Adhesive sheet, manufacturing method of adhesive sheet and manufacturing method of article

The adhesive sheet with controlled tack and hardness properties addresses slipperiness and blocking issues, ensuring easy handling and preventing damage during bending and curing.

JP2024154430AActive Publication Date: 2024-10-30DAI NIPPON PRINTING CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024072440
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-04-26
Publication Date
2024-10-30
Estimated Expiration
2043-04-18

AI Technical Summary

Technical Problem

Adhesive sheets used for bonding two members face challenges such as poor slipperiness, blocking resistance, and risk of cracking, lifting, or peeling during storage, winding, and bending, especially when high tackiness and bending are required.

Method used

An adhesive sheet with a base material and a first adhesive layer having a tack of less than 0.1N and Martens hardness between 20N/mm² and 130N/mm², which improves slipperiness and blocking resistance while preventing cracking and peeling during handling and curing.

Benefits of technology

The adhesive sheet achieves good slipperiness and anti-blocking properties, allowing easy insertion and alignment between members, and suppresses cracking, lifting, and peeling during winding and bending.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154430000001_ABST
    Figure 2024154430000001_ABST
Patent Text Reader

Abstract

To provide an adhesive sheet having excellent slipperiness and anti-blocking properties at an adhesion layer while capable of inhibiting a crack, lifting or removal of the adhesion layer in winding up or bending.SOLUTION: An adhesive sheet includes a base material and a first adhesion layer arranged on one side of the base material and containing a first curable adhesive agent. The first adhesion layer has tackiness of less than 0.1 N. The first adhesion layer has Martens hardness of 20 N / mm2 to 130 N / mm2, inclusive.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an adhesive sheet and a method for producing the same, as well as a method for producing an article using the adhesive sheet. [Background technology]

[0002] Adhesives that bond two components together are used in a variety of fields. Liquid adhesives are the mainstream of adhesives. However, liquid adhesives can cause problems such as uneven application, overflow, and dripping, making the bonding process more complicated.

[0003] Meanwhile, in recent years, the use of sheet-type adhesives, i.e., adhesive sheets, instead of liquid adhesives has been proposed. Furthermore, adhesive sheets containing a foaming agent (foamable adhesive sheets) have also been proposed (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2016 / 163514 [Patent Document 2] JP 2019-203062 A Summary of the Invention [Problem to be solved by the invention]

[0005] As a method for bonding two members using an adhesive sheet, for example, an adhesive sheet is placed between two members, and then the adhesive sheet is cured to bond the two members. In this method, for example, an adhesive sheet may be inserted into the gap between two members, or one member and an adhesive sheet may be inserted into a hole or groove of the other member. In these cases, if the adhesive sheet has high tack, the adhesive sheet has poor slipperiness, making it difficult to insert the adhesive sheet.

[0006] Furthermore, since there is a risk of blocking occurring during storage, it is desirable for the adhesive sheet to have good blocking resistance.

[0007] Furthermore, the adhesive sheet may be stored in a rolled state. When the adhesive sheet is placed between two members, the adhesive sheet may be folded to match the shape of the members. In these cases, the adhesive sheet may crack. In addition, when the adhesive sheet has an adhesive layer on one or both sides of the substrate, the adhesive layer may float or peel off from the substrate when the adhesive sheet is rolled up or folded. Therefore, it is also desirable that the adhesive layer is unlikely to crack, float, or peel off when the adhesive sheet is rolled up or folded.

[0008] The present disclosure has been made in consideration of the above-mentioned circumstances, and has as its main object to provide an adhesive sheet in which the adhesive layer has good slip properties and blocking resistance and which can suppress cracking, lifting, and peeling of the adhesive layer when rolled up or folded. [Means for solving the problem]

[0009] One embodiment of the present disclosure is an adhesive sheet having a substrate and a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, the first adhesive layer having a tack of less than 0.1 N and a Martens hardness of 20 N / mm 2 More than 130N / mm 2 An adhesive sheet is provided, which is:

[0010] Another embodiment of the present disclosure is a method for producing an adhesive sheet, comprising a first adhesive layer forming step of applying a first adhesive composition containing a first curable adhesive to one surface side of a substrate and drying the applied composition to form a first adhesive layer, wherein the tack of the first adhesive layer is less than 0.1 N, and in the first adhesive layer forming step, the Martens hardness of the first adhesive layer is less than 20 N / mm 2 More than 130N / mm 2 The present invention provides a method for producing an adhesive sheet, which comprises drying the first adhesive composition as follows:

[0011] Another embodiment of the present disclosure provides a method for manufacturing an article, comprising: a step of placing the above-mentioned adhesive sheet between a first member and a second member; and a step of curing the adhesive sheet to bond the first member and the second member. Effect of the Invention

[0012] The adhesive sheet of the present disclosure has an adhesive layer with good slip properties and blocking resistance, and exhibits the effect of being able to suppress cracking, lifting, and peeling of the adhesive layer when it is wound up or folded. [Brief description of the drawings]

[0013] [Figure 1] 1 is a schematic cross-sectional view showing an example of an adhesive sheet according to the present disclosure. [Diagram 2] FIG. 2 is a schematic perspective view showing another example of an adhesive sheet according to the present disclosure. [Diagram 3] 3 is a schematic cross-sectional view showing another example of an adhesive sheet according to the present disclosure. FIG. [Figure 4] 3 is a schematic cross-sectional view showing another example of an adhesive sheet according to the present disclosure. FIG. [Diagram 5] 3 is a schematic cross-sectional view showing another example of an adhesive sheet according to the present disclosure. FIG. [Figure 6] 3 is a schematic cross-sectional view showing another example of an adhesive sheet according to the present disclosure. FIG. [Figure 7] 3 is a schematic cross-sectional view showing another example of an adhesive sheet according to the present disclosure. FIG. [Figure 8] 1 is a schematic cross-sectional view showing an example of a method for producing an adhesive sheet in the present disclosure. [Figure 9] FIG. 2 is a schematic cross-sectional view showing an example of a method for producing an article according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The following describes the embodiments of the present disclosure with reference to the drawings. However, the present disclosure can be implemented in many different forms, and is not to be construed as being limited to the description of the embodiments exemplified below. In addition, the drawings may be schematic in terms of the width, thickness, shape, etc. of each part compared to the actual form in order to make the explanation clearer, but these are merely examples and do not limit the interpretation of the present disclosure. In addition, in this specification and each figure, elements similar to those described above with respect to the previous figures may be given the same reference numerals, and detailed explanations may be omitted as appropriate.

[0015] In this specification, when describing a mode in which another component is disposed on a certain component, the term "above" or "below" includes both a case in which another component is disposed directly above or below a certain component so as to be in contact with the component, and a case in which another component is disposed above or below a certain component with another component interposed therebetween, unless otherwise specified. In addition, in this specification, when describing a mode in which another component is disposed on the surface of a certain component, the term "on the surface side" or "on the surface" includes both a case in which another component is disposed directly above or below a certain component so as to be in contact with the component, and a case in which another component is disposed above or below a certain component with another component interposed therebetween, unless otherwise specified.

[0016] In this specification, the term "sheet" also includes members called "films." In addition, the term "films" also includes members called "sheets." In addition, the numerical ranges in this specification are average value ranges.

[0017] The adhesive sheet, the method for producing the adhesive sheet, and the method for producing the article according to the present disclosure will be described in detail below.

[0018] A. Adhesive sheet The inventors of the present disclosure have conducted intensive research into adhesive sheets having adhesive layers on one or both sides of a substrate. First, in order to improve the slipperiness of the adhesive layer, for example, it is effective to make the adhesive layer non-adhesive (tack-free). However, if the adhesive layer is non-adhesive, the adhesive layer tends to become hard, and therefore the adhesive layer is prone to cracking, lifting, and peeling when the adhesive sheet is wound up and folded. Next, when the adhesive layer is non-adhesive and the adhesive sheet is wound up in a roll, it is common to wind the adhesive sheet in a roll without disposing a separator on the side of the non-adhesive adhesive layer opposite the substrate, in consideration of cost reduction and prevention of separator misalignment. However, in this case, since the non-adhesive adhesive layer is not protected by a separator, blocking may occur. When the adhesive layer is non-adhesive, in order to improve the blocking resistance of the adhesive layer, for example, it is effective to harden the adhesive layer. However, as described above, if the adhesive layer is too hard, the adhesive layer is likely to crack, float, or peel off when the adhesive sheet is wound or folded. The inventors of the present disclosure have conducted extensive research and found that by setting the tack of the adhesive layer within a predetermined range and the Martens hardness of the adhesive layer within a predetermined range, it is possible to achieve a good balance between improving the slipperiness and blocking resistance of the adhesive layer and suppressing the cracking, floating, or peeling of the adhesive layer when the adhesive sheet is wound or folded. The present disclosure is based on such findings.

[0019] The adhesive sheet of the present disclosure has a substrate and a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, the first adhesive layer having a tack of less than 0.1 N and a Martens hardness of 20 N / mm 2 More than 130N / mm 2 The following is the result.

[0020] In the present disclosure, by having the tack of the first adhesive layer be less than a specified value and the Martens hardness of the first adhesive layer be within a specified range, it is possible to achieve a good balance between improving the slipperiness and blocking resistance of the first adhesive layer and suppressing cracking, lifting, and peeling of the first adhesive layer when wound up and folded.

[0021] Furthermore, in the present disclosure, the tackiness of the first adhesive layer is less than a predetermined value, and the first adhesive layer is substantially non-adhesive (tack-free), thereby improving the handleability and workability of the adhesive sheet.

[0022] The adhesive sheet of the present disclosure has three preferred embodiments.

[0023] A first embodiment of the adhesive sheet in the present disclosure has a substrate and a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, the first adhesive layer having a tack of less than 0.1 N and a Martens hardness of 20 N / mm 2 More than 130N / mm 2 The following is the result.

[0024] Fig. 1 is a schematic cross-sectional view illustrating a first embodiment of an adhesive sheet according to the present disclosure. Adhesive sheet 10A in Fig. 1 has a substrate 1 and a first adhesive layer 2 that is disposed on one side of substrate 1 and contains a first curable adhesive. Adhesive sheet 10A does not have another adhesive layer on the other side of substrate 1. The tack of first adhesive layer 2 is less than a predetermined value, and the Martens hardness of first adhesive layer 2 is within a predetermined range.

[0025] In the adhesive sheet 10A shown in Fig. 1, the tack of the first adhesive layer 2 is less than a predetermined value, so the first adhesive layer 2 is substantially non-tacky (tack-free). Therefore, when the adhesive sheet 10A is wound into a roll, a separator is usually not placed on the surface of the first adhesive layer 2 opposite the substrate 1, in consideration of cost reduction and prevention of separator misalignment. In this case, as shown in Fig. 2, for example, in the roll-shaped adhesive sheet 10A, the first adhesive layer 2 and the substrate 1 come into contact with each other, and blocking is a concern.

[0026] When improving the slipperiness and blocking resistance, for example, it is effective to harden the first adhesive layer. However, when the first adhesive layer is hardened, when the adhesive sheet is wound into a roll and when the adhesive sheet is folded, the first adhesive layer is likely to crack, or the first adhesive layer is likely to float or peel off from the substrate. In addition, for example, when the first adhesive layer further contains a foaming agent, if the first adhesive layer is hard, the first adhesive layer is difficult to expand when foaming and curing, and the foaming ratio decreases. Then, when the adhesive sheet is placed between two members and then the first adhesive layer is foamed and cured to fill and bond the gap between the two members, the gap between the two members cannot be sufficiently filled, and the adhesiveness after foaming and curing decreases.

[0027] In contrast, in the first embodiment, since the Martens hardness of the first adhesive layer is within a predetermined range, the first adhesive layer is prevented from cracking, lifting, or peeling when the adhesive sheet is wound or folded, while the slipperiness of the first adhesive layer is improved and blocking of the first adhesive layer is prevented. In addition, when the first adhesive layer contains a foaming agent, the adhesiveness after foaming and curing is also improved.

[0028] In the first embodiment, the tack of the first adhesive layer is less than a predetermined value, and the first adhesive layer is substantially non-adhesive (tack-free), so that the slipperiness of the first adhesive layer is good. Therefore, for example, when the two members are bonded by placing an adhesive sheet between two members and then curing the adhesive sheet, the adhesive sheet can be smoothly inserted into the gap between the two members. Alternatively, the other member and the adhesive sheet can be smoothly inserted into the hole or groove of one member. Alternatively, the other member can be inserted into the gap after placing the adhesive sheet in the hole or groove of one member. Also, when the other member is moved relative to one member to align the two members, the other member can be smoothly moved relative to the one member while the other member is inserted into the hole or groove of the one member, and alignment can be easily performed.

[0029] A second embodiment of the adhesive sheet in the present disclosure has a substrate, a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, and a second adhesive layer disposed on the other side of the substrate and containing a second curable adhesive, wherein the tack of the first adhesive layer and the second adhesive layer is less than 0.1 N, and the Martens hardness of the first adhesive layer and the second adhesive layer is less than 20 N / mm 2 More than 130N / mm 2 The following is the result.

[0030] Fig. 3 is a schematic cross-sectional view illustrating a second embodiment of an adhesive sheet according to the present disclosure. Adhesive sheet 10B in Fig. 3 has a substrate 1, a first adhesive layer 2 disposed on one side of substrate 1 and containing a first curable adhesive, and a second adhesive layer 3 disposed on the other side of substrate 1 and containing a second curable adhesive. The tack of first adhesive layer 2 and second adhesive layer 3 is less than a predetermined value, and the Martens hardness of first adhesive layer 2 and second adhesive layer 3 is within a predetermined range.

[0031] 3, the tack of the first adhesive layer 2 and the second adhesive layer 3 is less than a predetermined value, so the first adhesive layer 2 and the second adhesive layer 3 are substantially non-tacky (tack-free). Therefore, when the adhesive sheet 10B is wound into a roll, in consideration of cost reduction and prevention of separator misalignment, a separator is usually not placed on the surface of the first adhesive layer 2 opposite the substrate 1 and on the surface of the second adhesive layer 3 opposite the substrate 1. In this case, the first adhesive layer 2 and the second adhesive layer 3 come into contact with each other, which raises concerns about blocking.

