Automotive exterior panels
The panel's controlled metallographic structure and manufacturing process enhance dent resistance and surface quality by ensuring uniform strain and precipitate distribution, addressing the challenges of complex shaping in automobile exterior panels.
Patent Information
- Application Number
- JP2021572821
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-24
- Filing Date
- 2021-01-22
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2041-01-22
AI Technical Summary
Automobile exterior panels require improved dent resistance and surface quality after molding, as existing technologies do not adequately address the issue of dents and surface irregularities caused by plastic deformation during complex shaping.
A panel composed of a steel plate containing martensite with controlled metallographic structure and specific surface roughness, precipitate distribution, and uniform strain properties, achieved through a manufacturing process involving tempering and bake hardening treatments.
The solution provides panels with excellent surface quality and enhanced dent resistance, ensuring uniform deformation and reduced surface irregularities, suitable for automotive applications.
Smart Images

Figure 0007574226000008 
Figure 0007574226000009 
Figure 0007574226000010
Abstract
Description
[Technical field]
[0001] The present invention relates to a panel. [Background technology]
[0002] In recent years, there has been a demand for improved fuel efficiency in automobiles to protect the global environment. To improve fuel efficiency, there is a demand for even higher strength in automotive steel sheets in order to reduce the weight of vehicle bodies while ensuring safety. This demand for higher strength is not limited to structural members and pillars, but is also increasing for automotive exterior panels (hoods, fender panels, door panels, roof panels, etc.). In response to this demand, materials have been developed with the aim of achieving both strength and elongation (formability).
[0003] On the other hand, the shapes of exterior panel parts of automobiles tend to become increasingly complex. When steel plates are made stronger and thinner to reduce weight, unevenness is more likely to occur on the surface of the steel plate when it is formed into a complex shape. If unevenness occurs on the surface, the appearance after forming deteriorates. Since not only characteristics such as strength but also design and surface quality are important for exterior panels, they are required to have excellent appearance after forming. In other words, automobile exterior panels are required to have an appearance (surface properties) that does not result in surface roughness or patterns after forming.
[0004] Regarding the relationship between the post-forming appearance and material properties of steel sheets used for exterior panels, for example, Patent Document 1 discloses a ferritic thin steel sheet in which the area fraction of crystals having a crystal orientation within ±15° from the {001} plane parallel to the steel sheet surface is set to 0.25 or less and the average grain size of said crystals is set to 25 μm or less in order to improve the surface properties after stretching. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-156079 A Summary of the Invention [Problem to be solved by the invention]
[0006] In addition to having good surface properties after material forming, the outer panel of an automobile is required to have good dent resistance. Dent resistance refers to the difficulty of a depression (dent) remaining after a load is removed when a local load is applied to the panel for some reason. In an actual automobile body, a dent occurs when an outer panel such as a door is pressed hard with a finger or palm, or when a flying stone hits the panel while driving. A dent occurs when a part of the panel to which a load is applied undergoes plastic deformation. Therefore, when the strain of the panel when a load is applied to the panel reaches a certain magnitude, the strain remains even after the load is removed, and a dent occurs. The minimum value of the load that generates a certain residual strain in the panel is called the dent load, and the larger the dent load, the better the dent resistance. Patent Document 1 does not disclose anything about improving dent resistance.
[0007] In view of the above background, one object of the present invention is to provide a panel which has excellent appearance after being molded from a material and has excellent dent resistance. [Means for solving the problem]
[0008] The present invention relates to the following panels:
[0009] (1) A panel having a steel plate containing martensite, The surface roughness parameter (Sa) in the flat portion of the center side portion of the panel is Sa≦0.500 μm, In the lath of the martensite, precipitates with a major axis of 0.05 μm to 1.00 μm and an aspect ratio of 3 or more are arranged at 15 pieces / μm 2 More than a ratio YS1 / YS2 of a yield stress YS1 measured using a tensile test piece cut out from the flat portion to a yield stress YS2 measured using a tensile test piece cut out from an end portion of the panel, being 0.90 to 1.10.
[0010] (2) The panel according to (1) above, wherein the ratio YS1 / TS1 of the yield stress YS1 to the tensile strength TS1 of the tensile test specimen cut out from the flat portion is 0.85 or more.
[0011] (3) The panel according to (1) or (2) above, wherein the hardness of the flat portion is 133 to 300 Hv.
[0012] (4) The panel according to any one of (1) to (3) above, wherein the flat portion has a thickness of 0.20 mm to 0.60 mm.
[0013] (5) The panel according to any one of (1) to (4) above, wherein the steel plate is a dual-phase steel plate.
[0014] (6) The panel according to any one of (1) to (5) above, wherein the panel has a tensile strength of 400 to 900 MPa. Effect of the Invention
[0015] According to the present invention, it is possible to provide a panel that has excellent appearance after being molded from a material and has excellent dent resistance. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is an image diagram showing the state of precipitates in a high-strength steel plate as a raw material for the steel plate according to this embodiment. [Diagram 2] Fig. 2(A) is a plan view of a part used in the dent resistance evaluation, and Fig. 2(B) is a cross-sectional view taken along line IIB-IIB in Fig. 2(A). [Diagram 3] FIG. 3 is a side view of a test device for measuring the dent resistance of a part and a cross-sectional view of the part, and shows the cross section of the part taken along line IIB-IIB in FIG. 2(A). [Figure 4] FIG. 4 is a graph showing the relationship between the index and the dent depth of each part. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] In the following, first, the circumstances under which the present invention was conceived will be described, and then an embodiment will be described in detail.
[0018] <How the present invention was conceived> In order to reduce the weight of an automobile body, the thickness of the body members constituting the automobile body is being reduced. The body members include panels. The panels are integrally molded products. The panels are, for example, exterior members of an automobile. Examples of the panels include outer panels of a hood, quarter panels such as fender panels, outer door panels, and roof panels.
[0019] Such panels are formed by cutting cold-rolled steel sheets, press-forming them, painting them, and baking them after painting (bake hardening treatment). Bake hardening is a phenomenon in which interstitial elements (mainly carbon) move and adhere to dislocations (linear defects that are the elementary process of plastic deformation) that enter steel sheets by cold plastic processing (pre-strain), inhibiting their movement and increasing their strength. It is also called strain aging. For such steel sheets, baking treatment is usually performed as a heat treatment after final annealing. Here, it was found that the occurrence of surface irregularities during forming, which causes deterioration of the appearance after forming, is caused by uneven deformation during forming due to unevenness in the strength of the steel sheet of the panel. Therefore, it is considered to perform a tempering treatment on the panel material in order to improve the appearance by suppressing surface irregularities during forming by eliminating the hardness difference in each part of the panel and increasing the homogeneity of each part of the panel. However, it was previously thought that the amount of bake hardening would decrease if tempering was performed after the above-mentioned final annealing. This is because tempering reduces the amount of solute carbon, which reduces the amount of bake hardening. Furthermore, the tempering also reduces the yield stress and hardness. However, the inventors of the present application have found, as a result of intensive research, that if the tempering process is performed in a temperature range corresponding to the Si (silicon) concentration of the panel material after the final annealing and then the bake hardening process is performed, the amount of bake hardening increases. The increase in the amount of bake hardening improves the yield stress, and thus improves the dent resistance. As a result of further intensive research, the inventors of the present application have come up with a panel that has excellent appearance after forming and excellent dent resistance by performing the tempering process on a panel material having properties that provide excellent appearance after forming.
