A catalyst for phenol hydroxylation reaction and a preparation method thereof

CN122722299APending Publication Date: 2026-09-11CHINA CATALYST HLDG CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611106521.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-24
Publication Date
2026-09-11

AI Technical Summary

Technical Problem

在甲醇为溶剂的苯酚羟基化反应中,较好的反应结果为苯酚转化率26.9%、对邻比2.46,转化率偏低

Benefits of technology

本发明是一种复合型催化剂,以钛硅分子筛TS-1为原料,负载氧化铁并进行络合脱除表面部分的氧化铁,所得分子筛再进行纯硅分子筛的水热包覆过程,最终得到用于苯酚羟基化反应的催化剂。本发明提供的催化剂性能稳定,在苯酚羟基化反应中表现出更高的转化率和对邻比,更适用于对苯二酚工业化生产需求。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122722299A_ABST
    Figure CN122722299A_ABST
Patent Text Reader

Abstract

This invention relates to a catalyst for the hydroxylation reaction of phenol and its preparation method, belonging to the field of catalyst preparation. The catalyst of this invention is a composite catalyst, using titanium silicate molecular sieve TS-1 as raw material, loading iron oxide and performing complexation to remove part of the iron oxide, then subjecting the resulting molecular sieve to a hydrothermal coating process with pure silica molecular sieve, finally obtaining the catalyst for the hydroxylation reaction of phenol. The catalyst provided by this invention has stable performance, exhibiting higher conversion rate and ortho-para ratio in the hydroxylation reaction of phenol, making it more suitable for the industrial production needs of hydroquinone.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalyst preparation, and relates to a catalyst for the hydroxylation reaction of phenol and its preparation method. Background Technology

[0002] Hydroquinone, as an important chemical intermediate, has been widely used in industries such as dyes, pesticides, pharmaceuticals, and rubber. Among these, catechol and hydroquinone have particularly wide applications. Catechol has extensive uses in industries such as rubber, pharmaceuticals, pesticides, dyes, photosensitive materials, and fragrances, serving as a rubber hardener, hair dye, antioxidant, developer on photosensitive materials, anti-peeling agent in paints, and an important intermediate for insecticides such as carbofuran, adrenaline, and vanillin. In my country, 80% of catechol is used in the pesticide sector. Pesticides such as carbofuran, propoxur, and ethoxysulfuron produced from catechol have advantages such as high efficiency, low toxicity, and low residue, and their applications are very broad. Hydroquinone has wide applications in the pharmaceutical, dye and pigment, and electronics and optics industries. In recent years, with the support of long-term policies on domestic substitution in PEEK materials, new energy, and semiconductors, hydroquinone is expected to see even broader application prospects.

[0003] In my country, the main methods for producing hydroquinone are still the traditional methods such as the diisopropylbenzene oxidation method, the aniline oxidation method (used by most domestic manufacturers), and the bisphenol A method. Faced with increasingly severe environmental problems, the drawbacks of traditional processes are becoming increasingly apparent, such as long production processes, low production capacity, excessive waste, and high costs. The phenol hydroxylation method, using phenol and hydrogen peroxide as raw materials, is considered the most green chemistry-compliant method for hydroquinone production due to its readily available raw materials, mild reaction conditions, fewer byproducts, reduced waste pollution, and lower production costs. It is also the most promising method for the 21st century. Since its development, the phenol hydroxylation process has received widespread attention and research; therefore, the development of novel catalysts has become a key research focus.