[0032] When improving the slipperiness and blocking resistance, for example, it is effective to harden the first adhesive layer and the second adhesive layer. However, when the first adhesive layer and the second adhesive layer are hardened, when the adhesive sheet is wound into a roll shape and when the adhesive sheet is folded, the first adhesive layer and the second adhesive layer are likely to crack, or the first adhesive layer and the second adhesive layer are likely to float or peel off from the substrate. In addition, for example, when at least one of the first adhesive layer and the second adhesive layer further contains a foaming agent, if the adhesive layer containing the foaming agent is hard, the adhesive layer is difficult to expand when foaming and curing, and the foaming ratio decreases. Then, when the adhesive sheet is placed between two members and then the adhesive layer containing the foaming agent is foamed and cured to fill and bond the gap between the two members, the gap between the two members cannot be sufficiently filled, and the adhesion after foaming and curing decreases.

[0033] In contrast, in the second embodiment, when the tack of the first adhesive layer and the second adhesive layer is less than a predetermined value, the Martens hardness of the first adhesive layer and the second adhesive layer is within a predetermined range, so that the first adhesive layer and the second adhesive layer are prevented from cracking, lifting, or peeling when the adhesive sheet is wound or folded, while the slipperiness of the first adhesive layer and the second adhesive layer is improved, and blocking of the first adhesive layer and the second adhesive layer can be prevented. In addition, when at least one of the first adhesive layer and the second adhesive layer contains a foaming agent, the adhesion after foaming and curing is also improved.

[0034] In the second embodiment, the tack of the first adhesive layer and the second adhesive layer is less than a predetermined value, and the first adhesive layer and the second adhesive layer are substantially non-adhesive (tack-free), so that the slipperiness of the first adhesive layer and the second adhesive layer is good. Therefore, for example, when the two members are bonded by placing an adhesive sheet between two members and then curing the adhesive sheet, the adhesive sheet can be smoothly inserted into the gap between the two members. Alternatively, the other member and the adhesive sheet can be smoothly inserted into the hole or groove of one member. Alternatively, the other member can be inserted into the gap after placing the adhesive sheet in the hole or groove of one member. Also, when the other member is moved relative to one member to align the two members, the other member can be smoothly moved relative to the one member while the other member is inserted into the hole or groove of the one member, and alignment can be easily performed.

[0035] A third embodiment of an adhesive sheet in the present disclosure has a substrate, a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, a second adhesive layer disposed on the other side of the substrate and containing a second curable adhesive, and a separator disposed on the side of the second adhesive layer opposite the substrate, wherein the tack of the first adhesive layer is less than 0.1 N, the tack of the second adhesive layer is 0.1 N or more, and the Martens hardness of the first adhesive layer is 20 N / mm 2 More than 130N / mm 2 The following is the result.

[0036] Fig. 4 is a schematic cross-sectional view illustrating a third embodiment of an adhesive sheet according to the present disclosure. Adhesive sheet 10C in Fig. 4 has a substrate 1, a first adhesive layer 2 that is disposed on one side of substrate 1 and contains a first curable adhesive, a second adhesive layer 3 that is disposed on the other side of substrate 1 and contains a second curable adhesive, and a separator 4 that is disposed on the side of second adhesive layer 3 opposite substrate 1. The tack of first adhesive layer 2 is less than a predetermined value, the tack of second adhesive layer 3 is equal to or greater than a predetermined value, and the Martens hardness of first adhesive layer 2 is within a predetermined range.

[0037] In the adhesive sheet 10C shown in FIG. 4, the tack of the first adhesive layer 2 is less than a predetermined value, so the first adhesive layer 2 is substantially non-adhesive (tack-free). Therefore, when the adhesive sheet 10C is wound into a roll, a separator is usually not placed on the surface of the first adhesive layer 2 opposite the substrate 1, in consideration of cost reduction and prevention of separator misalignment. On the other hand, since the second adhesive layer 3 is adhesive, a separator 4 is placed on the surface of the second adhesive layer 3 opposite the substrate 1. In this case, the first adhesive layer 2 and the separator 4 come into contact with each other, so blocking is a concern.

[0038] When improving the slipperiness and blocking resistance, for example, it is effective to harden the first adhesive layer. However, when the first adhesive layer is hardened, when the adhesive sheet is wound into a roll and when the adhesive sheet is folded, the first adhesive layer is likely to crack, or the first adhesive layer is likely to float or peel off from the substrate. In addition, for example, when the first adhesive layer further contains a foaming agent, if the first adhesive layer is hard, the first adhesive layer is difficult to expand when foaming and curing, and the foaming ratio decreases. Then, when the adhesive sheet is placed between two members and then the first adhesive layer is foamed and cured to fill and bond the gap between the two members, the gap between the two members cannot be sufficiently filled, and the adhesiveness after foaming and curing decreases.

[0039] In contrast, in the third embodiment, when the tack of the first adhesive layer is less than a predetermined value, the Martens hardness of the first adhesive layer is within a predetermined range, so that the first adhesive layer is prevented from cracking when the adhesive sheet is wound and folded, and the slipperiness of the first adhesive layer is improved, thereby preventing blocking of the first adhesive layer. In addition, when the first adhesive layer contains a foaming agent, the adhesiveness after foaming and curing is also improved.

[0040] In the third embodiment, the tack of the first adhesive layer is less than a predetermined value, and the first adhesive layer is substantially non-tacky (tack-free), so that the slipperiness of the first adhesive layer is good. On the other hand, the tack of the second adhesive layer is equal to or greater than a predetermined value, so that the adhesion of the second adhesive layer to the member can be improved. Therefore, for example, when the two members are bonded by placing an adhesive sheet between two members and then curing the adhesive sheet, the surface of the second adhesive layer of the adhesive sheet is attached to one member, and then the one member to which the adhesive sheet is attached can be smoothly inserted into the hole or groove of the other member. In addition, when inserting the one member to which the adhesive sheet is attached into the hole or groove of the other member, peeling and positional deviation of the adhesive sheet from the one member can be suppressed. In addition, when moving one member relative to the other member to align the two members, one member can be smoothly moved relative to the other member while the one member to which the adhesive sheet is attached is inserted into the hole or groove of the other member, and alignment can be easily performed.

[0041] Here, non-tacky is generally used mainly to mean low adhesive strength. In the present disclosure, "substantially non-tacky" means that the tack is less than 0.1 N.

[0042] "Adhesion" is a concept that is included in "bonding." The two are sometimes distinguished in that "adhesion" is used to mean a temporary adhesive phenomenon, whereas "bonding" is used to mean a substantially permanent adhesive phenomenon (Iwanami Shoten Physics and Chemistry Dictionary, 5th Edition). "Adhesiveness" and "adhesive strength" refer to the property of adhering through pressure and the adhesive strength at that time.

[0043] In this specification, the "adhesiveness of the adhesive layer" and the "adhesive strength of the adhesive layer" refer to the adhesiveness and adhesive strength of the adhesive layer before curing, unless otherwise specified. In addition, in this specification, the "adhesiveness of the adhesive layer" and the "adhesive strength of the adhesive layer" refer to the adhesiveness and adhesive strength of the adhesive layer after curing, unless otherwise specified.

[0044] Hereinafter, various embodiments of the adhesive sheet according to the present disclosure will be described.

[0045] I. First embodiment of adhesive sheet A first embodiment of the adhesive sheet in the present disclosure has a substrate and a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, the first adhesive layer having a tack of less than 0.1 N and a Martens hardness of 20 N / mm 2 More than 130N / mm 2 The adhesive sheet of this embodiment does not have another adhesive layer on the other side of the substrate.

[0046] Each component of the adhesive sheet of this embodiment will be described below.

[0047] 1.First adhesive layer The first adhesive layer in this embodiment is disposed on one side of the substrate and contains a first curable adhesive. Also, in this embodiment, the tack of the first adhesive layer is less than a predetermined value, and the Martens hardness of the first adhesive layer is within a predetermined range.

[0048] (1) Physical properties of the first adhesive layer The tack of the first adhesive layer in this embodiment is less than 0.1 N, and may be 0.05 N or less, or may be 0.02 N or less. When the tack of the first adhesive layer is within the above range, the first adhesive layer can be made substantially non-adhesive (tack-free). In addition, the slipperiness of the first adhesive layer is improved.

[0049] Here, the tack of the first adhesive layer is measured by a probe tack test. Specifically, a cylindrical stainless steel probe with a diameter of 5 mm is pressed against the surface of the first adhesive layer of the foamable adhesive sheet under conditions of a temperature of 23±5°C and a humidity of 50±30%RH with a load of 0.1 N and a speed of 30 mm / min, and after holding for 1.0 second, it is peeled off at a speed of 30 mm / min, and the load at the time of peeling is measured. This measurement is performed five times, and the average value is taken as the tack. For example, a tack tester "TAC-II" manufactured by RHESCA can be used as the probe tack tester.

[0050] In this embodiment, the method of controlling the tackiness of the first adhesive layer includes, for example, a method of adjusting the composition of the first adhesive layer. Specifically, in the first adhesive layer containing an epoxy resin and a curing agent, the tackiness of the first adhesive layer can be reduced by using an epoxy resin that is solid at room temperature or a curing agent that is solid at room temperature. In addition, in the first adhesive layer containing an epoxy resin and a curing agent, the tackiness of the first adhesive layer can be reduced by including an epoxy resin with a high softening temperature or an epoxy resin with a large weight average molecular weight. For example, the tackiness of the first adhesive layer can be reduced by including multiple types of epoxy resins with different softening temperatures in the first adhesive layer, that is, by including one epoxy resin and another epoxy resin whose softening temperature is 25° C. or higher and 10° C. or higher than the softening temperature of the one epoxy resin in the first adhesive layer. Also, for example, the first adhesive layer can be made to contain multiple types of epoxy resins with different weight average molecular weights, that is, the first adhesive layer can be made to contain one epoxy resin and another epoxy resin whose weight average molecular weight is 370 or more and is 300 or more greater than the weight average molecular weight of the one epoxy resin, thereby reducing the tack of the first adhesive layer. More specifically, the first adhesive layer containing an epoxy resin and a curing agent can be made to contain a first epoxy resin with a low softening temperature and a low molecular weight, and a second epoxy resin with a high softening temperature and a high molecular weight, as described below, as the epoxy resin. Also, the first adhesive layer containing an epoxy resin and a curing agent can be made to contain an acrylic resin compatible with the epoxy resin, as described below, thereby reducing the tack of the first adhesive layer.

[0051] The Martens hardness of the first adhesive layer in this embodiment is 20 N / mm 2 Above 30N / mm 2 It may be more than 40N / mm 2 If the Martens hardness of the first adhesive layer is in the above range, blocking resistance can be improved. In addition, the Martens hardness of the first adhesive layer may be 130 N / mm 2Less than 110N / mm 2 It may be less than 90N / mm 2 If the Martens hardness of the first adhesive layer is in the above range, cracking, lifting, and peeling of the first adhesive layer can be suppressed when the adhesive sheet is wound and folded. Specifically, the Martens hardness of the first adhesive layer may be 20 N / mm 2 More than 130N / mm 2 Less than 30N / mm 2 More than 110N / mm 2 It may be less than 40N / mm 2 More than 90N / mm 2 It may be the following.

[0052] Here, the Martens hardness of the first adhesive layer is measured by an indentation method in accordance with ISO 14577. The Martens hardness (HM) is calculated by the following formula. HM=F / As (In the above formula, F is the indentation load, and As is the surface area of ​​the indenter at the indentation depth.) The ultra-microhardness tester used can be a Fischer Instruments Picodentor HM500. The following indenters are used. The measurement conditions are also shown below. The indentation load is set small to eliminate dependency on thickness. Specifically, the indentation load is set so that the indentation depth is approximately 1 / 10 or less of the first adhesive layer.

[0053] (Indenter) ·Shape: Square pyramid Material: Diamond

[0054] (Measurement conditions) Push-in load: 25mN ·Load time: 20 seconds ·Holding time: 5 seconds ·Temperature: 23±5℃ ·Humidity: 50±30%RH

[0055] In this embodiment, methods for controlling the Martens hardness of the first adhesive layer include, for example, adjusting the composition of the first adhesive layer and adjusting the drying conditions when forming the first adhesive layer.

[0056] In the method of adjusting the composition of the first adhesive layer, specifically, when an epoxy resin that is solid at room temperature or a curing agent that is solid at room temperature is used in the first adhesive layer containing an epoxy resin and a curing agent, the Martens hardness of the first adhesive layer tends to be increased. In addition, when an epoxy resin with a high softening temperature or an epoxy resin with a large weight average molecular weight is contained in the first adhesive layer containing an epoxy resin and a curing agent, the Martens hardness of the first adhesive layer tends to be increased. For example, when the first adhesive layer contains a plurality of epoxy resins with different softening temperatures, that is, when the first adhesive layer contains one epoxy resin and another epoxy resin whose softening temperature is 25°C or higher and 10°C or higher than the softening temperature of the one epoxy resin, the Martens hardness of the first adhesive layer tends to be increased. Also, for example, by making the first adhesive layer contain a plurality of epoxy resins with different weight average molecular weights, that is, by making the first adhesive layer contain one epoxy resin and another epoxy resin whose weight average molecular weight is 370 or more and is 300 or more greater than the weight average molecular weight of the one epoxy resin, the Martens hardness of the first adhesive layer tends to be increased. More specifically, in the first adhesive layer containing an epoxy resin and a curing agent, as described later, by making the first adhesive layer contain a first epoxy resin with a low softening temperature and a low molecular weight and a second epoxy resin with a high softening temperature and a high molecular weight, the Martens hardness of the first adhesive layer tends to be increased. Also, in the first adhesive layer containing an epoxy resin and a curing agent, as described later, by making the first adhesive layer contain an acrylic resin compatible with the epoxy resin, the Martens hardness of the first adhesive layer tends to be increased.

