Method for recovering Si, C and TiO2 based on chlorinated waste brine quenching slag

By employing steps such as water quenching and dissolution, precipitation separation, and fluidized bed separation, Si, C, and TiO2 are recovered from the quenching slag of chlorinated waste brine, thus solving the problem of resource waste, achieving efficient resource recovery and recycling, and reducing environmental risks.

CN121551357APending Publication Date: 2026-02-24PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP

Patent Information

Application Number
CN202511881922.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-12
Publication Date
2026-02-24

AI Technical Summary

Technical Problem

In the existing process of resource recovery from chlorinated waste salts, resources such as Si, C, and TiO2 in the water-quenched slag are seriously wasted, leading to resource waste and environmental risks.

Method used

Through steps such as water quenching and dissolution, precipitation separation, pressure filtration and dehydration, dilute acid dissolution, reducing agent reaction, and fluidized bed separation, petroleum coke and TiO2 in water-quenched slag are recovered. Hydrocyclone classification and enrichment and ceramic membrane concentration technologies are used to achieve the effective utilization of materials such as SiO2.

Benefits of technology

It effectively recovers resources such as TiO2 and C from water-quenched slag, avoids landfill disposal, saves costs, realizes resource recycling, and improves the efficiency and environmental friendliness of resource treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121551357A_ABST
    Figure CN121551357A_ABST
Patent Text Reader

Abstract

The invention provides a method for recovering Si, C and TiO2 based on chlorinated waste salt water quenching slag, which comprises the following steps: sequentially carrying out water quenching dissolution, precipitation separation and filter pressing dehydration treatment on chlorinated waste salt to obtain water quenching slag and supernate; adding a dilute acid solution into the water-quenched slag, dissolving, and adding a reducing agent for reaction to obtain slurry; carrying out solid-liquid separation on the slurry to obtain a solid material and filtrate; the filtrate is pumped into a boiling bed separator, the petroleum coke and TiO2 are intercepted by a medium material layer, clear liquid is discharged, then the medium material layer is subjected to backwashing regeneration, and the desorbed petroleum coke and TiO2 are subjected to graded enrichment by a hydrocyclone, so that petroleum coke slurry and TiO2 slurry are obtained. According to the method, TiO2, C and other resources in the water-quenched slag obtained after molten salt chlorination waste salt water quenching are recycled, and the technical problem that in the existing chlorination waste salt resourceful treatment process, Si, C, TiO2 and other resources in the water-quenched slag are wasted is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of titanium alloy solid waste utilization technology, and in particular to a method for recovering Si, C and TiO2 from quenched slag of chlorinated waste brine. Background Technology

[0002] The process of preparing titanium tetrachloride from titanium slag molten salt chlorination generates high-temperature (700℃~750℃) molten waste salt slag, with a production volume of approximately 400 kg / t TiCl4. The soluble salt content is as high as 80% or more. Currently, the main treatment method is to cool the waste salt slag, neutralize it, and landfill it. Resource-based treatment involves leaching at room temperature, neutralizing and removing impurities, and recovering salt. However, leaching at room temperature is not only time-consuming, but also causes the equipment to easily stick to the slag when cooling the slag using a roller mill-ball mill, resulting in severe corrosion, making continuous operation impossible and hindering engineering applications.

[0003] The existing process of quenching, oxidation, magnesium removal, and brine reuse in molten salt chlorination wastewater treatment has solved the engineering application problems of chlorination wastewater, recovering iron (Fe), magnesium (Mg), manganese (Mn), and sodium chloride (NaCl) resources, achieving the goal of solid waste resource utilization. However, insoluble waste residue (water-quenched slag) still exists during the quenching process of wastewater. Its main components are silicon dioxide (SiO2), titanium dioxide (TiO2), carbon (C), ferric oxide (Fe2O3), aluminum oxide (Al2O3), calcium (Ca), and magnesium (Mg), especially titanium dioxide, which accounts for about 22% to 25%, and most of it exists in the rutile form; at the same time, the slag (wet slag) contains some sodium chloride and Fe. 3+ Fe 2+ If the components are directly disposed of through stockpiling and landfilling, based on the existing resource recovery process, approximately 120 kg of water-quenched slag will be generated for every ton (t) of titanium tetrachloride produced. According to the current titanium tetrachloride production, approximately 5,000 tons of TiO2, approximately 4,000 tons of C, and 10,000 tons of NaCl will be wasted annually.

