achieved. At the same time, a microbially triggered degradation mechanism is used to avoid conflict with UV stabilizers.

Benefits of technology

It achieves an environmentally friendly and biodegradable high-strength salt film, extends service life, and degrades efficiently after disposal, meeting environmental protection requirements, reducing brine pollution, and improving service life and degradation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of film materials, and particularly discloses an environment-friendly high-strength salt film and a preparation method thereof.The salt film is prepared from, by weight, 90-110 parts of grafted PVC, 35-45 parts of environment-friendly plasticizer, 3.0-4.5 parts of heat stabilizer, 0.3-0.6 part of benzotriazole ultraviolet light absorber, 0.4-0.8 part of hindered amine light stabilizer, 0.2-0.4 part of antioxidant, 0.5-1.5 parts of lubricant, 10-20 parts of filler and 1-2 parts of degradation promoting agent. Through the cooperation of the ultraviolet light absorber, the light stabilizer and the antioxidant, the anti-aging performance is realized, and the service life of the smoke film is prolonged; meanwhile, by enhancing the compatibility between the PVC resin and the auxiliaries, migration of the auxiliaries is reduced, and pollution to brine is reduced; in addition, degradation of PVC is enhanced by adopting a degradation promoting agent of a microbial environmental degradation triggering mechanism, non-interference to the service life and high-efficiency degradation after waste are realized, and two contradictory performances of environmental friendliness, degradability and weather resistance are met.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The application belongs to the technical field of film materials, and particularly relates to an environmentally-friendly high-strength salt film and a preparation method thereof. BACKGROUND

[0002] Salt industry special film (hereinafter referred to as "salt film") is mainly used for covering salt crystallization ponds to realize the functions of rain prevention, fresh water drainage and anti-seepage. Since the 1970s, plastic film has been applied in salt industry, and the salt film has experienced evolution from single function to specialization and serialization. The early film mainly has the basic waterproof function, with the maturation of the calendar expansion process, the modern salt film has the characteristics of high tensile strength, acid and alkali corrosion resistance, aging resistance, etc., the width can reach 2000-4500mm, the thickness range is 0.08-0.20mm, and the service life is about 3-5 years. At present, China's sea salt production is the largest in the world, and the demand for salt film is stable and continuously increasing.

[0003] Although the salt film technology is relatively mature, the salt industry PVC film still has the problems of easy brittleness, short service life, plasticizer migration polluting brine, and difficult treatment after being discarded. For the above problems, the patent CN1359972A prolongs the service life by adding ultraviolet absorbers and metal soap heat stabilizers to enhance the weather resistance and mechanical strength of the film, but does not weaken the degradation difficulty. For example, the patent CN107298834B uses polylactic acid as a base resin to reduce the degradation difficulty of the discarded film, but the polylactic acid film has high cost and high brittleness, and is easy to be damaged if not handled properly, affecting the sealing performance. Therefore, the application aims to provide a PVC salt film which is environmentally-friendly and degradable, and has weather resistance and high strength. SUMMARY

[0004] In order to overcome the shortcomings of the prior art, the application strengthens the compatibility between PVC resin and additives to reduce the migration of additives and reduce the pollution to brine, and at the same time, a degradation promoter of a microbial environment degradation trigger mechanism is used to avoid the conflict with ultraviolet stabilizers and the like, to strengthen the degradation of PVC, to realize the non-interference on the service life and the efficient degradation after being discarded, to meet the two contradictory performances of environmental-friendly and degradable and weather resistance. In addition, the ultraviolet absorbers, light stabilizers and antioxidants are synergized to realize the aging resistance performance, and the service life is improved.

[0005] To achieve the above purpose, the technical scheme adopted by the application is: The application provides an environment-friendly high-strength salt film, which comprises the following raw materials in parts by weight: 90-110 parts of grafted PVC, 35-45 parts of environment-friendly plasticizer, 3.0-4.5 parts of thermal stabilizer, 0.3-0.6 parts of benzotriazole ultraviolet absorber, 0.4-0.8 parts of hindered amine light stabilizer, 0.2-0.4 parts of antioxidant, 0.5-1.5 parts of lubricant, 10-20 parts of filler and 1-2 parts of degradation promoter.

