Manufacturing method of cyclic siloxane compound, hollow particle and manufacturing method thereof, and manufacturing method of silica particle

A method using a cyclic siloxane compound with specific organic groups bonded to silicon atoms in a siloxane skeleton addresses the complexity and heat resistance issues of existing hollow particle production, resulting in particles with enhanced thermal stability and a straightforward manufacturing process.

JP2024172198APending Publication Date: 2024-12-12NIPPON SHOKUBAI CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023089754
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Existing methods for producing hollow particles, such as those described in Patent Document 1, are complex and do not adequately address the need for improved heat resistance, requiring a simpler and more efficient production method that can yield hollow particles with enhanced thermal stability.

Method used

The production of hollow particles involves using a cyclic siloxane compound with a cyclic skeleton composed of siloxane bonds, where silicon atoms are bonded to polymerizable unsaturated groups and alkyl or aryl groups, and is achieved through hydrolysis and condensation of silane monomers followed by radical polymerization in the presence of a hydrocarbon solvent, allowing for the formation of a crosslinked structure with controlled hollowness and high silicon content.

Benefits of technology

This method enables the production of hollow particles with excellent heat resistance and a high thermal decomposition initiation temperature, along with a simple and efficient process for obtaining the necessary raw materials, facilitating the use of these particles in various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024172198000001
    Figure 2024172198000001
  • Figure 2024172198000002
    Figure 2024172198000002
Patent Text Reader

Abstract

To provide a hollow particle with excellent heat resistance, a manufacturing method thereof, and a method of easily obtaining a compound to be served as a raw material of the hollow particle.SOLUTION: A hollow particle includes a structure derived from a cyclic siloxane compound. The cyclic siloxane compound includes a cyclic skeleton including a siloxane bond. Each of silicon atoms composing the cyclic skeleton is bonded with an organic group selected from a polymerizable unsaturated group, an alkyl group having 1 to 10 carbon atoms, and an aryl group having 6 to 10 carbon atoms. At least one silicon atom composing the cyclic skeleton is bonded with the polymerizable unsaturated group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a cyclic siloxane compound, hollow particles and a method for producing the same, and a method for producing silica particles. [Background technology]

[0002] Taking advantage of their hollow structure, hollow resin particles are expected to be used in insulation materials, low-reflection materials, low-refractive index materials, low-dielectric materials, microcapsules, and more.

[0003] For example, Patent Document 1 discloses organic-inorganic hybrid hollow particles, which are hollow particles having a shell consisting of at least one layer, the hollow particles having an average particle diameter of 10 to 200 nm, and the at least one layer being made of a silicon-containing vinyl resin. In Patent Document 1, a reactive monomer having a radical reactive functional group and a non-radical reactive functional group is polymerized based on either one of the two functional groups to prepare polymer particles, and a non-reactive solvent is mixed with the reactive monomer in advance or absorbed after the preparation of the polymer particles to contain the polymer particles, and then the polymer and the non-reactive solvent are phase-separated by polymerization based on the remaining functional group of the two functional groups, and then the non-reactive solvent is removed to obtain hollow particles. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-61664 A Summary of the Invention [Problem to be solved by the invention]

[0005] In Patent Document 1, as described above, hollow particles are produced by phase separation of a polymer and a non-reactive solvent through two-stage polymerization, but a simpler method is desired. In addition, heat resistance may be required for hollow particles depending on the application.

[0006] Therefore, an object of the present invention is to provide hollow particles having good heat resistance and a method for producing the same, as well as to provide a method for easily obtaining compounds that are raw materials for the hollow particles. [Means for solving the problem]

[0007] The present invention which achieves the above object is as follows. [1] A hollow particle containing a structure derived from a cyclic siloxane compound, The cyclic siloxane compound has a cyclic skeleton formed of siloxane bonds, each of the silicon atoms constituting the cyclic skeleton has an organic group bonded thereto selected from a polymerizable unsaturated group, an alkyl group having 1 to 10 carbon atoms, and an aryl group having 6 to 10 carbon atoms; At least one of the silicon atoms constituting the cyclic skeleton has a polymerizable unsaturated group bonded to it. [2] The hollow particle according to [1], wherein the silicon ratio is 10 to 40 mass %. [3] The hollow particle according to [1] or [2], which has a hollow ratio of 10 to 60%. [4] The hollow particle according to any one of [1] to [3], wherein the cyclic siloxane compound is a cyclic siloxane compound having two or more polymerizable unsaturated groups in one molecule. [5] The hollow particles according to any one of [1] to [4], which have an average particle size of 0.1 to 100 μm. [6] The hollow particles according to any one of [1] to [5], which have a thermal decomposition starting temperature of 200° C. or higher. [7] Having a cyclic skeleton formed of siloxane bonds, each of the silicon atoms constituting the cyclic skeleton has an organic group bonded thereto selected from a polymerizable unsaturated group, an alkyl group having 1 to 10 carbon atoms, and an aryl group having 6 to 10 carbon atoms; A method for producing a cyclic siloxane compound in which at least one of the silicon atoms constituting the cyclic skeleton has a polymerizable unsaturated group bonded thereto, comprising the steps of: A step of hydrolyzing and condensing a silane monomer in a solvent containing water to prepare a dispersion containing the cyclic siloxane compound; and removing water from the dispersion. A method for producing a cyclic siloxane compound. [8] A step of producing the cyclic siloxane compound by the production method described in [7], and obtaining a solvent-cyclic siloxane compound mixture from the obtained cyclic siloxane compound and a hydrocarbon solvent; a step of stirring the solvent-cyclic siloxane compound mixture in a solvent containing water to radically polymerize the cyclic siloxane compound. [9] obtaining a solvent-cyclic siloxane compound mixture from a cyclic siloxane compound and a hydrocarbon solvent; a step of stirring the solvent-cyclic siloxane compound mixture in a solvent containing water to radically polymerize the cyclic siloxane compound, The cyclic siloxane compound has a cyclic skeleton formed of siloxane bonds, each of the silicon atoms constituting the cyclic skeleton has an organic group bonded thereto selected from a polymerizable unsaturated group, an alkyl group having 1 to 10 carbon atoms, and an aryl group having 6 to 10 carbon atoms; A method for producing hollow particles, wherein at least one of the silicon atoms constituting the cyclic skeleton has a polymerizable unsaturated group bonded thereto.

