Anionic polymer containing oxygenated fluorene polyarylate pendant side chains
By designing an oxygen-containing fluorene polyaryl suspended side-chain anion exchange polymer, the problems of alkali resistance and ionic conductivity of anion exchange membranes in high-alkali environments were solved, achieving efficient ion transport and improved mechanical properties under strong alkaline conditions.
Patent Information
- Application Number
- CN202610446320.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-04-07
- Publication Date
- 2026-06-26
AI Technical Summary
Existing anion exchange membranes are not alkali-resistant enough in high-temperature, high-concentration, and strong alkaline environments, and are easily degraded, leading to rapid decay of ionic conductivity and deterioration of mechanical properties, making it difficult to meet the requirements for long-term stable operation.
An oxygen-containing fluorene polyaryl suspended side-chain anionic polymer was used to construct an efficient ion transport channel by introducing an oxygen fluorene structure and a suspended side-chain strategy. By combining the hydrophilicity regulation of the main chain with the functional optimization of the suspended side chain, the alkali resistance and ionic conductivity of the membrane material were improved.
At 80℃, the hydroxide ion conductivity of the anion exchange membrane can reach up to 170.2 mS/cm, maintaining good mechanical properties. The dry membrane has excellent tensile strength and exhibits minimal conductivity loss after immersion in a strong alkaline solution at 80℃ for more than 1800 hours, demonstrating excellent alkali resistance and durability.
Smart Images

Figure CN122277846A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer technology, and specifically discloses an oxygen-containing fluorene polyaryl suspended side-chain anionic polymer. Background Technology
[0002] In recent years, water electrolysis for hydrogen production and hydrogen energy utilization technologies have become highly promising pathways for building a sustainable energy system. Among these, water electrolyzers and fuel cells based on anion exchange membranes (AEMs) can efficiently and cost-effectively convert green electricity into clean hydrogen energy, thereby achieving the interconversion of electrical and chemical energy. In these devices, the AEM serves as a core component, physically separating the anode and cathode to prevent direct mixing of fuel and oxidant, ensuring safe and stable operation. Furthermore, it provides a continuous and efficient transport channel for hydroxide ions, ensuring the continuous progress of electrode reactions and maintaining charge balance within the battery. Compared to the relatively mature proton exchange membrane (PEM) system, AEMs offer numerous irreplaceable advantages under alkaline conditions: not only are oxygen reduction reaction kinetics faster and electrode reactions more efficient, but more importantly, they eliminate the high dependence on precious metal catalysts such as platinum and iridium, significantly reducing the overall manufacturing cost and the barriers to industrial application.
[0003] Existing anion exchange membranes still suffer from insufficient alkali resistance: under high temperature and high concentration of strong alkali environments, the cation exchange sites inside the membrane are susceptible to OH-. - Degradation occurs due to nucleophilic attack and Hoffmann elimination reactions, while the polymer backbone is prone to breakage or segment oxidation, leading to a rapid decline in ionic conductivity and deterioration of mechanical properties, making it difficult to meet the requirements for long-term stable operation. Therefore, further improving the alkali resistance of polyaryl suspended anion exchange membranes is a core and necessary requirement for promoting their industrial application.
[0004] Considering the performance regulation mechanism of anion exchange membranes, the alkali resistance of membrane materials depends primarily on their internal microstructure's response to hydroxide ions (OH-). - The ability to block osmosis and the precise control of local alkali concentration. If the effective alkali concentration in the micro-region where the cation functional groups are located can be effectively reduced, the OH- ionization can be weakened at its source. - Nucleophilic attack and degradation of functional groups further enhance the alkali resistance of membrane materials. Furthermore, the ion conductivity of membrane materials mainly relies on the orderly aggregation of cationic groups on the suspended side chains and the construction of continuous ion transport channels. Therefore, there is an inherent trade-off between ionic conductivity and alkaline stability; a single structural modification cannot simultaneously achieve both core properties. Thus, there is an urgent need to develop a synergistic modification strategy that couples the regulation of main-chain hydrophilicity with the optimization of suspended side chain function to achieve simultaneous improvement in alkali resistance and ionic conductivity. Simultaneously, the technology should facilitate the large-scale mass production of anion exchange membranes. Summary of the Invention
[0005] To address the problems existing in the prior art, the first aspect of the present invention proposes an oxygen-containing fluorene polyaryl suspended side-chain anionic polymer, characterized in that the oxygen-containing fluorene polyaryl suspended side-chain anionic polymer includes structural unit I and / or structural unit II; , ; Z1 and Z2 are each independently selected from , , , ; R1, R2, and R3 are each independently selected from hydrogen, substituted or unsubstituted branched alkyl, substituted or unsubstituted branched alkyl, substituted or unsubstituted piperidinyl, and substituted or unsubstituted aryl. The ring Ar is selected from , The plurality of R b Each of the X molecules is independently selected from any of the branched alkyl groups (C3 to C10) or the straight-chain alkyl groups (C1 to C10) that are substituted or unsubstituted. - Selected from anions.
[0006] In some first aspect embodiments, R1, R2, and R3 are each independently selected from alkyl, hydrogen, and alkyl groups substituted with one or more halogens. The X - Selected from anions, the plurality of R c Each is independently selected from any branched alkyl group (C3 to C10) or a straight alkyl group (C1 to C10) that is substituted or unsubstituted; The n is selected from any positive integer from 1 to 5; Preferably, the R b and R c Each is independently selected from methyl, ethyl, and isopropyl, wherein X - Selected from OH - .
[0007] In some first aspect embodiments, the oxygen-containing fluorene polyaryl suspended side-chain anionic polymer structure is any one of I-a, I-b, I-c, and I-d; , , , ; The x5 is selected from 0.15 to 0.45; the x6 is selected from 0.6 to 0.9; R1, R2, R3, and Ar are defined as in any of the first aspects.
