Silicon carbide crystal growth device

By using porous graphite sheets and graphite rings in the silicon carbide crystal growth device, the problems of carbon inclusions and temperature gradient distribution during the silicon carbide crystal growth process in the traditional PVT method are solved, and the quality of the silicon carbide crystal and the service life of the crucible are improved. .

CN221918323UActive Publication Date: 2024-10-29ZHEJIANG IVSEMITEC CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202420572835.3
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-03-22
Publication Date
2024-10-29
Estimated Expiration
2034-03-22

AI Technical Summary

Technical Problem

Silicon carbide crystals grown by the traditional PVT method are prone to radial corrosion and micro-cracks at the edge of the seed crystal, and carbon inclusion defects are formed internally, which reduces the growth quality of the silicon carbide crystal.

Method used

A silicon carbide crystal growth device including a crucible, a first porous graphite sheet, a second porous graphite sheet and a seed crystal holder is designed. The porous graphite sheet is used to filter large particles and provide thermal insulation to improve the temperature gradient distribution. Reduce the formation of carbon inclusions and maintain Si/C balance through graphite rings.

Benefits of technology

It improves the growth quality of silicon carbide crystals, extends the service life of the crucible, and improves production efficiency and utilization of silicon carbide powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221918323U_ABST
    Figure CN221918323U_ABST
Patent Text Reader

Abstract

The utility model relates to the technical field of semiconductors, in particular to a silicon carbide crystal growing device which comprises a crucible, a first porous graphite sheet, a second porous graphite sheet and a seed crystal support. In the process of growing the silicon carbide crystal based on the PVT method, the first porous graphite flake and the second porous graphite flake filter large-particle carbon aggregates, so that the formation of carbon inclusion in the crystal is reduced, and the crystal quality is improved; meanwhile, the first porous graphite flakes and the second porous graphite flakes have a heat insulation effect, so that gradient distribution of temperature in the crucible is improved, the temperature of a silicon carbide powder area is increased, the silicon carbide powder is fully sublimated, the utilization rate of the silicon carbide powder is increased, Si / C balance of a silicon carbide seed crystal area is maintained, and the growth quality of silicon carbide crystals is improved; and the growth rate of the silicon carbide crystals is accelerated, so that the production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of semiconductors, in particular to a silicon carbide crystal growth device. Background Art

[0002] 4H-SiC has the characteristics of wide bandgap, high breakdown electric field, high thermal conductivity and high saturated electron drift velocity. In the manufacture of high-power, high-frequency and high-temperature semiconductor electronic devices, the performance of 4H-SiC far exceeds that of silicon crystals. 4H-SiC has great potential.

[0003] At present, the PVT (physical vapor transport) method for growing silicon carbide crystals is the most common process in the industry. The seed crystal is fixed on the top of a cylindrical crucible, and the silicon carbide powder is placed below the crucible. The silicon carbide powder is in the high-temperature area at the bottom. Under high temperature conditions, the silicon carbide powder undergoes non-stoichiometric sublimation and decomposition to generate gaseous components Si m C n , and then the gas phase component Si m C n Through transportation, the silicon carbide powder moves from the bottom area with high axial temperature to the silicon carbide seed crystal area at the top of the low temperature area, sublimation and crystallization occur on the growth interface of the silicon carbide seed crystal, so that the growth interface gradually advances to the silicon carbide powder area, and finally silicon carbide crystals grow.

[0004] However, SiC crystals grown by the traditional PVT method are prone to radial corrosion at the edge of the seed crystal, thereby inducing the formation of microtubes or even microcracks. In addition, carbon inclusion defects are also formed inside the growing SiC crystals, reducing the growth quality of the SiC crystals. Utility Model Content

[0005] In order to solve the above technical problems, the utility model provides a silicon carbide crystal growth device, comprising:

[0006] Crucible, a first porous graphite sheet, a second porous graphite sheet, and a seed crystal holder;

[0007] The crucible has an opening at the top, silicon carbide powder is contained in the crucible, the inner wall of the crucible has a first assembly structure, and the height of the silicon carbide powder is smaller than the first assembly structure of the inner wall of the crucible; the seed crystal support cover is arranged at the opening of the crucible, and a silicon carbide seed crystal is arranged on the side of the seed crystal support facing the silicon carbide powder;

[0008] The first porous graphite sheet is disposed on the surface of the silicon carbide powder;

[0009] The second porous graphite sheet cooperates with the first assembly structure of the crucible.

