Piezoelectric composite material and preparation method therefor, and ultrasonic transducer

By adding mica powder, glass microbeads and boron nitride to the passive phase, and using specific process methods, the thermal stability and processing difficulty of type 1-3 piezoelectric composite materials are solved, and high temperature resistance is improved and yield rate, suitable for high power ultrasonic transducers.

WO2024230409A1PCT designated stage expired Publication Date: 2024-11-14RONGHAI SUPERSONIC MEDICINE EN

Patent Information

Application Number
PCT/CN2024/087698
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-06
Filing Date
2024-04-15
Publication Date
2024-11-14

Smart Images

  • Figure CN2024087698_14112024_PF_FP_ABST
    Figure CN2024087698_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of materials, and in particular to a piezoelectric composite material and a preparation method therefor, and an ultrasonic transducer. The piezoelectric composite material is composed of an active phase and a passive phase. The passive phase comprises an epoxy resin, a filler, and a curing agent. The filler comprises at least one of mica powder, glass microspheres, and boron nitride. According to the present invention, by adding a specific filler (at least one of mica powder, glass microspheres, and boron nitride) to the passive phase, the high-temperature-resistant stability of the piezoelectric composite material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Piezoelectric composite material, preparation method thereof and ultrasonic transducer Technical Field

[0001] The present invention relates to the field of material technology, and in particular to a piezoelectric composite material, a preparation method thereof and an ultrasonic transducer. Background Art

[0002] Ultrasound therapy is a treatment method for certain diseases that utilizes the mechanical, cavitation, and thermal effects of ultrasound. High-intensity focused ultrasound (HIFU) is a minimally invasive technology capable of treating both deep and superficial tumors in the body. It plays a particularly important role in the treatment of various benign and malignant solid tumors, including uterine fibroids, liver cancer, and pancreatic cancer. Typically, HIFU therapy uses a high-power ultrasonic transducer with a special focusable geometry as the core component of the treatment device. This transducer is a functional device based on the inverse piezoelectric effect that converts electrical energy into acoustic energy.

[0003] Piezoelectric composites are materials with piezoelectric effects, consisting of at least one piezoelectric phase material and a non-piezoelectric phase material connected in a specific manner. They are key core materials for ultrasonic transducers. Based on the connectivity of each phase (i.e., how each phase connects to itself in spatial distribution), two-phase piezoelectric composites can be divided into various types, such as 0-0, 0-1, 0-2, 0-3, 1-1, 1-2, and 1-3. Typically, the first digit represents the piezoelectric phase, and the second represents the non-piezoelectric phase.

[0004] 1-3 piezoelectric composite materials are a key core material for the new generation of ultrasonic transducers. They offer advantages such as low acoustic impedance and high electromechanical coupling coefficient, making them an important material for transducers in hydrophones, medical imaging, and nondestructive testing. 1-3 piezoelectric composite ceramics are composed of piezoelectric ceramics and polymers. The piezoelectric effect of the piezoelectric ceramics generates deformation, forming ultrasonic waves. Therefore, the piezoelectric ceramic is called the active phase, and the polymer is the passive phase.

[0005] However, the low softening point, large thermal expansion and poor thermal diffusivity of high molecular polymers lead to the risk of mismatch in thermal and mechanical properties between the piezoelectric ceramic phase and the high molecular polymer in 1-3 piezoelectric composite materials. In particular, focused ultrasonic transducers require the 1-3 piezoelectric composite materials to be prepared into spherical or curved surfaces, and the complex processing technology results in low yields. When the ultrasonic transducer operates continuously at high power, a large amount of heat will be generated. This heat will cause the high molecular polymer of the passive phase material to soften, the mechanical properties to degrade, and the bonding strength to weaken, ultimately affecting the normal output and service life of the transducer. The passive phase has weak thermal conductivity, and this defect is highlighted when the temperature of the transducer rises during operation.

[0006] Summary of the Invention

[0007] In view of this, the present invention provides a piezoelectric composite material, a preparation method thereof, and an ultrasonic transducer, which are used to solve the technical problem of poor thermal stability of existing 1-3 type piezoelectric composite materials.

[0008] In an exemplary embodiment of the present invention, the present invention provides a piezoelectric composite material, which is composed of an active phase and a passive phase, the passive phase includes epoxy resin, filler and curing agent, and the filler includes at least one of mica powder, glass beads and boron nitride.