[0008] In some first-aspect embodiments, the oxygen-containing fluorene polyaryl suspended side-chain anionic polymer structure is such as II-e; ; R1, R2, R3, and Ar are defined as in any of the first aspects.
[0009] In the II-e structure, the sum of x1 and x3 satisfies 0.1≤x1+x3≤0.4; and / or, the sum of x2 and x4 satisfies 0.5≤x2+x4≤0.9; and / or, the sum of x1 and x4 satisfies 0.70≤x1+x4≤0.95; and / or, the sum of x2 and x3 satisfies 0.05≤x2+x3≤0.15.
[0010] A second aspect of this invention provides an oxygen-containing fluorene polyaryl suspended side-chain anionic polymer, with the following structure: , , , , , ; The sum of x1 and x3 is 0.2; and / or the sum of x2 and x4 is 0.8; and / or the sum of x1 and x4 is 0.9; and / or the sum of x2 and x3 is 0.1.
[0011] A third aspect of this invention provides a method for preparing an oxygen-containing fluorene polyaryl suspended side-chain anionic polymer, comprising: Step 1: Mix any one or both of the aromatic compound and heteroaromatic compound with the ketone aldehyde monomer in a first organic solvent, control the temperature, add acid, and obtain the target precursor polymer; Step 2: Mix any alkylamine or base with the target precursor polymer and a second organic solvent to obtain the oxygen-containing fluorene polyaryl suspended side-chain anionic polymer as described in the first aspect.
[0012] In some third-aspect embodiments, the aromatic compound is selected from one or more of meta-terphenyl, biphenyl, and para-terphenyl.
[0013] In some third-aspect embodiments, the heteroaromatic compound is selected from fluorene.
[0014] In some third aspect embodiments, the ketaldehyde monomer is selected from one or more of 7-bromo-1,1,1-trifluoro-2-heptanone, 2,2,2-trifluoroacetophenone, 4-piperidinecarboxaldehyde, or their hydrochloride salts.
[0015] In some third aspect embodiments, the acid is selected from one or more of trifluoroacetic acid and trifluoromethanesulfonic acid.
[0016] In some third aspect embodiments, the first organic solvent and the second organic solvent are each independently selected from one or more of dichloromethane, DMF, dimethyl sulfoxide, N-methylpyrrolidone, methanol, toluene, isopropanol, and tetrahydrofuran.
[0017] In some third aspect embodiments, the molar amount of ketone-aldehyde monomer added to each 1L of the first organic solvent is 0.5~2.5mol.
[0018] In some third aspect embodiments, the molar amount of aromatic compound added to each 1L of the first organic solvent is 400~800 mmol.
[0019] In some third aspect embodiments, the molar amount of heteroaromatic compounds added to the first organic solvent is 100-400 mmol.
[0020] A fourth aspect of the present invention provides an anion exchange membrane, characterized in that it comprises an oxygen-containing fluorene polyaryl suspended side-chain anion polymer as described in any one of the first aspects.
[0021] In some third aspect embodiments, the dry membrane tensile strength of the exchange membrane is 45 MPa or higher.
[0022] In some third aspect embodiments, the elongation at break is 30-50%.
[0023] In some third aspect embodiments, the wet film tensile strength is 38 MPa or higher.
[0024] In some third aspect embodiments, the hydroxide ion conductivity at 80°C is 120~180 mS / cm, the swelling rate is 15~25%, and the water absorption rate is less than 55%.
[0025] The fifth aspect of this invention proposes the application of the anion exchange membrane described in the third aspect in the preparation of fuel cells, water electrolysis hydrogen production devices, flow batteries, or carbon dioxide reduction devices.
[0026] In this invention, fluorene (98% purity) and biphenyl (99% purity) were purchased from Aladdin Biochemical Technology Co., Ltd.; 7-bromo-1,1,1-trifluoro-2-heptanone (98% purity) was provided by Xiamen Jiamo Technology Co., Ltd.; trifluoromethanesulfonic acid (99% purity), 2,2,2-trifluoroacetophenone (98% purity), trifluoroacetic acid (99.9% purity) and trimethylamine ethanol solution (30% mass fraction) were purchased from Bailingwei Technology Co., Ltd.; dichloromethane (analytical grade), dimethyl sulfoxide (analytical grade), N,N-dimethylformamide (analytical grade), ethyl acetate (analytical grade), methanol (analytical grade), N-methylpyrrolidone (analytical grade) and anhydrous ethanol (analytical grade) were purchased from Sinopharm Chemical Reagent Co., Ltd.
[0027] The following testing methods can be found in the paper: Fan L, Lin C, Ma Y, et al. In-situ self-crosslinked poly (biphenylalkylene) anion exchange membranes for durable water electrolysis[J]. Journal of Membrane Science , 2025: 124812. (1) Conductivity testing methods and experimental procedures The ionic conductivity of AEM in its fully hydrated state was tested using a VersaSTAT 3F (Princeton) electrochemical workstation via a four-electrode method. The AEM to be tested was cut into 1×5 cm strips and immersed in 1 M KOH solution for 24 h for ion exchange, with the alkali solution being replaced every 8 h. After ion exchange, it was rinsed with deionized water and immersed for 24 h to remove residual alkali solution before testing, with the deionized water being replaced every 8 h. The entire electrode assembly and testing process was carried out under nitrogen protection in deionized water at a test temperature of 80℃ and an AC impedance test frequency of 0.1 Hz–0.1 MHz. The ionic conductivity calculation formula (1) is as follows: σ = L / RWT (1) Where L is the distance between the electrodes (cm); R is the measured impedance of the AEM (kΩ); W and T are the width (cm) and thickness (μm) of the AEM in the fully hydrated state, respectively.