[0010] Optionally, the crucible is a graphite crucible.

[0011] Optionally, the pore size of the first porous graphite sheet and the second porous graphite sheet ranges from 70 μm to 150 μm, and the porosity ranges from 30% to 50%.

[0012] Optionally, the first porous graphite sheet and the second porous graphite sheet are coated with a TaC coating.

[0013] Optionally, the first assembly structure is a stepped structure or a slotted structure; and the second porous graphite sheet has an edge structure that matches the first assembly structure of the crucible.

[0014] Optionally, it further includes a first graphite ring, wherein the first graphite ring is disposed between the first porous graphite sheet and the second porous graphite sheet;

[0015] The outer side wall of the first graphite ring is adapted to the first assembly structure of the crucible, and the first graphite ring cooperates with the first assembly structure of the crucible.

[0016] Optionally, the upper surface of the first graphite ring serves as a first assembly structure of the inner wall of the crucible.

[0017] Optionally, the inner side wall of the first graphite ring is in the shape of an inverted truncated cone; the thickness of the first graphite ring ranges from 5 mm to 15 mm.

[0018] Optionally, it further includes a second graphite ring, wherein the second graphite ring is disposed between the second porous graphite sheet and the seed crystal holder;

[0019] The second porous graphite sheet is disposed on the surface of the first graphite ring;

[0020] The second graphite ring is arranged on the surface of the second porous graphite sheet.

[0021] Optionally, the thickness of the second graphite ring ranges from 5 mm to 15 mm.

[0022] In summary, the advantages and beneficial effects of the utility model are:

[0023] The utility model provides a silicon carbide crystal growth device, which comprises a crucible, a first porous graphite sheet, a second porous graphite sheet and a seed crystal holder. In the process of growing silicon carbide crystals based on the PVT method, the first porous graphite sheet and the second porous graphite sheet filter large-particle carbon aggregates, reduce the formation of carbon inclusions inside the silicon carbide crystals, and improve the crystallization quality; at the same time, the first porous graphite sheet and the second porous graphite sheet have a heat-insulating effect, improve the gradient distribution of the temperature inside the crucible, increase the temperature of the silicon carbide powder area, make the silicon carbide powder fully sublime, improve the utilization rate of the silicon carbide powder, maintain the Si / C balance in the silicon carbide seed crystal area, and improve the growth quality of the silicon carbide crystal; while the first porous graphite sheet and the second porous graphite sheet increase the temperature of the silicon carbide powder area, they reduce the temperature of the surface of the silicon carbide seed crystal, so that the radial temperature gradient in the crucible is enlarged and the radial temperature gradient is more uniform, thereby improving the radial temperature gradient in the crucible, which is more conducive to the growth of silicon carbide crystals, thereby improving the production efficiency of silicon carbide crystals.

[0024] In addition, the first graphite ring and the second graphite ring provide a carbon source for the growth environment, further maintaining the Si / C balance in the silicon carbide seed crystal region, improving the growth quality of the silicon carbide crystal, and correspondingly reducing the corrosion of the crucible during the growth of the silicon carbide crystal, thereby improving the service life of the crucible. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A schematic cross-sectional structure diagram of a silicon carbide crystal growth device provided in this embodiment;

[0026] Figure 2a A schematic diagram of temperature simulation of a side of the silicon carbide seed crystal facing the silicon carbide powder material in a silicon carbide crystal growth device provided in this embodiment without a second porous graphite sheet;

[0027] Figure 2b A schematic diagram of temperature simulation on the surface of the silicon carbide powder material in a silicon carbide crystal growth device provided in this embodiment without a second porous graphite sheet;

[0028] Figure 2c A schematic diagram of temperature simulation of a silicon carbide crystal growth device provided in this embodiment, with a side of the silicon carbide seed crystal of the second porous graphite sheet facing the silicon carbide powder;

[0029] Figure 2d A schematic diagram of temperature simulation on the surface of the silicon carbide powder of a silicon carbide crystal growth device provided in this embodiment having a second porous graphite sheet. DETAILED DESCRIPTION

[0030] In the early stage of silicon carbide crystal growth, Si in silicon carbide powder is preferentially sublimated, making the atmosphere near the silicon carbide seed crystal rich in Si. As the silicon carbide powder continues to sublimate, the Si in the silicon carbide powder is continuously consumed, resulting in an unstable Si / C ratio near the silicon carbide seed crystal. At the same time, as the silicon carbide crystal grows, the silicon carbide powder is graphitized, and the graphite crucible or other graphite parts are corroded, resulting in excessive carbon. A carbon-rich environment is gradually formed in the graphite crucible, and excessive carbon particles agglomerate to form carbon aggregates. The carbon aggregates are brought to the silicon carbide crystal growth area by the growth atmosphere, resulting in the growing silicon carbide crystals being wrapped in carbon, which in turn leads to a decrease in the growth quality of the silicon carbide crystal. Therefore, the utility model provides a silicon carbide crystal growth device to solve the above problems.

