Halogen-free resin composition, and electric wire and cable
A halogen-free resin composition with specific polyolefin and maleic anhydride-modified polyolefin ratios, combined with metal hydroxide and carbon black, addresses the need for enhanced flame retardancy, oil resistance, and low-temperature resistance in electric wires and cables, especially for railway vehicles.
Patent Information
- Application Number
- JP2024069530
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-04-23
- Publication Date
- 2024-11-27
AI Technical Summary
Existing halogen-free resin compositions for electric wires and cables, particularly those used in railway vehicles, lack sufficient flame retardancy and have inconsistent performance across various sizes and structures, necessitating further improvements in flame retardancy, oil resistance, and low-temperature properties.
A halogen-free resin composition comprising 60 to 70% crystalline polyolefin with a melting point of 110°C or higher, 30 to 40% maleic anhydride-modified polyolefin, 180 to 220 parts of metal hydroxide per 100 parts of the base polymer, and 1 to 10 parts of carbon black, which enhances flame retardancy, oil resistance, and low-temperature resistance.
The composition achieves improved flame retardancy, oil resistance, and low-temperature resistance, ensuring excellent performance in electric wires and cables, particularly those used in railway vehicles.
Smart Images

Figure 2024164812000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a halogen-free resin composition and an electric wire and cable using the same. [Background technology]
[0002] Electric wires and cables used in railway vehicles and the like are required to have properties such as flame retardancy, oil resistance, fuel resistance, and low temperature resistance in addition to general tensile strength and elongation.
[0003] In order to give electric wires and cables high flame retardancy, materials in which bromine-based flame retardants are added to polyolefins are used. However, since materials that contain a lot of halogens such as bromine generate large amounts of toxic gases when burned, electric wires and cables that use halogen-free materials that do not contain halogens are becoming more popular from the perspective of fire safety and reducing environmental impact.
[0004] In particular, because there is a risk that malfunctions in the electric wires and cables used in railway vehicles could lead to accidents, EN standards (EN50264, 50306, etc.) require them to be highly flame retardant, as well as oil-resistant, fuel-resistant, and low-temperature-resistant.
[0005] For example, Patent Document 1 (JP 2014-24910 A) discloses a cable that has flame retardancy and improved oil resistance, low temperature characteristics, and resistance to external damage. The cable uses a halogen-free flame-retardant resin composition consisting of a base polymer containing 60 to 70 mass% linear low-density polyethylene (LLDPE), 10 mass% or more ethylene-vinyl acetate copolymer (EVA) having a melt flow rate (MFR) of 100 or more, and 10 to 20 mass% maleic acid-modified polyolefin, and a metal hydroxide and carbon black added in a ratio of 150 to 220 parts by mass per 100 parts by mass of the base polymer.
[0006] In addition, Patent Document 2 (JP 2020-125459 A) discloses a cable that has flame retardancy, oil resistance, and improved low temperature characteristics by using a halogen-free flame-retardant resin composition that has a base polymer having 60 to 70 parts by mass of polyolefin, 10 to 35 parts by mass of maleic anhydride-modified polyolefin, and 5 to 30 parts by mass of ethylene-vinyl acetate copolymer (EVA), a metal hydroxide added in a ratio of 150 to 250 parts by mass per 100 parts by mass of the base polymer, and carbon black added in a ratio of 1 to 30 parts by mass per 100 parts by mass of the base polymer, wherein the melting point of the polyolefin is 110°C or higher and the gel fraction after crosslinking is 85% or higher. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2014-24910 A [Patent Document 2] JP 2020-125459 A Summary of the Invention [Problem to be solved by the invention]
[0008] The resin compositions described in Patent Documents 1 and 2 above have been found to have limited flame retardancy when applied to cables of various sizes and different structures, and further improvements in flame retardancy are desired.
[0009] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a halogen-free resin composition that is halogen-free yet has good flame retardancy, oil resistance and low temperature resistance, and an insulated wire or cable using the same. Other objects and novel features will become apparent from the description of this specification and the accompanying drawings. [Means for solving the problem]
[0010] One embodiment of the halogen-free resin composition is a halogen-free resin composition comprising a base polymer, a metal hydroxide, and carbon black, wherein the base polymer comprises 60 to 70 mass% of a crystalline polyolefin and 30 to 40 mass% of a maleic anhydride modified polyolefin, the crystalline polyolefin comprising a first crystalline polyolefin having a melting point of 110°C or higher, and contains 180 to 220 mass parts of the metal hydroxide and 1 part by mass or more and less than 10 parts by mass of the carbon black per 100 mass parts of the base polymer.
[0011] An electric wire according to one embodiment has an insulating layer formed from the above-mentioned halogen-free resin composition.A cable according to one embodiment has a sheath (coating layer) formed from the above-mentioned halogen-free resin composition. Effect of the Invention
[0012] According to one embodiment, it is possible to obtain a halogen-free resin composition that is halogen-free yet has good flame retardancy, oil resistance, and low temperature resistance, and an electric wire and cable using the same.
[0013] By using the halogen-free resin composition as a covering material for electric wires or cables, it is possible to impart good flame retardancy, oil resistance, and low temperature resistance. [Brief description of the drawings]
[0014] [Figure 1] 1 is a cross-sectional view showing a structural example of an electric wire according to an embodiment; [Diagram 2] 1 is a cross-sectional view showing an example of the structure of a cable according to an embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] An embodiment of the present invention will be described below with reference to the drawings. In all the drawings for explaining the embodiment, the same reference numerals are used for components having the same functions, and the repeated description will be omitted. In the following embodiment, the description of the same or similar parts will not be repeated as a rule unless it is particularly necessary.
[0016] <Preliminary considerations> The resin compositions described in Patent Documents 1 and 2 above use a crystalline polyolefin such as linear low-density polyethylene (LLDPE) mixed with an ethylene-vinyl acetate copolymer (EVA) and a maleic acid-modified polyolefin.