[0028] (2) Water absorption rate (WU) and swelling rate (SR) were determined as follows: Anion exchange membranes were cut into 3.0 × 3.0 cm samples and immersed in 1 M KOH solution for 24 h for OH testing. -Ion exchange was performed, with the alkali solution replaced every 8 hours, followed by immersion in ultrapure water at 80 °C for 24 hours. After removal, excess water was wiped off the surface, and the wet film mass and length were recorded and labeled as W. wet and L wet Afterwards, the anion exchange membrane was dried in a vacuum drying oven at 80℃, and the weight and length W of the membrane in the dry state were measured. dry and L dry The water absorption rate and swelling rate are calculated using formulas (2) and (3): WU(%) = (M wet -M dry ) / M dry ×100% (2) SR(%) = (L wet -L dry ) / L dry ×100% (3) (3) The alkaline stability test was conducted by immersing the membrane sample in 2 M KOH at 80°C and measuring the change in conductivity of the membrane sample at intervals.
[0029] Anion exchange membranes undergo SN2 nucleophilic substitution and Hofmann elimination reactions in high-temperature and high-alkalinity environments, resulting in the degradation of functional groups within the membrane and a decrease in ion transport performance. The alkalinity stability of anion exchange membranes is determined by measuring the change in conductivity before and after the alkali resistance test.
[0030] (4) 1 The H NMR spectrum was obtained by a Bruker AVANCE NEO 500 nuclear magnetic resonance spectrometer; the microphase structure of the anion exchange membrane was characterized by a Dimension FastScan atomic force microscope; the mechanical properties of the anion exchange membrane were measured by an INSTRON 3343 universal testing machine; and the infrared spectrum was obtained by a Bruker Vertex 70V Fourier transform infrared spectrometer.
[0031] Advantages of this invention: This invention overcomes the shortcomings of traditional polyarylether materials, such as easy main chain breakage and degradation under strong alkaline conditions, by introducing a dibenzofuran structure, thus improving the chemical and thermal stability of the material. By utilizing a suspended side chain strategy to introduce benzene rings, quaternary ammonium groups, or piperidine groups, it effectively promotes microphase separation within the polymer, enabling the construction of efficient ion transport channels. This allows the membrane material to achieve good hydroxide ion conductivity while maintaining a low swelling ratio, reaching a maximum of 170.2 mS / cm at 80℃. The polymer exhibits excellent mechanical properties, with outstanding dry membrane tensile strength and excellent alkali resistance and durability, showing minimal conductivity loss after immersion in a strong alkaline (KOH) solution at 80℃ for over 1800 hours. The anion exchange membrane prepared by this invention has good application value in fuel cells and water electrolysis for hydrogen production, demonstrating strong commercial potential. Attached Figure Description
[0032] Figure 1 Example 1: Poly(fluorene) suspended trimethylamine anionic polymer 1 H NMR spectrum; Figure 2 Example 2: Poly(oxyfluorene-m-terphenyl) suspended trimethylamine precursor 1 H NMR spectrum; Figure 3 Example 2: Poly(oxyfluorene-m-terphenyl) suspended trimethylamine quaternized polymer 1 H NMR spectrum; Figure 4 Example 2: Conductivity of poly(oxyfluorene-m-terphenyl) suspended trimethylamine anion exchange membrane as a function of temperature; Figure 5 Example 2: Conductivity retention rate of poly(oxyfluorene-m-terphenyl) suspended trimethylamine anion exchange membrane after alkali resistance test; Figure 6 Example 2: Power density curve of poly(oxyfluorene-m-terphenyl) suspended trimethylamine anion exchange membrane; Figure 7 Example 2: Polarization performance diagram of a water electrolysis hydrogen production device with a poly(oxyfluorene-m-terphenyl) suspended trimethylamine anion exchange membrane; Figure 8 Example 3: Poly(oxyfluorene-biphenyl) suspended trimethylamine quaternized polymer 1 H NMR spectrum; Figure 9 Example 4: Poly(oxyfluorene-biphenyl) suspended piperidine polymer 1 H NMR spectrum; Figure 10 Example 4: Polarization performance diagram of a water electrolysis hydrogen production device using a poly(oxyfluorene-biphenyl) suspended piperidine anion exchange membrane; Figure 11 Example 6: Poly(oxyfluorene-biphenyl) (suspended trimethylamine-hydrophobic segment) precursor polymer 1 H NMR spectrum.
[0033] Figure 12 Comparative Example 1: Poly(oxyfluorene-biphenyl) suspended trimethylamine quaternized polymer 1 H NMR spectrum. Detailed Implementation
[0034] The technical solutions of the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0035] Example 1 Example 1 prepared a poly(fluorene) suspended trimethylamine anion exchange membrane, the structural formula of which is as follows:
[0036] 10 mmol of fluorene and 12 mmol of 7-bromo-1,1,1-trifluoro-2-heptanone were placed in a flask and dissolved in 10 mL of dichloromethane. A mixture of trifluoroacetic acid and trifluoromethanesulfonic acid (volume ratio 1:10, total volume 11 mL) was slowly added dropwise at 0 °C with stirring. The reaction was continued at this temperature for 2 hours. When the system gradually became viscous and no longer stuck to the walls, ethanol was immediately added to quench the reaction and the mixture was sheared. The resulting product was redissolved in dichloromethane and washed again with ethanol. Finally, the polymer was filtered and vacuum dried to obtain the target precursor polymer in 98% yield.
[0037] 4 g of the prepared target precursor polymer was dissolved in N,N-dimethylformamide (40 mL), and then an ethanol solution of trimethylamine (8 mL, 30 wt%) was added. The mixture was stirred at room temperature for 24 h to ensure complete quaternization. After the reaction was complete, the reaction liquid was added dropwise to ethyl acetate to precipitate the polymer. After washing several times, the product was collected by filtration and dried in a vacuum oven at 80 °C for 24 h to obtain a white fibrous solid, a poly(oxyfluorene)-suspended trimethylamine anionic polymer, with a yield of 99%.