[0057] In addition, in the method of adjusting the drying conditions when forming the first adhesive layer, for example, when the first adhesive layer is formed by applying the first adhesive composition to one side of the substrate and drying it, the Martens hardness of the first adhesive layer can be controlled by adjusting the drying conditions. Examples of the drying conditions include the drying temperature, heat history, and wind speed. Examples of the heat history include the heating rate and the total amount of heat. For example, when the drying temperature is high, the Martens hardness of the first adhesive layer tends to increase. On the other hand, when the drying temperature is low, the Martens hardness of the first adhesive layer tends to decrease. Also, for example, when the heating rate is high, the total amount of heat increases when the drying time is constant, so the Martens hardness of the first adhesive layer tends to increase. On the other hand, when the heating rate is low, the total amount of heat decreases when the drying time is constant, so the Martens hardness of the first adhesive layer tends to decrease. Also, for example, when the total amount of heat received by the first adhesive layer increases, the Martens hardness of the first adhesive layer tends to increase. On the other hand, when the total amount of heat received by the first adhesive layer is reduced, the Martens hardness of the first adhesive layer tends to be reduced. Also, for example, when the wind speed is increased, the drying speed is increased, so the Martens hardness of the first adhesive layer tends to be increased. On the other hand, when the wind speed is decreased, the drying speed is decreased, so the Martens hardness of the first adhesive layer tends to be reduced.

[0058] In addition, in this embodiment, when the first adhesive layer contains a foaming agent as described later, the first adhesive layer can be foamed at an expansion ratio of, for example, 1.5 times or more and 15 times or less. The expansion ratio may be, for example, 3.5 times or more, 4 times or more, or 4.5 times or more. The expansion ratio may be, for example, 9 times or less, 8.5 times or less, or 8 times or less. If the expansion ratio is too small, the gap between the two members cannot be sufficiently filled, and the adhesiveness after foaming and curing may decrease. If the expansion ratio is too large, the porosity of the first adhesive layer after foaming and curing may increase, and the adhesiveness after foaming and curing may decrease.

[0059] Here, the expansion ratio is calculated by the following formula. Expansion ratio (times) = thickness of first adhesive layer after curing / thickness of first adhesive layer before curing

[0060] (2) Material of the first adhesive layer (a) a first curing adhesive The first curable adhesive contained in the first adhesive layer in this embodiment can be a curable adhesive generally used in the adhesive layer of an adhesive sheet. Examples of the first curable adhesive include a heat-curable adhesive and a light-curable adhesive. Among them, a heat-curable adhesive is preferred. A heat-curable adhesive can be applied even when the member does not have transparency, such as a metal member.

[0061] The first curable adhesive is preferably an epoxy resin adhesive. That is, the first curable adhesive preferably contains an epoxy resin and a curing agent. In general, the epoxy resin adhesive has a hard and tough cured film, and is suitable for bonding hard material members such as metal and glass members. In addition, the epoxy resin adhesive generally has excellent heat resistance, insulating properties, chemical resistance, etc., has small curing shrinkage, and can be used in a wide range of applications.

[0062] In addition, when the first curable adhesive is an epoxy resin adhesive, the first curable adhesive preferably further contains an acrylic resin compatible with the epoxy resin. By using an acrylic resin compatible with the epoxy resin, the toughness of the first adhesive layer can be increased. This can improve the adhesiveness after curing.

[0063] (i) Epoxy resin The epoxy resin in this embodiment is a compound that has at least one epoxy group or glycidyl group and is cured by a crosslinking polymerization reaction in combination with a curing agent. The epoxy resin also includes a monomer having at least one epoxy group or glycidyl group.

[0064] As the epoxy resin, an epoxy resin generally used in the adhesive layer of an adhesive sheet can be used. In particular, the curable adhesive preferably contains, as the epoxy resin, a first epoxy resin having a softening temperature of 50° C. or higher and an epoxy equivalent of 5000 g / eq or less, and a second epoxy resin having a softening temperature higher than that of the first epoxy resin and a weight average molecular weight of 20,000 or more. By using the first epoxy resin and the second epoxy resin in combination, an adhesive sheet having good blocking resistance and adhesiveness after curing can be obtained. Furthermore, the tackiness (tackiness) of the first adhesive layer can be reduced, and an adhesive sheet having good slipperiness can be obtained.

[0065] For example, when only improving the adhesiveness after curing is required, it is more effective to use an epoxy resin with a low molecular weight (low epoxy equivalent) than an epoxy resin with a high molecular weight (high epoxy equivalent). However, when an epoxy resin with a low molecular weight (low epoxy equivalent) is used, the epoxy resins with low molecular weight (low epoxy equivalent) are assimilated with each other when the adhesive sheet is wound into a roll, for example, and blocking is likely to occur.

[0066] In contrast, when a first epoxy resin having a relatively low softening temperature (relatively high crystallinity) and a low molecular weight (low epoxy equivalent) is used, the first epoxy resin melts rapidly and changes to a low-viscosity liquid when the temperature reaches or exceeds the softening temperature. Therefore, it is easy to improve the adhesiveness after curing. On the other hand, since the first epoxy resin has a relatively high crystallinity, it can suppress the occurrence of blocking compared to an epoxy resin having a relatively low crystallinity or an epoxy resin having no crystallinity. However, when only the first epoxy resin is used, there is a possibility that the effect of suppressing the occurrence of blocking is insufficient or the adhesiveness (tackiness) of the first adhesive layer becomes too high. Therefore, by further using a second epoxy resin having a relatively high softening temperature (relatively low crystallinity) and a high molecular weight, it is possible to improve the effect of suppressing the occurrence of blocking and to suppress the adhesiveness (tackiness) of the first adhesive layer to a low level.

[0067] (i-1) First epoxy resin The first epoxy resin has a softening temperature of 50° C. or higher and an epoxy equivalent of 5000 g / eq or lower. The first epoxy resin has a relatively low softening temperature (relatively high crystallinity) compared to the second epoxy resin described below. The first epoxy resin has relatively high crystallinity and a low molecular weight, which makes it easy to improve adhesion and blocking resistance after curing. In addition, since the first epoxy resin has a low molecular weight, the crosslinking density can be increased, and a first adhesive layer having good mechanical strength, chemical resistance, and curing properties can be obtained. In addition, the first epoxy resin is preferably an epoxy resin that is solid at room temperature (23° C.).

[0068] The softening temperature of the first epoxy resin is usually 50° C. or higher, and may be 55° C. or higher, or may be 60° C. or higher. On the other hand, the softening temperature of the first epoxy resin is, for example, 150° C. or lower. The softening temperature is measured by the ring and ball method in accordance with JIS K7234:1986.

[0069] The epoxy equivalent of the first epoxy resin is, for example, 5000 g / eq or less, may be 3000 g / eq or less, may be 1000 g / eq or less, or may be 600 g / eq or less. On the other hand, the epoxy equivalent of the first epoxy resin is, for example, 90 g / eq or more, may be 100 g / eq or more, or may be 110 g / eq or more. The epoxy equivalent is the number of grams of a resin containing 1 gram equivalent of an epoxy group. The epoxy equivalent is measured by a method in accordance with JIS K7236:2009, which corresponds to ISO 3001 (Plastics-Epoxy compounds-Determination of epoxy equivalent).

[0070] The first epoxy resin may be a monofunctional epoxy resin, a difunctional epoxy resin, a trifunctional epoxy resin, or a tetrafunctional or higher functional epoxy resin.

[0071] The weight average molecular weight (Mw) of the first epoxy resin is usually smaller than the weight average molecular weight (Mw) of the second epoxy resin described below. The Mw of the first epoxy resin is, for example, 6,000 or less, and may be 4,000 or less, or may be 3,000 or less. On the other hand, the Mw of the first epoxy resin is, for example, 400 or more. Mw is a value calculated in terms of polystyrene as measured by gel permeation chromatography (GPC).

[0072] The melt viscosity of the first epoxy resin at 150°C is, for example, 0.005 Pa·s or more, may be 0.015 Pa·s or more, may be 0.03 Pa·s or more, may be 0.05 Pa·s or more, or may be 0.1 Pa·s or more. If the melt viscosity is too low, good foaming properties may not be obtained. In addition, if the melt viscosity of the first epoxy resin is too low (if the crystallinity of the first epoxy resin is too high), the adhesion (tackiness) of the resulting first adhesive layer may be high. The reason for this is presumably that if the melt viscosity of the first epoxy resin is too low (if the crystallinity of the first epoxy resin is too high), when it is mixed with the second epoxy resin or the acrylic resin, its crystallinity is greatly reduced, and the Tg of the entire adhesive composition is reduced. On the other hand, the melt viscosity of the first epoxy resin at 150°C is, for example, 10 Pa·s or less, may be 5 Pa·s or less, or may be 2 Pa·s or less. If the melt viscosity is too high, the uniformity of the resulting first adhesive layer may be reduced. The melt viscosity is measured in accordance with JIS K6862:1984, which corresponds to ISO 2555 (Resins in the liquid state or as emulsions or dispersions-Determination of Brookfield RV viscosity), using a Brookfield type single cylinder rotational viscometer and a thermocell for heating the solution.

[0073] Next, the constitution of the first epoxy resin will be described. Examples of the first epoxy resin include aromatic epoxy resins, aliphatic epoxy resins, alicyclic epoxy resins, and heterocyclic epoxy resins. Specific examples of the first epoxy resin include bisphenol-type epoxy resins, novolac-type epoxy resins, and modified epoxy resins. Examples of the bisphenol-type epoxy resins include bisphenol A-type epoxy resins and bisphenol F-type epoxy resins. Examples of the novolac-type epoxy resins include bisphenol A novolac-type epoxy resins and cresol novolac-type epoxy resins. Examples of the modified epoxy resins include urethane-modified epoxy resins and rubber-modified epoxy resins. Other specific examples include biphenyl-type epoxy resins, stilbene-type epoxy resins, triphenolmethane-type epoxy resins, alkyl-modified triphenolmethane-type epoxy resins, triazine nucleus-containing epoxy resins, dicyclopentadiene-modified phenol-type epoxy resins, naphthalene-type epoxy resins, glycol-type epoxy resins, and pentaerythritol-type epoxy resins. The first epoxy resin may be one type or two or more types.

[0074] Bisphenol A type epoxy resins can exist in a liquid state at room temperature or in a solid state at room temperature depending on the number of repeating units of the bisphenol skeleton. Bisphenol A type epoxy resins having, for example, 2 to 10 bisphenol skeletons in the main chain are solid at room temperature. In particular, bisphenol A type epoxy resins are preferred in that they can improve heat resistance.

[0075] In particular, the first epoxy resin is preferably a bisphenol A novolac type epoxy resin represented by the following general formula (1).

[0076] [ka]

[0077] In the general formula (1), R 1 is C m H2m (m is 1 or more and 3 or less), 2 and R 3 are each independently p H 2p+1 (p is 1 or more and 3 or less), and n is 0 or more and 10 or less.

[0078] In the general formula (1), R 1 m in is 1, that is, R 1 is preferably -CH2-. Similarly, R 2 and R 3 p in is 1, that is, R 2 and R 3 is preferably -CH3. Furthermore, the hydrogen bonded to the benzene ring in general formula (1) may be substituted with other elements or other groups.

[0079] The content of the first epoxy resin may be, for example, 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, or 25 parts by mass or more, when the resin component contained in the first adhesive layer is 100 parts by mass. If the content of the first epoxy resin is too small, the adhesiveness and blocking resistance after curing may be reduced. On the other hand, the content of the first epoxy resin may be, for example, 90 parts by mass or less, 80 parts by mass or less, 70 parts by mass or less, 60 parts by mass or less, 50 parts by mass or less, or 40 parts by mass or less, when the resin component contained in the first adhesive layer is 100 parts by mass. If the content of the first epoxy resin is too high, the content of the second epoxy resin and the acrylic resin will be relatively low, and it may be difficult to balance the blocking resistance, the adhesion of the first adhesive layer to the substrate, and the adhesiveness after curing.

[0080] (i-2) Second epoxy resin The second epoxy resin has a higher softening temperature than the first epoxy resin and a weight average molecular weight of 20,000 or more. The second epoxy resin has a relatively high softening temperature (relatively low crystallinity) compared to the above-mentioned first epoxy resin. The second epoxy resin has relatively low crystallinity and high molecular weight, so that it is easy to improve blocking resistance. Furthermore, the second epoxy resin has relatively low crystallinity and high molecular weight, so that it is possible to suppress an increase in adhesion (tackiness) caused by the first epoxy resin. Moreover, it is preferable that the second epoxy resin is an epoxy resin that is solid at room temperature (23°C).

[0081] The weight average molecular weight (Mw) of the second epoxy resin is usually larger than the weight average molecular weight (Mw) of the first epoxy resin. The Mw of the second epoxy resin is usually 20,000 or more, may be 30,000 or more, or may be 35,000 or more. On the other hand, the Mw of the second epoxy resin is, for example, 100,000 or less.

[0082] The epoxy equivalent of the second epoxy resin may be larger, smaller, or the same as that of the first epoxy resin. The epoxy equivalent of the second epoxy resin is, for example, 4000 g / eq or more, 5000 g / eq or more, or 6000 g / eq or more. On the other hand, the epoxy equivalent of the second epoxy resin is, for example, 20000 g / eq or less.

[0083] The second epoxy resin may be a monofunctional epoxy resin, a difunctional epoxy resin, a trifunctional epoxy resin, or a tetrafunctional or higher functional epoxy resin.

[0084] The softening temperature of the second epoxy resin is usually higher than that of the first epoxy resin. The difference between the two is, for example, 10° C. or more, and may be 20° C. or more, or may be 30° C. or more. The softening temperature of the second epoxy resin is, for example, 80° C. or more, and may be 90° C. or more. On the other hand, the softening temperature of the second epoxy resin is, for example, 180° C. or less.

[0085] The composition of the second epoxy resin is the same as that of the first epoxy resin described above, and therefore the description thereof will be omitted here.

[0086] The content of the second epoxy resin may be, for example, 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, 30 parts by mass or more, 35 parts by mass or more, 40 parts by mass or more, or 45 parts by mass or more, when the resin component contained in the first adhesive layer is taken as 100 parts by mass. If the content of the second epoxy resin is too small, the blocking resistance may be reduced. On the other hand, the content of the second epoxy resin may be, for example, 90 parts by mass or less, 85 parts by mass or less, 80 parts by mass or less, or 75 parts by mass or less, when the resin component contained in the first adhesive layer is taken as 100 parts by mass. If the content of the second epoxy resin is too high, the contents of the first epoxy resin and the acrylic resin become relatively small, and it may be difficult to balance the blocking resistance, the adhesion of the first adhesive layer to the substrate, and the adhesion after curing.