[0004] CN 113582224 B discloses a method for the resource utilization of molten salt chlorination slag from titanium dioxide waste acid leaching, comprising: water quenching the molten salt chlorination slag with water, adding titanium dioxide waste acid for leaching, and separating to obtain supernatant 1; the supernatant is reduced, crystallized, and separated to obtain a Fe-removed solution; the pH of the Fe-removed solution is adjusted to 5.5-6.0, and separated to obtain supernatant 2; supernatant 2 is separated by nanofiltration to obtain a solution containing Mg and Mn and a solution containing Na, and finally Mg, Mn, and Na are recovered respectively. This prior art co-processes titanium dioxide waste acid and molten salt chlorination slag, and extracts and recovers Sc, Mg, Mn, Ti, Fe, and sodium chloride salts respectively, so as to achieve efficient utilization of resources in the titanium dioxide industry. However, this prior art does not involve the recovery of petroleum coke in the molten salt chlorination slag, and the recovered TiO2 exists in the slag containing SiO2 and CaSO4.

[0005] CN 113816399 A discloses a method for recycling NaCl and recovering Fe, Mn, and Mg resources from titanium slag. The method includes: a) leaching; b) preparing a mixed brine; c) preparing magnesium-removed NaCl brine; d) preparing and drying the NaCl product for reuse in a molten salt chlorination furnace; e) preparing saturated initial brine using an ion-exchange membrane with caustic soda; f) deep reduction and impurity removal; and g) synergistic removal of Mg. 2+ CO3 2- SO4 2- Plasma, h, neutralization filtration for impurity removal, i, deep impurity removal. This existing technology solves the resource utilization problem of molten salt chlorination slag, realizes the recycling of NaCl molten salt chlorination, and also breaks through the balance cycle of Cl element in the molten salt chlorination industry and chlor-alkali chemical industry. However, this existing technology does not recover petroleum coke from molten salt chlorination slag and lacks a specific enrichment and recovery process for TiO2. Based on this, there is room for improvement in terms of the waste of C and TiO2 in the water-quenched slag during the resource recovery process of chlorinated waste salt. Summary of the Invention

[0006] One of the technical problems to be solved by this invention is that the existing waste chlorinated waste salt resource treatment process wastes resources such as Si, C, and TiO2 in the water quenching slag.

[0007] To address the aforementioned technical problems, embodiments of the present invention provide a method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine, comprising: Step 1: The chloride waste salt is subjected to water quenching and dissolution, precipitation and separation, and pressure filtration and dehydration treatment in sequence to obtain water quenching residue and supernatant; Step 2: Add dilute acid solution to the water-quenched slag, dissolve it, and then add a reducing agent to react and obtain a slurry; Step 3: Perform solid-liquid separation on the slurry to obtain solid material and filtrate; Step 4: The filtrate is fed into a fluidized bed separator. After the petroleum coke and TiO2 are intercepted by the medium layer, the clear liquid is discharged. Then the medium layer is backwashed and regenerated. The desorbed petroleum coke and TiO2 are classified and enriched by a hydrocyclone to obtain petroleum coke slurry and TiO2 slurry.

[0008] In one embodiment, in step 1, the chlorinated waste salt at 650℃~720℃ is dispersed by high-speed water flow and then quickly quenched and dissolved. After quenching, the liquid is transported to the first sedimentation tank by a slag pump. The undissolved slag and some iron hydroxide form a slag-containing slurry in the lower layer of the first sedimentation tank. The upper layer of the first sedimentation tank is the supernatant. The slag-containing slurry is pumped to the first plate and frame filter press for dewatering to obtain water-quenched slag. The supernatant can be recycled.

[0009] In one embodiment, the mass ratio of water used for quenching to waste chloride salt is 16-20:1. The supernatant is used as a water source for quenching the waste chloride salt until the Cl in the supernatant in the first sedimentation tank is reduced. - Once the concentration is greater than or equal to the predetermined concentration, the supernatant undergoes downstream resource recovery processing.

[0010] In one embodiment, in step 2, the water-quenched slag is transferred to a pulping tank, and a dilute acid solution is added to the pulping tank at a mass ratio of 3 to 3.5:1 between the dilute acid solution and the water-quenched slag. After stirring and dissolving, a reducing agent is added, and the reduction reaction is carried out for 5 to 10 minutes to obtain a slurry.

[0011] In one embodiment, the reducing agent is iron powder, and the iron powder reacts with Fe in the dissolution system after dissolution in the pulping tank. 3+ The molar ratio is 1.02 to 1.05:2.

[0012] In one embodiment, in step 3, the slurry is fed into a second plate and frame filter press under stirring to perform solid-liquid separation by pressing and washing, resulting in solid material and filtrate, the filtrate carrying petroleum coke and TiO2.

[0013] In one embodiment, in step 4, the filtrate is fed into a fluidized bed separator. Under the boiling flow of the medium layer, the petroleum coke and TiO2 in the filtrate are gradually intercepted. The clear liquid is discharged through the filter layer to the second sedimentation tank. When the filtration pressure difference is greater than or equal to 0.2 MPa, the filtrate feed is stopped, and the medium layer is backwashed and regenerated. Under the synergistic effect of the backwash airflow and backwash water flow and the rotation of the filter media, the petroleum coke and TiO2 on the surface of the filter media are desorbed. The desorbed petroleum coke and TiO2 rise with the backwash water to the top hydrocyclone, realizing the graded enrichment of petroleum coke and TiO2. The enriched petroleum coke product and the enriched titanium dioxide product are discharged to the corresponding recovery tanks to obtain petroleum coke slurry and TiO2 slurry. The medium layer is composed of filter media.

