Biocomposites based on biodegradable polymers
Patent Information
- Application Number
- JP2024524476
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-19
- Filing Date
- 2022-10-19
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2042-10-19
Smart Images

Figure 2024539261000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of biodegradable polymeric materials. In particular, the present invention relates to a biocomposite comprising a poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) base and a method for producing the same. [Background technology]
[0002] Plastics have played an important role in the development of human society in the last century. Traditional polymers such as polyolefins are mainly used in disposable applications and accumulate in the environment after disposal [Non-Patent Document 1]. The long-term existence of these polymers has polluted our land, water and air, causing environmental and public health crises, indicating that such polymers are not suitable for applications where plastics are used for a short period of time and then discarded [Non-Patent Documents 2, 3]. Recycling is a reasonable option, but the contamination of plastic packaging and the deterioration of its properties during melt processing make mechanical recycling costly and unfeasible [Non-Patent Document 4].
[0003] Plant and microbial derived (i.e., bio-based) polymers are susceptible to microbial enzymatic action and hydrolysis and are therefore biodegradable [5]. The growing demand for renewable polymers has forced governments and legislative bodies around the world to develop laws / policies to ban single-use conventional plastics and promote alternative renewable plastics [6].
[0004] Poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) is a biobased, biodegradable thermoplastic derived directly from microorganisms that has shown promising properties to replace single-use plastics for a wide range of applications. In addition to its biodegradability, PHBV has mechanical properties comparable to a wide range of commodity plastics, making it attractive for food packaging and consumer goods applications. However, PHBV is significantly more expensive than conventional plastics, and its brittleness prevents its widespread use.
[0005] The use of natural fillers such as hemp fiber, cellulose nanocrystals, hydroxyapatite, wheat straw fiber, wood and wood flour, coffee grounds, agave fiber, lignin, miscanthus fiber, chitin, soybean hulls, distiller's dried grains and other agricultural residues to form polymer-based composites has been explored by many studies.
[0006] It is well known that the incorporation of natural fillers into renewable polymers can restrict polymer chain mobility, increase melt viscosity, and limit the melt processing of biocomposites.
[0007] Thus, there is a need for cost-competitive biodegradable materials with desirable mechanical and / or thermomechanical properties and processability that can be prepared from biodegradable polymers and sustainable, low-cost, biodegradable fillers to replace traditional plastics.
[0008] This background information is provided for the purpose of making known information believed by the applicant to be of possible relevance to the present invention. It is not necessarily intended, nor should it be construed, that any of the preceding information constitutes prior art against the present invention. [Prior art documents] [Non-patent literature]
[0009] [Non-Patent Document 1] A. Chamas, H. Moon, J. Zheng, Y. Qiu, T. Tabassum, JH Jang, M. Abu-Omar, SLScott, S. Suh, Degradation Rates of Plastics in the Environment, ACS Sustainable Chemistry & Engineering 8(9)(2020)3494-3511. [Non-Patent Document 2] AESchwarz, TNLigthart, E. Boukris, T. van Harmelen, Sources, transport, and accumulation of different types of plastic litter in aquatic environments: A review study, Marine Pollution Bulletin 143 (2019) 92-100. [Non-Patent Document 3] K. Pabortsava, RSLampitt, High concentrations of plastic hidden beneath the surface of the Atlantic Ocean, Nature Communications 11(1)(2020)4073. [Non-Patent Document 4] JNHahladakis, E. Iacovidou, An overview of the challenges and trade-offs in closing the loop of post-consumer plastic waste (PCPW): Focus on recycling, Journal of Hazardous Materials 380 (2019) 120887. [Non-Patent Document 5] KWMeereboer, M. Misra, AK Mohanty, Review of recent advances in the biodegradability of polyhydroxyalkanoate(PHA) bioplastics and their composites, Green Chemistry 22(17)(2020)5519-5558. [Non-Patent Document 6] K. Ghosh, BHJones, Roadmap to Biodegradable Plastics-Current State and Research Needs, ACS Sustainable Chemistry & Engineering 9(18)(2021)6170-6187. [Non-Patent Document 7] J.Topping, Investigations on the Theory of the Brownian Movement, Physics Bulletin 7(10)(1956)281-281. [Non-Patent Document 8] D.Romanzini,A.Lavoratti,HLOrnaghi,SCAmico,AJZattera,Influence of fiber content on the mechanical and dynamic mechanical properties of glass / ramie polymer composites,Materials & Design 47(2013)9-15. Summary of the Invention
[0010] The object of the present invention is to provide a biodegradable biocomposite based on poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV).
[0011] According to an aspect of the present invention, there is provided a composition for use in the manufacture of a biodegradable composite material, the composition comprising: a) about 30 to about 99.5 wt. % of a polymer component comprising poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) or a mixture of PHBV-polybutylene adipate terephthalate (PBAT); b) about 0.5 to about 60 wt. % of hemp residue; and c) optionally about 0.1 to 50 wt. % of maleic anhydride, glycidyl methacrylate, pyromellitic anhydride, acrylic acid, polyacrylic acid ... and / or one or more compatibilizers selected from maleic anhydride, glycidyl methacrylate, pyromellitic anhydride, acrylic acid, polyacrylic acid, methylene diphenyl diisocyanate, poly(glycidyl methacrylate), copolymers of glycidyl methacrylate, and copolymers of acrylic acid.
