Molded Articles Containing Zeolite Materials Having Framework-Type MFI

A chemical molded article with a Type I nitrogen adsorption/desorption isotherm and MFI structure, combined with a binder, enhances propylene oxide yield and reduces by-products in the epoxidation of propene, addressing the limitations of existing catalysts.

JP7574216B2Active Publication Date: 2024-10-28BASF SE
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021564365
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-29
Filing Date
2020-04-27
Publication Date
2024-10-28
Estimated Expiration
2040-04-27

AI Technical Summary

Technical Problem

Existing catalysts for the epoxidation of propene to propylene oxide suffer from low selectivity and high production of by-products, with a need for improved molded articles that enhance propylene oxide yield and reduce by-product formation.

Method used

Development of a chemical molded article comprising a zeolite material with a Type I nitrogen adsorption/desorption isotherm and a skeletal MFI structure containing Si, O, and Ti, combined with a binder, exhibiting a total pore volume of at least 0.4 mL/g and a breaking strength of at least 6N, which is produced through a method involving a colloidal silica dispersion and hydrothermal treatment.

Benefits of technology

The solution significantly improves propylene oxide selectivity and yield while maintaining excellent mechanical strength and catalyst life, reducing by-product formation in the epoxidation reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574216000001
    Figure 0007574216000001
  • Figure 0007574216000002
    Figure 0007574216000002
  • Figure 0007574216000003
    Figure 0007574216000003
Patent Text Reader

Abstract

1. A chemical shaped article comprising a zeolitic material exhibiting a Type I nitrogen adsorption / desorption isotherm, determined as described in Reference Example 1, and having a framework type MFI and a framework structure comprising Si, O, and Ti, the shaped article further comprising a binder for the zeolitic material, the binder comprising Si and O, the shaped article exhibiting a total pore volume of at least 0.4 mL / g and a crush strength of at least 6 N.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a chemically shaped article, in particular a shaped article comprising a specific binder and a specific zeolite material having a framework type MFI and a framework structure containing Si, O and Ti. [Background technology]

[0002] Titanium-containing zeolitic materials of structure type MFI exhibit type I nitrogen adsorption / desorption isotherms (e.g. titanium silicalite-1) and are known to be efficient catalysts, including for example epoxidation reactions. In industrial scale processes, typically run in a continuous mode, the zeolitic materials are usually used in the form of shaped articles that contain a suitable binder in addition to the catalytically active zeolitic material.

[0003] US2016 / 250624A1 relates to a method for producing a molded article containing a hydrophobic zeolite material, and a method for producing the same.

[0004] US6551546B1 relates to a method for producing a shaped body comprising at least one porous oxide material and at least one metal oxide.

[0005] DE 19859561 A1 likewise relates to a method for producing shaped bodies which comprise at least one porous oxide material and at least one metal oxide.

[0006] US7825204B2 relates to extrudates containing inorganic oxides and discloses comb-branched polymers. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] US2016 / 250624A1 [Patent Document 2] US6551546B1 [Patent Document 3] DE19859561A1 [Patent Document 4] US7825204B2 Summary of the Invention [Problem to be solved by the invention]

[0008] The object of the present invention is to provide new and advantageous shaped articles comprising zeolitic materials with framework type MFI, which have advantageous properties, in particular improved propylene oxide selectivity, when used as catalysts or catalyst components, in particular in the epoxidation reaction of propene to propylene oxide. A further object of the present invention is to provide a process for preparing such shaped articles, in particular a process which gives shaped articles with advantageous properties, preferably when used as catalysts or catalyst components, in particular in oxidation or epoxidation reactions. A further object of the present invention is to provide an improved process for the epoxidation of propene with hydrogen peroxide as oxidizing agent, which shows very low selectivity with respect to by-products and by-products of the epoxidation reaction, while at the same time allowing very high propylene selectivity.

[0009] Surprisingly, it has been found that when certain specific binder precursor materials are used for the production of molded articles, and when intermediate molded articles comprising zeolitic materials having framework MFI are subjected to specific post-treatments, it is possible to provide such molded articles exhibiting said advantageous properties.In particular, it has been found that, when used as a catalyst in the epoxidation reaction of propene to propylene oxide, and compared with the molded articles of the prior art, it is possible to provide molded articles which exhibit a significant improvement in the selectivity and yield of propylene oxide, and which further exhibit excellent life properties. [Means for solving the problem]

[0010] Thus, the present invention relates to a chemical molding comprising a zeolite material having a framework MFI and a framework structure comprising Si, O and Ti, which exhibits a nitrogen adsorption / desorption isotherm of type I, the molding further comprises a binder for the zeolite material, the binder comprising Si and O, the molding exhibiting a total pore volume of at least 0.4 mL / g and a crushing strength of at least 6 N. In particular, the present invention relates to a chemical molding comprising a zeolite material having a framework MFI and a framework structure comprising Si, O and Ti, the molding further comprises a binder for the zeolite material, the binder comprising Si and O, the molding exhibiting a total pore volume of at least 0.4 mL / g, the molding further comprises a binder for the zeolite material, the binder comprising Si and O, the molding exhibiting a total pore volume of at least 0.4 mL / g, the molding further comprises a binder for the zeolite material, the binder comprising Si and O, the molding exhibiting a crushing strength of at least 6 N, the molding further comprises a nitrogen adsorption / desorption isotherm of type I, the molding further comprises a binder for the zeolite material, the binder comprising Si and O, the molding exhibiting a total pore volume of at least 0.4 mL / g, the molding further comprises a binder for the zeolite material, the binder comprising Si and O, the molding exhibiting a crushing strength of at least 6 N ... crushing strength of at least 6 N, the molding further comprises a binder for the zeolite material, the binder comprising Si and O, the molding further comprises a crushing strength of at least 6 N, the molding further comprises a crushing strength of at least 6

[0011] According to the invention, a moulding is understood to be a three-dimensional entity resulting from a moulding process, and therefore the term "molding" is used synonymously with the term "shaped body".

[0012] The present invention further relates to a method for producing a chemical molded article comprising a zeolitic material exhibiting a nitrogen adsorption / desorption isotherm of type I, determined as described in Reference Example 1, and having a framework type MFI and a framework structure comprising Si, O and Ti, said molded article further comprising a binder for said zeolitic material, said binder comprising Si and O, preferably a method for producing a chemical molded article according to the invention described herein, comprising the following steps: (i) providing a zeolitic material exhibiting a type I nitrogen adsorption / desorption isotherm, determined as described in Reference Example 1, and having framework type MFI and a framework structure comprising Si, O and Ti; (ii) providing a binder precursor comprising a colloidal dispersion of silica in water, said binder precursor exhibiting a volume-based particle size distribution characterized by a Dv10 value of at least 35 nanometers, a Dv50 value of at least 45 nanometers, and a Dv90 value of at least 65 nanometers, determined as described in Example 5; (iii) preparing a mixture comprising the zeolitic material provided in step (i) and the binder precursor provided in step (ii); (iv) molding the mixture obtained from step (iii) to obtain a precursor of a molded article; (v) preparing a mixture comprising the precursor of the shaped article obtained from step (iv) and water, and subjecting the mixture to a water treatment under hydrothermal conditions to obtain a water-treated precursor of the shaped article; (vi) Calcining the water-treated precursor of the molded article in a gas atmosphere to obtain the molded article.

[0013] The present invention further relates to a chemical shaped article comprising particles of a zeolitic material exhibiting a nitrogen adsorption / desorption isotherm of type I, determined as described in Reference Example 1, and having framework type MFI and a framework structure comprising Si, O and Ti, said article further comprising a binder for said particles, said binder comprising Si and O, preferably a chemical shaped article obtainable or obtained by the process of the present invention as described herein.

[0014] The present invention further relates to the use of the inventive shaped articles described herein as adsorbents, absorbents, catalysts or catalyst components, preferably as catalysts or catalyst components, more preferably as Lewis acid catalysts or Lewis acid catalyst components, as isomerization catalysts or isomerization catalyst components, as oxidation catalysts or oxidation catalyst components, as aldol condensation catalysts or aldol condensation catalyst components or as Prins reaction catalysts or Prins reaction catalyst components.

[0015] The present invention further relates to a process for oxidizing an organic compound, preferably for epoxidizing an organic compound, more preferably for epoxidizing an organic compound having at least one C-C double bond, preferably a C2-C10 alkene, more preferably a C2-C5 alkene, more preferably a C2-C4 alkene, more preferably a C2 or C3 alkene, more preferably propene, comprising contacting the organic compound, preferably in a continuous mode, with a catalyst comprising the shaped article described herein.

[0016] The present invention further relates to a process for the production of propylene oxide, comprising reacting propene, preferably in a continuous mode, in a methanol solution with hydrogen peroxide in the presence of a catalyst comprising the shaped article described herein to obtain propylene oxide.

[0017] The present invention further relates to the use of a colloidal dispersion of silica in water as binder precursor for the preparation of a chemical moulding, preferably for the preparation of a moulding as described herein, further comprising a binder obtained from said binder precursor, comprising a zeolitic material exhibiting a nitrogen adsorption / desorption isotherm of type I, determined as described in Reference Example 1, and having a framework type MFI and a framework structure comprising Si, O and Ti, said silica having a diameter of at least 35 nanometres, preferably in the range of 35 to 80 nanometres, more preferably in the range of 40 to 75 nanometres, more preferably in the range of 45 to 70 nanometres, determined as described in Reference Example 5. The molded article preferably exhibits a volume-based particle size distribution characterized by a Dv10 value of at least 45 nanometers, preferably in the range of 45 to 125 nanometers, more preferably in the range of 55 to 115 nanometers, more preferably in the range of 65 to 105 nanometers, and a Dv90 value of at least 65 nanometers, preferably in the range of 65 to 200 nanometers, more preferably in the range of 85 to 180 nanometers, more preferably in the range of 95 to 160 nanometers, and the molded article preferably exhibits a total pore volume of at least 0.4 mL / g, determined as described in Reference Example 2, and a breaking strength of at least 6 N, determined as described in Reference Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] With respect to the chemically molded article of the present invention, it is preferred that 95 to 100 mass%, preferably 98 to 100 mass%, more preferably 99 to 100 mass%, more preferably at least 99.5 to 100 mass%, more preferably 99.9 to 100 mass%, of the zeolite material contained in the molded article is composed of Si, O, Ti, and optionally H.

[0019] With respect to the zeolite material contained in the chemically formed article, it is preferred that the zeolite material contains Ti in an amount in the range of 0.2 to 5 mass %, preferably in the range of 0.5 to 4 mass %, more preferably in the range of 1.0 to 3 mass %, more preferably in the range of 1.2 to 2.5 mass %, more preferably in the range of 1.4 to 2.2 mass %, calculated as elemental Ti and based on the total mass of the zeolite material.

[0020] Furthermore, it is preferred that the zeolite material contained in the molded article is titanium silicalite-1.

[0021] With regard to the binder, it is preferable that 95 to 100 mass%, preferably 98 to 100 mass%, more preferably 99 to 100 mass%, more preferably at least 99.5 to 100 mass%, more preferably 99.9 to 100 mass% of the binder contained in the molded article is composed of Si and O.

[0022] The molded article preferably contains the binder in an amount, calculated as SiO2, based on the total mass of the molded article, in the range of 2 to 90 mass%, more preferably in the range of 5 to 70 mass%, more preferably in the range of 10 to 50 mass%, more preferably in the range of 15 to 30 mass%, and more preferably in the range of 20 to 25 mass%.

[0023] Furthermore, it is preferable that 95 to 100 mass %, more preferably 98 to 100 mass %, more preferably 99 to 100 mass %, more preferably at least 99.5 to 100 mass %, more preferably 99.9 to 100 mass % of the molded article is made of the zeolite material and the binder.

[0024] The molded article preferably contains micropores having a pore diameter in the range of 0.1 to less than 2 nm as determined in Reference Example 4. Furthermore, the molded article preferably contains mesopores having a pore diameter in the range of 2 to 50 nm as determined in Reference Example 4. Thus, it is particularly preferable that the molded article contains micropores having a pore diameter in the range of 0.1 to less than 2 nm as determined in Reference Example 4, and mesopores having a pore diameter in the range of 2 to 50 nm as determined in Reference Example 4.

[0025] Preferably, the molded article disclosed herein exhibits a total pore volume in the range of 0.4 to 1.5 mL / g, more preferably in the range of 0.4 to 1.2 mL / g, more preferably in the range of 0.4 to 1.0 mL / g, the pore volume being determined as described in Reference Example 2.

[0026] Furthermore, the molded article disclosed in this specification preferably exhibits a breaking strength in the range of 6 to 25 N, more preferably in the range of 7 to 20 N, more preferably in the range of 8 to 15 N, the breaking strength being determined as described in Reference Example 3.

[0027] It is preferred that the shaped article is a strand. It is particularly preferred that the strand shaped article has a hexagonal, rectangular, quadratic, triangular, elliptical or circular cross section, more preferably a circular cross section. It is particularly preferred that the strand shaped article is an extrudate.

[0028] When the molded article is a strand having a circular cross section, the diameter of the cross section is preferably in the range of 0.5 to 5 mm, more preferably in the range of 1 to 3 mm, more preferably in the range of 1.5 to 2 mm. It is particularly preferred that the molded article, which is a strand having a circular cross section with a specific diameter disclosed herein, is an extrudate.

[0029] Thus, it is preferred that the shaped articles disclosed herein are extrudates.

[0030] The molded article preferably has a water bending parameter, determined as described in Reference Example 11, in the range of 1.0 to 2.5, more preferably 1.3 to 2.0, more preferably 1.6 to 1.8, more preferably 1.6 to 1.75, and more preferably 1.6 to 1.72.

[0031] Furthermore, the molded article has a BET specific surface area of ​​300 to 450 m, as determined in the manner described in Reference Example 6. 2 / g, more preferably 310 to 400m 2 / g, more preferably 320 to 375 m 2 It is preferable to express it in the range of / g.

[0032] Regarding the crystallinity of the molded article, it is preferable that the molded article exhibits a crystallinity, determined as described in Reference Example 7, in the range of 50 to 100%, more preferably in the range of 50 to 90%, and more preferably in the range of 50 to 80%.

[0033] With regard to the propylene oxide activity of the molded article, it is preferred that the molded article exhibits a propylene oxide activity, determined as described in Reference Example 9, of at least 4.5% by mass, more preferably in the range of 4.5 to 11% by mass, more preferably in the range of 4.5 to 10% by mass.

[0034] It is preferred that the molded article exhibits a pressure drop rate, determined as described in Reference Example 9, in the range of 0.005 to 0.019 bar (abs) / min, more preferably in the range of 0.006 to 0.017 bar (abs) / min, more preferably in the range of 0.007 to 0.015 bar (abs) / min.