[0038] Take 0.14 g of the quaternized polymer and add 9 mL of dimethyl sulfoxide, stirring until completely dissolved. Filter the resulting mixture through a 0.45 μm polytetrafluoroethylene (PTFE) needle filter, then cast it uniformly onto a clean, flat glass plate. Dry the glass plate in an 80 °C vacuum oven for 24 h, remove and cool to room temperature, then carefully peel it off to form a membrane. The membrane is then annealed under the same conditions for 24 h to remove residual solvent. Finally, the resulting membrane is immersed in a 1 mol / L potassium hydroxide solution for 48 h for ion exchange. After complete ion exchange, repeatedly rinse with deionized water to remove residual alkali from the membrane surface and store in deionized water for later use.
[0039] Example 2 Example 2 prepared a poly(oxyfluorene-m-terphenyl) suspended trimethylamine anion exchange membrane, the structural formula of which is as follows:
[0040] 8 mmol of m-terphenyl, 2 mmol of fluorene, and 13 mmol of 7-bromo-1,1,1-trifluoro-2-heptanone were dissolved in dichloromethane (DCM, 10 mL). A mixture of trifluoroacetic acid (TFA) and trifluoromethanesulfonic acid (TFSA) (1 / 10 mL) was then added dropwise to this solution. The reaction mixture was stirred at 0 °C for 12 h. Once the system became viscous, the reaction was immediately terminated with ethanol. The resulting product was redissolved in dichloromethane and washed again with ethanol. Finally, the polymer was filtered and dried under vacuum to obtain the target precursor polymer in 96% yield.
[0041] The precursor polymer (5 g) was dissolved in N,N-dimethylformamide (50 mL), followed by the addition of trimethylamine ethanol solution (10 mL, 30 wt%). The reaction was carried out at room temperature for 24 h to ensure complete quaternization. After the reaction was completed, the polymer was precipitated with ethyl acetate, washed, collected by vacuum filtration, and dried at 80 °C for 24 h to obtain a white fibrous solid product with a yield of 99%.
[0042] The quaternized polymer (0.14 g) obtained in step two of Example 2 was dissolved in 9 mL of dimethyl sulfoxide and stirred until completely dissolved. The resulting mixture was then filtered through a 0.45 μm polytetrafluoroethylene (PTFE) syringe filter and cast onto a clean, flat glass substrate. After vacuum drying at 80 °C for 24 h, it was cooled to room temperature and then peeled off to obtain the membrane material. The membrane was then further annealed in a vacuum oven at 80 °C for 24 h. Finally, the resulting anion exchange membrane (AEM) was immersed in a 1 mol / L potassium hydroxide solution for 48 h for ion exchange. After complete ion exchange, the residual alkali was washed off with deionized water and stored in deionized water for later use.
[0043] When the poly(oxyfluorene-m-terphenyl) suspended trimethylamine anion exchange membrane of Example 2 is applied to a fuel cell, the MEA assembled with this membrane achieves 1.3 W / cm² at a back pressure of 1.3 bar / 1.3 bar. -2 The maximum peak power density.
[0044] Figure 4 The conductivity of the poly(oxyfluorene-m-terphenyl) suspended trimethylamine anion exchange membrane in Example 2 is shown as a function of temperature. Figure 5 The conductivity retention rate of the poly(oxyfluorene-m-terphenyl) suspended trimethylamine anion exchange membrane after the alkali resistance test in Example 2 is shown in the graph. Figure 6 The power density curve of the poly(oxyfluorene-m-terphenyl) suspended trimethylamine anion exchange membrane in Example 2 is shown. Figure 7 The polarization performance diagram of the water electrolysis hydrogen production device using the poly(oxyfluorene-m-terphenyl) suspended trimethylamine anion exchange membrane of Example 2 is shown.
[0045] Example 3 Example 3 prepared a poly(oxyfluorene-biphenyl) suspended trimethylamine anion exchange membrane, the structural formula of which is as follows:
[0046] Biphenyl (7 mmol), fluorene (3 mmol), and 7-bromo-1,1,1-trifluoro-2-heptanone (13 mmol) were dissolved in dichloromethane (DCM, 10 mL). A mixture of trifluoroacetic acid (TFA) and trifluoromethanesulfonic acid (TFSA) (1 / 10 mL) was then added dropwise to this solution. The reaction mixture was stirred at 0 °C for 12 h. Once the system became viscous, the reaction was immediately terminated with ethanol. The resulting product was redissolved in dichloromethane and washed again with ethanol. Finally, the polymer was filtered and dried under vacuum to obtain the target precursor polymer in 96% yield.
[0047] The precursor polymer (5 g) was dissolved in N,N-dimethylformamide (50 mL), followed by the addition of trimethylamine ethanol solution (10 mL, 30 wt%). The reaction was carried out at room temperature for 24 h to ensure complete quaternization. After the reaction was completed, the polymer was precipitated with ethyl acetate, washed, collected by vacuum filtration, and dried at 80 °C for 24 h to obtain a white fibrous solid product with a yield of 97%.
[0048] A white fibrous solid product (0.14 g) was dissolved in 9 mL of dimethyl sulfoxide and stirred until completely dissolved. The resulting mixture was then filtered through a 0.45 μm polytetrafluoroethylene (PTFE) syringe filter and cast onto a clean, flat glass substrate. After vacuum drying at 80 °C for 24 h, it was allowed to cool to room temperature and then peeled off to obtain the membrane material. The membrane was then further annealed in a vacuum oven at 80 °C for 24 h. Finally, the resulting anion exchange membrane (AEM) was immersed in a 1 mol / L potassium hydroxide solution for 48 h for ion exchange. After complete ion exchange, the residual alkali solution was washed off with deionized water, and the membrane was stored in deionized water for later use.