[0020] <Description of the embodiment> Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0021] <Panel> The panel used in this embodiment may be, for example, the panel described above. The panel is manufactured by the manufacturing method described above. The panel has a steel sheet containing martensite and a paint layer formed on the steel sheet. The steel sheet may include a plating layer on the surface, or may not have a plating layer formed on the surface. In addition, when the steel sheet has a plating layer, the "surface of the steel sheet" refers to the surface of the steel sheet excluding the plating layer. The panel may be composed of only the steel sheet without having a paint layer.
[0022] The panel includes three portions: (i) an edge portion, (ii) an end portion, and (iii) a central portion other than the edge portion and the end portion.
[0023] The edge portion of (i) above is a portion that is bent by hemming (HEM) processing or fixed to another part by welding such as spot welding. The end portion of (ii) above is a portion located toward the center of the panel from the edge portion, and is a portion that is removed from the portion that is fixed to another part by hemming, welding, etc. This end portion is, for example, a portion that is several mm toward the center of the panel from the edge portion, and is a portion that is substantially not affected by processing for fixing the panel to another part. In this case, "substantially not affected" means that the change in characteristics due to processing for fixing the panel to another part is within a few percent. The center side portion of (iii) above is visible from the outside of the automobile as the exterior of the automobile. In this specification, a portion of the center side portion of the panel with a curvature radius of 500 mm or more is called a flat portion.
[0024] <The surface roughness parameter (Sa) on the flat portion of the center part of the panel is Sa≦0.500μm> In this embodiment, the surface roughness parameter Sa in the flat portion of the center portion of the panel is preferably 0≦Sa≦0.500 μm. When a paint layer is formed on the panel, the flat portion in this case refers to the flat portion of the panel as a whole including the paint layer. The surface roughness parameter refers to the arithmetic mean height of the height from the average surface (a surface with a height of zero) on the surface of a 3 mm square test piece in the flat portion of the panel, for example. In this embodiment, to evaluate the surface roughness parameter Sa, first, the surface quality of the 3 mm square flat portion of the panel is measured with a laser microscope. Next, the measured surface is passed through a low-pass filter (λs) specified in JIS B0601:2013 to remove wavelength components of 0.8 mm or less from the measured surface. Then, the surface roughness parameter (Sa) specified in ISO25178 is evaluated for the measured surface smoothed by the low-pass filter (λs). If the surface roughness parameter Sa is greater than 0.500 μm, regardless of the presence or absence of a paint layer, the unevenness of the panel surface will become large, resulting in a poor appearance after the panel is molded. As described above, by obtaining the surface roughness parameter Sa based on a measurement surface that has been smoothed by removing wavelength components of 0.8 mm or less from the measurement surface, the true value of the surface roughness parameter Sa can be detected with high accuracy by removing measurement errors in the laser microscope (errors caused by the measurement accuracy of the laser microscope, errors caused by dust during measurement, errors caused by scratches made when the test specimen was created, etc.).
[0025] An example of control factors (requirements for metal structure) of the steel sheet for realizing the above-mentioned surface roughness parameter Sa will be described below.
[0026] <Metal structure of the surface layer> In the steel sheet according to this embodiment, when the sheet thickness is t, the depth range from the surface to t / 4 in the sheet thickness direction is divided into two regions, the depth range starting from the surface and ending at a depth position of 20 μm in the sheet thickness direction (depth direction) of the steel sheet is the surface layer region, and the range toward the center of the steel sheet with respect to the surface layer region is the internal region. Note that, when the steel sheet has a plating layer, the surface of the steel sheet excluding the plating layer is defined as the starting point of the surface layer region. As described above, the inventors have found that the occurrence of surface irregularities during forming is caused by non-uniform deformation during forming due to non-uniformity in the strength of the steel sheet in a microscopic region. In particular, it has been found that the occurrence of surface irregularities is greatly influenced by the metal structure of the surface layer region in the range of 0 to 20 μm from the surface in the sheet thickness direction (the range from the surface to a position 20 μm from the surface in the sheet thickness direction). Therefore, in the steel sheet according to this embodiment, the metal structure of the surface layer region is controlled, for example, as follows.
[0027] As structural requirements for the surface region, it is preferable that the main phase is ferrite and the volume fraction of martensite is 0.01 to 15.0%, and that the volume fraction of martensite is smaller than the volume fraction of martensite in the inner region. The volume fraction of ferrite, which is the main phase, is preferably in the range of 50% or more. In addition, the volume fraction of martensite in the metal structure of the surface region is preferably smaller than the volume fraction of martensite in the inner region.
[0028] The volume fraction of martensite in the surface layer region can be determined by the following method. A sample for observing the metal structure (microstructure) (size: approximately 20 mm in the rolling direction x 20 mm in the width direction x thickness of the steel plate) is taken from the flat part of the obtained steel plate, and the metal structure (microstructure) is observed from the surface to 1 / 4 of the plate thickness using an optical microscope, and the area ratio of martensite from the surface of the steel plate (surface excluding the plated layer if plating is present) to 20 μm is calculated. To prepare the sample, the plate thickness cross section perpendicular to the rolling direction is polished as the observation surface, and etched with LePeller's reagent. The "microstructure" is classified from 500x optical microscope photographs etched with LePeller's reagent. When observing with an optical microscope after LePeller's etching, each structure is observed in a different color, for example, bainite is black, martensite (including tempered martensite) is white, and ferrite is gray, making it easy to distinguish between martensite and other hard structures. Ten fields of view are observed at a magnification of 500 times at a position of 1 / 4 thickness from the surface layer of the steel plate etched with LePeller's reagent, and a region 20 μm from the surface layer of the steel plate in the structure photograph is specified, and image analysis is performed using image analysis software "Photoshop CS5" manufactured by Adobe to determine the area fraction of martensite. As an image analysis method, for example, the maximum brightness value Lmax and the minimum brightness value Lmin of the image are obtained from the image, and the area having pixels with brightness from Lmax-0.3 (Lmax-Lmin) to Lmax is defined as a white area, the area having pixels from Lmin to Lmin+0.3 (Lmax-Lmin) is defined as a black area, and the other areas are defined as a gray area, and the area fraction of martensite in the white area is calculated. The area fraction of martensite is measured for a total of 10 fields of view by performing image analysis in the same manner as above, and these are then averaged to calculate the volume fraction of martensite in the surface layer region.