[0017] Ethylene vinyl acetate copolymer (EVA) is considered to be a necessary component for blending a large amount of metal hydroxide to ensure sufficient flame retardancy, and furthermore, in Patent Document 2, carbon black is used as a flame retardant auxiliary agent, making it possible to increase the blending amount in an attempt to further improve flame retardancy. That is, the inventions described in these documents blend a metal hydroxide as a flame retardant into a base polymer in which EVA is added to a crystalline polyolefin.
[0018] However, because the resin compositions described in these patent documents may burn depending on the size of the cable, the inventors investigated the morphology of various resin compositions and cables to which they are applied when burned. In observing the morphology in detail, they discovered that the side chains of the EVA contained in the resin composition may undergo deacetylation, causing the carbonized layer formed during burning to foam and become brittle, which may result in lower flame retardancy than expected.
[0019] Therefore, the present inventors have investigated halogen-free resin compositions suitable for use in electric wires and cables and having improved flame retardancy, and have found a novel halogen-free resin composition described below.
[0020] <Halogen-free resin composition> The halogen-free resin composition of the present embodiment will be described in detail below.
[0021] The halogen-free resin composition according to the present embodiment, as described above, contains a base polymer, a metal hydroxide, and carbon black. The base polymer contains 60 to 70 mass % of a crystalline polyolefin and 30 to 40 mass % of a maleic anhydride modified polyolefin, and as the crystalline polyolefin, a first crystalline polyolefin having a melting point of 110°C or higher. The halogen-free resin composition contains 180 to 220 mass parts of a metal hydroxide and 1 part by mass or more and less than 10 parts by mass of carbon black per 100 parts by mass of the base polymer.
[0022] [Base polymer] The base polymer used in the present embodiment contains (1) a crystalline polyolefin and (2) a maleic anhydride-modified polyolefin. Each component will be described below.
[0023] (1) Crystalline polyolefin The crystalline polyolefin used here is a polyolefin having crystallinity. In the present embodiment, the crystalline polyolefin includes a crystalline polyolefin having a melting point of 110°C or higher. In this specification, the melting point can be determined by differential scanning calorimetry (DSC). By using such a polyolefin having a melting point of 110°C or higher, the oil resistance can be improved.
[0024] One method of oil resistance testing is to immerse a test piece in IRM902 test oil heated to 100°C for 72 hours, then check the tensile properties to see how much the tensile properties after immersion have changed compared to the tensile properties before immersion. For example, if the melting point falls below 110°C, the crystals will melt during the oil resistance test, making it difficult to prevent the oil from diffusing into the base polymer, and the rate of change in the tensile properties will increase.
[0025] Examples of polyolefins with a melting point of 110°C or higher include polyethylenes such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE), as well as polypropylene (PP). However, high-density polyethylene (HDPE) has too high a degree of crystallinity and a low breaking elongation, while polypropylene (PP) is prone to collapse when crosslinked by electron beam irradiation or the like. To obtain a balance of properties, it is preferable to use low-density polyethylene (LDPE), and it is more preferable to use linear low-density polyethylene (LLDPE).
[0026] The amount of crystalline polyolefin added is preferably 60 to 70% by mass when the base polymer is taken as 100% by mass. If it is less than 60% by mass, the oil resistance may be insufficient, and if it is more than 70% by mass, the low-temperature elongation may not be sufficient. In addition, when a low-molecular-weight polyethylene is used as the crystalline polyolefin, the molecular entanglement may disappear, and the elongation may decrease, so it is preferable to use one with an MFR (melt flow rate, JIS K 7210, 190°C, 2.16 kg load) of 10 g / 10 min or less.
[0027] The crystalline polyolefin may contain crystalline polyethylene having a melting point of 110° C. or higher [first crystalline polyolefin] as a polyolefin having a melting point of 110° C. or higher, and may further contain a crystalline polyolefin (excluding polyethylene) having a melting point of 100° C. or higher [second crystalline polyolefin] different from the first crystalline polyolefin. This makes it possible to improve the flexibility of the electric wire or cable while maintaining the oil resistance.
[0028] Examples of the second crystalline polyolefin include olefin block copolymers (OBC) such as ethylene block copolymers, ethylene ethyl acrylate copolymers (EEA), and ethylene butyl acrylate copolymers.
[0029] The above-mentioned crystalline polyethylene is preferably a polymer having a heat of fusion of 50 J / g or more, more preferably 75 J / g or more. If the heat of fusion is 50 J / g or more, the oil resistance can be improved. The heat of fusion is a value obtained by measuring with a differential scanning calorimeter (DSC) in the temperature range of -50°C to 200°C at a heating rate of 10°C / min.
[0030] When a first crystalline polyolefin made of polyethylene having a melting point of 110° C. or higher is used in combination with a second crystalline polyolefin having a melting point of 100° C. or higher, both oil resistance and flexibility can be achieved by making the first crystalline polyolefin 30% by mass or higher and the second crystalline polyolefin 20% by mass or higher. That is, it is preferable that the first crystalline polyolefin is contained in the base polymer at 30% by mass to 50% by mass, and the second crystalline polyolefin is contained in the base polymer at 20% by mass to 40% by mass.
[0031] (2) Maleic anhydride modified polyolefin The maleic anhydride modified polyolefin used here is a compound obtained by modifying a polyolefin with maleic anhydride.
[0032] Examples of polyolefins (before modification) used as materials to be modified include polyethylenes such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and very low-density polyethylene (VLDPE), and ethylene-α-olefins such as ethylene-methyl acrylate copolymers, ethylene-ethyl acrylate copolymers, ethylene-butyl acrylate copolymers, ethylene-butene-1 copolymers, ethylene-hexene-1 copolymers, and ethylene-octene-1 copolymers. Among these, ethylene-butene-1 copolymers, ethylene-hexene-1 copolymers, and ethylene-octene-1 copolymers have few crystals and are excellent in filler acceptance in resin compositions, and therefore are preferably used as materials for maleic anhydride-modified polyolefins.