[0035] Preferably, the molded article is used as a catalyst or catalyst component, in particular in the reaction for preparing propylene oxide from propene and hydrogen peroxide. In this respect, the molded article used as a catalyst in the reaction for preparing propylene oxide from propene and hydrogen peroxide, preferably in the continuous epoxidation reaction as described in Reference Example 10, preferably exhibits a hydrogen peroxide conversion rate in the range of 90-95%, whereby preferably the temperature of the cooling medium is in the range of 55-56° C. and the on-stream time is in the range of 200-600 hours, preferably the on-stream time is in the range of 300-600 hours, more preferably the on-stream time is in the range of 350-600 hours. In this respect, the term "on-stream time" refers to the duration of the continuous epoxidation reaction without catalyst regeneration.

[0036] The present invention further relates to a method for producing a chemical molded article comprising a zeolitic material exhibiting a nitrogen adsorption / desorption isotherm of type I, determined as described in Reference Example 1, and having a framework type MFI and a framework structure comprising Si, O and Ti, said molded article further comprising a binder for said zeolitic material, said binder comprising Si and O, preferably a method for producing a chemical molded article as described herein, comprising the following steps: (i) providing a zeolitic material exhibiting a type I nitrogen adsorption / desorption isotherm, determined as described in Reference Example 1, and having framework type MFI and a framework structure comprising Si, O and Ti; (ii) providing a binder precursor comprising a colloidal dispersion of silica in water, said binder precursor exhibiting a volume-based particle size distribution characterized by a Dv10 value of at least 35 nanometers, a Dv50 value of at least 45 nanometers, and a Dv90 value of at least 65 nanometers, determined as described in Example 5; (iii) preparing a mixture comprising the zeolitic material provided in step (i) and the binder precursor provided in step (ii); (iv) molding the mixture obtained from step (iii) to obtain a precursor of a molded article; (v) preparing a mixture comprising the precursor of the shaped article obtained from step (iv) and water, and subjecting the mixture to a water treatment under hydrothermal conditions to obtain a water-treated precursor of the shaped article; (vi) Calcining the water-treated precursor of the molded article in a gas atmosphere to obtain the molded article.

[0037] The volume-based particle size distribution of the colloidal dispersion of silica in water according to step (ii), determined as described in Reference Example 5, is preferably characterized by a Dv10 value in the range of 35 to 80 nanometers, more preferably in the range of 40 to 75 nanometers, more preferably in the range of 45 to 70 nanometers, a Dv50 value in the range of 45 to 125 nanometers, more preferably in the range of 55 to 115 nanometers, more preferably in the range of 65 to 105 nanometers, and a Dv90 value in the range of 65 to 200 nanometers, more preferably in the range of 85 to 180 nanometers, more preferably in the range of 95 to 160 nanometers.

[0038] It is further preferred that the volume-based particle size distribution of the colloidal dispersion of silica in water according to step (ii) is a unimodal distribution.

[0039] Regarding the content of silica contained in the colloidal dispersion of silica in water from step (ii), no particular restrictions are applied. It is preferred that the colloidal dispersion of silica in water from step (ii) contains silica in an amount in the range of 25-65% by weight, more preferably in the range of 30-60% by weight, more preferably in the range of 35-55% by weight, based on the total weight of silica and water.

[0040] It is preferred that 95 to 100% by weight, more preferably 98 to 100% by weight, more preferably 99 to 100% by weight of the binder precursor from step (ii) consists of a colloidal dispersion of silica in water.

[0041] Further, it is preferred that 95-100% by mass, more preferably 98-100% by mass, more preferably 99-100% by mass, more preferably at least 99.5-100% by mass, more preferably 99.9-100% by mass of the zeolitic material from step (i) consists of Si, O, Ti, and preferably H.

[0042] Regarding the content of Ti in the zeolitic material from step (i), no particular restrictions are applied. It is preferred that the zeolitic material from step (i) contains Ti in an amount in the range of 0.2-5 mass %, more preferably in the range of 0.5-4 mass %, more preferably in the range of 1.0-3 mass %, more preferably in the range of 1.2-2.5 mass %, more preferably in the range of 1.4-2.2 mass %, based on the total mass of the zeolitic material.

[0043] Preferably the zeolitic material according to step (i) is titanium silicalite-1.

[0044] Further, in the mixture prepared by step (iii) and subjected to step (iv), it is preferred that the mass ratio of the zeolite material, based on the total of the zeolite material and the binder calculated as SiO2, is in the range of 2 to 90%, more preferably in the range of 5 to 70%, more preferably in the range of 10 to 50%, more preferably in the range of 15 to 30%, more preferably in the range of 20 to 25%.

[0045] The mixture disclosed herein may comprise further components. It is preferred that the mixture prepared according to step (iii) and subjected to step (iv) further comprises one or more additives, more preferably one or more viscosity modifiers, or one or more mesopore formers, or one or more viscosity modifiers and one or more mesopore formers.

[0046] When the mixture prepared in step (iii) and subjected to step (iv) further contains one or more additives, it is preferable that 95 to 100 mass%, more preferably 98 to 100 mass%, more preferably 99 to 100 mass%, more preferably 99.5 to 100 mass%, more preferably 99.9 to 100 mass% of the mixture prepared in step (iii) and subjected to step (iv) consists of the zeolite material, the binder precursor, and the one or more additives.

[0047] Furthermore, when the mixture prepared by step (iii) and subjected to step (iv) further comprises one or more additives, it is preferred that the one or more additives are selected from the group consisting of water, alcohol, organic polymers, and mixtures of two or more thereof, the organic polymer is preferably selected from the group consisting of cellulose, cellulose derivatives, starch, polyalkylene oxides, polystyrene, polyacrylates, polymethacrylates, polyolefins, polyamides, polyesters, and mixtures of two or more thereof, the organic polymer is more preferably selected from the group consisting of cellulose ethers, polyalkylene oxides, polystyrene, and mixtures of two or more thereof, the organic polymer is more preferably selected from the group consisting of methylcellulose, carboxymethylcellulose, polyethylene oxide, polystyrene, and mixtures of two or more thereof, and more preferably the one or more additives comprise, more preferably consist of, water, carboxymethylcellulose, polyethylene oxide, and polystyrene.

[0048] Furthermore, when the mixture prepared by step (iii) and subjected to step (iv) further comprises one or more additives, it is preferred that in the mixture prepared by step (iii) and subjected to step (iv), the mass ratio of the zeolitic material to the one or more additives is in the range of 0.3:1 to 1:1, more preferably in the range of 0.4:1 to 0.8:1, more preferably in the range of 0.5:1 to 0.6:1.

[0049] When the mixture prepared by step (iii) and subjected to step (iv) further comprises a cellulose derivative as an additive, it is preferred that in the mixture prepared by step (iii) and subjected to step (iv), the mass ratio of the zeolitic material to the cellulose derivative, preferably cellulose ether, more preferably carboxymethylcellulose, is in the range of 10:1 to 53:1, more preferably in the range of 15:1 to 40:1, more preferably in the range of 20:1 to 35:1.

[0050] When the mixture prepared by step (iii) and subjected to step (iv) further comprises polyethylene oxide as an additive, it is preferred that the mass ratio of the zeolite material to the polyethylene oxide in the mixture prepared by step (iii) and subjected to step (iv) is in the range of 70:1 to 110:1, more preferably in the range of 75:1 to 100:1, more preferably in the range of 77:1 to 98:1.

[0051] When the mixture prepared by step (iii) and subjected to step (iv) further comprises polystyrene as an additive, it is preferred that the mass ratio of the zeolite material to polystyrene in the mixture prepared by step (iii) and subjected to step (iv) is in the range of 2:1 to 8:1, more preferably in the range of 3:1 to 6:1, more preferably in the range of 3.5:1 to 5:1.

[0052] When the mixture prepared by step (iii) and subjected to step (iv) further comprises water as an additive, it is preferred that the mass ratio of zeolitic material to water in the mixture prepared by step (iii) and subjected to step (iv) is in the range of 0.7:1 to 0.85:1, more preferably in the range of 0.72:1 to 0.8:1, more preferably in the range of 0.74:1 to 0.79:1.

[0053] It is particularly preferred that the mixture prepared by step (iii) and subjected to step (iv) further comprises a cellulose derivative, polyethylene oxide, polystyrene, and water as additives.

[0054] No particular restrictions apply with regard to the provision of the mixture in step (iii), i.e. how the mixture is prepared. It is preferred that the mixture is prepared by suitable mixing of the components, preferably by mixing in a kneader or mixing muller.

[0055] Further, it is preferred that the mixture obtained from step (iii) is shaped into strands, more preferably into strands having a circular cross section, by step (iv), wherein the strands having a circular cross section preferably have a diameter in the range of 0.5 to 5 mm, more preferably in the range of 1 to 3 mm, more preferably in the range of 1.5 to 2 mm.

[0056] Further, it is preferred that the mixture obtained from step (iii) and subjected to step (iv) has a plasticity, determined as described in Reference Example 12, in the range of 500 to 3000 N, more preferably in the range of 750 to 2000 N, more preferably in the range of 1000 to 1500 N.

[0057] With regard to the shaping in step (iv), no particular restrictions apply and shaping may be carried out by any conceivable means. It is preferred that the shaping according to step (iv) comprises extruding the mixture obtained from step (iii).

[0058] Suitable extrusion equipment is described, for example, in "Ullmann's Enzyklopaedie der Technischen Chemie", 4th edition, vol. 2, p. 295 et seq., 1972. In addition to the use of extruders, extrusion presses can also be used to prepare the shaped articles. If necessary, the extruder can be appropriately cooled during the extrusion process. The strands leaving the extruder through the extruder die head can be mechanically cut via a suitable wire or discontinuous gas stream.

[0059] The shaping according to step (iv) may comprise further process steps. The shaping according to step (iv) preferably further comprises drying the precursor of the shaped article in a gas atmosphere, said drying being preferably carried out at a temperature of the gas atmosphere in the range of 80-160°C, more preferably in the range of 100-140°C, more preferably in the range of 110-130°C, the gas atmosphere preferably comprising nitrogen, oxygen or a mixture thereof, the gas atmosphere being more preferably oxygen, air or lean air.

[0060] Furthermore, the shaping in step (iv) preferably further comprises calcining the dried precursor of the shaped body in a gas atmosphere, the calcination being preferably carried out at a gas atmosphere temperature in the range of 450 to 530°C, more preferably in the range of 470 to 510°C, more preferably in the range of 480 to 500°C, the gas atmosphere preferably comprising nitrogen, oxygen or a mixture thereof, the gas atmosphere being more preferably oxygen, air or lean air.

[0061] No particular restrictions are applied to the content of water in the mixture prepared in step (v). It is preferred that the mass ratio of the precursor of the molded article to water in the mixture prepared in step (v) is in the range of 1:1 to 1:30, more preferably in the range of 1:5 to 1:25, and more preferably in the range of 1:10 to 1:20.

[0062] Furthermore, it is preferable that 95 to 100 mass%, more preferably 98 to 100 mass%, more preferably 99 to 100 mass%, more preferably 99.5 to 100 mass%, and more preferably 99.9 to 100 mass% of the mixture prepared in step (v) consists of the precursor of the molded article and water.

[0063] Regarding the temperature of the mixture for the water treatment according to step (v), no particular limitation is applied. It is preferred that the water treatment according to step (v) comprises a temperature of the mixture in the range of 100 to 200°C, more preferably in the range of 125 to 175°C, more preferably in the range of 130 to 160°C, more preferably in the range of 135 to 155°C, more preferably in the range of 140 to 150°C.

[0064] The water treatment according to step (v) is preferably carried out under autogenous pressure, preferably in an autoclave.

[0065] The water treatment in step (v) is preferably carried out for 6 to 10 hours, more preferably 7 to 9 hours, and more preferably 7.5 to 8.5 hours.

[0066] It is further preferred that step (v) comprises separating the water-treated precursor of the shaped article from the mixture resulting from the water treatment.

[0067] When step (v) further comprises separating a precursor of the water-treated shaped article from the mixture obtained from the water treatment, it is preferred that separating the precursor of the water-treated shaped article from the mixture obtained from the water treatment comprises subjecting the mixture obtained from the water treatment to solid-liquid separation, preferably washing the separated precursor, and preferably drying the washed precursor.

[0068] Furthermore, when separating the water-treated precursor of the shaped article from the mixture obtained from the water treatment comprises subjecting the mixture obtained from the water treatment to solid-liquid separation, it is preferred that the solid-liquid separation according to step (v) comprises filtration, or centrifugation, or filtration and centrifugation.

[0069] When step (v) comprises washing the separated precursor, washing of the precursor is preferably carried out at least once with a liquid solvent system, which preferably comprises one or more of water, alcohol and mixtures of two or more thereof, and the water-treated shaped article precursor is more preferably washed with water.

[0070] When step (v) preferably further comprises drying the washed precursor, the drying according to step (v) comprises drying the precursor in a gas atmosphere, the drying being more preferably carried out at a gas atmosphere temperature in the range of 80-160°C, more preferably in the range of 100-140°C, more preferably in the range of 110-130°C, the gas atmosphere preferably comprising nitrogen, oxygen or a mixture thereof, the gas atmosphere being more preferably oxygen, air or lean air.

[0071] Regarding the temperature of the gas atmosphere for the calcination according to step (vi), no particular restrictions apply. It is preferred that the calcination according to step (vi) is carried out at a gas atmosphere temperature in the range of 400-490° C., more preferably in the range of 420-470° C., more preferably in the range of 440-460° C., the gas atmosphere preferably comprising nitrogen, oxygen or a mixture thereof, the gas atmosphere more preferably being oxygen, air or lean air.

[0072] The process of the invention described herein preferably comprises steps (i), (ii), (iii), (iv), (v) and (vi).

[0073] The present invention further relates to a chemical shaped article comprising particles of a zeolitic material exhibiting a nitrogen adsorption / desorption isotherm of type I, determined as described in Reference Example 1, and having a framework type MFI and a framework structure comprising Si, O and Ti, the article further comprising a binder for said particles, the binder comprising Si and O, the article preferably being obtainable or obtained by the method described herein.

[0074] The present invention further relates to the use of the shaped articles described herein as adsorbents, absorbents, catalysts or catalyst components, preferably as catalysts or catalyst components, more preferably as Lewis acid catalysts or Lewis acid catalyst components, as isomerization catalysts or isomerization catalyst components, as oxidation catalysts or oxidation catalyst components, as aldol condensation catalysts or aldol condensation catalyst components, or as Prins reaction catalysts or Prins reaction catalyst components.

[0075] The inventive shaped articles described herein are preferably used as oxidation catalysts or as oxidation catalyst components, more preferably as epoxidation catalysts or as epoxidation catalyst components, more preferably as epoxidation catalysts.