[0014] In one embodiment, backwashing and regeneration uses compressed air and fresh water, with the volume ratio of compressed air to filter media being 2.0 to 2.5:1 and the volume ratio of fresh water to filter media being 2.0 to 3.0:1.

[0015] In one embodiment, the method includes: step 5, processing the petroleum coke slurry and TiO2 slurry, sending the petroleum coke slurry to the raw material petroleum coke grinding system as raw material for later use, further concentrating the TiO2 slurry using a ceramic membrane, and doping the obtained TiO2 concentrate into titanium concentrate, which is then used directly as raw material in the chlorination furnace.

[0016] In one embodiment, the clarified liquid from step 4 is recycled or returned to the backend resource recovery system to simultaneously recover ferric hydroxide.

[0017] Through the above technical solution, the method for recovering Si, C and TiO2 from quenched slag based on chlorinated waste brine provided by the present invention recovers resources such as TiO2 and C from the water-quenched slag obtained after quenching molten salt chlorinated waste brine, and materials containing SiO2 and other materials can be effectively utilized, avoiding the risk of water-quenched slag stockpiling and saving the cost of stockpiling, and solving the technical problem of wasting Si, C and TiO2 resources in water-quenched slag in the existing chlorinated waste salt resource utilization process. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 This is a flowchart of a method for recovering Si, C, and TiO2 from quenched slag based on chlorinated waste brine, as disclosed in an embodiment of the present invention. Detailed Implementation

[0020] The embodiments of the present invention will be further described in detail below with reference to the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to illustrate the principles of the present invention by way of example, but should not be used to limit the scope of the present invention. The present invention can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

[0021] These embodiments are provided to make the invention thorough and complete, and to fully express the scope of the invention to those skilled in the art. Terms such as "comprising" or "including" mean that the element preceding the term encompasses the element listed after the term, and do not exclude the possibility of encompassing other elements. Furthermore, the terms "first," "second," and similar terms used in this invention do not indicate any order, quantity, or importance, but are merely used to distinguish different parts.

[0022] All terms used in this invention have the same meaning as understood by one of ordinary skill in the art to which this invention pertains, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries should be interpreted as having meanings consistent with their meanings in the context of the relevant art, and not as idealized or highly formalized, unless expressly defined herein.

[0023] Techniques, methods, and equipment known to those skilled in the art may not be discussed in detail, but where appropriate, they should be considered part of the specification.

[0024] Reference Figure 1 The present invention provides a method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine, comprising the following steps: Step 1: The chloride waste salt is subjected to water quenching and dissolution, precipitation and separation, and pressure filtration and dehydration treatment in sequence to obtain water quenching residue and supernatant; Step 2: Add dilute acid solution to the water-quenched slag, dissolve it, and then add a reducing agent to react and obtain a slurry; Step 3: Perform solid-liquid separation on the slurry to obtain solid material and filtrate; Step 4: The filtrate is fed into a fluidized bed separator. After the petroleum coke and TiO2 are intercepted by the medium layer, the clear liquid is discharged. Then the medium layer is backwashed and regenerated. The desorbed petroleum coke and TiO2 are classified and enriched by a hydrocyclone to obtain petroleum coke slurry and TiO2 slurry.

[0025] Compared with existing technologies, the method of the present invention for recovering Si, C and TiO2 from quenched slag of chlorinated waste brine can recover resources such as TiO2 and C from the water-quenched slag obtained after quenching molten salt chlorinated waste brine, and materials containing SiO2 can be effectively utilized. This avoids the risk of water-quenched slag stockpiling and saves the cost of stockpiling, thus solving the technical problem of wasting Si, C and TiO2 resources in water-quenched slag in the existing chlorinated waste salt resource utilization process.

[0026] In one embodiment, the chlorinated waste salt is waste salt produced by any of the chlorination processes, namely molten salt chlorination and fluidized bed chlorination. For example, the chlorinated waste salt is high-temperature molten waste salt slag discharged from a molten salt chlorination furnace. The chlorinated waste salt includes the following components: FeCl2, FeCl3, MgCl2, MnCl2, CaCl2, AlCl3, NaCl, TiO2, SiO2, and petroleum coke, wherein FeCl2, FeCl3, MgCl2, MnCl2, CaCl2, AlCl3, and NaCl are chloride salts. The main component of petroleum coke is carbon (C).