[0033] The method for modifying the unmodified polyolefin with maleic anhydride is not particularly limited and can be carried out by a known method, for example, by a reaction using only heat by heating. In addition, the maleic anhydride in the maleic anhydride-modified polyolefin may be graft copolymerized or block copolymerized.
[0034] The amount of the maleic anhydride modified polyolefin is 30 to 40% by mass relative to 100% by mass of the base polymer. If it is less than 30% by mass, the required low-temperature properties and flame retardancy may not be satisfied, whereas if it is more than 40% by mass, the interaction of the filler may become too strong, increasing the viscosity and deteriorating the processability during extrusion molding.
[0035] [Metal hydroxide] In this embodiment, a metal hydroxide is added to the base polymer as a flame retardant. Examples of the metal hydroxide used here include aluminum hydroxide, magnesium hydroxide, and calcium hydroxide.
[0036] Among them, it is preferable to use aluminum hydroxide and magnesium hydroxide. The heat absorption amount during decomposition of calcium hydroxide is about 1000 J / g, whereas the heat absorption amount of aluminum hydroxide and magnesium hydroxide is 1500 to 1600 J / g, which is high. Therefore, by adding aluminum hydroxide or magnesium hydroxide, the flame retardancy is improved.
[0037] Furthermore, it is preferable to select magnesium hydroxide, which has a higher decomposition temperature than aluminum hydroxide, and therefore, for example, the temperature during molding of the resin composition can be increased, improving molding processability.
[0038] The metal hydroxide may be surface-treated with a silane coupling agent, a titanate coupling agent, a fatty acid such as stearic acid, or the like in order to improve dispersibility.
[0039] The metal hydroxide preferably has a BET specific surface area of 5.0 or more. With a BET specific surface area of 5.0 or more, the interaction between the polymer and the metal hydroxide is strengthened, and the tensile strength is improved. The BET specific surface area can be calculated using nitrogen gas as the adsorbate in accordance with the "carrier gas method" of JIS Z 8830:2013.
[0040] The amount of the metal hydroxide added is 180 to 220 parts by mass per 100 parts by mass of the base polymer. If the amount is less than 180 parts by mass, sufficient flame retardancy cannot be obtained, and if the amount is more than 220 parts by mass, extrusion moldability decreases.
[0041] [Carbon black] The carbon black used here acts as a colorant. Any known carbon black can be used as the carbon black to be added without any particular limitation, but in consideration of the breaking elongation, it is preferable to use FT or MT class carbon.
[0042] The amount of carbon black to be added is preferably 1 part by mass or more and less than 10 parts by mass, and more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the base polymer. In the present embodiment, carbon black is not added as a flame retardant auxiliary as in Patent Document 2, for example, so that the amount of carbon black added may be about the same as that of a conventionally known coloring agent, and sufficient flame retardancy can be ensured even without adding an ethylene-vinyl acetate copolymer.
[0043] [Other additives] To the base polymer, flame retardant auxiliaries, crosslinking agents, crosslinking assistants, ultraviolet absorbers, light stabilizers, softeners, lubricants, colorants, reinforcing agents, surfactants, inorganic fillers, antioxidants, plasticizers, metal chelating agents, foaming agents, compatibilizers, processing assistants, stabilizers, etc. may be added.
[0044] Known flame retardant auxiliaries can be used as the flame retardant auxiliaries. Phosphorus-based flame retardant auxiliaries such as red phosphorus and triazine-based flame retardant auxiliaries such as melamine cyanurate are available, but they may generate phosphine gas or cyan gas, so they must be handled with care. Flame retardant auxiliaries other than these can also be used, and examples of such auxiliaries include clay, silica, zinc stannate, zinc borate, calcium borate, dolomide hydroxide, and silicone.
[0045] The resin composition of the above formulation has crosslinking properties and can be crosslinked by crosslinking treatment. Crosslinking treatments include chemical crosslinking using organic peroxides, sulfur compounds, silanes, etc., irradiation crosslinking using electron beams or radiation, and chemical crosslinking using other chemical reactions, and any crosslinking method can be applied. Among them, irradiation crosslinking using electron beams is more versatile than other irradiation crosslinking methods and does not have the risk of scorching during extrusion molding as with chemical crosslinking, so it is preferable to use it as the crosslinking treatment of this embodiment.
[0046] <Electric wire> Next, an electric wire according to one embodiment will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view showing an example of the configuration of the electric wire according to the present embodiment.
[0047] 1, the electric wire 11 according to the present embodiment includes a conductor 11a, an insulating inner layer 11b formed on the outer periphery of the conductor 11a, and an insulating outer layer 11c formed on the outer periphery of the insulating inner layer 11b. In this manner, the insulating layer covering the conductor 11a may have a two-layer structure including the insulating inner layer 11b and the insulating outer layer 11c.
[0048] The conductor 11a may be, for example, a stranded wire in which a plurality of strands (metal wires) are stranded together. The strands may be, for example, copper wires, copper alloy wires, aluminum wires, gold wires, silver wires, or the like, and may be metal-plated, such as tin or nickel, on the outer periphery.
[0049] For example, polyethylene or polybutylene terephthalate can be used as the insulating inner layer 11b. In addition, additives such as antioxidants, silane coupling agents including silicone rubber, flame retardants, flame retardant assistants, crosslinking agents, crosslinking assistants, crosslinking accelerators, hydrolysis inhibitors (e.g., polycarbodiimide compounds), lubricants (e.g., fatty acid metal salts, amide-based lubricants), softeners, plasticizers, inorganic fillers, carbon black, compatibilizers, stabilizers, metal chelating agents, ultraviolet absorbers, light stabilizers, and colorants may be added to the inner layer material as necessary. In addition, a composition crosslinked by silane water crosslinking or electron beam irradiation may be used as the insulating inner layer 11b. The above-mentioned halogen-free resin composition can be used as the insulating outer layer 11c.