[0076] When the molded article according to the present invention is used as an oxidation catalyst or as an oxidation catalyst component, the molded article is preferably used for the epoxidation reaction of an organic compound having at least one C-C double bond, preferably a C2-C10 alkene, more preferably a C2-C5 alkene, more preferably a C2-C4 alkene, more preferably a C2 or C3 alkene, more preferably a propene, more preferably a propene epoxidation reaction with hydrogen peroxide as an oxidizing agent, more preferably a propene epoxidation reaction with hydrogen peroxide as an oxidizing agent in a solvent comprising an alcohol, preferably methanol.

[0077] The present invention further relates to a process for oxidizing an organic compound, preferably for epoxidizing an organic compound, more preferably for epoxidizing an organic compound having at least one C-C double bond, preferably a C2-C10 alkene, more preferably a C2-C5 alkene, more preferably a C2-C4 alkene, more preferably a C2 or C3 alkene, more preferably propene, which comprises contacting the organic compound, preferably in a continuous mode, with a catalyst comprising a shaped article according to the present invention.

[0078] Hydrogen peroxide is preferably used as the oxidizing agent and the oxidation reaction is preferably carried out in a solvent, more preferably a solvent comprising an alcohol, preferably methanol.

[0079] According to the present invention, when hydrogen peroxide is used as oxidizing agent, it is considered that hydrogen peroxide is formed in situ during the reaction from hydrogen and oxygen or from other suitable precursors. More preferably, the term "hydrogen peroxide is used as oxidizing agent" or similar as used in the context of the present invention relates to an embodiment in which hydrogen peroxide is not formed in situ but is used as starting material, preferably in the form of a solution, preferably at least partially aqueous, more preferably an aqueous solution, said preferably aqueous solution having a preferred hydrogen peroxide concentration in the range of 20-60, more preferably 25-55% by weight, based on the total weight of the solution.

[0080] The present invention further relates to a process for the preparation of propylene oxide, which comprises reacting propene, preferably in a continuous mode, in a methanol solution with hydrogen peroxide in the presence of a catalyst comprising a shaped article according to the present invention to obtain propylene oxide.

[0081] The present invention further relates to the use of a colloidal dispersion of silica in water as binder precursor for the preparation of a chemical moulding, preferably for the preparation of a moulding as described herein, further comprising a binder obtained from said binder precursor, comprising a zeolitic material exhibiting a nitrogen adsorption / desorption isotherm of type I, determined as described in Reference Example 1, and having a framework type MFI and a framework structure comprising Si, O and Ti, said silica having a diameter of at least 35 nanometres, preferably in the range of 35 to 80 nanometres, more preferably in the range of 40 to 75 nanometres, more preferably in the range of 45 to 70 nanometres, determined as described in Reference Example 5. The molded article preferably exhibits a volume-based particle size distribution characterized by a Dv10 value of at least 45 nanometers, preferably in the range of 45 to 125 nanometers, more preferably in the range of 55 to 115 nanometers, more preferably in the range of 65 to 105 nanometers, and a Dv90 value of at least 65 nanometers, preferably in the range of 65 to 200 nanometers, more preferably in the range of 85 to 180 nanometers, more preferably in the range of 95 to 160 nanometers, and the molded article preferably exhibits a total pore volume of at least 0.4 mL / g, determined as described in Reference Example 2, and a breaking strength of at least 6 N, determined as described in Reference Example 3.

[0082] According to a further aspect, the present invention relates to a mixture comprising a zeolitic material exhibiting a nitrogen adsorption / desorption isotherm of type I, determined as described in Reference Example 1, and having a framework type MFI and a framework structure comprising Si, O and Ti, the mixture further comprising a colloidal dispersion of silica in water, said binder precursor exhibiting a volume-based particle size distribution characterized by a Dv10 value of at least 35 nanometers, a Dv50 value of at least 45 nanometers, and a Dv90 value of at least 65 nanometers, determined as described in Reference Example 5.

[0083] It is preferred that the mixture has a plasticity, determined as described in Reference Example 12, in the range of 500-3000 N, more preferably in the range of 750-2000 N, more preferably in the range of 1000-1500 N.

[0084] Further, the volume-based particle size distribution of the colloidal dispersion of silica in water, determined as described in Reference Example 5, is preferably characterized by a Dv10 value in the range of 35 to 80 nanometers, more preferably in the range of 40 to 75 nanometers, more preferably in the range of 45 to 70 nanometers, a Dv50 value in the range of 45 to 125 nanometers, preferably in the range of 55 to 115 nanometers, more preferably in the range of 65 to 105 nanometers, and a Dv90 value in the range of 65 to 200 nanometers, preferably in the range of 85 to 180 nanometers, more preferably in the range of 95 to 160 nanometers.

[0085] It is preferred that the volume-based particle size distribution of the colloidal dispersion of silica is unimodal.

[0086] Regarding the content of silica in the colloidal dispersion of silica in water, no particular restrictions apply. It is preferred that the colloidal dispersion of silica in water contains silica in an amount ranging from 25 to 65% by weight, more preferably from 30 to 60% by weight, more preferably from 35 to 55% by weight, based on the total weight of silica and water.

[0087] It is preferred that 95 to 100% by mass, preferably 98 to 100% by mass, and more preferably 99 to 100% by mass of the binder precursor consists of a colloidal dispersion of silica in water.

[0088] Furthermore, it is preferred that 95 to 100 mass%, preferably 98 to 100 mass%, more preferably 99 to 100 mass%, more preferably at least 99.5 to 100 mass%, more preferably 99.9 to 100 mass% of the zeolite material is composed of Si, O, Ti, and preferably H.

[0089] There is no particular limitation on the amount of Ti contained in the zeolite material. It is preferred that the zeolite material contains Ti in an amount in the range of 0.2 to 5 mass %, more preferably in the range of 0.5 to 4 mass %, more preferably in the range of 1.0 to 3 mass %, more preferably in the range of 1.2 to 2.5 mass %, more preferably in the range of 1.4 to 2.2 mass %, based on the total mass of the zeolite material.

[0090] Preferably the zeolitic material is titanium silicalite-1.

[0091] Further, in the mixture, the mass ratio of the zeolite material relative to the total of the zeolite material and the binder calculated as SiO2 is preferably in the range of 2 to 90%, more preferably in the range of 5 to 70%, more preferably in the range of 10 to 50%, more preferably in the range of 15 to 30%, more preferably in the range of 20 to 25%.

[0092] The mixture may comprise further components. Thus, it is preferred that the mixture further comprises one or more additives, more preferably one or more viscosity modifiers, or one or more mesopore formers, or one or more viscosity modifiers and one or more mesopore formers.

[0093] It is preferable that 95 to 100 mass%, more preferably 98 to 100 mass%, more preferably 99 to 100 mass%, more preferably 99.5 to 100 mass%, and more preferably 99.9 to 100 mass% of the mixture is composed of the zeolite material and the binder precursor. When the mixture further contains one or more additives, it is preferable that 95 to 100 mass%, more preferably 98 to 100 mass%, more preferably 99 to 100 mass%, more preferably 99.5 to 100 mass%, and more preferably 99.9 to 100 mass% of the mixture is composed of the zeolite material, the binder precursor, and one or more additives.

[0094] It is preferred that the one or more additives are selected from the group consisting of water, alcohol, organic polymers, and mixtures of two or more thereof, the organic polymer is preferably selected from the group consisting of cellulose, cellulose derivatives, starch, polyalkylene oxides, polystyrene, polyacrylates, polymethacrylates, polyolefins, polyamides, polyesters, and mixtures of two or more thereof, the organic polymer is more preferably selected from the group consisting of cellulose ethers, polyalkylene oxides, polystyrene, and mixtures of two or more thereof, the organic polymer is more preferably selected from the group consisting of methylcellulose, carboxymethylcellulose, polyethylene oxide, polystyrene, and mixtures of two or more thereof, and more preferably the one or more additives comprise, more preferably consist of, water, carboxymethylcellulose, polyethylene oxide, and polystyrene.

[0095] When the one or more additives are selected from the group consisting of water, alcohols, organic polymers, and mixtures of two or more thereof, it is preferred that in the mixture the mass ratio of the zeolite material to the one or more additives is in the range of 0.3:1 to 1:1, more preferably in the range of 0.4:1 to 0.8:1, more preferably in the range of 0.5:1 to 0.6:1.

[0096] When the one or more additives comprise a cellulose derivative, preferably a cellulose ether, more preferably carboxymethylcellulose, it is preferred that in the mixture the mass ratio of zeolitic material to cellulose derivative, preferably a cellulose ether, more preferably carboxymethylcellulose, is in the range of 10:1 to 53:1, more preferably in the range of 15:1 to 40:1, more preferably in the range of 20:1 to 35:1.

[0097] When the one or more additives include polyethylene oxide, it is preferred that the mass ratio of zeolitic material to polyethylene oxide in the mixture is in the range of 70:1 to 110:1, more preferably in the range of 75:1 to 100:1, more preferably in the range of 77:1 to 98:1.

[0098] When the one or more additives include polystyrene, it is preferred that the mass ratio of zeolitic material to polystyrene in the mixture is in the range of 2:1 to 8:1, more preferably in the range of 3:1 to 6:1, more preferably in the range of 3.5:1 to 5:1.

[0099] When the one or more additives comprise water, it is preferred that the mass ratio of zeolitic material to water in the mixture is in the range of 0.7:1 to 0.85:1, more preferably in the range of 0.72:1 to 0.8:1, more preferably in the range of 0.74:1 to 0.79:1.

[0100] It is particularly preferred that the one or more additives include a cellulose derivative, preferably a cellulose ether, more preferably carboxymethyl cellulose, polyethylene oxide, polystyrene, and water.

[0101] According to a further aspect, the present invention relates to a method for producing a mixture comprising a zeolitic material, water and silica, preferably a mixture as described above, said method comprising the steps of: (i') providing a zeolitic material exhibiting a type I nitrogen adsorption / desorption isotherm, determined as described in Reference Example 1, and having framework type MFI and a framework structure comprising Si, O and Ti; (ii') providing a colloidal dispersion of silica in water, said silica exhibiting a volume-based particle size distribution, determined as described in Reference Example 5, characterized by a Dv10 value of at least 35 nanometers, preferably in the range of 35 to 80 nanometers, more preferably in the range of 40 to 75 nanometers, more preferably in the range of 45 to 70 nanometers, a Dv50 value of at least 45 nanometers, preferably in the range of 45 to 125 nanometers, more preferably in the range of 55 to 115 nanometers, more preferably in the range of 65 to 105 nanometers, and a Dv90 value of at least 65 nanometers, preferably in the range of 65 to 200 nanometers, more preferably in the range of 85 to 180 nanometers, more preferably in the range of 95 to 160 nanometers, (iii') preparing a mixture comprising particles of the zeolitic material provided in step (i') and the binder precursor provided in step (ii').

[0102] The volume-based particle size distribution of the colloidal dispersion of silica in water according to step (ii'), determined as described in Reference Example 5, is preferably characterized by a Dv10 value in the range of 35 to 80 nanometers, preferably in the range of 40 to 75 nanometers, more preferably in the range of 45 to 70 nanometers, a Dv50 value in the range of 45 to 125 nanometers, preferably in the range of 55 to 115 nanometers, more preferably in the range of 65 to 105 nanometers, and a Dv90 value in the range of 65 to 200 nanometers, preferably in the range of 85 to 180 nanometers, more preferably in the range of 95 to 160 nanometers.

[0103] Furthermore, it is preferred that the volume-based particle size distribution of the colloidal dispersion of silica in water according to step (ii') is a unimodal distribution.

[0104] With regard to the content of silica contained in the colloidal dispersion of silica in water, it is preferred that the colloidal dispersion of silica in water from step (ii') comprises silica in an amount in the range of 25 to 65% by weight, more preferably in the range of 30 to 60% by weight, more preferably in the range of 35 to 55% by weight, based on the total weight of silica and water.

[0105] It is preferred that 95 to 100% by weight, more preferably 98 to 100% by weight, more preferably 99 to 100% by weight of the binder precursor from step (ii') consists of a colloidal dispersion of silica in water.

[0106] Furthermore, it is preferred that 95 to 100 mass %, more preferably 98 to 100 mass %, more preferably 99 to 100 mass %, more preferably at least 99.5 to 100 mass %, more preferably 99.9 to 100 mass %, of the zeolitic material from step (i') is composed of Si, O, Ti, and preferably H.

[0107] No particular limitation is applied regarding the amount of Ti contained in the zeolitic material from step (i'). It is preferred that the zeolitic material from step (i') contains Ti in an amount in the range of 0.2 to 5 mass %, preferably in the range of 0.5 to 4 mass %, more preferably in the range of 1.0 to 3 mass %, more preferably in the range of 1.2 to 2.5 mass %, more preferably in the range of 1.4 to 2.2 mass %, based on the total mass of the zeolitic material.

[0108] Preferably, the zeolitic material from step (i') is titanium silicalite-1.

[0109] With respect to the mass ratio of the zeolite material to the total of the zeolite material and the binder calculated as SiO2, in the mixture prepared in step (iii'), it is preferred that the mass ratio of the zeolite material to the total of the zeolite material and the binder calculated as SiO2 is in the range of 2 to 90%, more preferably in the range of 5 to 70%, more preferably in the range of 10 to 50%, more preferably in the range of 15 to 30%, more preferably in the range of 20 to 25%.

[0110] The mixture prepared according to step (iii') may comprise further components. It is preferred that the mixture prepared according to step (iii') further comprises one or more additives, more preferably one or more viscosity modifiers, or one or more mesopore formers, or one or more viscosity modifiers and one or more mesopore formers.

[0111] When the mixture prepared in step (iii') further contains one or more additives, it is preferable that 95 to 100 mass%, more preferably 98 to 100 mass%, more preferably 99 to 100 mass%, more preferably 99.5 to 100 mass%, more preferably 99.9 to 100 mass% of the mixture prepared in step (iii') consists of the zeolite material, the binder precursor, and the one or more additives.

[0112] It is preferred that the one or more additives are selected from the group consisting of water, alcohol, organic polymers, and mixtures of two or more thereof, the organic polymer is preferably selected from the group consisting of cellulose, cellulose derivatives, starch, polyalkylene oxides, polystyrene, polyacrylates, polymethacrylates, polyolefins, polyamides, polyesters, and mixtures of two or more thereof, the organic polymer is more preferably selected from the group consisting of cellulose ethers, polyalkylene oxides, polystyrene, and mixtures of two or more thereof, the organic polymer is more preferably selected from the group consisting of methylcellulose, carboxymethylcellulose, polyethylene oxide, polystyrene, and mixtures of two or more thereof, and more preferably the one or more additives comprise, more preferably consist of, water, carboxymethylcellulose, polyethylene oxide, and polystyrene.

