Catalyst, preparation method therefor, and use thereof

By catalyzing the deamination cyclization reaction under mild conditions using a carrier-loaded nickel-based catalyst, the problems of high catalyst cost and harsh reaction conditions in the existing technology are solved, and high-efficiency and low-cost preparation of piperidine is achieved, which has a wide range of industrial applications. prospect.

WO2024221494A1PCT designated stage expired Publication Date: 2024-10-31CATHAY BIOTECH INC +2

Patent Information

Application Number
PCT/CN2023/093215
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2023-05-10
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The existing technology has problems in catalyst selection and process conditions, such as high catalyst cost, harsh reaction conditions, many by-products, and high energy consumption. As a result, the industrial production cost of piperidine is high and it does not have the potential for large-scale production.

Method used

A carrier-supported nickel-based catalyst is used, including carriers such as alumina, silica, and diatomite, combined with nickel metal and its oxides, and the catalyst is prepared by co-precipitation, and is carried out in a dilute gas atmosphere at 80 to 200°C, 0.1 to 5 MPa The deamination cyclization reaction is carried out under the conditions to prepare efficient piperidine.

Benefits of technology

It achieves high-efficiency catalytic deamination cyclization reaction, reduces production costs, has high yield, high selectivity, simple operation, few by-products, and is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023093215-FTAPPB-I100001
    Figure PCTCN2023093215-FTAPPB-I100001
  • Figure PCTCN2023093215-FTAPPB-I100002
    Figure PCTCN2023093215-FTAPPB-I100002
  • Figure PCTCN2023093215-FTAPPB-I100003
    Figure PCTCN2023093215-FTAPPB-I100003
Patent Text Reader

Abstract

Disclosed in the present invention are a catalyst, a preparation method therefor, and a use thereof. The catalyst comprises 2-68 parts by weight of a carrier and 32-98 parts by weight of a metal catalyst. The metal catalyst contains a component (A) and an optional component (B), wherein the component (A) is a nickel metal and / or a nickel oxide, and the component (B) comprises at least one of Li, Na, K, Be, Mg, Ca, Cu, Co, Cr, Zr, Mo, Zn, Cd, Ru, Rh, Pd, Pt, LiO, Na2O, K2O, BeO, MgO, CaO, CuO, CoO, Cr2O3, ZrO2, Mo2O3, ZnO, CdO, RuO2, Rh2O3, PdO, and PtO2. The catalyst has high catalytic efficiency in a deamination cyclization reaction. Aliphatic nitrogen-containing heterocyclic compounds such as piperidine, pyrrolidine, morpholine, and piperazine are rapidly synthesized by means of one-step deamination cyclization reaction. The catalyst has the advantages of wide substrate range, high reaction efficiency, good selectivity, simple operation and small pollution, and has wide industrial application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Catalyst, preparation method and application thereof Technical Field

[0001] The present invention relates to the field of catalysts, and in particular to a catalyst, a preparation method thereof and an application thereof. Background Art

[0002] Heterocyclic compounds are an important class of organic compounds that are inseparable from human life. According to statistics, at least half of the drug molecules approved by the U.S. Food and Drug Administration (FDA) contain at least one nitrogen-containing heterocyclic ring. On the other hand, nitrogen-containing aliphatic heterocyclic compounds such as piperidine (C5H 11 N), pyrrolidine (C4H9N), morpholine (C4H9NO), cycloheximide (C7H 15 N), piperazine (C4H 10 N2) are widely used in the pharmaceutical and chemical fields as raw materials, catalysts, solvents, etc. In recent years, with the continuous development of new drug molecules and the upgrading of synthesis processes, the application fields of aliphatic nitrogen-containing heterocyclic compounds have been continuously broadened, and their application prospects are broad.

[0003] Traditional synthesis methods typically use the corresponding aromatic nitrogen-containing heterocycles in the presence of Raney nickel as a catalyst. Under high temperature and high pressure, catalytic hydrogenation can yield nitrogen-containing aliphatic heterocyclic compounds. Due to incomplete hydrogenation, the post-reaction material often contains some of the starting materials, and due to their similar molecular weight, subsequent separation and purification are difficult.

[0004] Regarding 2-piperidine carboxylate, a foreign literature (Tetrahedron: Asymmetry, 2006, 17(12): 1775-1779.) reported that an enzyme-catalyzed method can effectively convert lysine into 2-piperidine carboxylate, with the characteristics of low energy consumption and high yield. However, due to the unique selectivity of the enzyme, the conversion rate for lysine analogs is low and the substrate applicability is poor.

[0005] Pentamethylenediamine is an important C5 platform compound that can be obtained through biofermentation of biomass such as corn and straw. It is a fully bio-based 5-carbon molecule. There have been some reports on methods for preparing piperidine through catalytic deamination using pentamethylenediamine as a raw material under the action of a catalyst. The selection of catalyst is the key. Typical catalyst has: the U.S. Patent No. 2863872 disclosed in 1958 adopts silica gel, silica-alumina gel etc. as catalyst, prepares piperidines by gas-solid phase reaction in a fixed-bed reactor, reaction temperature 300-500 ℃, and reaction mass obtains product piperidines through condensation, distillation, and the highest yield is 62.3%; American scholars have reported a kind of noble metal catalyst, take pentamethylenediamine as raw material in diphenyl ether organic solvent, prepares piperidines under the existence of 2% (molar percentage) triphenylphosphine ruthenium chloride catalyst, reaction temperature 180 ℃, 5 hours, yield 79% (JOC, 1981,46,1759-1760); Japanese scholars then find in water, with 50% catalyst levels (with respect to pentamethylenediamine), using aluminum powder as additive, with>95% yield from pentamethylenediamine synthetic piperidines. The above-mentioned method for synthesizing piperidine using a catalyst, which uses silica gel as a catalyst for a fixed-bed gas-solid phase reaction, has low yields and produces a large amount of high-boiling-point by-products, which greatly complicates the purification and recovery of the product and increases production costs. While the piperidine synthesis method using noble metals as catalysts has improved yields, the catalysts are expensive and the reaction conditions are harsh, making it unsuitable for large-scale industrial production.

[0006] On the other hand, Chinese patent CN104844539A reports a process for converting bio-based 1,5-pentanediamine into piperidine. Piperidine can be obtained in the presence of a modified molecular sieve catalyst, but the temperature is above 300°C, the energy consumption is high, and the production cost is large, so it does not have the capacity for large-scale production.

[0007] Summary of the Invention

[0008] The present invention aims to solve one of the technical problems existing in the prior art. To this end, the present invention provides a catalyst and a preparation method and application thereof.

[0009] In a first aspect, the present invention provides a catalyst. According to an embodiment of the present invention, the catalyst comprises: 2 to 68 parts by weight of a carrier and 32 to 98 parts by weight of a metal catalyst, wherein the metal catalyst is supported on the carrier, wherein the metal catalyst is component (A) and optional component (B); wherein component (A) is nickel metal and / or nickel oxide; component (B) comprises at least one of Li, Na, K, Be, Mg, Ca, Cu, Co, Cr, Zr, Mo, Zn, Cd, Ru, Rh, Pd, Pt, LiO, Na2O, KO, BeO, MgO, CaO, CuO, CoO, Cr2O3, ZrO2, Mo2O3, ZnO, CdO, RuO2, Rh2O3, PdO, and PtO2; and the carrier comprises at least one of alumina, silicon oxide, diatomaceous earth, activated carbon, molecular sieve, and zeolite.

[0010] In a second aspect, the present invention provides a method for preparing the above-mentioned catalyst. According to an embodiment of the present invention, the method comprises: mixing the metal salts corresponding to component (A) and component (B) with a carrier, and co-precipitating to prepare the catalyst.

[0011] In a third aspect, the present invention provides a method for preparing an aliphatic nitrogen-containing heterocyclic compound. According to an embodiment of the present invention, the method comprises reacting an aliphatic diamine raw material and a catalyst at a temperature of 80 to 200° C. and a pressure of 0.1 to 5 MPa in a dilute gas atmosphere, and isolating the aliphatic nitrogen-containing heterocyclic compound after the reaction.

[0012] In a fourth aspect, the present invention provides a method for continuously preparing an aliphatic nitrogen-containing heterocyclic compound. According to an embodiment of the present invention, the method comprises: (a) loading a catalyst into a reaction apparatus; (b) introducing an aliphatic diamine raw material and a diluent gas into the reaction apparatus, and controlling the temperature and pressure of the reaction apparatus; and (c) collecting the product and separating the aliphatic nitrogen-containing heterocyclic compound.

[0013] In a fifth aspect, the present invention provides a method for preparing piperidine. According to an embodiment of the present invention, the method comprises reacting pentamethylenediamine in a dilute gas atmosphere at a temperature of 80 to 200°C and a pressure of 0.1 to 5 MPa, and separating the piperidine after the reaction.