[0012] According to an aspect of the present invention, there is provided a biocomposite material comprising a blend, the blend comprising: a) about 30 to about 99.5 wt% of a polymer component comprising poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) or a mixture of PHBV-polybutylene adipate terephthalate (PBAT); b) about 0.5 to about 60 wt% of hemp residue; and c) optionally about 0.1 to 50 wt% of maleic anhydride, glycidyl methacrylate, pyromellitic anhydride, acrylic acid, polyacrylic acid, methylene diamine ester, glycidyl methacrylate, pyromellitic anhydride, acrylic acid, polyacrylic acid, methylene diamine ester, glycidyl methacrylate, pyromellitic anhydride, glycidyl methacrylate ... PBAT grafted with one or more compatibilizers selected from diphenyl diisocyanate, poly(glycidyl methacrylate), copolymers of glycidyl methacrylate, and copolymers of acrylic acid, and / or blends with one or more compatibilizers selected from maleic anhydride, glycidyl methacrylate, pyromellitic anhydride, acrylic acid, polyacrylic acid, methylene diphenyl diisocyanate, poly(glycidyl methacrylate), copolymers of glycidyl methacrylate, and copolymers of acrylic acid.
[0013] According to an aspect of the present invention, there is provided a method of preparing a biocomposite material as described herein, comprising the steps of a) blending a polymer component with hemp residue and optionally a compatibilizer and / or PBAT grafted with a compatibilizer, and b) heating the blend at a temperature sufficient to melt at least the PHBV and / or the PBAT.
[0014] Further features and advantages of the present disclosure will become apparent from the following detailed description taken in conjunction with the accompanying drawings. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 illustrates tensile test and tensile modulus results for an exemplary biocomposite according to an embodiment of the present invention. [Diagram 2] FIG. 2 illustrates the elongation at break and tensile resistance of an exemplary biocomposite according to an embodiment of the present invention. [Diagram 3] 3A and 3B show storage modulus and tan δ, respectively, of an exemplary PHBV-hemp residue biocomposite versus temperature, according to an embodiment of the present invention. [Figure 4] 4A and 4B show storage modulus and tan δ, respectively, of an exemplary PHBV-PBAT-hemp residue biocomposite versus temperature, according to an embodiment of the present invention. [Diagram 5] 5A and 5B show storage modulus and tan δ, respectively, of an exemplary PHBV-PBAT-mPBAT-hemp residue biocomposite versus temperature, according to an embodiment of the present invention. [Figure 6] FIG. 6 illustrates the heat deflection temperature of exemplary PHBV-hemp residue biocomposites and PHBV-PBAT-hemp residue biocomposites with and without mPBAT according to an embodiment of the present invention. [Figure 7]Figures 7A-C show the rheological properties of PHBV-hemp residue biocomposites according to embodiments of the present invention, where Figure 7A shows the storage modulus, Figure 7B shows the loss modulus, and Figure 7C shows the complex viscosity. [Figure 8] Figures 8A-C show the rheological properties of PHBV-PBAT-hemp residue biocomposites according to embodiments of the present invention. Figure 8A shows the storage modulus, Figure 8B shows the loss modulus, and Figure 8C shows the complex viscosity. [Figure 9] Figures 9A-C show the rheological properties of PHBV-PBAT-hemp residue biocomposites with mPBAT according to embodiments of the present invention. Figure 9A shows the storage modulus, Figure 9B shows the loss modulus, and Figure 9C shows the complex viscosity. [Figure 10A] FIG. 10A illustrates the PHBV and water uptake of an exemplary biocomposite according to an embodiment of the present invention versus time in days. [Figure 10B] FIG. 10B illustrates the PHBV and water uptake of an exemplary biocomposite according to an embodiment of the present invention versus time in days. [Figure 10C] FIG. 10C illustrates the PHBV and water uptake of an exemplary biocomposite according to an embodiment of the present invention versus time in days. [Figure 10D] FIG. 10D illustrates the PHBV and water uptake of an exemplary biocomposite according to an embodiment of the present invention versus time in days. [Figure 11] 11A-D show morphological analysis of an exemplary PBAT-hemp residue biocomposite according to an embodiment of the present invention. [Figure 12] 12A-D show morphological analysis of an exemplary PHBV-PBAT-hemp residue biocomposite according to an embodiment of the present invention. [Figure 13] 13A-C show morphological analysis of an exemplary PHBV-PBAT-hemp residue biocomposite with mPBAT according to an embodiment of the present invention. [Figure 14]14A-C show morphological analysis of exemplary biocomposites of (A) PHBV, (B) (80:20-PHBV:PBAT) and (C) (80:20)-M with 30 wt% hemp residue according to embodiments of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0017] The articles "a" and "an" are used herein to refer to one or to more than one (i.e., to at least one) of the grammatical object of the article. By way of example, "an element" means one element or more than one element.
[0018] As used herein, the term "about" refers to a ±10% variation from the nominal value, and it should be understood that such a variation is always included in any given value provided herein, whether or not it is specifically referred to.
[0019] As used herein, the term "hemp residue" (HP) refers to crushed hemp stalk, hemp hurd and / or fiber that have been ground and / or sliced into micron-sized particles. The residue may be in the form of a powder or dust.
[0020] As used herein, the term "biodegradable" refers to materials that deteriorate or break down when exposed to sunlight or ultraviolet light, water or moisture, microorganisms such as bacteria and fungi, enzymes, or wind erosion.
[0021] As used herein, the term "bio-based" refers to materials made from substances derived from living (or former) organisms.
[0022] The present invention relates to novel compositions for producing poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) based biodegradable biocomposites and biodegradable biocomposite materials formed from these compositions.