[0087] The ratio of the first epoxy resin to the total of the first epoxy resin and the second epoxy resin is, for example, 5 mass% or more, optionally 10 mass% or more, optionally 15 mass% or more, or optionally 20 mass% or more, whereas the ratio of the first epoxy resin is, for example, 80 mass% or less, optionally 75 mass% or less, or optionally 60 mass% or less.

[0088] Furthermore, the total proportion of the first epoxy resin and the second epoxy resin to all epoxy resins contained in the first adhesive layer is, for example, 50 mass% or more, optionally 70 mass% or more, optionally 90 mass% or more, or optionally 100 mass%.

[0089] (ii) Acrylic resin The acrylic resin in this embodiment is a resin compatible with the epoxy resin. Since the acrylic resin is compatible with the epoxy resin, it is easy to improve the toughness of the first adhesive layer. As a result, the adhesion of the first adhesive layer to the substrate can be improved. In addition, the improved toughness of the adhesive layer can improve the adhesion after curing. Furthermore, it is considered that the acrylic resin acts as a compatibilizer for the foaming agent (for example, a foaming agent whose shell portion is an acrylonitrile copolymer resin), and uniformly disperses and foams, thereby improving the adhesion after curing. In addition, the hardness of the surface of the first adhesive layer can be maintained high by the compatibility of the acrylic resin with the epoxy resin. On the other hand, if the acrylic resin is incompatible with the epoxy resin, a soft portion is formed on the surface of the first adhesive layer, making the interface with the adherend less slippery, which may reduce workability.

[0090] The acrylic resin in this embodiment is compatible with the epoxy resin. The compatibility of the acrylic resin with the epoxy resin is confirmed by observing the cross section of the first adhesive layer of the adhesive sheet with a scanning electron microscope (SEM) or a transmission electron microscope (TEM) to see that no micron-sized islands are generated. More specifically, the average particle size of the islands is preferably 1 μm or less. In particular, the average particle size of the islands may be 0.5 μm or less, or may be 0.3 μm or less. It is preferable to have a large number of samples, for example, 100 or more. The area to be observed is in the range of 100 μm × 100 μm, or in the case where the average thickness of the first adhesive layer is 100 μm or less, in the range of the average thickness × 100 μm.

[0091] The weight average molecular weight (Mw) of the acrylic resin is, for example, 50,000 or more, may be 70,000 or more, or may be 100,000 or more. The first epoxy resin has a relatively high crystallinity, and the melt viscosity (or dynamic viscoelasticity) during heating becomes too low, which may cause shrinkage during hardening after foaming (between the end of foaming of the foaming agent and the hardening of the adhesive composition). However, by using an acrylic resin having a certain molecular weight, it is possible to prevent the melt viscosity from becoming too low, and shrinkage is less likely to occur during hardening after foaming. On the other hand, the Mw of the acrylic resin is, for example, 1,500,000 or less. The weight average molecular weight of the acrylic resin is measured by GPC (eluent: THF, standard substance: PS, sample: 20 μL, flow rate: 1 mL / min, column temperature: 40° C.).

[0092] The glass transition temperature (Tg) of the acrylic resin is, for example, 90° C. or higher, and may be 100° C. or higher. On the other hand, the Tg of the acrylic resin is, for example, 180° C. or lower. Tg is measured by a differential scanning calorimeter (DSC) in accordance with JIS K7121:2012, which corresponds to ISO 3146.

[0093] Acrylic resin has a storage modulus (E') of 1 x 10 at the foaming start temperature. 6 Pa or less. When E' at the foaming start temperature is low, the fluidity is improved and good foaming properties can be obtained. On the other hand, E' at the foaming start temperature may be, for example, 1×10 5 The foaming initiation temperature is a temperature that differs depending on the type of foaming agent. When two or more foaming agents are used, the foaming initiation temperature is the initiation temperature of the main foaming reaction.

[0094] Acrylic resin has a storage modulus (E') of 1 x 10 at the curing start temperature. 5Pa or more. As described above, shrinkage may occur during curing after foaming (from the end of foaming of the foaming agent to the curing of the adhesive composition), but by having a large E' at the curing start temperature, shrinkage can be suppressed and good shape retention can be obtained. The curing start temperature is a temperature that differs depending on the type of curing agent. In addition, when two or more types of curing agents are used as the curing agent, the start temperature of the main curing reaction is taken as the curing start temperature.

[0095] In addition, the average storage modulus (E') of acrylic resin at temperatures between 0°C and 100°C is 1×10 6 The average value of storage modulus (E') at temperatures between 0°C and 100°C may be, for example, 1 x 10 8 Pa or less.

[0096] The storage modulus (E') of the acrylic resin is measured by a dynamic viscoelasticity measurement method conforming to JIS K7244-1:1998. The measurement conditions are as follows: attachment mode: compression mode, frequency: 1Hz, temperature: -30℃ to 200℃, heating rate: 10℃ / min. The device used is the solid viscoelasticity analyzer "RSA-III" manufactured by TA Instruments.

[0097] The acrylic resin may have a polar group, such as an epoxy group, a hydroxyl group, a carboxyl group, a nitrile group, or an amide group.

[0098] The acrylic resin may be a homopolymer of an acrylic acid ester monomer, a mixed component containing two or more of the above homopolymers, or a copolymer of two or more of the acrylic acid ester monomers, a component containing one or more copolymers. The acrylic resin may also be a mixed component of the above homopolymer and the above copolymer. The "acrylic acid" of the acrylic acid ester monomer also includes the concept of methacrylic acid. Specifically, the acrylic resin may be a mixture of a methacrylate polymer and an acrylate polymer, or an acrylic acid ester polymer such as acrylate-acrylate, methacrylate-methacrylate, or methacrylate-acrylate. Among them, the acrylic resin preferably contains a copolymer of two or more of the acrylic acid ester monomers ((meth)acrylic acid ester copolymer).

[0099] Examples of the monomer components constituting the (meth)acrylic acid ester copolymer include the monomer components described in JP 2014-065889 A. The monomer components may have the above-mentioned polar group. Examples of the (meth)acrylic acid ester copolymer include ethyl acrylate-butyl acrylate-acrylonitrile copolymer, ethyl acrylate-acrylonitrile copolymer, and butyl acrylate-acrylonitrile copolymer. Note that "acrylic acid" such as methyl acrylate and ethyl acrylate also includes "methacrylic acid" such as methyl methacrylate and ethyl methacrylate.

[0100] The (meth)acrylic acid ester copolymer is preferably a block copolymer, and more preferably an acrylic block copolymer such as a methacrylate-acrylate copolymer. Examples of (meth)acrylates constituting the acrylic block copolymer include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, and benzidyl acrylate. These "acrylic acids" also include "methacrylic acid."

[0101] Specific examples of methacrylate-acrylate copolymers include acrylic copolymers such as methyl methacrylate-butyl acrylate-methyl methacrylate (MMA-BA-MMA) copolymers. MMA-BA-MMA copolymers also include block copolymers of polymethyl methacrylate-polybutyl acrylate-polymethyl methacrylate (PMMA-PBA-PMMA).

[0102] The acrylic copolymer may not have a polar group, or may be a modified product having the above-mentioned polar group partially introduced therein. The modified product is easily compatible with the epoxy resin, and therefore the adhesiveness is further improved.

[0103] Among them, the acrylic resin is preferably a (meth)acrylic acid ester copolymer having a first polymer portion having a glass transition temperature (Tg) of 10° C. or lower and a second polymer portion having a glass transition temperature (Tg) of 20° C. or higher. Such a (meth)acrylic acid ester copolymer has the first polymer portion that becomes a soft segment and the second polymer portion that becomes a hard segment.

[0104] The manifestation of the above-mentioned effect can be presumed as follows: By using an acrylic resin having both a soft segment and a hard segment, such as the above-mentioned (meth)acrylic acid ester copolymer, the hard segment contributes to heat resistance, and the soft segment contributes to toughness or flexibility, so that a first adhesive layer having good heat resistance, toughness, and flexibility can be obtained.

[0105] At least one of the first polymer portion and the second polymer portion contained in the (meth)acrylic acid ester copolymer has compatibility with epoxy resins. When the first polymer portion has compatibility with epoxy resins, flexibility can be increased. When the second polymer portion has compatibility with epoxy resins, cohesion and toughness can be increased.

[0106] When either the first polymer portion or the second polymer portion is incompatible with the epoxy resin, the (meth)acrylic acid ester copolymer has a compatible portion, which is a polymer portion that is compatible with the epoxy resin, and an incompatible portion, which is a polymer portion that is incompatible with the epoxy resin. In this case, when the (meth)acrylic acid ester copolymer is added to the adhesive composition, the compatible portion is compatible with the epoxy resin, and the incompatible portion is incompatible with the epoxy resin, so that fine phase separation occurs. As a result, a fine sea-island structure is developed. The sea-island structure varies depending on the type of (meth)acrylic acid ester copolymer, the compatibility of the first polymer portion and the second polymer portion contained in the (meth)acrylic acid ester copolymer, and the presence or absence of modification by introduction of a polar group, and examples thereof include a sea-island structure in which the compatible portion of the cured epoxy resin and the (meth)acrylic acid ester copolymer is a sea, and the incompatible portion of the (meth)acrylic acid ester copolymer is an island, a sea-island structure in which the incompatible portion of the (meth)acrylic acid ester copolymer is a sea, and the compatible portion of the cured epoxy resin and the (meth)acrylic acid ester copolymer is an island, and a sea-island structure in which the (meth)acrylic acid ester copolymer is a sea, and the cured epoxy resin is an island. By having such a sea-island structure, stress can be easily dispersed, so that interfacial failure can be avoided and excellent adhesion can be obtained after curing.

[0107] The (meth)acrylic acid ester copolymer is preferably a block copolymer, and more preferably an ABA block copolymer in which the compatible portion is polymer block A and the incompatible portion is polymer block B. Furthermore, it is preferable that the ABA block copolymer is an ABA block copolymer in which the first polymer portion is an incompatible portion, the second polymer portion is an compatible portion, the first polymer portion is polymer block B, and the second polymer portion is polymer block A. By using such an ABA block copolymer as the acrylic resin, in the case of a sea-island structure in which the compatible portion of the cured epoxy resin and the (meth)acrylic acid ester copolymer is the sea, and the incompatible portion of the (meth)acrylic acid ester copolymer is the island, the island portion can be made small. In addition, in the case of a sea-island structure in which the incompatible portion of the (meth)acrylic acid ester copolymer is the sea, and the compatible portion of the cured epoxy resin and the (meth)acrylic acid ester copolymer is the island, or in the case of a sea-island structure in which the (meth)acrylic acid ester copolymer is the sea, and the cured epoxy resin is the island, the sea portion can be made small.

[0108] The (meth)acrylic acid ester copolymer may be a modified product in which the above-mentioned polar group is introduced into a part of the first polymer segment or the second polymer segment.

[0109] The Tg of the first polymer portion contained in the above (meth)acrylic acid ester copolymer is 10°C or lower, and may be in the range of -150°C or higher and 10°C or lower, or in the range of -130°C or higher and 0°C or lower, or in the range of -110°C or higher and -10°C or lower.

[0110] The Tg of the first polymer portion is calculated according to the following formula based on the Tg(K) of each homopolymer described in "POLYMERHANDBOOK, Third Edition" (published by John Wiley & Sons, Inc.). 1 / Tg(K)=W1 / Tg1+W2 / Tg2+····+W n / Tg n W n : Mass fraction of each monomer Tgn : Tg(K) of the homopolymer of each monomer, and publicly available values ​​such as those in the Polymer Handbook (3rd Ed., J. Brandrup and EH Immergut, WILEY INTERSCIENCE) may be used. The same applies to the Tg of the second polymer portion described below.

[0111] The first polymer portion contained in the (meth)acrylic acid ester copolymer may be a homopolymer or a copolymer, but is preferably a homopolymer. The monomer component and polymer component constituting the first polymer portion may be a monomer component and polymer component capable of obtaining a first polymer portion having a Tg in a predetermined range, and examples thereof include acrylate monomers such as butyl acrylate, 2-ethylhexyl acrylate, isononyl acrylate, and methyl acrylate, other monomers such as vinyl acetate, acetal, and urethane, polar group-containing monomers containing the above-mentioned polar groups, and copolymers such as EVA.

[0112] The Tg of the second polymer portion contained in the above (meth)acrylic acid ester copolymer is 20°C or higher, and may be in the range of 20°C or higher and 150°C or lower, 30°C or higher and 150°C or lower, or 40°C or higher and 150°C or lower.

[0113] The second polymer portion contained in the (meth)acrylic acid ester copolymer may be a homopolymer or a copolymer, but is preferably a homopolymer. The monomer component constituting the second polymer portion may be any monomer component capable of obtaining a second polymer portion having a Tg in a predetermined range, and examples thereof include acrylic acid ester monomers such as methyl methacrylate, other monomers such as acrylamide, styrene, vinyl chloride, amide, acrylonitrile, cellulose acetate, phenol, urethane, vinylidene chloride, methylene chloride, and methacrylonitrile, and polar group-containing monomers containing the above-mentioned polar groups.

[0114] A specific example of the (meth)acrylic acid ester copolymer having the above-mentioned first polymer portion and second polymer portion is the above-mentioned MMA-BA-MMA copolymer.

[0115] The content of the acrylic resin may be, for example, 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, 7 parts by mass or more, or 10 parts by mass or more, when the resin component contained in the first adhesive layer is 100 parts by mass. If the content of the acrylic resin is too small, the adhesion of the first adhesive layer to the substrate and the adhesiveness after curing may be reduced. On the other hand, the content of the acrylic resin may be, for example, 60 parts by mass or less, 50 parts by mass or less, 40 parts by mass or less, 35 parts by mass or less, or 30 parts by mass or less, when the resin component contained in the first adhesive layer is 100 parts by mass. If the content of the acrylic resin is too high, the contents of the first epoxy resin and the second epoxy resin become relatively small, and it may be difficult to balance the blocking resistance, the adhesion of the first adhesive layer to the substrate, and the adhesiveness after curing.