[0031] In order to facilitate understanding by those skilled in the art, the present invention will be further described in detail below in conjunction with specific embodiments.

[0032] The terms "first", "second", and similar words used in the specification and claims of this application do not indicate any order, quantity or importance, but are only used to distinguish different components. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present application, unless otherwise specified, the meaning of "multiple" is two or more. Positional terms such as "upper", "lower", "horizontal direction", "vertical direction", "same vertical line" are defined relative to the orientation schematically placed in the accompanying drawings, and it should be understood that these directional terms are relative concepts, which are used for description and clarification relative to, and may change accordingly according to changes in the orientation in which the device is placed.

[0033] The utility model provides a silicon carbide crystal growth device, such as Figure 1 As shown, including:

[0034] Crucible 80, first porous graphite sheet 60, second porous graphite sheet 40, first graphite ring 50, second graphite ring 30, seed crystal holder 10;

[0035] The crucible 80 has an opening at the top, and the crucible 80 contains silicon carbide powder 70. The inner wall of the crucible has a first assembly structure, and the height of the silicon carbide powder 70 is smaller than the first assembly structure of the inner wall of the crucible 80. The seed crystal holder 10 is covered at the opening of the crucible 80, and a silicon carbide seed crystal 20 is arranged on the side of the seed crystal holder 10 facing the silicon carbide powder 70.

[0036] The first porous graphite sheet 60 is disposed on the surface of the silicon carbide powder 70;

[0037] The outer side wall of the first graphite ring 50 is adapted to the first assembly structure of the crucible 80, and the first graphite ring 50 cooperates with the first assembly structure of the crucible 80;

[0038] The second porous graphite sheet 40 is disposed on the surface of the first graphite ring 50;

[0039] The second graphite ring 30 is disposed on the surface of the second porous graphite sheet 40 .

[0040] Specifically, in this embodiment, the crucible 80 is a graphite crucible.

[0041] In this embodiment, the seed crystal holder 10 is directly disposed to cover the opening of the crucible 80 .

[0042] In other embodiments, the seed crystal holder has a second assembly structure, the second assembly structure is adapted to the second graphite ring and the opening of the crucible, and the seed crystal holder cover is arranged at the opening of the crucible and cooperates with the second graphite ring and the opening of the crucible.

[0043] In other embodiments, the second assembly structure is a stepped structure, a slot-shaped structure or other suitable structures, and the shape and size of the second assembly structure can be adjusted as needed.

[0044] In this embodiment, the particle size of the silicon carbide powder 70 contained in the crucible 80 ranges from 8 meshes to 40 meshes.

[0045] In this embodiment, the distance between the surface of the silicon carbide powder 70 and the surface of the silicon carbide seed crystal 20 facing the silicon carbide powder 70 is 10 cm.

[0046] In this embodiment, the height of the first porous graphite sheet 60 and the second porous graphite sheet 40 ranges from 2 mm to 5 mm, and the height of the first porous graphite sheet 60 and the second porous graphite sheet 40 is along the axial direction of the silicon carbide crystal growth device.

[0047] In this embodiment, the first porous graphite sheet 60 and the second porous graphite sheet 40 are coated with TaC coating to reduce corrosion of the first porous graphite sheet 60 and the second porous graphite sheet 40 during the growth of silicon carbide crystals.

[0048] In this embodiment, the pore sizes of the first porous graphite sheet 60 and the second porous graphite sheet 40 are in the range of 70 μm to 150 μm, and the porosity is in the range of 30% to 50%.