[0050] Also, other resin compositions containing halogen-free flame retardants may be used as the insulating outer layer 11c. It is preferable that halogen-free flame retardants are not added to phosphorus-based flame retardants such as red phosphorus or triazine-based flame retardants such as melamine cyanurate. The polymer applied to the insulating outer layer 11c is not particularly limited as long as it is halogen-free. For example, polyolefins such as high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), very low density polyethylene (VLDPE), and ethylene-acrylate copolymers can be used. Rubber materials can also be used, and examples of such materials include ethylene-propylene copolymer rubber, ethylene-propylene-diene ternary copolymer rubber, acrylic rubber, ethylene-acrylate copolymer rubber, ethylene-octene copolymer rubber, ethylene-vinyl acetate copolymer rubber, ethylene-butene-1 copolymer rubber, butadiene-styrene copolymer rubber, isobutylene-isoprene copolymer rubber, and block copolymer rubber having a polystyrene block. Engineering plastics can also be used, such as polyethylene terephthalate, polybutylene terephthalate, polyphenylene ether, polycarbonate, polyamide, polyphenylene sulfide, polyether ether ketone, polyethylene naphthalate, polybutylene naphthalate, polyether sulfone, etc., and thermoplastic elastomers thereof can also be used. The base polymer may be a single polymer or a blend of two or more polymers.
[0051] In the insulating outer layer 11c, a crosslinking agent, a crosslinking assistant, a flame retardant assistant, an ultraviolet absorber, a light stabilizer, a softener, a lubricant, a colorant, a reinforcing agent, a surfactant, an inorganic filler, a plasticizer, a metal chelating agent, a foaming agent, a compatibilizer, a processing assistant, a stabilizer, and the like can be added to the resin composition composed of the above-mentioned materials, as necessary.
[0052] From the viewpoint of oil resistance, crosslinking is necessary. The crosslinking treatment may be chemical crosslinking using an organic peroxide or a silane compound, irradiation crosslinking using an electron beam or radiation, or crosslinking using other chemical reactions, and any crosslinking method may be used.
[0053] By adopting such a two-layer structure, the electrical insulation can be improved by the insulating inner layer 11b on the conductor 11a side, and the flame retardancy can be improved by the insulating outer layer 11c which is the outermost layer.
[0054] 1, the insulating layer covering the conductor 11a has a two-layer structure consisting of an inner insulating layer 11b and an outer insulating layer 11c, but it may have a three or more layer structure or may be a single layer. In either case, by using the above-mentioned halogen-free resin composition as the outermost layer, the characteristics of the halogen-free insulated wire can be improved.
[0055] The electric wire 11 of the present embodiment is manufactured, for example, as follows. First, a resin composition for forming the insulating inner layer 11b and the insulating outer layer 11c is prepared. In the present embodiment, as the resin composition which is a feature of the present embodiment, for example, a material containing a crystalline polyolefin and a maleic anhydride modified polyolefin as a base polymer, a metal hydroxide, and carbon black is melt-kneaded to obtain the resin composition of the present embodiment.
[0056] Then, the conductor 11a is prepared. Then, the resin composition is extruded by an extrusion molding machine so as to cover the periphery of the conductor 11a, thereby forming the insulating inner layer 11b, and then the resin composition of the present embodiment is extruded so as to cover the periphery of the insulating inner layer 11b, thereby forming the insulating outer layer 11c. Furthermore, the resin composition is crosslinked as necessary, thereby manufacturing the electric wire 11.
[0057] <Cable> Next, a cable according to an embodiment will be described with reference to Fig. 2. Fig. 2 is a cross-sectional view showing an example of the configuration of a cable according to the present embodiment.
[0058] As shown in Fig. 2, the cable 12 according to the present embodiment includes two twisted electric wires 11 (twisted core, see Fig. 1), a separator 12b provided on the outside of the twisted core, a shield braid 12c provided so as to cover the separator, and a sheath (outer jacket layer, covering layer) 12d that covers the shield braid 12c. By using the above-mentioned halogen-free resin composition for the sheath 12d, the characteristics of the halogen-free cable can be improved.
[0059] The number of electric wires 11 may be one or more. The material of separator 12b is not particularly limited, and it may be provided on the outside of shield braid 12c. Shield braid 12c is made of a conductive material, typically a metal material, to provide a shielding effect.
[0060] There is no limit to the uses of such wires and cables. For example, they can be used as insulated wires or cables for railroad cars.
[0061] The cable 12 of this embodiment is manufactured, for example, as follows. First, two electric wires 11 are manufactured by the above-mentioned method. Then, the two electric wires 11 are twisted together with staple yarn, paper tape, jute, or the like, and then, a separator 12b and a shield braid 12c are formed in this order by a known method so as to cover the twisted electric wires. Furthermore, the resin composition of this embodiment is extruded around the outer periphery of the shield braid 12c thus obtained in the same manner as in the above-mentioned electric wire manufacturing method, to form a sheath 12d of a predetermined thickness. In this manner, the cable 12 of this embodiment can be manufactured.
[0062] In the above, the cable 12 of this embodiment is described using the above-mentioned electric wire 11 as an example, but this is not limited to this, and an electric wire using a general-purpose material for the insulating layer can also be used. EXAMPLES
[0063] The halogen-free resin composition, electric wire, and cable of the present embodiment will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0064] <Preparation of halogen-free resin composition> In Examples 1 to 11, halogen-free resin compositions were produced according to the blending ratios shown in Table 1, and in Comparative Examples 1 to 5, according to the blending ratios shown in Table 2. The blending amounts in Tables 1 and 2 are in parts by mass. That is, the blending materials shown in Tables 1 and 2 were kneaded using a pressure kneader, extruded using a strand, cooled, and then pelletized. The blending ratios of the halogen-free resin compositions in each Example and Comparative Example will be described in detail later.