[0006] The benzotriazole ultraviolet absorber can efficiently absorb ultraviolet rays with a wavelength of 290-400 nm, thereby improving weather resistance; the hindered amine light stabilizer can effectively inhibit the photo-oxidation process by capturing free radicals, thereby significantly delaying film aging, brittleness and discoloration; and the antioxidant can prevent thermal-oxidative aging during processing and use. The film has the aging resistance performance by the synergistic effect of the above-mentioned ultraviolet absorber, light stabilizer and antioxidant, thereby improving the service life. Meanwhile, the grafted PVC is selected as the film-forming matrix to improve the compatibility with the additives, reduce the migration of the additives and avoid the pollution of brine.

[0007] In some embodiments, the environment-friendly plasticizer comprises epoxy soybean oil and acetyl tributyl citrate.

[0008] In some embodiments, the mass ratio of the epoxy soybean oil and the acetyl tributyl citrate is 1:(2.5-4.5).

[0009] The epoxy soybean oil with a biological source is non-toxic, environment-friendly, easily biodegradable and has the function of thermal stabilizer. The acetyl tributyl citrate has good compatibility with PVC, high plasticizing efficiency, non-toxicity and good biodegradability. The two components have a synergistic plasticizing effect in the formula, the acetyl tributyl citrate provides the core flexibility and low-temperature toughness required by the film, and the epoxy soybean oil provides the thermal stability and durability.

[0010] In some embodiments, the preparation steps of the grafted PVC are as follows: The dispersant is dissolved in deionized water, then a pH buffer is used to maintain the pH at 6.8-7.2, vacuum is extracted and replaced by nitrogen, VCM is added, then maleic anhydride and initiator-DOP solution are added, the kettle body is sealed, stirring is started, and the reaction is carried out at 58-64 DEG C until the pressure drops to 0.28-0.32 MPa, then the unreacted VCM is recovered by vacuum flash, and the remaining PVC slurry is washed and vacuum dried to constant weight, thereby obtaining the grafted PVC.

[0011] The strong dipole-dipole interaction between the strong polar carboxylic anhydride groups of maleic anhydride and the epoxy groups of the epoxy soybean oil and the ester groups of acetyl tributyl citrate in the grafted PVC greatly increases the affinity of the plasticizer to the resin, significantly reduces the migration rate of the plasticizer, thereby prolonging the service life of the film and preventing brine pollution. At the same time, the polar surface of the grafted PVC has similar polarity and surface energy as the PCL layer of the pro-degradant, which can improve the interfacial compatibility between the two, making the pro-degradant more uniformly dispersed in the PVC matrix and more firmly bonded at the interface, reducing stress defects and improving the mechanical strength of the film.

[0012] In some embodiments, the dispersant comprises PVA and hydroxypropyl methyl cellulose.

[0013] Preferably, the mass ratio of the PVA and hydroxypropyl methyl cellulose is 1:(0.2-0.8).

[0014] In some embodiments, the initiator is a peroxide compound.

[0015] In some embodiments, the mass ratio of the VCM and maleic anhydride is 1:(0.015-0.030).

[0016] By controlling the amount of maleic anhydride to avoid excessive crosslinking or gel formation, the mechanical properties of the grafted PVC are affected.

[0017] In some embodiments, the heat stabilizer is a calcium-zinc composite stabilizer.

[0018] The use of a non-toxic and environmentally friendly calcium-zinc composite stabilizer instead of toxic lead and cadmium salt stabilizers improves environmental protection.

[0019] In some embodiments, the filler is active calcium carbonate.

[0020] Active calcium carbonate as a filler can effectively reduce costs and improve film rigidity, stiffness, and tear resistance. Lubricants can reduce friction between materials and equipment during processing, prevent roll sticking, and ensure smooth processing.

[0021] In some embodiments, the preparation steps of the pro-degradant are as follows: S1, respectively configure 0.5-1.5 mol / L [Fe(EDTA)] - stock solution A and 0.5-1.5 mol / L [Mn(EDTA)] 2- stock solution B, and co-spray dry stock solution A and stock solution B to obtain a complex catalyst powder; S2, a PCL-dichloromethane solution with a concentration of 3-5 wt% is configured, and a complex catalyst powder is added thereto, and homogenized at 5-15 °C to obtain a suspension; the rotation speed is maintained at 7000-9000 rpm, the suspension is added to a PVA aqueous solution, and sheared for 8-15 min, then a displacement liquid is added thereto until no solid is precipitated, the solid is collected, washed, dried, and sieved to obtain a degradation promoter.