[0029] As a structural requirement for the surface layer region, the average crystal grain size of martensite is preferably 0.01 to 4.0 μm.
[0030] The average grain size of martensite in the surface layer region can be determined by the following method. As above, 10 fields of view were observed at 500x magnification at 1 / 4 thickness from the surface of the steel plate etched with LePeller's reagent, and a 20μm×200μm region was selected from the surface of the steel plate in the microstructure photograph. Image analysis was performed in the same manner as above using Adobe's Photoshop CS5 image analysis software to calculate the area occupied by martensite and the number of martensite particles. These were added together and the area occupied by martensite was divided by the number of martensite particles to calculate the average area per martensite particle. The circle equivalent diameter was calculated from this area and number of particles, which was taken as the average crystal grain size of martensite.
[0031] In the steel sheet according to the present embodiment, the metal structure other than ferrite and martensite is a hard structure (residual structure), and is, for example, one or more of pearlite, retained austenite, and bainite. From the viewpoint of improving strength, it is preferable that the metal structure is one or more of bainite.
[0032] As a structural requirement of the surface layer region, it is preferable that ferrite is the main phase, martensite is the second phase, and hard structures other than ferrite and martensite are the remaining structure. More specifically, it is preferable that in the surface layer region, the volume fraction of ferrite is 50% or more, the volume fraction of martensite is 0.01 to 15.0%, the volume fraction of the remaining structure is 0 to 49.99%, and the total of the structures is 100%. In the surface layer region, the total volume fraction of the volume fractions of ferrite and the second phase is preferably 50.01% or more, preferably 65.0% or more, and more preferably 85% or more. In addition, in the surface layer region, the volume fraction of the remaining structure is preferably 35% or less, more preferably 15% or less.
[0033] <Metal structure of the internal region> In this embodiment, the metal structure of the internal region does not substantially affect the surface roughness parameter Sa, but it is preferable that the metal structure satisfy the following structure requirements. That is, in the steel sheet according to this embodiment, after controlling the metal structure of the surface layer region as described above, it is preferable that the metal structure of the internal region ranging from a position more than 20 μm from the surface in the sheet thickness direction to a position 1 / 4 of the sheet thickness from the surface in the sheet thickness direction (t / 4, where t is the sheet thickness) satisfy the following structure requirements.
[0034] As structural requirements for the internal region, it is preferable that ferrite be the main phase and that the volume fraction of martensite be 2.0 to 25.0%. The volume fraction of ferrite, which is the main phase, is preferably in the range of 50% or more.
[0035] As a structural requirement of the internal region, it is preferable that ferrite is the main phase, martensite is the second phase, and hard structures other than ferrite and martensite are the remaining structure. More specifically, it is preferable that in the internal region, the volume fraction of ferrite is 50% or more, the volume fraction of martensite is 2.0 to 25.0%, the volume fraction of the remaining structure is 0 to 48.0%, and the total of the structures is 100%. In the internal region, the total volume fraction of the volume fractions of ferrite and the second phase is preferably 52.0% or more, preferably 75.0% or more, and more preferably 90% or more. In addition, in the internal region, the volume fraction of the remaining structure is preferably 25% or less, more preferably 10% or less.
[0036] As a structural requirement for the internal region, the average crystal grain size of martensite is preferably 1.0 μm or more and 5.0 μm or less, and is larger than the average crystal grain size of martensite in the surface layer structure.
[0037] The volume fraction and average grain size of martensite in the internal region can also be obtained by using a steel plate etched with LePeller's reagent, selecting a range from the surface of the sample to a position of more than 20 μm to 1 / 4 of the plate thickness in the plate thickness direction, and analyzing it in the same manner as for the surface region. When the thickness of the steel plate exceeds 0.4 mm, the internal region is preferably in the range from more than 20 μm to 100 μm from the surface in the plate thickness direction.
[0038] <Other organizations> <In the laths of martensite in the steel plate, precipitates with a major axis of 0.05 μm to 1.00 μm and an aspect ratio of 3 or more are counted at 15 / μm. 2 > In this embodiment, the first heat treatment described later produces precipitates with a major axis of 0.05 μm or more and 1.00 μm or less and an aspect ratio of 1:3 or more at a density of 15 precipitates / μm. 2It is preferable that the number density is equal to or more than 100 nm. In this embodiment, the aspect ratio refers to the ratio between the longest diameter (major diameter) of the precipitate and the longest diameter (minor diameter) of the precipitate perpendicular to the longest diameter (minor diameter). The precipitate is not particularly limited as long as it satisfies the requirements of the major diameter and aspect ratio, and may be, for example, a carbide. In particular, in this embodiment, the precipitate may contain iron carbide or may be made of iron carbide. According to this embodiment, by including a relatively large amount of such precipitates in the structure, it is possible to suppress dislocation cell formation caused by, for example, entanglement of dislocations, and to increase the amount of dislocations fixed due to carbon diffused during bake hardening, and as a result, it is possible to significantly increase the amount of bake hardening. The size of the dislocation cells generated in the martensite is about several tens of nm or more and several hundreds of nm or less. Therefore, in order to suppress the generation of dislocation cells, the precipitates must be of the same size. If the major diameter is less than 0.05 μm, the formation of dislocation cells cannot be suppressed. Therefore, the major axis of the precipitates is preferably 0.05 μm or more, and more preferably 0.10 μm or more. If the major axis is larger than 1.00 μm, the precipitates become coarse, significantly reducing the amount of solute carbon and reducing the amount of bake hardening. Therefore, the major axis of the precipitates is preferably 1.00 μm or less, and more preferably 0.80 μm or less.
[0039] The shape of the precipitates is preferably acicular rather than spherical, and the aspect ratio is preferably 1:3 or more. If the aspect ratio is less than 1:3, the precipitates are considered to be spherical, and the generation of dislocation cells cannot be suppressed. Therefore, the aspect ratio is set to 1:3 or more, and more preferably 1:5 or more.
[0040] The precipitation location of the precipitates is preferably within the laths. This is because dislocation cells are most easily formed within the laths, and dislocation cells are rarely found between the laths. Here, the lath refers to a structure generated within the prior austenite grain boundaries by martensitic transformation. For ease of understanding, FIG. 1 is an image showing the precipitation state of precipitates in a high-strength steel plate as the material of the steel plate according to this embodiment. Referring to FIG. 1, it can be seen that in a lath structure 13 generated within a prior austenite grain boundary 12 in the microsegregation of Si having a uniform structure 11, needle-like precipitates 15 are uniformly precipitated over the entire surface of the laths 14, not between the laths 14. The number density of the precipitates 15 is preferably 15 / μm 2 More preferably, 20 particles / μm 2 More preferably, 30 particles / μm 2 More preferably, 40 particles / μm 2 That's all.