[0113] When the mixture prepared in step (iii') comprises one or more additives, it is preferred that the mass ratio of the zeolitic material to the one or more additives in the mixture prepared in step (iii') is in the range of 0.3:1 to 1:1, more preferably in the range of 0.4:1 to 0.8:1, more preferably in the range of 0.5:1 to 0.6:1.

[0114] When the mixture prepared by step (iii) and subjected to step (iv) comprises a cellulose derivative, preferably a cellulose ether, more preferably carboxymethylcellulose, it is preferred that in the mixture prepared by step (iii) and subjected to step (iv), the mass ratio of zeolitic material to the cellulose derivative, preferably a cellulose ether, more preferably carboxymethylcellulose, is in the range of 10:1 to 53:1, more preferably in the range of 15:1 to 40:1, more preferably in the range of 20:1 to 35:1.

[0115] When the mixture prepared by step (iii) and subjected to step (iv) contains polyethylene oxide, it is preferred that the mass ratio of zeolitic material to polyethylene oxide in the mixture prepared by step (iii) and subjected to step (iv) is in the range of 70:1 to 110:1, more preferably in the range of 75:1 to 100:1, more preferably in the range of 77:1 to 98:1.

[0116] When the mixture prepared by step (iii) and subjected to step (iv) contains water, it is preferred that the mass ratio of zeolitic material to water in the mixture prepared by step (iii) and subjected to step (iv) is in the range of 0.7:1 to 0.85:1, more preferably in the range of 0.72:1 to 0.8:1, more preferably in the range of 0.74:1 to 0.79:1.

[0117] Preferably, the preparation of the mixture according to step (iii) comprises mixing in a kneader or mixing muller.

[0118] Further, the method for producing a mixture comprising zeolitic material, water and silica described herein preferably comprises steps (i), (ii) and (iii).

[0119] According to yet a further aspect of the present invention, the present invention relates to a mixture obtainable or obtained by the process described herein, preferably a mixture as described herein.

[0120] The present invention is further illustrated by the following embodiments and combinations of embodiments, as indicated by the dependency and back references. In particular, in each instance where a range of embodiments is mentioned, it is to be noted that in the context of a term such as "the molded article according to any one of embodiments 1 to 4", all embodiments within this range are intended to be expressly disclosed to those skilled in the art, i.e., the wording of this term is understood by those skilled in the art to be equivalent to "the method according to any one of embodiments 1, 2, 3, and 4". Furthermore, it is to be expressly noted that the set of the following embodiments represents a suitably constructed part of the description directed to the general and preferred aspects of the present invention, rather than the combination of claims that determines the scope of protection.

[0121] 1. A chemical molded article comprising a zeolite material exhibiting a type I nitrogen adsorption / desorption isotherm as determined in Reference Example 1 and having a framework type MFI and a framework structure comprising Si, O and Ti, the molded article further comprising a binder for the zeolite material, the binder comprising Si and O, the molded article exhibiting a total pore volume of at least 0.4 mL / g as determined in Reference Example 2, and a breaking strength of at least 6 N as determined in Reference Example 3.

[0122] 2. The molded article according to embodiment 1, wherein 95 to 100% by mass, preferably 98 to 100% by mass, more preferably 99 to 100% by mass, more preferably at least 99.5 to 100% by mass, more preferably 99.9 to 100% by mass of the zeolite material contained in the molded article is composed of Si, O, Ti, and optionally H.

[0123] 3. The molded article according to embodiment 1 or 2, wherein the zeolitic material contains Ti in an amount in the range of 0.2 to 5% by mass, calculated as elemental Ti and based on the total mass of the zeolitic material, preferably in the range of 0.5 to 4% by mass, more preferably in the range of 1.0 to 3% by mass, more preferably in the range of 1.2 to 2.5% by mass, more preferably in the range of 1.4 to 2.2% by mass.

[0124] 4. The molded article of any one of the preceding claims, wherein the zeolitic material contained in the molded article is titanium silicalite-1.

[0125] 5. The molded article according to any one of embodiments 1 to 4, wherein 95 to 100% by mass, preferably 98 to 100% by mass, more preferably 99 to 100% by mass, more preferably at least 99.5 to 100% by mass, more preferably 99.9 to 100% by mass of the binder contained in the molded article is composed of Si and O.

[0126] 6. The molded article according to any one of the preceding claims, comprising a binder in an amount, calculated as SiO2, in the range of 2 to 90% by mass, preferably in the range of 5 to 70% by mass, more preferably in the range of 10 to 50% by mass, more preferably in the range of 15 to 30% by mass, more preferably in the range of 20 to 25% by mass, based on the total mass of the molded article.

[0127] 7. The molded article according to any one of embodiments 1 to 6, wherein 95 to 100% by mass, preferably 98 to 100% by mass, more preferably 99 to 100% by mass, more preferably at least 99.5 to 100% by mass, more preferably 99.9 to 100% by mass of the molded article consists of the zeolite material and the binder.

[0128] 8. The molded article according to any one of the preceding claims, comprising micropores having a pore diameter in the range of 0.1 to less than 2 nm, as determined in Reference Example 4, and mesopores having a pore diameter in the range of 2 to 50 nm, as determined in Reference Example 4.

[0129] 9. The molded article according to any one of the preceding embodiments, having a total pore volume in the range of 0.4 to 1.5 mL / g, preferably in the range of 0.4 to 1.2 mL / g, more preferably in the range of 0.4 to 1.0 mL / g.

[0130] 10. The molded article according to any one of the preceding embodiments, exhibiting a breaking strength in the range of 6 to 25 N, preferably in the range of 7 to 20 N, more preferably in the range of 8 to 15 N.

[0131] 11. The shaped article of any one of the preceding embodiments, which is a strand having a hexagonal, rectangular, quadratic, triangular, elliptical, or circular cross-section, more preferably a circular cross-section.

[0132] 12. The molded article according to embodiment 11, having a cross-sectional diameter in the range of 0.5 to 5 mm, preferably in the range of 1 to 3 mm, and more preferably in the range of 1.5 to 2 mm.

[0133] 13. The shaped article according to any one of the preceding embodiments, preferably 11 or 12, which is an extrudate.

[0134] 14. The molded article according to any one of embodiments 1 to 13, having a tortuosity parameter for water, determined as described in Reference Example 11, in the range of 1.0 to 2.5, preferably in the range of 1.3 to 2.0, more preferably in the range of 1.6 to 1.8, more preferably in the range of 1.6 to 1.75, and more preferably in the range of 1.6 to 1.72.

[0135] 15. The BET specific surface area is determined as described in Reference Example 6 and is 300 to 450 m 2 / g, preferably 310 to 400m 2 / g, more preferably 320 to 375 m 2 15. The article of any one of the preceding claims, wherein the average molecular weight is in the range of 1 / g.

[0136] 16. The molded article according to any one of embodiments 1 to 15, having a crystallinity, determined as described in Reference Example 7, in the range of 50 to 100%, preferably in the range of 50 to 90%, more preferably in the range of 50 to 80%.

[0137] 17. The molded article according to any one of the preceding embodiments, having a propylene oxide activity, determined as described in Reference Example 9, of at least 4.5% by weight, preferably in the range of 4.5 to 11% by weight, more preferably in the range of 4.5 to 10% by weight.

[0138] 18. The molded article according to any one of the preceding embodiments, having a pressure drop rate, determined as described in Reference Example 9, in the range of 0.005 to 0.019 bar(abs) / min, preferably in the range of 0.006 to 0.017 bar(abs) / min, more preferably in the range of 0.007 to 0.015 bar(abs) / min.

[0139] 19. The molded article according to any one of the preceding claims for use as a catalyst in a reaction for preparing propylene oxide from propene and hydrogen peroxide, wherein the catalyst exhibits a hydrogen peroxide conversion in the range of 90-95%, determined in a continuous epoxidation reaction as described in Reference Example 10, the cooling medium temperature is in the range of 55-56°C, the on-stream time is in the range of 200-600 hours, preferably the on-stream time is in the range of 300-600 hours, more preferably the on-stream time is in the range of 350-600 hours, and the term "on-stream time" refers to the duration of the continuous epoxidation reaction without catalyst regeneration.

[0140] 20. A method for producing a chemical molded article comprising a zeolitic material having a nitrogen adsorption / desorption isotherm of type I, determined as described in Reference Example 1, and having a framework type MFI and a framework structure comprising Si, O and Ti, the molded article further comprising a binder for the zeolitic material, the binder comprising Si and O, preferably a molded article according to any one of the preceding claims, comprising the steps of: (i) providing a zeolitic material exhibiting a type I nitrogen adsorption / desorption isotherm, determined as described in Reference Example 1, and having framework type MFI and a framework structure comprising Si, O and Ti; (ii) providing a binder precursor comprising a colloidal dispersion of silica in water, said binder precursor exhibiting a volume-based particle size distribution characterized by a Dv10 value of at least 35 nanometers, a Dv50 value of at least 45 nanometers, and a Dv90 value of at least 65 nanometers, determined as described in Example 5; (iii) preparing a mixture comprising the zeolitic material provided in step (i) and the binder precursor provided in step (ii); (iv) molding the mixture obtained from step (iii) to obtain a precursor of a molded article; (v) preparing a mixture comprising the precursor of the shaped article obtained from step (iv) and water, and subjecting the mixture to a water treatment under hydrothermal conditions to obtain a water-treated precursor of the shaped article; (vi) Calcining the water-treated precursor of the molded article in a gas atmosphere to obtain the molded article. A manufacturing method comprising:

[0141] 21. The method according to embodiment 20, wherein the volume-based particle size distribution of the colloidal dispersion of silica in water according to step (ii), determined as described in Example 5, is characterized by a Dv10 value in the range of 35 to 80 nanometers, preferably in the range of 40 to 75 nanometers, more preferably in the range of 45 to 70 nanometers, a Dv50 value in the range of 45 to 125 nanometers, preferably in the range of 55 to 115 nanometers, more preferably in the range of 65 to 105 nanometers, and a Dv90 value in the range of 65 to 200 nanometers, preferably in the range of 85 to 180 nanometers, more preferably in the range of 95 to 160 nanometers.

[0142] 22. The method of embodiment 20 or 21, wherein the volume-based particle size distribution of the colloidal dispersion of silica in water according to step (ii) is a monomodal distribution.

[0143] 23. The method according to any one of embodiments 20 to 22, wherein the colloidal dispersion of silica in water in step (ii) comprises silica in an amount in the range of 25 to 65% by weight, preferably in the range of 30 to 60% by weight, more preferably in the range of 35 to 55% by weight, based on the combined weight of silica and water.

[0144] 24. The method according to any one of embodiments 20 to 23, wherein 95 to 100% by weight, preferably 98 to 100% by weight, more preferably 99 to 100% by weight, of the binder precursor from step (ii) consists of a colloidal dispersion of silica in water.

[0145] 25. The method according to any one of embodiments 20 to 24, wherein 95 to 100% by weight, preferably 98 to 100% by weight, more preferably 99 to 100% by weight, more preferably at least 99.5 to 100% by weight, more preferably 99.9 to 100% by weight, of the zeolitic material from step (i) consists of Si, O, Ti, and preferably H.

[0146] 26. The method according to any one of embodiments 20 to 25, wherein the zeolitic material from step (i) comprises Ti in an amount in the range of 0.2 to 5% by weight, preferably in the range of 0.5 to 4% by weight, more preferably in the range of 1.0 to 3% by weight, more preferably in the range of 1.2 to 2.5% by weight, more preferably in the range of 1.4 to 2.2% by weight, based on the total weight of the zeolitic material.

[0147] 27. The method of any one of embodiments 20 to 26, wherein the zeolitic material from step (i) is titanium silicalite-1.

[0148] 28. The method according to any one of embodiments 20 to 27, wherein in the mixture prepared by step (iii) and subjected to step (iv), the mass ratio of the zeolitic material relative to the total of the zeolitic material and the binder, calculated as SiO2, is in the range of 2 to 90%, preferably in the range of 5 to 70%, more preferably in the range of 10 to 50%, more preferably in the range of 15 to 30%, more preferably in the range of 20 to 25%.

[0149] 29. The method of any one of embodiments 20 to 28, wherein the mixture prepared by step (iii) and subjected to step (iv) further comprises one or more additives, preferably one or more viscosity modifiers, or one or more mesopore formers, or one or more viscosity modifiers and one or more mesopore formers.

[0150] 30. The method of embodiment 29, wherein 95 to 100% by weight, preferably 98 to 100% by weight, more preferably 99 to 100% by weight, more preferably 99.5 to 100% by weight, more preferably 99.9 to 100% by weight of the mixture prepared in step (iii) and subjected to step (iv) consists of the zeolitic material, the binder precursor, and one or more additives.

[0151] 31. The method of embodiment 29 or 30, wherein the one or more additives are selected from the group consisting of water, alcohol, organic polymers, and mixtures of two or more thereof; the organic polymer is preferably selected from the group consisting of cellulose, cellulose derivatives, starch, polyalkylene oxides, polystyrene, polyacrylates, polymethacrylates, polyolefins, polyamides, polyesters, and mixtures of two or more thereof; the organic polymer is more preferably selected from the group consisting of cellulose ethers, polyalkylene oxides, polystyrene, and mixtures of two or more thereof; the organic polymer is more preferably selected from the group consisting of methylcellulose, carboxymethylcellulose, polyethylene oxide, polystyrene, and mixtures of two or more thereof; more preferably the one or more additives comprise, more preferably consist of, water, carboxymethylcellulose, polyethylene oxide, and polystyrene.

[0152] 32. The method of any one of embodiments 29 to 31, wherein in the mixture prepared by step (iii) and subjected to step (iv), the mass ratio of zeolitic material to the one or more additives is in the range of 0.3:1 to 1:1, preferably in the range of 0.4:1 to 0.8:1, and more preferably in the range of 0.5:1 to 0.6:1.

[0153] 33. In the mixture prepared by step (iii) and subjected to step (iv), the mass ratio of the zeolitic material to the cellulose derivative, preferably cellulose ether, more preferably carboxymethylcellulose, is in the range of 10:1 to 53:1, preferably in the range of 15:1 to 40:1, more preferably in the range of 20:1 to 35:1; the mass ratio of the zeolite material to the polyethylene oxide is in the range of 70:1 to 110:1, preferably in the range of 75:1 to 100:1, more preferably in the range of 77:1 to 98:1; the mass ratio of the zeolite material to the polystyrene is in the range of 2:1 to 8:1, preferably in the range of 3:1 to 6:1, more preferably in the range of 3.5:1 to 5:1; The mass ratio of the zeolite material to water is in the range of 0.7:1 to 0.85:1, preferably in the range of 0.72:1 to 0.8:1, more preferably in the range of 0.74:1 to 0.79:1. 33. A method according to any one of embodiments 29 to 32.