[0022] The working principle of the degradation promoter avoids conflict with ultraviolet stabilizers, realizes degradation on demand, and basically does not play a role during the service life of the film; after being discarded, the polymer chain is catalytically oxidized and degraded under the action of light, heat and oxygen, and is broken into low molecular weight fragments, and is finally decomposed by microorganisms.

[0023] During the service life of the salt pan, the PVC film is in a high-salt, strong ultraviolet outdoor environment, and PCL as the shell can effectively resist the erosion of ultraviolet and salt water, significantly reducing the diffusion flux of water, oxygen and H2O2 to the core, so that the complex catalyst cannot contact PVC and its degradation intermediates during the service life of the film, and remains in a low active state. When the film completes its mission and is discarded in a landfill, composting environment or soil, a rich microbial community serves as a trigger condition to start working, and some naturally occurring microorganisms (such as bacteria and fungi) can secrete hydrolytic enzymes (such as lipase), which can specifically break the ester bond in the PCL molecular chain, causing it to biodegrade. As the PCL shell is gradually decomposed and eroded by microorganisms, its structural integrity is destroyed, eventually leading to the rupture of the shell and the exposure of the internal complex catalyst.

[0024] The exposed high-efficiency catalyst immediately reacts with the oxygen and water permeating from the environment and the PVC itself, starts the catalytic oxidative degradation chain reaction, generates a large number of free radicals, attacks and breaks the PVC molecular chain, and the specific performance is as follows: PVC will slowly produce hydroperoxide (POOH) under the action of light and oxygen, and these substances can produce trace amounts of hydrogen peroxide (H2O2) upon decomposition. In the complex powder, Fe 3+ / Fe 2+ as a redox couple, while Mn 3+ →Fe 2+ cycling promotes a synergistic mechanism that catalyzes the decomposition of hydrogen peroxide, generating more highly reactive hydroxyl radicals (·OH); the active oxygen species such as hydroxyl radicals have extremely strong oxidizing ability, which will attack the PVC molecular chain and form macromolecular radicals by stealing hydrogen atoms; the macromolecular radicals will undergo chain scission reactions in the presence of oxygen, resulting in a sharp decrease in molecular weight; the decrease in molecular weight directly leads to the loss of mechanical properties of the film (becoming brittle and powdering), and macroscopically, the film breaks into fragments.

[0025] In some embodiments, in step S1, the volume ratio of the solution A and the solution B is 1:(0.8-1.2).

[0026] In some embodiments, in step S1, the particle size of the complex catalyst powder is 1-5 μm.

[0027] In some embodiments, in step S2, the mass ratio of PCL to the complex catalyst powder is 1:(1-2).

[0028] By controlling the concentration of the PCL-dichloromethane solution, the incomplete coating or the formation of gel balls or fibrous structures is avoided.

[0029] Another aspect of the present application provides a preparation method of the above-mentioned environmentally friendly high-strength salt film, and the specific steps are as follows: Mixing: Put the grafted PVC into a 100-120°C mixing machine, first add the heat stabilizer, benzotriazole ultraviolet absorber, hindered amine light stabilizer, antioxidant, pro-degradant and solid lubricant, mix for 1-2 min, then add the environmentally friendly plasticizer, and finally add the filler, mix for 10-30 min, and then stir and cool to below 40°C; Extrusion molding: select a co-rotating parallel twin-screw extruder equipped with a melt pump and an automatic screen changer to extrude the material; the process parameters of the extruder are as follows: zone 1: 130-140°C, zone 2: 150-160°C, zone 3: 160-170°C, and die head: 165-175°C; Calendering: adopt a coat hanger type T die, the material is immediately introduced into a three-roll calender after being extruded from the die lip, the three-roll temperature is as follows: upper roll: 80-90°C, middle roll: 70-80°C, and lower roll: 60-70°C, to obtain a calendered film; Post-treatment: introduce the calendered film into a cooling roll group through a traction roll, cool to room temperature, and adopt an automatic tension control system for winding, and store the wound film at room temperature for aging, to obtain the environmentally friendly high-strength salt film.

[0030] In some embodiments, in the extrusion molding, the melt pressure of the melt pump is 15-25 MPa, and the size of the automatic screen changer is 80-120 mesh screen.