[0041] In this embodiment, the morphology and number density of the precipitates 15 are determined by observation with an electron microscope, for example, measured by TEM (transmission electron microscope) observation. Specifically, a thin film sample is cut out from the inner region of the steel sheet and observed in a bright field. 2 The number of precipitates 15 with a major axis of 0.05 μm or more and 1 μm or less and an aspect ratio of 1:3 or more is counted. This operation is performed in five or more consecutive fields of view, and the average is taken as the number density.
[0042] <The ratio YS1 / YS2, which is the yield stress YS1 measured using a tensile test piece cut from the flat part and the yield stress YS2 measured using a tensile test piece cut from the end of the panel, is 0.90 to 1.10.> When the ratio YS1 / YS2 between the yield stress YS1 and the yield stress YS2 is 0.90 to 1.10, the strain is uniformly distributed over the entire flat portion and the end portion of the panel, and the bake hardening during the paint baking occurs uniformly over the entire steel plate including the flat portion and the end portion. When the ratio YS1 / YS2 is less than 0.90 or more than 1.10, the strain amount is uneven over the entire flat portion and the end portion of the panel, and the bake hardening amount during the paint baking occurs unevenly. The yield stress YS1 can be determined by a tensile test performed in accordance with JIS Z 2241 using a JIS No. 5 test piece cut out perpendicular to the rolling direction from the flat portion of the panel. The yield stress YS2 can be determined by a tensile test performed in accordance with JIS Z 2241 using a JIS No. 5 test piece cut out perpendicular to the rolling direction from the end portion of the panel.
[0043] [Ratio of yield stress YS1 to tensile strength TS1 of tensile test piece cut from flat part: 0.85 or more] The ratio YS1 / TS1 of the yield stress YS1 to the tensile strength TS1 in a tensile test piece cut out from a flat portion of the panel is preferably 0.85 or more. When this ratio is 0.85 or more, a higher strain can be applied to the panel, and the yield stress of the panel is increased, thereby improving the dent resistance. The tensile strength TS1 can be determined by a tensile test performed in accordance with JIS Z 2241 using a JIS No. 5 test piece cut out from the flat portion of the panel in a direction perpendicular to the rolling direction.
[0044] [Hardness of flat part: 133~300Hv] The hardness of the flat portion of the panel is preferably 133 to 300 HV. When the Vickers hardness is in this range, the tensile strength of the panel can be estimated to be 400 to 900 MPa. The hardness was measured using a micro Vickers hardness tester in accordance with JIS Z2244:2009. The measurement was performed at any five points located at 1 / 4 depth from the surface on the cross section of the flat portion of the panel, with a test force of 4.9 N. The average of the obtained Vickers hardnesses was regarded as the hardness of the flat portion of the panel.
[0045] [Thickness of flat part: 0.20mm~0.60mm] The thickness of the flat portion of the panel is 0.20 mm to 0.60 mm. If the thickness is less than the lower limit, the panel becomes too thin and it is difficult to ensure sufficient dent resistance. On the other hand, if the thickness exceeds the upper limit, the panel becomes heavy and it is difficult to obtain a reputation as a lightweight panel.
[0046] [The steel plate is a dual-phase steel plate] The steel plate is preferably a high-tensile steel plate. The steel plate is preferably a dual-phase steel plate. The dual-phase steel plate contains ferrite as a soft structure and martensite as a hard structure, and has high strength and excellent workability during panel forming. In the DP steel, martensite and ferrite are distributed in a mosaic pattern, and hard parts that are transformation-strengthened and soft parts that are not transformation-strengthened coexist. When the DP steel is used as a high-strength steel plate, deformation due to cold plastic working (press forming) mainly occurs in the ferrite, which is a soft structure. Note that the high-strength steel plate may contain at least ferrite and martensite, and steels other than DP steel may be used.
[0047] [Panel tensile strength: 400~900MPa] The tensile strength of the panel is preferably 400 to 900 MPa. If the tensile strength of the panel is below the lower limit, it is difficult to achieve a thin panel while ensuring the strength of the panel. On the other hand, if the tensile strength of the panel is above the upper limit, the workability of the panel is reduced.
[0048] <About the plating layer> The steel sheet according to this embodiment may have a plating layer on the surface. By having a plating layer on the surface, corrosion resistance is improved, which is preferable. Applicable plating is not particularly limited, but examples thereof include hot-dip galvanizing, alloyed hot-dip galvanizing, electrogalvanizing, Zn-Ni plating (electric alloy galvanizing), Sn plating, Al-Si plating, alloyed electrogalvanizing, hot-dip zinc-aluminum alloy plating, hot-dip zinc-aluminum-magnesium alloy plating, hot-dip zinc-aluminum-magnesium alloy-Si plated steel sheet, and zinc-vapor-deposited Al plating.
[0049] <About the paint layer> A paint layer is formed on the surface of the steel plate according to this embodiment. The paint layer is the part of the panel that is directly visible. If a plating layer is formed, the paint layer is formed on the plating layer. In the case of an automotive panel, the paint has a thickness of about 100 μm. The paint layer in the automotive panel includes, in order from the steel plate side, an electrodeposition paint layer, an intermediate paint layer, a base coat layer, and a clear coat layer. The thickness of the electrodeposition paint layer is, for example, 15 to 20 μm. The thickness of the intermediate paint layer is, for example, 25 to 35 μm. The thickness of the base coat layer is, for example, 10 to 15 μm. The thickness of the clear coat layer is, for example, 30 to 40 μm.
[0050] <Chemical composition> The chemical composition of the steel sheet according to this embodiment can be exemplified as follows. Chemical composition, in mass%, C: 0.020% or more, 0.145% or less, Si: 0.010% or more, 3.000% or less, Mn: 0.45% or more, 2.25% or less, P:0.030% or less, S: 0.020% or less, Sol.Al: 0.30% or less, N: 0.0100% or less, B: 0~0.0050%, Mo: 0-0.80%, Ti: 0 to 0.20%, Nb: 0-0.10%, Cr: 0-0.70%, Ni: 0-0.25%, and the balance being Fe and impurities. Here, impurities refer to components that are mixed in due to various factors in the manufacturing process, including raw materials such as ores and scraps, when industrially manufacturing steel plate, and are not components that are intentionally added to the steel plate according to this embodiment.
[0051] [Si:0.010%~3.000%] Silicon is an element necessary for the precipitation of fine and large amounts of iron carbides and other precipitates that suppress dislocation cells. When the Si content is 0. 01 If the Si content is less than 0%, even if the segregation is made uniform, sufficient effect cannot be obtained, and coarse precipitates are generated, making it impossible to suppress the formation of dislocation cells. Therefore, the Si content is preferably 0.010% or more, more preferably 0.050% or more. On the other hand, if the Si content exceeds 3.000%, the effect of precipitating fine and large amounts of precipitates becomes saturated, which unnecessarily increases costs and deteriorates surface properties. Therefore, the Si content is preferably 3.000% or less, and more preferably 2.000% or less.