[0023] The biocomposite material of the present invention can exhibit improved tensile modulus and similar tensile strength and heat deflection compared to the original PHBV, making it a promising candidate for consumer goods, rigid packaging applications and additive manufacturing.
[0024] In one aspect, the present invention provides a composition for use in the manufacture of a biodegradable biocomposite material, the composition comprising: a) about 30 to about 99.5% by weight of a polymer component comprising poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) or a mixture of PHBV and polybutylene adipate terephthalate (PBAT); b) about 0.5 to about 60% by weight of hemp residue; and c) optionally about 0.1 to 50% by weight of maleic anhydride, glycidyl methacrylate, pyromellitic anhydride, acrylic acid, polyacrylic acid, methylene diphenyl diisocyanate, PBAT grafted with one or more compatibilizers selected from poly(glycidyl methacrylate), copolymers of glycidyl methacrylate, and copolymers of acrylic acid, and / or one or more compatibilizers selected from maleic anhydride, glycidyl methacrylate, pyromellitic anhydride, acrylic acid, polyacrylic acid, methylene diphenyl diisocyanate, poly(glycidyl methacrylate), copolymers of glycidyl methacrylate, and copolymers of acrylic acid.
[0025] In another aspect, the present invention provides a biodegradable biocomposite material comprising a blend, the blend comprising about 30 to about 99.5% by weight of a polymer component comprising poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) or a mixture of PHBV and polybutylene adipate terephthalate (PBAT), about 0.5 to about 60% by weight of hemp residue, and optionally about 0.1 to 50% by weight of maleic anhydride, glycidyl methacrylate, pyromellitic anhydride, acrylic acid, polyacrylic acid, methyl methacrylate ... and / or blends of PBAT grafted with one or more compatibilizers selected from maleic anhydride, glycidyl methacrylate, pyromellitic anhydride, acrylic acid, polyacrylic acid, methylene diphenyl diisocyanate, poly(glycidyl methacrylate), copolymers of glycidyl methacrylate, and copolymers of acrylic acid.
[0026] In some embodiments, the polymer component is poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV).
[0027] In some embodiments, the polymer component is a mixture of PHBV and polybutylene adipate terephthalate (PBAT).
[0028] In some embodiments, the PHBV-PBAT mixture comprises about 10% to about 90% by weight PHBV and about 90% to about 10% by weight PBAT, based on the total weight of the blend.
[0029] In some embodiments, the PHBV-PBAT mixture comprises about 50 to about 90 wt % PHBV and about 50 to about 10 wt % PBAT, based on the total weight of the blend.
[0030] In some embodiments, the PHBV-PBAT mixture comprises about 70 to about 90 wt % PHBV and about 30 to about 10 wt % PBAT, based on the total weight of the blend.
[0031] In some embodiments, the composition or composite comprises about 40-90% of the PHBV component and about 10-60% of the HP.
[0032] In some embodiments, the compositions and / or biocomposite materials of the present invention comprise one or more compatibilizers selected from maleic anhydride, pyromellitic anhydride, acrylic acid, polyacrylic acid, methylene diphenyl diisocyanate, and copolymers of acrylic acid.
[0033] In some embodiments, the compositions and / or biocomposite materials of the present invention comprise one or more compatibilizers selected from maleic anhydride, glycidyl methacrylate, pyromellitic anhydride, and methylene diphenyl diisocyanate.
[0034] In some embodiments, the compositions and / or biocomposite materials of the present invention comprise PBAT grafted with one or more of maleic anhydride, glycidyl methacrylate, pyromellitic anhydride, and acrylic acid.
[0035] In some embodiments, the compositions and / or biocomposite materials of the present invention comprise about 5% to 20% by weight of PBAT grafted with one or more compatibilizers.
[0036] The hemp residue of the present invention can be prepared by milling and / or crushing hemp stalks to obtain micron-sized particles. In some embodiments, the hemp residue comprises crushed hemp hurds and bast fibers. In some embodiments, the hemp residue consists primarily of hemp huds and residual bast fibers. In some embodiments, the hemp residue consists of hemp hurds. In some embodiments, the residue is in the form of a powder.
[0037] In some embodiments, prior to milling or grinding, the hemp stalk fiber is washed with about 2-10% aqueous sodium hydroxide solution (1 part by weight of stalk per 10 parts by weight of solution) and then dried.
[0038] In some embodiments, the hemp residue comprises particles having a length of about 75-150 μm and an average aspect ratio of about 3.5-5. In some embodiments, the hemp residue comprises particles having a length of about 75-150 μm and an average aspect ratio of about 3.5-5. In some embodiments, the hemp residue comprises particles having a length of about 1.0-2.0 g / cm 3 has a density of
[0039] In some embodiments, the hemp residue comprises about 60-75% by weight cellulose, 5-15% by weight hemicellulose and about 10-25% by weight lignin.
[0040] In some embodiments, the hemp residue is processed to remove tetrahydrocannabinol (THC) and cannabidiol (CBD).
[0041] In some embodiments, the compositions and / or biocomposite materials of the present invention comprise about 30 wt. % PHBV-PBAT blend, about 60 wt. % HP residue, and about 10 wt. % PBAT grafted with maleic anhydride.
[0042] In some embodiments, the composition and / or biocomposite material comprises about 1 to about 3 weight percent of a treating agent, such as glycerol monostearate and stearic acid.
[0043] In some embodiments, the composition and / or biocomposite material comprises one or more inorganic fillers (talc, clay, wollastonite, montmorillonite, or alkali or alkaline earth metal carbonates, bicarbonates, oxides, or sulfates).