[0031] Compared with the prior art, the present application has the following beneficial effects: 1. The present application provides a PVC salt film which is environmentally friendly, degradable, and weather-resistant and high-strength, the environmental friendliness of the salt film is improved by using a compounded degradable plasticizer and a non-toxic calcium-zinc composite stabilizer; the aging resistance is realized by the synergy of the ultraviolet absorber, the light stabilizer and the antioxidant, and the service life is improved; meanwhile, the compatibility between the base resin and the additives is improved by grafting polar groups to PVC, the migration of the additives is reduced, and the brine is prevented from being polluted.

[0032] 2、In the aspect of enhancing the degradability of PVC salt film, the application uses microbe-triggered pro-degradation agent, avoids the conflict with ultraviolet stabilizer, and realizes degradation on demand. During the service life of the salt field, the PVC film is in the open environment of high salt and strong ultraviolet light. The PCL of the pro-degradation agent as the shell can effectively resist the erosion of ultraviolet light and salt water, significantly reduces the diffusion flux of water, oxygen and H2O2 to the core, and keeps the complex catalyst in a low active state without contacting PVC and its degradation intermediates during the service life of the film. When the film is discarded in the landfill, composting environment or soil after completing the mission, the hydrolytic enzyme secreted by the microbe can specifically break the ester bond in the PCL molecular chain, so that the PCL shell is gradually decomposed and eroded by the microbe, and the internal complex catalyst is exposed to start the catalytic oxidative degradation chain reaction to attack the PVC molecular chain. DETAILED DESCRIPTION

[0033] The application will be described below in combination with specific embodiments. It should be noted that the following examples are examples of the application and are only used to illustrate the application, but not to limit the application. Other combinations and various modifications within the concept of the application can be made without departing from the main idea or scope of the application. It is worth noting that the raw materials used in the following preparation examples and examples are from any manufacturer on the market unless otherwise specified: PCL, Mn=50000; PVA, type PVA-217; PVC, type SG5; active calcium carbonate, brand LD-3000; calcium-zinc composite stabilizer, type Nanjing Puli Yi-PKJ5205.

[0034] Preparation Example 1 The preparation steps of the pro-degradation agent A are as follows: S1, respectively configure 0.9 mol / L [Fe(EDTA)] - stock solution A and 0.9 mol / L [Mn(EDTA)] 2- stock solution B, co-spray dry stock solution A and stock solution B at a volume ratio of 1:1, inlet 180°C, outlet 75°C, to obtain complex catalyst powder with a particle size of 3±0.2 μm; S2, configure 500 g of PCL-dichloromethane solution with a concentration of 4 wt%, add 30 g of complex catalyst powder to it, homogenize at 10°C and 8000 rpm for 3 min to obtain a suspension; keep the speed at 8000 rpm, add the suspension to 1000 mL of PVA aqueous solution with a concentration of 5 wt%, shear at 12000 rpm for 10 min, add isopropyl alcohol until no solid is precipitated, collect the solid, wash with deionized water, dry at 40°C to constant weight, and pass through a 200 mesh sieve to obtain the pro-degradation agent A.

[0035] Preparation Example 2 The preparation steps of the degradation promoter B are different from those of Preparation Example 1 in that step S1 is adjusted as follows: S1, 0.9 mol / L [Fe(EDTA)] stock solution is prepared - The stock solution is spray-dried at an inlet temperature of 180°C and an outlet temperature of 75°C to obtain a complex catalyst powder with a particle size of 3±0.2 μm.

[0036] Preparation Example 3 The preparation steps of the degradation promoter C are different from those of Preparation Example 1 in that in step S2, the amount of the complex catalyst powder is 16 g.

[0037] Preparation Example 4 The preparation steps of the degradation promoter D are different from those of Preparation Example 1 in that in step S2, the amount of the complex catalyst powder is 44 g.

[0038] Preparation Example 5 The preparation steps of the degradation promoter E are as follows: 0.9 mol / L [Fe(EDTA)] stock solution and 0.9 mol / L [Mn(EDTA)] stock solution are prepared respectively - 0.9 mol / L [Fe(EDTA)] stock solution and 0.9 mol / L [Mn(EDTA)] stock solution are prepared respectively 2- The stock solutions A and B are co-spray-dried at a volume ratio of 1:1 at an inlet temperature of 180°C and an outlet temperature of 75°C to obtain the degradation promoter E with a particle size of 3±0.2 μm.