[0014] In a sixth aspect, the present invention provides a method for continuously preparing piperidine. According to an embodiment of the present invention, the method comprises: (i) loading a catalyst into a reaction apparatus; (ii) introducing pentamethylenediamine as a raw material and a diluent gas into the reaction apparatus, and controlling the temperature and pressure of the reaction apparatus; and (iii) collecting the product and separating it to obtain piperidine.

[0015] In a seventh aspect, the present invention provides a bio-based piperidine prepared using the above-described method. According to embodiments of the present invention, the bio-based piperidine has a platinum-cobalt color number of less than 8, a purity greater than 99.7%, a water content of less than 1000 ppm, a pyridine content of less than 1000 ppm, preferably less than 10 ppm, a pentamethylenediamine content of less than 100 ppm, and a density of 0.860-0.865 g / L.

[0016] In an eighth aspect of the present invention, a bio-based piperidine is provided. According to an embodiment of the present invention, the bio-based piperidine is prepared using bio-based pentamethylenediamine as a raw material.

[0017] In a ninth aspect of the present invention, the present invention provides an application of bio-based piperidine. According to an embodiment of the present invention, the application includes the application of bio-based piperidine as a rubber accelerator, pesticide, and pharmaceutical synthesis raw material.

[0018] The present invention has the following beneficial effects:

[0019] (1) The present invention provides a catalyst that has high catalytic efficiency for deamination cyclization reaction and reduces production costs;

[0020] (2) The present invention utilizes commonly available aliphatic diamines or their salts as raw materials to rapidly synthesize aliphatic nitrogen-containing heterocyclic compounds through a one-step deamination cyclization reaction. This method has the advantages of a wide substrate range, high reaction efficiency, good selectivity, simple operation, and low pollution, and has broad industrial application prospects.

[0021] (3) The present invention can obtain piperidine in high yield and high selectivity under mild conditions. The process is simple to operate, produces few by-products, and causes little pollution. Piperidine can be obtained quickly, has the potential for large-scale production, and is conducive to industrial application.

[0022] (4) The present invention provides a bio-based piperidine. Compared with the existing commercially available piperidine, all carbon atoms of the bio-based piperidine are derived from bio-based raw materials. The quality meets the industry standard T-4485-2002, is equivalent to that of commercially available piperidine, and does not contain pyridine impurities. It can be further used in rubber accelerators, pesticides, medicines and other fields.

[0023] Additional aspects and advantages of the present invention will be set forth in part in the description which follows and, in part, will be obvious from the description which follows, or may be learned by practice of the present invention. DETAILED DESCRIPTION

[0024] The present invention will be further described below in conjunction with preferred embodiments and comparative examples. It should be noted that the embodiments described are only representative embodiments and do not represent all embodiments. The specific description below is illustrative rather than restrictive and should not be used to limit the scope of protection of the present invention.

[0025] In a first aspect, the present invention provides a catalyst. According to an embodiment of the present invention, the catalyst comprises: 2 to 68 parts by weight of a carrier and 32 to 98 parts by weight of a metal catalyst, wherein the metal catalyst is supported on the carrier, wherein the metal catalyst is component (A) and optional component (B); wherein component (A) is nickel metal and / or nickel oxide; component (B) comprises at least one of Li, Na, K, Be, Mg, Ca, Cu, Co, Cr, Zr, Mo, Zn, Cd, Ru, Rh, Pd, Pt, LiO, Na2O, KO, BeO, MgO, CaO, CuO, CoO, Cr2O3, ZrO2, Mo2O3, ZnO, CdO, RuO2, Rh2O3, PdO, and PtO2; and the carrier comprises at least one of alumina, silica, diatomaceous earth, activated carbon, molecular sieve, and zeolite, preferably at least one of alumina, silica, and diatomaceous earth. The inventors discovered that component (A) can undergo redox reactions to form different chemical states such as 0, +1, and +2, which can cause primary amines to undergo β-hydrogen elimination to form imines. The imines can further undergo deamination cyclization and reduction reactions to generate cyclic secondary amine compounds. Component (B) can provide active centers, reduce the reaction activation energy, and enable the reaction to proceed at lower temperatures.

[0026] According to a specific embodiment of the present invention, the mass ratio of component (A) to component (B) is (30-80): (0-12).

[0027] According to a specific embodiment of the present invention, component (B) is preferably Na and Mg. The inventors have found that the introduction of Na and Mg enhances the basicity of the catalyst surface, reduces the adsorption of amine compounds on the catalyst surface, thereby extending the catalyst life, and reduces the formation of by-products, thereby improving selectivity.

[0028] According to a specific embodiment of the present invention, component (B) is preferably Cr and Na.

[0029] According to a specific embodiment of the present invention, the support is preferably at least one of alumina, silica, and diatomaceous earth. The inventors have discovered that alumina can react with the nickel in component (A) to induce hydrogen overflow, thereby enhancing catalytic activity. The introduction of silica and alumina can also modulate the surface acidity and alkalinity of the catalyst, thereby regulating catalytic activity.

[0030] In the present invention, when the supported nickel-based catalyst contains magnesium, the magnesium is preferably present in the form of magnesium oxide. When the supported nickel-based catalyst contains sodium, the sodium is preferably present in the form of sodium oxide. When the supported nickel-based catalyst contains chromium, the chromium is preferably present in the form of metallic chromium and chromium oxide.

[0031] In a second aspect, the present invention provides a method for preparing the above-mentioned catalyst. According to an embodiment of the present invention, the method comprises: mixing the metal salts corresponding to component (A) and component (B) with a carrier, and co-precipitating to prepare the catalyst.

[0032] According to a specific embodiment of the present invention, component (A) is nickel metal and / or nickel oxide, and component (B) includes at least one of Li, Na, K, Be, Mg, Ca, Cu, Co, Cr, Zr, Mo, Zn, Cd, Ru, Rh, Pd, Pt, LiO, Na2O, K2O, BeO, MgO, CaO, CuO, CoO, Cr2O3, ZrO2, Mo2O3, ZnO, CdO, RuO2, Rh2O3, PdO, and PtO2.

[0033] According to a specific embodiment of the present invention, the metal salts corresponding to the above-mentioned component (A) and component (B) are preferably nickel nitrate, magnesium nitrate, chromium nitrate and sodium carbonate.

[0034] According to a specific embodiment of the present invention, the carrier includes at least one of aluminum oxide, silicon oxide, diatomaceous earth, activated carbon, molecular sieve and zeolite, preferably at least one of aluminum oxide, silicon oxide and diatomaceous earth.

[0035] According to a specific embodiment of the present invention, the mass ratio of the salt corresponding to component (A), the salt corresponding to component (B), and the carrier is (30-80): (0-12): (5-30).

[0036] According to a specific embodiment of the present invention, nickel nitrate, magnesium nitrate and sodium carbonate are mixed with water, and then aluminum oxide and / or silicon oxide and / or diatomaceous earth are added to prepare the catalyst by co-precipitation.

[0037] According to a specific embodiment of the present invention, nickel nitrate, chromium nitrate and sodium carbonate are mixed with water, and then aluminum oxide and / or silicon oxide and / or diatomaceous earth are added to prepare the catalyst by co-precipitation.

[0038] It should be noted that the co-precipitation method is a conventional method in the art and will not be described in detail here.

[0039] It should be noted that the characteristics and advantages described above for the catalyst are also applicable to the preparation method of the catalyst and will not be repeated here.

[0040] In a third aspect, the present invention provides a method for preparing an aliphatic nitrogen-containing heterocyclic compound. The method comprises reacting an aliphatic diamine raw material and a catalyst in a dilute gas atmosphere at a temperature of 80 to 200° C. and a pressure of 0.1 to 5 MPa, and separating the aliphatic nitrogen-containing heterocyclic compound after the reaction. The aliphatic diamine raw material comprises an aliphatic diamine or a salt thereof having the following structural formula:

[0041] wherein m is any integer in the range of 0-3, n is any integer in the range of 0-3, m+n≥1, R1 is hydrogen or methyl, R2 to R5 are independently selected from any one of hydrogen, methyl, carboxyl or ester, and X is selected from any one of CH2, O, NH, NMe or NEt.

[0042] According to a specific embodiment of the present invention, the aliphatic diamine raw material includes at least one of an aliphatic diamine, an aliphatic diamine diluted with a solvent, and a salt solution of an aliphatic diamine.

[0043] According to a specific embodiment of the present invention, the solvent in the solvent-diluted aliphatic diamine includes at least one of water, alkanes, alcohols, acids, esters, amides, aromatic hydrocarbons, pyridine and organic amines, with a concentration of 10 to 100 wt%, preferably 20 to 100 wt%.