[0004] Developing catalysts with high ortho-parallel ratios is essential to meet future market demands. Chinese invention patent CN 109499572 A discloses a method for obtaining a phenol hydroxylation catalyst by mixing a metal salt (iron and copper salt) alcohol solution with a silica alcohol gel and then supercritically drying it. This method yields a higher catechol yield, exceeding 40% in the reaction, while the hydroquinone yield is between 1% and 3%. Although this invention has a high conversion rate, the hydroquinone yield is very low. Chinese invention patent CN 122102149 A relates to a method for synthesizing micron-sized TS-2 molecular sieves with hierarchical pores, comprising the following steps: first, obtaining highly dispersed SiO2-TiO2 precursor powder via spray drying; then, obtaining micron-sized TS-2 molecular sieves via hydrothermal crystallization; next, mixing the micron-sized TS-2 molecular sieves with an organic alkali solution and deionized water, and treating under hydrothermal conditions to obtain micron-sized TS-2 molecular sieves with hierarchical pore structures. In the hydroxylation reaction of phenol using methanol as solvent, the better reaction results were a phenol conversion rate of 26.9% and a para-ortho ratio of 2.46, which is relatively low.

[0005] It is evident that catalysts have a significant impact on the hydroxylation reaction of phenol, and the development of novel hydroxylation catalysts has practical significance for industrial application. Summary of the Invention

[0006] This invention provides a catalyst for the hydroxylation reaction of phenol and its preparation method. The catalyst activity is improved by loading iron oxide and the para-ortho ratio is improved by coating with pure silicon molecular sieve, so that the catalyst has good catalytic performance in the hydroxylation reaction of phenol.

[0007] To achieve the above objectives and effects, the present invention employs the following catalyst preparation scheme.

[0008] A method for preparing a catalyst for the hydroxylation reaction of phenol includes mixing TS-1 molecular sieve with iron-doped framework with a template agent and water, adding a silicon source, hydrothermally crystallizing, drying, and calcining.

[0009] Furthermore, the preparation process of the framework-doped iron-rich TS-1 molecular sieve includes: (1) Mix TS-1 molecular sieve with an aqueous solution containing iron salt, perform hydrothermal treatment I, and dry I; (2) Mix the dried material with an organic acid ammonium aqueous solution, perform hydrothermal treatment II, drying II, and calcination II.

[0010] Furthermore, the mass ratio of TS-1 molecular sieve to iron salt is 0.015~0.05:1, and the liquid-solid mass ratio of TS-1 molecular sieve to aqueous solution containing iron salt is 2~4:1.

[0011] Furthermore, the iron salt is ferric nitrate nonahydrate.

[0012] Furthermore, the mass concentration of the organic acid ammonium aqueous solution is 0.5%~2.0%, and the liquid-solid mass ratio of the dried material to the organic acid ammonium aqueous solution is 10~20:1.

[0013] Furthermore, the organic ammonium acid is selected from at least one of ammonium citrate, ammonium acetate, and ammonium oxalate.

[0014] Furthermore, the mass ratio of each material fed is TS-1 molecular sieve with iron doped skeleton: silicon source: template agent: water = 1:1~3:0.15~0.5:2~10.

[0015] Furthermore, the silicon source is tetraethyl orthosilicate, and the template agent is tetrapropylammonium hydroxide.

[0016] Furthermore, the hydrothermal crystallization temperature is 160~180℃, the time is 48~120h, the drying temperature is 80~100℃, and the calcination temperature is 500~600℃.

[0017] Furthermore, the temperature of the hydrothermal treatment I is 60~120℃, the time is 4~12h, and the temperature of the drying I is 80~120℃.

[0018] Furthermore, the temperature of the hydrothermal treatment II is 50~100℃, the time is 2~8h, the temperature of the drying II is 80~120℃, and the temperature of the calcination II is 450~600℃.

[0019] The present invention also provides a catalyst prepared by the above preparation method, wherein the catalyst has an MFI topology and a grain size of 200~400 nm.

[0020] The present invention also provides the application of the catalyst prepared by the above method in the hydroxylation reaction of phenol.

[0021] Furthermore, using methanol as a solvent and hydrogen peroxide as an oxidant, with a phenol to hydrogen peroxide molar ratio of 1.9 to 2.1, the phenol conversion rate is greater than 44%, and the ortho-para ratio is greater than 2.5.