[0044] In some embodiments, the composition and / or biocomposite material further comprises about 0.5 to about 5% by weight of a colorant, such as a mineral and / or a dye, hi some embodiments, the composition comprises about 1% by weight of a colorant.
[0045] In another aspect, the present invention provides a method for preparing the biodegradable biocomposite material of the present invention, comprising blending a polymer component with hemp residue and optionally one or more compatibilizers and / or PBAT grafted with a compatibilizer as described herein, and heating the blend at a temperature sufficient to melt at least the PHBV and / or PBAT.
[0046] In some embodiments, the method includes extruding the blend at an extrusion temperature sufficient to melt at least the PHBV and / or the PBAT, hi some embodiments, the blend is extruded through a screw extruder at a screw speed of about 80 to about 120 rpm and a process temperature of about 150°C to about 220°C.
[0047] In some embodiments, the polymeric components and hemp residue are dried to remove residual moisture prior to processing. Drying can be accomplished in a conventional oven at about 60 to about 100° C., or by common industrial drying methods such as a desiccant wheel dryer or Munters desiccant wheel (overnight at about 40 to 60° C.).
[0048] In some embodiments, the produced biocomposite material is air cooled and pelletized.
[0049] In some embodiments, the PBAT grafted with a compatibilizer can be prepared by combining PBAT, one or more compatibilizers, and a free radical initiator to form a reaction mixture and melt processing the reaction mixture to form the grafted PBAT.
[0050] In some embodiments, PBAT is first mixed with one or more compatibilizers and heated to a temperature sufficient to melt the at least one compatibilizer, followed by the addition of a free radical initiator prior to melt processing.
[0051] In some embodiments, melt processing is accomplished at a temperature of from about 150°C to about 220°C.
[0052] In some embodiments, melt processing comprises melt extrusion, which in some embodiments is carried out by a screw extruder at a screw speed of about 80-120 rpm and a feed rate of about 300-750 g / h.
[0053] In some embodiments, the produced biocomposite is dried to remove unreacted compatibilizer.
[0054] In some embodiments, the biocomposite material of the present invention comprises PBAT grafted with one or more compatibilizers, which are: a) first preparing the grafted PBAT by combining PBAT with one or more compatibilizers and a free radical initiator to form a reaction mixture and melt processing the reaction mixture to form the grafted PBAT; b) thereafter, mixing the grafted PBAT prepared in step a) with a polymer component, hemp residue and optional fillers and extruding the mixture at a processing temperature sufficient to melt at least the PHBV and / or the PBAT; It can be prepared by
[0055] In one aspect, the present invention provides a biocomposite material produced by the methods described herein.
[0056] In order to obtain a better understanding of the invention described herein, the following examples are described with reference to the accompanying drawings, in which: These examples are intended to describe exemplary embodiments of the invention and are not intended to limit the scope of the invention in any manner. EXAMPLES
[0057] Example 1: Preparation of Hemp Powder (HP) To produce HP, the bast fibers were removed from the stem and remaining woody core (also called hurd), and the remaining fibers were processed through a flour mill to produce a fine powder of hemp hurd and remaining fibers as micron-sized particles. The moisture content of the resulting HP was less than 1.5%.
[0058] Example 2: Preparation of MA-grafted PBAT An industrially available melt extrusion technique was employed to produce MA-grafted PBAT (mPBAT). First, PBAT pellets were mixed with 5 wt% maleic anhydride (MA) and stored in a hot air oven at 80 °C for about 30 min to melt the MA and form a thin crust coating on the PBAT pellets. The mixture was cooled and mixed with 1 wt% dicumyl peroxide (DCP) as a reaction initiator and stirred before melt processing. Reactive extrusion was carried out by a twin-screw extruder (Process11 Parallel Twin-Screw Extruder, Thermo Fisher Scientific) using a die-to-feed temperature profile of 130 / 135 / 140 / 150 / 150 / 140 / 135 / 130 °C. The screw speed was 60 rpm (length 440 mm and diameter 11 mm, i.e., L / D 40:1) and the feed rate was about 500 g / h. The resulting mPBAT was then pelletized, weighed, and dried in a vacuum oven at 100 mbar pressure for 24 hours at a temperature of 80° C. Once the sample was cleaned of unreacted MA, it was placed in an airtight container until further use.
[0059] Example 3: Preparation of biocomposite materials PHBV biocomposites with HP / mPBAT or PHBV-PBAT biocomposites were first mixed with PHBV or a mixture of PHBV and PBAT at various concentrations of HP and mPBAT (weight percent) as shown in Table 1, and then dried overnight at 80°C in a hot air oven. The mixtures were extruded in a twin-screw extruder (Process11 Parallel Twin-Screw Extruder, Thermo Fisher Scientific) at 180°C and a screw speed of 100 rpm. The blends were injection molded using a HAAKE Mini-Jet Pro (Thermo Fisher Scientific, Waltham, MA, USA) at a cylinder temperature of 180°C, a mold temperature of 60°C, and a pressure of 700 bar with a 10 s hold. The specimens were further conditioned at room temperature and 50% RH for 48 h before testing. [Table 1]
[0060] Characterization Tensile tests were performed across all samples at a crosshead speed of 5 mm / min and a gauge length of 25 mm using a Mandel-Shimadzu (AGS-X) tensile testing machine (Shimadzu Corporation, Kyoto, Japan) equipped with a load cell of 500 N. Five specimens were tested for each sample, and the averages along with the standard deviations were reported according to ASTM D638 type V.