[0009] In an exemplary embodiment of the present invention, the active phase comprises a piezoelectric ceramic.

[0010] In an exemplary embodiment of the present invention, the epoxy resin includes bisphenol A epoxy resin.

[0011] In an exemplary embodiment of the present invention, in the passive phase, the filler accounts for 0.02 wt% to 40 wt%, preferably 0.02 wt% to 35 wt%.

[0012] In an exemplary embodiment of the present invention, the curing agent includes an amine curing agent.

[0013] In an exemplary embodiment of the present invention, in the passive phase, the mass ratio of the curing agent to the epoxy resin is 1-3:5, preferably 1.5-3:5.

[0014] In an exemplary embodiment of the present invention, the volume ratio of the active phase to the epoxy resin is 30-80:100, preferably 30-65:100.

[0015] In an exemplary embodiment of the present invention, the filler includes mica powder, glass microspheres and boron nitride.

[0016] In an exemplary embodiment of the present invention, the mass ratio of mica powder, glass microspheres and boron nitride is 10-15:5-10:5-15, preferably 10-12:8-10:5-12.

[0017] In an exemplary embodiment of the present invention, the passive phase further includes an additive, and the additive includes at least one of a toughening agent and a coupling agent.

[0018] In an exemplary embodiment of the present invention, the toughening agent includes a polymer containing a hydroxyl group, an ester group, and an ether group.

[0019] In an exemplary embodiment of the present invention, the coupling agent includes a silane coupling agent.

[0020] In an exemplary embodiment of the present invention, the additive accounts for 0.02 wt% to 13 wt% of the passive phase, and preferably 0.05 wt% to 12 wt%.

[0021] In addition, the inventors also found that the piezoelectric composite materials prepared by the existing process are prone to cracking and deformation.

[0022] In order to solve the technical problem that the piezoelectric composite material prepared by the existing process is prone to cracking, deformation, etc., in an exemplary embodiment of the present invention, the present invention also provides a method for preparing the piezoelectric composite material as described above, the preparation method comprising:

[0023] After cutting, cleaning and drying the active phase, place it in the caulking mold;

[0024] Add filler to epoxy resin, stir evenly and then add curing agent to obtain a mixture, pour the mixture into the caulking mold, fill the gap, degas, and then place it in an oven for constant temperature treatment. After the surface of the mixture is cured, process it to a preset thickness, heat it again until the mixture is completely softened, then place it in a molding mold, and take it out after it is completely cured.

[0025] In an exemplary embodiment of the present invention, the constant temperature treatment includes: first constant temperature treatment at 35±5°C for 2-4 hours, then constant temperature treatment at 40±5°C for 1-2 hours, preferably, first constant temperature treatment at 35±3°C for 2.5-4 hours, then constant temperature treatment at 40±3°C for 1.5-2 hours.

[0026] In an exemplary embodiment of the present invention, the temperature is heated to 60±5°C, preferably 60±3°C.

[0027] In an exemplary embodiment of the present invention, the present invention further provides an ultrasonic transducer, which includes the piezoelectric composite material as described above or the piezoelectric composite material prepared according to the preparation method as described above.

[0028] As described above, the piezoelectric composite material, its preparation method and ultrasonic transducer of the present invention have the following beneficial effects:

[0029] The present invention can improve the high temperature resistance of the piezoelectric composite material by adding specific fillers in the passive phase.

[0030] The piezoelectric composite material of the present invention can be die-cast into various shapes as tooling changes, has a high yield rate and a wide range of applications.

[0031] The present invention further solves the technical problem that piezoelectric composite materials are prone to cracking and deformation when prepared using existing processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] FIG1 is a flow chart of cutting piezoelectric ceramics;

[0033] FIG2 is a graph showing the electromechanical coupling coefficients of the piezoelectric composite materials prepared in Examples 1-4 and Comparative Example 1 as a function of temperature. DETAILED DESCRIPTION

[0034] The present invention is further illustrated below through specific examples. However, it should be noted that the specific material ratios, process conditions and results described in the embodiments of the present invention are only used to illustrate the present invention and are not intended to limit the scope of protection of the present invention. Any equivalent changes or modifications made based on the spirit of the present invention should be included in the scope of protection of the present invention.