[0022] As one embodiment of the present invention, a method for preparing a catalyst for the hydroxylation reaction of phenol includes the following specific preparation steps: (1) Mix the titanium silicon molecular sieve TS-1 with an aqueous solution of ferric nitrate nonahydrate, add the mixture to the crystallization kettle, heat to 60~120℃ and keep it at that temperature for 4~12h. After the heat treatment is completed, cool down and remove from the kettle, wash with water, filter, and dry at 80~120℃.

[0023] (2) Mix the dried material in (1) with an organic acid ammonium aqueous solution, keep the mixture at 50~100℃ for 2~8h, cool it down and remove it from the kettle, wash it with water, filter it, dry it at 80~120℃, and roast it at 450~600℃.

[0024] (3) Mix tetrapropylammonium hydroxide aqueous solution (25% by mass) with deionized water, add tetraethyl orthosilicate dropwise, stir for 2 hours after the dropwise addition is completed, add the molecular sieve obtained in step (2), and stir evenly.

[0025] (4) The mixture in (3) is loaded into a stainless steel high-pressure reactor and crystallized at 160~180℃ for 48~120h. After cooling, filtering, washing, drying at 80~100℃, and calcining at 500~600℃, a catalyst for the hydroxylation reaction of phenol is obtained.

[0026] The beneficial effects of this invention include: This invention relates to a composite catalyst. Using TS-1 titanium-silicon molecular sieve as raw material, iron oxide is loaded and subjected to complexation to remove some of the surface iron oxide. The resulting molecular sieve is then subjected to a hydrothermal coating process with pure silicon molecular sieve, ultimately yielding a catalyst for the hydroxylation of phenol. The catalyst provided by this invention exhibits stable performance, demonstrating higher conversion rates and a higher para-ortho ratio in the hydroxylation of phenol, making it more suitable for the industrial production of hydroquinone. Attached Figure Description

[0027] Figure 1 The XRD pattern of CAT-1 titanium silicate molecular sieve is shown. Figure 2 SEM image of titanium silicate molecular sieve CAT-1. Detailed Implementation

[0028] The following embodiments will further illustrate the present invention, but do not limit the scope of the invention.

[0029] All reagents used in the examples are commercially available chemically pure reagents with a purity of not less than 98%.

[0030] To better illustrate the present invention, the preparation process of titanium-containing molecular sieves is described, but it is not limited to titanium-silicon molecular sieves prepared by the following method. Any commercially available titanium-silicon molecular sieve TS-1 can be used in the present invention.

[0031] Preparation method of titanium-silicon molecular sieve TS-1: Using silica sol as silicon source, tetrabutyl titanate as titanium source, and tetrapropylammonium bromide as template agent, crystallization is carried out at 150~200℃ for 12~48h. After filtration, washing, drying and calcination, titanium-silicon molecular sieve is obtained.

[0032] The catalyst prepared in this invention is used in the hydroxylation reaction of phenol. In the hydroxylation reaction of phenol using methanol as solvent and hydrogen peroxide as oxidant, 1g of catalyst, 30g of methanol, and 30g of phenol are packed into a four-necked flask. The temperature is raised to 60°C, and 20g of hydrogen peroxide (27.5% by mass concentration) is added dropwise. The reaction is allowed to proceed for 2 hours, and samples are taken for analysis. The reaction results are analyzed using gas chromatography, and the reaction indicators are phenol conversion rate (X) and ortho-para ratio (B). Example 1

[0033] (1) Mix 100g of titanium silicon molecular sieve TS-1 with 300g of ferric nitrate nonahydrate aqueous solution (mass concentration 0.8%), add the mixture to the crystallization kettle, heat to 80℃ and keep it at that temperature for 10h. After the heat treatment is completed, cool down and remove from the kettle, wash with water, filter, and dry at 100℃.

[0034] (2) Mix the dried material in (1) with 1800g of ammonium citrate aqueous solution (mass concentration 2.0%), keep the mixture at 70℃ for 6h, cool it down and remove it from the kettle, wash it with water, filter it, dry it at 100℃, and roast it at 500℃ for 4h.