[0116] (iii) Hardener The curing agent in this embodiment is appropriately selected according to the type of the first curing adhesive. When the first curing adhesive is, for example, an epoxy resin adhesive, the curing agent can be a curing agent generally used in epoxy resin adhesives. The curing agent is preferably solid at 23°C. A curing agent that is solid at 23°C can extend the storage stability (pot life) compared with a curing agent that is liquid at 23°C. The curing agent may be a latent curing agent. The curing agent may be a curing agent that undergoes a curing reaction by heat, or may be a curing agent that undergoes a curing reaction by light. The curing agent may be used alone or in combination of two or more types.

[0117] The reaction initiation temperature of the curing agent is, for example, 110°C or higher, and may be 130°C or higher. If the reaction initiation temperature is too low, the reaction starts early, and curing occurs in a state where the flexibility and fluidity of the resin component is low, and uniform curing may be difficult to occur. On the other hand, the reaction initiation temperature of the curing agent is, for example, 200°C or lower. If the reaction initiation temperature is too high, the resin component may deteriorate. In addition to the epoxy resin, when a resin with high heat resistance, such as a phenolic resin, is used, the resin component is less deteriorated, so the reaction initiation temperature of the curing agent may be, for example, 300°C or lower. The reaction initiation temperature of the curing agent is determined by differential scanning calorimetry (DSC).

[0118] Specific examples of the curing agent include imidazole-based curing agents, phenol-based curing agents, amine-based curing agents, acid anhydride-based curing agents, isocyanate-based curing agents, and thiol-based curing agents.

[0119] Examples of imidazole-based curing agents include imidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-isopropylimidazole, 2-phenylimidazole, carboxylates of imidazole compounds, and adducts with epoxy compounds. It is also preferable that the imidazole-based curing agent has a hydroxyl group. Since crystallization occurs due to hydrogen bonds between hydroxyl groups, the reaction initiation temperature tends to be high.

[0120] Examples of the phenol-based curing agent include phenol resins. Examples of the phenol resin include resol-type phenol resins and novolac-type phenol resins. From the viewpoint of the adhesion of the first adhesive layer to the substrate, phenol-type novolac resins having a Tg of 110° C. or less are particularly preferred. In addition, a phenol-based curing agent and an imidazole-based curing agent may be used in combination. In this case, it is preferred to use an imidazole-based curing agent as a curing catalyst.

[0121] In addition, the first adhesive layer contains a phenolic resin, which improves heat resistance, but on the other hand, there is a concern that the toughness may decrease. Therefore, when the first adhesive layer contains a phenolic resin, it is preferable that an intermediate layer is disposed between the substrate and the first adhesive layer, as described below.

[0122] The phenol resin is preferably a biphenyl type from the viewpoint of heat resistance. The phenol resin may be a resin in which the phenol nucleus is modified. By modifying the phenol nucleus, for example, the heat resistance can be further improved.

[0123] Examples of the amine-based curing agent include aliphatic amines, aromatic amines, alicyclic amines, and polyamidoamines. Examples of the aliphatic amines include diethylenetriamine (DETA), triethylenetetramine (TETA), and metaxylylenediamine (MXDA). Examples of the aromatic amines include diaminodiphenylmethane (DDM), m-phenylenediamine (MPDA), and diaminodiphenylsulfone (DDS). Examples of the amine-based curing agent include dicyandiamide-based curing agents such as dicyandiamide (DICY), organic acid dihydrazide-based curing agents, amine adduct-based curing agents, and ketimine-based curing agents.

[0124] Examples of the acid anhydride-based curing agent include alicyclic acid anhydrides (liquid acid anhydrides) and aromatic acid anhydrides. Examples of the alicyclic acid anhydrides (liquid acid anhydrides) include hexahydrophthalic anhydride (HHPA), methyltetrahydrophthalic anhydride (MTHPA), etc. Examples of the aromatic acid anhydrides include trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), benzophenonetetracarboxylic acid (BTDA), etc.

[0125] The isocyanate-based curing agent may, for example, be a blocked isocyanate.

[0126] Examples of the thiol-based curing agent include ester-bonded thiol compounds, aliphatic ether-bonded thiol compounds, and aromatic ether-bonded thiol compounds.

[0127] The content of the curing agent is, for example, 1 part by mass or more and 40 parts by mass or less, when the resin component contained in the first adhesive layer is 100 parts by mass. For example, when an imidazole-based curing agent is used as the main component as the curing agent, the content of the curing agent is, for example, 1 part by mass or more and 15 parts by mass or less, when the resin component contained in the first adhesive layer is 100 parts by mass. On the other hand, when a phenol-based curing agent is used as the main component as the curing agent, the content of the curing agent is, for example, 5 parts by mass or more and 40 parts by mass or less, when the resin component contained in the first adhesive layer is 100 parts by mass. In addition, using an imidazole-based curing agent or a phenol-based curing agent as the main component as the curing agent means that the mass ratio of the imidazole-based curing agent or the phenol-based curing agent is the highest in the curing agent.

[0128] (b) Foaming agent In this embodiment, the first adhesive layer preferably contains a foaming agent. After the adhesive sheet is placed between two members, the first adhesive layer of the adhesive sheet is foamed and cured, thereby filling the gap between the two members and bonding them together.

[0129] The foaming agent in this embodiment may be a foaming agent generally used in the adhesive layer of an adhesive sheet. The foaming agent may be a foaming agent that undergoes a foaming reaction due to heat or a foaming agent that undergoes a foaming reaction due to light.

[0130] The foaming start temperature of the foaming agent is preferably equal to or higher than the softening temperature of the base of the curable adhesive such as epoxy resin, and equal to or lower than the activation temperature of the curing reaction of the base of the curable adhesive such as epoxy resin. The foaming start temperature of the foaming agent is, for example, 70°C or higher, and may be 100°C or higher. If the foaming start temperature is too low, the reaction starts early, and foaming occurs in a state where the flexibility and fluidity of the resin component are low, and it may be difficult to generate uniform foaming. On the other hand, the foaming start temperature of the foaming agent is, for example, 210°C or lower. If the foaming start temperature is too high, the resin component may deteriorate.

[0131] The softening temperature of the base material of the curable adhesive such as an epoxy resin is measured by the ring and ball method specified in JIS K7234:1986.

[0132] Examples of the foaming agent include organic foaming agents and inorganic foaming agents. Examples of the organic foaming agent include azo foaming agents such as azodicarbonamide (ADCA), azobisformamide, and azobisisobutyronitrile, fluorinated alkane foaming agents such as trichloromonofluoromethane, hydrazine foaming agents such as paratoluenesulfonylhydrazide, semicarbazide foaming agents such as p-toluenesulfonylsemicarbazide, triazole foaming agents such as 5-morpholyl-1,2,3,4-thiatriazole, and N-nitroso foaming agents such as N,N-dinitrosoterephthalamide. Examples of the inorganic foaming agent include ammonium carbonate, ammonium hydrogen carbonate, ammonium nitrite, ammonium borohydride, and azides.

[0133] Alternatively, a microcapsule type foaming agent may be used as the foaming agent. The microcapsule type foaming agent preferably has a core made of a thermal expansion agent such as a hydrocarbon and a shell made of a resin such as an acrylonitrile copolymer.

[0134] The average particle size of the foaming agent may be, for example, 7 μm or more, 10 μm or more, 13 μm or more, or 17 μm or more. On the other hand, the average particle size of the foaming agent is preferably equal to or less than the average thickness of the first adhesive layer, and may be, for example, 24 μm or less.

[0135] The average particle size of the foaming agent is the particle size at 50% of the cumulative value in the particle size distribution obtained by the laser diffraction scattering method. In addition, when measuring the average particle size of the foaming agent, the first adhesive layer is dissolved in a solvent to separate the foaming agent. The solvent is not particularly limited as long as it can dissolve components other than the foaming agent contained in the first adhesive layer, and is appropriately selected depending on the type of curable adhesive contained in the first adhesive layer, and for example, a solvent used in the adhesive composition used to form the first adhesive layer can be used. Specifically, methyl ethyl ketone, ethyl acetate, toluene, etc. can be used.

[0136] The content of the foaming agent is, for example, 0.5 parts by mass or more, 2 parts by mass or more, 3 parts by mass or more, 4 parts by mass or more, or 5 parts by mass or more, based on 100 parts by mass of the resin component contained in the first adhesive layer. On the other hand, the content of the foaming agent is, for example, 25 parts by mass or less, 20 parts by mass or less, or 15 parts by mass or less, based on 100 parts by mass of the resin component contained in the first adhesive layer. If the content of the foaming agent is too small, the expansion ratio of the first adhesive layer may be small, and the adhesiveness may be reduced. On the other hand, if the content of the foaming agent is too large, the content of the curable adhesive may be relatively small, and the cohesive force may be reduced, and the adhesiveness may be reduced.

[0137] (c) Other ingredients In the present embodiment, for example, when the first curable adhesive is an epoxy resin adhesive, the first adhesive layer may contain only an epoxy resin and an acrylic resin as the resin component, or may further contain other resins, such as urethane resins.

[0138] The total ratio of the first epoxy resin, the second epoxy resin and the acrylic resin to the resin components contained in the first adhesive layer is, for example, 70 mass% or more, optionally 80 mass% or more, optionally 90 mass% or more, or optionally 100 mass%.

[0139] The content of the resin component in the first adhesive layer is, for example, 60% by mass or more, optionally 70% by mass or more, optionally 80% by mass or more, or optionally 90% by mass or more.

[0140] The first adhesive layer may contain, as necessary, for example, a silane coupling agent, a filler, an antioxidant, a light stabilizer, an ultraviolet absorber, a lubricant, a plasticizer, an antistatic agent, a crosslinking agent, and a colorant. Examples of the silane coupling agent include epoxy-based silane coupling agents. Examples of the filler include inorganic fillers such as calcium carbonate, aluminum hydroxide, magnesium hydroxide, antimony trioxide, zinc borate, molybdenum compounds, and titanium dioxide. Examples of the antioxidant include phenol-based antioxidants and sulfur-based antioxidants.

[0141] (3) Configuration of the first adhesive layer The thickness of the first adhesive layer is not particularly limited. In particular, when the first adhesive layer contains a foaming agent, the thickness of the first adhesive layer is preferably equal to or greater than the average particle size of the foaming agent. The average thickness of the first adhesive layer is, for example, 10 μm or more, may be 15 μm or more, or may be 20 μm or more. If the first adhesive layer is too thin, there is a possibility that the adhesion to the substrate and the adhesiveness after curing cannot be sufficiently obtained. On the other hand, the average thickness of the first adhesive layer is, for example, 200 μm or less, may be 150 μm or less, or may be 100 μm or less. If the first adhesive layer is too thick, there is a possibility that the surface quality will deteriorate.

[0142] Here, the average thickness of the first adhesive layer is a value measured from a cross section of the adhesive sheet in the thickness direction observed by a transmission electron microscope (TEM), a scanning electron microscope (SEM) or a scanning transmission electron microscope (STEM), and is the average thickness value of 10 randomly selected points. The same method for measuring the average thickness of other layers of the adhesive sheet is also applied.

[0143] The first adhesive layer may be a continuous layer or a discontinuous layer. Examples of the discontinuous layer include a pattern such as a stripe or a dot. The surface of the first adhesive layer may have an uneven shape such as an embossed shape.

[0144] The method for forming the first adhesive layer will be described later in "B. Method for producing adhesive sheet", so description thereof will be omitted here.

[0145] 2. Base material The substrate in this embodiment is, for example, a member that supports the first adhesive layer.

[0146] The substrate in this embodiment is preferably insulating. The substrate is preferably in the form of a sheet. The substrate may have a single layer structure or a multi-layer structure. The substrate may or may not have a porous structure inside.

[0147] Examples of the substrate include a resin substrate and a nonwoven fabric.

[0148] Examples of the resin contained in the resin substrate include polyester resin, polycarbonate, polyarylate, polyurethane, polyamide resin, polyimide resin, polysulfone resin, polyether ketone resin, polyphenylene sulfide (PPS), modified polyphenylene oxide, etc. Examples of the polyester resin include polyethylene terephthalate (PET), polybutylene terephthalate, polyethylene naphthalate (PEN), and aromatic polyester. Examples of the polyamide resin include polyamide and polyether amide. Examples of the polyimide resin include polyimide, polyether imide, and polyamide imide. Examples of the polysulfonic acid resin include polysulfone and polyether sulfone. Examples of the polyether ketone resin include polyether ketone and polyether ether ketone. In addition, liquid crystal polymer (LCP) may be used as the resin.

[0149] The glass transition temperature of the resin is, for example, 80° C. or higher, may be 140° C. or higher, or may be 200° C. or higher.

[0150] Examples of the nonwoven fabric include nonwoven fabrics containing fibers such as cellulose fibers, polyester fibers, nylon fibers, aramid fibers, polyphenylene sulfide fibers, liquid crystal polymer fibers, glass fibers, metal fibers, and carbon fibers.

[0151] The substrate may be subjected to a surface treatment on the surface on which the first adhesive layer is to be disposed in order to enhance adhesion to the first adhesive layer.

[0152] The average thickness of the substrate is not particularly limited, but may be, for example, 2 μm or more, 5 μm or more, or 9 μm or more, and may be, for example, 200 μm or less, 100 μm or less, or 50 μm or less.

[0153] 3.First middle layer The adhesive sheet in this embodiment may have a first intermediate layer between the substrate and the first adhesive layer. The first intermediate layer can improve the adhesion of the first adhesive layer to the substrate. Furthermore, the first intermediate layer can, for example, relieve the stress on the bent portion when the adhesive sheet is folded, or relieve the stress on the cut portion when the adhesive sheet is cut. As a result, the lifting or peeling of the first adhesive layer from the substrate can be suppressed when the adhesive sheet is bent or cut.

[0154] For example, in adhesive sheet 10A shown in FIG. 5, substrate 1, first intermediate layer 5, and first adhesive layer 2 are disposed in this order in the thickness direction.

[0155] The material contained in the first intermediate layer is not particularly limited as long as it can increase the adhesion between the substrate and the first adhesive layer and can relieve stress, and is appropriately selected depending on the materials of the substrate and the adhesive layer, etc. Examples include polyester, polyvinyl chloride, polyvinyl acetate, polyurethane, a polymer obtained by copolymerizing at least two or more of them, a crosslinked product thereof, and a mixture thereof.