[0035] The present invention provides a piezoelectric composite material, which is composed of an active phase and a passive phase, wherein the passive phase includes an epoxy resin, a filler and a curing agent;

[0036] The volume ratio of the active phase to the epoxy resin is 30-80:100, and the active phase includes piezoelectric ceramics;

[0037] In the passive phase, the filler accounts for 0.02wt%-40wt% and the additive accounts for 0.02wt%-13wt%;

[0038] In the passive phase, the mass ratio of the curing agent to the epoxy resin is 1-3:5, and the curing agent includes an amine curing agent;

[0039] Epoxy resins include bisphenol A epoxy resins;

[0040] The filler includes at least one of mica powder, glass microbeads and boron nitride.

[0041] In an exemplary embodiment of the present invention, the filler includes mica powder, glass microspheres and boron nitride, and the mass ratio of mica powder, glass microspheres and boron nitride is 10-15:5-10:5-15.

[0042] In an exemplary embodiment of the present invention, the passive phase further includes an additive, the additive including at least one of a toughening agent and a coupling agent, the toughening agent includes a polymer containing a hydroxyl group, an ester group, and an ether group, and the coupling agent includes a silane coupling agent.

[0043] In an exemplary embodiment of the present invention, the present invention further provides a method for preparing the piezoelectric composite material as described above, comprising:

[0044] After cutting, cleaning and drying the active phase, place it in the caulking mold;

[0045] Adding filler to epoxy resin, stirring evenly, and then adding curing agent to obtain a mixture;

[0046] Pour the mixture into the caulking mold, fill the gap, degas, and then place it in an oven for constant temperature treatment at 35±5℃ for 2-4h, then at 40±5℃ for 1-2h. After the surface of the mixture is cured, process it to the preset thickness, heat it to 60±5℃ again to soften the mixture completely, then place it in the molding mold and take it out after it is completely cured.

[0047] In an exemplary embodiment of the present invention, the present invention further provides an ultrasonic transducer, which includes the piezoelectric composite material as described above or the piezoelectric composite material prepared according to the preparation method as described above.

[0048] The scheme of the present invention is illustrated below by specific embodiments. It should also be understood that the following examples are only used to specifically illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention all fall within the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific numerical values ​​exemplified below.

[0049] Example 1

[0050] This embodiment provides a piezoelectric composite material, which is prepared according to the following steps:

[0051] S1. As shown in Figure 1, fix the piezoelectric ceramic PZT-8 (as shown in Figure a) and cut it one by one. After cutting one side, rotate the piezoelectric ceramic PZT-8 90° and cut the other side. Then, clean and dry it, and then place it in the caulking mold.

[0052] S2. 15g of mica powder was added to 70.83g of bisphenol A epoxy resin E-51 and stirred, followed by addition of 14.17g of 593 modified fatty amine curing agent to obtain a mixture;

[0053] The volume ratio of piezoelectric ceramic PZT-8 to bisphenol A epoxy resin E-51 is 60:100;

[0054] S3. Pour the mixture into the caulking mold in which the piezoelectric ceramic PZT-8 has been placed in step S1, fill the gap, and vacuum degas for 10 minutes. Then place it in an oven and treat it at a constant temperature of 35°C for 2 hours, then at a constant temperature of 40°C for 2 hours. After the surface of the mixture is solidified, process it to a thickness of 2 mm, heat it to 60°C again to completely soften the mixture, and then place it in a forming mold with a curvature radius of 170 mm. Take it out after it is completely solidified to obtain a piezoelectric composite material.

[0055] The piezoelectric composite material prepared in this embodiment did not show any cracking or deformation.

[0056] Example 2

[0057] This embodiment provides a piezoelectric composite material, which is prepared according to the following steps:

[0058] S1. As shown in Figure 1, fix the piezoelectric ceramic PZT-4 and cut one side (as shown in Figure b). After completion, rotate the piezoelectric ceramic PZT-4 90° and cut the other side (as shown in Figure c). Then, clean and dry it, and then place it in the caulking mold.