[10] The method for producing hollow particles according to [8] or [9], further comprising a step of emulsifying the solvent-cyclic siloxane compound mixture prior to the radical polymerization step.

[11] The method for producing hollow particles according to any one of [8] to

[10] , wherein the amount of the hydrocarbon solvent is 10 to 200 parts by mass per 100 parts by mass of the cyclic siloxane compound.

[12] The method for producing hollow particles according to any one of [8] to

[11] , wherein the cyclic siloxane compound has a silicon content of 10 to 40 mass %.

[13] Producing hollow particles by the production method according to any one of [8] and [9]; A method for producing silica particles, comprising calcining the hollow particles.

[14] Producing hollow particles by the production method according to any one of

[10] to

[12] ; A method for producing silica particles, comprising calcining the hollow particles. Effect of the Invention

[0008] According to the present invention, hollow particles having excellent heat resistance can be obtained by a simple method, and compounds serving as raw materials for such hollow particles can also be easily obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention includes hollow particles and a method for producing the same, as well as a method for producing a cyclic siloxane compound that is a raw material for the hollow particles, and a method for producing silica particles by calcining the hollow particles.

[0010] 1. Cyclic siloxane compounds The cyclic siloxane compound used as the raw material for the hollow particles of the present invention has a cyclic skeleton formed of siloxane bonds, each of which has bonded to it an organic group selected from a polymerizable unsaturated group, an alkyl group having 1 to 10 carbon atoms, and an aryl group having 6 to 10 carbon atoms, and at least one of the silicon atoms which make up the cyclic skeleton is bonded to a polymerizable unsaturated group.

[0011] The cyclic skeleton consisting of siloxane bonds is preferably a cyclic skeleton consisting of only siloxane bonds, in which two or more -Si-O- units are continuously bonded in a ring. The number of -Si-O- units in the cyclic siloxane compound is 2 or more, and the upper limit may be, for example, 8, preferably 3 to 6, and more preferably 3 to 4.

[0012] Each of the silicon atoms forming the cyclic skeleton formed of siloxane bonds is bonded with two O atoms and two organic groups selected from a polymerizable unsaturated group, an alkyl group having 1 to 10 carbon atoms, and an aryl group having 6 to 10 carbon atoms, and at least one of the silicon atoms constituting the cyclic skeleton is bonded with a polymerizable unsaturated group. The two organic groups bonded to each silicon atom may be the same or different, and the combination of the two organic groups bonded to the silicon atom may be the same or different for each silicon atom.

[0013] The polymerizable unsaturated group in the organic group includes a group having a vinyl group or a (meth)acryloyl group at the terminal, and a group represented by the following formula (1) is preferable.

[0014] [ka]

[0015] In formula (1), R 11 represents hydrogen, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 10 carbon atoms; R 12 represents an alkylene group having 1 to 10 carbon atoms or a divalent aromatic hydrocarbon group having 6 to 10 carbon atoms, m is 0 or 1, n is 0 or 1, and the group represented by formula (1) is bonded to a silicon atom at *.

[0016] R 11 Examples of the alkyl group having 1 to 10 carbon atoms in the formula include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl groups; branched alkyl groups such as isopropyl, isobutyl, isopentyl, neopentyl, and 2-ethylhexyl groups; and the like. Of these, linear alkyl groups are preferred, and the linear alkyl group preferably has 1 to 7 carbon atoms, more preferably 1 to 4, even more preferably 1 or 2, and even more preferably 1.

[0017] R 11Examples of the aryl group having 6 to 10 carbon atoms in the formula (I) include a phenyl group, an o-tolyl group, an m-tolyl group, a p-tolyl group, a 2-ethylphenyl group, a 3-ethylphenyl group, a 4-ethylphenyl group, a 2,3-dimethylphenyl group, a 2,4-dimethylphenyl group, an o-isopropylphenyl group, an m-isopropylphenyl group, a p-isopropylphenyl group, and a 4-butylphenyl group.

[0018] Of these, R 11 is preferably hydrogen or an alkyl group having 1 to 10 carbon atoms, more preferably hydrogen or a linear alkyl group having 1 to 7 carbon atoms, further preferably hydrogen or an alkyl group having 1 to 2 carbon atoms (methyl group or ethyl group), and particularly preferably hydrogen or a methyl group.