[0035] (3) Mix 14g of tetrapropylammonium hydroxide aqueous solution (mass concentration 25%) with 69.5g of deionized water, add 20g of tetraethyl orthosilicate dropwise, stir for 2h after the dropwise addition is completed, add 10g of molecular sieve obtained in step (2), and stir evenly.

[0036] (4) The mixture in (3) was placed in a stainless steel high-pressure reactor and crystallized at 170°C for 72 h. After cooling, filtering, washing, drying at 100°C, and calcining at 550°C for 4 h, the catalyst CAT-1 for the hydroxylation reaction of phenol was obtained. The XRD pattern and SEM image of CAT-1 are shown in the attached figure. Example 2

[0037] (1) Mix 100g of titanium silicon molecular sieve TS-1 with 400g of ferric nitrate nonahydrate aqueous solution (mass concentration 1.0%), add the mixture to the crystallization kettle, heat to 100℃ and keep it at that temperature for 12h. After the heat treatment is completed, cool down and remove from the kettle, wash with water, filter, and dry at 100℃.

[0038] (2) Mix the dried material in (1) with 1800g of ammonium citrate aqueous solution (mass concentration 2.0%), keep the mixture at 70℃ for 6h, cool it down and remove it from the kettle, wash it with water, filter it, dry it at 100℃, and roast it at 500℃ for 4h.

[0039] (3) Mix 14g of tetrapropylammonium hydroxide aqueous solution (mass concentration 25%) with 69.5g of deionized water, add 20g of tetraethyl orthosilicate dropwise, stir for 2h after the dropwise addition is completed, add 10g of molecular sieve obtained in step (2), and stir evenly.

[0040] (4) The mixture in (3) was placed into a stainless steel high-pressure reactor, crystallized at 170°C for 72 h, cooled, filtered, washed, dried at 100°C, and calcined at 550°C for 4 h to obtain the catalyst CAT-2 for the hydroxylation reaction of phenol. Example 3

[0041] (1) Mix 100g of titanium silicon molecular sieve TS-1 with 300g of ferric nitrate nonahydrate aqueous solution (mass concentration 0.8%), add the mixture to the crystallization kettle, heat to 80℃ and keep it at that temperature for 10h. After the heat treatment is completed, cool down and remove from the kettle, wash with water, filter, and dry at 100℃.

[0042] (2) Mix the dried material in (1) with 1500g of ammonium oxalate aqueous solution (mass concentration 1.0%), keep the mixture at 80℃ for 6h, cool it down and remove it from the kettle, wash it with water, filter it, dry it at 100℃, and roast it at 500℃ for 4h.

[0043] (3) Mix 16g of tetrapropylammonium hydroxide aqueous solution (mass concentration 25%) with 88g of deionized water, add 25g of tetraethyl orthosilicate dropwise, stir for 2h after the dropwise addition is completed, add 10g of molecular sieve obtained in step (2), and stir evenly.

[0044] (4) The mixture in (3) was placed into a stainless steel high-pressure reactor, crystallized at 170°C for 96 h, cooled, filtered, washed, dried at 100°C, and calcined at 550°C for 4 h to obtain the catalyst CAT-3 for the hydroxylation reaction of phenol. Example 4

[0045] (1) Mix 100g of titanium silicon molecular sieve TS-1 with 300g of ferric nitrate nonahydrate aqueous solution (mass concentration 0.8%), add the mixture to the crystallization kettle, heat to 80℃ and keep it at that temperature for 10h. After the heat treatment is completed, cool down and remove from the kettle, wash with water, filter, and dry at 100℃.

[0046] (2) Mix the dried material in (1) with 1200g of ammonium acetate aqueous solution (mass concentration 0.6%), keep the mixture at 80℃ for 4h, cool it down and remove it from the kettle, wash it with water, filter it, dry it at 100℃, and calcine it at 500℃ for 4h.