[0027] In one embodiment, in step 1, the chloride waste salt at 650℃~720℃ is rapidly dissolved by high-speed water flow after being dispersed. The quenched solution is then pumped to a first sedimentation tank. Undissolved slag and some ferric hydroxide (Fe(OH)3) form a slag-containing slurry in the lower layer of the first sedimentation tank, while the upper layer is the supernatant. The slag-containing slurry is pumped to a first plate and frame filter press for dewatering. After unloading from the first plate and frame filter press, water-quenched slag is obtained, and the supernatant can be recycled. The water-quenched slag includes undissolved slag and some ferric hydroxide. The undissolved slag includes the original water-insoluble components of the chloride waste salt (such as SiO2, TiO2, and petroleum coke) and Ca from the chloride waste salt quenching system during the water quenching process. 2+ Al 3+ Mg 2+Secondary precipitates such as calcium aluminum magnesium silicate ((Ca,Al,Mg)SiO3) are formed by the reaction with trace amounts of silicates. In addition, the water-quenched slag carries some chloride salts. The supernatant is a brine solution, which is recycled as wash water for quenching the chloride wastewater until the chloride content in the supernatant of the first sedimentation tank is reduced. - Once the concentration reaches or equals a predetermined concentration, the supernatant is used as qualified crude brine for downstream resource recovery. The predetermined concentration is 210 g / L. When the Cl in the supernatant... - A concentration greater than or equal to 210 g / L and a salt water density greater than 1.24 g / cm³ 3 At that time, the supernatant was qualified crude brine. During the process of using the supernatant for circulating water quenching, the pH of the supernatant gradually decreased from 7.0 to around 1.0. When the pH of the supernatant was greater than 2.2, the Fe in the supernatant... 3+ Some Fe(OH)3 precipitate will be generated. The filter cloth pore size of the first plate and frame filter press is 20μm~25μm. A high-temperature circulating water quenching process is used to treat the chloride waste salt. After water quenching, the quenched slag and solution undergo solid-liquid separation. The resulting supernatant is returned for circulating water quenching until it meets the requirements, and then undergoes downstream resource recovery treatment. The supernatant contains Fe... 3+ Fe 2+ Al 3+ Mn 2+ Mg 2 + Ca 2+ Cl - Na + Plasma. Step 1 is achieved through a water flushing system, a brine circulation system, and a slag discharge system.

[0028] In one embodiment, the water used for quenching includes fresh water, supernatant, and / or other wash water generated from subsequent treatment. The mass ratio of the water used for quenching to the waste chloride salt is 16–20:1.

[0029] In one embodiment, after pressure filtration and dehydration, the main components of the water-quenched slag are: NaCl, SiO2, TiO2, petroleum coke, Fe(OH)3, calcium aluminum magnesium silicate ((Ca,Al,Mg)SiO3), and trace impurities, wherein the mass content of NaCl is 52%~56%, the mass content of SiO2 is 15%~18%, the mass content of petroleum coke is 10%~12%, the mass content of TiO2 is 8%~10%, the mass content of Fe(OH)3 is 6%~10%, the mass content of calcium aluminum magnesium silicate ((Ca,Al,Mg)SiO3) is 1.5%~5%, and the mass content of trace impurities is ≤1%.

[0030] In one embodiment, in step 2, the water-quenched slag is transferred to a pulping tank. A dilute acid solution is added to the pulping tank at a mass ratio of 3-3.5:1 (dilute acid solution to water-quenched slag). After stirring and dissolving, a reducing agent is added, and the reduction reaction is carried out for 5-10 minutes to obtain a slurry. The dilute acid solution is a dilute hydrochloric acid solution with an HCl mass fraction of 1.0%-2.0%. The reducing agent is iron powder, which reacts with the Fe in the dissolved system after dissolution in the pulping tank. 3+ The molar ratio is 1.02–1.05:2. Commercially available qualified iron powder is used, with a purity ≥92% and a mesh size of 80–100 mesh. Dilute hydrochloric acid solution reacts with Fe(OH)3 in the water-quenched slag to produce Fe. 3+ Ions, while simultaneously dissolving some of the chloride salts carried in the water-quenched slag and releasing Fe. 3+ (from FeCl3), Fe 2+ (from FeCl2), Al 3 + Mn 2+ Mg 2+ Ca 2+ Cl - Na + Plasma, all ions enter the dissolution system, and Fe is removed by adding iron powder. 3+ Reduced to Fe 2+ The reaction formula is 2Fe 3+ +Fe=3Fe 2+ Iron powder and Fe in the dissolved system 3+ The theoretical molar ratio should be 1:2. A slight excess of iron powder is used to ensure that Fe... 3+ Complete reduction, and because iron powder preferentially reacts with Fe. 3+ The reaction will not introduce additional impurities or leave residues in the slag.