[0049] Example 4 Example 4 prepared a poly(oxyfluorene-biphenyl) suspended piperidine anion exchange membrane, the structural formula of which is as follows:
[0050] Biphenyl (75 mmol) was added to a 500 mL reactor, followed by 100 mL of dichloromethane; then 4-piperidine carboxaldehyde hydrochloride (112.2 mmol) and fluorene (25 mmol) were added sequentially. The system temperature was lowered to -15 °C, and after mechanical stirring for a period of time, a mixed acid reagent consisting of 50 mL of trifluoromethanesulfonic acid and 5 mL of trifluoroacetic acid was slowly added dropwise. After the addition was complete, the temperature was raised to 0 °C, and the reaction continued for 3 h. When the viscosity of the reaction solution increased significantly, it was quenched in an aqueous potassium carbonate solution, precipitating the crude polymer product. The crude product was washed several times with a mixed solution of deionized water and potassium carbonate until neutral. The solid was filtered and dried at 80 °C for 24 h to obtain the suspended piperidine precursor polymer. The yield was 96%.
[0051] 10 g of the suspended piperidine precursor polymer was weighed into a 250 mL round-bottom flask, and 20 mL of dimethyl sulfoxide was added and stirred until completely dissolved. Then, potassium carbonate (50.6 mmol) and 10 mL of iodomethane solution were added, and the mixture was reacted at 40 °C in the dark for 36 h. After the reaction was complete, the mixture was slowly added dropwise to ethyl acetate to precipitate the polymer. The product was filtered, preliminarily dried, and then washed repeatedly with deionized water to remove residual inorganic salts. Finally, it was dried under vacuum at 80 °C for 24 h to obtain the quaternized polymer. The yield was 98%.
[0052] Weigh 0.25 g of the quaternized polymer prepared in Example 4 above, dissolve it in 20 mL of N-methylpyrrolidone, and stir until the solution is homogeneous and transparent. Filter the casting solution through a 0.45 μm PTFE syringe filter to remove insoluble impurities, and then uniformly cast it into a clean glass mold. Place the glass mold under vacuum drying at 80 °C for 24 h. After drying, peel off the polymer film. Immerse the obtained film in a 1 mol / L KOH solution at room temperature for 48 h to complete ion exchange. Then, repeatedly rinse the film surface with deionized water to remove residual alkali, and finally store it in deionized water for later use.
[0053] Example 5 Example 5 prepared a poly(oxyfluorene-p-terphenyl) suspended piperidine anion exchange membrane, the structural formula of which is as follows:
[0054] 70 mmol of terphenyl was added to a 500 mL reactor, followed by 100 mL of dichloromethane, and then 112.2 mmol of 4-piperidine carboxaldehyde hydrochloride and 30 mmol of fluorene. The system temperature was lowered to -15 °C, and after mechanical stirring for a period of time, a mixed acid reagent consisting of 50 mL of trifluoromethanesulfonic acid and 5 mL of trifluoroacetic acid was slowly added dropwise. After the addition was complete, the temperature was raised to 0 °C, and the reaction was continued for 3 h. When the viscosity of the reaction solution increased significantly, it was quenched in an aqueous potassium carbonate solution, precipitating the crude polymer product. The crude product was washed several times with a mixed solution of deionized water and potassium carbonate until neutral. The solid was filtered and dried at 80 °C for 24 h to obtain a suspended piperidine precursor polymer with a yield of 95%.
[0055] 10 g of the suspended piperidine-type precursor polymer was weighed into a 250 mL round-bottom flask, and 20 mL of dimethyl sulfoxide was added and stirred until completely dissolved. Then, 7 g of potassium carbonate and 10 mL of iodomethane solution were added, and the mixture was reacted at 40 °C in the dark for 36 h. After the reaction was complete, the mixture was slowly added dropwise to ethyl acetate to precipitate the polymer. The product was filtered, preliminarily dried, and then washed repeatedly with deionized water to remove residual inorganic salts. Finally, it was dried under vacuum at 80 °C for 24 h to obtain the precursor polymer. The yield was 98%.
[0056] Weigh 0.25 g of the precursor polymer prepared in Example 5 above and dissolve it in 20 mL of N-methylpyrrolidone, stirring until the solution is homogeneous and transparent. Filter the casting solution through a 0.45 μm PTFE syringe filter to remove insoluble impurities, then uniformly cast it into a clean glass mold. Place the glass mold under vacuum drying at 80 °C for 24 h. After drying, peel off the polymer film. Immerse the obtained film in 1 mol / L KOH solution at room temperature for 48 h to complete ion exchange. Then, repeatedly rinse the film surface with deionized water to remove residual alkali, and finally store it in deionized water for later use.
[0057] Example 6 Example 6 prepared a poly(fluorene-biphenyl) (suspended trimethylamine-hydrophobic segment) anion exchange membrane, the structural formula of which is as follows:
[0058] Biphenyl (8 mmol), fluorene (2 mmol), 7-bromo-1,1,1-trifluoro-2-heptanone (10.8 mmol), and 2,2,2-trifluoroacetophenone (1.2 mmol) were weighed and added to 10 mL of dichloromethane. The mixture was stirred until completely dissolved to obtain a homogeneous solution. The reaction system was cooled to 0°C, and then 11 mL of a mixed acid prepared from trifluoroacetic acid and trifluoromethanesulfonic acid at a volume ratio of 1:10 was slowly added dropwise. After the addition was complete, the reaction was continued for 6 h with stirring. When the reaction system gradually became highly viscous and acid precipitation occurred without sticking to the walls, methanol was quickly added to quench the reaction. The resulting crude product was then shredded and dissolved in dichloromethane for recrystallization. The product was washed four times with methanol over 48 h to ensure complete acid removal. Finally, the solid product was collected by filtration and dried under vacuum at 80°C for 24 h to obtain the target precursor polymer of Example 6, with a yield of 98%.