[0049] When the silicon carbide crystal grows, the silicon carbide powder 70 in the crucible 80 is continuously sublimated. Since the C in the silicon carbide powder 70 is not easy to sublime, after the silicon carbide crystal grows for a period of time, the silicon carbide powder 70 in the crucible 80 gradually forms a carbon-rich environment, causing carbon particles to agglomerate to form carbon aggregates. The first porous graphite sheet 60 and the second porous graphite sheet 40 in the silicon carbide crystal growth device have a certain porosity, so that the larger-sized carbon aggregates formed in the silicon carbide powder 70 are filtered, thereby preventing the carbon aggregates from being brought to the silicon carbide crystal growth area by the growth atmosphere, reducing the formation of carbon encapsulation in the silicon carbide crystal, and thereby improving the growth quality of the silicon carbide crystal.

[0050] In the present embodiment, the first porous graphite sheet 60 and the second porous graphite sheet 40 increase the temperature of the silicon carbide powder 70 region, promote the sublimation of C in the silicon carbide powder 70, so that more C components are contained in the gas phase, and the Si / C ratio in the gas phase component is reduced to maintain the Si / C balance in the gas phase component and improve the utilization rate of the silicon carbide powder 70; at the same time, the temperature of the side of the silicon carbide seed crystal 20 facing the silicon carbide powder 70 is reduced, and the radial temperature gradient in the crucible 80 is increased, which is beneficial to the convex growth of the silicon carbide crystal growth interface.

[0051] The model of the silicon carbide crystal growth device is imported into COMSOL software for temperature simulation, such as Figure 2a to 2d As shown, a temperature comparison diagram of the side of the silicon carbide seed crystal 20 facing the silicon carbide powder 70 and the surface of the silicon carbide powder 70 when the second porous graphite sheet 40 is present and when the second porous graphite sheet 40 is present between the first graphite ring 50 and the second graphite ring 30 is obtained. From the temperature comparison diagram, it can be seen that the surface temperature of the silicon carbide powder 70 with the second porous graphite sheet 40 is higher than the temperature of the silicon carbide powder 70 without the second porous graphite sheet 40, and the radial temperature difference in the silicon carbide powder 70 area is small, which is conducive to the sublimation of the silicon carbide powder 70, thereby maintaining the Si / C ratio in the gas phase component, and also improving the utilization rate of the silicon carbide powder 70, and also accelerating the growth rate of the silicon carbide crystal.

[0052] The temperature of the side of the silicon carbide seed crystal 20 facing the silicon carbide powder 70 when having the second porous graphite sheet 40 is lower than the temperature of the side of the seed crystal 20 facing the silicon carbide powder 70 when not having the second porous graphite sheet 40. As can be seen from the figure, the temperature of the surface of the silicon carbide seed crystal 20 with the second porous graphite sheet 40 shows an overall downward trend compared with the temperature of the surface of the silicon carbide seed crystal 20 without the second porous graphite sheet 40, and the temperature reduction range of the central area of ​​the surface of the silicon carbide seed crystal 20 is higher than that of the edge area of ​​the surface of the silicon carbide seed crystal 20, that is, the radial temperature difference of the surface of the silicon carbide seed crystal 20 is greater than that without the second porous graphite sheet 40, which is more conducive to the convex growth of the silicon carbide crystal in the early stage; and the temperature distribution curve of the surface of the silicon carbide seed crystal 20 of the silicon carbide crystal growth device when having the second porous graphite sheet 40 is smoother, that is, the temperature fluctuation of the edge area of ​​the surface of the silicon carbide seed crystal 20 is smaller, which is more conducive to the convex growth of the silicon carbide crystal.

[0053] The second porous graphite sheet 40 increases the temperature of the silicon carbide powder 70 area at the bottom of the crucible 80, while lowering the temperature of the surface of the silicon carbide seed crystal 20. As can be seen from the figure, in the early stage of the growth of the silicon carbide crystal, that is, within 10 hours after the start of the growth of the silicon carbide crystal, the radial temperature gradient in the crucible 80 is enlarged. As the thickness of the silicon carbide crystal increases, the radial temperature gradient becomes more uniform as the silicon carbide crystal growth interface extends toward the surface of the silicon carbide powder 70, thereby improving the radial temperature gradient in the crucible 80 and being more conducive to the growth of silicon carbide crystals.

[0054] Therefore, it can be seen from the temperature simulation results that when the second porous graphite sheet 40 is provided between the first graphite ring 50 and the second graphite ring 30, the Si / C ratio in the gas phase component is maintained, the utilization rate of the silicon carbide powder 70 is improved, the convex growth of the silicon carbide crystal is facilitated, and the growth quality of the silicon carbide crystal is improved.

[0055] In this embodiment, the inner vertical surface of the first graphite ring 50 is in the shape of an inverted truncated cone.