[0044] According to a specific embodiment of the present invention, the salt solution of the aliphatic diamine includes at least one of hydrochloride, carbonate / bicarbonate, sulfate, phosphate and organic acid salt, and the concentration is 10-100 wt%, preferably 20-100 wt%.

[0045] The inventors have discovered that, under the reaction conditions, the raw materials of aliphatic diamines can be rapidly synthesized into aliphatic nitrogen-containing heterocyclic compounds through a deamination cyclization reaction as shown in the next step. This preparation method has the characteristics of a wide substrate range, high reaction efficiency, good selectivity, simple operation, and low pollution. It has broad industrial application prospects. At the same time, ammonia as a by-product can be converted into compounds such as ammonia water, liquid ammonia, ammonium sulfate, etc. for application in other fields.

[0046] According to a specific embodiment of the present invention, the above-mentioned catalyst is preferably the catalyst described in any technical solution of the first aspect of the present invention, which will not be described in detail here.

[0047] According to a specific embodiment of the present invention, the added amount of the catalyst is 0.1 to 10 wt% of the aliphatic diamine, preferably 0.5 to 5 wt%, for example, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt%, 5.5 wt%, 6 wt%, 6.5 wt%, 7 wt%, 7.5 wt%, 8 wt%, 8.5 wt%, 9 wt%, 9.5 wt%, etc.

[0048] According to a specific embodiment of the present invention, the reaction temperature is preferably 100-180° C., for example, 110° C., 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., etc. A lower reaction temperature can effectively avoid the formation of side reactions, while reducing production energy consumption and reducing safety hazards.

[0049] According to a specific embodiment of the present invention, the reaction pressure is preferably 0.5-3 MPa, for example, 0.6 MPa, 0.7 MPa, 0.8 MPa, 0.9 MPa, 1.0 MPa, 1.5 MPa, 2.0 MPa, 2.5 MPa, etc.

[0050] According to a specific embodiment of the present invention, the diluent gas includes at least one of hydrogen, ammonia, nitrogen, argon, and water vapor, preferably hydrogen. Since the reaction does not consume any gas in principle, the diluent gas serves only as a shielding gas. Therefore, the gas flow rate is sufficient to maintain a constant pressure within the system.

[0051] It should be noted that the apparatus for the above reaction is not particularly limited, for example, a microreactor, a reaction kettle, a round-bottom flask, etc.

[0052] It should be noted that the above separation methods are conventional technologies in the art, such as any one of atmospheric distillation, vacuum distillation, atmospheric rectification, and vacuum rectification, and will not be described in detail here.

[0053] It should be noted that the features and advantages described above for the catalyst and its preparation method are also applicable to the method for preparing aliphatic nitrogen-containing heterocyclic compounds, and will not be repeated here.

[0054] In a fourth aspect of the present invention, the present invention provides a method for continuously preparing an aliphatic nitrogen-containing heterocyclic compound. According to an embodiment of the present invention, the method comprises:

[0055] Sa: Load the catalyst into the reaction device

[0056] In this step, the catalyst is loaded into the reaction device. The raw material of the aliphatic diamine contains an aliphatic diamine or a salt thereof having the following structural formula:

[0057] wherein m is any integer in the range of 0-3, n is any integer in the range of 0-3, m+n≥1, R1 is hydrogen or methyl, R2 to R5 are independently selected from any one of hydrogen, methyl, carboxyl or ester, and X is selected from any one of CH2, O, NH, NMe or NEt.

[0058] According to a specific embodiment of the present invention, the above-mentioned catalyst is preferably the catalyst described in any technical solution of the first aspect of the present invention, which will not be described in detail here.

[0059] According to a specific embodiment of the present invention, the reaction apparatus includes at least one of a fixed bed reactor, a fluidized bed reactor and a slurry bed reactor.

[0060] Sb: Feed the raw materials of aliphatic diamine and diluent gas into the reaction device and control the temperature and pressure of the reaction device

[0061] In this step, the raw material of the aliphatic diamine and the diluent gas are introduced into the reaction device, and the temperature and pressure of the reaction device are controlled. Preferably, the raw material of the aliphatic diamine and the diluent gas are preheated before being introduced into the reaction device.

[0062] According to a specific embodiment of the present invention, the aliphatic diamine raw material includes at least one of an aliphatic diamine, an aliphatic diamine diluted with a solvent, and a salt solution of an aliphatic diamine.

[0063] According to a specific embodiment of the present invention, the solvent in the solvent-diluted aliphatic diamine includes at least one of water, alkanes, alcohols, acids, esters, amides, aromatic hydrocarbons, pyridine and organic amines, with a concentration of 10 to 100 wt%, preferably 20 to 100 wt%.

[0064] According to a specific embodiment of the present invention, the salt solution of the aliphatic diamine includes at least one of hydrochloride, carbonate / bicarbonate, sulfate, phosphate and organic acid salt, and the concentration is 10-100 wt%, preferably 20-100 wt%.

[0065] According to a specific embodiment of the present invention, the temperature of the reaction device is 80-200° C., preferably 100-180° C., for example, 90° C., 110° C., 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., 190° C., etc. A lower reaction temperature can effectively avoid the formation of side reactions, while reducing production energy consumption and reducing safety hazards.

[0066] According to a specific embodiment of the present invention, the pressure of the reaction device is 0.1-5 MPa, preferably 0.5-3 MPa, for example, 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.6 MPa, 0.7 MPa, 0.8 MPa, 0.9 MPa, 1.0 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, etc.

[0067] According to a specific embodiment of the present invention, the dilution gas includes at least one of hydrogen, ammonia, nitrogen, argon and water vapor, preferably hydrogen.

[0068] According to a specific embodiment of the present invention, the molar ratio of the diluent gas to the raw material of the aliphatic diamine is (0-1):1, such as 0.2:1, 0.4:1, 0.6:1, 0.8:1, etc.

[0069] According to a specific embodiment of the present invention, the mass space velocity of the raw material of the aliphatic diamine is 0.1 to 10 h -1 , preferably 0.1 to 3 hours -1 , for example 0.5h -1 , 1h -1 , 1.5h -1 , 2h -1 , 2.5h -1 , 3.5h -1 , 4h -1 , 4.5h -1 , 5h - 1 , 5.5h -1 , 6h -1 , 6.5h -1 , 7h -1 , 7.5h -1 , 8h -1 , 8.5h -1 , 9h -1 , 9.5h -1 wait.

[0070] Sc: Collect the product and separate the aliphatic nitrogen-containing heterocyclic compound

[0071] In this step, the product is collected and separated to obtain an aliphatic nitrogen-containing heterocyclic compound.

[0072] It should be noted that the above separation methods are conventional technologies in the art, such as any one of atmospheric distillation, vacuum distillation, atmospheric rectification, and vacuum rectification, and will not be described in detail here.

[0073] It should be noted that the characteristics and advantages described above for the preparation method of aliphatic nitrogen-containing heterocyclic compounds are also applicable to the method for continuously preparing aliphatic nitrogen-containing heterocyclic compounds, and will not be repeated here.

[0074] In a fifth aspect, the present invention provides a method for preparing piperidine. According to an embodiment of the present invention, the method comprises reacting pentamethylenediamine and a catalyst in a dilute gas atmosphere at a temperature of 80 to 200°C and a pressure of 0.1 to 5 MPa, and separating the piperidine after the reaction.

[0075] The inventors found that the reaction can obtain piperidine with high yield and high selectivity under mild conditions. The process is simple to operate, has few by-products and little pollution, can quickly obtain piperidine, has the potential for large-scale production, and is conducive to industrial application.

[0076] According to a specific embodiment of the present invention, the above-mentioned catalyst is preferably the catalyst described in any technical solution of the first aspect of the present invention, which will not be described in detail here.

[0077] According to a specific embodiment of the present invention, the raw material of pentamethylenediamine includes at least one of pentamethylenediamine, a fermentation broth of a pentamethylenediamine salt, a treated liquid of a fermentation broth of a pentamethylenediamine salt, an enzyme conversion liquid of a pentamethylenediamine salt, a treated liquid of an enzyme conversion liquid of a pentamethylenediamine salt, a pentamethylenediamine salt solution, and pentamethylenediamine diluted with a solvent.

[0078] According to a specific embodiment of the present invention, the solvent in the solvent-diluted pentamethylenediamine includes at least one of water, alkanes, alcohols, acids, esters, amides, aromatic hydrocarbons, pyridine and organic amines, with a concentration of 10 to 100 wt%, preferably 20 to 100 wt%.

[0079] According to a specific embodiment of the present invention, the pentamethylenediamine salt solution includes at least one of pentamethylenediamine hydrochloride, pentamethylenediamine carbonate / bicarbonate, pentamethylenediamine sulfate, pentamethylenediamine phosphate and pentamethylenediamine organic acid salt, with a concentration of 10 to 100 wt%, preferably 20 to 100 wt%.