[0059] Weigh 4 g of the precursor polymer prepared in Example 6 and add it to 40 mL of N,N-dimethylformamide. Stir until the system is homogeneous and clear. Then, add 30 wt% trimethylamine ethanol solution (10 mL) to the solution and react at room temperature for 24 h. After the reaction is complete, the liquid is added dropwise to ethyl acetate to allow the polymer to precipitate completely. The precipitated polymer is washed four times with ethyl acetate, filtered, and the solid product is collected. The collected solid is then placed in a vacuum oven at 80 °C and dried for 24 h to obtain a white fibrous solid product with a yield of 98%.
[0060] In the structural formula of Example 6, x1+x2+x3+x4=1; x1+x3=0.2; x2+x4=0.8; x1+x4=0.9; x2+x3=0.1.
[0061] A white fibrous solid product (0.14 g) was dissolved in 9 mL of dimethyl sulfoxide and stirred until completely dissolved. The resulting mixture was then filtered through a 0.45 μm polytetrafluoroethylene (PTFE) syringe filter and cast onto a clean, flat glass substrate. After vacuum drying at 80 °C for 24 h, it was allowed to cool to room temperature and then peeled off to obtain the membrane material. The membrane was then further annealed in a vacuum oven at 80 °C for 24 h. Finally, the resulting anion exchange membrane (AEM) was immersed in a 1 mol / L potassium hydroxide solution for 48 h for ion exchange. After complete ion exchange, the residual alkali solution was washed off with deionized water, and the membrane was stored in deionized water for later use.
[0062] Comparative Example 1 Comparative Example 1 prepared a poly(oxyfluorene-biphenyl) suspended trimethylamine anion exchange membrane, whose structure was similar to that of Example 2, except that m-terphenyl was replaced with biphenyl. Its structural formula is as follows:
[0063] Preparation of poly(oxyfluorene-biphenyl) suspended trimethylamine precursor polymer Biphenyl (8 mmol), fluorene (2 mmol), and 7-bromo-1,1,1-trifluoro-2-heptanone (12 mmol) were added to 10 mL of dichloromethane and stirred until completely dissolved. The reaction system was placed at 0 °C, and then a mixed acid solution of trifluoroacetic acid and trifluoromethanesulfonic acid (volume ratio 1:10, total volume 11 mL) was slowly added dropwise to the homogeneous solution. The reaction was stirred for 7 h, and the reaction system became highly viscous. Methanol was quickly added to quench the reaction. The obtained crude product was chopped and redissolved in dichloromethane, and then washed four times with methanol over 48 h until the acid was completely removed. Finally, the solid product was collected by filtration and dried under vacuum at 80 °C for 24 h to obtain the target precursor polymer of Comparative Example 1, with a product yield of 98%.
[0064] Weigh 5 g of the precursor polymer prepared in Comparative Example 1 and add it to 45 mL of N,N-dimethylformamide. Stir until the system is homogeneous and clear. Then, add 11 mL of trimethylamine ethanol solution (30 wt%) to the solution and react at room temperature for 24 h. After the reaction is complete, the liquid is added dropwise to ethyl acetate to allow the polymer to precipitate completely. The precipitated polymer is washed four times with ethyl acetate, filtered, and the solid product is collected. The collected solid is then placed in a vacuum oven at 80 °C and dried for 24 h to obtain a white fibrous solid product with a yield of 98%.
[0065] 0.38 g of a white fibrous solid product was dissolved in 24 mL of dimethyl sulfoxide to obtain a homogeneous mixed solution. This mixed solution was filtered through a polytetrafluoroethylene (PTFE) syringe filter (0.45 μm pore size) to remove impurities. The filtered solution was then cast onto a clean, flat glass substrate. The glass substrate was placed in a vacuum drying oven and dried at 80 °C for 24 h. After the system cooled to room temperature, the membrane material on the substrate was peeled off to obtain the membrane sample. Finally, the prepared anion exchange membrane was immersed in a 1 mol / L potassium hydroxide solution for 48 h to complete the ion exchange process. After complete ion exchange, the membrane material was repeatedly rinsed with deionized water to remove residual alkali. After rinsing, the membrane material was stored in deionized water for later use.
[0066] Comparative Example 2 Comparative Example 2 prepared a poly(oxyfluorene-p-terphenyl) suspended piperidine anion exchange membrane, the structural formula of which is as follows:
[0067] The specific synthesis steps of Comparative Example 2 and Example 5 are the same as the film-forming steps, except that the proportion of fluorene is reduced and the proportion of terphenyl is increased. The amount of fluorene added is (10 mmol) and the amount of terphenyl added is (90 mmol). Other additions and operations remain unchanged.
[0068] Comparative Example 2 prepared a poly(oxyfluorene-p-terphenyl) suspended piperidine anion exchange membrane. The MEA assembled from this membrane achieved 0.9 W / cm² at a back pressure of 1.3 bar / 1.3 bar. -2 The maximum peak power density.
[0069] Comparative Example 3
[0070] Compared with Example 6, Comparative Example 3 differs in the preparation of the precursor polymer, specifically in the following steps: Biphenyl (8 mmol), fluorene (2 mmol), 7-bromo-1,1,1-trifluoro-2-heptanone (10.8 mmol), and 4-(tetrafluoromethyl)-1,1,1-trifluoroacetophenone (1.2 mmol) were weighed and added to 10 mL of dichloromethane. The mixture was stirred until completely dissolved, resulting in a homogeneous solution. The reaction system was cooled to 0°C, and then 11 mL of a mixed acid (prepared from trifluoroacetic acid and trifluoromethanesulfonic acid at a volume ratio of 1:10) was slowly added dropwise. After the addition was complete, the reaction was continued for 5 hours with stirring. When the reaction system gradually became highly viscous and acid precipitation occurred without sticking to the walls, methanol was quickly added to quench the reaction. The resulting crude product was then shredded and dissolved in dichloromethane for recrystallization. The mixture was washed four times with methanol over 48 hours to ensure complete acid removal. Finally, the solid product was collected by vacuum filtration and dried at 80°C for 24 hours to obtain the target precursor polymer of Comparative Example 3, with a yield of 97%.