[0031] In one embodiment, in step 3, the slurry is fed into a second plate and frame filter press under stirring for solid-liquid separation through filtration and washing, yielding solid material and filtrate. The filtrate carries fine particles of petroleum coke and TiO2, and is transported to a storage tank as raw material for the next process. The solid material mainly consists of coarse particles of SiO2 and calcium aluminum magnesium silicate ((Ca,Al,Mg)SiO3), with a SiO2 mass content ≥90%. The solid material can be directly used as filter media for multi-media filters or as other intermediate raw materials after drying, crushing, and sieving. Fresh water is used for washing. Fresh water is also known as clean water. The second plate and frame filter press is fully automatic, equipped with filter cloth with a pore size of 20μm to 25μm, a filtration pressure of ≤0.6Mpa, and a two-stage washing process. After washing, the discharged wash water, once tested and deemed compliant, is reused as a dilution acid solution. The entire process, including filter plate pressing, pressurized feeding, washing, filter cake pressing, and filter plate unloading, is fully automated, efficiently retaining coarse solid particles. The filtrate is then transported to a storage tank. The slurry is fed into the second plate and frame filter press under stirring at a speed of 80r / min to 120r / min. This process achieves the separation of coarse and fine particles through the control of the filter cloth pore size in the second plate and frame filter press. Impurity ions are removed through water washing, and the water-quenched slurry undergoes solid-liquid separation and recovery to obtain filtrate containing fine TiO2 particles, fine petroleum coke particles, and solids.

[0032] In one embodiment, in step 4, the filtrate is fed into a fluidized bed separator. Under the boiling flow of the media layer, fine petroleum coke and fine TiO2 particles in the filtrate are gradually intercepted. The clarified liquid is discharged through the filter layer to the second sedimentation tank. When the filtration pressure difference is greater than or equal to 0.2 MPa, the filtrate feed is stopped, and the media layer is backwashed and regenerated. Under the synergistic effect of the backwash airflow, backwash water flow, and filter media rotation, fine petroleum coke and fine TiO2 particles are desorbed from the filter media surface. The desorbed fine petroleum coke and fine TiO2 particles rise with the backwash water to the top hydrocyclone for fractional enrichment. The enriched petroleum coke product and enriched titanium dioxide product are discharged to the corresponding recovery tanks, respectively, to obtain petroleum coke slurry and TiO2 slurry. The media layer is composed of filter media. After drying, the carbon content of the petroleum coke slurry is ≥98%. Filtration pressure differential refers to the difference between the inlet and outlet pressures of a fluidized bed separator. Fluidized bed separators are commercially available equipment, equipped with one or more hydrocyclones connected in parallel at the top. The bed media consists of wear-resistant particles with a particle size of 0.5 mm to 1.0 mm. During normal operation, the filtration pressure differential is controlled to not exceed 0.2 MPa. The hydrocyclones are made of wear-resistant materials such as polyurethane, with a cone angle of 10° to 20°, a pressure of 0.1 MPa to 0.3 MPa, and a separation particle size of 1 μm to 300 μm. Backwashing and regeneration use compressed air and fresh water, with a compressed air to filter media volume ratio of 2.0 to 2.5:1 and a fresh water to filter media volume ratio of 2.0 to 3.0:1. Under the rapid swirling action of the hydrocyclones, petroleum coke and TiO2 are fractionally enriched through centrifugal force and discharged from the hydrocyclone overflow port (petroleum coke, light phase) and underflow port (TiO2, heavy phase), respectively. This process uses a fluidized bed separator to separate petroleum coke and TiO2, which are then either recycled separately or centrally dried and used together in a chlorination furnace. The clarified liquid obtained from the fluidized bed separator contains a small amount of impurity ions and can be returned as the first-stage washing liquid in step 3 for further washing.

[0033] In one embodiment, the clarified liquid from step 4 is either recycled or returned to the downstream resource recovery system for simultaneous recovery of ferric hydroxide. When the HCl mass concentration in the clarified liquid is greater than or equal to 1%, the clarified liquid can be recycled to dissolve water-quenched slag to ensure the dissolution effect; when the HCl mass concentration in the clarified liquid is less than 1%, the Fe concentration in the clarified liquid is relatively high, and the clarified liquid is directly sent to the downstream resource recovery system for iron precipitation recovery. After removing impurities such as iron, the brine is NaCl brine, which is further evaporated and crystallized by mechanical vapor recompression (MVR) to recover NaCl salt.

[0034] In some embodiments, the method of the present invention for recovering Si, C and TiO2 from quenched slag of chlorinated waste brine includes: step 5, processing petroleum coke slurry and TiO2 slurry, sending the petroleum coke slurry to the raw material petroleum coke grinding system as raw material for later use, further concentrating the TiO2 slurry using a ceramic membrane, and doping the obtained TiO2 concentrate into titanium concentrate, which is then used directly as raw material in the chlorination furnace, wherein the TiO2 concentrate has a TiO2 mass content ≥85% after drying.