[0154] 34. The method of any one of embodiments 20 to 33, wherein the preparation of the mixture according to step (iii) comprises mixing in a kneader or mixing muller.

[0155] 35. The method according to any one of embodiments 20 to 34, wherein step (iv) forms the mixture resulting from step (iii) into strands, preferably strands having a circular cross-section, wherein the strands having a circular cross-section preferably have a diameter in the range of 0.5 to 5 mm, more preferably in the range of 1 to 3 mm, more preferably in the range of 1.5 to 2 mm.

[0156] 36. The method according to any one of embodiments 20 to 35, wherein the mixture prepared by step (iii) and subjected to step (iv) has a plasticity, determined as described in Reference Example 12, in the range of 500 to 3000 N, preferably in the range of 750 to 2000 N, more preferably in the range of 1000 to 1500 N.

[0157] 37. The method of any one of embodiments 20 to 36, wherein the shaping according to step (iv) comprises extruding the mixture resulting from step (iii).

[0158] 38. The method according to any one of embodiments 20 to 37, wherein the shaping according to step (iv) further comprises drying the precursor of the shaped article in a gas atmosphere, the drying being preferably carried out at a temperature of the gas atmosphere in the range of 80 to 160°C, preferably in the range of 100 to 140°C, more preferably in the range of 110 to 130°C, the gas atmosphere preferably comprising nitrogen, oxygen or a mixture thereof, the gas atmosphere being more preferably oxygen, air or lean air.

[0159] 39. The method according to any one of embodiments 20 to 36, wherein the shaping according to step (iv) further comprises a step of preferably calcining the dried precursor of the shaped body in a gas atmosphere, and the calcination is preferably carried out at a temperature of the gas atmosphere of 450 to 530° C., more preferably 470 to 510° C., more preferably 480 to 500° C., and the gas atmosphere is preferably nitrogen, oxygen or a mixture thereof, and the gas atmosphere is more preferably oxygen, air or lean air.

[0160] 40. The method of any one of embodiments 20 to 39, wherein in the mixture prepared in step (v), the mass ratio of the precursor of the shaped article to water is in the range of 1:1 to 1:30, preferably in the range of 1:5 to 1:25, and more preferably in the range of 1:10 to 1:20.

[0161] 41. The method according to any one of embodiments 20 to 40, wherein 95 to 100% by mass, preferably 98 to 100% by mass, more preferably 99 to 100% by mass, more preferably 99.5 to 100% by mass, more preferably 99.9 to 100% by mass of the mixture prepared in step (v) consists of precursors of the shaped article and water.

[0162] 42. The process according to any one of embodiments 20 to 41, wherein the water treatment according to step (v) comprises a temperature of the mixture in the range of 100 to 200°C, preferably in the range of 125 to 175°C, more preferably in the range of 130 to 160°C, more preferably in the range of 135 to 155°C, more preferably in the range of 140 to 150°C.

[0163] 43. The method of any one of embodiments 20 to 42, wherein the water treatment according to step (v) is carried out under autogenous pressure, preferably in an autoclave.

[0164] 44. The method according to any one of embodiments 20 to 43, wherein the water treatment in step (v) is carried out for 6 to 10 hours, preferably 7 to 9 hours, more preferably 7.5 to 8.5 hours.

[0165] 45. The method of any one of embodiments 20 to 44, wherein step (v) comprises separating the water-treated precursor of the shaped article from the mixture resulting from the water treatment.

[0166] 46. ​​The method of embodiment 45, wherein separating the precursor of the water-treated shaped article from the mixture resulting from the water treatment comprises subjecting the mixture resulting from the water treatment to solid-liquid separation, preferably washing the separated precursor, and preferably drying the washed precursor.

[0167] 47. The method of embodiment 46, wherein the solid-liquid separation according to step (v) comprises filtration, or centrifugation, or filtration and centrifugation.

[0168] 48. The method according to claim 46 or 47, wherein the washing according to step (v) comprises at least one washing of the precursor with a liquid solvent system, the liquid solvent system preferably comprising one or more of water, alcohol and mixtures of two or more thereof, and the water-treated precursor of the shaped article is more preferably washed with water.

[0169] 49. The method according to any one of embodiments 46 to 48, wherein the drying according to step (v) comprises drying the precursor in a gas atmosphere, and the drying is more preferably carried out at a temperature of the gas atmosphere in the range of 80 to 160° C., more preferably in the range of 100 to 140° C., more preferably in the range of 110 to 130° C., and the gas atmosphere preferably comprises nitrogen, oxygen, or a mixture thereof, and the gas atmosphere is more preferably oxygen, air, or lean air.

[0170] 50. The process according to any one of embodiments 20 to 49, wherein the calcination according to step (vi) is carried out at a temperature in a gas atmosphere in the range of 400 to 490° C., preferably in the range of 420 to 470° C., more preferably in the range of 440 to 460° C., the gas atmosphere preferably comprising nitrogen, oxygen, or a mixture thereof, and more preferably the gas atmosphere is oxygen, air, or lean air.

[0171] 51. The method according to any one of embodiments 20 to 50, comprising steps (i), (ii), (iii), (iv), (v) and (vi).

[0172] 52. A chemical molding comprising particles of a zeolitic material having a type I nitrogen adsorption / desorption isotherm determined as described in Reference Example 1 and having a framework type MFI and a framework structure comprising Si, O and Ti, the molding further comprising a binder for the particles, the binder comprising Si and O, preferably the chemical molding according to any one of embodiments 1 to 19, obtainable or obtained by the method according to any one of embodiments 20 to 51.

[0173] 53. Use of a shaped article according to any one of embodiments 1 to 19 or according to embodiment 52 as an adsorbent, absorbent, catalyst or catalyst component, preferably as a catalyst or catalyst component, more preferably as a Lewis acid catalyst or Lewis acid catalyst component, as an isomerization catalyst or isomerization catalyst component, as an oxidation catalyst or oxidation catalyst component, as an aldol condensation catalyst or aldol condensation catalyst component, or as a Prins reaction catalyst or Prins reaction catalyst component.

[0174] 54. The use according to embodiment 53 as an oxidation catalyst or as an oxidation catalyst component, preferably as an epoxidation catalyst or as an epoxidation catalyst component, more preferably as an epoxidation catalyst.

[0175] 55. The use according to embodiment 54 of an organic compound having at least one C-C double bond, preferably a C2-C10 alkene, more preferably a C2-C5 alkene, more preferably a C2-C4 alkene, more preferably a C2 or C3 alkene, more preferably for the epoxidation of propene, more preferably for the epoxidation of propene with hydrogen peroxide as oxidant, more preferably for the epoxidation of propene with hydrogen peroxide as oxidant in a solvent comprising an alcohol, preferably methanol.

[0176] 56. A process for oxidizing an organic compound, preferably for epoxidizing an organic compound, more preferably for epoxidizing an organic compound having at least one C-C double bond, preferably a C2-C10 alkene, more preferably a C2-C5 alkene, more preferably a C2-C4 alkene, more preferably a C2 or C3 alkene, more preferably propene, comprising contacting the organic compound, preferably in a continuous mode, with a catalyst according to any one of embodiments 1 to 19, or comprising a shaped article according to embodiment 52.

[0177] 57. The method of embodiment 56, wherein hydrogen peroxide is used as the oxidizing agent, and the oxidation reaction is preferably carried out in a solvent, more preferably in a solvent comprising an alcohol, preferably methanol.

[0178] 58. A process for producing propylene oxide, comprising reacting propene, preferably in a continuous mode, in a methanol solution with hydrogen peroxide in the presence of a catalyst comprising a shaped article according to any one of embodiments 1 to 19 or according to embodiment 52 to obtain propylene oxide.

[0179] 59. A method for preparing a chemical molded article, preferably for preparing a molded article according to any one of embodiments 1 to 19, comprising using a colloidal dispersion of silica in water as a binder precursor, comprising a zeolitic material having a nitrogen adsorption / desorption isotherm of type I, determined as described in Reference Example 1, and having a framework MFI and a framework structure comprising Si, O and Ti, and further comprising a binder obtained from said binder precursor, wherein said silica has a Dv10 of at least 35 nanometers, preferably in the range of 35 to 80 nanometers, more preferably in the range of 40 to 75 nanometers, more preferably in the range of 45 to 70 nanometers, determined as described in Reference Example 5. a volume-based particle size distribution characterized by a Dv50 value of at least 45 nanometers, preferably in the range of 45 to 125 nanometers, more preferably in the range of 55 to 115 nanometers, more preferably in the range of 65 to 105 nanometers, and a Dv90 value of at least 65 nanometers, preferably in the range of 65 to 200 nanometers, more preferably in the range of 85 to 180 nanometers, more preferably in the range of 95 to 160 nanometers, and said molded article preferably exhibits a total pore volume of at least 0.4 mL / g, determined as described in Reference Example 2, and a breaking strength of at least 6 N, determined as described in Reference Example 3.

[0180] The present invention is further illustrated by the following further embodiments and combinations of embodiments, as indicated by the dependency and back reference. In particular, in each instance where a range of embodiments is mentioned, it is to be noted that in the context of a term such as "a mixture according to any one of embodiments 1' to 4'", all embodiments within this range are intended to be expressly disclosed to those skilled in the art, i.e., the wording of this term is understood by those skilled in the art to be equivalent to "a mixture according to any one of embodiments 1', 2', 3', and 4'". Furthermore, it is to be expressly noted that the following set of embodiments represents a suitably constructed part of the description directed to the general and preferred aspects of the present invention, rather than the combination of claims that determines the scope of protection.

[0181] 1'. A mixture comprising a zeolitic material exhibiting a Type I nitrogen adsorption / desorption isotherm as determined as described in Reference Example 1 and having a framework type MFI and a framework structure comprising Si, O and Ti, the mixture further comprising a colloidal dispersion of silica in water, the binder precursor exhibiting a volume-based particle size distribution characterized by a Dv10 value of at least 35 nanometers, a Dv50 value of at least 45 nanometers, and a Dv90 value of at least 65 nanometers as determined as described in Reference Example 5.

[0182] 2'. The mixture according to embodiment 1', having a plasticity, determined as described in Reference Example 12, in the range of 500 to 3000 N, preferably in the range of 750 to 2000 N, more preferably in the range of 1000 to 1500 N.

[0183] 3'. The mixture according to embodiment 1' or 2', wherein the volume-based particle size distribution of the colloidal dispersion of silica in water, determined as described in Example 5, is characterized by a Dv10 value in the range of 35 to 80 nanometers, preferably in the range of 40 to 75 nanometers, more preferably in the range of 45 to 70 nanometers, a Dv50 value in the range of 45 to 125 nanometers, preferably in the range of 55 to 115 nanometers, more preferably in the range of 65 to 105 nanometers, and a Dv90 value in the range of 65 to 200 nanometers, preferably in the range of 85 to 180 nanometers, more preferably in the range of 95 to 160 nanometers.

[0184] 4'. The mixture of any one of embodiments 1' to 3', wherein the volume-based particle size distribution of the colloidal dispersion of silica is unimodal.

[0185] 5'. The method of any one of embodiments 1' to 4', wherein the colloidal dispersion of silica in water comprises silica in an amount in the range of 25 to 65% by weight, preferably in the range of 30 to 60% by weight, more preferably in the range of 35 to 55% by weight, based on the combined weight of silica and water.

[0186] 6'. The method of any one of embodiments 1' to 5', wherein 95 to 100% by weight, preferably 98 to 100% by weight, more preferably 99 to 100% by weight of the binder precursor consists of a colloidal dispersion of silica in water.

[0187] 7'. The mixture according to any one of embodiments 1' to 6', wherein 95 to 100% by weight, preferably 98 to 100% by weight, more preferably 99 to 100% by weight, more preferably at least 99.5 to 100% by weight, more preferably 99.9 to 100% by weight of the zeolitic material consists of Si, O, Ti, and preferably H.

[0188] 8'. The method according to any one of embodiments 1' to 7', wherein the zeolitic material comprises Ti in an amount in the range of 0.2 to 5% by weight, preferably in the range of 0.5 to 4% by weight, more preferably in the range of 1.0 to 3% by weight, more preferably in the range of 1.2 to 2.5% by weight, more preferably in the range of 1.4 to 2.2% by weight, based on the total weight of the zeolitic material, and the zeolitic material is preferably titanium silicalite-1.

[0189] 9'. The mixture according to any one of embodiments 1' to 8', wherein the mass ratio of the zeolitic material in the mixture, based on the total of the zeolitic material and the binder, calculated as SiO2, is in the range of 2 to 90%, preferably in the range of 5 to 70%, more preferably in the range of 10 to 50%, more preferably in the range of 15 to 30%, more preferably in the range of 20 to 25%.

[0190] 10'. The mixture of any one of embodiments 1' to 9', further comprising one or more additives, preferably one or more viscosity modifiers, or one or more mesopore formers, or one or more viscosity modifiers and one or more mesopore formers.

[0191] 11'. The mixture according to any one of embodiments 1' to 10', wherein 95 to 100% by weight, preferably 98 to 100% by weight, more preferably 99 to 100% by weight, more preferably 99.5 to 100% by weight, more preferably 99.9 to 100% by weight of the mixture consists of the zeolite material, the binder precursor, and the one or more additives.

[0192] 12'. The mixture of any one of embodiments 1' to 11', wherein the one or more additives are selected from the group consisting of water, alcohol, organic polymers, and mixtures of two or more thereof; the organic polymer is preferably selected from the group consisting of cellulose, cellulose derivatives, starch, polyalkylene oxides, polystyrene, polyacrylates, polymethacrylates, polyolefins, polyamides, polyesters, and mixtures of two or more thereof; the organic polymer is more preferably selected from the group consisting of cellulose ethers, polyalkylene oxides, polystyrene, and mixtures of two or more thereof; the organic polymer is more preferably selected from the group consisting of methylcellulose, carboxymethylcellulose, polyethylene oxide, polystyrene, and mixtures of two or more thereof; and more preferably the one or more additives comprise, more preferably consist of, water, carboxymethylcellulose, polyethylene oxide, and polystyrene.

[0193] 13'. The method of embodiment 12', wherein in the mixture, the mass ratio of the zeolite material to the one or more additives is in the range of 0.3:1 to 1:1, preferably in the range of 0.4:1 to 0.8:1, and more preferably in the range of 0.5:1 to 0.6:1.

[0194] 14'. In the mixture: the mass ratio of the zeolitic material to the cellulose derivative, preferably cellulose ether, more preferably carboxymethylcellulose, is in the range of 10:1 to 53:1, preferably in the range of 15:1 to 40:1, more preferably in the range of 20:1 to 35:1; the mass ratio of the zeolite material to the polyethylene oxide is in the range of 70:1 to 110:1, preferably in the range of 75:1 to 100:1, more preferably in the range of 77:1 to 98:1; the mass ratio of the zeolite material to the polystyrene is in the range of 2:1 to 8:1, preferably in the range of 3:1 to 6:1, more preferably in the range of 3.5:1 to 5:1; The mass ratio of the zeolite material to water is in the range of 0.7:1 to 0.85:1, preferably in the range of 0.72:1 to 0.8:1, more preferably in the range of 0.74:1 to 0.79:1. A mixture according to embodiment 12' or 13'.