[0052] <Production method> Next, a preferred method for manufacturing the panel according to the present embodiment will be described. The panel according to the present embodiment can obtain the effects as long as it has the above-mentioned characteristics regardless of the manufacturing method. However, the following method is preferable because it can be manufactured stably.
[0053] [Manufacturing method for high-strength steel plate with minimal unevenness] A high-strength steel sheet as a material for a steel sheet having excellent surface appearance due to small surface irregularities can be manufactured by the following manufacturing method, for example. Specifically, the high-strength steel sheet as a material for the steel sheet constituting the panel according to the present embodiment can be manufactured by a manufacturing method including the following steps (ii) to (i-vi). (ii) a heating step of heating a steel slab having the above chemical composition to 1000°C or higher; (i-ii) a hot rolling process in which the steel slab is hot-rolled at 950°C or less to obtain a hot-rolled steel sheet; (i-iii) After the hot rolling process, the hot-rolled steel sheet is subjected to the residual stress σ s a stress applying step of applying stress so that the absolute value of (i-iv) The hot-rolled steel sheet after the stress application process is subjected to a cumulative rolling reduction R CR a cold rolling process for obtaining a cold-rolled steel sheet by performing cold rolling in which the degree of hardness is 70 to 90%; (iv) an annealing process in which the cold-rolled steel sheet is heated at an average heating rate of 1.5 to 10.0°C / s from 300°C to a soaking temperature T1°C that satisfies the following formula (1), and then annealed at the soaking temperature T1°C for 30 to 150 seconds; 1275-27×ln(σs)-4.5×R CR ≦ T1 ≦ 1275-25×ln(σs)-4×R CR ... (1) (i-vi) A cooling process in which the cold-rolled steel sheet after the annealing process is cooled to a temperature range of 550 to 650°C so that the average cooling rate from T1°C to 650°C is 1.0 to 10.0°C / s, and then cooled to a temperature range of 200 to 490°C so that the average cooling rate is 5.0 to 500.0°C / s.
[0054] After the cooling step, a plating step of forming a plating layer on the surface may be included.
[0055] In the stress application process, the surface of the hot-rolled steel sheet is rubbed with a brush to apply residual stress σ s The stress is set to 150 MPa to 450 MPa. The brush used for applying stress is a brush used for polishing and grinding, and an example of the brush is Hotani Co., Ltd. model number: M-33. The brush has, for example, a configuration in which a large number of hard bristles are provided on the outer peripheral surface of a cylindrical brush body. The brush is moved when applying stress by, for example, rotating the brush at a rotation speed of 1200 rpm so as to face the traveling direction of the steel sheet (so that the rotation axis of the brush body is parallel to the width direction of the hot-rolled steel sheet). The contact pressure of the brush with the hot-rolled steel sheet is changed to control the residual stress σ s The residual stress σ of hot-rolled steel sheets caused by brushing can be changed. sThe application of the stress is not intended to change the thickness of the hot-rolled steel sheet, and the thickness of the hot-rolled steel sheet is maintained before and after the stress application process. In the stress application process, the thickness of the hot-rolled steel sheet is not changed, and the surface of the hot-rolled steel sheet is rubbed to apply a residual stress σ s For example, in a process of grinding the surface of a hot-rolled steel sheet with a grinding tool to reduce the sheet thickness, it cannot be said that residual stress such as that imparted in the stress imparting process of the present invention is generated.
[0056] [Method of manufacturing panels from high-strength steel sheets] Next, an example of a method for manufacturing a panel having excellent dent resistance from a high-strength steel sheet completed through the above-mentioned annealing process (final annealing) will be described. That is, an example of a method for manufacturing a panel having excellent surface appearance and dent resistance will be described by imparting a property of excellent surface appearance to the high-strength steel sheet itself and further subjecting the high-strength steel sheet to a heat treatment so as to impart excellent dent resistance to the high-strength steel sheet.
[0057] In a preferred method for manufacturing a panel in this embodiment, the high strength steel sheet after final annealing is subjected to a heat treatment before and after the cold plastic working. This method is (ii-i) a first heat treatment step of subjecting the high-strength steel plate to a heat treatment at a temperature T11 satisfying the following formula (2) for 60 to 900 seconds; (ii-ii) a blanking step of cutting the high strength steel plate into a blank shape; (ii-iii) a cold plastic working step of cold plastic working the blank to obtain a steel member; (ii-vi) a painting process for painting the steel members; (ii-v) A second heat treatment step of subjecting the steel members to a heat treatment at a temperature T12 of 80 to 200° C. for 300 to 1800 seconds to obtain a panel. 80×Si+100≦T11≦125×Si+250 (2) However, Si in the above formula (2) means the Si content (mass%) in the high-strength steel plate. [First heat treatment process] The high-strength steel sheet that has been subjected to the final annealing is then subjected to a first heat treatment step, which may be, for example, a tempering step.
[0058] The temperature T11 of the high-strength steel plate is preferably set within the range of the above formula (2). By setting the temperature T11 in the first heat treatment step to the above lower limit or higher, the effect of the major axis of the precipitates being 0.05 μm or more can be obtained. Also, by setting the temperature T11 to the above upper limit or lower, the effect of the number density being high and the major axis of the precipitates being 1.00 μm or less can be obtained.
[0059] In the first heat treatment step, the high strength steel sheet is preferably held at a constant temperature T11 within the range of the above formula (2) for 60 to 900 seconds. By holding the temperature T11 for a time period equal to or longer than the above lower limit in the first heat treatment step, the effect of stably precipitating iron carbides can be obtained. In addition, by holding the temperature T11 for a time period equal to or shorter than the above upper limit, the effect of increasing the number density of precipitates and having a major axis of 1.00 μm or less can be obtained. The high strength steel sheet that appears after the first heat treatment has precipitates with a major axis of 0.05 μm to 1.00 μm and an aspect ratio of 3 or more in the laths of martensite in the above-mentioned region at a density of 15 precipitates / μm. 2 It has the property of having the above.
[0060] [Blanking process] The high-strength steel plate that has been subjected to the first heat treatment is formed into a blank by blanking to a predetermined size. Note that the first heat treatment may be performed after the high-strength steel plate is formed into the blank.
[0061] [Cold plastic working process] Next, the blank is subjected to cold plastic working to form the steel member before it is baked and painted. Specifically, the blank is subjected to form forming as cold plastic working to form the steel member before it is baked and painted. The shape of the steel member corresponds to the shape of the panel.
[0062] Forming creates a steel component by applying prestrain to the entire blank. The amount of strain applied by forming is, for example, about 2%. By appropriately designing the forming conditions, such as the amount of punch movement in cold plastic processing, and the mold, and applying a prestrain of about 2%, the amount of bake hardening can be made sufficiently large.