[0080] The present invention does not particularly limit the specific preparation method of the enzymatic conversion liquid of pentamethylenediamine salt or the fermentation liquid of pentamethylenediamine salt prepared by direct fermentation. A person skilled in the art can select specific raw materials and determine specific process parameters of the enzymatic conversion process according to existing technologies to obtain the enzymatic conversion liquid of pentamethylenediamine salt or the fermentation liquid of pentamethylenediamine salt.

[0081] Specifically, when the mixture containing pentamethylenediamine salt is a pentamethylenediamine salt enzyme conversion solution, it can be obtained by reacting a lysine salt solution under the action of lysine decarboxylase (LDC). The lysine salt can be an inorganic salt or an organic salt of lysine, such as lysine hydrochloride or lysine sulfate.

[0082] When the mixture containing pentamethylenediamine salt is a fermentation broth of pentamethylenediamine salt, it is generally obtained by the following method: using genetic technology to upregulate the expression of lysine decarboxylase in a strain capable of producing lysine, or recombinantly expressing lysine decarboxylase, the produced lysine can be simultaneously converted into pentamethylenediamine during the fermentation process, thereby directly obtaining a fermentation broth containing pentamethylenediamine salt. The present invention has no particular requirements for the recombinant bacteria, as long as pentamethylenediamine can be produced. For example, PCT / CN2015 / 094121 discloses a method for directly producing pentamethylenediamine by fermentation. Those skilled in the art will understand how to optimize the culture medium components, ratios, and fermentation process parameters based on the specific recombinant bacteria.

[0083] According to a specific embodiment of the present invention, the pentamethylenediamine is preferably bio-based pentamethylenediamine. Specifically, bio-based pentamethylenediamine refers to pentamethylenediamine synthesized from biomass-derived compounds such as glucose and lysine through enzyme reaction, yeast reaction or fermentation reaction in the monomer synthesis process. The bio-based content of bio-based pentamethylenediamine can be determined by a method for measuring the radioactive C14 content, such as the American Society for Testing and Materials standard ASTM-D6866 method. By using bio-based pentamethylenediamine as a raw material, it is independent of petroleum resources and does not cause serious pollution to the environment, thereby reducing carbon dioxide emissions, reducing the generation of the greenhouse effect, adapting to the carbon neutrality development trend, and further preparing bio-based piperidine.

[0084] According to a specific embodiment of the present invention, the added amount of the catalyst is 0.1-10wt% of the pentamethylenediamine raw material, preferably 0.5-5wt%, for example, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt%, etc.

[0085] According to a specific embodiment of the present invention, the reaction temperature is preferably 100-180° C., for example, 110° C., 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., etc. A lower reaction temperature can effectively avoid the formation of side reactions, while reducing production energy consumption and reducing safety hazards.

[0086] According to a specific embodiment of the present invention, the reaction pressure is preferably 0.5-3 MPa, for example, 0.6 MPa, 0.7 MPa, 0.8 MPa, 0.9 MPa, 1.0 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, etc.

[0087] According to a specific embodiment of the present invention, the diluent gas includes at least one of hydrogen, ammonia, nitrogen, argon, and water vapor, preferably hydrogen. Since the reaction does not consume any gas in principle, the diluent gas serves only as a shielding gas. Therefore, the gas flow rate is sufficient to maintain a constant pressure within the system.

[0088] It should be noted that the apparatus for the above reaction is not particularly limited, for example, a microreactor, a reaction kettle, a round-bottom flask, etc.

[0089] It should be noted that the above separation methods are conventional technologies in the art, such as any one of atmospheric distillation, vacuum distillation, atmospheric rectification, and vacuum rectification, and will not be described in detail here.

[0090] It should be noted that the features and advantages described above for the catalyst and its preparation method are also applicable to the method for preparing piperidine and will not be described in detail here.

[0091] In a sixth aspect of the present invention, the present invention provides a method for continuously preparing piperidine. According to an embodiment of the present invention, the method comprises:

[0092] Si: Load the catalyst into the reaction device

[0093] In this step, the catalyst is loaded into the reaction device. According to a specific embodiment of the present invention, the catalyst is preferably the catalyst described in any technical solution of the first aspect of the present invention, which will not be described in detail here.

[0094] According to a specific embodiment of the present invention, the reaction apparatus includes at least one of a fixed bed reactor, a fluidized bed reactor and a slurry bed reactor.

[0095] Sii: The raw materials of pentamethylenediamine and diluent gas are introduced into the reaction device, and the temperature and pressure of the reaction device are controlled.

[0096] In this step, the raw material of pentamethylenediamine and the diluent gas are introduced into the reaction device, and the temperature and pressure of the reaction device are controlled. Preferably, the raw material of pentamethylenediamine and the diluent gas are preheated before being introduced into the reaction device.

[0097] According to a specific embodiment of the present invention, the pentamethylenediamine raw material includes at least one of pentamethylenediamine, a fermentation broth of a pentamethylenediamine salt, a treated liquid of a fermentation broth of a pentamethylenediamine salt, an enzyme conversion liquid of a pentamethylenediamine salt, a treated liquid of an enzyme conversion liquid of a pentamethylenediamine salt, a pentamethylenediamine salt solution, and pentamethylenediamine diluted with a solvent.

[0098] According to a specific embodiment of the present invention, the solvent in the solvent-diluted pentamethylenediamine includes at least one of water, alkanes, alcohols, acids, esters, amides, aromatic hydrocarbons, pyridine and organic amines, with a concentration of 10 to 100 wt%, preferably 20 to 100 wt%.

[0099] According to a specific embodiment of the present invention, the pentamethylenediamine salt solution includes at least one of hydrochloride, carbonate / bicarbonate, sulfate, phosphate and organic acid salt, with a concentration of 10 to 100 wt%, preferably 20 to 100 wt%.

[0100] The present invention does not particularly limit the specific preparation method of the enzymatic conversion liquid of pentamethylenediamine salt or the fermentation liquid of pentamethylenediamine salt prepared by direct fermentation. A person skilled in the art can select specific raw materials and determine specific process parameters of the enzymatic conversion process according to existing technologies to obtain the enzymatic conversion liquid of pentamethylenediamine salt or the fermentation liquid of pentamethylenediamine salt.

[0101] Specifically, when the mixture containing pentamethylenediamine salt is a pentamethylenediamine salt enzyme conversion solution, it can be obtained by reacting a lysine salt solution under the action of lysine decarboxylase (LDC). The lysine salt can be an inorganic salt or an organic salt of lysine, such as lysine hydrochloride or lysine sulfate.

[0102] When the mixture containing pentamethylenediamine salt is a fermentation broth of pentamethylenediamine salt, it is generally obtained by the following method: using genetic technology to upregulate the expression of lysine decarboxylase in a strain capable of producing lysine, or recombinantly expressing lysine decarboxylase, the produced lysine can be simultaneously converted into pentamethylenediamine during the fermentation process, thereby directly obtaining a fermentation broth containing pentamethylenediamine salt. The present invention has no particular requirements for the recombinant bacteria, as long as pentamethylenediamine can be produced. For example, PCT / CN2015 / 094121 discloses a method for directly producing pentamethylenediamine by fermentation. Those skilled in the art will understand how to optimize the culture medium components, ratios, and fermentation process parameters based on the specific recombinant bacteria.

[0103] According to a specific embodiment of the present invention, the pentamethylenediamine is bio-based pentamethylenediamine. Specifically, bio-based pentamethylenediamine refers to pentamethylenediamine synthesized from biomass-derived compounds such as glucose and lysine through enzyme reactions, yeast reactions, or fermentation reactions in the monomer synthesis process. The biobased content of bio-based pentamethylenediamine can be determined by measuring the radioactive C14 content, such as the American Society for Testing and Materials standard ASTM-D6866 method. By using bio-based pentamethylenediamine as a raw material, it is independent of petroleum resources and does not cause serious pollution to the environment. It can reduce carbon dioxide emissions, reduce the generation of the greenhouse effect, adapt to the development trend of carbon neutrality, and further prepare bio-based piperidine.

[0104] According to a specific embodiment of the present invention, the temperature of the reaction device is 80-200° C., preferably 100-180° C., for example, 90° C., 110° C., 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., 190° C., etc. A lower reaction temperature can effectively avoid the formation of side reactions, while reducing production energy consumption and reducing safety hazards.

[0105] According to a specific embodiment of the present invention, the pressure is 0.1-5 MPa, preferably 0.5-3 MPa, for example, 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.6 MPa, 0.7 MPa, 0.8 MPa, 0.9 MPa, 1.0 MPa, 1.5 MPa, 2.0 MPa, 2.5 MPa, etc.

[0106] According to a specific embodiment of the present invention, the dilution gas includes at least one of hydrogen, ammonia, nitrogen, argon and water vapor, preferably hydrogen.