[0039] Preparation Example 6 The preparation steps of the grafted PVC-A are as follows: The dispersant (0.8 g PVA and 0.4 g hydroxypropyl methylcellulose) is dissolved in deionized water, and then a 1 mol / L NaHCO3 solution is used to maintain the pH at 7. Vacuum is applied and replaced with nitrogen. Then, 1000 g VCM is added, followed by the addition of 22 g maleic anhydride and 6 g EHP-DOP solution with a concentration of 0.1 wt%. The kettle body is sealed, and stirring is started. The reaction is carried out at 62°C until the pressure drops to 0.3 MPa. The unreacted VCM is recovered by vacuum flash evaporation. The remaining PVC slurry is first washed with a 55°C, pH 8.0 Na2CO3 solution, and then with deionized water. Vacuum drying is carried out at 50°C until a constant weight is obtained, thereby obtaining the grafted PVC-A.

[0040] Preparation Example 7 The preparation steps of the grafted PVC-B are different from those of Preparation Example 6 in that the amount of maleic anhydride is 13 g.

[0041] Preparation Example 8 The preparation step of the grafted PVC-C is different from that of Preparation Example 6 in that the amount of maleic anhydride is 32 g.

[0042] Example 1 An environmentally friendly high-strength salt film contains, by weight parts, the following raw materials: grafted PVC-A 100 parts, environmentally friendly plasticizer (epoxy soybean oil 8.8 parts, acetyl citric acid tributyl ester 31.2 parts) 40 parts, calcium-zinc composite stabilizer 3.6 parts, benzotriazole ultraviolet absorber (UV-326) 0.45 parts, hindered amine light stabilizer (HALS-622) 0.6 parts, antioxidant 1010 0.3 parts, lubricant (polyethylene wax) 0.8 parts, active calcium carbonate 15 parts, and pro-degradation agent-A 1.5 parts.

[0043] The preparation method of the environmentally friendly high-strength salt film in this embodiment specifically includes the following steps: Mixing: Put the grafted PVC-A into a 110°C mixer, first add the calcium-zinc composite stabilizer, UV-326, HALS-622, antioxidant 1010, pro-degradation agent A, and polyethylene wax, mix for 2 min, then add the environmentally friendly plasticizer, and finally add the active calcium carbonate. Mix for 20 min and cool to below 40°C under stirring; Extrusion molding: Select a co-rotating parallel twin-screw extruder equipped with a melt pump (melt pressure 20 MPa) and an automatic screen changer (100 mesh screen) to extrude the material. The process parameters of the extruder are: zone 1: 135°C, zone 2: 155°C, zone 3: 165°C, and die head: 170°C; Calendering: Use a coat hanger type T-die, the material is extruded from the die lip and immediately enters a three-roll calender. The three-roll temperature is: upper roll: 85°C, middle roll: 75°C, and lower roll: 65°C. The calendered film is obtained; Post-processing: The calendered film passes through a traction roller and enters a cooling roller group, cools to room temperature, and is wound using an automatic tension control system. The wound film is stored and aged at room temperature, and the environmentally friendly high-strength salt film is obtained.

[0044] Example 2 An environmentally friendly high-strength salt film contains, by weight parts, the following raw materials: grafted PVC-A 90 parts, environmentally friendly plasticizer (epoxy soybean oil 10 parts, acetyl citric acid tributyl ester 25 parts) 35 parts, calcium-zinc composite stabilizer 3.0 parts, benzotriazole ultraviolet absorber (UV-326) 0.3 parts, hindered amine light stabilizer (HALS-622) 0.4 parts, antioxidant 1010 0.2 parts, lubricant (polyethylene wax) 0.5 parts, active calcium carbonate 10 parts, and pro-degradation agent-A 1 part.

[0045] The preparation method of the environment-friendly high-strength salt film in this embodiment specifically comprises the following steps: Mixing: Put the grafted PVC-A into a 100°C mixer, first add calcium-zinc composite stabilizer, UV-326, HALS-622, antioxidant 1010, pro-degradant A and polyethylene wax, mix for 2 min, then add the environment-friendly plasticizer, and finally add active calcium carbonate, stir for 15 min and cool to below 40°C; Extrusion molding: Select a co-rotating parallel twin-screw extruder equipped with a melt pump (melt pressure 15 MPa) and an automatic screen changer (80 mesh screen) to extrude the material; the extruder process parameters are: zone 1: 130°C, zone 2: 150°C, zone 3: 160°C, and die head: 165°C; Calendering: Use a coat hanger type T-die, the material is extruded from the die lip and immediately enters a three-roll calender, the three-roll temperature is: upper roll: 80°C, middle roll: 70°C, and lower roll: 60°C, to obtain a calendered film; Post-processing: The calendered film passes through a traction roller and enters a cooling roller group, cools to room temperature, and is wound up using an automatic tension control system. The wound film is stored and aged at room temperature to obtain the environment-friendly high-strength salt film.