[0065] <Manufacture of electric wires and cables> First, an electric wire (see FIG. 1) was produced. Here, 19 tin-plated copper conductors with a diameter of 0.18 mm were used as the conductors 11a. Polybutylene terephthalate (manufactured by Mitsubishi Engineering Plastics Corporation, product name: Novaduran 5026) was used as the insulating inner layer 11b. The insulating outer layer 11c was made by kneading 30 parts by mass of polyethylene (manufactured by Prime Polymer, product name: Hi-Zex 5305E), 30 parts by mass of ethylene-ethyl acrylate-maleic anhydride terpolymer (manufactured by Arkema, product name: Bondine LX4110), 10 parts by mass of maleic anhydride modified ethylene-α-olefin (manufactured by Mitsui Chemicals, product name: Toughma MA7020), 30 parts by mass of ethylene-ethyl acrylate copolymer (manufactured by Japan Polyethylene, product name: Rexpearl A1150), and 150 parts by mass of magnesium hydroxide (manufactured by Kyowa Chemical, product name: Kisuma 5L) in a 14-inch open roll and pelletizing with a granulator. A 40 mm extruder was used to extrude two layers on the outside of the conductor 11a so that the thickness of the insulating inner layer 11b was 0.1 mm and the thickness of the insulating outer layer 11c was 0.16 mm, and the conductor 11a was covered with the insulating inner layer 11b and the insulating outer layer 11c. The obtained electric wire 11 was irradiated with an electron beam to perform crosslinking.
[0066] Next, a cable (see FIG. 2) was manufactured using the electric wire 11. Two of the obtained electric wires 11 were twisted together to form a twisted core, on which a 32 μm polyethylene terephthalate separator 12b was wrapped, and on top of that, a shield braid 12c with a braid density of 80% was formed using a 0.11 mm tin-plated copper conductor to form a core.
[0067] The composition shown in Tables 1 and 2 was extruded onto the above core using a 40 mm extruder to a thickness of 0.7 mm to form a sheath 12d. The sheath 12d of the obtained cable was irradiated with an electron beam at the dose shown in Tables 1 and 2 to crosslink the sheath 12d, thereby producing a cable 12. Detailed operations and the like related to the production of the cable 12 will be described later.
[0068] <Evaluation and Judgment> The sheath 12d of the cable 12 obtained above was tested and evaluated for each of the properties of extrusion moldability, tensile strength, elongation, oil-resistant tensile strength retention, oil-resistant elongation retention, low-temperature elongation, and flame retardancy as described below, and the results are summarized in Tables 1 and 2.
[0069] [Extrusion moldability] When the sheath was extruded, it was rated as ◯ (good) if it could be extruded without any problems, and it was rated as × (not good) if it could not be extruded due to high viscosity of the halogen-free resin composition.
[0070] [Tensile test] The twisted cores and other components were pulled out of the resulting cable, and the tubular sheath was punched out with a No. 6 dumbbell to obtain a test specimen. The test specimen was pulled at room temperature (25°C) at a displacement rate of 250 mm / min, and the load until break and the length after elongation (Lb) were measured. The tensile strength (units [MPa]) was calculated from the load. In addition, the breaking elongation ((Lb-La) / La) x 100 [%]) was calculated from the initial length La and the length after elongation Lb. Breaking elongation of 200% or more was rated as ◎ (excellent), 150% or more but less than 200% was rated as ○ (good), and less than 150% was rated as × (unacceptable).
[0071] [Low temperature test] The twisted cores and other components were pulled out of the resulting cable, and the tubular sheath was punched out using a No. 6 dumbbell to obtain a test specimen. The test specimen was held at -50°C and pulled at a displacement rate of 25 mm / min in a -50°C atmosphere, and the elongation (L2) until breakage was measured. The low-temperature elongation ((L2 / L1) x 100[%]) was calculated from the initial length L1 and the elongation L2. A low-temperature elongation of 50% or more was rated as ◎ (excellent), 30% or more but less than 50% was rated as ○ (good), and less than 30% was rated as × (unacceptable).
[0072] [Oil resistance test] The twisted cores were pulled out of the cable, and the tubular sheath was punched out with a No. 6 dumbbell to obtain a test specimen. The test specimen was immersed in IRM902 test oil heated to 100°C for 72 hours, after which it was pulled at a displacement rate of 250 mm / min, and the stress and elongation until break were measured. The oil-resistant tensile strength retention rate ((A2 / A1) x 100[%]) and oil-resistant elongation retention rate ((B2 / B1) x 100[%]) were calculated from the tensile strength (A1) and elongation at break (B1) of the test specimen before immersion in the test oil, and the tensile strength (A2) and elongation at break (B2) of the test specimen after immersion in the test oil.
[0073] If the oil-resistant tensile strength retention rate was within the range of 70-130%, it was rated as ○ (good), and if it was outside the range of 70-130%, it was rated as × (not good). In particular, if it was within the range of 85-115%, it was rated as ◎ (excellent).
[0074] If the oil resistance elongation at break was within the range of 60-140%, it was rated as ○ (good), if it was outside the range of 60-140%, it was rated as × (not good). In particular, if it was within the range of 80-120%, it was rated as ⊚ (excellent).
[0075] [Combustion test (flame retardancy)] A 600mm long cable was cut as a test specimen, held vertically and exposed to a flame for 60 seconds, after which the flame was removed. If the fire self-extinguished, it was rated as ◎ (excellent). For specimens that did not self-extinguish, the same test was performed twice in a row with different test specimens, and if the fire self-extinguished in at least one of the three tests, it was rated as ○ (good). For specimens that did not self-extinguish all three times, the test specimen was held at a 60° incline, exposed to a flame for 60 seconds, and then the flame was removed, if the fire self-extinguished, it was rated as △ (passable). If the fire did not self-extinguish even in this 60° inclined combustion test, it was rated as × (unacceptable).
[0076] [comprehensive evaluation] As for the overall evaluation, in the evaluation of the above-mentioned properties other than extrusion moldability (tensile test (elongation at break), low temperature test (elongation at low temperature), oil resistance test (oil-resistant tensile strength retention, oil-resistant elongation at break retention), and combustion test (flame retardancy)), those that were all marked with ◎ were rated as ◎ (excellent), those that included ○ were rated as ○ (good), and those that included × were rated as × (unacceptable).