[0063] [Painting process] Next, the steel member is painted. This painting includes, for example, three types of painting: electrodeposition painting, intermediate coating, and top coating (base and clear coating). Water-based paint or solvent-based paint is used for painting. In the electrodeposition painting process, the steel member is submerged in an electrodeposition tank containing paint, and the entire surface of the steel member is subjected to electrodeposition painting. In the intermediate coating painting process, the entire surface of the steel member is sprayed with paint from a spray nozzle by a painting robot or by manual labor by a worker, thereby applying intermediate coating. In the top coating painting process, the entire surface of the steel member is sprayed with paint from a spray nozzle by a painting robot or by manual labor by a worker, thereby applying top coating. As a result, the surface of the steel member is formed with a paint film having a thickness of about 100 μm.
[0064] [Second heat treatment process] The above-mentioned painting process includes a second heat treatment process. The second heat treatment is a baking and drying process for baking the paint film onto the steel member, and is a process for baking and hardening the steel member. The second heat treatment process may be carried out after electrodeposition painting and before undercoat painting, between undercoat painting and undercoat painting which are performed multiple times, after undercoat painting and before topcoat painting, between topcoat painting and topcoat painting which are performed multiple times, or after topcoat painting.
[0065] As described above, the temperature T12 of the steel members in the second heat treatment step is preferably set in the range of 80°C to 200°C. By setting the temperature T12 in the second heat treatment step to be equal to or higher than the above lower limit, the paint can be reliably baked onto the steel members, and the steel members can be more reliably hardened. Furthermore, if the temperature T12 exceeds the above upper limit, the cost of the panel manufacturing process increases. Therefore, the upper limit of the holding temperature is preferably set to 200°C or lower.
[0066] As described above, the holding time at temperature T12 in the second heat treatment is preferably set in the range of 300 to 1800 seconds. By setting the holding time in the second heat treatment step to be equal to or greater than the above lower limit, the paint can be reliably baked onto the steel members, and the steel members can be more reliably hardened. Furthermore, if the holding time exceeds 1800 seconds, the cost of the panel manufacturing process increases. Therefore, the holding time is preferably set to 1800 seconds or less.
[0067] In the second heat treatment step, the steel members are preferably held continuously at a constant temperature T12 within the above temperature range for 300 to 1800 seconds. By holding the temperature T12 for a time period equal to or longer than the above lower limit in the second heat treatment step, it is possible to obtain the effect of more reliably baking the paint. Furthermore, if the holding time for the temperature T12 exceeds the above upper limit, the manufacturing costs of the panel will increase. For this reason, it is preferable that the holding time for T12 be 1800 seconds or less.
[0068] The panel of this embodiment is completed through the painting process including the second heat treatment process described above.
[0069] In this embodiment, the high-strength steel plate used as the material for the panel is made more uniform by the first heat treatment process such as tempering, and the blank is uniformly strained during cold plastic working. As a result, the amount of bake hardening in the second heat treatment as a bake hardening process can be increased. This makes it possible to realize a panel that has excellent appearance and dent resistance after being formed from the material.
[0070] As described above, according to this embodiment, in a panel made of a steel plate containing martensite, the surface roughness parameter (Sa) in the flat portion of the center portion is Sa≦0.500 μm. This makes it possible to reduce unevenness on the panel surface. Furthermore, in the laths of martensite, precipitates with major axes of 0.05 μm to 1.00 μm and aspect ratios of 3 or more are formed at a density of 15 precipitates / μm. 2 or more. This can increase the amount of dislocations that are fixed due to carbon, etc., that diffuse during bake hardening, and as a result, the amount of bake hardening in the second heat treatment step can be significantly increased. Furthermore, the YS1 / YS2 ratio in the tensile test piece cut out from the flat portion is 0.90 to 1.10. This allows even strain to be applied to the entire flat portion and end portion of the panel, and bake hardening during paint baking occurs evenly throughout the steel plate in these flat portions and end portions. As described above, by specifying the surface roughness parameter Sa, the number density of precipitates, and YS1 / YS2, it is possible to achieve both excellent surface properties and excellent dent resistance in most of the range of plate thicknesses that are practically used for panels, particularly automobile exterior panels. And, for panels that have been requested to be made thinner in recent years, it is only when considering the compatibility of excellent surface properties and excellent dent resistance that the condition of the surface roughness parameter Sa≦0.500 μm and the number density of precipitates in the lath of 15 / μm are satisfied. 2 The above conditions have been devised. Furthermore, from the viewpoint of ensuring uniform dent resistance, the condition that YS1 / YS2 is 0.90 to 1.10 has been devised. By setting the number density of precipitates to 15 or more and setting YS1 / YS2 to 0.90 to 1.10, the uniformity of deformation during forming of the steel sheet is improved, and the occurrence of unevenness on the steel sheet surface can be suppressed. In this way, the panel of this embodiment can exhibit the synergistic effects of excellent surface quality and dent resistance in a thin panel. EXAMPLES
[0071] Next, an embodiment of the present invention will be described. The conditions in the embodiment are one example of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to this one example of conditions. The present invention can adopt various conditions as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.
[0072] <Production of high-strength steel plates> Steels having the chemical compositions shown in the billet Nos. A to E in Table 1 were melted, and slabs having a thickness of 240 to 300 mm were produced by continuous casting. The obtained slabs were heated to the temperatures shown in Table 2. The heated slabs were hot-rolled under the conditions shown in Table 2, and then coiled. In the hot rolling process, after the slab was heated, rough rolling was performed in a temperature range of 1050°C or higher and the heating temperature or lower, and reverse rolling with a rolling reduction of 30% or less per pass was performed for 8 passes, and the rolling reduction difference between two passes (return pass - forward pass) during one round trip was set to 10%, and after the rough rolling, the rolling was held for 7 seconds until finish rolling, and the subsequent finish rolling process was performed in four consecutive rolling stands, with the rolling reduction of the first stand being 20%. The coil was then unwound and the hot-rolled steel sheet was subjected to stress application. During this process, the surface residual stress was measured online using a portable X-ray residual stress measuring device while measuring the residual stress σ shown in Table 2. s The contact pressure of the brush on the steel plate surface was changed so that the contact pressure was such ... After that, the rolling reduction ratio (cumulative rolling reduction ratio R CR ) and cold rolling was performed to obtain steel sheets A1 to A2, B1 to B3, C1 to C2, D1 to D2, and E1 to E4.
[0073] Thereafter, annealing was performed under the conditions shown in Table 3, and the steel sheets were cooled to a temperature range of 550 to 650°C at the cooling rate shown in Table 3, and then cooled to the temperature shown in Table 3. Some of the steel sheets were also subjected to various plating processes to form a plating layer on the surface. In the table, CR indicates no plating, GI indicates hot-dip galvanizing, GA indicates alloyed hot-dip galvanizing, EG indicates electroplating, and Zn-Al-Mg, etc. indicate that plating containing these elements was performed.