[0195] 15'. A method for producing a mixture comprising a zeolitic material, water, and silica, preferably a mixture as described in any one of embodiments 1' to 14', comprising the steps of: (i') providing a zeolitic material exhibiting a type I nitrogen adsorption / desorption isotherm, determined as described in Reference Example 1, and having framework type MFI and a framework structure comprising Si, O and Ti; (ii') providing a colloidal dispersion of silica in water, said silica exhibiting a volume-based particle size distribution, determined as described in Reference Example 5, characterized by a Dv10 value of at least 35 nanometers, preferably in the range of 35 to 80 nanometers, more preferably in the range of 40 to 75 nanometers, more preferably in the range of 45 to 70 nanometers, a Dv50 value of at least 45 nanometers, preferably in the range of 45 to 125 nanometers, more preferably in the range of 55 to 115 nanometers, more preferably in the range of 65 to 105 nanometers, and a Dv90 value of at least 65 nanometers, preferably in the range of 65 to 200 nanometers, more preferably in the range of 85 to 180 nanometers, more preferably in the range of 95 to 160 nanometers, (iii') preparing a mixture comprising particles of the zeolitic material provided in step (i') and the binder precursor provided in step (ii'). The method includes:

[0196] 16'. The method according to embodiment 15', wherein the volume-based particle size distribution of the colloidal dispersion of silica in water according to step (ii'), determined as described in Example 5, is characterized by a Dv10 value in the range of 35 to 80 nanometers, preferably in the range of 40 to 75 nanometers, more preferably in the range of 45 to 70 nanometers, a Dv50 value in the range of 45 to 125 nanometers, preferably in the range of 55 to 115 nanometers, more preferably in the range of 65 to 105 nanometers, and a Dv90 value in the range of 65 to 200 nanometers, preferably in the range of 85 to 180 nanometers, more preferably in the range of 95 to 160 nanometers.

[0197] 17'. The method of embodiment 15' or 16', wherein the volume-based particle size distribution of the colloidal dispersion of silica in water according to step (ii') is a monomodal distribution.

[0198] 18'. The method according to any one of embodiments 15' to 17', wherein the colloidal dispersion of silica in water from step (ii') comprises silica in an amount in the range of 25 to 65% by weight, preferably in the range of 30 to 60% by weight, more preferably in the range of 35 to 55% by weight, based on the combined weight of silica and water.

[0199] 19'. The method of any one of embodiments 15' to 18', wherein 95 to 100% by weight, preferably 98 to 100% by weight, more preferably 99 to 100% by weight, of the binder precursor from step (ii') consists of a colloidal dispersion of silica in water.

[0200] 20'. The method according to any one of embodiments 15' to 19', wherein 95 to 100% by weight, preferably 98 to 100% by weight, more preferably 99 to 100% by weight, more preferably at least 99.5 to 100% by weight, more preferably 99.9 to 100% by weight, of the zeolitic material from step (i') consists of Si, O, Ti, and preferably H.

[0201] 21'. The method according to any one of embodiments 15' to 20', wherein the zeolitic material from step (i') comprises Ti in an amount in the range of 0.2 to 5% by weight, preferably in the range of 0.5 to 4% by weight, more preferably in the range of 1.0 to 3% by weight, more preferably in the range of 1.2 to 2.5% by weight, more preferably in the range of 1.4 to 2.2% by weight, based on the total weight of the zeolitic material.

[0202] 22'. The method of any one of embodiments 15' to 21', wherein the zeolitic material from step (i') is titanium silicalite-1.

[0203] 23'. The method according to any one of embodiments 15' to 22', wherein in the mixture prepared in step (iii'), the mass ratio of the zeolitic material relative to the sum of the zeolitic material and the binder, calculated as SiO2, is in the range of 2 to 90%, preferably in the range of 5 to 70%, more preferably in the range of 10 to 50%, more preferably in the range of 15 to 30%, more preferably in the range of 20 to 25%.

[0204] 24'. The method of any one of embodiments 15' to 23', wherein the mixture prepared by step (iii') further comprises one or more additives, preferably one or more viscosity modifiers, or one or more mesopore formers, or one or more viscosity modifiers and one or more mesopore formers.

[0205] 25'. The method according to embodiment 24', wherein 95 to 100% by mass, preferably 98 to 100% by mass, more preferably 99 to 100% by mass, more preferably 99.5 to 100% by mass, more preferably 99.9 to 100% by mass of the mixture prepared in step (iii') consists of the zeolite material, the binder precursor, and one or more additives.

[0206] 26'. The method of embodiment 24' or 25', wherein the one or more additives are selected from the group consisting of water, alcohol, organic polymers, and mixtures of two or more thereof; the organic polymer is preferably selected from the group consisting of cellulose, cellulose derivatives, starch, polyalkylene oxides, polystyrene, polyacrylates, polymethacrylates, polyolefins, polyamides, polyesters, and mixtures of two or more thereof; the organic polymer is more preferably selected from the group consisting of cellulose ethers, polyalkylene oxides, polystyrene, and mixtures of two or more thereof; the organic polymer is more preferably selected from the group consisting of methylcellulose, carboxymethylcellulose, polyethylene oxide, polystyrene, and mixtures of two or more thereof; and more preferably the one or more additives comprise, more preferably consist of, water, carboxymethylcellulose, polyethylene oxide, and polystyrene.

[0207] 27'. The method of any one of embodiments 24' to 26', wherein in the mixture prepared by step (iii'), the mass ratio of zeolitic material to the one or more additives is in the range of 0.3:1 to 1:1, preferably in the range of 0.4:1 to 0.8:1, more preferably in the range of 0.5:1 to 0.6:1.

[0208] 28'. In the mixture prepared by step (iii) and subjected to step (iv), the mass ratio of the zeolitic material to the cellulose derivative, preferably cellulose ether, more preferably carboxymethylcellulose, is in the range of 10:1 to 53:1, preferably in the range of 15:1 to 40:1, more preferably in the range of 20:1 to 5:1; the mass ratio of the zeolite material to the polyethylene oxide is in the range of 70:1 to 110:1, preferably in the range of 75:1 to 100:1, more preferably in the range of 77:1 to 98:1; the mass ratio of the zeolite material to the polystyrene is in the range of 2:1 to 8:1, preferably in the range of 3:1 to 6:1, more preferably in the range of 3.5:1 to 5:1; The mass ratio of the zeolite material to water is in the range of 0.7:1 to 0.85:1, preferably in the range of 0.72:1 to 0.8:1, more preferably in the range of 0.74:1 to 0.79:1. A method according to any one of embodiments 24' to 27'.

[0209] 29'. The method of any one of embodiments 15' to 28', wherein the preparation of the mixture according to step (iii) comprises mixing in a kneader or mixing muller.

[0210] 30'. The method according to any one of embodiments 15' to 29', comprising steps (i), (ii) and (iii).

[0211] 31'. A mixture obtainable or obtained by a method according to any one of embodiments 15' to 29', preferably a mixture according to any one of embodiments 1' to 14'.

[0212] 32'. Use of a mixture according to any one of embodiments 1' to 14' or according to embodiment 31' for preparing a chemical article, preferably a chemical article according to any one of embodiments 1 to 19 or embodiment 52.

[0213] The present invention will be further described with reference to the following Reference Examples, Examples and Comparative Examples. EXAMPLES

[0214] Reference Example 1: Determination of N2 adsorption / desorption isotherms Nitrogen adsorption / desorption isotherms were measured at 77 K according to the method disclosed in DIN 66131. ​​The isotherms were measured at liquid nitrogen temperature using a Micrometrics ASAP2020M and Tristar system.

[0215] Reference Example 2: Determination of total pore volume The total pore volume was determined via mercury intrusion porosimetry in accordance with DIN 66133.

[0216] Reference Example 3: Determination of breaking strength The breaking strengths referred to in the context of the present invention are understood to be those determined by a breaking strength tester Z2.5 / TS1S (supplier: Zwick GmbH&Co., D-89079, Ulm, Germany). Regarding the principle of this machine and its operation, reference is made to the instruction manual "Register 1: Betriebsanleitung / Sicherheitshandbuch für die Material-Pruefmaschine Z2.5 / TS1S", edition 1.5, December 2001, by Zwick GmbH&Co., Technische Dokumentation, August-Nagel-Strasse 11, D-89079 Ulm, Germany, respectively. The machine is equipped with a fixed horizontal table on which the strands are placed. The strands are actuated against the fixed table by a plunger with a diameter of 3 mm, which is free to move vertically. The device is operated with a preload of 0.5 N, a shear rate under the preload of 10 mm / min, and a subsequent test rate of 1.6 mm / min. A vertically movable plunger was connected to a load cell for picking up the force and during the measurements, the strand was actuated against a fixed turntable on which the mouldings to be investigated (strands) were placed, by moving towards the table. The plunger was applied perpendicular to the longitudinal axis of the strand. With the machine, increasing forces were applied to a given strand, which will be described later, via the plunger until the strand broke. The force at which the strand broke is called the breaking strength of the strand. The control of the experiment was carried out using a computer which registered and evaluated the measurement results. The obtained value is the average value when in each case 10 strands were measured.

[0217] Reference Example 5: Determination of Dv10, Dv50, and Dv90 values Samples were analyzed using a Zetasizer Nano from Malvern Instruments GmbH, Herrenberg, Germany. First, the pH value of a given sample was determined so that it could be diluted in the same pH range. Samples were diluted to a measurement concentration of 0.005% with Millipore water at pH=9.1 and then filtered (5 micrometer). Measurements were performed at 25°C.

[0218] Reference Example 6: Determination of BET specific surface area The BET specific surface area was determined by nitrogen physical adsorption at 77 K according to the method disclosed in DIN 66131. ​​For the determination of the BET specific surface area, N2 sorption isotherms were measured at the temperature of liquid nitrogen using a Micrometrics ASAP2020M and Tristar system.

[0219] Reference Example 7: Powder X-ray diffraction and crystallinity determination Powder X-ray diffraction (PXRD) data were collected using a diffractometer (D8Advance Series II, Bruker AXS GmbH) equipped with a LYNXEYE detector operated with a copper anode X-ray tube operated at 40 kV and 40 mA, the geometry was Bragg-Brentano, and an air scattering shield was used to reduce air scattering.

[0220] Crystallinity calculation: The crystallinity of the samples was determined using the software DIFFRAC.EVA from Bruker AXS GmbH, Karlsruhe. The method is described in the user manual, page 121. Default parameters were used for the calculation.

[0221] Calculation of phase composition: The phase composition was calculated on the raw data using the software DIFFRAC.TOPAS from Bruker AXS GmbH, Karlsruhe. Using the identified crystal structures of the phases, the instrumental parameters and the crystallite sizes of the individual phases, a diffraction pattern was simulated. This was fitted to the data and a function was added to model the background intensity.

[0222] Data collection: Samples were homogenized in a mortar and then pressed into a standard flat sample holder provided by Bruker-AXS GmbH for Bragg-Brentano geometric data collection. A glass plate was used to compress and flatten the sample powder to achieve a flat surface. Data were collected in the 2-theta angle range of 2-70° with a 2-theta step size of 0.02° and the variable divergence slit was set at an angle of 0.1°. The crystalline content represents the intensity of the crystalline signal relative to the total scattered intensity (DIFFRAC.EVA User Manual, Bruker AXS GmbH, Karlsruhe).

[0223] Reference Example 8: Determination of C value (BET C constant) C values ​​were determined by the usual calculation ((slope / intercept)+1) based on a plot of the BET value 1 / (V((p / p0)-1)) versus p / p0, as known to those skilled in the art. p is the partial vapor pressure (in Pa) of the adsorbed gas in equilibrium with the surface at 77.4 K (bp of liquid nitrogen), p0 is the saturation pressure (in Pa) of the adsorbed gas, and V is the pressure at standard temperature and pressure (STP) [273.15 K and atmospheric pressure (1.013×10 5 is the volume of adsorbed gas in mL at 10 Pa.

[0224] Reference Example 9: Determination of Propylene Oxide Activity and Pressure Drop Rate (PO Test) In the PO test, a preliminary test procedure to evaluate the possible suitability of the molded articles as epoxidation catalysts for propene, the molded articles were tested in a glass autoclave by reacting propene with an aqueous hydrogen peroxide solution (30% by weight) to obtain propylene oxide. In particular, 0.5 g of the molded article was introduced together with 45 mL of methanol into a glass autoclave cooled to -25°C. 20 mL of liquid propene was forced into the glass autoclave, which was then heated to 0°C. At this temperature, 18 g of an aqueous hydrogen peroxide solution (30% by weight in water) was introduced into the glass autoclave. After 5 hours of reaction at 0°C, the mixture was heated to room temperature and analyzed by gas chromatography for the propylene oxide content of the liquid phase. The propylene oxide content of the liquid phase (in % by weight) is the result of the PO test, i.e. the propylene oxide activity of the molded article. The pressure drop rate was determined following the pressure progression during the abovementioned PO test. The progress of pressure was recorded using an S-11 transmitter (Wika Alexander Wiegand SE & Co. KG) placed in the pressure line of the autoclave and a graphic plotter Buddeberg 6100A. The obtained data were read out and a pressure rise curve was drawn. The pressure drop rate (PDR) was determined by the following formula: PDR = [p(max)-p(min)] / delta t During the ceremony, PDR / (bar / min) = Pressure Drop Rate p(max) / bar = maximum pressure at the start of the reaction p(min) / bar = minimum pressure observed during the reaction Delta t / min = the time difference between the start of the reaction and the time when p(min) is observed

[0225] Example 10: Determination of the performance of propylene epoxidation catalysts In a continuous epoxidation reaction setup, a vertically arranged tubular reactor (length: 1.4 m, external diameter 10 mm, internal diameter: 7 mm) equipped with a jacket for thermal stabilization was filled with 15 g of extrusions in the form of strands as described in each of the following examples. The remaining reactor volume was filled with inert material (steatite spheres with a diameter of 2 mm) up to a height of about 5 cm at the lower end of the reactor and the remainder at the upper end of the reactor. The following flow rates of starting materials were passed through the reactor: methanol (49 g / h), hydrogen peroxide (9 g / h, used as an aqueous hydrogen peroxide solution with a hydrogen peroxide content of 40% by weight), propylene (7 g / h, polymer grade). A cooling medium was passed through the cooling jacket to regulate the temperature of the reaction mixture so that the hydrogen peroxide conversion, determined on the basis of the reaction mixture leaving the reactor, was essentially constant at 90%. The pressure in the reactor was kept constant at 20 bar (abs) and the reaction mixture, except for the fixed bed catalyst, consisted of a single liquid phase. The reactor effluent downstream of the pressure control valve was collected, weighed and analyzed. Organic components were analyzed by two separate gas chromatographs. Hydrogen peroxide content was determined colorimetrically using the titanyl sulfate method. The selectivity for a given propylene oxide was determined relative to propene and hydrogen peroxide and was calculated as 100 times the ratio of the moles of propylene oxide in the effluent divided by the moles of propene or hydrogen peroxide in the feed.