[0107] According to a specific embodiment of the present invention, the molar ratio of the diluent gas to the raw material of pentamethylenediamine is (0-1):1, for example, 0.2:1, 0.4:1, 0.6:1, 0.8:1, etc.

[0108] According to a specific embodiment of the present invention, the mass space velocity of the raw material of pentamethylenediamine is 0.1~10h -1 , preferably 0.1 to 3 hours -1 , for example 0.5h -1 , 1h -1 , 1.5h -1 , 2h -1 , 2.5h -1 , 3.5h -1 , 4h -1 , 4.5h -1 , 5h -1 , 5.5h -1 , 6h -1 , 6.5h -1 , 7h -1 , 7.5h -1 , 8h -1 , 8.5h -1 , 9h -1 , 9.5h -1 wait.

[0109] Siii: Collect the product and separate the piperidine

[0110] In this step, the product is collected and isolated to obtain piperidine.

[0111] It should be noted that the above separation methods are conventional technologies in the art, such as any one of atmospheric distillation, vacuum distillation, atmospheric rectification, and vacuum rectification, and will not be described in detail here.

[0112] It should be noted that the features and advantages described above for the preparation method of piperidine are also applicable to the method for continuous preparation of piperidine, and will not be described in detail here.

[0113] In a seventh aspect, the present invention provides a bio-based piperidine prepared using the above-described method. According to embodiments of the present invention, the bio-based piperidine has a platinum-cobalt color number of less than 8, a purity of >99.7%, a water content of less than 1000 ppm, a pyridine content of less than 1000 ppm, preferably less than 10 ppm, a pentamethylenediamine content of less than 100 ppm, and a density of 0.860-0.865 g / L.

[0114] According to a specific embodiment of the present invention, the bio-based piperidine does not contain pyridine.

[0115] According to a specific embodiment of the present invention, the bio-based piperidine does not contain pentamethylenediamine.

[0116] In its eighth aspect, the present invention provides a bio-based piperidine, wherein the raw material for preparing the bio-based piperidine is bio-based pentamethylenediamine. Specifically, the bio-based pentamethylenediamine is synthesized from biomass-derived compounds such as glucose and lysine through an enzyme reaction, yeast reaction, or fermentation reaction during the monomer synthesis process. The biobased content of the bio-based pentamethylenediamine can be determined by measuring the radioactive C14 content, such as the American Society for Testing and Materials standard ASTM-D6866 method.

[0117] According to a specific embodiment of the present invention, the platinum-cobalt color number of the bio-based piperidine is less than 8, the purity is >997%, the water content is below 1000 ppm, the pyridine content is below 1000 ppm, preferably below 10 ppm, the pentamethylenediamine content is below 100 ppm, and the density is 0.860-0.865 g / L.

[0118] According to a specific embodiment of the present invention, the bio-based piperidine does not contain pyridine.

[0119] According to a specific embodiment of the present invention, the bio-based piperidine does not contain pentamethylenediamine.

[0120] In a ninth aspect of the present invention, the present invention provides an application of bio-based piperidine. According to an embodiment of the present invention, the application includes the application of bio-based piperidine as a rubber accelerator, pesticide, and pharmaceutical synthesis raw material.

[0121] According to a specific embodiment of the present invention, the rubber accelerator includes at least one of dipentamethylenethiuram tetrasulfide, dipentamethylenethiuram disulfide, 1-piperidinyldithiocarbamate, and dipentamethylenethiuram hexasulfide.

[0122] According to a specific embodiment of the present invention, the pesticide includes at least one of mepiquat and chlorpyrifos.

[0123] According to a specific embodiment of the present invention, the medicine includes at least one of minoxidil, roxatidine acetate hydrochloride and dipyridamole raw materials.

[0124] It should be noted that the characteristics and advantages described above for bio-based piperidine are also applicable to the application of this bio-based piperidine and will not be repeated here.

[0125] Below, the scheme of the present invention will be explained in conjunction with embodiment.It will be understood by those skilled in the art that the following examples are only used to illustrate the present invention and should not be regarded as limiting the scope of the present invention.In the embodiment, if specific technology or conditions are not indicated, the technology or conditions described in the literature in this area or the product instructions are used.The reagents or instruments used are not indicated by the manufacturer, and are all conventional products that can be obtained by commercial purchase.

[0126] Bio-based pentamethylenediamine was purchased from Cathay (Jinxiang) Biomaterials Co., Ltd.

[0127] The preparation method of the catalyst used in the following examples is as follows:

[0128] Catalyst A: At room temperature, 1820g of nickel nitrate and 142g of magnesium nitrate were dissolved in 10L of water. 1050g of sodium carbonate solvent was added to 10L of water. Under vigorous stirring, the nickel-containing solution was added dropwise to the sodium carbonate solution, and 200g of diatomaceous earth was added. After the addition was completed, the mixture was stirred for 3h and filtered. The resulting filter cake was dispersed in 5L of 0.25% NaOH solution, stirred for 2h, filtered, and the filter cake was dried to obtain catalyst powder. The catalyst was granulated to obtain a crude catalyst, which was heated and activated under H2 atmosphere before use.

[0129] Catalyst B: At room temperature, 1820g of nickel nitrate and 119g of chromium nitrate were dissolved in 10L of water. 1050g of sodium carbonate solvent was added to 10L of water. Under vigorous stirring, the nickel-containing solution was added dropwise to the sodium carbonate solution, and 200g of diatomaceous earth was added. After the addition was completed, the mixture was stirred for 3h and filtered. The resulting filter cake was dispersed in 5L of 0.25% NaOH solution, stirred for 2h, filtered, and the filter cake was dried to obtain catalyst powder. The catalyst was granulated to obtain a crude catalyst, which was heated and activated under H2 atmosphere before use.

[0130] Catalyst C: At room temperature, 1820g of nickel nitrate was dissolved in 10L of water with vigorous stirring, and 200g of aluminum oxide was added. After the addition was completed, the mixture was stirred for 3h and filtered. The resulting filter cake was dispersed in 5L of 0.25% NaOH solution and stirred for 2h. The filter cake was dried to obtain catalyst powder. The catalyst was granulated to obtain a crude catalyst, which was heated and activated under H2 atmosphere before use.

[0131] Example 1

[0132] At room temperature, 80g of bio-based pentamethylenediamine and 0.2g of Catalyst A were added to a 1L autoclave. The autoclave was closed, the atmosphere was purged with nitrogen, and 0.5MPa of hydrogen was introduced. The heat was turned on with stirring, and the temperature was raised to 180°C for 17 hours. After the reaction, the reaction system was cooled to room temperature, and the pressure in the autoclave was slowly reduced. The exhaust gas was absorbed by water to produce ammonia. The catalyst and product in the autoclave were separated by filtration to obtain a liquid containing bio-based piperidine. The bio-based pentamethylenediamine conversion rate was 86.69%, and the bio-based piperidine selectivity was 97.8% (the conversion rate is the proportion of pentamethylenediamine consumed, and the selectivity is the proportion of consumed pentamethylenediamine converted to piperidine). The product was distilled to obtain bio-based piperidine with a purity of >99.7%.

[0133] The indicators of the prepared bio-based piperidine are shown in Table 1 below, and the testing items are carried out in accordance with the HG / T4485-2012 standard.

[0134] Table 1

[0135] Example 2

[0136] At room temperature, 80g of bio-based pentamethylenediamine and 0.2g of Catalyst B were added to a 1L autoclave. The autoclave was closed, the atmosphere purged with nitrogen, and filled with 0.5MPa of hydrogen. Heating and stirring were then initiated, and the temperature was raised to 180°C for 17 hours. After the reaction, the system was cooled to room temperature, and the pressure in the autoclave was slowly reduced. The exhaust gas was absorbed by water to produce ammonia water. The catalyst and product in the autoclave were then filtered to separate, yielding a liquid containing bio-based piperidine. The bio-based pentamethylenediamine conversion was 72.31%, and the bio-based piperidine selectivity was 90.2%.

[0137] Example 3

[0138] At room temperature, 80g of bio-based pentamethylenediamine and 0.2g of Catalyst C were added to a 1L autoclave. The autoclave was closed, the atmosphere purged with nitrogen, and filled with 0.5MPa of hydrogen. Heating and stirring were then initiated, and the temperature was raised to 180°C for 17 hours. After the reaction, the reaction system was cooled to room temperature, and the pressure in the autoclave was slowly reduced. The exhaust gas was absorbed by water to produce ammonia water. The catalyst and product in the autoclave were then filtered to separate, yielding a liquid containing bio-based piperidine. The bio-based pentamethylenediamine conversion was 100%, and the bio-based piperidine selectivity was 98.2%.