[0074] <Production of bent parts using high-strength steel sheets> The first heat treatment (tempering) was performed on the steel sheets A1-A2, B1-B3, C1-C2, D1-D2, and E1-E4, which are high-strength steel sheets (cold-rolled steel sheets). The temperature of the high-strength steel sheets in the first heat treatment and the holding time at this temperature are shown in Table 4. Then, the high-strength steel sheets that were subjected to the first heat treatment were subjected to cold plastic working shown in Table 4 to form the cold-rolled steel sheets into the shape of a panel. As shown in Figures 2(A) and 2(B), the panel was a panel 200 formed from a 400 mm square steel sheet into a hogback shape with a ridge R of 1200 mm in the flat part at the center. Note that Figure 2(A) is a plan view of the part 200 used in the dent resistance evaluation. Figure 2(B) is a cross-sectional view taken along the line IIB-IIB in Figure 2(A). Next, the part formed into the shape of a panel was subjected to a second heat treatment (bake hardening) to produce a part that is a panel. The part numbers are as set forth in Table 4. The temperature of the parts in the second heat treatment and the hold time at this temperature are given in Table 4.
[0075] The metal structure of the surface layer region and the internal region of the obtained parts were observed. In addition, the number density of precipitates with a major axis of 0.05 μm to 1.00 μm and an aspect ratio of 3 or more was measured in the martensite laths of the internal region. The results are shown in Table 5.
[0076] The volume fraction of martensite in the surface layer region was determined by the following method. A sample (20 mm in the rolling direction × 20 mm in the width direction × thickness of the steel sheet) for observing the metal structure (microstructure) was taken from the flat part of the steel sheet of the obtained part, and the metal structure was observed from the surface layer of the steel sheet to 1 / 4 of the sheet thickness using an optical microscope, and the area ratio of martensite from the surface of the steel sheet (surface excluding the plating layer if plating was present) to 20 μm was calculated. To prepare the sample, the sheet thickness cross section perpendicular to the rolling direction was polished as the observation surface and etched with LePeller's reagent. The "microstructure" was classified from an optical microscope photograph at a magnification of 500 times, which was etched with LePeller's reagent. Ten fields of view were observed at a magnification of 500 times at a position of 1 / 4 thickness from the surface layer of the steel plate etched with LePeller's reagent, and a region 20 μm from the surface layer of the steel plate in the structure photograph was specified, and image analysis was performed using Adobe's "Photoshop CS5" image analysis software to determine the area fraction of martensite. Image analysis was performed in the same manner as above for a total of 10 fields of view to measure the area fraction of martensite, and these were then averaged to calculate the volume fraction of martensite in the surface layer region.
[0077] The average grain size of martensite in the surface layer region was determined by the following method. In the same manner as for the determination of the volume fraction of martensite, 10 fields of view were observed at a magnification of 500 times at a 1 / 4 thickness position from the surface layer of the steel plate etched with LePeller's reagent, and a 20 μm × 200 μm area was selected from the surface layer of the steel plate in the microstructure photograph, and image analysis was performed using Adobe's "Photoshop CS5" image analysis software to calculate the area occupied by martensite and the number of martensite particles. These were added together, and the area occupied by martensite was divided by the number of martensite particles to calculate the average area per martensite particle. From this area and number of particles, the circle equivalent diameter was calculated to be the average crystal grain size of martensite.
[0078] The volume fraction and average grain size of martensite in the internal region were also obtained by using steel plates etched with LePeller's reagent, selecting a range from the surface of the sample to a position of more than 20 μm to 1 / 4 of the plate thickness in the plate thickness direction, and analyzing the range in the same manner as for the surface region.
[0079] The precipitate number density refers to the density of precipitates with a major axis of 0.05 μm or more and 1.00 μm or less and an aspect ratio of 1:3 or more. The morphology and number density of precipitates are determined by observation with an electron microscope, and in this embodiment, they were measured by observation with a transmission electron microscope (TEM). Specifically, for the internal region, a thin film sample was cut out from a region from 3 / 8 to 1 / 4 of the thickness of the flat part of the steel plate, based on the surface of the flat part of the steel plate. The thin film sample was then observed in a bright field, and a 1 μm diameter was measured at an appropriate magnification of 10,000 to 100,000 times. 2 The number of precipitates with a major axis of 0.05 μm or more and 1 μm or less and an aspect ratio of 1:3 or more was counted. This operation was performed in five or more consecutive fields of view, and the average was taken as the number density.
[0080] Furthermore, the yield stress ratio YS1 / YS2 between the flat part and the end part, the ratio of yield stress to tensile strength YS1 / TS1, the tensile strength, the hardness of the flat part, and the panel thickness of the obtained parts were measured. The results are shown in Table 6. Table 6 also shows the steel type of the parts. DP steel stands for Dual Phase steel, and TRIP steel stands for Transformation Induced Plasticity steel.
[0081] Regarding the calculation of the yield stress ratio YS1 / YS2, the yield stress YS1 was determined by a tensile test performed in accordance with JIS Z 2241 using a JIS No. 5 test piece with the flat part cut out perpendicular to the rolling direction. The yield stress YS2 was determined by a tensile test performed in accordance with JIS Z 2241 using a JIS No. 5 test piece with the end cut out perpendicular to the rolling direction.
[0082] Regarding the calculation of the stress ratio YS1 / TS1, the tensile strength TS1 was determined by a tensile test performed in accordance with JIS Z 2241 using a JIS No. 5 test piece cut out from a flat portion perpendicular to the rolling direction.
[0083] The hardness of the flat part was measured using a micro Vickers hardness tester in accordance with JIS Z2244:2009. Measurements were performed at five arbitrary points at 1 / 4 depth from the surface on the cross section of the steel plate, with a test force of 4.9 N. The average of the obtained Vickers hardness values was regarded as the hardness of the flat part of the part.
[0084] [Table 1]
[0085] [Table 2]
[0086] [Table 3]
[0087] [Table 4]
[0088] [Table 5]
[0089] [Table 6]
[0090] [Table 7]
[0091] [Panel evaluation] [Panel surface quality evaluation] The manufactured parts were also evaluated for surface quality. The surface quality of a 3 mm square flat part of the part was measured using a laser microscope to obtain the measured surface, and wavelength components of 0.8 mm or less were removed from the measured surface using a low-pass filter (λs) specified in JIS B0601:2013, after which the surface was evaluated using the surface roughness parameter (Sa) specified in ISO25178. The evaluation standard for the surface quality of a part was that if Sa was 0.500 μm or less, the appearance after molding was good.
[0092] [Dent resistance evaluation] 3 is a side view of a test apparatus 20 for measuring the dent resistance of a part 200 and a cross-sectional view of the part 200, and the cross-section of the part 200 is shown along line IIB-II B in FIG. 2(A). Referring to FIG. 3, the test apparatus 20 has a load section 220. The load section 220 has two support columns 221a and 221b. These two support columns 221a and 221b are connected by a beam-shaped connecting section 222. An indenter rod holding section 223 that allows an indenter rod 224 to move up and down is provided at the center of the connecting section 222. The indenter rod 224 is provided with a held section 225 that is supported on the indenter rod holding section 223.