[0019] R 12 In the above, examples of the alkylene group having 1 to 10 carbon atoms include linear alkylene groups such as methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, nonylene, and decylene; and branched alkylene groups such as methylmethylene, dimethylmethylene, methylethylene, dimethylethylene, methylpropylene, and dimethylpropylene. Of these, linear alkylene groups are preferred. The number of carbon atoms in the alkyl group is preferably 1 to 7, more preferably 1 to 5, even more preferably 2 to 4, and even more preferably 3.

[0020] R 12 The aromatic hydrocarbon group having 6 to 10 carbon atoms in the formula (I) is preferably an aromatic hydrocarbon group having 6 to 8 carbon atoms. Specific examples thereof include a phenylene group, a methylphenylene group, a dimethylphenylene group, and an ethylphenylene group, with the phenylene group being particularly preferred.

[0021] Specific examples of the group represented by the above formula (1) include vinyl groups; (meth)acryloyloxy groups; (meth)acrylic acid alkyl groups such as methyl (meth)acrylate groups, ethyl (meth)acrylate groups, propyl (meth)acrylate groups, n-butyl (meth)acrylate groups, isobutyl (meth)acrylate groups, t-butyl (meth)acrylate groups, n-pentyl (meth)acrylate groups, isopentyl (meth)acrylate groups, t-pentyl (meth)acrylate groups, n-hexyl (meth)acrylate groups, and n-heptyl (meth)acrylate groups; styryl groups, and the like. 1-7 More preferably, it is an alkyl group, and more preferably, it is a vinyl group or a (meth)acrylic acid C 1-5 An alkyl group is more preferred, and a vinyl group or a (meth)acrylic acid C 2-4 An alkyl group is more preferred, and a vinyl group or a propyl (meth)acrylate group is particularly preferred.

[0022] Among the organic groups bonded to each of the silicon atoms constituting the cyclic skeleton, examples of the alkyl group having 1 to 10 carbon atoms include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl groups; and branched alkyl groups such as isopropyl, isobutyl, isopentyl, neopentyl, and 2-ethylhexyl groups. Of these, linear alkyl groups are preferred, and the number of carbon atoms in the linear alkyl group is preferably 1 to 7, more preferably 1 to 4, even more preferably 1 or 2, and even more preferably 1.

[0023] Among the organic groups bonded to each of the silicon atoms constituting the cyclic skeleton, examples of the aryl group having 6 to 10 carbon atoms include a phenyl group, an o-tolyl group, a m-tolyl group, a p-tolyl group, a 2-ethylphenyl group, a 3-ethylphenyl group, a 4-ethylphenyl group, a 2,3-dimethylphenyl group, a 2,4-dimethylphenyl group, an o-isopropylphenyl group, a m-isopropylphenyl group, a p-isopropylphenyl group, and a 4-butylphenyl group.

[0024] It is preferable that at least one silicon atom constituting the cyclic skeleton has a polymerizable unsaturated group and an alkyl group having 1 to 10 carbon atoms bonded thereto as the organic group, and all silicon atoms constituting the cyclic skeleton have a polymerizable unsaturated group (vinyl group or (meth)acrylic acid C) bonded thereto as the organic group. 1-5 Alkyl groups are preferred, vinyl groups or (meth)acrylic acid C 2-4 It is more preferable that the alkyl group having 1 to 2 carbon atoms is bonded to the aryl group (an alkyl group is preferable).

[0025] The silicon ratio in the cyclic siloxane compound is preferably 10% by mass or more, more preferably 12% by mass or more, and even more preferably 14% by mass or more, with the upper limit being, for example, 40% by mass or less, more preferably 30% by mass or less.

[0026] The weight average molecular weight of the cyclic siloxane compound is, for example, 300-1,000, preferably 350-800, and more preferably 400-700.

[0027] Examples of a method for producing such a cyclic siloxane compound include a method including a step of hydrolyzing and condensing a silane monomer in a solvent containing water to prepare a dispersion liquid containing the cyclic siloxane compound (hereinafter, step S1), and a step of removing water from the dispersion liquid (hereinafter, step S2).

[0028] The silane monomer may be one or a combination of two or more compounds in which two organic groups, selected from a polymerizable unsaturated group, an alkyl group having 1 to 10 carbon atoms, and an aryl group having 6 to 10 carbon atoms, and two hydrolyzable groups are bonded to a silicon atom. It is preferable that at least one of the silane monomers has at least one of the two organic groups bonded to the silicon atom being a polymerizable unsaturated group.

[0029] The organic group in the silane monomer has the same meaning as the organic group in the cyclic siloxane compound described above, and all of the details, including the preferred ranges, can be referred to.