[0226] Reference Example 11: Determination of tortuosity parameters for water Tortuosity parameters were measured as described in the experimental section of US20070099299A1. In particular, NMR analysis to do this was carried out at 25°C and 1 bar with a resonance frequency of 125 MHz 1H using a FEGRIS NT NMR spectrometer (see Stallmach et al., Annual Reports on NMR Spectroscopy 2007, Vol. 61, pp. 51-131). The pulse program used for the PFG NMR self-diffusion analysis was stimulated spin-echo with pulsed magnetic field gradient according to Figure 1b of US20070099299A1. For each sample, spin-echo decay curves were measured at different diffusion times (between 7 and 100 ms) by stepwise increasing the strength of the magnetic field gradient (up to a maximum of gmax = 10 T / m). From the spin-echo decay curves, the time dependence of the self-diffusion coefficient of the interstitial water was determined by equations (5) and (6) of US20070099299A1. Calculation of tortuosity: Time dependence of the mean second-order shift from the self-diffusion coefficient D(Δ) obtained by using equation (7) of US20070099299A1

number

number

number

number

[0227] Reference Example 12: Determination of plasticity The plasticity referred to in the context of the present invention is understood to be determined via a table-top testing machine Z010 / TN2S (supplier Zwick, D-89079 Ulm, Germany). Regarding the principle of this machine and its operation, reference is made to the instruction manual "Betriebsanleitung der Material-Pruefmaschine", edition 1.1, by Zwick Technische Dokumentation, August-Nagel-Strasse 11, D-89079 Ulm, Germany (1999), respectively. The Z010 testing machine is equipped with a fixed horizontal table on which a steel test vessel was placed, which contained a cylindrical section with an inner diameter of 26 mm and an internal height of 75 mm. The vessel was filled with the composition to be measured in such a way that the mass filled in the vessel did not contain air inclusions. The filling level was 10 mm below the upper end of the cylindrical section. Above the center of the cylindrical section of the vessel containing the composition to be measured was a plunger with a spherical lower end, the diameter of the sphere being 22.8 mm, which could be freely moved vertically. The plunger was attached to the load cell of a testing machine with a maximum test load of 10 kN. During the measurement, the plunger was moved vertically downwards and thus into the composition in the test vessel. Under the test conditions, the plunger was moved with a reserve force of 1.0 N, a reserve force speed of 100 mm / min and a subsequent test speed of 14 mm / min. The measurement was terminated when the measured force reached a value less than 70% of the maximum force previously measured in this measurement. The experiment was controlled by a computer which registered and evaluated the measurement results. The measured maximum force (F_max in N) corresponds to the plasticity referred to in the context of the present invention.

[0228] Example 1: Providing particles of a zeolitic material having a framework type MFI Titanium silicalite-1 (TS-1) powder was prepared according to the following recipe: TEOS (tetraethyl orthosilicate) (300 kg) was charged into a stirred tank reactor at room temperature and stirring (100 rpm) was started. In the second vessel, 60 kg TEOS and 13.5 kg TEOT (tetraethyl orthotitanate) were first mixed and then added to the TEOS in the first vessel. Then, another 360 kg TEOS was added to the mixture in the first vessel. Next, the contents of the first vessel were stirred for 10 minutes, after which 950 g TPAOH (tetrapropylammonium hydroxide) was added. Stirring was continued for 60 minutes. Ethanol released by hydrolysis was separated by distillation at a bottom temperature of 95 °C. Then, 300 kg water was added to the contents of the first vessel, and an amount of water equivalent to the amount of distillate was further added. The resulting mixture was stirred for 1 hour. Crystallization was carried out at 175 °C under autogenous pressure within 12 hours. The resulting titanium silicalite-1 crystals were isolated, dried and calcined in air for 6 hours at a temperature of 500° C. The resulting particles of zeolitic material exhibited a Ti content of 1.9% by mass, calculated as elemental Ti.

[0229] Example 2: Preparation of molded articles using colloidal silica binder precursors with particle size distribution according to the invention Forming: The particles of the zeolite material of Example 1 (105.3 g) and carboxymethylcellulose (4.0 g; Walocel™, Mw=15,000 g) were mixed in a kneader for 5 minutes. Then, an aqueous polystyrene dispersion (100.7 g; 33.7 g polystyrene) was added continuously. After 10 minutes, polyethylene oxide (1.33 g) was added. After 10 minutes, an aqueous colloidal silica binder precursor (70 g; 50 wt. % SiO2; Dv10=51 nm; Dv50=72 nm; Dv90=111; Nalco Chemical Co.) was added. After another 10 minutes, 10 mL of water was added, and after another 5 minutes, another 10 mL of water was added. The total kneading time was 40 minutes. The moldable mass obtained from the kneading, having a plasticity of 1283 N, was extruded at a pressure of 130 bar through a matrix with a circular hole having a diameter of 1.9 mm. The strand obtained was dried in an oven in air at a temperature of 120° C. for 4 hours and calcined in air at a temperature of 490° C. for 5 hours. The breaking strength of the strand, determined as described herein above, was 1.4 N.

[0230] Water treatment: 36 g of these strands were divided into 4 portions of 9 g each and mixed with 180 g of deionized water per portion. The mixture obtained was heated in an autoclave for 8 hours at a temperature of 145° C. Afterwards, the water-treated strands obtained were separated and sieved through a 0.8 mm sieve. Afterwards, the strands obtained were washed with deionized water and subjected to a nitrogen flow at ambient temperature. Each washed strand was subsequently dried in air at a temperature of 120° C. for 4 hours and then calcined in air at a temperature of 450° C. for 2 hours.

[0231] The resulting material had a TOC of less than 0.1 g / 100 g, a Si content of 44 g / 100 g, and a Ti content of 1.4 g / 100 g. The strand breaking strength, determined as described hereinabove, was 8 N, and the total pore volume, determined as described hereinabove, was 0.83 mL / g. The tortuosity parameter for water was 1.60. The BET specific surface area was 356 m 2 / g and the C value was -356.

[0232] Example 3: Preparation of molded articles using colloidal silica binder precursors with particle size distribution according to the invention Molding: The particles of the zeolitic material of Example 1 (105.3 g) and carboxymethylcellulose (4.0 g; Walocel™, Mw=15,000 g) were mixed in a kneader for 5 minutes. Then, an aqueous polystyrene dispersion (100.7 g; 33.7 g polystyrene) was added continuously. After 10 minutes, polyethylene oxide (1.33 g) was added. After 10 minutes, an aqueous colloidal silica binder precursor (70 g; 40% by weight SiO2; Dv10=68 nm; Dv50=97 nm; Dv90=151 nm; Nalco Chemical Co.) was added. After another 10 minutes, 20 mL of water was added. The total mixing time was 35 minutes. The moldable mass obtained from the mixing was extruded at a pressure of 150 bar through a matrix with circular holes of 1.9 mm in diameter. The resulting strands were dried in an oven in air at a temperature of 120° C. for 4 hours and calcined in air at a temperature of 490° C. for 5 hours. The breaking strength of the strands, determined as described above herein, was 1.0 N.

[0233] Water treatment: 36 g of these strands were divided into 4 portions of 9 g each and mixed with 180 g of deionized water per portion. The mixture obtained was heated in an autoclave for 8 hours at a temperature of 145° C. Afterwards, the water-treated strands obtained were separated and sieved through a 0.8 mm sieve. Afterwards, the strands obtained were washed with deionized water and subjected to a nitrogen flow at ambient temperature. Each washed strand was subsequently dried in air at a temperature of 120° C. for 4 hours and then calcined in air at a temperature of 450° C. for 2 hours.

[0234] The resulting material had a TOC of less than 0.1 g / 100 g, a Si content of 44 g / 100 g, and a Ti content of 1.4 g / 100 g. The strand breaking strength, determined as described hereinabove, was 11 N, and the total pore volume, determined as described hereinabove, was 0.84 mL / g. The tortuosity parameter for water was 1.71. The BET specific surface area was 352 m 2 / g, and the C value was -500.

[0235] Example 4: Preparation of molded articles using colloidal silica binder precursors with particle size distribution according to the invention Molding: The particles of the zeolitic material of Example 1 (105.3 g) and carboxymethylcellulose (4.0 g; Walocel™, Mw=15,000 g) were mixed in a kneader for 5 minutes. Then, an aqueous polystyrene dispersion (100.7 g; 33.7 g polystyrene) was added continuously. After 10 minutes, polyethylene oxide (1.33 g) was added. After 10 minutes, an aqueous colloidal silica binder precursor (70 g; 50% by weight SiO2; Dv10=56; Dv50=81 nm; Dv90=129 nm; Nalco Chemical Co.) was added. After another 10 minutes, 20 mL of water was added. The total mixing time was 35 minutes. The moldable mass obtained from the mixing was extruded at a pressure of 150 bar through a matrix with circular holes of 1.9 mm in diameter. The strands obtained were dried in an oven in air at a temperature of 120° C. for 4 hours and calcined in air at a temperature of 490° C. for 5 hours. The breaking strength of the strands, determined as described herein above, was 1.5 N.

[0236] Water treatment: 36 g of these strands were divided into 4 portions of 9 g each and mixed with 180 g of deionized water per portion. The mixture obtained was heated to a temperature of 145° C. for 8 hours in an autoclave. The water-treated strands obtained were then separated and sieved through a 0.8 mm sieve. The strands obtained were then washed with deionized water and subjected to a nitrogen flow at ambient temperature. Each washed strand was subsequently dried in air at a temperature of 120° C. for 4 hours and then calcined in air at a temperature of 450° C. for 2 hours.

[0237] The resulting material had a TOC of less than 0.1 g / 100 g, a Si content of 44 g / 100 g, and a Ti content of 1.4 g / 100 g. The strand breaking strength, determined as described hereinabove, was 12 N, and the total pore volume, determined as described hereinabove, was 0.82 mL / g. The tortuosity parameter for water was 1.67. The BET specific surface area was 353 m 2 / g and the C value was -395.

[0238] Comparative Example 1: Preparation of a Molded Article Using a Colloidal Silica Binder Precursor with a Particle Size Distribution Not According to the Invention Molding: The particles of the zeolitic material of Example 1 (105.3 g) and carboxymethylcellulose (4.0 g; Walocel™, Mw=15,000 g) were mixed in a kneader for 5 minutes. Then, an aqueous polystyrene dispersion (100.7 g; 33.7 g polystyrene) was added continuously. After 10 minutes, polyethylene oxide (1.33 g) was added. After 10 minutes, an aqueous colloidal silica binder precursor (70 g; 40% by weight of SiO2; Dv10=28 nm; Dv50=37 nm; Dv90=52 nm; Ludox® AS-40) was added. After another 10 minutes, 20 mL of water was added. The total kneading time was 35 minutes. The moldable mass obtained from the kneading, with a plasticity of 3321 N, was extruded at a pressure of 100 bar through a matrix with a circular hole with a diameter of 1.9 mm. The resulting strands were dried in an oven in air at a temperature of 120° C. for 4 hours and calcined in air at a temperature of 490° C. for 5 hours. The breaking strength of the strands, determined as described herein above, was 1.6 N.

[0239] Water treatment: 36 g of these strands were divided into 4 portions of 9 g each and mixed with 180 g of deionized water per portion. The mixture obtained was heated in an autoclave for 8 hours at a temperature of 145° C. Afterwards, the water-treated strands obtained were separated and sieved through a 0.8 mm sieve. Afterwards, the strands obtained were washed with deionized water and subjected to a nitrogen flow at ambient temperature. Each washed strand was subsequently dried in air at a temperature of 120° C. for 4 hours and then calcined in air at a temperature of 450° C. for 2 hours.

[0240] The resulting material had a TOC of less than 0.1 g / 100 g, a Si content of 44 g / 100 g, and a Ti content of 1.5 g / 100 g. The strand breaking strength, determined as described hereinabove, was 5 N, and the total pore volume, determined as described hereinabove, was 0.89 mL / g. The tortuosity parameter for water was 1.73. The BET specific surface area was 389 m 2 / g and the C value was -547.

[0241] Summary of breaking strength values The following table 1 summarizes the breaking strength values ​​of the molded articles prepared above. Obviously, the molded articles of the present invention show significantly higher, and therefore highly advantageous, values. Moreover, as can be seen from the table, the improvement in breaking strength values ​​achieved by the water treatment according to step (v) of the method of the present invention is significantly better than the respective improvement according to the prior art method.

[0242] [Table 1]

[0243] Example 5: Testing of the molded articles as catalysts for the epoxidation of propene Example 5.1: Preliminary Test - PO Test The molded articles of the examples were preliminarily tested for their general suitability as epoxidation catalysts by the PO test described in Reference Example 9. The respective resulting values ​​of propylene oxide activity are shown in Table 2 below.

[0244] [Table 2]

[0245] Apparently, the molded article according to the present invention exhibits very good propylene-ethylene oxide activity according to the PO test, and is a promising candidate for catalyst in industrial continuous epoxidation reaction.

[0246] Example 5.2: Catalytic properties of the molded articles in a continuous epoxidation reaction The properties of the molded articles of the present invention were compared with those of the prior art molded articles in a continuous epoxidation reaction as described in Reference Example 10. After significant time on stream (TOS), the hydrogen peroxide conversion rates of the molded articles according to Examples 3 and 4 were compared with the respective molded articles according to the prior art (Comparative Example 1), with the following results according to Table 3:

[0247] [Table 3]

[0248] Citations - US2016 / 250624A1 - US6551546B1 -DE19859561A1 - US7825204B2

Claims

1. A chemical molded article comprising a zeolitic material exhibiting a Type I nitrogen adsorption / desorption isotherm and having a framework type MFI and a framework structure comprising Si, O and Ti, said molded article further comprising a binder for said zeolitic material, said binder comprising Si and O, said molded article exhibiting a total pore volume of at least 0.4 mL / g and a crush strength of at least 6N.