[0046] Example 3 An environment-friendly high-strength salt film, by weight, comprises the following raw materials: grafted PVC-A 110 parts, environment-friendly plasticizer (epoxy soybean oil 8.2 parts, acetyl citrate tributyl ester 36.8 parts) 45 parts, calcium-zinc composite stabilizer 4.5 parts, benzotriazole ultraviolet absorber (UV-326) 0.6 parts, hindered amine light stabilizer (HALS-622) 0.8 parts, antioxidant 1010 0.4 parts, lubricant (polyethylene wax) 1.5 parts, active calcium carbonate 20 parts, and pro-degradant-A 2 parts.

[0047] The preparation method of the environment-friendly high-strength salt film in this embodiment specifically comprises the following steps: Mixing: Put the grafted PVC-A into a 100°C mixer, first add calcium-zinc composite stabilizer, UV-326, HALS-622, antioxidant 1010, pro-degradant A and polyethylene wax, mix for 2 min, then add the environment-friendly plasticizer, and finally add active calcium carbonate, stir for 15 min and cool to below 40°C; Extrusion molding: Select a co-rotating parallel twin-screw extruder equipped with a melt pump (melt pressure 15 MPa) and an automatic screen changer (80 mesh screen) to extrude the material; the extruder process parameters are: zone 1: 130°C, zone 2: 150°C, zone 3: 160°C, and die head: 165°C; Calendering: using a hanger type T-die, the material is extruded from the die lip and immediately enters a three-roll calender, the three-roll temperature is upper roll: 90°C, middle roll: 80°C, lower roll: 70°C, to obtain a calendered film; Post-processing: the calendered film passes through a traction roller and enters a cooling roller group, is cooled to room temperature, and is wound using an automatic tension control system. The wound film is stored at room temperature for aging, to obtain an environmentally friendly high-strength salt film.

[0048] Example 4 This example provides an environmentally friendly high-strength salt film and a preparation method thereof, and the specific implementation manner is the same as that of Example 1, except that the degradation promoter A is replaced by the same amount of degradation promoter B.

[0049] Example 5 This example provides an environmentally friendly high-strength salt film and a preparation method thereof, and the specific implementation manner is the same as that of Example 1, except that the degradation promoter A is replaced by the same amount of degradation promoter C.

[0050] Example 6 This example provides an environmentally friendly high-strength salt film and a preparation method thereof, and the specific implementation manner is the same as that of Example 1, except that the degradation promoter A is replaced by the same amount of degradation promoter D.

[0051] Example 7 This example provides an environmentally friendly high-strength salt film and a preparation method thereof, and the specific implementation manner is the same as that of Example 1, except that the degradation promoter A is replaced by the same amount of degradation promoter E.

[0052] Example 8 This example provides an environmentally friendly high-strength salt film and a preparation method thereof, and the specific implementation manner is the same as that of Example 1, except that the grafting PVC-A is replaced by the same amount of grafting PVC-B.

[0053] Example 9 This example provides an environmentally friendly high-strength salt film and a preparation method thereof, and the specific implementation manner is the same as that of Example 1, except that the grafting PVC-A is replaced by the same amount of grafting PVC-C.

[0054] Comparative Example 1 This example provides an environmentally friendly high-strength salt film and a preparation method thereof, and the specific implementation manner is the same as that of Example 1, except that the grafting PVC-A is replaced by the same amount of grafting PVC-C.

[0055] Comparative Example 2 The comparative example provides an environmentally friendly high-strength salt film and a preparation method thereof, and the specific embodiment is the same as that of Example 1, except that the raw material does not contain the degradation-promoting agent A.

[0056] Performance test 1. Strength test: According to GB / T 529-2008 “Determination of tear strength of vulcanized or thermoplastic rubber”, the salt film (thickness of 1.2 mm) provided by Examples 1-8 was subjected to a right-angle tear strength test.