[0047] (3) Mix 12g of tetrapropylammonium hydroxide aqueous solution (mass concentration 25%) with 51g of deionized water, add 15g of tetraethyl orthosilicate dropwise, stir for 2h after the dropwise addition is completed, add 10g of molecular sieve obtained in step (2), and stir evenly.

[0048] (4) The mixture in (3) was placed into a stainless steel high-pressure reactor, crystallized at 170°C for 72 h, cooled, filtered, washed, dried at 100°C, and calcined at 550°C for 4 h to obtain the catalyst CAT-4 for the hydroxylation reaction of phenol. Example 5

[0049] (1) Mix 100g of titanium silicon molecular sieve TS-1 with 300g of ferric nitrate nonahydrate aqueous solution (mass concentration 0.6%), add the mixture to the crystallization kettle, heat to 60℃ and keep warm for 8h. After the heat preservation is completed, cool down and remove from the kettle, wash with water, filter, and dry at 100℃.

[0050] (2) Mix the dried material in (1) with 1000g of ammonium acetate aqueous solution (mass concentration 0.6%), keep the mixture at 70℃ for 6h, cool it down and remove it from the kettle, wash it with water, filter it, dry it at 100℃, and calcine it at 500℃ for 4h.

[0051] (3) Mix 14g of tetrapropylammonium hydroxide aqueous solution (mass concentration 25%) with 69.5g of deionized water, add 20g of tetraethyl orthosilicate dropwise, stir for 2h after the dropwise addition is completed, add 10g of molecular sieve obtained in step (2), and stir evenly.

[0052] (4) The mixture in (3) was loaded into a stainless steel high-pressure reactor, crystallized at 170°C for 72 h, cooled, filtered, washed, dried at 100°C, and calcined at 550°C for 4 h to obtain the catalyst CAT-5 for the hydroxylation reaction of phenol. Comparative Example 1

[0053] (1) Mix 100g of titanium-silicon molecular sieve TS-1 with 300g of an aqueous solution of ferric nitrate nonahydrate (mass concentration 0.8%), add the mixture to a crystallization reactor, heat to 80℃ and hold for 10h. After holding, cool down, remove from the reactor, wash with water, filter, dry at 100℃, and calcine at 500℃ for 4h. The resulting catalyst is designated as D-1. Comparative Example 2

[0054] (1) Mix 100g of titanium silicon molecular sieve TS-1 with 300g of ferric nitrate nonahydrate aqueous solution (mass concentration 0.8%), add the mixture to the crystallization kettle, heat to 80℃ and keep it at that temperature for 10h. After the heat treatment is completed, cool down and remove from the kettle, wash with water, filter, and dry at 100℃.

[0055] (2) The dried material in (1) was mixed with 1800g of ammonium citrate aqueous solution (mass concentration 2.0%). The mixture was kept at 70℃ for 6h, cooled and removed from the reactor, washed with water, filtered, dried at 100℃, and calcined at 500℃ for 4h. The catalyst was obtained and denoted as D-2. Comparative Example 3

[0056] (1) Mix 14g of tetrapropylammonium hydroxide aqueous solution (mass concentration 25%) with 69.5g of deionized water, add 20g of tetraethyl orthosilicate dropwise, stir for 2h after the dropwise addition is completed, add 10g of titanium silicon molecular sieve TS-1, and stir evenly.

[0057] (2) The mixture in (1) was loaded into a stainless steel high-pressure reactor, crystallized at 170°C for 72 hours, cooled, filtered, washed, dried at 100°C, and calcined at 550°C for 4 hours to obtain the catalyst, which was designated as D-3. Comparative Example 4

[0058] (1) Mix 100g of titanium silicon molecular sieve TS-1 with 300g of ferric nitrate nonahydrate aqueous solution (mass concentration 0.8%), add the mixture to the crystallization kettle, heat to 80℃ and keep warm for 10h. After the heat preservation is completed, cool down and remove from the kettle, wash with water, filter, dry at 100℃, and calcine at 500℃ for 4h.