[0030] The two organic groups bonded to silicon in one molecule of the silane monomer may be the same or different. At least one of the silane monomers has an organic group bonded to silicon, one of which is a polymerizable unsaturated group (vinyl group or (meth)acryloyl C). 1-5 Alkyl groups are preferred, vinyl groups or (meth)acrylic acid C 2-4 It is preferable that one of the organic groups bonded to silicon is a polymerizable unsaturated group (vinyl group or (meth)acryloyl group, more preferably an alkyl group) and the other is an alkyl group having 1 to 10 carbon atoms (particularly an alkyl group having 1 to 2 carbon atoms). In all of the silane monomers used, one of the organic groups bonded to silicon is a polymerizable unsaturated group (vinyl group or (meth)acryloyl group, more preferably an alkyl group) and the other is an alkyl group having 1 to 10 carbon atoms (particularly an alkyl group having 1 to 2 carbon atoms). 1-5 Alkyl groups are preferred, vinyl groups or (meth)acrylic acid C 2-4 It is more preferable that the other is an alkyl group having 1 to 2 carbon atoms.

[0031] The two hydrolyzable groups bonded to the silicon atom of the silane monomer may be the same or different, and may be -OR a1 (R a1 represents an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an acyl group having 2 to 10 carbon atoms), a halogen atom, a cyano group, an isocyanate group, etc., -OR a1 More preferred is a group represented by R a1 is an alkyl group having 1 to 4 carbon atoms, -OR a1 It is more preferable that:

[0032] The hydrolysis and condensation of the silane monomer in step S1 is carried out in a solvent containing water, and the solvent may contain an organic solvent in addition to water. Examples of the organic solvent include alcohols such as methanol and ethanol; ketones such as acetone and methyl ethyl ketone; esters such as ethyl acetate; (cyclo)paraffins such as isooctane and cyclohexane; ethers such as dioxane and diethyl ether; and aromatic hydrocarbons such as benzene and toluene. These may be used alone or in combination of two or more. Among the organic solvents, alcohols are more preferred, and methanol or ethanol is even more preferred. The amount of the organic solvent is preferably 0 to 50 parts by mass, more preferably 5 to 40 parts by mass, and even more preferably 10 to 30 parts by mass, relative to 100 parts by mass of the total amount of the organic solvent and water.

[0033] The amount of the silane monomer charged per 100 parts by mass of water is preferably 3 to 30 parts by mass, and more preferably 5 to 20 parts by mass.

[0034] The hydrolysis and condensation of the silane monomer is preferably carried out in the presence of a catalyst, which may be an acid catalyst or a basic catalyst, and is preferably carried out in the presence of a basic catalyst.

[0035] Examples of the basic catalyst include ammonia, amines, quaternary ammonium compounds, alkali metal hydroxides, alkaline earth metal hydroxides, etc. The basic catalyst is preferably ammonia, and examples thereof include ammonia; ammonia generators such as urea; and the like, with ammonia being particularly preferred.

[0036] The amount of the catalyst (when a plurality of types are used, the total amount) is preferably 0.005 to 0.2 parts by mass, and more preferably 0.01 to 0.1 parts by mass, based on 100 parts by mass of the silane-based monomer.

[0037] The hydrolysis and condensation of the silane monomer can be carried out, for example, by mixing the silane monomer with a solvent containing water, further mixing a catalyst as necessary, and stirring for preferably 10 minutes to 100 hours, more preferably 30 minutes to 50 hours, even more preferably 1 to 10 hours, and even more preferably 1 to 2 hours. The temperature during the stirring is preferably 0 to 100° C., more preferably 10 to 70° C., and even more preferably 20 to 50° C. The order of addition of water, a solvent other than water that is used as necessary, the silane monomer, and the catalyst that is used as necessary is not particularly limited, but it is preferable to mix the water and the catalyst first, and then add the silane monomer (particularly dropwise) and the solvent other than water thereto.

[0038] After obtaining a dispersion liquid containing the cyclic siloxane compound by hydrolysis and condensation of the silane monomer in the step S1, a step S2 of removing water from the dispersion liquid is performed. The dispersion liquid is separated into an oil phase and an aqueous phase by leaving it to stand for a predetermined time or centrifuging it, and the aqueous phase is removed, and oily cyclic siloxane compound particles can be obtained by removing the aqueous phase.

[0039] 2.Hollow particles The hollow particles of the present invention are hollow resin particles obtained by polymerizing the above-mentioned cyclic siloxane compound by the method described below, that is, they have a structure derived from the above-mentioned cyclic siloxane compound.

[0040] The cyclic siloxane compound contains both silicon and the organic group, and the hollow particles obtained by polymerizing the compound by the method described below are particles in which an organic component and an inorganic component (silicon) are combined, and the hollow particles of the present invention can increase the silicon ratio. As shown in the examples described below, the silicon ratio in the hollow particles can be determined by calculating the mass equivalent to silicon atoms when fired in an oxidizing atmosphere and dividing it by the mass of the hollow particles. In the hollow particles of the present invention, the silicon ratio can be 10% by mass or more, preferably 11% by mass or more, and more preferably 12% by mass or more, and the upper limit is, for example, 40% by mass or less, preferably 35% by mass or less, and more preferably 30% by mass or less.

[0041] The hollow particles of the present invention contain a silicon component together with an organic component, and therefore have good heat resistance, and specifically, the thermal decomposition starting temperature can be increased. The thermal decomposition starting temperature is, for example, 200°C or higher, more preferably 220°C or higher, and the upper limit is not particularly limited, but may be, for example, 300°C or lower. The thermal decomposition starting temperature can be measured by the method shown in the examples described later, and the temperature at which the weight loss rate per unit time (ΔTg / min) exceeds 0.2% / min when the hollow particles of the present invention are heated from room temperature is taken as the thermal decomposition starting temperature.