[0077] [Table 1]
[0078] [Table 2]
[0079] Example 1 Crystalline polyolefin 1 (LLDPE, manufactured by Prime Polymer, product name: SP1510; melting point 117°C) 60 parts by mass, modified polyolefin 1 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, Inc., product name: TAFMA MH7020) 40 parts by mass, metal hydroxide 1 (magnesium hydroxide, manufactured by Konoshima Chemical Co., Ltd., product name: Magseeds S4) 180 parts by mass, colorant (carbon black, manufactured by Asahi Carbon Co., Ltd., product name: Asahi Thermal) 2 parts by mass, A halogen-free resin composition was prepared by kneading 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, product name: Irganox 1010), 1 part by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, product name: Adeka STAB AO-18), 1 part by mass of lubricant (zinc stearate, manufactured by Sakai Chemical Industry Co., Ltd., product name: SZ-P), and 4 parts by mass of crosslinking assistant agent (trimethylolpropane trimethacrylate (TMPT), manufactured by Shin-Nakamura Chemical Industry Co., Ltd.). This was used as a sheath material to manufacture a cable as described above. In Example 1, it was irradiated with electron beam at 75 kGy.
[0080] As shown in Table 1, in Example 1, all the characteristics (except for extrusion moldability) were rated as ⊚, and the overall rating was ⊚.
[0081] Example 2 Crystalline polyolefin 1 (LLDPE, manufactured by Prime Polymer, product name: SP1510; melting point 117°C) 60 parts by mass, modified polyolefin 1 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, product name: TAFMA MH7020) 30 parts by mass, modified polyolefin 2 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, product name: TAFMA MH5040) 10 parts by mass, metal hydroxide 2 (aluminum hydroxide, manufactured by Huber, product name: MARTIANL A cable was manufactured using a halogen-free resin composition as a sheath material, which was kneaded with 220 parts by mass of OL-104C), 2 parts by mass of colorant (carbon black, manufactured by Asahi Carbon Co., Ltd., product name: Asahi Thermal), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, product name: Irganox 1010), 1 part by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA Co., Ltd., product name: Adeka STAB AO-18), 1 part by mass of lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., product name: SZ-P), and 4 parts by mass of crosslinking assistant agent (trimethylolpropane trimethacrylate (TMPT), manufactured by Shin-Nakamura Chemical Co., Ltd.). In Example 2, the cable was irradiated with an electron beam at 125 kGy. From Table 1, in Example 2, all the characteristics were ◎ or ○, and the overall evaluation was ○.
[0082] (Examples 3 to 6) Crystalline polyolefin 1 (LLDPE, manufactured by Prime Polymer, product name: SP1510; melting point 117°C) 30 to 40 parts by mass, Crystalline polyolefin 2 (olefin block copolymer (OBC), manufactured by Dow Chemical, product name: INFUSE9100; melting point 120°C) 30 to 40 parts by mass, Modified polyolefin 1 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, product name: TAFMA MH7020) 30 parts by mass, Metal hydroxide 1 (magnesium hydroxide, manufactured by Konoshima Chemical, product name: Magseeds S4) 180 to 200 parts by mass, Colorant (Carbon A cable was manufactured using a halogen-free resin composition as a sheath material, which was kneaded with 2 parts by mass of 100% 1 ...
[0083] (Examples 7 to 10) Crystalline polyolefin 1 (LLDPE, manufactured by Prime Polymer, product name: SP1510; melting point 117°C) 30 to 40 parts by mass, Crystalline polyolefin 2 (olefin block copolymer (OBC), manufactured by Dow Chemical, product name: INFUSE9100; melting point 120°C) 30 to 40 parts by mass, Modified polyolefin 2 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, product name: Toughma MH5040) 30 parts by mass, Metal hydroxide 1 (magnesium hydroxide, manufactured by Kamishima Kogyo Co., Ltd., product name: Magseeds S4) 180 to 200 parts by mass, Colorant (carbon A cable was manufactured using a halogen-free resin composition as a sheath material, which was kneaded with 2 parts by mass of black (manufactured by Asahi Carbon Co., Ltd., product name: Asahi Thermal), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, product name: Irganox 1010), 1 part by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, product name: Adeka STAB AO-18), 1 part by mass of lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., product name: SZ-P), and 4 parts by mass of crosslinking assistant (trimethylolpropane trimethacrylate (TMPT), manufactured by Shin-Nakamura Chemical Co., Ltd.). In Examples 7 to 10, the electron beam was irradiated at 125 kGy. From Table 1, in Examples 7 to 10, all the characteristics were rated as ◎ or ○, and the overall evaluation was also rated as ○.
[0084] Example 11 Crystalline polyolefin 1 (LLDPE, manufactured by Prime Polymer, product name: SP1510; melting point 117°C) 40 parts by mass, Crystalline polyolefin 3 (ethylene-ethyl acrylate copolymer (EEA), manufactured by Japan Polyethylene, product name: A3100; melting point 104°C) 30 parts by mass, Modified polyolefin 1 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, product name: Toughma MH7020) 30 parts by mass, Metal hydroxide 1 (magnesium hydroxide, manufactured by Konoshima Chemical, product name: Magseeds S4) 180 parts by mass, Colorant (carbon black A cable was manufactured using a halogen-free resin composition as a sheath material, which was kneaded with 2 parts by mass of antioxidant 1 (manufactured by Asahi Carbon Co., Ltd., product name: Asahi Thermal), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, product name: Irganox 1010), 1 part by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA Corporation, product name: Adeka STAB AO-18), 1 part by mass of lubricant (zinc stearate, manufactured by Sakai Chemical Industry Co., Ltd., product name: SZ-P), and 4 parts by mass of crosslinking assistant agent (trimethylolpropane trimethacrylate (TMPT), manufactured by Shin-Nakamura Chemical Industry Co., Ltd.). In Example 11, the cable was irradiated with an electron beam at 100 kGy. From Table 1, in Example 11, all the characteristics were ◎ or ○, and the overall evaluation was also ○.