[0156] The crosslinked body is a crosslinked body obtained by crosslinking the above-mentioned resin with a curing agent. Examples of the curing agent include isocyanate-based curing agents. In addition, for example, when the reactive group / NCO equivalent is 1, it is preferable to add the isocyanate-based curing agent in a ratio of 0.5% by mass or more and 20% by mass or less to the resin.

[0157] Among them, the first intermediate layer preferably contains a crosslinked resin. The crosslinked resin is one that does not melt even at high temperatures. This can improve the adhesive strength at high temperatures, that is, the heat resistance. In addition, when the crosslinked resin is crosslinked by, for example, an isocyanate-based curing agent, the flexibility of the first intermediate layer is improved, and cracks in the first adhesive layer and lifting and peeling of the adhesive layer from the substrate when the adhesive sheet is bent can be suppressed.

[0158] The average thickness of the first intermediate layer is not particularly limited, and may be, for example, 0.1 μm or more, may be 0.5 μm or more, or may be 1 μm or more. If the first intermediate layer is too thin, the effect of suppressing peeling of the first adhesive layer from the substrate when the adhesive sheet is bent and cut may not be sufficiently obtained. On the other hand, the average thickness of the first intermediate layer may be, for example, 4 μm or less, or may be 3.5 μm or less. Since the first intermediate layer itself usually does not have high heat resistance, if the first intermediate layer is too thick, the heat resistance (adhesive strength at high temperatures) may decrease.

[0159] The first intermediate layer can be formed, for example, by applying a resin composition and removing the solvent. Examples of the application method include roll coating, reverse roll coating, transfer roll coating, gravure coating, gravure reverse coating, comma coating, rod coating, blade coating, bar coating, wire bar coating, die coating, lip coating, and dip coating.

[0160] 4. Adhesive sheet The adhesive sheet of this embodiment does not have another adhesive layer on the other side of the substrate. In the adhesive sheet of this embodiment, it is preferable that the first adhesive layer is disposed on one outermost surface and the substrate is disposed on the other outermost surface. When the adhesive sheet is wound into a roll, blocking caused by contact between the first adhesive layer and the substrate can be suppressed.

[0161] The adhesive sheet in this embodiment has an average thickness of, for example, 10 μm or more, and may be 20 μm or more, whereas the adhesive sheet has an average thickness of, for example, 1000 μm or less, and may be 200 μm or less.

[0162] The adhesive sheet in this embodiment preferably has good shape retention. The bending moment based on JIS P8125-2:2017 corresponding to ISO 2493-2 is, for example, 3 gf·cm or more, and may be 5 gf·cm or more. On the other hand, the bending moment may be, for example, less than 40 gf·cm, and may be less than 30 gf·cm. Conventionally, in adhesive sheets, a method of increasing the bending moment to improve shape retention and insertion into narrow gaps is common. In contrast, the inventors of the present disclosure have found that shape retention can be guaranteed by devising the shape, and that a high bending moment has other disadvantages, so that the bending moment is preferably within the above range in consideration of other characteristics. If the bending moment is smaller than the above range, it may be difficult to maintain the shape even by devising folding or the like. In addition, if the bending moment is larger than the above range, the shape will return to its original state after folding, so it is necessary to heat the sheet during folding or to make a crease at the fold. Heating the sheet reduces its lifespan, and striations can reduce the insulation properties of that area.

[0163] The adhesive sheet in this embodiment preferably has high adhesiveness after curing. The shear adhesive strength based on JIS K6850:1999 corresponding to ISO 4587 may be, for example, 2.10 MPa or more, 2.40 MPa or more, or 3.0 MPa or more at 23 ° C. In addition, the shear adhesive strength may be, for example, 0.27 MPa or more, 0.55 MPa or more, or 0.58 MPa or more at 200 ° C. For example, in a high-strength acrylic foam adhesive tape that does not require heating, the shear adhesive strength is about 1 MPa or more and 2 MPa or less at room temperature, and there is no heat resistance at 200 ° C. Therefore, if the shear adhesive strength is in the above range at 23 ° C., there is an advantage in terms of strength. In addition, if the shear adhesive strength is in the above range at 200 ° C., it can be applied to applications requiring heat resistance around the engine of an automobile or similar.

[0164] In the adhesive sheet of this embodiment, it is preferable that the electrical insulation after curing is high. The breakdown voltage based on JIS C2107:2011 corresponding to IEC 60454-2 is, for example, preferably 3 kV or more, more preferably 5 kV or more. When the breakdown voltage is in the above range, it becomes possible to apply it to rust prevention and around copper wires. In addition, in the adhesive sheet after curing, the thermal conductivity is, for example, preferably 0.1 W / mK or more, more preferably 0.15 W / mK or more. When the thermal conductivity is in the above range, it is possible to miniaturize the parts and promote the curing reaction during heating.

[0165] The use of the adhesive sheet in this embodiment is not particularly limited. For example, the adhesive sheet in this embodiment can be used in a case where the adhesive sheet is placed between two members and then cured to bond the two members.

[0166] The method for producing the adhesive sheet in this embodiment is not particularly limited, and will be described in the section "B. Method for producing adhesive sheet" below.

[0167] II. Second embodiment of adhesive sheet A second embodiment of the adhesive sheet in the present disclosure has a substrate, a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, and a second adhesive layer disposed on the other side of the substrate and containing a second curable adhesive, wherein the tack of the first adhesive layer and the second adhesive layer is less than 0.1 N, and the Martens hardness of the first adhesive layer and the second adhesive layer is less than 20 N / mm 2 More than 130N / mm 2 The following is the result.

[0168] Each component of the adhesive sheet of this embodiment will be described below.

[0169] 1. First adhesive layer and second adhesive layer The physical properties, material, thickness, and formation method of the first adhesive layer in this embodiment are the same as those of the first adhesive layer in the above-mentioned first embodiment. The physical properties, material, thickness, and formation method of the second adhesive layer in this embodiment are the same as those of the first adhesive layer in the above-mentioned first embodiment.

[0170] In addition, when measuring the Martens hardness of the first adhesive layer, the Martens hardness of the first adhesive layer is measured after removing the second adhesive layer from the adhesive sheet. On the other hand, when measuring the Martens hardness of the second adhesive layer, the Martens hardness of the second adhesive layer is measured after removing the first adhesive layer from the adhesive sheet. Examples of the method for removing the first adhesive layer or the second adhesive layer include a method of wiping with a solvent and a method of scraping. In the case of the method of wiping with a solvent, the solvent is not particularly limited as long as it dissolves the first adhesive layer or the second adhesive layer and does not dissolve the substrate, and for example, a solvent contained in the adhesive composition used to form the adhesive layer can be used.

[0171] In this embodiment, it is preferable that at least one of the first adhesive layer and the second adhesive layer contains a foaming agent. After placing the adhesive sheet between two members, the first adhesive layer of the adhesive sheet is foamed and cured to fill and adhere the space between the two members. In this case, only the first adhesive layer may contain a foaming agent, only the second adhesive layer may contain a foaming agent, or both the first adhesive layer and the second adhesive layer may contain a foaming agent. Among them, it is preferable that both the first adhesive layer and the second adhesive layer contain a foaming agent. The adhesiveness after foaming and curing can be improved.

[0172] 2. Base material The substrate in this embodiment is a member that supports the first adhesive layer and the second adhesive layer, and is the same as the substrate in the first embodiment.

[0173] 3. First and second intermediate layers The adhesive sheet in this embodiment may have a first intermediate layer between the substrate and the first adhesive layer, and the adhesive sheet in this embodiment may have a second intermediate layer between the substrate and the second adhesive layer.

[0174] For example, in adhesive sheet 10B shown in Fig. 6, a first adhesive layer 2 is disposed on one surface side of substrate 1, a second adhesive layer 3 is disposed on the other surface side of substrate 1, a first intermediate layer 5 is disposed between substrate 1 and first adhesive layer 2, and a second intermediate layer 6 is disposed between substrate 1 and second adhesive layer 3. Note that, although adhesive sheet 10B has both first intermediate layer 5 and second intermediate layer 6 in Fig. 6, it may have only one of them.

[0175] It is sufficient that an intermediate layer is disposed between the substrate and at least one of the adhesive layers, and for example, an intermediate layer may be disposed only between the substrate and one of the adhesive layers, or an intermediate layer may be disposed between the substrate and both of the adhesive layers. Among these, it is preferable that an intermediate layer is disposed between the substrate and both of the adhesive layers.

[0176] The material, thickness and formation method of the first and second intermediate layers are the same as those of the first intermediate layer in the first embodiment.

[0177] 4. Adhesive sheet In the adhesive sheet of this embodiment, it is preferable that a first adhesive layer is disposed on one outermost surface and a second adhesive layer is disposed on the other outermost surface, which can suppress blocking caused by contact between the first adhesive layer and the second adhesive layer when the adhesive sheet is wound into a roll.

[0178] The thickness, physical properties, uses, and manufacturing method of the adhesive sheet are the same as those of the adhesive sheet of the first embodiment described above.

[0179] III. Third embodiment of adhesive sheet A third embodiment of an adhesive sheet in the present disclosure has a substrate, a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, a second adhesive layer disposed on the other side of the substrate and containing a second curable adhesive, and a separator disposed on the side of the second adhesive layer opposite the substrate, wherein the tack of the first adhesive layer is less than 0.1 N, the tack of the second adhesive layer is 0.1 N or more, and the Martens hardness of the first adhesive layer is 20 N / mm 2 More than 130N / mm 2 The following is the result.

[0180] Each component of the adhesive sheet of this embodiment will be described below.

[0181] 1.First adhesive layer The physical properties, material, thickness and formation method of the first adhesive layer in this embodiment are the same as those of the first adhesive layer in the first embodiment described above.

[0182] In addition, when measuring the Martens hardness of the first adhesive layer, the Martens hardness of the first adhesive layer is measured after removing the second adhesive layer from the adhesive sheet. The method of removing the second adhesive layer is the same as that described in the second embodiment above.

[0183] 2.Second adhesive layer The second adhesive layer in this embodiment is disposed on the other surface side of the substrate, and the tack of the second adhesive layer is equal to or greater than a predetermined value.

[0184] (1) Physical properties of the second adhesive layer The tack of the second adhesive layer in this embodiment is 0.1N or more, may be 0.3N or more, or may be 0.5N or more. By having the tack of the second adhesive layer in the above range, the adhesion of the second adhesive layer to the member can be improved. In addition, the tack of the second adhesive layer is, for example, 10N or less, may be 5N or less, or may be 3N or less. If the tack of the second adhesive layer is too high, reworkability is reduced, and when the surface of the second adhesive layer of the adhesive sheet is attached to one of the members, it may be difficult to correct the positional deviation of the adhesive sheet.

[0185] Here, the method for measuring the tackiness of the second adhesive layer is the same as the method for measuring the tackiness of the first adhesive layer.

[0186] In this embodiment, the method of controlling the tackiness of the second adhesive layer includes, for example, a method of adjusting the composition of the second adhesive layer. Specifically, in the second adhesive layer containing an epoxy resin and a curing agent, when an epoxy resin that is liquid at room temperature is used or when a curing agent that is liquid at room temperature is used, the tackiness of the second adhesive layer tends to be high. In addition, in the second adhesive layer containing an epoxy resin and a curing agent, when an epoxy resin with a low softening temperature is contained or an epoxy resin with a small weight average molecular weight is contained, the tackiness of the second adhesive layer tends to be high. In addition, the tackiness of the second adhesive layer tends to be high by adding a tackifier resin to the second adhesive layer. Note that, when a curing agent that is liquid at room temperature is used, the tackiness tends to be high, but the storage stability may be reduced. Therefore, it is preferable to adjust the tackiness of the second adhesive layer by adjusting the properties and type of components other than the curing agent, such as the epoxy resin.

[0187] (2) Material for the second adhesive layer The second adhesive layer in this embodiment comprises a second curable adhesive.

[0188] (a) a second curable adhesive The second curable adhesive contained in the second adhesive layer in this embodiment is the same as the first curable adhesive used in the first adhesive layer in the above-mentioned first embodiment. In particular, the second curable adhesive is preferably an epoxy resin adhesive.

[0189] Hereinafter, an example in which the second curable adhesive is an epoxy resin adhesive will be described.

[0190] (i) Epoxy resin The epoxy resin in this embodiment is the same as the epoxy resin used in the first adhesive layer in the first embodiment described above.

[0191] As the epoxy resin, any epoxy resin generally used for the adhesive layer of an adhesive sheet can be used.

[0192] Examples of the epoxy resin include aromatic epoxy resins, aliphatic epoxy resins, alicyclic epoxy resins, and heterocyclic epoxy resins. Specific examples of the second epoxy resin are the same as those of the first epoxy resin used in the first adhesive layer in the first embodiment described above.

[0193] The epoxy resin may be a monofunctional epoxy resin, a difunctional epoxy resin, a trifunctional epoxy resin, or a tetrafunctional or higher functional epoxy resin.

[0194] Among them, it is preferable to use, as the epoxy resin, an epoxy resin that is liquid at room temperature, such as a bisphenol A type epoxy resin or a bisphenol F type epoxy resin, and an epoxy resin with a low softening point, because by using these epoxy resins, it is easy to adjust the tack of the second adhesive layer to within a predetermined range.

[0195] (ii) Acrylic resin When the second curable adhesive is an epoxy resin adhesive, the second adhesive layer may further contain an acrylic resin that is compatible with the epoxy resin, which can improve film-forming properties.

[0196] The acrylic resin is the same as the acrylic resin used in the first adhesive layer in the first embodiment described above.

[0197] (iii) Hardener The curing agent is the same as the curing agent used in the first adhesive layer in the first embodiment described above. In addition, as the curing agent, a curing agent that is solid at room temperature or a curing agent that is liquid at room temperature can be used. Among them, a curing agent that is solid at room temperature is preferred from the viewpoint of storage stability.

[0198] (b) Foaming agent In this embodiment, it is preferable that at least one of the first adhesive layer and the second adhesive layer contains a foaming agent. After placing the adhesive sheet between two members, the first adhesive layer of the adhesive sheet is foamed and cured to fill and adhere the space between the two members. In this case, only the first adhesive layer may contain a foaming agent, only the second adhesive layer may contain a foaming agent, or both the first adhesive layer and the second adhesive layer may contain a foaming agent. Among them, it is preferable that both the first adhesive layer and the second adhesive layer contain a foaming agent. The adhesiveness after foaming and curing can be improved.