[0061] Dynamic mechanical analysis (DMA) was performed using a dynamic mechanical analyzer (Q800 DMA, TA Instruments). Samples were heated from -80°C to 120°C at a heating ramp rate of 3°C / min. A dual cantilever clamp was used at a frequency of 1 Hz and strain of 0.2%.
[0062] A dynamic mechanical analyzer (Q800 DMA, TA Instruments) was used to estimate the heat deflection temperature (HDT) of each blend with a three-point bending modulus and a heating ramp rate of 2° C. / min. As described in the ASTM 648-07 standard, Equation 1 was used to calculate the required force for each sample in this analysis.
number
number
number
[0063] The rheology of the blends was studied using a parallel plate viscometer (HAAKE MARS III, Thermo Fisher Scientific) with sample thickness and diameter of 1.55 mm and 20 mm, respectively. A frequency sweep from 0.01 to 100 Hz was performed at 200 °C with a constant strain of 0.1% (in the linear viscoelastic region) and a plate spacing of 1 mm.
[0064] Scanning electron microscopy (SEM) was performed using an Oxford Instruments Quanta FEG250 Environmental SEM (Abingdon, UK) without sputter coating to study the fracture surface morphology of the blends. Micrographs were taken from freeze-fractured tensile specimens to investigate the interaction of HP and the polymer matrix.
[0065] Water absorption tests were conducted on 0, 10, 30 and 60% HP blends. Five specimens of each sample were first weighed and then immersed in 70 mL of distilled water in a glass container at room temperature. The weight of the specimens was recorded after 24 hours and further tested every 4 days thereafter.
[0066] The impact resistance of the prepared biocomposites was evaluated using an Izod impact tester according to ASTM D256. Tests were performed using a TMI impact tester from Testing Machines Inc. (Model 43-02) and the average of five specimens was reported along with the standard deviation.
[0067] Mechanical properties of PHBV-based biocomposite materials Figure 1 shows the ultimate tensile strength (UTS) and tensile modulus (TM) of the fabricated biocomposite materials. For PHBV, the UTS increased slightly from 33.2 MPa to 35.3 MPa for the incorporation of 20% hemp residue powder (HP), and decreased to 27 MPa for the incorporation of 60% HP. The interfacial delamination of the PHBV matrix and HP at high concentrations is believed to be the main cause of premature fracture of the specimens after unidirectional tension. Also, the localized accumulation of HP particles due to higher loading ratio creates weak areas in the biocomposite that inhibit proper load transfer, decreasing the UTS. For the PHBV-PBAT (80:20) matrix, the incorporation of 10% HP showed a slight improvement in UTS from 30.9 to 31.7 MPa, but further increase in HP loading ratio resulted in a decrease to 24.8 MPa. Since PBAT is a relatively soft material, it affects the UTS of the PHBV-PBAT (80:20) biocomposite. Moreover, its phase separation and insolubility with PHBV also contribute to the decrease in UTS. For the blend of PHBV-PBAT with 10% maleated PBAT (mPBAT), the incorporation of 50% HP further increases the UTS to 33.1 MPa. The use of 10% mPBAT acts as a compatibilizer between PBAT, PHBV and HP. The functional mPBAT reacts with HP to produce HP-grafted PBAT, while partial reaction can also occur with PHBV. The incorporation of mPBAT improved the interfacial adhesion of HP with the polymer matrix and enhanced the compatibility of PBAT with PHBV. The sufficient interfacial interaction of HP with the matrix increased the UTS, which was comparable to that of the original PHBV even after the addition of 50% HP loading.
[0068] The tensile modulus of PHBV-HP gradually increased from 1,691 MPa to 2,609 MPa with an increase in HP loading to 60%. The increase in tensile modulus demonstrated an improvement in the stiffness of the developed biocomposite, which is a measure of resistance to an applied unidirectional deformation. The addition of PBAT and mPBAT to the 60%HP system resulted in a decrease in the tensile modulus to 2,426 MPa and 2,100 MPa, respectively, in comparison to PHBV-60%HP. This is not surprising considering that PBAT is a soft and flexible polymer and its incorporation resulted in a decrease in stiffness. In comparison, the addition of 60%HP along with PHBV-PBAT and mPBAT showed a higher tensile modulus than the pristine PHBV. Meanwhile, the incorporation of mPBAT contributes to an improvement in the impact resistance of the biocomposite.
[0069] Breaking elongation and Izod impact resistance Figure 2 shows the elongation at break and Izod impact resistance of the developed biocomposites. It is known that the incorporation of reinforcement or filler dramatically reduces the elongation at break or extensibility of biocomposites. The elongation at break of pure PHBV was about 3% and decreased to about 1% after the addition of 60% HP. A similar trend is observed in the case of PHBV-PBAT biocomposites. Meanwhile, a comparable elongation at break (about 3%) to PHBV was observed with the incorporation of mPBAT by using 30% HP filler. Reactive extrusion of biocomposites with mPBAT gave sufficient tensile strength and relatively high elongation at break by using up to 30% HP. The reactive extrusion chemistry works at higher HP loadings, which was shown by the obtained impact resistance data. The impact resistance of mPBAT and PHBV-PBAT matrices with 50% HP (23.3 J / m) was comparable to that of pristine PHBV (23.2 J / m). A decrease in HP loading (20%) promoted an increase in impact resistance (25.8 J / m).