[0059] S2. 15g of glass beads were added to 70.83g of bisphenol A epoxy resin E-51 and stirred, followed by addition of 14.17g of 593 modified fatty amine curing agent to obtain a mixture;

[0060] The volume ratio of the piezoelectric ceramic PZT-4 to the bisphenol A epoxy resin E-51 is 50:100;

[0061] S3. Pour the mixture into the caulking mold in which the piezoelectric ceramic PZT-4 has been placed in step S1, fill the gap, and vacuum degas for 10 minutes. Then place it in an oven and treat it at a constant temperature of 35°C for 2 hours, and then at a constant temperature of 40°C for 2 hours. After the surface of the mixture is solidified, process it to a thickness of 3mm, heat it to 60°C again to completely soften the mixture, and then place it in a forming mold with a curvature radius of 140mm. Take it out after it is completely solidified to obtain a piezoelectric composite material.

[0062] Example 3

[0063] This embodiment provides a piezoelectric composite material, which is prepared according to the following steps:

[0064] As shown in Figure 1, fix the piezoelectric ceramic PZT-8 (as shown in Figure a) and cut it one by one. After cutting one side, rotate the piezoelectric ceramic PZT-8 90° and cut the other side. Then clean and dry it, and then place it in the caulking mold.

[0065] S2 was added 15g of boron nitride 70.83g of bisphenol A epoxy resin E-51, stirred, followed by addition of 14.17g 593 modified fatty amine curing agent to obtain a mixture;

[0066] The volume ratio of piezoelectric ceramic PZT-8 to bisphenol A epoxy resin E-51 is 30:100;

[0067] S3. Pour the mixture into the caulking mold in which the piezoelectric ceramic PZT-8 has been placed in step S1, fill the gap, and vacuum degas for 10 minutes. Then place it in an oven and treat it at a constant temperature of 35°C for 4 hours, then at a constant temperature of 40°C for 2 hours. After the surface of the mixture is solidified, process it to a thickness of 2 mm, heat it to 60°C again to completely soften the mixture, then bend it and completely apply it to a cylindrical tooling with a diameter of 10 mm. After it is completely solidified, take it out to obtain a piezoelectric composite material.

[0068] Example 4

[0069] The difference between this embodiment and embodiment 1 is that:

[0070] S2 5g of mica powder, 5g of glass beads and 5g of boron nitride were added to 70.83g of bisphenol A epoxy resin E-51, stirred, and then added 593 modified fatty amine, stirred, and then added 14.17g of 593 modified fatty amine curing agent to obtain a mixture;

[0071] The volume ratio of the piezoelectric ceramic PZT-8 to the bisphenol A epoxy resin E-51 is 60:100.

[0072] Example 5

[0073] The difference between this embodiment and embodiment 1 is that:

[0074] S2 9g of mica powder, 3g of glass beads and 3g of boron nitride were added to 70.83g of bisphenol A epoxy resin E-51 and stirred, followed by addition of 14.17g of 593 modified fatty amine curing agent to obtain a mixture;

[0075] The volume ratio of the piezoelectric ceramic PZT-8 to the bisphenol A epoxy resin E-51 is 60:100.

[0076] Example 6

[0077] The difference between this embodiment and embodiment 1 is that:

[0078] S2 15g of mica powder, 5g VL-1 toughening agent and 1g γ-aminopropyl triethoxysilane were added to 64.83g of bisphenol A epoxy resin E-51 and stirred, followed by addition of 14.17g of 593 modified fatty amine curing agent to obtain a mixture;

[0079] The volume ratio of the piezoelectric ceramic PZT-8 to the bisphenol A epoxy resin E-51 is 60:100.

[0080] Comparative Example 1

[0081] The difference between this comparative example and Example 1 is that:

[0082] S2 was added 14.17g 593 modified fatty amine curing agent to 70.83g bisphenol A epoxy resin E-51 to obtain a mixture;

[0083] The volume ratio of the piezoelectric ceramic PZT-8 to the bisphenol A epoxy resin E-51 is 60:100.

[0084] Performance Testing

[0085] The high temperature resistance of the piezoelectric composite materials obtained in Examples 1-4 and Comparative Example 1 was tested. The specific steps were as follows: the resonant frequencies f of the piezoelectric composite materials obtained in Examples 1-4 and Comparative Example 1 were directly read on an impedance analyzer at 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, and 50°C, respectively. r and the anti-resonance frequency f a Then, the electromechanical coupling coefficient k of the piezoelectric composite materials prepared in Examples 1-4 and Comparative Example 1 at the corresponding temperature is calculated according to formula (I): t :

[0086] Among them, k t is the electromechanical coupling coefficient; f r is the resonant frequency in KHz, f a is the anti-resonance frequency in KHz. The results are shown in Table 1 and Figure 2.