[0042] The hollow ratio of the hollow particles can be freely controlled, particularly by employing the manufacturing method described below, and can be adjusted within a wide range, for example, from 10% to 60%. The hollow ratio may be 15% or more, 20% or more, or 50% or less, or 40% or less.

[0043] The hollow particles are also preferably such that the cyclic siloxane compound has two or more polymerizable unsaturated groups in one molecule, and in this case, the hollow particles have a crosslinked structure derived from the cyclic siloxane compound having two or more polymerizable unsaturated groups in one molecule, and therefore have excellent heat resistance and solvent resistance. Such a crosslinked structure can be, for example, 13 This can be confirmed by C-NMR, etc.

[0044] The average particle diameter of the hollow particles is, for example, 0.1 to 100 μm. The average particle diameter is preferably 0.2 μm or more, more preferably 5 μm or more, and is preferably 90 μm or less, more preferably 70 μm or less, and even more preferably 50 μm or less. The average particle diameter can be measured as shown in the examples described later, and means a diameter equivalent to 50% of the cumulative volume of the major axis of the particles measured by SEM observation.

[0045] The hollow particles of the present invention can be produced by a method including a step of mixing the cyclic siloxane compound with a hydrocarbon solvent to obtain a hydrocarbon solvent-cyclic siloxane compound mixture (hereinafter, mixture M) (hereinafter, step S3), and a step of stirring the mixture M in a solvent containing water to radically polymerize the cyclic siloxane compound (hereinafter, step S4). According to such a production method, the hollow ratio of the hollow particles can be widely controlled. The cyclic siloxane compound used in producing the hollow particles of the present invention may be produced by the hydrolysis and condensation of the above-mentioned silane monomer, or may be produced by other methods.

[0046] In step S3 to obtain mixture M, a cyclic siloxane compound is mixed with a hydrocarbon solvent, so that in mixture M, the cyclic siloxane compound is mixed uniformly with the hydrocarbon solvent. In the next step S4, such mixture M is stirred in a solvent containing water to allow radical polymerization to proceed. Due to the difference in polarity, the resin component polymerized from the cyclic siloxane compound and the hydrocarbon solvent are phase-separated in one step of step S4, while at the same time the resin component gathers on the more polar solvent side (outside) containing water, forming a shell, and resin particles encapsulating the hydrocarbon solvent, i.e., hollow resin particles, can be formed.

[0047] The hydrocarbon solvent may be an aliphatic hydrocarbon solvent or an aromatic hydrocarbon solvent, and may be used alone or in combination of two or more. In particular, it is preferable to use one or more aliphatic hydrocarbon solvents in combination with one or more aromatic hydrocarbon solvents, or to use only one or more aliphatic hydrocarbon solvents (without aromatic hydrocarbon solvents). The aliphatic hydrocarbon solvent is preferably a linear saturated hydrocarbon solvent, more preferably a linear saturated hydrocarbon solvent having 5 to 20 carbon atoms, and particularly preferably octane or hexadecane. Examples of aromatic hydrocarbon solvents include benzene, toluene, xylene, trimethylbenzene, etc., and toluene is preferable.

[0048] The ratio of the hydrocarbon solvent to 100 parts by mass of the cyclic siloxane compound is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, more preferably 30 parts by mass or more, and is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and even more preferably 120 parts by mass or less. By adjusting the ratio of the hydrocarbon solvent to 100 parts by mass of the cyclic siloxane compound, the hollow ratio of the obtained hollow particles can be controlled.

[0049] In step S4, the mixture M is stirred in a solvent containing water to radically polymerize the cyclic siloxane compound. More specifically, the mixture M, water, and a radical polymerization initiator may be mixed and stirred. The radical polymerization method is not particularly limited, but suspension polymerization is preferable. The radical polymerization initiator may be mixed when preparing the mixture M, may be mixed in the solvent containing water in step S4, or may be mixed during the emulsification step described below, but is preferably mixed in the mixture M. The radical polymerization initiator is preferably a thermal polymerization initiator, and examples of the radical polymerization initiator include a peroxide-based polymerization initiator and an azo compound-based polymerization initiator. Examples of the peroxide-based polymerization initiator include benzoyl peroxide, lauroyl peroxide, octanoyl peroxide, orthochlorobenzoyl peroxide, orthomethoxybenzoyl peroxide, methyl ethyl ketone peroxide, diisopropyl peroxydicarbonate, cumene hydroperoxide, cyclohexanone peroxide, t-butyl hydroperoxide, and diisopropylbenzene hydroperoxide. Examples of the azo compound polymerization initiator include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,3-dimethylbutyronitrile), 2,2'-azobis-(2-methylbutyronitrile), 2,2'-azobis(2,3,3-trimethylbutyronitrile), 2,2'-azobis(2-isopropylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-4-methoxy-2,4-dimethylvaleronitrile, 2-(carbamoylazo)isobutyronitrile, 4,4'-azobis(4-cyanovaleric acid), and dimethyl-2,2'-azobisisobutyrate. These may be used alone or in combination of two or more. Among these, peroxide polymerization initiators are preferred. The amount of the polymerization initiator to be charged is not particularly limited, but is preferably 0.1 to 6 parts by mass, and more preferably 1 to 5 parts by mass, per 100 parts by mass of the cyclic siloxane compound to be charged.