[0056] In the present embodiment, the thickness range of the first graphite ring 50 is 5 mm to 15 mm, and the wall thickness of the first graphite ring 50 close to the surface of the silicon carbide powder 70 is smaller than the wall thickness of the first graphite ring 50 away from the surface of the silicon carbide powder 70, wherein the thickness of the first graphite ring 50 is the wall thickness of the first graphite ring 50, i.e., along the radial direction of the silicon carbide crystal growth device.

[0057] In this embodiment, the thickness of the second graphite ring 30 ranges from 5 mm to 15 mm. The thickness of the second graphite ring 30 is the wall thickness of the second graphite ring 30 , that is, along the radial direction of the silicon carbide crystal growth device.

[0058] Since the temperature of the edge of the crucible 80 is higher than that of the center of the crucible 80, the silicon carbide powder 70 in the edge area of ​​the crucible 80 sublimates first before the silicon carbide powder 70 in the center of the crucible 80, which results in the carbonization of the silicon carbide powder 70 in the edge area of ​​the crucible 80 earlier and more serious than the carbonization of the silicon carbide powder 70 in the center area. By setting the inner surface of the first graphite ring 50 in an inverted truncated cone shape, the inner diameter of the first graphite ring 50 close to the surface of the silicon carbide powder 70 is smaller than the inner diameter of the first graphite ring 50 away from the surface of the silicon carbide powder 70. The inner diameter on one side, that is, the width of the graphite substrate on the surface side of the first graphite ring 50 close to the silicon carbide powder 70 is greater than the width of the graphite substrate on the surface side of the first graphite ring 50 away from the silicon carbide powder 70. The wider graphite substrate on the surface side of the first graphite ring 50 close to the silicon carbide powder 70 blocks the carbon aggregates in the silicon carbide powder 70 area from being transported from the edge of the first porous graphite sheet 60 through the gaps in the first porous graphite sheet 60 to the silicon carbide crystal growth area, thereby preventing the carbon aggregates from entering the interior of the growing silicon carbide crystals and improving the growth quality of the silicon carbide crystals.

[0059] In this embodiment, the first graphite ring 50 and the second graphite ring 30 are detachable graphite parts, and the first graphite ring 50 and the second graphite ring 30 are replaced in one furnace.

[0060] In other embodiments, the first graphite ring and the second graphite ring are replaced in multiple furnaces.

[0061] The first graphite ring 50 and the second graphite ring 30 provide a carbon source during the growth of silicon carbide crystals, continuously replenish C into the growth atmosphere, further reduce the Si / C ratio in the gas phase components, balance the Si / C ratio in the growth environment, and correspondingly reduce the corrosion of the crucible 80 during the growth of silicon carbide crystals, thereby increasing the service life of the crucible 80.

[0062] In this embodiment, the first assembly structure is a stepped structure, a slot-shaped structure or other suitable structures, and the shape and size of the first assembly structure can be adjusted as needed.

[0063] In other embodiments, the upper surface of the first graphite ring serves as the first assembly structure of the inner wall of the crucible.

[0064] In other embodiments, the corresponding silicon carbide crystal growth device does not have the first graphite ring, the second porous graphite sheet cooperates with the first assembly structure of the crucible, and the second porous graphite sheet has an edge structure adapted to the first assembly structure of the crucible.

[0065] In other embodiments, the corresponding silicon carbide crystal growth device does not have the second graphite ring.

[0066] The utility model also provides a silicon carbide crystal growth method, using the above-mentioned silicon carbide crystal growth device, comprising:

[0067] Step S10, providing a silicon carbide crystal growth device filled with silicon carbide powder;

[0068] Step S20, placing the silicon carbide crystal growth device containing silicon carbide powder in a suitable position in the growth furnace;

[0069] Step S30, regulating the growth conditions in the growth furnace to grow silicon carbide crystals;

[0070] Step S40, cooling and returning the pressure of the growth furnace;

[0071] Step S50, depressurizing the growth furnace to atmospheric pressure and taking out the silicon carbide crystal.

[0072] Specifically, step S10 is performed to provide a silicon carbide crystal growth device containing silicon carbide powder 70 .

[0073] In this embodiment, the silicon carbide powder 70 is loaded into the crucible 80, and the first porous graphite sheet 60, the second porous graphite sheet 40, the first graphite ring 50, the second graphite ring 30, the seed crystal holder 10 are assembled with the crucible 80 to obtain a silicon carbide crystal growth device containing the silicon carbide powder 70.