[0087] Table 1 Test results

[0088] As shown in Table 1, the electromechanical coupling coefficient of the piezoelectric composite material in Comparative Example 1 (without filler) changes more steeply with increasing temperature, while the electromechanical coupling coefficient of the piezoelectric composite material in Example 1 (with filler) changes more gently. This result demonstrates that the addition of specific fillers to the passive phase of the present invention can improve the high-temperature stability of the piezoelectric composite material.

[0089] As shown in Table 1 and Figure 2, compared to the piezoelectric composite materials of Examples 1, 2, and 3 (fillers consisting of one of mica powder, glass microspheres, and boron nitride), the electromechanical coupling coefficient of the piezoelectric composite material of Example 4 (filler consisting of mica powder, glass microspheres, and boron nitride in a mass ratio of 10:10:10) remains relatively stable as the temperature increases. This result indicates that the present invention can further improve the high-temperature stability of the piezoelectric composite material by selecting the filler composition (including mica powder, glass microspheres, and boron nitride, with a mass ratio of mica powder, glass microspheres, and boron nitride of 10-15:5-10:5-15).

[0090] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the present invention. Anyone skilled in the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by one of ordinary skill in the art without departing from the spirit and technical principles disclosed herein are intended to be covered by the claims of the present invention.

Claims

1. A piezoelectric composite material, characterized in that: The piezoelectric composite material consists of an active phase and a passive phase. The passive phase includes epoxy resin, filler and curing agent. The filler includes at least one of mica powder, glass microbeads and boron nitride.

2. The piezoelectric composite material according to claim 1, characterized in that: The active phase includes piezoelectric ceramics; and / or, the volume ratio of the active phase to the epoxy resin is 30-80:100; And / or, the epoxy resin comprises bisphenol A epoxy resin; And / or, in the passive phase, the filler accounts for 0.02wt%-40wt%; and / or, the curing agent comprises an amine curing agent; And / or, in the passive phase, the mass ratio of the curing agent to the epoxy resin is 1-3:

5.

3. The piezoelectric composite material according to claim 1, characterized in that: The filler includes mica powder, glass microspheres and boron nitride.

4. The piezoelectric composite material according to claim 3, characterized in that: The mass ratio of the mica powder, the glass microbeads and the boron nitride is 10-15:5-10:5-15.

5. The piezoelectric composite material according to claim 1, characterized in that: The passive phase further includes an additive, wherein the additive includes at least one of a toughening agent and a coupling agent.

6. The piezoelectric composite material according to claim 5, characterized in that: The toughening agent includes a polymer containing a hydroxyl group, an ester group and an ether group; And / or, the coupling agent includes a silane coupling agent.

7. The piezoelectric composite material according to claim 5, characterized in that: In the passive phase, the additive accounts for 0.02wt%-13wt%.

8. The method for preparing the piezoelectric composite material according to any one of claims 1 to 7, characterized in that: The preparation method comprises: After the active phase is cut, cleaned, dried, and placed in a caulking mold; Add filler to epoxy resin, stir evenly, then add curing agent to obtain a mixture, pour the mixture into the caulking mold, fill the gap, degas, and then place it in an oven for constant temperature treatment. After the surface of the mixture is cured, it is processed to a preset thickness, heated again until the mixture is completely softened, and then placed in a molding mold and taken out after it is completely cured.

9. The preparation method according to claim 8, characterized in that: The constant temperature treatment includes: firstly, constant temperature treatment at 35±5°C for 2-4h, and then constant temperature treatment at 40±5°C for 1-2h; and / or, heated to 60±5°C.

10. An ultrasonic transducer, characterized in that: The ultrasonic transducer comprises the piezoelectric composite material according to any one of claims 1 to 7 or the piezoelectric composite material prepared by the preparation method according to claim 7 or 8.

Citation Information

Patent Citations

  • Piezoelectric composite material of wide-band transducer

    CN101499512A

  • Intelligent monitoring maintenance-free buckling restrained brace for piezoelectric composite material sensing layer

    CN103422586A

  • Shear vibration-based piezoelectric composite material and preparation method therefor

    CN106876576A

Cited By

  • Optical matching layer and preparation method thereof

    CN122103809A

  • Optical matching layer and method for producing same

    CN122103809B