[0070] Thermomechanical properties of PHBV biocomposites The dynamic mechanical properties of the various composite formulations were evaluated using DMA. The storage modulus of the specimens at -50°C, 0°C, 25°C, and 50°C are shown in Table 2, and the corresponding curves versus temperature are shown in Figures 3A, 3B, 4A, 4B, 5A, and 5B. As evident from Table 3, the incorporation of HP enhanced the storage modulus in all the composite combinations. The storage modulus of PHBV at 25°C (4359 Mpa) was enhanced by 127.5% to 9916 Mpa with the addition of 60% HP, indicating that the materials at 25°C have improved elastic behavior after the incorporation of HP. A similar trend was observed in the case of PHBV-PBAT matrix. Increasing the temperature to 50°C did not have a significant effect on the storage modulus, which means that the materials fabricated in a wider temperature range maintained their elastic behavior.
[0071] The loss tangent (tan δ) of the biocomposites is also shown in Table 2. For PHBV, the tan δ peak showed a glass transition that increased from about 17 °C to about 28 °C with a gradual increase in HP loading to 60%. This decrease can be attributed to the decrease in the amorphous fraction in the biocomposite. The height of the tan δ peak also decreased, indicating the chain mobility restriction resulting from the rigid HP particles. In contrast, the PHBV-PBAT matrix showed two distinct tan δ peaks at about 20 °C and about 27 °C, which correspond to the glass transitions of PHBV and PBAT, respectively. The incorporation of HP and mPBAT significantly shifted the tan δ peak to higher temperatures and reduced the peak height. The incorporation of mPBAT into the highly filled (>30% HP) PHBV-PBAT matrix resulted in a significant suppression of the tan δ peak, indicating an improvement in the interfacial interaction of the HP matrix. This was also confirmed by determining the theoretical parameters used to predict the viscoelastic properties of the developed biocomposites. [Table 2]
[0072] Storage modulus of PHBV biocomposite To predict the storage modulus in the presence of HP, the effectiveness factor and reinforcement efficiency factor were adopted. Equation 4 proposed by Einstien [J. Topping, Investigations on the Theory of the Brownian Movement, Physics Bulletin 7(10)(1956)281-281.] can be used to evaluate the filler reinforcement by calculating the reinforcement efficiency factor (r).
number
[0073] The loading level of the filler and its dispersion affect the reinforcement efficiency factor (r), which is E c / E m Against V f The linear plot of r can be obtained from the linear plot of r. Higher values of r correspond to less aggregation and uniform dispersion. The calculated values of r for various biocomposites are listed in Table 3. The r values for PHBV-HP, PHBV-PBAT-HP and PHBV-PBAT-HP-M biocomposites were 1.47, 1.81 and 1.85, respectively. Higher r values were obtained for composites containing mPBAT, indicating enhanced reinforcement due to the improved dispersion effect of HP in such formulations. Furthermore, the values of r were used to theoretically calculate the storage modulus of each biocomposite, and the values of r were found to be within the error margin from the experimental values (Table 3).
[0074] Since the storage modulus corresponds to the stored energy in the biocomposite, an increase in temperature affects its value due to the molecular motion and frequency of the polymer chains. The incorporation of HPs increased the storage modulus of each specimen due to the restriction of chain movement by the hard HPs. The effectiveness of the fillers can be evaluated by calculating the reinforcement effectiveness factor (C), which was estimated using Equation 5 [Non-Patent Document 8: D. Romanzini, A. Lavoratti, HL Ornaghi, SCA Mico, AJ Zattera, Influence of fiber content on the mechanical and dynamic mechanical properties of glass / ramie polymer composites, Materials & Design 47 (2013) 9-15].
number
[0075] Heat resistance of PHBV biocomposite From the packaging application point of view, the heat resistance of biocomposites is an important parameter, especially for packaging and encapsulation applications of hot beverages and thermal products. This can be quantitatively evaluated by measuring the heat deflection temperature (HDT). Figure 6 shows the heat deflection temperature (HDT) of the composite formulations. The HDT of the original PHBV was 116°C, which increased to 170°C after the addition of 60% HP. The incorporation of HP limits the mobility of the polymer chains even at higher temperatures and resists deformation depending on the loading ratio. In contrast, the addition of the softer PBAT reduced the HDT value to about 157°C. This resulted from the improvement of the overall composite chain behavior and the reduction of the load-bearing capacity at higher temperatures. It is known that the compatibilizer mPBAT contains lower molecular weight polymer chains and its use can contribute to the reduction of the HDT. On the other hand, after the addition of 60% HP in PHBV-PBAT in the presence of mPBAT, a HDT higher than 120 °C was shown, which was higher than that of pristine PHBV. Overall, the thermal resistance of the biocomposite is maintained even after the incorporation of high loading of HP (60%).
[0076] Rheological properties of PHBV biocomposites Parallel plate viscometer is used to determine the dynamic rheological properties of the developed biocomposites. The corresponding storage modulus, loss modulus and complex viscosity versus frequency are shown in Figures 7A-7C, 8A-8C and 9A-9C. The storage modulus of the composites was found to increase with HP incorporation, suggesting the elastic behavior of the material. A similar trend was also observed for the loss modulus of the biocomposite samples. Since melt processing of the material requires a certain threshold of viscosity, it is of paramount importance to know the effect of HP composition on the melt viscosity. The incorporation of 60% HP in the PHBV matrix alone results in a complex viscosity of 1.8 Mpa.s at a frequency of 1 Hz (corresponding to 60 rpm), which increases to 2.6 MPa.s due to the higher order chain entanglement of PBAT molecules. Meanwhile, the incorporation of mPBAT into the biocomposite led to a decrease in the complex viscosity to 1.02 MPa.s, which was mainly attributed to the presence of low molecular weight PBAT chains and wetting of HP, which promoted the chains sliding on its surface and reduced the molecular friction force. Overall, the decrease in complex viscosity of the developed formulation is helpful for smooth melt extrusion processing without reaching the threshold screw torque.