[0035] In one embodiment, the ceramic membrane is a tubular ceramic membrane or a flat ceramic membrane, and the material is one of silicon carbide, titanium, or polyphenylene sulfide (PPS), with a filtration pore size of 40nm to 100nm and a filtration pressure of ≤0.2Mpa.

[0036] The method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine according to the present invention is specifically implemented as follows: high-temperature molten waste salt slag discharged from a molten salt chlorination furnace is used as chlorinated waste salt. Example 1 Chlorinated waste salt at around 700℃ is quenched by high-speed flushing water with a water-to-chlorinated waste salt mass ratio of 18. After quenching, the liquid is pumped to the first sedimentation tank. Undissolved slag and some ferric hydroxide form a slag-containing slurry in the lower layer of the first sedimentation tank. The slag-containing slurry is then pumped to the first plate and frame filter press for dewatering. The filter cloth of the first plate and frame filter press has a pore size of 20μm to 25μm. The main components of the water-quenched slag are shown in Table 1.

[0037] Table 1. Composition analysis results of water-quenched slag / %

[0038] The water-quenched slag and a 2.0% HCl solution were added to the pulping tank at a mass ratio of 1:3. After stirring and dissolving, the iron powder and Fe in the dissolved system were added together. 3+ Iron powder was added as a reducing agent at a molar ratio of 1.02:2 for a reduction reaction. The reaction time was controlled at 10 min. After the reaction, the slurry was fed into a second plate and frame filter press under stirring for filtration and two washings to obtain solid material and filtrate. The main components of the dried solid material are shown in Table 2. It can be used as filter material for multi-media filters or other intermediate raw materials.

[0039] Table 2. Analysis results of solid composition of dried material / %

[0040] The filtrate is fed into a fluidized bed separator. Under the boiling flow of the medium layer, fine petroleum coke and fine TiO2 particles in the filtrate are gradually intercepted, and the clear liquid is discharged. When the filtration pressure difference is greater than or equal to 0.2 MPa, the filtrate feed is stopped, and the filter media is backwashed and regenerated. The volume ratio of compressed air to filter media and the volume ratio of fresh water to filter media for backwashing are both 2.0:1. After cyclone separation by the top hydrocyclone, the enriched petroleum coke product and the enriched titanium dioxide product are discharged to the corresponding recovery tanks, respectively, to obtain petroleum coke slurry and TiO2 slurry. The petroleum coke slurry is sampled, dried, and analyzed for carbon content. Its carbon content reaches 98.3%, and it can be incorporated into the raw petroleum coke grinding system. The TiO2 slurry is further concentrated using a flat-plate ceramic membrane, sampled, and dried. Its main components are shown in Table 3. The obtained TiO2 concentrate is incorporated into titanium concentrate and used directly as a raw material in the chlorination furnace.

[0041] Table 3. Component analysis results of dried TiO2 concentrate / %

[0042] The clarified liquid discharged from the fluidized bed separator was analyzed. When the HCl concentration in the clarified liquid was greater than or equal to 1%, the clarified liquid was returned to the water-quenched slag pulping tank to continue dissolving the water-quenched slag, while a small amount of fresh dilute hydrochloric acid solution was added to the pulping tank. When the HCl concentration in the clarified liquid was less than 1%, the Fe concentration was 13 g / L. The clarified liquid underwent downstream resource recovery treatment. By adjusting the pH and adding a precipitant, Fe was precipitated into Fe(OH)2 and Fe(OH)3. After drying, the Fe grade was 38%, which could be added to iron concentrate or steelmaking cooling pellets for utilization. At the same time, the NaCl brine obtained after removing iron, magnesium, etc., was evaporated and crystallized by MVR and separated. The composition of the obtained NaCl salt is shown in Table 4, which can be directly applied to the chlor-alkali system.

[0043] Table 4. Analysis results of NaCl salt composition separated by crystallization / %

[0044] Example 2 Chlorinated waste salt at around 700℃ is quenched by high-speed flushing water with a water-to-chlorinated waste salt mass ratio of 16. After quenching, the liquid is pumped to the first sedimentation tank. Undissolved slag and some ferric hydroxide form a slag-containing slurry in the lower layer of the first sedimentation tank. The slag-containing slurry is then pumped to the first plate and frame filter press for dewatering. The filter cloth of the first plate and frame filter press has a pore size of 20μm to 25μm. The main components of the water-quenched slag are shown in Table 5.

[0045] Table 5. Composition analysis results of water-quenched slag / %

[0046] The water-quenched slag and a 1.0% HCl dilute hydrochloric acid solution were added to the pulping tank at a mass ratio of 1:3.5. After stirring and dissolving, the iron powder and Fe in the dissolved system were added together. 3+ Iron powder was added as a reducing agent at a molar ratio of 1.02:2 for a reduction reaction. The reaction time was controlled at 8 minutes. After the reaction, the slurry was fed into a second plate and frame filter press under stirring for filtration and two washings to obtain solid material and filtrate. The main components of the dried solid material are shown in Table 6. It can be used as filter material for multi-media filters or other intermediate raw materials.