[0139] Example 4

[0140] Approximately 100 g of Catalyst A was loaded into a stainless steel reactor with an inner diameter of 20 mm and a length of 720 mm. Electric heating and automatic temperature control were used. The reactor bottom was filled with a 20-40 mesh inert material, and the catalyst bed was filled with a 20-40 mesh inert material. The raw material, bio-based pentamethylenediamine, was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction conditions and results are shown in Table 2.

[0141] Table 2: Catalyst A for the synthesis of piperidine under hydrogen atmosphere reaction conditions and results

[0142] Example 5

[0143] Approximately 100 g of Catalyst A was loaded into a stainless steel reactor with an inner diameter of 20 mm and a length of 720 mm. Electric heating and automatic temperature control were used. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. The raw bio-based pentamethylenediamine was mixed with nitrogen carrier gas and passed through the catalyst bed from top to bottom. The reaction conditions and results are shown in Table 3.

[0144] Table 3 Catalyst A is used for the reaction conditions and results of piperidine synthesis under nitrogen atmosphere

[0145] Example 6

[0146] Approximately 100 g of Catalyst C was loaded into a stainless steel reactor with an inner diameter of 20 mm and a length of 720 mm. Electric heating and automatic temperature control were used. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. The raw bio-based pentamethylenediamine was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction conditions and results are shown in Table 4.

[0147] Table 4 Reaction conditions and results of catalyst C for piperidine synthesis

[0148] Example 7

[0149] Approximately 100 g of catalyst C was loaded into a fixed-bed reactor with an inner diameter of 20 mm and a length of 720 mm. Electric heating was used, and the temperature was automatically controlled. The bottom of the reactor was filled with an inert material with a mesh size of 20 to 40, and the top of the catalyst was filled with an inert material with a mesh size of 20 to 40. The raw material, diaminobenzene, was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C, and the space velocity was 1 h. -1 , pressure is 0.2 MPa, the molar ratio of hydrogen to diamine is 0.2, the reaction conversion rate is 100%, and the selectivity of the product pyrrolidine is 99.5%.

[0150] Example 8

[0151] At room temperature, 80g of butanediamine and 0.2g of Catalyst C were added to a 1L autoclave. The autoclave was closed, the atmosphere purged with nitrogen, and filled with 0.5MPa of hydrogen. Heating and stirring were initiated, and the temperature was raised to 180°C for 17 hours. After the reaction, the reaction system was cooled to room temperature, and the pressure in the autoclave was slowly reduced. The exhaust gas was absorbed by water to produce ammonia water. The catalyst and product in the autoclave were separated by filtration to obtain piperidine liquid. The butanediamine conversion was 99.7%, and the pyrrolidine selectivity was 98.1%.

[0152] Example 9

[0153] About 100g of catalyst C was loaded into a fixed-bed reactor with an inner diameter of 20mm and a length of 720mm. Electric heating was used and the temperature was automatically controlled. The bottom of the reactor was filled with an inert material of 20-40 mesh, a certain amount of catalyst was filled in the reactor, and the upper part of the catalyst was filled with an inert material of 20-40 mesh. The raw material hexamethylenediamine was mixed with the carrier gas hydrogen and passed through the catalyst bed from top to bottom. The reaction temperature was 150℃ and the space velocity was 1h. -1 , pressure 0.2 MPa, molar ratio of hydrogen to hexamethylenediamine 0.2, reaction conversion rate 100%, and selectivity of product cycloheximide 83.6%.

[0154] Example 10

[0155] About 100g of catalyst C was loaded into a fixed-bed reactor with an inner diameter of 20mm and a length of 720mm. Electric heating was used and the temperature was automatically controlled. The bottom of the reactor was filled with an inert material of 20-40 mesh, a certain amount of catalyst was filled in the reactor, and the upper part of the catalyst was filled with an inert material of 20-40 mesh. The raw material heptanediamine was mixed with the carrier gas hydrogen and passed through the catalyst bed from top to bottom. The reaction temperature was 150℃ and the space velocity was 1h. -1 , pressure 0.2 MPa, molar ratio of hydrogen to heptyldiamine 0.2, reaction conversion rate 100%, product cycloheptylimine selectivity 72.3%.

[0156] Example 11

[0157] About 100g of catalyst C was loaded into a fixed-bed reactor with an inner diameter of 20mm and a length of 720mm. Electric heating was used and the temperature was automatically controlled. The bottom of the reactor was filled with an inert material of 20-40 mesh, a certain amount of catalyst was filled in the reactor, and the upper part of the catalyst was filled with an inert material of 20-40 mesh. A 20% aqueous solution of the raw material lysine was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the space velocity was 1h. -1 , pressure 0.2 MPa, molar ratio of hydrogen to lysine was 0.2, reaction conversion rate was 56%, and selectivity of product 2-piperidinic acid was 72.3%.

[0158] Example 12

[0159] Approximately 100 g of catalyst C was loaded into a fixed-bed reactor with an inner diameter of 20 mm and a length of 720 mm. Electric heating and automatic temperature control were used. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. The raw material, 2-methyl-1,5-pentanediamine, was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the space velocity was 1 h. -1 , pressure 0.2 MPa, molar ratio of hydrogen to 2-methyl-1,5-pentanediamine 0.2, reaction conversion rate 100%, product 3-methylpiperidine selectivity 99.6%.

[0160] Example 13

[0161] Approximately 100 g of catalyst C was loaded into a fixed-bed reactor with an inner diameter of 20 mm and a length of 720 mm. Electric heating was used, and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. The raw material ethylenediamine was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C, and the space velocity was 1 h. -1 , pressure 0.2 MPa, molar ratio of hydrogen to ethylenediamine 0.2, reaction conversion rate 100%, product piperazine selectivity 97.2%.

[0162] Example 14

[0163] At room temperature, 80g of ethylenediamine and 0.2g of Catalyst C were added to a 1L autoclave. The autoclave was closed, the atmosphere purged with nitrogen, and filled with 0.5MPa of hydrogen. The heat was turned on with stirring, and the temperature was raised to 180°C for 17 hours. After the reaction, the reaction system was cooled to room temperature, and the pressure in the autoclave was slowly reduced. The exhaust gas was absorbed by water to produce ammonia water. The catalyst and product in the autoclave were separated by filtration to obtain piperidine liquid. The ethylenediamine conversion was 100%, and the piperazine selectivity was 99.2%.

[0164] Example 15

[0165] About 100g of catalyst C was loaded into a fixed bed reactor with an inner diameter of 20mm and a length of 720mm. Electric heating was used and the temperature was automatically controlled. The bottom of the reactor was filled with an inert material of 20-40 mesh, a certain amount of catalyst was filled in the reactor, and the top of the catalyst was filled with an inert material of 20-40 mesh. The raw material diglycolamine was mixed with the carrier gas hydrogen and passed through the catalyst bed from top to bottom. The reaction temperature was 150℃ and the space velocity was 1h. -1 , pressure 0.2 MPa, molar ratio of hydrogen to diglycolamine 0.2, reaction conversion rate 100%, product morpholine selectivity 98.6%.

[0166] Example 16

[0167] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. The reactor was heated electrically and the temperature was automatically controlled. The bottom of the reactor was filled with an inert material of 20-40 mesh, and the top of the catalyst was filled with an inert material of 20-40 mesh. The raw material 1,4-cis-cyclohexanediamine was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the space velocity was 1 h. -1 , pressure 0.2 MPa, molar ratio of hydrogen to 1,4-cis-cyclohexanediamine was 0.2, reaction conversion rate was 100%, and selectivity of product 7-azabicyclo[2.2.1]heptane was 91.6%.

[0168] Example 17

[0169] Approximately 100 g of catalyst C was loaded into a fixed-bed reactor with an inner diameter of 20 mm and a length of 720 mm. Electric heating was used, and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. The raw material, N-methylpentanediamine, was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C, and the space velocity was 1 h. -1 , pressure 0.2 MPa, molar ratio of hydrogen to N-monomethylpentanediamine 0.2, reaction conversion rate 100%, product N-methylpiperidine selectivity 99.7%.

[0170] Example 18

[0171] At room temperature, 80g of N-monomethylpentanediamine and 0.2g of Catalyst C were added to a 1L autoclave. The autoclave was closed, the atmosphere was purged with nitrogen, and 0.5MPa of hydrogen was introduced. The reaction was heated and stirred, and the temperature was raised to 180°C for 17 hours. After the reaction, the reaction system was cooled to room temperature, and the pressure in the autoclave was slowly reduced. The exhaust gas was absorbed by water to produce aqueous ammonia. The catalyst and product in the autoclave were separated by filtration to obtain a piperidine liquid. The N-monomethylpentanediamine conversion was 100%, and the N-methylpiperidine selectivity was 99.6%.

[0172] Example 19

[0173] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. The reactor was electrically heated and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A 20% solution of pentamethylenediamine in cyclohexane was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the space velocity was 1 h. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 100%, product piperidine selectivity 99.4%.