[0077] Water absorption of PHBV biocomposite Most lignocellulosic biofillers are hydrophilic in nature and are known to absorb large amounts of water. It is envisioned that HP, a lignocellulosic material, also has high water absorption that can be carried over to the PHBV-PBAT composite. Understanding the water absorption behavior and their impact on the biocomposite is essential since water absorption is directly related to the dimensional stability of the biocomposite end product. Plots of water absorption percentage versus time in days are given in Figures 10A-10D. In the case of PHBV, a clear increase in water absorption was shown with increasing HP loading. In contrast, biocomposites with PHBV-PBAT matrix showed relatively low water absorption at higher HP loading. This suggests that a coating develops on the hemp powder surface due to the presence of PBAT, preventing its water absorption. Furthermore, the use of mPBAT compatibilizer, which formed chemical bonds with the HP particles, prevents water molecule diffusion and its direct access to the HP particles.
[0078] In terms of water absorption, water molecules can penetrate the surface by various mechanisms, such as capillary transport through micropores, diffusion through micropores between polymer chains, and diffusion through gaps between biofillers and polymer domains. However, diffusion through micropores between biofillers and polymer domains is the most prominent reason for water absorption. Mainly, water molecules can be absorbed directly by biofillers and through the interface between biofillers and matrix by the formation of hydrogen bonds. The use of mPBAT as a compatibilizer develops a coating on HP, which prevents direct access to HP by water molecules. In addition, the chemical bond between mPBAT and HP improves the interfacial adhesion between biofillers and matrix (also confirmed by SEM microscopy analysis of fractured surfaces), which ultimately greatly reduces the diffusion of water molecules through the interface. Overall, the use of mPBAT compatibilizer is not only effective in improving mechanical properties, but is equally important in preventing water absorption for biocomposites, mainly at higher loadings.
[0079] It can be seen from the previous chapter that the incorporation of mPBAT into PHBV-PBAT HP results in a biocomposite with relatively high stiffness and low water absorption. The formulation developed in this study results in a biocomposite with similar properties of pristine PHBV. The reaction of mPBAT with HP and limited reaction with PHBV during reactive extrusion process leads to an anchoring effect where the PBAT chains connected to HP interact with the PHBV-PBAT matrix and increase the interfacial interaction of HP with other polymer chains. Morphological images of the fracture surface of the pristine matrix and its biocomposites at 10%, 30% and 60% HP loading are shown in Figures 11A-11D, 12A-12D and 13A-13C. Morphological analysis of these polymers and composites suggests proper dispersion of the filler. Wetting of HP with the polymer chains is seen in Figures 14A-14C. In the case of PHBV-30 HP biocomposite, HP is fully exposed outside the matrix showing lower interfacial adhesion. On the other hand, in the case of (80:20)-M with 30% HP, the filler particles are found to be fully coated by the polymer domains, which helps in stress transfer against the applied force. This enhanced interfacial interaction is responsible for stress transfer between the matrix and filler, which resulted in improved mechanical strength and modulus along with impact strength and reduced water absorption.
[0080] While the present invention has been described with reference to certain specific embodiments, various modifications thereof will become apparent to those skilled in the art without departing from the spirit and scope of the invention. All such modifications as become apparent to those skilled in the art are intended to be included within the scope of the following claims.
Claims
1. A composition for use in the manufacture of a biodegradable biocomposite material, comprising: a) about 30% to about 99.5% by weight of a polymer component comprising poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) or a mixture of PHBV and polybutylene adipate terephthalate (PBAT); b) about 0.5% to about 60% by weight of hemp residue; c) optionally, from about 0.1% to about 50% by weight, PBAT grafted with one or more compatibilizers selected from maleic anhydride, glycidyl methacrylate, pyromellitic anhydride, acrylic acid, polyacrylic acid, methylene diphenyl diisocyanate, poly(glycidyl methacrylate), copolymers of glycidyl methacrylate and copolymers of acrylic acid, and / or one or more compatibilizers selected from maleic anhydride, glycidyl methacrylate, pyromellitic anhydride, acrylic acid, polyacrylic acid, methylene diphenyl diisocyanate, poly(glycidyl methacrylate), copolymers of glycidyl methacrylate, and copolymers of acrylic acid; A composition comprising:
2. The composition of claim 1, wherein the polymer component is poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV).
3. 2. The composition of claim 1, wherein the polymer component is the mixture of PHBV and polybutylene adipate terephthalate (PBAT).
4. 4. The composition of claim 3, wherein the PHBV-PBAT mixture comprises about 10% to about 90% by weight of PHBV and about 90% to about 10% by weight of PBAT, based on the total weight of the mixture.
5. 4. The composition of claim 3, wherein the PHBV-PBAT mixture comprises about 50% to about 90% by weight of PHBV and about 50% to about 10% by weight of PBAT, based on the total weight of the mixture.
6. 6. The composition of claim 1, wherein the composition comprises from about 40% to about 90% by weight of the polymer component and from about 10% to about 60% by weight of hemp residue.