[0047] Table 6. Analysis results of solid composition after drying / %

[0048] The filtrate is fed into a fluidized bed separator. Under the boiling flow of the medium layer, fine petroleum coke and fine TiO2 particles in the filtrate are gradually intercepted, and the clear liquid is discharged. When the filtration pressure difference is greater than or equal to 0.2 MPa, the filtrate feed is stopped, and the filter media is backwashed and regenerated. The volume ratio of compressed air to filter media and the volume ratio of fresh water to filter media for backwashing are both 2.5:1. After cyclone separation by the top hydrocyclone, the enriched petroleum coke product and the enriched titanium dioxide product are discharged to the corresponding recovery tanks, respectively, to obtain petroleum coke slurry and TiO2 slurry. The petroleum coke slurry is sampled, dried, and analyzed for carbon content. Its carbon content reaches 98.6%, which can be incorporated into the raw petroleum coke grinding system. The TiO2 slurry is further concentrated using a flat ceramic membrane, sampled, and dried. Its main components are shown in Table 7. The obtained TiO2 concentrate is incorporated into titanium concentrate and used directly as a raw material in the chlorination furnace.

[0049] Table 7. Component analysis results of dried TiO2 concentrate / %

[0050] The clarified liquid discharged from the fluidized bed separator was analyzed. When the HCl concentration in the clarified liquid was greater than or equal to 1%, the clarified liquid was returned to the water-quenched slag pulping tank to continue dissolving the water-quenched slag, while a small amount of fresh dilute hydrochloric acid solution was added to the pulping tank. When the HCl concentration in the clarified liquid was less than 1%, the Fe concentration was 16 g / L. The clarified liquid underwent downstream resource recovery treatment. By adjusting the pH and adding a precipitant, Fe was precipitated into Fe(OH)2 and Fe(OH)3. After drying, the Fe grade was 40.2%, which could be added to iron concentrate or steelmaking cooling pellets for utilization. At the same time, the NaCl brine obtained after removing iron, magnesium, etc., was evaporated and crystallized by MVR and separated. The composition of the obtained NaCl salt is shown in Table 8, which can be directly applied to the chlor-alkali system.

[0051] Table 8. Analysis results of NaCl salt composition separated by crystallization / %

[0052] This invention relates to a method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine, and to a method for recovering Ti resources from quenched slag of chlorinated waste brine, as well as a comprehensive utilization approach for C and Si resources. This method is applicable to the resource-based treatment of waste salt generated from molten salt chlorination processes. The process includes: pre-treatment with chlorinated waste brine quenching, where soluble resources such as Fe, Mn, Mg, Na, and Cl in the chlorinated waste brine are dissolved in water through a water quenching process; the quenched slag is dissolved and slurried in a dilute acid solution; and Fe... 3+ This invention utilizes an integrated technical route combining acid washing, water washing, aeration cyclone filtration, membrane filtration, and plate and frame filter press to achieve multi-resource graded recovery. Cyclone separation recovers petroleum coke and TiO2, bottom material filter press recovers SiO2 and quartz sand, and the filtrate recovers Fe, Mg, and NaCl resources. Water-quenched slag undergoes further recovery of residual Fe and Na through step-by-step washing via filter press. No additional organic reagents are added throughout the process. The recovered TiO2, C, and NaCl salts can be directly returned to the molten salt chlorination furnace for resource recycling. This improves the clean production and utilization level of the molten salt chlorination process while reducing production costs and the environmental risks of landfilling waste salt and water-quenched slag. This method can be widely applied in the treatment of waste salt from titanium slag molten salt chlorination processes and in the resource utilization of waste in areas similar to chlorinated waste salt.

[0053] The various embodiments of the present invention have now been described in detail. To avoid obscuring the concept of the invention, some details known in the art have not been described. Those skilled in the art will fully understand how to implement the technical solutions disclosed herein based on the above description.

[0054] While specific embodiments of the present invention have been described in detail by way of examples, those skilled in the art should understand that the above examples are for illustrative purposes only and are not intended to limit the scope of the invention. Those skilled in the art should understand that modifications can be made to the above embodiments or equivalent substitutions can be made to some technical features without departing from the scope and spirit of the invention. In particular, as long as there is no structural conflict, the various technical features mentioned in the embodiments can be combined in any manner.