[0199] The foaming agent is the same as the foaming agent used in the first adhesive layer in the first embodiment described above.

[0200] (c) Other ingredients In the present embodiment, for example, when the second curable adhesive is an epoxy resin adhesive, the second adhesive layer may contain only an epoxy resin and an acrylic resin as the resin component, or may further contain other resins, such as urethane resins.

[0201] The total ratio of epoxy resin and acrylic resin to the resin components contained in the second adhesive layer is, for example, 70 mass% or more, optionally 80 mass% or more, optionally 90 mass% or more, or optionally 100 mass%.

[0202] The content of the resin component in the second adhesive layer is, for example, 60% by mass or more, optionally 70% by mass or more, optionally 80% by mass or more, or optionally 90% by mass or more.

[0203] The second adhesive layer may contain an additive, if necessary. The additive may be the same as the additive used in the first adhesive layer in the first embodiment described above.

[0204] (3) Configuration of the second adhesive layer When the second adhesive layer further contains a foaming agent, the foaming ratio is the same as the foaming ratio of the first adhesive layer in the first embodiment described above.

[0205] The average thickness of the second adhesive layer is similar to the average thickness of the first adhesive layer in the first embodiment described above.

[0206] The second adhesive layer may be a continuous layer or a discontinuous layer. The surface of the second adhesive layer may have an uneven shape such as an embossed shape.

[0207] The method for forming the second adhesive layer is the same as the method for forming the first adhesive layer in the above-mentioned first embodiment.

[0208] 3.Base material The substrate in this embodiment is a member that supports the first adhesive layer and the second adhesive layer, and is the same as the substrate in the first embodiment.

[0209] 4. Separator The separator in this embodiment is disposed on the side of the second adhesive layer opposite the substrate.

[0210] The separator is not particularly limited as long as it can be peeled off from the second adhesive layer, and can have a strength sufficient to protect the second adhesive layer. Examples of such separators include release films and release papers. The separator may have a single-layer structure or a multi-layer structure.

[0211] An example of a separator having a single layer structure is a fluororesin film.

[0212] In addition, examples of the separator having a multi-layer structure include laminates having a release layer on one or both sides of a substrate layer. Examples of the substrate layer include resin films such as polypropylene, polyethylene, and polyethylene terephthalate, and papers such as fine paper, coated paper, and impregnated paper. Materials for the release layer are not particularly limited as long as they have releasability, and examples include silicone compounds, organic compound-modified silicone compounds, fluorine compounds, aminoalkyd compounds, melamine compounds, acrylic compounds, polyester compounds, and long-chain alkyl compounds. These compounds can be any of emulsion type, solvent type, and solventless type.

[0213] 5. First and second intermediate layers The adhesive sheet in this embodiment may have a first intermediate layer between the substrate and the first adhesive layer, and the adhesive sheet in this embodiment may have a second intermediate layer between the substrate and the second adhesive layer.

[0214] For example, in adhesive sheet 10C shown in Fig. 7, a first intermediate layer 5 is disposed between substrate 1 and first adhesive layer 2, and a second intermediate layer 6 is disposed between substrate 1 and second adhesive layer 3. Note that, although adhesive sheet 10B in Fig. 7 has both first intermediate layer 5 and second intermediate layer 6, it may have only one of them.

[0215] It is sufficient that an intermediate layer is disposed between the substrate and at least one of the adhesive layers, and for example, an intermediate layer may be disposed only between the substrate and one of the adhesive layers, or an intermediate layer may be disposed between the substrate and both of the adhesive layers. Among these, it is preferable that an intermediate layer is disposed between the substrate and both of the adhesive layers.

[0216] The material, thickness and formation method of the first and second intermediate layers are the same as those of the first intermediate layer in the first embodiment.

[0217] 6. Adhesive sheet In the adhesive sheet of this embodiment, it is preferable that a first adhesive layer is disposed on one outermost surface and a separator is disposed on the other outermost surface, which can suppress blocking caused by contact between the first adhesive layer and the separator when the adhesive sheet is wound into a roll.

[0218] The thickness, physical properties, uses, and manufacturing method of the adhesive sheet are the same as those of the adhesive sheet of the first embodiment described above.

[0219] B. Manufacturing method of adhesive sheet The inventors of the present disclosure have conducted intensive research into a method for producing an adhesive sheet having an adhesive layer on one or both sides of a substrate. First, as described in the above section "A. Adhesive Sheet", for example, hardening the adhesive layer is effective in improving the slipperiness and blocking resistance of the adhesive layer. However, if the adhesive layer becomes too hard, the adhesive layer is likely to crack, float, and peel when the adhesive sheet is wound and folded. Next, in the adhesive sheet, for example, an adhesive composition is applied to a substrate and dried to form an adhesive layer. At this time, if the drying temperature is low, blocking of the adhesive layer may not be suppressed. In addition, the drying temperature needs to be lower than the curing temperature of the adhesive layer. Furthermore, when the adhesive layer contains a foaming agent, the drying temperature needs to be lower than the foaming start temperature or decomposition temperature of the foaming agent. Therefore, the drying temperature cannot be made too high. Therefore, it is important to optimize the drying temperature. However, it has been found that even if the drying temperature and drying time are set to a predetermined temperature and time, blocking of the adhesive layer may or may not occur if the coating and drying device is different. The inventors of the present disclosure have conducted extensive research and found that the blocking of the adhesive layer can be suppressed by setting the drying conditions using the hardness of the adhesive layer as an index. They also found that by setting the tack of the adhesive layer to a predetermined range and drying the adhesive composition so that the Martens hardness of the adhesive layer is within a predetermined range when the adhesive layer is formed, it is possible to achieve a good balance between improving the slipperiness and blocking resistance of the adhesive layer and suppressing cracking, lifting, and peeling of the adhesive layer when it is wound up and folded. The present disclosure is based on such findings.

[0220] A method for producing an adhesive sheet according to the present disclosure includes a first adhesive layer forming step of applying a first adhesive composition containing a first curable adhesive to one side of a substrate and drying the applied composition to form a first adhesive layer, the first adhesive layer having a tack of less than 0.1 N, and the first adhesive layer having a Martens hardness of 20 N / mm 2 More than 130N / mm 2 The first adhesive composition is dried as follows.

[0221] 8(a)-(b) are process diagrams illustrating a method for producing an adhesive sheet according to the present disclosure. First, as shown in Fig. 8(a), a first adhesive composition 2a containing a first curable adhesive is applied to one surface of a substrate 1 and dried. As a result, a first adhesive layer 2 is formed as shown in Fig. 8(b).

[0222] In the present disclosure, by drying the first adhesive composition in the first adhesive layer formation process so that the tack of the first adhesive layer is less than a predetermined value and the Martens hardness of the first adhesive layer is within a predetermined range, it is possible to achieve a good balance between improving the slipperiness and blocking resistance of the first adhesive layer and suppressing cracking, lifting, and peeling of the first adhesive layer when it is wound up or folded.

[0223] In this manner, in the present disclosure, by using the Martens hardness of the first adhesive layer as an index of drying conditions and optimizing the drying conditions, it is possible to improve the blocking resistance while suppressing the cracking, lifting, and peeling of the first adhesive layer during winding and folding. Therefore, the blocking resistance can be improved regardless of the coating and drying device used.

[0224] Moreover, the adhesive sheet produced by the adhesive sheet producing method according to the present disclosure exhibits the same effects as the adhesive sheet described above.

[0225] Hereinafter, each step of the method for producing an adhesive sheet according to the present disclosure will be described.

[0226] 1. First adhesive layer formation process In the first adhesive layer forming step of the present disclosure, a first adhesive composition containing a first curable adhesive is applied to one side of a substrate and dried to form a first adhesive layer. In the first adhesive layer forming step, the Martens hardness of the first adhesive layer is 20 N / mm 2 More than 130N / mm 2 The first adhesive composition is dried as follows.

[0227] The first adhesive composition contains a first curable adhesive. The first adhesive composition may also contain a foaming agent. The components contained in the first adhesive composition are the same as the components contained in the first adhesive layer in the adhesive sheet described above.

[0228] The first adhesive composition may or may not contain a solvent. In this specification, the solvent is used in a broad sense including not only a strict solvent (a solvent that dissolves a solute) but also a dispersion medium. The solvent contained in the first adhesive composition is volatilized and removed when the first adhesive composition is dried.

[0229] The first adhesive composition can be obtained by mixing each component, and kneading and dispersing as necessary. As a mixing and dispersing method, a general kneading and dispersing machine, for example, a two-roll mill, a three-roll mill, a pebble mill, a tron ​​mill, a Szegvari attritor, a high-speed impeller dispersing machine, a high-speed stone mill, a high-speed impact mill, a disperser, a high-speed mixer, a ribbon blender, a co-kneader, an intensive mixer, a tumbler, a blender, a disperser, a homogenizer, or an ultrasonic dispersing machine can be used.

[0230] Examples of methods for applying the first adhesive composition include roll coating, reverse roll coating, transfer roll coating, gravure coating, gravure reverse coating, comma coating, rod coating, blade coating, bar coating, wire bar coating, die coating, lip coating, and dip coating.

[0231] The method for drying the applied first adhesive composition is not particularly limited as long as it is a method that can dry the first adhesive composition so that the Martens hardness of the first adhesive layer falls within a specified range, and examples of the method include heat drying.

[0232] In this process, the Martens hardness of the first adhesive layer is 20 N / mm 2 More than 130N / mm 2The first adhesive composition is dried so that the Martens hardness of the first adhesive layer is the same as the Martens hardness of the first adhesive layer in the adhesive sheet described above.

[0233] Drying conditions that affect the Martens hardness of the first adhesive layer include, for example, the drying temperature, the heat history, and the wind speed. Examples of the heat history include, for example, the temperature rise rate and the total amount of heat. For example, when the drying temperature is high, the Martens hardness of the first adhesive layer tends to increase. On the other hand, when the drying temperature is low, the Martens hardness of the first adhesive layer tends to decrease. Also, for example, when the temperature rise rate is fast, the total amount of heat increases when the drying time is constant, so the Martens hardness of the first adhesive layer tends to increase. On the other hand, when the temperature rise rate is slow, the total amount of heat decreases when the drying time is constant, so the Martens hardness of the first adhesive layer tends to decrease. Also, for example, when the total amount of heat received by the first adhesive layer increases, the Martens hardness of the first adhesive layer tends to increase. On the other hand, when the total amount of heat received by the first adhesive layer decreases, the Martens hardness of the first adhesive layer tends to decrease. Also, for example, when the wind speed is fast, the drying speed increases, so the Martens hardness of the first adhesive layer tends to increase. On the other hand, when the wind speed is slow, the drying speed is slow, and the Martens hardness of the first adhesive layer tends to be small.

[0234] The drying conditions are appropriately set so that the Martens hardness of the first adhesive layer is within a predetermined range. The drying temperature is, for example, 80° C. or more, may be 85° C. or more, or may be 90° C. or more. The drying temperature is, for example, 130° C. or less, may be 120° C. or less, or may be 110° C. or less. Specifically, the drying temperature is 80° C. or more and 130° C. or less, may be 85° C. or more and 120° C. or less, or may be 90° C. or more and 110° C. or less. The drying time is, for example, 1 minute or more, may be 1 minute 30 seconds or more, or may be 2 minutes or more. The drying time is, for example, 15 minutes or less, may be 10 minutes or less, or may be 8 minutes or less. Specifically, the drying time is 1 minute or more and 15 minutes or less, may be 1 minute 30 seconds or more and 10 minutes or less, or may be 2 minutes or more and 8 minutes or less. The temperature rise rate is, for example, 0.2° C. / second or more, may be 0.5° C. / second or more, or may be 0.8° C. / second or more. The temperature rise rate is, for example, 5.0° C. / sec or less, may be 4.0° C. / sec or less, or may be 3.0° C. / sec or less. Specifically, the temperature rise rate is 0.2° C. / sec or more and 5.0° C. / sec or less, may be 0.5° C. / sec or more and 4.0° C. / sec or less, or may be 0.8° C. / sec or more and 3.0° C. / sec or less. The wind speed is, for example, 1 m / sec or more, may be 3 m / sec or more, or may be 5 m / sec or more. The wind speed is, for example, 20 m / sec or less, may be 18 m / sec or less, or may be 15 m / sec or less. Specifically, the wind speed is 1 m / sec or more and 20 m / sec or less, may be 3 m / sec or more and 18 m / sec or less, or may be 5 m / sec or more and 15 m / sec or less.

[0235] The tackiness of the first adhesive layer is less than a predetermined value, and is the same as the tackiness of the first adhesive layer in the adhesive sheet described above.

[0236] 2.Second adhesive layer formation process The manufacturing method of the adhesive sheet in the present disclosure may include a second adhesive layer formation step of forming a second adhesive layer by applying a second adhesive composition containing a second curable adhesive to the other side of the substrate or one side of the separator and drying it.

[0237] When producing the adhesive sheet of the second embodiment described above, in the second adhesive layer forming step, the Martens hardness of the second adhesive layer is 20 N / mm 2 More than 130N / mm 2 The second adhesive composition is dried as follows: In this case, the second adhesive layer forming step is the same as the first adhesive layer forming step described above.

[0238] In the above case, the first adhesive layer forming step and the second adhesive layer forming step may be performed simultaneously or sequentially. Among them, it is preferable to perform the first adhesive layer forming step and the second adhesive layer forming step simultaneously. If the first adhesive layer forming step and the second adhesive layer forming step are performed sequentially, the first adhesive layer or the second adhesive layer will be more dried, and the drying conditions may deviate from the preferable conditions. In addition, when the first adhesive layer forming step and the second adhesive layer forming step are performed sequentially, the drying conditions may be set so that the Martens hardness of the first adhesive layer and the second adhesive layer after the first adhesive layer forming step and the second adhesive layer forming step is within a predetermined range.

[0239] On the other hand, when producing the adhesive sheet of the above-mentioned third embodiment, the drying conditions in the second adhesive layer forming step are not particularly limited.