[0050] In step S4, the temperature for radically polymerizing the cyclic siloxane compound can be appropriately selected depending on the radical polymerization initiator used, but is preferably 30 to 100° C., more preferably 50 to 80° C., in terms of ease of reaction control. The reaction time of the radical polymerization is preferably 0.5 to 40 hours, more preferably 1 to 30 hours. It is also preferable that the radical polymerization is carried out in an inert gas atmosphere such as nitrogen.

[0051] It is also preferable to further carry out a step of emulsifying the mixture M before the step S4 of radically polymerizing the cyclic siloxane compound. Specifically, the mixture M may be mixed with a solvent containing water and a dispersion stabilizer, and stirred. The emulsification step is preferably carried out at about 20 to 40° C. for about 3 to 60 minutes. Examples of the dispersion stabilizer include water-soluble polymeric dispersants such as polyvinyl alcohol, polyvinylpyrrolidone, cellulose, gelatin, sodium polyacrylate, and sodium polymethacrylate, anionic surfactants such as alkali metal alkyl sulfate, ammonium alkyl sulfate, sodium dodecyl polyglycol ether sulfate, sodium sulfolicinoate, alkyl sulfonate, fatty acid salt, alkylaryl sulfonate, high alkyl naphthalene sulfonate, naphthalene sulfonate formalin condensate, dialkyl sulfosuccinate, polyoxyethylene alkyl sulfate salt, and polyoxyethylene alkylaryl sulfate salt, and nonionic surfactants such as polyoxyethylene alkyl ether, polyoxyethylene alkylphenyl ether, polyoxyethylene fatty acid ester, sorbitan fatty acid ester, polyoxysorbitan fatty acid ester, polyoxyethylene alkylamine, glycerin fatty acid ester, and oxyethylene-oxypropylene block polymer. These may be used alone or in combination of two or more. The amount of the dispersion stabilizer used is preferably 0.1 to 10 parts by mass per 100 parts by mass of the charged amount of the cyclic siloxane compound.

[0052] The hollow particles formed in step S4 may be isolated from the emulsion using a conventional method such as filtration, centrifugation, vacuum concentration, etc. The hollow particles are then classified as necessary, and usually washed and dried. The washing may be performed using ion-exchanged water or an alcohol such as methanol.

[0053] 3. Manufacturing method of silica particles The hollow particles are produced by the above-mentioned method for producing hollow particles, and the hollow particles are then calcined to obtain silica particles. The calcination conditions are generally adjusted appropriately based on the temperature and time at which the resin is incinerated.

[0054] The hollow particles of the present invention contain silicon and can provide hollow particles having excellent strength and heat resistance. The hollow particles and a resin composition containing the hollow particles can be used for heat insulating materials, low reflectance materials, low refractive index materials, low dielectric materials, etc. EXAMPLES

[0055] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and can of course be modified within the scope of the above and below-mentioned aims, and all such modifications are within the technical scope of the present invention.

[0056] The following Production Examples, Examples and Comparative Examples were evaluated by the methods shown below.

[0057] (1) Measurement of polymer weight average molecular weight (Mw) using gel permeation chromatography (GPC) Equipment: Tosoh Corporation HLC-8420GPC EcoSEC Elite-WS Detector: RI Column: Tosoh Corporation TSKgel GMHHR-H Column temperature: 40℃ Flow rate: 1.0mL / min Calibration curve: Tosoh Corporation TSKstandard POLYSTYRENE (peak top molecular weight (Mp) 5,480,000, 2,890,000, 190,000, 37,900, 5,970, 1,110) Eluent: tetrahydrofuran (THF) Method for preparing a measurement sample solution: 0.1 g of sample was dissolved in 1.2 g of THF.

[0058] (2) Check the hollow shape The shapes of the resin particles and silica particles can be confirmed by cutting the particles using ion milling (IB-19530CP, manufactured by JEOL Ltd., accelerating voltage: 6 kV, processing time: 5 hours) and then observing the particle shape with a SEM (JSM-6510, manufactured by JEOL Ltd., accelerating voltage: 20 kV, magnification: ×30,000, coating: platinum sputtering).

[0059] (3) Measurement of average particle size and hollowness The average particle size and hollowness of the resin particles can be determined by SEM (JSM-7600F manufactured by JEOL Ltd., transmission measurement, acceleration voltage 20 kV). A particle dispersion liquid dispersed in water or a solvent was collected and observed at a measurement magnification where the number of particles contained in one field of view was 100 to 300. In the obtained electron microscope images of five fields of view, the major axis (length in the major axis direction) of each particle was measured for any 100 particles of particle diameter (primary particle diameter) contained therein, and the outer diameter OD calculated as the arithmetic average value on a volume basis was taken as the average particle diameter. The diameter of the hollow part was taken as the inner diameter ID, and the arithmetic average value was calculated in the same manner as the outer diameter OD. The hollow ratio was calculated based on the following formula using the outer diameter OD and the inner diameter ID described above. Hollowness ratio (%) = (inner diameter ID) 3 / (Outer diameter OD) 3 ×100

[0060] (4) Measurement of silicon ratio in resin particles The silicon ratio of the resin particles was calculated by calculating the mass equivalent to silicon atoms from the ash mass (this is the SiO2 mass) when the particles were fired at 900°C in an oxidizing atmosphere such as air, and dividing the silicon atom mass by the mass of the resin particles subjected to the firing treatment. Note that, in order to calculate the mass equivalent to the silicon atom mass from the ash mass, it can be obtained by multiplying the ash mass by 0.4672 (silicon atom mass / SiO2 formula mass).