[0057] 2. Brine immersion migration test: The film sample was immersed in a saturated sodium chloride solution and accelerated aging in an oven at 60°C, and after 7 days, the sample was taken out, the solution was observed whether it became turbid, and the chemical oxygen demand (COD) was tested by AgNO3 precipitation method, and the increase of COD value indicated the presence of organic matter dissolution.

[0058] 3. Degradation test ① Artificial accelerated UV aging test: the salt film provided by Examples 1-8 was placed in a UV aging box (cycle conditions: UVB lamp, 8h UV light at 60°C, 4h condensation at 50°C); the sample was taken out after 600h, and the tensile strength retention rate was tested; ② Compost degradation test: the salt film provided by Examples 1-8 was cut into pieces and mixed with mature compost, and was placed in a biochemical oxygen demand determination bottle and cultured at 58±2°C and 50% humidity for 180 days, the amount of carbon dioxide produced by the reactor was monitored, and the biodegradation rate was calculated by calculating the ratio of the actual amount of carbon dioxide produced to the theoretical amount of carbon dioxide that could be produced (more than 70%, meeting the basic requirements of international “compostable” materials); after the test was completed, the film residue was taken out and the morphological change was observed.

[0059] The test results are shown in Table 1.

[0060] Table 1 Test results As can be seen from the data in Table 1, the right-angle tear strength of the salt film of Examples 1-3 can reach 130-150 kN / m, indicating that the salt film is not easy to be torn when impacted by sharp objects (such as salt stubs), and can effectively resist accidental collisions of salt collection machinery. After being immersed in brine, the brine still remains clear and transparent, and combined with the small change range of the COD value, it indicates that the plasticizers and other auxiliaries used in the salt film are locked in the matrix, and have strong resistance to migration and low pollution to brine.

[0061] In the artificial accelerated ultraviolet aging test, the tensile strength retention rate of the salt film of Example 1-3 is maintained at 92% or more, indicating that the performance decreases slowly and the service life can be effectively prolonged; and in the compost degradation test, the salt film biodegradation rate is more than 80% (meeting the basic requirements of the international "compostable" materials), and is degraded to powder, which is difficult to distinguish with the naked eye; in combination with the two types of degradation tests, it can be known that the salt film provided in the application realizes non-interference on the service life and efficient degradation after being discarded. Compared with Example 1, the degradation promoter of Example 4 lacks manganese source, which is not conducive to the cycle promotion of Fe 3+ →Fe 2+ , resulting in weakened catalysis, although the biodegradation rate decreases, but it also meets the basic requirements of the international "compostable" materials.

[0062] Compared with Example 1, the degradation promoter of Example 5-6 changes the ratio of complex catalyst to PCL in preparation, which may cause incomplete PCL coating or self-aggregation phenomenon, which may expose the metal core, thereby conflicting with ultraviolet absorbers, light stabilizers and the like, thereby reducing the tensile strength retention rate; the metal core of the degradation promoter of Example 7 is not protected by the PCL layer, resulting in further reduction of the tensile strength retention rate.

[0063] Compared with Example 1, Examples 8-9 change the ratio of VCM to maleic anhydride when grafting PVC, which may cause excessive crosslinking or gel, thereby affecting the mechanical properties of the grafted PVC, and the straight tear strength decreases in part. The PVC used in Comparative Example 1 is not grafted with maleic anhydride, which weakens the bonding force between the resin matrix and the plasticizer, filler and the like, although the COD value increases in part, but the solution is still clear and transparent. Comparative Example 2 does not use a degradation promoter, and the weather-resistant additive contained therein has a synergistic plasticizing effect, which makes the tensile strength retention rate decrease slowly, but the biodegradation rate decreases sharply.

[0064] The above-described examples and comparative examples do not limit the application in any form, although the application has been disclosed as above with the preferred embodiments, however, it is not intended to limit the application, any person skilled in the art can make some changes or modifications to the above-mentioned disclosed technical content without departing from the scope of the technical solution of the application, and equivalent embodiments with equivalent changes are obtained, as long as they do not deviate from the technical solution of the application, any simple modification, equivalent change and modification of the above examples according to the technical essence of the application, all still belong to the scope of the technical solution of the application.