[0071] Weigh 4 g of the precursor polymer prepared in Comparative Example 3 and add it to 40 mL of N,N-dimethylformamide. Stir until the system is homogeneous and clear. Then, add 10 mL of trimethylamine ethanol solution (30 wt%) to the solution and react at room temperature for 24 h. After the reaction is complete, the liquid is added dropwise to ethyl acetate to allow the polymer to precipitate completely. The precipitated polymer is washed four times with ethyl acetate, filtered, and the solid product is collected. The collected solid is then placed in a vacuum oven at 80 °C and dried for 24 h to obtain a white fibrous solid product with a yield of 98%.
[0072] A white fibrous solid product (0.14 g) was dissolved in 9 mL of dimethyl sulfoxide and stirred until completely dissolved. The resulting mixture was then filtered through a 0.45 μm polytetrafluoroethylene (PTFE) syringe filter and cast onto a clean, flat glass substrate. After vacuum drying at 80 °C for 24 h, the substrate was cooled to room temperature and then peeled off to obtain the membrane material. The membrane was then further annealed in a vacuum oven at 80 °C for 24 h. Finally, the resulting anion exchange membrane (AEM) was immersed in a 1 mol / L potassium hydroxide solution for 48 h for ion exchange. After complete ion exchange, residual alkali was washed off with deionized water, and the membrane was stored in deionized water for later use.
[0073] Comparative Example 4
[0074] In the structural formula of Comparative Example 4, x1+x2+x3+x4=1; x1+x3=0.2; x2+x4=0.8; x1+x4=0.85; x2+x3=0.15, indicating an increased proportion of 2,2,2-trifluoroacetophenone. The preparation method of its precursor polymer is as follows: Biphenyl (8 mmol), fluorene (2 mmol), 7-bromo-1,1,1-trifluoro-2-heptanone (10.2 mmol), and 2,2,2-trifluoroacetophenone (1.8 mmol) were placed in a jacketed reactor and added to 10 mL of dichloromethane with stirring until completely dissolved. The reaction system was cooled to 0 °C, and 11 mL of a mixed acid solution prepared from trifluoroacetic acid and trifluoromethanesulfonic acid at a volume ratio of 1:10 was slowly added dropwise. After the addition was completed, the reaction was stirred for about 6 h. When the system gradually became highly viscous and acid precipitation without sticking to the walls occurred, methanol was quickly added to quench the reaction. The obtained crude product was shredded, dissolved in dichloromethane, and recrystallized; then washed repeatedly with methanol four times for 48 h to completely remove residual acid. The solid product was collected by vacuum filtration and dried under vacuum at 80 °C for 24 h to obtain the target precursor polymer of Comparative Example 4, with a yield of 96%.
[0075] Weigh 4 g of the precursor polymer prepared in Comparative Example 4 and add it to 40 mL of N,N-dimethylformamide. Stir until the system is homogeneous and clear. Then, add 10 mL of trimethylamine ethanol solution (30 wt%) to the solution and react at room temperature for 24 h. After the reaction is complete, the liquid is added dropwise to ethyl acetate to allow the polymer to precipitate completely. The precipitated polymer is washed four times with ethyl acetate, filtered, and the solid product is collected. The collected solid is then placed in a vacuum oven at 80 °C and dried for 24 h to obtain a white fibrous solid product with a yield of 98%.
[0076] A white fibrous solid product (0.14 g) was dissolved in 9 mL of dimethyl sulfoxide and stirred until completely dissolved. The resulting mixture was then filtered through a 0.45 μm polytetrafluoroethylene (PTFE) syringe filter and cast onto a clean, flat glass substrate. After vacuum drying at 80 °C for 24 h, it was allowed to cool to room temperature and then peeled off to obtain the membrane material. The membrane was then further annealed in a vacuum oven at 80 °C for 24 h. Finally, the resulting anion exchange membrane (AEM) was immersed in a 1 mol / L potassium hydroxide solution for 48 h for ion exchange. After complete ion exchange, the residual alkali solution was washed off with deionized water, and the membrane was stored in deionized water for later use.
[0077] Example 7 The performance of the anion exchange membranes prepared in Examples 1 to 6 and Comparative Examples 1 to 4 was tested, and the results are shown in Table 1: Table 1 Summary of performance parameters of anion exchange membranes ; The swelling rate is the swelling rate along the length (%). Examples 1 to 6 of this invention significantly improve the overall performance of anion exchange membranes by introducing an oxyfluorene structure and combining it with a suspended side chain strategy. Through a reasonable combination of hydrophilic and hydrophobic blocks, the membranes achieve a balance in indicators such as alkaline immersion stability, swelling ratio, conductivity, and tensile strength, reaching 3.2 A cm⁻¹ in a 1.8V water electrolysis hydrogen production test. -2 Performance.
[0078] Compared to Comparative Examples 1 to 4, it exhibits significant performance advantages. After soaking in a 2M KOH solution at 80°C for 1800 hours, the formulation of Example 4 retains up to 96% of its conductivity, effectively overcoming the defect of easy breakage of the main chain in traditional materials. In contrast, Comparative Example 2, with a similar structure, has a minimum conductivity of only 90%. In terms of performance balance, Example 2 achieves a conductivity as high as 170.2 mS / cm (80°C).