Claims

1. A method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine, characterized in that, Includes the following steps: Step 1: The chloride waste salt is subjected to water quenching and dissolution, precipitation and separation, and pressure filtration and dehydration treatment in sequence to obtain water quenching residue and supernatant; Step 2: Add a dilute acid solution to the water-quenched slag, dissolve it, and then add a reducing agent to react and obtain a slurry; Step 3: Perform solid-liquid separation on the slurry to obtain solid material and filtrate; Step 4: The filtrate is fed into a fluidized bed separator. After the petroleum coke and TiO2 are intercepted by the medium layer, the clear liquid is discharged. Then, the medium layer is backwashed and regenerated. The desorbed petroleum coke and TiO2 are classified and enriched by a hydrocyclone to obtain petroleum coke slurry and TiO2 slurry.

2. The method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine according to claim 1, characterized in that, In step 1, the chlorinated waste salt at 650℃~720℃ is rapidly dissolved by high-speed water flow after being dispersed. The quenched liquid is then pumped to the first sedimentation tank by a slag pump. Undissolved slag and some ferric hydroxide form a slag-containing slurry in the lower layer of the first sedimentation tank. The upper layer of the first sedimentation tank is the supernatant. The slag-containing slurry is pumped to the first plate and frame filter press for dewatering to obtain water-quenched slag. The supernatant can be recycled.

3. The method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine according to claim 2, characterized in that, The mass ratio of quenching water to the chloride waste salt is 16-20:

1. The supernatant is used as a water source for quenching the chloride waste salt until the Cl in the supernatant in the first sedimentation tank is reduced. - Once the concentration is greater than or equal to a predetermined concentration, the supernatant undergoes downstream resource recovery processing.

4. The method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine according to claim 1, characterized in that, In step 2, the water-quenched slag is transferred to a pulping tank. The dilute acid solution is added to the pulping tank at a mass ratio of 3 to 3.5:1 between the dilute acid solution and the water-quenched slag. After stirring and dissolving, a reducing agent is added, and the reduction reaction is carried out for 5 to 10 minutes to obtain the slurry. The dilute acid solution is a dilute hydrochloric acid solution, and the mass fraction of HCl in the dilute hydrochloric acid solution is 1.0% to 2.0%.

5. The method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine according to claim 4, characterized in that, The reducing agent is iron powder, and the iron powder reacts with the Fe in the dissolution system after dissolution in the pulping tank. 3+ The molar ratio is 1.02 to 1.05:

2.

6. The method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine according to claim 1, characterized in that, In step 3, the slurry is fed into a second plate and frame filter press under stirring to perform solid-liquid separation by pressing, washing, and obtaining the solid material and the filtrate, wherein the filtrate carries the petroleum coke and the TiO2.

7. The method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine according to claim 1, characterized in that, In step 4, the filtrate is fed into a fluidized bed separator. Under the boiling flow of the medium layer, the petroleum coke and TiO2 in the filtrate are gradually intercepted. The clear liquid is discharged through the filter layer to the second sedimentation tank. When the filtration pressure difference is greater than or equal to 0.2 MPa, the filtrate feed is stopped, and the medium layer is backwashed and regenerated. Under the synergistic effect of the backwash airflow and backwash water flow and the rotation of the filter media, the petroleum coke and TiO2 on the surface of the filter media are desorbed. The desorbed petroleum coke and TiO2 rise with the backwash water to the top hydrocyclone, realizing the graded enrichment of petroleum coke and TiO2. The enriched petroleum coke product and the enriched titanium dioxide product are discharged into the corresponding recovery tanks to obtain the petroleum coke slurry and the TiO2 slurry. The medium layer is composed of filter media.

8. The method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine according to claim 7, characterized in that, The backwashing and regeneration process uses compressed air and fresh water, with the volume ratio of compressed air to filter media being 2.0 to 2.5:1 and the volume ratio of fresh water to filter media being 2.0 to 3.0:

1.

9. The method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine according to claim 1, characterized in that, include: Step 5: Process the petroleum coke slurry and the TiO2 slurry. Send the petroleum coke slurry to the raw material petroleum coke grinding system as raw material for later use. Further concentrate the TiO2 slurry using a ceramic membrane. The resulting TiO2 concentrate is mixed into titanium concentrate and used directly as raw material in the chlorination furnace.

10. The method for recovering Si, C, and TiO2 from quenched slag of chlorinated waste brine according to claim 1, characterized in that, The clarified liquid from step 4 can be recycled or returned to the back-end resource recovery system to simultaneously recover ferric hydroxide.

Citation Information

Patent Citations

  • Methods for the resource utilization of titanium dioxide waste acid leaching molten salt chlorination slag

    CN113582224B

  • Method for recycling NaCl and simultaneously recovering Fe, Mn and Mg resources in titanium slag

    CN113816399A

Cited By

  • Method for preparing high-purity silica powder and titanium dioxide based on chlorinated waste brine quenching slag

    CN122144782A

  • Method for preparing silicon micro-powder based on chlorinated waste brine quenched slag in-situ carbon thermal reduction

    CN122254520A