Claims

1. An environmentally friendly high-strength salt film, characterized by, By weight parts, comprising the following raw materials: grafting PVC 90-110 parts, environmental plasticizer 35-45 parts, thermal stabilizer 3.0-4.5 parts, benzotriazole ultraviolet absorber 0.3-0.6 parts, hindered amine light stabilizer 0.4-0.8 parts, antioxidant 0.2-0.4 parts, lubricant 0.5-1.5 parts, filler 10-20 parts, prodegradation agent 1-2 parts.

2. The environmentally friendly high strength salt film according to claim 1, characterized in that, The environmental plasticizer comprises epoxy soybean oil and acetyl tributyl citrate.

3. The environmentally friendly high strength salt film according to claim 1, wherein, The preparation steps of the grafting PVC are as follows: The dispersant is dissolved in deionized water, then the pH is maintained at 6.8-7.2 with a pH buffer, vacuum nitrogen replacement is carried out, VCM is added, then maleic anhydride and initiator-DOP solution are added, sealed, stirring is started, and reaction is carried out at 58-64°C until the pressure drops to 0.28-0.32 MPa, then the unreacted VCM is recovered by vacuum flash, and the remaining PVC slurry is washed and vacuum dried to constant weight, thereby obtaining the grafting PVC.

4. The environmentally friendly high strength salt film according to claim 3, characterized in that, The mass ratio of VCM to maleic anhydride is 1:(0.015-0.030).

5. The environmentally friendly high strength salt film according to claim 1, wherein, The thermal stabilizer is a calcium-zinc composite stabilizer.

6. The environmentally friendly high strength salt film according to claim 1, wherein, The filler is active calcium carbonate.

7. The environmentally friendly high strength salt film according to claim 1, wherein, The preparation steps of the prodegradation agent are as follows: S1, 0.5-1.5 mol / L [Fe(EDTA)] is configured respectively - stock solution A and 0.5-1.5 mol / L [Mn(EDTA)] 2- stock solution B, stock solution A and stock solution B are co-spray dried to obtain a complex catalyst powder; S2, a PCL-dichloromethane solution with a concentration of 3-5 wt% is configured, the complex catalyst powder is added thereto, homogenization is carried out at 5-15°C to obtain a suspension, the rotation speed is maintained at 7000-9000 rpm, the suspension is added to the PVA aqueous solution, shearing is carried out for 8-15 min, then the displacement liquid is added thereto until no solid is precipitated, the solid is collected, washed, dried, and sieved, thereby obtaining the prodegradation agent.

8. The environmentally friendly high strength salt film according to claim 7, wherein, In step S1, the volume ratio of the storage solution A to the storage solution B is 1:(0.8-1.2).

9. The environmentally friendly high strength salt film according to claim 7, wherein, In step S2, the mass ratio of PCL to complex catalyst powder is 1:(1-2).

10. A preparation method of the environmental high-strength salt film according to any one of claims 1-9, specifically comprising the following steps: Mixing: the grafting PVC is put into a 100-120°C mixer, the thermal stabilizer, benzotriazole ultraviolet absorber, hindered amine light stabilizer, antioxidant, prodegradation agent, and solid lubricant are added first, mixed for 1-2 min, then the environmental plasticizer is added, and finally the filler is added, mixed for 10-30 min, and cooled to below 40°C by stirring; Extrusion molding: a co-rotating parallel twin-screw extruder equipped with a melt pump and an automatic screen changer is selected to extrude the material; the process parameters of the extruder are as follows: zone 1: 130-140°C, zone 2: 150-160°C, zone 3: 160-170°C, and die head: 165-175°C; Calendering: a clothes hanger type T die is adopted, the material is extruded from the die lip, immediately enters a three-roll calender, the three-roll temperature is as follows: upper roll: 80-90°C, middle roll: 70-80°C, and lower roll: 60-70°C, thereby obtaining the calendered film; Post-treatment: the calendered film passes through a traction roller and enters a cooling roller group, is cooled to room temperature, is wound by an automatic tension control system, and is stored for aging at room temperature after winding, thereby obtaining the environmental high-strength salt film.

Citation Information

Patent Citations

  • A biodegradable slow-release multifunctional agricultural film and its preparation method

    CN107298834B

  • Process for preparing weatherability polyvinyl chloride film containing hindered amine as light stabilizer

    CN1359972A

Cited By

  • Preparation method of benzotriazole needle-like crystal