[0074] In this embodiment, the height of the silicon carbide powder 70 is smaller than the first assembly structure of the inner wall of the crucible 80 .

[0075] There is a certain distance between the surface of the silicon carbide powder 70 and the side of the silicon carbide seed crystal 20 facing the silicon carbide powder 70 .

[0076] In this embodiment, the first porous graphite sheet 60 and the second porous graphite sheet 40 are coated with TaC coating to reduce corrosion of the first porous graphite sheet 60 and the second porous graphite sheet 40 during the growth of silicon carbide crystals.

[0077] In this embodiment, the pore sizes of the first porous graphite sheet 60 and the second porous graphite sheet 40 are in the range of 70 μm to 150 μm, and the porosity is in the range of 30% to 50%.

[0078] When the silicon carbide crystal grows, the silicon carbide powder 70 in the crucible 80 continues to sublime. Since C in the silicon carbide powder 70 is not easy to sublime, after the silicon carbide crystal grows for a period of time, the silicon carbide powder 70 in the crucible 80 gradually forms a carbon-rich environment, causing carbon particles to agglomerate to form carbon aggregates. The first porous graphite sheet 60 and the second porous graphite sheet 40 have a certain porosity, so that larger-sized carbon aggregates formed in the silicon carbide powder 70 are filtered to prevent the carbon aggregates from being carried to the silicon carbide crystal growth area by the growth atmosphere, thereby reducing the formation of carbon inclusions in the growing silicon carbide crystals, thereby improving the growth quality of the silicon carbide crystals.

[0079] Execute step S20 to place the silicon carbide crystal growth device in a growth furnace.

[0080] In this embodiment, the silicon carbide crystal growth device containing the silicon carbide powder 70 is placed in a growth furnace, and the position of the silicon carbide crystal growth device is adjusted by a stepping motor to provide a suitable position for subsequent silicon carbide crystal growth.

[0081] Step S30 is executed to adjust the growth conditions in the growth furnace to grow silicon carbide crystals.

[0082] In this embodiment, the step of regulating the growth conditions in the growth furnace includes:

[0083] Step S301, evacuating the growth furnace;

[0084] In this embodiment, the step of evacuating the growth furnace includes:

[0085] performing a first vacuuming of the growth furnace to a first target pressure;

[0086] The molecular pump of the growth furnace is turned on to perform a second vacuum pumping on the growth furnace to a second target pressure. In this embodiment, the first target pressure in the growth furnace is in the range of 0.5 Pa to 5 Pa, and the second target pressure in the growth furnace is in the range of 5*10 -3 Pa~5*10 -2 Pa.

[0087] Step S302, maintaining the internal pressure of the growth furnace, and first heating the growth furnace to a first target temperature;

[0088] In this embodiment, the temperature range of the first target temperature is 1100° C. to 1200° C., and the temperature rise rate of the first heating is in the range of 6° C. / min to 7° C. / min.

[0089] In this embodiment, when the growth furnace is heated for the first time, the molecular pump of the growth furnace is maintained to evacuate the growth furnace to maintain the internal pressure of the growth furnace.

[0090] Step S303, maintaining the internal pressure of the growth furnace, and performing a second heating on the growth furnace to a second target temperature;

[0091] In this embodiment, the temperature range of the second target temperature is 1500° C. to 1700° C., and the temperature rise rate of the second heating is in the range of 2° C. / min to 3° C. / min.

[0092] In this embodiment, when the growth furnace is subjected to the second heating, the molecular pump of the growth furnace is turned off, and the growth furnace is evacuated by a mechanical pump to maintain the internal pressure of the growth furnace.

[0093] Step S304, maintaining the second target temperature in the growth furnace, introducing argon gas and doping gas into the growth furnace, and controlling the pressure in the growth furnace to be the first target pressure;

[0094] In this embodiment, the flow rate of the argon gas is in the range of 100 ml / min to 200 ml / min, and the flow rate of the doping gas is in the range of 5 ml / min to 10 ml / min.

[0095] In this embodiment, the doping gas is nitrogen. In this embodiment, the first target pressure ranges from 200 mbar to 400 mbar.

[0096] Step S305 , performing a third heating on the growth furnace to a third target temperature, and controlling the pressure in the growth furnace to be a second target pressure.

[0097] In this embodiment, the third target temperature ranges from 1900° C. to 2000° C., the third heating time ranges from 1 h to 5 h, and the second target pressure ranges from 100 mbar to 200 mbar.