[0079] Example 6, by introducing hydrophobic segments, optimized the swelling ratio to 20% while maintaining a high conductivity of 155 mS / cm, thus resolving the trade-off between high conductivity and dimensional stability. In contrast, Comparative Example 1 had a swelling ratio as high as 50%. The examples also demonstrated superior mechanical strength; for instance, the dry film tensile strength of Example 4 reached 60 MPa, far exceeding the 23 MPa of Comparative Example 1. All examples achieved a current density of 2.9 A / cm² in the 1.8V water electrolysis test. 2 The above is significantly better than the comparative example's 2.5~2.6 A / cm. 2 This demonstrates its strong commercial potential in the fields of fuel cells and water electrolysis for hydrogen production.
Claims
1. An oxygen-containing fluorene polyaryl suspended side-chain anionic polymer, characterized in that, The oxygen-containing fluorene polyaryl suspended side-chain anionic polymer includes structural unit I and / or structural unit II; 、 ; Z1 and Z2 are each independently selected from , , , ; R1, R2, and R3 are each independently selected from hydrogen, substituted or unsubstituted branched alkyl, substituted or unsubstituted branched alkyl, substituted or unsubstituted piperidinyl, and substituted or unsubstituted aryl. The ring Ar is selected from , The plurality of R b Each of the X molecules is independently selected from any of the branched alkyl groups (C3 to C10) or the straight-chain alkyl groups (C1 to C10) that are substituted or unsubstituted. - Selected from anions.
2. The oxygen-containing fluorene polyaryl suspended side-chain anionic polymer according to claim 1, characterized in that, R1, R2, and R3 are each independently selected from alkyl groups, hydrogen groups, and alkyl groups substituted with one or more halogens. The X - Selected from anions, the plurality of R c Each is independently selected from any branched alkyl group (C3 to C10) or a straight alkyl group (C1 to C10) that is substituted or unsubstituted; The n is selected from any positive integer from 1 to 5; Preferably, the R b and R c Each is independently selected from methyl, ethyl, and isopropyl, wherein X - Selected from OH - .
3. The oxygen-containing fluorene polyaryl suspended side-chain anionic polymer according to any one of claims 1 to 3, characterized in that, The oxygen-containing fluorene polyaryl suspended side-chain anionic polymer structure is any one of I-a, I-b, I-c, or I-d; 、 、 、 ; The x5 is selected from 0.15 to 0.45; the x6 is selected from 0.6 to 0.9; R1, R2, R3, and Ar are defined as in any one of claims 1 to 4.
4. The oxygen-containing fluorene polyaryl suspended side-chain anionic polymer according to any one of claims 1 to 4, characterized in that, The oxygen-containing fluorene polyaryl suspended side-chain anionic polymer structure is as shown in II-e; R1, R2, R3, and Ar are defined as in any one of claims 1 to 4.
5. In the II-e structure, the sum of x1 and x3 satisfies 0.1≤x1+x3≤0.4; and / or, the sum of x2 and x4 satisfies 0.5≤x2+x4≤0.9; and / or, the sum of x1 and x4 satisfies 0.70≤x1+x4≤0.95; and / or, the sum of x2 and x3 satisfies 0.05≤x2+x3≤0.
15.
6. An oxygen-containing fluorene polyaryl suspended side-chain anionic polymer, with the following structure: 、 、 、 、 、 ; The sum of x1 and x3 is 0.2; and / or the sum of x2 and x4 is 0.8; and / or the sum of x1 and x4 is 0.9; and / or the sum of x2 and x3 is 0.
1.
7. Preparation of an oxygen-containing fluorene polyaryl suspended side-chain anionic polymer, comprising: Step 1: Mix any one or both of the aromatic compound and heteroaromatic compound with the ketone aldehyde monomer in a first organic solvent, control the temperature, add acid, and obtain the target precursor polymer; Step 2: Mix any alkylamine or base with the target precursor polymer and a second organic solvent to obtain the oxygen-containing fluorene polyaryl suspended side-chain anionic polymer as described in claims 1 to 6.
8. The preparation of the oxygen-containing fluorene polyaryl suspended side-chain anionic polymer according to claim 7, characterized in that, The aromatic compound is selected from one or more of m-terphenyl, biphenyl, and p-terphenyl; and / or, the heteroaromatic compound is selected from fluorene; and / or, the ketone-aldehyde monomer is selected from one or more of 7-bromo-1,1,1-trifluoro-2-heptanone, 2,2,2-trifluoroacetophenone, 4-piperidinecarboxaldehyde or their hydrochloride salts; and / or, the acid is selected from one or more of trifluoroacetic acid and trifluoromethanesulfonic acid; and / or, the first organic solvent and the second organic solvent are each independently selected from one or more of dichloromethane, DMF, dimethyl sulfoxide, N-methylpyrrolidone, methanol, toluene, isopropanol, and tetrahydrofuran; and / or, the molar amount of ketone-aldehyde monomer added per 1L of the first organic solvent is 0.5~2.5mol; and / or, the molar amount of aromatic compound added per 1L of the first organic solvent is 400~800mmol; and / or, the molar amount of heteroaromatic compound added to the first organic solvent is 100~400mmol.
9. An anion exchange membrane, characterized in that, The membrane comprises an oxygen-containing fluorene polyaryl suspended side-chain anionic polymer as described in any one of claims 1 to 6, preferably wherein the dry membrane tensile strength is 45 MPa or higher; and / or the elongation at break is 30-50%; and / or the wet membrane tensile strength is 38 MPa or higher; and / or the hydroxide ion conductivity at 80°C is 120-180 mS / cm, the swelling ratio is 15-25%, and the water absorption rate is less than 55%.
10. The application of the anion exchange membrane according to claim 9 in the preparation of fuel cells, water electrolysis hydrogen production devices, flow batteries or carbon dioxide reduction devices.