2. 95-100% by weight, preferably 98-100% by weight, more preferably 99-100% by weight, more preferably at least 99.5-100% by weight, more preferably 99.9-100% by weight, of the zeolitic material contained in the molded article consists of Si, O, Ti, and optionally H; and the zeolitic material comprises Ti in an amount in the range of 0.2 to 5 mass %, preferably in the range of 0.5 to 4 mass %, more preferably in the range of 1.0 to 3 mass %, more preferably in the range of 1.2 to 2.5 mass %, more preferably in the range of 1.4 to 2.2 mass %, calculated as elemental Ti and based on the total mass of the zeolitic material, 2. The molded article of claim 1, wherein the zeolite material contained in the molded article is preferably titanium silicalite-1.

3. The binder contained in the molded article is composed of 95 to 100% by mass, preferably 98 to 100% by mass, more preferably 99 to 100% by mass, more preferably at least 99.5 to 100% by mass, more preferably 99.9 to 100% by mass of Si and O, and the molded article is made of the binder, SiO 2 Calculated as above, based on the total mass of the molded article, in the range of 2 to 90 mass%, preferably in the range of 5 to 70 mass%, more preferably in the range of 10 to 50 mass%, more preferably in the range of 15 to 30 mass%, more preferably in the range of 20 to 25 mass%. The molded article according to claim 1 or 2.

4. 4. The molded article according to claim 1, wherein 95 to 100% by weight, preferably 98 to 100% by weight, more preferably 99 to 100% by weight, more preferably at least 99.5 to 100% by weight, more preferably 99.9 to 100% by weight of the molded article consists of the zeolite material and the binder.

5. The molded article according to any one of claims 1 to 4, exhibiting a total pore volume in the range of 0.4 to 1.5 mL / g, preferably in the range of 0.4 to 1.2 mL / g, more preferably in the range of 0.4 to 1.0 mL / g, and a breaking strength in the range of 6 to 25 N, preferably in the range of 7 to 20 N, more preferably in the range of 8 to 15 N.

6. Features: a tortuosity parameter for water, determined as described in Reference Example 11, in the range from 1.0 to 2.5, preferably in the range from 1.3 to 2.0, more preferably in the range from 1.6 to 1.8, more preferably in the range from 1.6 to 1.75, more preferably in the range from 1.6 to 1.72; - BET specific surface area, determined as described in Reference Example 6, is between 300 and 450 m 2 / g, preferably 310 to 400 m 2 / g, more preferably 320 to 375 m 2 / g range, a crystallinity, determined as described in Example 7, in the range of 50 to 100%, preferably in the range of 50 to 90% and more preferably in the range of 50 to 80%; a propylene oxide activity, determined as described in Example 9, of at least 4.5% by weight, preferably in the range of 4.5 to 11% by weight, more preferably in the range of 4.5 to 10% by weight; a pressure drop rate, determined as described in Example 9, in the range of 0.005 to 0.019 bar (abs) / min, preferably in the range of 0.006 to 0.017 bar (abs) / min, more preferably in the range of 0.007 to 0.015 bar (abs) / min; when used as catalyst in the reaction for the preparation of propylene oxide from propene and hydrogen peroxide, it exhibits a hydrogen peroxide conversion in the range of 90-95%, determined in a continuous epoxidation reaction as described in Reference Example 10, at a cooling medium temperature in the range of 55-56° C. and an on-stream time in the range of 200-600 hours, preferably an on-stream time in the range of 300-600 hours, more preferably an on-stream time in the range of 350-600 hours, "on-stream time" referring to the duration of the continuous epoxidation reaction without catalyst regeneration; The molded article according to any one of claims 1 to 5, exhibiting one or more of the following:

7. A method for producing a chemical moulding comprising a zeolitic material, which exhibits a nitrogen adsorption / desorption isotherm of type I, determined as described in Reference Example 1, and which has a framework type MFI and a framework structure comprising Si, O and Ti, said moulding further comprising a binder for said zeolitic material, said binder comprising Si and O, preferably a method for producing a chemical moulding according to any one of claims 1 to 6, comprising the following steps: (i) providing a zeolitic material exhibiting a type I nitrogen adsorption / desorption isotherm, determined as described in Example 1, and having framework type MFI and a framework structure comprising Si, O and Ti; (ii) providing a binder precursor comprising a colloidal dispersion of silica in water, said binder precursor exhibiting a volume-based particle size distribution characterized by a Dv10 value of at least 35 nanometers, a Dv50 value of at least 45 nanometers, and a Dv90 value of at least 65 nanometers, determined as described in Example 5; (iii) preparing a mixture comprising the zeolitic material provided in step (i) and the binder precursor provided in step (ii); (iv) molding the mixture obtained from step (iii) to obtain a precursor of the molded article; (v) preparing a mixture comprising the precursor of the shaped article obtained from step (iv) and water, and subjecting said mixture to a water treatment under hydrothermal conditions to obtain a water-treated precursor of the shaped article; (vi) calcining the water-treated precursor of the molded article in a gas atmosphere to obtain the molded article. A method comprising:

8. 8. The method of claim 7, wherein the volume-based particle size distribution of the colloidal dispersion of silica in water from step (ii) is characterized by a Dv10 value in the range of 35 to 80 nanometers, preferably in the range of 40 to 75 nanometers, more preferably in the range of 45 to 70 nanometers, a Dv50 value in the range of 45 to 125 nanometers, preferably in the range of 55 to 115 nanometers, more preferably in the range of 65 to 105 nanometers, and a Dv90 value in the range of 65 to 200 nanometers, preferably in the range of 85 to 180 nanometers, more preferably in the range of 95 to 160 nanometers, determined as described in Reference Example 5, and wherein preferably 95 to 100%, more preferably 98 to 100%, more preferably 99 to 100% by weight of the binder precursor from step (ii) consists of a colloidal dispersion of silica in water.

9. In the mixture prepared by step (iii) and subjected to step (iv), the mass ratio of the zeolite material to the SiO 2and the binder, calculated as: The organic polymer is preferably selected from the group consisting of cellulose, cellulose derivatives, starch, polyalkylene oxides, polystyrene, polyacrylates, polymethacrylates, polyolefins, polyamides, polyesters, and mixtures of two or more thereof, the organic polymer is more preferably selected from the group consisting of cellulose ethers, polyalkylene oxides, polystyrene, and mixtures of two or more thereof, the organic polymer is more preferably selected from the group consisting of methylcellulose, carboxymethylcellulose, polyethylene oxide, polystyrene, and mixtures of two or more thereof, More preferably, the one or more additives comprise, more preferably consist of, water, carboxymethylcellulose, polyethylene oxide, and polystyrene.

10. In the mixture prepared by step (iii) and subjected to step (iv), the mass ratio of said zeolitic material to said one or more additives is in the range of from 0.3:1 to 1:1, preferably in the range of from 0.4:1 to 0.8:1, more preferably in the range of from 0.5:1 to 0.6:1; the mass ratio of said zeolitic material to said cellulose derivative, preferably said cellulose ether, more preferably said carboxymethylcellulose, is in the range of from 10:1 to 53:1, preferably in the range of from 15:1 to 40:1, more preferably in the range of from 20:1 to 35:1; the mass ratio of said zeolitic material to said polyethylene oxide is in the range of from 70:1 to 110:1, preferably in the range of from 75:1 to 100:1, more preferably in the range of from 77:1 to 98:1; the mass ratio of said zeolitic material to said polystyrene is in the range from 2:1 to 8:1, preferably in the range from 3:1 to 6:1, more preferably in the range from 3.5:1 to 5:1; the mass ratio of said zeolitic material to said water is in the range of from 0.7:1 to 0.85:1, preferably in the range of from 0.72:1 to 0.8:1, more preferably in the range of from 0.74:1 to 0.79:1; The method according to claim 9, wherein the mixture prepared by step (iii) and subjected to step (iv) has a plasticity, determined as described in Reference Example 12, in the range of 500 to 3000 N, more preferably in the range of 750 to 2000 N, more preferably in the range of 1000 to 1500 N.

11. 11. The method according to any one of claims 7 to 10, wherein the shaping according to step (iv) further comprises drying the precursor of the shaped article in a gas atmosphere, said drying being preferably carried out at a temperature of the gas atmosphere in the range of 80 to 160°C, preferably in the range of 100 to 140°C, more preferably in the range of 110 to 130°C, said gas atmosphere preferably comprising nitrogen, oxygen or a mixture thereof, more preferably oxygen, air or lean air, and wherein the shaping according to step (iv) further comprises calcining the dried precursor of the shaped article in a gas atmosphere, said calcination being preferably carried out at a temperature of the gas atmosphere in the range of 450 to 530°C, preferably in the range of 470 to 510°C, more preferably in the range of 480 to 500°C, said gas atmosphere preferably comprising nitrogen, oxygen or a mixture thereof, more preferably oxygen, air or lean air.

12. 12. The method according to any one of claims 7 to 11, wherein in the mixture prepared in step (v), the mass ratio of the precursor of the shaped article to the water is in the range of 1:1 to 1:30, preferably in the range of 1:5 to 1:25, more preferably in the range of 1:10 to 1:20, and preferably 95 to 100% by weight, more preferably 98 to 100% by weight, more preferably 99 to 100% by weight, more preferably 99.5 to 100% by weight, more preferably 99.9 to 100% by weight of the mixture prepared by step (v) consists of the precursor of the shaped article and the water.

13. 13. The process according to any one of claims 7 to 12, wherein the water treatment according to step (v) comprises a temperature of the mixture in the range of 100 to 200°C, preferably in the range of 125 to 175°C, more preferably in the range of 130 to 160°C, more preferably in the range of 135 to 155°C, more preferably in the range of 140 to 150°C, and wherein the water treatment according to step (v) is carried out under autogenous pressure, preferably in an autoclave.

14. 14. The method according to any one of claims 7 to 13, wherein step (v) further comprises separating the water-treated precursor of the shaped article from the mixture obtained from the water treatment, said separating preferably comprising subjecting the mixture obtained from the water treatment to a solid-liquid separation, preferably washing the separated precursor, and preferably drying the preferably washed precursor, and wherein said drying according to step (v) preferably comprises drying the precursor in a gas atmosphere, wherein drying is preferably carried out at a temperature of said gas atmosphere in the range of 80 to 160°C, more preferably in the range of 100 to 140°C, more preferably in the range of 110 to 130°C, and wherein said gas atmosphere preferably comprises nitrogen, oxygen or a mixture thereof, and wherein said gas atmosphere is more preferably oxygen, air or lean air.

15. 15. The method according to any one of claims 7 to 14, wherein the calcination according to step (vi) is carried out at a temperature in the range of 400 to 490°C, preferably in the range of 420 to 470°C, more preferably in the range of 440 to 460°C, in said gas atmosphere, said gas atmosphere preferably comprising nitrogen, oxygen or a mixture thereof, said gas atmosphere being more preferably oxygen, air or lean air.

16. 7. A method of using a shaped article according to any one of claims 1 to 6 as an adsorbent, absorbent, catalyst or catalyst component, preferably as a catalyst or catalyst component, more preferably as a Lewis acid catalyst or Lewis acid catalyst component, as an isomerization catalyst or isomerization catalyst component, as an oxidation catalyst or oxidation catalyst component, as an aldol condensation catalyst or aldol condensation catalyst component, or as a Prins reaction catalyst or Prins reaction catalyst component, preferably as an oxidation catalyst or oxidation catalyst component, preferably as an epoxidation catalyst or epoxidation catalyst component, more preferably as an epoxidation catalyst, Preferably, a method of using an organic compound having at least one C-C double bond, preferably a C2 to C10 alkene, more preferably a C2 to C5 alkene, more preferably a C2 to C4 alkene, more preferably a C2 or C3 alkene, more preferably for the epoxidation reaction of propene, more preferably for the epoxidation reaction of propene with hydrogen peroxide as oxidant, more preferably for the epoxidation reaction of propene with hydrogen peroxide as oxidant in a solvent comprising an alcohol, preferably methanol.

17. 10. The method of claim 1, further comprising the step of preparing a binder obtained from said binder precursor, comprising a zeolitic material having a nitrogen adsorption / desorption isotherm of type I, determined as described in Reference Example 1, and having a framework type MFI and a framework structure comprising Si, O and Ti, and further comprising the step of preparing a chemical moulding, preferably a moulding according to any one of claims 1 to 6, wherein the silica has a Dv10 value of at least 35 nanometers, preferably in the range of 35 to 80 nanometers, more preferably in the range of 40 to 75 nanometers, more preferably in the range of 45 to 70 nanometers, determined as described in Reference Example 5, 2. A method for producing a molded article comprising the steps of: a) forming a molded article having a volume-based particle size distribution characterized by a Dv50 value of at least 45 nanometers, preferably in the range of 45 to 125 nanometers, more preferably in the range of 55 to 115 nanometers, more preferably in the range of 65 to 105 nanometers, and a Dv90 value of at least 65 nanometers, preferably in the range of 65 to 200 nanometers, more preferably in the range of 85 to 180 nanometers, more preferably in the range of 95 to 160 nanometers; and b) forming a molded article having a total pore volume of at least 0.4 mL / g, determined as described in Reference Example 2, and a breaking strength of at least 6 N, determined as described in Reference Example 3.

18. A mixture comprising a zeolitic material exhibiting a type I nitrogen adsorption / desorption isotherm as determined as described in Reference Example 1 and having a framework type MFI and a framework structure comprising Si, O and Ti, said mixture further comprising a colloidal dispersion of silica in water, said binder precursor exhibiting a volume-based particle size distribution characterized by a Dv10 value of at least 35 nanometers, a Dv50 value of at least 45 nanometers, and a Dv90 value of at least 65 nanometers as determined as described in Reference Example 5; The mixture preferably has a plasticity, determined as described in Reference Example 12, in the range of 500 to 3000 N, preferably in the range of 750 to 2000 N, more preferably in the range of 1000 to 1500 N; said colloidal dispersion of silica in water comprises said silica in an amount in the range of 25 to 65% by weight, more preferably 30 to 60% by weight, more preferably 35 to 55% by weight, based on the combined weight of said silica and said water, and preferably 95 to 100% by weight, more preferably 98 to 100% by weight, more preferably 99 to 100% by weight of said binder precursor consists of said colloidal dispersion of silica in water; In the mixture, the mass ratio of the zeolite material is 2 With respect to the total amount of the binder, calculated as follows: The mixture preferably further comprises one or more additives, preferably one or more viscosity modifiers, or one or more mesopore formers, or one or more viscosity modifiers and one or more mesopore formers.

19. 19. Use of a mixture according to claim 18 for producing a chemical moulding, preferably a chemical moulding according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Production of shaped bodies, for example containing titanium, silicon, and lithium, using a metal oxide sol

    DE19859561A1

  • Fine powder and molded articles containing zeolite material containing Ti and Zn.

    JP2015512845A

  • Use of zeolitic materials in processes for producing zeolitic materials and converting oxygenates to olefins

    JP2016502487A

  • Method for producing zeolite and zeolite-type

    JP2016529190A

  • Molded articles made from hydrophobic zeolite-based materials and methods for manufacturing the same

    JP2016535718A