[0240] In the above case, the first adhesive layer forming step and the second adhesive layer forming step may be performed simultaneously or sequentially. Among them, it is preferable to perform the first adhesive layer forming step and the second adhesive layer forming step simultaneously. Alternatively, it is preferable to apply the first adhesive composition to one side of the substrate, apply the second adhesive composition to one side of the separator, laminate the coating of the second adhesive composition with the separator to the other side of the substrate, and dry the first adhesive composition and the second adhesive composition to form the first adhesive layer and the second adhesive layer. In the case of these procedures, one drying is sufficient, so that the drying conditions of the first adhesive composition are easily adjusted to suitable conditions. In addition, if the first adhesive layer forming step and the second adhesive layer forming step are performed in sequence, the first adhesive layer will be dried more, and the drying conditions may deviate from the suitable conditions. However, when the first adhesive layer forming step and the second adhesive layer forming step are performed in sequence, the drying conditions may be set so that the Martens hardness of the first adhesive layer after the first adhesive layer forming step and the second adhesive layer forming step is within a predetermined range.

[0241] 3. Intermediate layer formation process The method for producing an adhesive sheet in the present disclosure may include a first intermediate layer forming step of forming a first intermediate layer on one side of the substrate before the first adhesive layer forming step. Also, the method for producing an adhesive sheet in the present disclosure may include a second intermediate layer forming step of forming a second intermediate layer on the other side of the substrate before the second adhesive layer forming step. The materials and forming methods of the first intermediate layer and the second intermediate layer are the same as those described in the above section "A. Adhesive Sheet".

[0242] C. Method of Manufacturing the Article A method for manufacturing an article according to the present disclosure includes a placement step of placing the above-mentioned adhesive sheet between a first member and a second member, and a bonding step of curing the adhesive sheet to bond the first member and the second member.

[0243] 9(a)-(b) are process diagrams showing an example of a method for manufacturing an article according to the present disclosure. First, as shown in FIG. 9(a), an adhesive sheet 10 is disposed between a first member 20a and a second member 20b. Next, as shown in FIG. 9(b), the adhesive sheet 10 is cured, for example, by heating. The first member 20a and the second member 20b are adhered (joined) by the cured adhesive sheet 11. This results in an article 100 in which the adhesive sheet 11 is disposed between the first member 20a and the second member 20b.

[0244] In the method for manufacturing an article according to the present disclosure, the adhesive sheet described above is used, so that the ease of insertion can be improved when inserting an adhesive sheet into the gap between two members, when inserting one member into the gap after placing the adhesive sheet in the hole or groove of the other member, or when inserting the other member to which the adhesive sheet is attached into the hole or groove of the one member. In addition, even if the adhesive sheet is folded in advance when placing the adhesive sheet between the first member and the second member, cracking, lifting, and peeling of the adhesive layer can be suppressed. Therefore, an article having good adhesion between the first member and the second member can be obtained.

[0245] The method for producing the article according to the present disclosure will now be described.

[0246] 1. Adhesive sheet The adhesive sheet used in the method for producing an article in the present disclosure is the same as the adhesive sheet described above.

[0247] 2.Placement process In the disposing step in the present disclosure, the method of disposing the adhesive sheet between the first member and the second member is not particularly limited. When using the adhesive sheet of the first embodiment and the adhesive sheet of the second embodiment, for example, a method of inserting an adhesive sheet into the gap between the first member and the second member, a method of disposing an adhesive sheet in the hole or groove of the first member, and then inserting a second member into the gap after disposing an adhesive sheet in the hole or groove of the first member, and a method of inserting a second member with an adhesive sheet disposed thereon into a hole or groove of the first member. In addition, when using the adhesive sheet of the third embodiment, for example, a method of inserting a second member with an adhesive sheet attached thereto into a hole or groove of the first member.

[0248] The material and shape of the first member and the second member are not particularly limited and are appropriately selected depending on the application.

[0249] 3.Gluing process In the bonding step of the present disclosure, the method of curing the adhesive sheet can be, for example, heating or light irradiation. Among them, it is preferable to cure the adhesive sheet by heating. The method of curing by heating can be applied even when the first member and the second member are not transparent, such as when the first member and the second member are made of metal.

[0250] The heating conditions are appropriately set depending on the types of the curable adhesive and foaming agent contained in the adhesive layer, the type of the base material, etc. The heating temperature is, for example, 130° C. or higher and 200° C. or lower. The heating time is, for example, 3 minutes or higher and 3 hours or lower.

[0251] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES

[0252] First, an adhesive composition having the composition (parts by mass) shown in Table 1 below was prepared. Details of each material listed in Table 1 are shown in Table 2. A highly insulating polyethylene naphthalate film (PEN film, manufactured by Toyobo Co., Ltd., Teonex Q5100-100, thickness 100 μm) was prepared as a substrate. The adhesive composition was applied to one surface of this substrate using a coating device so that the thickness after coating would be a predetermined thickness. Thereafter, the composition was dried in a coating dryer at a predetermined temperature for a predetermined time to form a first adhesive layer.

[0253] [evaluation] (1) Tuck For the tackiness of the first adhesive layer, a 5mm diameter cylindrical stainless steel probe was pressed against the surface of the first adhesive layer of the adhesive sheet at a temperature of 23±5°C and a humidity of 50±30%RH with a load of 0.1N and a speed of 30mm / min, and held for 1.0 second, then peeled off at a speed of 30mm / min, and the load at the time of peeling was measured using a tackiness tester "TAC-II" manufactured by RHESCA. This measurement was carried out five times, and the average value was taken as the tackiness.

[0254] (2) Martens hardness Using a Fisher Instruments Picodentor HM500, a diamond indenter in the shape of a regular pyramid was pressed against the surface of the first adhesive layer of the adhesive sheet at a temperature of 23±5°C and a humidity of 50±30%RH with a pressing load of 25mN and a loading time of 20 seconds, and then held for 5 seconds, after which the load was reduced to 0mN for the same time as the loading time, to measure the Martens hardness. This measurement was performed 8 times, and the average value was taken as the measured value. When measuring, the surface opposite the first adhesive layer of the adhesive sheet was cured with adhesive on a glass slide, eliminating the dependency on the contact surface.

[0255] (3) Blocking resistance The adhesive sheet was cut into a size of 5 cm x 5 cm, and two adhesive sheets were stacked together so that the first adhesive layers overlapped each other. The blocking resistance was measured using a blocking tester at 2 kg / cm 2 The samples were stored at 23° C. and 50% RH for 10 days, and the blocking resistance was evaluated according to the following criteria. A: There is no transfer or peeling of the first adhesive layer, and the adhesive sheets peel off naturally. B: There is no transfer or peeling of the first adhesive layer, and the adhesive sheets do not peel off naturally, but can be peeled off with very light force. C: The first adhesive layer has been transferred or peeled off, or the adhesive sheets do not peel off naturally and are so tightly attached that they make a peeling sound.

[0256] (5) Cross bending test The adhesive sheet was cut into a size of 3 cm x 3 cm, and the adhesive sheet was folded in half by 180° so that the surface of the first adhesive layer was on the inside and the size was 3 cm x 1.5 cm. Next, the adhesive sheet in this state was folded in half again by 180° so that the size was 1.5 cm x 1.5 cm. Then, it was confirmed whether the first adhesive layer was lifted from the substrate. The adhesion by the cross bending test was evaluated according to the following criteria. A: There is no floating in the folded parts. B: There is a gap at the bend.

[0257] (6) Cutter cutting test The surface of the adhesive sheet on the side of the first adhesive layer was cut with a cutter (OLFA Cutter Knife A Plus) at a speed of 20 mm / s to 100 mm / s to a length of 100 mm. Then, it was confirmed whether the first adhesive layer was lifted from the substrate at the cut surface. The adhesion by the cutter cutting test was evaluated according to the following criteria. A: There is absolutely no lifting on the cut surface. B: There is some lift on the cut surface. C: The cut surface is completely lifted.

[0258] [Table 1]

[0259] [Table 2]

[0260] [Table 3]

[0261] [Table 4]

[0262] [Table 5]

[0263] [Table 6]

[0264] It was confirmed that when the tack and Martens hardness of the first adhesive layer are within the specified ranges, the blocking resistance is good, and cracking, lifting, and peeling of the adhesive layer during winding and bending can be suppressed.

[0265] The present disclosure provides the following inventions. [1] An adhesive sheet having a substrate and a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, The tack of the first adhesive layer is less than 0.1 N; The first adhesive layer has a Martens hardness of 20 N / mm 2 More than 130N / mm 2 Below is the adhesive sheet. [2] A second adhesive layer containing a second curable adhesive is provided on the side of the substrate opposite to the first adhesive layer, The tack of the second adhesive layer is less than 0.1 N; The second adhesive layer has a Martens hardness of 20 N / mm 2 More than 130N / mm 2 The adhesive sheet according to [1] below. [3] A second adhesive layer containing a second curable adhesive and a separator are provided in this order on the side of the substrate opposite to the first adhesive layer, The adhesive sheet according to [1], wherein the second adhesive layer has a tack of 0.1 N or more. [4] The adhesive sheet according to [1], wherein the first adhesive layer contains a foaming agent. [5] The adhesive sheet according to [2] or [3], wherein at least one of the first adhesive layer and the second adhesive layer contains a foaming agent. [6] The adhesive sheet according to [1], wherein the first adhesive layer contains an epoxy resin. [7] The adhesive sheet according to [2] or [3], wherein the first adhesive layer and the second adhesive layer contain an epoxy resin. [8] A method for producing an adhesive sheet, comprising a first adhesive layer forming step of applying a first adhesive composition containing a first curable adhesive to one surface side of a substrate, and drying the applied composition to form a first adhesive layer, The tack of the first adhesive layer is less than 0.1 N; In the first adhesive layer forming step, the Martens hardness of the first adhesive layer is 20 N / mm 2 More than 130N / mm 2 The method for producing an adhesive sheet comprises drying the first adhesive composition as follows: [9] A second adhesive layer forming step of applying a second adhesive composition containing a second curable adhesive to the other surface side of the substrate and drying the composition to form a second adhesive layer; The tack of the second adhesive layer is less than 0.1 N; In the second adhesive layer forming step, the Martens hardness of the first adhesive layer is 20 N / mm 2 More than 130N / mm 2 The method for producing an adhesive sheet according to [6], further comprising drying the second adhesive composition so as to obtain the following:

[10] The method for producing an adhesive sheet according to [8], wherein the first adhesive composition contains a foaming agent.

[11] The method for producing an adhesive sheet according to [9], wherein at least one of the first adhesive composition and the second adhesive composition contains a foaming agent.

[12] The method for producing an adhesive sheet according to [8], wherein the first adhesive composition contains an epoxy resin.

[13] The method for producing an adhesive sheet according to [9], wherein the first adhesive composition and the second adhesive composition contain an epoxy resin.

[14] A step of placing the adhesive sheet according to any one of [1] to [7] between a first member and a second member; a bonding step of curing the adhesive sheet to bond the first member and the second member; A method for producing an article having the following structure: [Explanation of symbols]

[0266] 1 … Base material 2 … First adhesive layer 3...Second adhesive layer 4 … Separator 5 … First middle layer 6 … Second intermediate layer 10, 10A, 10B, 10C … adhesive sheet 11 ... Adhesive sheet after curing 20a … First member 20b … Second member 100 … Goods

Claims

1. An adhesive sheet having a substrate and a first adhesive layer disposed on one surface side of the substrate and containing a first curable adhesive, The tack of the first adhesive layer is less than 0.1 N; The first adhesive layer has a Martens hardness of 20 N / mm 2 130N / mm or more 2 Below is the adhesive sheet.

2. A second adhesive layer containing a second curable adhesive is provided on the side of the substrate opposite to the first adhesive layer, The tack of the second adhesive layer is less than 0.1 N; The second adhesive layer has a Martens hardness of 20 N / mm 2 130N / mm or more 2 The adhesive sheet according to claim 1 , wherein:

3. A second adhesive layer containing a second curable adhesive and a separator are provided in this order on the side of the substrate opposite to the first adhesive layer, The adhesive sheet according to claim 1 , wherein the second adhesive layer has a tack of 0.1 N or more.

4. The adhesive sheet according to claim 1 , wherein the first adhesive layer contains a foaming agent.

5. The adhesive sheet according to claim 2 or 3, wherein at least one of the first adhesive layer and the second adhesive layer contains a foaming agent.

6. The adhesive sheet according to claim 1 , wherein the first adhesive layer contains an epoxy resin.

7. The adhesive sheet according to claim 2 or 3, wherein the first adhesive layer and the second adhesive layer contain an epoxy resin.

8. A method for producing an adhesive sheet, comprising a first adhesive layer forming step of applying a first adhesive composition containing a first curable adhesive to one surface side of a substrate, and drying the applied composition to form a first adhesive layer, The tack of the first adhesive layer is less than 0.1 N; In the first adhesive layer forming step, the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 The method for producing an adhesive sheet comprises drying the first adhesive composition so as to obtain the following:

9. a second adhesive layer forming step of applying a second adhesive composition containing a second curable adhesive to the other surface side of the substrate and drying the composition to form a second adhesive layer; The tack of the second adhesive layer is less than 0.1 N; In the second adhesive layer forming step, the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 The method for producing an adhesive sheet according to claim 8 , wherein the second adhesive composition is dried so that:

10. The method for producing an adhesive sheet according to claim 8 , wherein the first adhesive composition contains a foaming agent.

11. The method for producing an adhesive sheet according to claim 9 , wherein at least one of the first adhesive composition and the second adhesive composition contains a foaming agent.

12. The method for producing an adhesive sheet according to claim 8 , wherein the first adhesive composition contains an epoxy resin.

13. The method for producing an adhesive sheet according to claim 9 , wherein the first adhesive composition and the second adhesive composition contain an epoxy resin.

14. a positioning step of positioning the adhesive sheet according to any one of claims 1 to 3 between a first member and a second member; a bonding step of curing the adhesive sheet to bond the first member and the second member; A method for producing an article having the following structure:

Citation Information

Patent Citations

  • Adhesive sheet

    JP2018021203A

  • Adhesive sheet

    JP2019214729A

  • Adhesive composition and foamable adhesive sheet

    JP2020076059A

  • Adhesive sheet

    JP2021006646A

  • Manufacturing method of expandable adhesive sheet and article

    JP2021155495A