[0093] When the indenter rod 224 is moved downward by a motor mechanism or the like, a steel semi-spherical indenter 226 with a radius of 25 mm attached to the tip of the indenter rod 224 descends. The tip of the indenter 226 comes into contact with the center of the upper surface of the test panel 200 placed on the base 211 at approximately the center of the convex portion in the central side portion, and a load controlled to a predetermined constant value is applied to the center of the upper surface. As a result, a dent mark is formed on the test panel 200. Here, it is assumed that the load applied to the test panel 200 is constant. If the test panel 200 has good dent resistance, the dent mark formed will be shallow. In this embodiment, the dent resistance of the test panel 200 was evaluated by measuring the dent depth when a load of 20 kgf was applied to the test panel 200 by the indenter 226.
[0094] In this example, a spherical indenter 226 with a radius of 25 mm was pressed into the part with a force of 20 kgf and held for 5 seconds. The depression remaining after unloading was measured with a three-point dial gauge with a span of 40 mm, and the dent depth (mm) was recorded. Since the dent depth depends on the steel type and plate thickness of the part, parts that fall below the index S defined by the following formula were deemed to have excellent dent resistance. The index S indicates the standard dent depth. Formula: S=-0.0006×TS×t 2 +0.292 In addition, TS is the tensile strength and t is the thickness of the steel plate. The relationship between the index S and the dent depth of each part is shown in Figure 4. The horizontal axis of the graph in Figure 4 is TS x t 2 The vertical axis indicates the dent depth (mm). The line segment shown in FIG. 4 indicates the index S (index line).
[0095] [comprehensive evaluation] Table 7 shows the surface roughness parameter Sa of each part and the results of the dent resistance evaluation. Parts with a surface roughness parameter Sa of 0.500 μm or less were evaluated as having less surface irregularities and excellent appearance. In the dent resistance evaluation, parts with a dent depth of index S or less were evaluated as having excellent dent resistance. Table 7 also shows the ratio of dent depth to index S, and it can be seen that the smaller the ratio, the better the dent resistance.
[0096] Based on Tables 5 to 7, in the examples (Examples) in which the surface roughness parameter Sa, the number density of precipitates in the lath of martensite, and the yield stress ratio YS1 / YS2 of the flat portion are in the preferred range, the surface quality evaluation and the dent resistance evaluation of the panel cleared the standards. That is, in the Examples, the formation of surface irregularities after processing is suppressed, and further, it was demonstrated that the dent resistance is excellent. In particular, among the Examples, the parts D1a, D2a, E1a, E2a, and E4a have the number density of precipitates in the lath of martensite of 40 or more. These parts have the ninth, first, sixth, third, and second lowest index ratios among all the parts. Thus, it was demonstrated that, among the 18 Examples and Comparative Examples, the Examples in which the number density is 40 or more have particularly excellent dent resistance.
[0097] On the other hand, it was demonstrated that, for the examples (comparative examples) in which any one or more of the surface roughness parameter Sa, the number density of precipitates in the lath of martensite, and the yield stress ratio YS1 / YS2 of the flat portion were out of the preferred range, the surface properties were non-uniform, resulting in patterns or irregularities, or the dent resistance was poor, making them unsuitable for use as exterior panels. More specifically, the comparative example part A2a had a poor appearance because the surface roughness parameter Sa was below the standard. In addition, the part B1b had a yield stress ratio YS1 / YS2 out of the preferred range, so that the strain amount was biased in each part of the panel, and as a result, the bake hardening amount during paint baking was biased, resulting in dent resistance below the standard. In addition, the parts B2a and B3a had a poor appearance because the surface roughness parameter Sa was below the standard. In addition, the part C1b had a yield stress ratio YS1 / YS2 out of the preferred range, so that the dent resistance was below the standard for the above-mentioned reason. In addition, the surface roughness parameter Sa of the part C2a was below the standard, and therefore the appearance was poor. In addition, the number density of the precipitates in the martensite laths of the parts D1b and E1b was significantly below the preferred range, and the dent resistance was poor because the bake hardening was not sufficient. In addition, the surface roughness parameter Sa of the part E3a was below the standard, and therefore the appearance was poor. [Industrial Applicability]
[0098] The present invention can be widely applied to panels.
Claims
1. An automobile exterior panel having a steel plate containing martensite, The surface roughness parameter (Sa) in the flat portion of the central portion of the automobile exterior panel is Sa≦0.500 μm; In the lath of the martensite, precipitates having a major axis of 0.05 μm to 1.00 μm and an aspect ratio of 3 or more are arranged at 15 pieces / μm 2 More than The yield stress YS measured on a tensile test piece cut from the flat portion 1 and the yield stress YS measured on a tensile test piece cut from the end of the automobile exterior panel. 2 Compared to YS 1 / Y.S. 2 An automobile exterior panel, wherein the modulus of elasticity is 0.90 to 1.
10.
2. The yield stress YS of the tensile test piece cut out from the flat portion 1 and tensile strength TS 1 Compared to YS 1 / TS 1 2. The automotive skin panel of claim 1, wherein:
3. 3. The automobile exterior panel according to claim 1, wherein the hardness of the flat portion is 133 to 300 Hv.
4. The automobile exterior panel according to any one of claims 1 to 3, wherein the plate thickness of the flat portion is 0.20 mm to 0.60 mm.
5. The automobile exterior panel according to any one of claims 1 to 4, wherein the steel sheet is a dual-phase steel sheet.
6. The automobile exterior panel according to any one of claims 1 to 5, wherein the panel has a tensile strength of 400 to 900 MPa.
7. The automobile exterior panel further comprises an edge portion, the edge portion is a portion that is processed for being fixed to a member other than the automobile exterior panel and is fixed to the other member, The end portion is a portion adjacent to the edge portion and not fixed to the other member, The automobile exterior panel according to any one of claims 1 to 6, wherein the flat portion is disposed at a position extending from the end portion toward a central portion of the automobile exterior panel, and has a radius of curvature of 500 mm or more.
8. The steel plate further contains ferrite, 8. The automobile exterior panel according to claim 7, wherein in a surface region ranging from the surface of the steel plate to 20 μm in the plate thickness direction, when the volume fraction of the entire structure is 100%, the volume fraction of the ferrite is 50% or more, and the volume fraction of the martensite is 0.01% to 15.0%.
9. An automobile exterior panel as described in claim 8, wherein the chemical composition of the steel plate contains, by mass percentage, 0.010% or more and 3.000% or less of Si.
10. An automobile exterior panel as described in claim 9, wherein the plate thickness of the flat portion is 0.20 mm to 0.60 mm, and the tensile strength of the automobile exterior panel is 400 MPa to 900 MPa.
Citation Information
Patent Citations
Spinning method and multifilament yarn
JP1983046113A
Ferritic thin steel sheet
JP2016156079A
JPP4177478B
JPP6606905B