[0085] Comparative Example 1 Crystalline polyolefin 1 (LLDPE, manufactured by Prime Polymer, product name: SP1510; melting point 117°C) 55 parts by mass, non-crystalline amorphous polyolefin (ethylene vinyl acetate copolymer (EVA), manufactured by Mitsui Dow Polychemicals, product name: EV45X) 15 parts by mass, modified polyolefin 3 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, product name: TAFMA MH7010) 30 parts by mass, metal hydroxide 1 (magnesium hydroxide, manufactured by Konoshima Chemical Co., Ltd., product name: Magseeds S4) 180 parts by mass, colorant (carbon black, A cable was manufactured using a halogen-free resin composition as a sheath material, which was made by kneading 2 parts by mass of Asahi Thermal (manufactured by Asahi Carbon Co., Ltd., product name: Asahi Thermal), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, product name: Irganox 1010), 1 part by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, product name: Adeka STAB AO-18), 1 part by mass of lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., product name: SZ-P), and 4 parts by mass of crosslinking assistant (trimethylolpropane trimethacrylate (TMPT), manufactured by Shin-Nakamura Chemical Co., Ltd.). In Comparative Example 1, the cable was irradiated with an electron beam at 75 kGy.
[0086] As can be seen from Table 2, in Comparative Example 1, the content of crystalline polyolefin was insufficient, so the oil-resistant tensile strength retention was not within the range of 70 to 130%, and the low-temperature elongation was below 30%, and each of these was rated as ×, resulting in an overall rating of ×.
[0087] Comparative Example 2 Crystalline polyolefin 1 (LLDPE, manufactured by Prime Polymer, product name: SP1510; melting point 117°C) 50 parts by mass, Crystalline polyolefin 3 (ethylene-ethyl acrylate copolymer (EEA), manufactured by Japan Polyethylene, product name: A3100; melting point 104°C) 30 parts by mass, Modified polyolefin 1 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, product name: Toughma MH7020) A cable was manufactured using a halogen-free resin composition as a sheath material, which was kneaded with 20 parts by mass of 100% ethylene glycol, 180 parts by mass of metal hydroxide 1 (magnesium hydroxide, manufactured by Kamishima Chemical Co., Ltd., product name: Magseeds S4), 2 parts by mass of colorant (carbon black, manufactured by Asahi Carbon Co., Ltd., product name: Asahi Thermal), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, product name: Irganox 1010), 1 part by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, product name: Adeka STAB AO-18), 1 part by mass of lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., product name: SZ-P), and 4 parts by mass of crosslinking assistant (trimethylolpropane trimethacrylate (TMPT), manufactured by Shin-Nakamura Chemical Co., Ltd.). In Comparative Example 2, the cable was irradiated with an electron beam at 75 kGy.
[0088] As can be seen from Table 2, in Comparative Example 2, the content of modified polyolefin was insufficient, so that the low-temperature elongation was below 30% and the evaluation was poor, resulting in an overall evaluation of poor.
[0089] Comparative Example 3 Crystalline polyolefin 1 (LLDPE, manufactured by Prime Polymer, product name: SP1510; melting point 117°C) 50 parts by mass, modified polyolefin 1 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, product name: TAFMA MH7020) 30 parts by mass, modified polyolefin 2 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, product name: TAFMA MH7040) 20 parts by mass, metal hydroxide 3 (aluminum hydroxide, manufactured by Huber, product name: MARTIANL A cable was manufactured using a halogen-free resin composition as a sheath material, which was kneaded with 240 parts by mass of OL-104C), 2 parts by mass of a colorant (carbon black, manufactured by Asahi Carbon Co., Ltd., product name: Asahi Thermal), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, product name: Irganox 1010), 1 part by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA Corporation, product name: Adeka STAB AO-18), 1 part by mass of a lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., product name: SZ-P), and 4 parts by mass of a crosslinking assistant (trimethylolpropane trimethacrylate (TMPT), manufactured by Shin-Nakamura Chemical Co., Ltd.). In Comparative Example 3, the cable was irradiated with an electron beam at 75 kGy.
[0090] As can be seen from Table 2, in Comparative Example 3, the amount of metal hydroxide added was large and the amount of modified polyolefin was also large, so the breaking elongation was below 150% and the evaluation was poor, resulting in an overall evaluation of poor.
[0091] Comparative Example 4 Crystalline polyolefin 1 (LLDPE, manufactured by Prime Polymer, product name: SP1510; melting point 117°C) 40 parts by mass, crystalline polyolefin 3 (ethylene-ethyl acrylate copolymer (EEA), manufactured by Japan Polyethylene, product name: A3100; melting point 104°C) 50 parts by mass, modified polyolefin 1 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, product name: TAFMA MH7020) 10 parts by mass, metal hydroxide 2 (aluminum hydroxide, manufactured by Huber, product name: MARTIANL A cable was produced using a halogen-free resin composition as a sheath material, which was kneaded with 160 parts by mass of OL-104ZO), 2 parts by mass of colorant (carbon black, manufactured by Asahi Carbon Co., Ltd., product name: Asahi Thermal), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, product name: Irganox 1010), 1 part by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA Corporation, product name: Adeka STAB AO-18), 1 part by mass of lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., product name: SZ-P), and 4 parts by mass of crosslinking assistant agent (trimethylolpropane trimethacrylate (TMPT), manufactured by Shin-Nakamura Chemical Co., Ltd.). In Comparative Example 4, the cable was irradiated with an electron beam at 125 kGy.
[0092] As can be seen from Table 2, in Comparative Example 4, the content of the metal hydroxide was insufficient, so that the flame retardancy test was scored as x, and the overall evaluation was also scored as x.