7. The composition of any one of claims 1 to 6, wherein the composition comprises about 5% to 20% by weight of the PBAT grafted with the one or more compatibilizers.
8. 8. The composition of claim 1, wherein the hemp residue comprises particles having a length of about 75 to about 150 μm and an average aspect ratio of about 3.5 to about 5.
9. The hemp residue has a density of about 1.0 to about 2.0 g / cm 3 The composition of claim 1 having a density of
10. 10. The composition according to any one of claims 1 to 9, wherein the hemp residue comprises about 60% to about 75% by weight of cellulose, about 5% to about 15% by weight of hemicellulose and about 10% to about 25% by weight of lignin.
11. 11. The composition of any one of claims 1 to 10, wherein the hemp residue has been processed to remove THC and CBD.
12. 12. The composition of any one of claims 1 to 11, further comprising about 1 to about 3 weight percent of a treating agent such as glycerol monostearate and stearic acid.
13. 13. The composition according to any one of claims 1 to 12, further comprising one or more inorganic fillers (talc, clay, wollastonite, montmorillonite or alkali or alkaline earth metal carbonates, bicarbonates, oxides or sulfates).
14. A biocomposite material produced from the composition of any one of claims 1 to 13.
15. 1. A biocomposite material comprising a blend, the blend comprising: a) about 30% to about 99.5% by weight of a polymer component comprising poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) or a mixture of PHBV and polybutylene adipate terephthalate (PBAT); b) about 0.5% to about 60% by weight of hemp residue; c) optionally, from about 0.1% to 50% by weight, PBAT grafted with one or more compatibilizers selected from maleic anhydride, glycidyl methacrylate, pyromellitic anhydride, acrylic acid, polyacrylic acid, methylene diphenyl diisocyanate, poly(glycidyl methacrylate), copolymers of glycidyl methacrylate and copolymers of acrylic acid, and / or and one or more compatibilizers selected from maleic anhydride, pyromellitic anhydride, acrylic acid, polyacrylic acid, and methylene diphenyl diisocyanate, said mixture being heated.
16. 16. The biocomposite material of claim 15, wherein the polymer component is poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV).
17. 16. The biocomposite material of claim 15, wherein the polymer component is the mixture of PHBV and polybutylene adipate terephthalate (PBAT).
18. 18. The biocomposite material of claim 17, wherein the PHBV-PBAT mixture comprises about 5% to about 95% by weight PHBV and about 95% to about 5% by weight PBAT, based on the total weight of the blend.
19. 18. The biocomposite material of claim 17, wherein the PHBV-PBAT mixture comprises about 50% to about 90% by weight PHBV and about 50% to about 10% by weight PBAT, based on the total weight of the blend.
20. 20. The biocomposite material of any one of claims 15 to 19, wherein the composition comprises about 40% to about 90% by weight of the polymer component and about 10% to about 60% by weight of hemp residue.
21. 21. The biocomposite material of claim 20, wherein the composition comprises about 5% to 20% by weight of the PBAT grafted with the one or more compatibilizers.
22. 22. The biocomposite material of any one of claims 15 to 21, wherein the hemp residue comprises particles having a length of about 75 to about 150 μm and an average aspect ratio of about 3.5 to about 5.
23. The hemp residue has a density of about 1.0 to about 2.0 g / cm 3 23. The biocomposite material according to any one of claims 15 to 22, having a density of
24. 24. The biocomposite material according to any one of claims 15 to 23, wherein the hemp residue comprises about 60% to about 75% by weight of cellulose, 5-15% by weight of hemicellulose and about 10% to about 25% by weight of lignin.
25. 25. The biocomposite material of any one of claims 15 to 24, wherein the hemp residue has been processed to remove tetrahydrocannabinol (THC) and cannabidiol (CBD).
26. 26. The biocomposite material of any one of claims 16 to 25, further comprising about 1 to about 3 wt. % of a treating agent such as glycerol monostearate and stearic acid.
27. 27. The biocomposite material according to any one of claims 16 to 26, further comprising an inorganic filler (talc, clay, wollastonite, montmorillonite or an alkali or alkaline earth metal carbonate, bicarbonate, oxide or sulfate).
28. A method for preparing a biocomposite material according to any one of claims 15 to 27, comprising the steps of: a) blending said polymer component with said hemp residue and optionally said one or more compatibilizers and / or said PBAT grafted with one or more compatibilizers; b) heating the admixture at a temperature sufficient to melt at least the PHBV and / or PBAT; A method for providing the above.
29. 30. The method of claim 28, wherein heating the admixture comprises extruding the admixture at an extrusion temperature sufficient to melt at least the PHBV and / or PBAT.
30. 30. The method of claim 29, wherein the blend is extruded through a screw extruder at a screw speed of about 80 to about 120 rpm and a processing temperature of about 150°C.
31. The composite material comprises PBAT grafted with the compatibilizer, and the method comprises: preparing the compatibilizer-grafted PBAT by combining PBAT, the one or more compatibilizers, and a free radical initiator to form a reaction mixture and melt processing the reaction mixture to form the compatibilizer-grafted PBAT.
31. The method of any one of claims 28 to 30, further comprising:
32. 32. The method of claim 31 , wherein the melt processing comprises melt extrusion.
Citation Information
Patent Citations
Biodegradable molding products and films from blends of starch esters and polyesters
JP1996502552A
Use of plastic materials made from polymer mixtures
JP2002529567A
Fat-aromatic biodegradable polyester
JP2011520005A
Polylactic acid-based mulching film
JP2014162799A