[0059] (2) Mix 14g of tetrapropylammonium hydroxide aqueous solution (mass concentration 25%) with 69.5g of deionized water, add 20g of tetraethyl orthosilicate dropwise, stir for 2h after the dropwise addition is completed, add 10g of titanium silicon molecular sieve TS-1 obtained in step (1), and stir evenly.

[0060] (3) The mixture in (2) was loaded into a stainless steel high-pressure reactor, crystallized at 170°C for 72 hours, cooled, filtered, washed, dried at 100°C, and calcined at 550°C for 4 hours to obtain the catalyst, which was designated as D-4.

[0061] The performance evaluation results of the samples obtained from the comparative examples and the embodiments are listed in Table 1.

[0062] Table 1. Catalytic performance evaluation results of each sample catalyst

Claims

1. A method for preparing a catalyst for the hydroxylation reaction of phenol, characterized in that, This includes mixing TS-1 molecular sieves with iron-doped framework with template agent and water, adding silicon source, hydrothermally crystallizing, drying, and calcining.

2. The preparation method according to claim 1, characterized in that, The preparation process of the framework-doped iron-rich TS-1 molecular sieve includes: (1) Mix TS-1 molecular sieve with an aqueous solution containing iron salt, perform hydrothermal treatment I, and dry I; (2) Mix the dried material with an organic acid ammonium aqueous solution, perform hydrothermal treatment II, drying II, and calcination II.

3. The preparation method according to claim 2, characterized in that, The mass ratio of TS-1 molecular sieve to iron salt is 0.015~0.05:1, and the liquid-solid mass ratio of TS-1 molecular sieve to aqueous solution containing iron salt is 2~4:

1. And / or, the iron salt is ferric nitrate nonahydrate.

4. The preparation method according to claim 2 or 3, characterized in that, The mass concentration of the organic acid ammonium aqueous solution is 0.5%~2.0%, and the liquid-solid mass ratio of the dried material to the organic acid ammonium aqueous solution is 10~20:1; And / or, the organic ammonium acid is selected from at least one of ammonium citrate, ammonium acetate, and ammonium oxalate.

5. The preparation method according to claim 1, characterized in that, The mass ratio of each material fed is: TS-1 molecular sieve with iron doped skeleton: silicon source: template agent: water = 1:1~3:0.15~0.5:2~10; And / or, the silicon source is tetraethyl orthosilicate, and the template agent is tetrapropylammonium hydroxide.

6. The preparation method according to any one of claims 1 to 5, characterized in that, The hydrothermal crystallization temperature is 160~180℃, the time is 48~120h, the drying temperature is 80~100℃, and the calcination temperature is 500~600℃.

7. The preparation method according to any one of claims 2 to 6, characterized in that, The temperature of the hydrothermal treatment I is 60~120℃, and the time is 4~12h; the temperature of the drying I is 80~120℃. And / or, the temperature of the hydrothermal treatment II is 50~100℃, the time is 2~8h, the temperature of the drying II is 80~120℃, and the temperature of the calcination II is 450~600℃.

8. A catalyst prepared by the method according to any one of claims 1 to 7, characterized in that, The catalyst has an MFI topology and a grain size of 200~400nm.

9. The use of a catalyst prepared by any one of claims 1 to 7 in the hydroxylation reaction of phenol.

10. The application according to claim 9, characterized in that, Using methanol as solvent and hydrogen peroxide as oxidant, with a phenol to hydrogen peroxide molar ratio of 1.9 to 2.1, the phenol conversion rate is greater than 44%, and the ortho-para ratio is greater than 2.5.

Citation Information

Patent Citations

  • Phenol hydroxylation catalyst, preparation method thereof and method for synthesizing hydroquinone

    CN109499572A

  • Method for synthesizing micron-sized TS-2 molecular sieve with hierarchical pores

    CN122102149A