[0093] Comparative Example 5 Crystalline polyolefin 1 (LLDPE, manufactured by Prime Polymer, product name: SP1510; melting point 117°C) 60 parts by mass, non-crystalline amorphous polyolefin (ethylene vinyl acetate copolymer (EVA), manufactured by Mitsui Dow Polychemicals, product name: EV45X) 30 parts by mass, modified polyolefin 1 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, product name: TAFMA MH7020) 10 parts by mass, metal hydroxide 2 (aluminum hydroxide, manufactured by Huber, product name: MARTIANL A cable was produced using a halogen-free resin composition as a sheath material, which was kneaded with 180 parts by mass of OL-104ZO), 2 parts by mass of colorant (carbon black, manufactured by Asahi Carbon Co., Ltd., product name: Asahi Thermal), 2 parts by mass of antioxidant 1 (phenol-based antioxidant, manufactured by BASF, product name: Irganox 1010), 1 part by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA Corporation, product name: Adeka STAB AO-18), 1 part by mass of lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., product name: SZ-P), and 4 parts by mass of crosslinking assistant agent (trimethylolpropane trimethacrylate (TMPT), manufactured by Shin-Nakamura Chemical Co., Ltd.). In Comparative Example 5, the cable was irradiated with an electron beam at 75 kGy.
[0094] As can be seen from Table 2, in Comparative Example 5, the content of modified polyolefin was insufficient, so that the low-temperature elongation was below 30% and the evaluation was poor, resulting in an overall evaluation of poor.
[0095] From the above results, it was found that Examples 1 to 11 were excellent in all evaluations, and were halogen-free resin compositions that could improve flame retardancy while maintaining oil resistance and low-temperature properties, and were suitable for the insulating layer of electric wires and the sheath (coating layer) of cables.
[0096] Although the present invention has been described with reference to the above-mentioned embodiment and examples, the present invention is not limited to the above-mentioned embodiment and examples, and various modifications can be made without departing from the spirit and scope of the present invention. [Industrial Applicability]
[0097] The halogen-free resin composition of the present invention can be used not only for halogen-free, flame-retardant electric wires and cables, but also for sheets, films, panels, mats, pipes, protective materials, fillers, fibers, resin molded products, resin substrates, stationery, building materials, connectors, bushes, grommets, terminal blocks, terminal internal insulators, etc., which require halogen-free flame retardancy. [Explanation of symbols]
[0098] 11 Electric wire 11a Conductor 11b Insulating inner layer 11c Insulating outer layer 12 Cable 12b Separator 12c shield braid 12d Sheath
Claims
1. A halogen-free resin composition comprising a base polymer, a metal hydroxide, and carbon black, The base polymer contains 60 to 70% by mass of a crystalline polyolefin and 30 to 40% by mass of a maleic anhydride modified polyolefin, and the crystalline polyolefin includes a crystalline polyolefin having a melting point of 110° C. or higher; A crosslinkable halogen-free resin composition comprising 180 to 220 parts by mass of the metal hydroxide and 1 part by mass or more but less than 10 parts by mass of the carbon black relative to 100 parts by mass of the base polymer.
2. A halogen-free resin composition comprising a base polymer, a metal hydroxide, and carbon black, The base polymer contains 60 to 70% by mass of a crystalline polyolefin and 30 to 40% by mass of a maleic anhydride modified polyolefin, and the crystalline polyolefin includes a crystalline polyolefin having a melting point of 110° C. or higher; The composition contains 180 to 220 parts by mass of the metal hydroxide and 1 part by mass or more but less than 10 parts by mass of the carbon black relative to 100 parts by mass of the base polymer, The halogen-free resin composition is a crosslinked product obtained by subjecting the base polymer to a crosslinking treatment.
3. The halogen-free resin composition according to claim 1 or 2, A halogen-free resin composition that does not contain an ethylene-vinyl acetate copolymer as the base polymer.
4. The halogen-free resin composition according to claim 1 or 2, The crystalline polyolefin includes a first crystalline polyolefin which is a polyethylene having a melting point of 110° C. or more, and a second crystalline polyolefin which is a polyolefin (excluding polyethylene) having a melting point of 100° C. or more, The base polymer contains 30% by mass or more of the first crystalline polyolefin and 20% by mass or more of the second crystalline polyolefin, A halogen-free resin composition comprising 180 to 220 parts by mass of the metal hydroxide per 100 parts by mass of the base polymer.
5. The halogen-free resin composition according to claim 1 or 2, The halogen-free resin composition, wherein the crystalline polyolefin is a polymer having a heat of fusion of 50 J / g or more.
6. The halogen-free resin composition according to claim 1 or 2, The halogen-free resin composition, wherein the metal hydroxide has a BET specific surface area of 5.0 or more.
7. An electric wire having a conductor and an insulating layer provided around the conductor, The insulating layer is a halogen-free resin composition containing a base polymer, a metal hydroxide, and carbon black, the base polymer containing 60 to 70 mass % of a first crystalline polyolefin having a melting point of 110°C or higher and 30 to 40 mass % of a maleic anhydride modified polyolefin, and the halogen-free resin composition containing 180 to 220 parts by mass of the metal hydroxide and 1 part by mass or more but less than 10 parts by mass of the carbon black per 100 parts by mass of the base polymer.
8. A cable having an electric wire and a coating layer provided on the outside thereof, The covering layer is a halogen-free resin composition containing a base polymer, a metal hydroxide, and carbon black, the base polymer containing 60 to 70 mass % of a first crystalline polyolefin having a melting point of 110°C or higher and 30 to 40 mass % of a maleic anhydride modified polyolefin, and the halogen-free resin composition containing 180 to 220 parts by mass of the metal hydroxide and 1 part by mass or more but less than 10 parts by mass of the carbon black per 100 parts by mass of the base polymer.
Citation Information
Patent Citations
Halogen-free flame-retardant resin composition, insulated electric wire, and cable
JP2014024910A
Non-halogen resin composition, electric wire and cable
JP2020125459A
Cited By
Flame retardant polyamide composition
JP2024528079A