[0174] Example 20

[0175] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. The reactor was electrically heated and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A 20% solution of pentamethylenediamine in piperidine was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the space velocity was 1 h / min. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 100%, product piperidine selectivity 99.2%.

[0176] Example 21

[0177] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. The reactor was electrically heated and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A 20% solution of pentamethylenediamine in toluene was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the space velocity was 1 h / min. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 86%, product piperidine selectivity 99.5%.

[0178] Example 22

[0179] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. The reactor was electrically heated and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A 20 wt% solution of pentamethylenediamine in pyridine was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the air space velocity was 1 h / min. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 75%, product piperidine selectivity 98.7%.

[0180] Example 23

[0181] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. The reactor was electrically heated and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A 20 wt% solution of pentamethylenediamine in cyclohexane was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the space velocity was 1 h / min. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 100%, product piperidine selectivity 99.6%.

[0182] Example 24

[0183] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. The reactor was electrically heated and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A 20% methanol solution of pentamethylenediamine was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the space velocity was 1 h / min. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 100%, product piperidine selectivity 69.6%.

[0184] Example 25

[0185] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. The reactor was electrically heated and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A 20% aqueous solution of pentamethylenediamine was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the air velocity was 1 h / min. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 72%, product piperidine selectivity 90.6%.

[0186] Example 26

[0187] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. The reactor was electrically heated and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A 20% aqueous solution of pentamethylenediamine hydrochloride was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the air velocity was 1 h / min. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 22%, product piperidine hydrochloride selectivity 95.6%.

[0188] Example 27

[0189] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. The reactor was electrically heated and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A 20% aqueous solution of pentamethylenediamine carbonate was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the air space velocity was 1 h / min. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 43%, product piperidine carbonate selectivity 95.6%.

[0190] Example 28

[0191] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. The reactor was electrically heated and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A 20% aqueous solution of pentamethylenediamine sulfate was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the air velocity was 1 h / min. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 21%, product piperidine sulfate selectivity 90.6%.

[0192] Example 29

[0193] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. The reactor was electrically heated and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A 20% aqueous solution of pentamethylenediamine phosphate was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 150°C and the air velocity was 1 h / min. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 34%, product piperidine phosphate selectivity 91.8%.

[0194] Comparative Example 1

[0195] At room temperature, 80g of pentamethylenediamine and 0.2g of Ru / C catalyst (purchased from Adamas Reagents) were added to a 1L autoclave. The autoclave was closed, the atmosphere purged with nitrogen, and filled with 0.5MPa of hydrogen. The heat was turned on with stirring, and the temperature was raised to 180°C for 17 hours. After the reaction, the reaction system was cooled to room temperature, and the pressure in the autoclave was slowly reduced. The exhaust gas was absorbed by water to produce ammonia water. The catalyst and product in the autoclave were separated by filtration to obtain piperidine liquid. The pentamethylenediamine conversion was 41.3%, and the piperidine selectivity was 89%.

[0196] Comparative Example 2

[0197] At room temperature, 80g of pentamethylenediamine and 0.2g of Ru / C catalyst (purchased from Adamas Reagents) were added to a 1L autoclave. The autoclave was closed, the atmosphere purged with nitrogen, and filled with 0.5MPa of hydrogen. The heat was turned on with stirring, and the temperature was raised to 200°C for 17 hours. After the reaction, the reaction system was cooled to room temperature, and the pressure in the autoclave was slowly reduced. The exhaust gas was absorbed by water to produce ammonia water. The catalyst and product in the autoclave were separated by filtration to obtain piperidine liquid. The pentamethylenediamine conversion was 82.6%, and the piperidine selectivity was 82%.

[0198] Comparative Example 3

[0199] At room temperature, 80g of pentamethylenediamine and 0.2g of Ru / C catalyst (purchased from Adamas Reagents) were added to a 1L autoclave. The autoclave was closed, the atmosphere purged with nitrogen, and filled with 0.5MPa of hydrogen. The heat was turned on with stirring, and the temperature was raised to 160°C for 17 hours. After the reaction, the reaction system was cooled to room temperature, and the pressure in the autoclave was slowly reduced. The exhaust gas was absorbed by water to produce ammonia water. The catalyst and product in the autoclave were separated by filtration to obtain piperidine liquid. The pentamethylenediamine conversion was 21.9%, and the piperidine selectivity was 93%.

[0200] Comparative Example 4

[0201] At room temperature, 80g of pentamethylenediamine and 0.2g of Catalyst C were added to a 1L autoclave. The autoclave was closed, the atmosphere purged with nitrogen, and filled with 0.5MPa of hydrogen. Heating and stirring were initiated, and the temperature was raised to 80°C for 17 hours. After the reaction, the reaction system was cooled to room temperature, and the pressure in the autoclave was slowly reduced. The exhaust gas was absorbed by water to produce aqueous ammonia. The catalyst and product in the autoclave were separated by filtration to obtain piperidine liquid. The pentamethylenediamine conversion was 6.7%, and the piperidine selectivity was 99.7%.

[0202] Comparative Example 5

[0203] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. Electric heating and automatic temperature control were used. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A mixture of pentamethylenediamine and hydrogen as carrier gas was passed through the catalyst bed from top to bottom. The reaction temperature was 70°C and the space velocity was 0.5 h / min. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 9.7%, product piperidine selectivity 99.8%.

[0204] Comparative Example 6

[0205] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. The reactor was electrically heated and the temperature was automatically controlled. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A 20 wt% solution of pentamethylenediamine in pyridine was mixed with hydrogen as a carrier gas and passed through the catalyst bed from top to bottom. The reaction temperature was 70°C and the space velocity was 10 h / min. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 11.3%, product piperidine selectivity 99.9%.

[0206] Comparative Example 7

[0207] Approximately 100 g of catalyst C was loaded into a reactor with an inner diameter of 20 mm and a length of 720 mm. Electric heating and automatic temperature control were used. The bottom of the reactor was filled with a 20-40 mesh inert material, and the top of the catalyst was filled with a 20-40 mesh inert material. A mixture of pentamethylenediamine and hydrogen as carrier gas was passed through the catalyst bed from top to bottom. The reaction temperature was 220°C and the space velocity was 0.5 h / min. -1 , pressure 0.2 MPa, molar ratio of hydrogen to pentamethylenediamine 0.2, reaction conversion rate 100%, product piperidine selectivity 61.5%.

[0208] Comparative Example 8

[0209] At room temperature, 80g of butanediamine and 0.2g of Ru / C catalyst (purchased from Adamas Reagents) were added to a 1L autoclave. The autoclave was closed, the atmosphere purged with nitrogen, and filled with 0.5MPa of hydrogen. Heating and stirring were then turned on, and the temperature was raised to 180°C for 17 hours. After the reaction, the reaction system was cooled to room temperature, and the pressure in the autoclave was slowly reduced. The exhaust gas was absorbed by water to produce ammonia water. The catalyst and product in the autoclave were separated by filtration to obtain pyrrolidine liquid. The butanediamine conversion was 51.3%, and the pyrrolidine selectivity was 88%.

[0210] Comparative Example 9

[0211] At room temperature, 80g of N-monomethylpentanediamine and 0.2g of Ru / C catalyst (purchased from Adamas Reagents) were added to a 1L autoclave. The autoclave was closed, the atmosphere was purged with nitrogen, and 0.5MPa of hydrogen was introduced. The reactor was heated and stirred, and the temperature was raised to 180°C for 17 hours. After the reaction, the reaction system was cooled to room temperature, and the pressure in the reactor was slowly reduced. The exhaust gas was absorbed by water to produce ammonia water. The catalyst and product in the reactor were separated by filtration to obtain N-methylpiperidine liquid. The N-monomethylpentanediamine conversion rate was 61.7%, and the N-methylpiperidine selectivity was 92%.

[0212] The foregoing descriptions of specific exemplary embodiments of the present invention are for purposes of illustration and description. These descriptions are not intended to limit the invention to the precise forms disclosed, and it is apparent that many variations and modifications are possible in light of the foregoing teachings. The exemplary embodiments have been selected and described for the purpose of explaining the specific principles of the invention and their practical application, thereby enabling those skilled in the art to realize and utilize a variety of exemplary embodiments of the invention and various options and modifications. The scope of the invention is intended to be defined by the claims and their equivalents.

Claims

1. A catalyst, characterized in that The catalyst comprises: 2 to 68 parts by weight of a carrier and 32 to 98 parts by weight of a metal catalyst, wherein the metal catalyst is supported on the carrier, wherein the metal catalyst is component (A) and optional component (B); Wherein, the component (A) is nickel metal and / or nickel oxide; The component (B) includes at least one of Li, Na, K, Be, Mg, Ca, Cu, Co, Cr, Zr, Mo, Zn, Cd, Ru, Rh, Pd, Pt, LiO, Na2O, KO, BeO, MgO, CaO, CuO, CoO, Cr2O3, ZrO2, Mo2O3, ZnO, CdO, RuO2, Rh2O3, PdO, and PtO2; The carrier includes at least one of alumina, silica, diatomaceous earth, activated carbon, molecular sieve and zeolite.