[0061] (5) Thermal decomposition temperature of resin particles The thermal decomposition onset temperature of the resin particles can be measured using a thermogravimetric and differential thermal analyzer (STA7200RV, Hitachi High-Tech Science). Specifically, the measurement was performed under the conditions of a sample weight of 20 mg, a heating rate of 10°C / min (maximum temperature reached: 900°C), and in air (flow rate of 200 mL / min), and the temperature at which the time change in the weight loss rate (ΔTg / min) exceeded 0.2% / min was defined as the thermal decomposition onset temperature.

[0062] (6) Confirmation of silica formation The generation of silica particles can be confirmed by the disappearance of peaks of organic functional groups (2900 / cm, 1400 / cm: CH, 1700 / cm: C=O, 1200 / cm: CO) in an IR spectrum (JASCO FT / IR6200, KBr method).

[0063] <Preparation of cyclic siloxane compound> Manufacturing Example 1 In a glass container, 44.8 parts of ion-exchanged water (meaning parts by mass; the same applies below unless otherwise specified) and 0.094 parts of 28% by mass ammonia water were added, and a stirrer was inserted and stirred at 300 rpm. 4.6 parts of 3-methacryloxypropylmethyldimethoxysilane (hereinafter referred to as MPDS), a silane monomer, and 10.8 parts of methanol were added thereto and stirred at 30°C for 90 minutes to carry out hydrolysis and condensation reaction of 3-methacryloxypropylmethyldimethoxysilane, thereby producing an emulsion of polysiloxane particles (cyclic siloxane compound particles) having methacryloxy groups (step S1).

[0064] Next, the obtained emulsion was centrifuged to separate the oil phase and the water phase to obtain oily particles (step S2). The oily particles were measured using a mass spectrometer (JEOL JMS-T100LP AccuTOF LC-Plus (JEOL MS-5414DART ion source)) to detect a cyclic siloxane compound, which is a 3-methacryloxypropylmethyldimethoxysilane trimer (hereinafter referred to as 3MPDS). The molecular weight of the obtained oily particles was measured using gel permeation chromatography (GPC), and the weight average molecular weight was 528.

[0065] Manufacturing Example 2 Oily particles were obtained by the same manufacturing method as in Manufacturing Example 1, except that 1.7 parts of MPDS and 2.9 parts of dimethoxyvinylmethylsilane (hereinafter referred to as DMVS) were used instead of 4.6 parts of MPDS. When the oily particles were measured with a mass spectrometer in the same manner as in Manufacturing Example 1, a cyclic siloxane compound, which is a co-condensation product of one molecule of 3-methacryloxypropylmethyldimethoxysilane and two molecules of dimethoxyvinylmethylsilane (MPDS-2DMVS), was detected. When the molecular weight in the particles of the obtained cyclic siloxane compound was measured using gel permeation chromatography (GPC), the weight average molecular weight was 417.

[0066] <Preparation of resin particles> Example 1-1 In a container, 1.32 parts of 3MPDS obtained in Production Example 1 as a cyclic siloxane compound, 0.05 parts of polymerization initiator benzoyl peroxide, 0.54 parts of hexadecane, and 0.8 parts of toluene were charged, and a mixture of a hydrocarbon solvent and a cyclic siloxane compound was prepared (step S3). Separately, 20 parts of a 0.1% by mass polyvinyl alcohol (manufactured by Mitsubishi Chemical Corporation, "GOHSENOL GH-17R") aqueous solution was charged into a Schlenk flask and kept at 30°C. The mixture of the hydrocarbon solvent and the cyclic siloxane compound prepared therein was dispersed at 30°C for 15 minutes at 4000 rpm with an ultrasonic homogenizer (Nippon Seiki Biomixer), and then stirred at 300 rpm and heated to 70°C under a nitrogen atmosphere, and kept at 70°C for 24 hours to carry out a polymerization reaction of 3MPDS. The obtained emulsion was subjected to solid-liquid separation, and the obtained cake was washed with ion-exchanged water and dried to obtain hollow resin particles 1. The average particle size of the obtained particles 1 was 20.4 μm.

[0067] Example 1-2 Hollow resin particles 2 were obtained by the same production method as in Example 1-1, except that 1.32 parts of MPDS-2DMVS obtained in Production Example 2 was used instead of 3MPDS, and 0.66 parts of octane was used instead of hexadecane and toluene. The average particle size of the obtained particles 2 was 19.5 μm.