[0098] Step S306, performing a fourth heating on the growth furnace so that a temperature gradient is formed in the growth furnace, wherein the temperature of the upper part of the growth furnace is lower than the temperature of the lower part of the growth furnace.

[0099] In this embodiment, after the fourth heating, the temperature range of the upper part of the growth furnace is 2100° C. to 2200° C., the temperature range of the lower part of the growth furnace is 2200° C. to 2300° C., and the time range of the fourth heating is 5 h to 15 h.

[0100] Step S307, maintaining the gradient temperature in the growth furnace and decreasing the pressure in the growth furnace in a stepwise manner;

[0101] In this embodiment, the step-by-step decline includes:

[0102] reducing the second target pressure to a third target pressure;

[0103] In this embodiment, the third target pressure ranges from 50 mbar to 100 mbar, and the time range for reducing the second target pressure to the third target pressure is from 1 hour to 5 hours;

[0104] reducing the third target pressure to a fourth target pressure;

[0105] In this embodiment, the fourth target pressure ranges from 25 mbar to 50 mbar, and the time range for reducing the third target pressure to the fourth target pressure is from 1 hour to 5 hours.

[0106] reducing the fourth target pressure to a fifth target pressure;

[0107] In this embodiment, the fifth target pressure ranges from 5 to 10 mbar, and the time range for reducing the fourth target pressure to the fifth target pressure is from 5 to 10 hours.

[0108] When the fourth target temperature and the fifth target pressure are reached, the silicon carbide crystals begin to grow. During the growth of the silicon carbide crystals, the first porous graphite sheet 60 and the second porous graphite sheet 40 have a certain porosity, so that the larger carbon aggregates formed in the silicon carbide powder 70 are filtered, preventing the carbon aggregates from being carried to the silicon carbide crystal growth area by the growth atmosphere, thereby reducing the formation of carbon inclusions in the growing silicon carbide crystals, thereby improving the growth quality of the silicon carbide crystals.

[0109] At the same time, the first graphite ring 50 and the second graphite ring 30 provide a carbon source during the growth of silicon carbide crystals, continuously replenishing C into the growth atmosphere, further reducing the Si / C ratio in the gas phase components, balancing the Si / C ratio in the growth environment, and also reducing the corrosion of the crucible 80 by the silicon carbide powder 70, thereby increasing the service life of the crucible 80.

[0110] Furthermore, the inner vertical surface of the first graphite ring 50 is in the shape of an inverted truncated cone. Since the temperature of the edge of the crucible 80 is higher than that of the center of the crucible 80, the silicon carbide powder 70 in the edge area of ​​the crucible 80 sublimates first before the silicon carbide powder 70 in the center of the crucible 80, which results in the carbonization of the silicon carbide powder 70 in the edge area of ​​the crucible 80 earlier and more seriously than the silicon carbide powder 70 in the center area. The inner vertical surface of the first graphite ring 50 is set to be in the shape of an inverted truncated cone, that is, the inner diameter of the first graphite ring 50 close to the surface of the silicon carbide powder 70 is smaller, so that The width of the graphite substrate of the first graphite ring 50 close to the surface side of the silicon carbide powder 70 is greater than the width of the graphite substrate of the first graphite ring 50 away from the surface side of the silicon carbide powder 70. The wider graphite substrate of the first graphite ring 50 close to the surface side of the silicon carbide powder 70 blocks the carbon aggregates in the silicon carbide powder 70 area from being transported from the edge of the first porous graphite sheet 60 through the gaps in the first porous graphite sheet 60 to the silicon carbide crystal growth area, thereby preventing the carbon aggregates from entering the interior of the growing silicon carbide crystals and improving the growth quality of the silicon carbide crystals.

[0111] Step S308, maintaining the pressure and temperature in the growth furnace after the step-wise decrease;

[0112] In this embodiment, the time range for maintaining the pressure and temperature in the growth furnace after the step-wise decrease is 80 hours to 120 hours.

[0113] Step S40 is executed to reduce the temperature and return the pressure of the growth furnace.

[0114] In this embodiment, the time range of the temperature reduction and pressure return is 10 hours to 20 hours. After the temperature reduction and pressure return, the temperature in the growth furnace drops to room temperature, and the pressure in the growth furnace is 800 mbar.

[0115] Step S50 is executed to release the pressure of the growth furnace to atmospheric pressure and take out the silicon carbide crystal.