2. The catalyst according to claim 1, characterized in that The mass ratio of the component (A) to the component (B) is (30-80):(0-12).

3. A method for preparing the catalyst according to claim 1 or 2, characterized in that: The method comprises: mixing the metal salts corresponding to the component (A) and the component (B) with a carrier, and co-precipitating to prepare a catalyst.

4. The method according to claim 3, characterized in that The mass ratio of the salt corresponding to the component (A), the salt corresponding to the component (B) and the carrier is (30-80): (0-12): (5-30); Optionally, the component (A) is nickel metal and / or nickel oxide; Optionally, the component (B) includes at least one of Li, Na, K, Be, Mg, Ca, Cu, Co, Cr, Zr, Mo, Zn, Cd, Ru, Rh, Pd, Pt, LiO, Na2O, K2O, BeO, MgO, CaO, CuO, CoO, Cr2O3, ZrO2, Mo2O3, ZnO, CdO, RuO2, Rh2O3, PdO, and PtO2; Optionally, the carrier includes at least one of alumina, silica, diatomaceous earth, activated carbon, molecular sieve and zeolite.

5. A method for preparing an aliphatic nitrogen-containing heterocyclic compound, characterized in that: The method comprises: reacting a raw material of an aliphatic diamine and a catalyst under the conditions of a temperature of 80 to 200° C. and a pressure of 0.1 to 5 MPa in a diluent gas atmosphere, and separating to obtain an aliphatic nitrogen-containing heterocyclic compound after the reaction, wherein the raw material of the aliphatic diamine contains an aliphatic diamine or a salt thereof having the following structural formula: Wherein, m is any integer in the range of 0-3, n is any integer in the range of 0-3, m+n≥1, R1 is hydrogen or methyl, R2 to R5 are independently selected from any one of hydrogen, methyl, carboxyl or ester, and X is selected from any one of CH2, O, NH, NMe or NEt.

6. The method according to claim 5, characterized in that The catalyst is the catalyst according to claim 1 or 2; Optionally, the catalyst is added in an amount of 0.1 to 10 wt %, preferably 0.5 to 5 wt % of the aliphatic diamine raw material; Optionally, the temperature is 100 to 180°C; Optionally, the pressure is 0.5 to 3 MPa; Optionally, the dilution gas includes at least one of hydrogen, ammonia, nitrogen, argon and water vapor, preferably hydrogen.

7. A method for continuously preparing aliphatic nitrogen-containing heterocyclic compounds, characterized in that: The method comprises: (a) loading a catalyst into a reaction device; (b) introducing a raw material of an aliphatic diamine and a diluent gas into a reaction device, and controlling the temperature and pressure of the reaction device, preferably the raw material of the aliphatic diamine and the diluent gas are preheated before being introduced into the reaction device; (c) collecting the product and separating the aliphatic nitrogen-containing heterocyclic compound; The raw material of the aliphatic diamine contains an aliphatic diamine or a salt thereof having the following structural formula: wherein m is any integer in the range of 0-3, n is any integer in the range of 0-3, m+n≥1, R1 is hydrogen or methyl, R2 to R5 are independently selected from any one of hydrogen, methyl, carboxyl or ester, and X is selected from any one of CH2, O, NH, NMe or NEt.

8. The method according to claim 7, characterized in that In step (a), the catalyst is the catalyst according to claim 1 or 2; Optionally, in step (a), the reaction apparatus comprises at least one of a fixed bed reactor, a fluidized bed reactor and a slurry bed reactor; Optionally, in step (b), the temperature is 80 to 200°C, preferably 100 to 180°C; Optionally, in step (b), the pressure is 0.1 to 5 MPa, preferably 0.5 to 3 MPa; Optionally, in step (b), the diluent gas comprises at least one of hydrogen, ammonia, nitrogen, argon and water vapor, preferably hydrogen; Optionally, in step (b), the molar ratio of the diluent gas to the raw material of the aliphatic diamine is (0-1):1; Optionally, in step (b), the mass space velocity of the raw material of the aliphatic diamine is 0.1 to 10 h -1 , preferably 0.1 to 3 hours -1 .

9. A method for preparing piperidine, characterized in that: The method comprises: reacting pentamethylenediamine raw materials and a catalyst under the conditions of a temperature of 80-200° C. and a pressure of 0.1-5 MPa in a dilute gas atmosphere, and separating and obtaining piperidine after the reaction.

10. The method according to claim 9, characterized in that The catalyst of the reaction is the catalyst according to claim 1 or 2; Optionally, the catalyst is added in an amount of 0.1 to 10 wt %, preferably 0.5 to 5 wt %, of the raw material of pentamethylenediamine; Optionally, the temperature is 100 to 180°C; Optionally, the pressure is 0.5 to 3 MPa; Optionally, the diluent gas includes at least one of hydrogen, ammonia, nitrogen, argon and water vapor, preferably hydrogen; Optionally, the raw material of pentamethylenediamine is bio-based pentamethylenediamine, and bio-based piperidine is prepared.

11. A method for continuously preparing piperidine, characterized in that: The method comprises: (i) loading the catalyst into a reaction device; (ii) introducing a raw material of pentamethylenediamine and a diluent gas into a reaction device, and controlling the temperature and pressure of the reaction device. Preferably, the raw material of pentamethylenediamine and the diluent gas are preheated before being introduced into the reaction device; (iii) collecting the product and isolating the piperidine.

12. The method according to claim 11, characterized in that In step (i), the catalyst is the catalyst according to claim 1 or 2; Optionally, in step (i), the reaction apparatus comprises at least one of a fixed bed reactor, a fluidized bed reactor and a slurry bed reactor; Optionally, in step (ii), the temperature is 80 to 200°C, preferably 100 to 180°C; Optionally, in step (ii), the pressure is 0.1 to 5 MPa, preferably 0.5 to 3 MPa; Optionally, in step (ii), the raw material of pentamethylenediamine is bio-based pentamethylenediamine; Optionally, in step (ii), the diluent gas comprises at least one of hydrogen, ammonia, nitrogen, argon and water vapor, preferably hydrogen; Optionally, in step (ii), the molar ratio of the diluent gas to the raw material of pentamethylenediamine is (0-1):1; Optionally, in step (ii), the mass space velocity of the raw material of pentamethylenediamine is 0.1 to 10 h -1 , preferably 0.1 to 3 hours -1 .

13. A bio-based piperidine prepared by the method according to claim 10, characterized in that: The bio-based piperidine has a platinum-cobalt color number of less than 8, a purity of>99.7%, a water content of less than 1000 ppm, a pyridine content of less than 1000 ppm, preferably less than 10 ppm, a pentamethylenediamine content of less than 100 ppm, and a density of 0.860-0.865 g / L.

14. The bio-based piperidine according to claim 13, characterized in that The bio-based piperidine does not contain pyridine; and / or, The bio-based piperidine does not contain pentamethylenediamine.

15. A bio-based piperidine, characterized in that: It is prepared using bio-based pentamethylenediamine as raw material; Optionally, the bio-based piperidine has a platinum-cobalt color number of less than 8, and / or, Purity>99.7%, and / or, The water content is below 1000 ppm; and / or, The pyridine content is below 1000 ppm, preferably below 10 ppm; and / or, The content of pentamethylenediamine is below 100 ppm; and / or, The density is 0.860-0.865g / L.

16. The bio-based piperidine according to claim 15, characterized in that The bio-based piperidine does not contain pyridine; and / or, The bio-based piperidine does not contain pentamethylenediamine.

17. A use of the bio-based piperidine as claimed in claim 15 or 16, characterized in that: The applications include the use of bio-based piperidine as a rubber accelerator, pesticide and pharmaceutical synthesis raw material; Optionally, the rubber accelerator includes at least one of dipentamethylenethiuram tetrasulfide, dipentamethylenethiuram disulfide, piperidinium 1-piperidinyl dithiocarboxylate and dipentamethylenethiuram hexasulfide; Optionally, the pesticide includes at least one of mepiquat and chloranil; Optionally, the medicine comprises at least one of minoxidil, roxatidine acetate hydrochloride and dipyridamole raw materials.

Citation Information

Patent Citations

  • Piperidine preparation method

    CN104844539A

  • Oligomerization catalyst and process for the production thereof

    CN110270359A

  • Dry reforming of methane using a nickel-based bi-metallic catalyst

    US20230050019A1

Cited By

  • Industrial method for continuous and efficient catalytic synthesis of m-nitroaniline