[0068] Comparative Example 1-1 A four-neck flask equipped with a cooling tube, a thermometer, and a dropping port was charged with 666.7 parts of a 10% aqueous solution of polyvinyl alcohol (Kuraray's "Poval PVA-205") and kept at 25°C. A solution of 60.0 parts of methyl methacrylate, 40.0 parts of ethylene glycol dimethacrylate, and 2.0 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) (Wako Pure Chemical Industries, Ltd.'s "V-65") was added as monomer components from the dropping port while stirring at 200 rpm, and the mixture was kept for 2 hours to prepare a suspension. The suspension was heated to 65°C under a nitrogen atmosphere while continuing to stir, to carry out radical polymerization of the monomer components. The emulsion after the radical polymerization was subjected to solid-liquid separation, and the obtained cake was washed with ion-exchanged water and dried to obtain solid resin particles 3. The average particle diameter of the obtained resin particles 3 was 29.8 μm.

[0069] Comparative Example 1-2 Solid resin particles 4 were obtained by the same production method as in Comparative Example 1-1, except that 60.0 parts of methyl methacrylate and 100 parts of 3MPDS were used instead of 40.0 parts of ethylene glycol dimethacrylate. The average particle size of the obtained resin particles 4 was 41.7 μm.

[0070] The results of the examples and comparative examples are shown in Table 1.

[0071] [Table 1]

[0072] <Preparation of silica particles> Example 2-1 Resin particles 1 were baked to obtain silica particles 5. The shape of silica particles 5 was confirmed by the above-mentioned method, and it was found to be hollow.

[0073] Example 2-2 Silica particles 6 were obtained by the same production method as in Example 2-1, except that resin particles 2 were used instead of resin particles 1. When the shape of silica particles 6 was confirmed by the above-mentioned method, it was found to be hollow.

Claims

1. A hollow particle including a structure derived from a cyclic siloxane compound, The cyclic siloxane compound has a cyclic skeleton formed of siloxane bonds, each of the silicon atoms constituting the cyclic skeleton has an organic group bonded thereto selected from a polymerizable unsaturated group, an alkyl group having 1 to 10 carbon atoms, and an aryl group having 6 to 10 carbon atoms; At least one of the silicon atoms constituting the cyclic skeleton has a polymerizable unsaturated group bonded thereto.

2. 2. The hollow particles according to claim 1, wherein the silicon ratio is 10 to 40 mass %.

3. 2. The hollow particle according to claim 1, having a hollow ratio of 10 to 60%.

4. 2. The hollow particle according to claim 1, wherein the cyclic siloxane compound has two or more polymerizable unsaturated groups in one molecule.

5. 2. The hollow particles according to claim 1, having an average particle size of 0.1 to 100 μm.

6. 6. The hollow particles according to claim 1, wherein the thermal decomposition starting temperature is 200° C. or higher.

7. It has a cyclic skeleton formed of siloxane bonds, each of the silicon atoms constituting the cyclic skeleton has an organic group bonded thereto selected from a polymerizable unsaturated group, an alkyl group having 1 to 10 carbon atoms, and an aryl group having 6 to 10 carbon atoms; A method for producing a cyclic siloxane compound having a polymerizable unsaturated group bonded to at least one silicon atom constituting the cyclic skeleton, comprising the steps of: A step of hydrolyzing and condensing a silane monomer in a solvent containing water to prepare a dispersion containing the cyclic siloxane compound; and removing water from the dispersion. A method for producing a cyclic siloxane compound.

8. A step of producing the cyclic siloxane compound by the production method according to claim 7, and obtaining a solvent-cyclic siloxane compound mixture from the obtained cyclic siloxane compound and a hydrocarbon solvent; a step of stirring the solvent-cyclic siloxane compound mixture in a solvent containing water to radically polymerize the cyclic siloxane compound.

9. obtaining a solvent-cyclic siloxane compound mixture from a cyclic siloxane compound and a hydrocarbon solvent; a step of stirring the solvent-cyclic siloxane compound mixture in a solvent containing water to radically polymerize the cyclic siloxane compound, The cyclic siloxane compound has a cyclic skeleton formed of siloxane bonds, each of the silicon atoms constituting the cyclic skeleton has an organic group bonded thereto selected from a polymerizable unsaturated group, an alkyl group having 1 to 10 carbon atoms, and an aryl group having 6 to 10 carbon atoms; At least one of the silicon atoms constituting the cyclic skeleton has a polymerizable unsaturated group bonded thereto.

10. 10. The method for producing hollow particles according to claim 8, further comprising the step of emulsifying the solvent-cyclic siloxane compound mixture prior to the step of radical polymerization.

11. 10. The method for producing hollow particles according to claim 8, wherein the amount of the hydrocarbon solvent is 10 to 200 parts by mass based on 100 parts by mass of the cyclic siloxane compound.

12. The method for producing hollow particles according to claim 8 or 9, wherein the cyclic siloxane compound has a silicon content of 10 to 40 mass %.

13. Producing hollow particles by the production method according to claim 8 or 9, A method for producing silica particles, comprising calcining the hollow particles.

14. A method for producing hollow particles according to claim 10, A method for producing silica particles, comprising calcining the hollow particles.

Citation Information

Patent Citations

  • Silica-based microparticle, method for producing dispersion with the same, and base material with coating film

    JP2001233611A

  • Organic-inorganic hybrid hollow particle and use therefor

    JP2017061664A

  • Resin particle, and method for producing the same

    JP2021176937A

  • Hollow particles, heat insulating coating material and heat insulating coating film

    JP2022118409A

  • Hollow-particle dispersion

    WO2019177013A1