[0116] In the present embodiment, the first porous graphite sheet 60 and the second porous graphite sheet 40 increase the temperature of the silicon carbide powder 70 region, promote the sublimation of C in the silicon carbide powder 70, so that the gas phase contains more C components, and reduce the Si / C ratio in the gas phase component to maintain the Si / C balance in the gas phase component and improve the utilization rate of the silicon carbide powder 70; at the same time, the temperature of the side of the silicon carbide seed crystal 20 facing the silicon carbide powder 70 is reduced, and the radial temperature gradient in the crucible 80 is increased, which is beneficial to the convex growth of the silicon carbide crystal growth interface.

[0117] In this embodiment, the first graphite ring 50 and the second graphite ring 30 are detachable graphite parts, and the first graphite ring 50 and the second graphite ring 30 are replaced in one furnace. In other embodiments, the first graphite ring 50 and the second graphite ring 30 are replaced in multiple furnaces.

[0118] This embodiment utilizes the provided silicon carbide crystal growth device to improve the quality of the prepared silicon carbide crystals, and correspondingly reduces the corrosion of the crucible during the growth of the silicon carbide crystals, thereby increasing the service life of the crucible.

[0119] Finally, it should be noted that any modification or equivalent replacement of part or all of the technical features based on the device structure of the utility model and the technical solution of the described embodiment, which does not deviate from the essence of the corresponding technical solution of the utility model, belongs to the patent scope of the device structure of the utility model and the described implementation scheme.

Claims

1. A silicon carbide crystal growth device, characterized in that: include: Crucible, a first porous graphite sheet, a second porous graphite sheet, and a seed crystal holder; The crucible has an opening at the top, silicon carbide powder is contained in the crucible, the inner wall of the crucible has a first assembly structure, and the height of the silicon carbide powder is smaller than the first assembly structure of the inner wall of the crucible; the seed crystal support cover is arranged at the opening of the crucible, and a silicon carbide seed crystal is arranged on the side of the seed crystal support facing the silicon carbide powder; The first porous graphite sheet is disposed on the surface of the silicon carbide powder; The second porous graphite sheet cooperates with the first assembly structure of the crucible.

2. A silicon carbide crystal growth device as claimed in claim 1, characterized in that: The crucible is a graphite crucible.

3. A silicon carbide crystal growth device as claimed in claim 1, characterized in that: The pore sizes of the first porous graphite sheet and the second porous graphite sheet are in the range of 70 μm to 150 μm, and the porosity is in the range of 30% to 50%.

4. A silicon carbide crystal growth device as claimed in claim 1, characterized in that: The first porous graphite sheet and the second porous graphite sheet are coated with a TaC coating.

5. The silicon carbide crystal growth device according to claim 1, characterized in that: The first assembly structure is a step-shaped structure or a slot-shaped structure; the second porous graphite sheet has an edge structure that matches the first assembly structure of the crucible.

6. A silicon carbide crystal growth device as claimed in claim 1, characterized in that: Also includes a first graphite ring, the first graphite ring is disposed between the first porous graphite sheet and the second porous graphite sheet; The outer side wall of the first graphite ring is adapted to the first assembly structure of the crucible, and the first graphite ring cooperates with the first assembly structure of the crucible.

7. A silicon carbide crystal growth device as claimed in claim 6, characterized in that: The upper surface of the first graphite ring serves as a first assembly structure of the inner side wall of the crucible.

8. A silicon carbide crystal growth device as claimed in claim 6, characterized in that: The inner side wall of the first graphite ring is in the shape of an inverted truncated cone; the thickness of the first graphite ring ranges from 5 mm to 15 mm.

9. A silicon carbide crystal growth device as claimed in claim 6, characterized in that: Also includes a second graphite ring, the second graphite ring is arranged between the second porous graphite sheet and the seed crystal holder; The second porous graphite sheet is disposed on the surface of the first graphite ring; The second graphite ring is arranged on the surface of the second porous graphite sheet.

10. A silicon carbide crystal growth device as claimed in claim 9, characterized in that: The thickness of the second graphite ring ranges from 5 mm to 15 mm.

Citation Information

Cited By

  • Silicon carbide single crystal growth device and method for improving powder utilization rate

    CN119553358A

  • Silicon carbide single crystal growth apparatus and method for improving powder utilization

    CN119553358B

  • Method and device for growing silicon carbide crystals

    CN120649144A