SEQUESTRANTES DE ALDEÍDO PARA REDUZIR O TEOR DE ODORANTES EM COMPOSIÇÕES DE POLÍMEROS CONTENDO RECICLADOS

By adding anthranilamide and barbituric acid to recycled polypropylene compositions, the challenges of mechanical properties and impurity issues are addressed, enhancing recyclability and reducing aldehydes for improved automotive applications.

BR112025024731A2Pending Publication Date: 2026-11-10BOREALIS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
BR112025024731
Authority / Receiving Office
BR · BR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-17
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Current recycling technologies for polypropylene-based materials face challenges in achieving high recycling rates due to unsatisfactory mechanical properties and inferior processing, leading to frequent energy recovery rather than material reuse, especially in automotive applications, and recycled materials often contain mixtures of polypropylene and polyethylene, complicating purification.

Method used

Incorporation of specific additives such as anthranilamide and barbituric acid into polypropylene compositions derived from recycled materials to reduce aldehyde content, enhancing the recyclability and odorant reduction.

Benefits of technology

Effectively reduces aldehyde content in recycled polypropylene compositions, improving their suitability for automotive applications by maintaining mechanical properties and processing efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a polypropylene composition (PC) being a mixed-plastic polypropylene blend containing recycled material, to articles comprising said polypropylene composition, as well as to the use of certain additives for the reduction of aldehyde content in compositions derived at least partially from recyclates.
Need to check novelty before this filing date? Find Prior Art

Description

1 / 45 “ALDEHYDE SEQUESTRANTS TO REDUCE ODORANT CONTENT IN POLYMER COMPOSITIONS CONTAINING RECYCLED MATERIALS” Field of Invention

[0001] The present invention relates to a polypropylene composition (PC - polypropylene composition) that is a blend of mixed polypropylene plastics containing recycled material, to articles comprising said polypropylene composition, as well as to the use of certain additives for reducing the aldehyde content in compositions derived, at least partially, from recycled materials. Background of the Invention

[0002] Over the last decade, concern has grown regarding plastics and the environmental sustainability of their use in current quantities. This has led to new legislation concerning the disposal, collection, and recycling of polyolefins. Additionally, there have been efforts in several countries to increase the percentage of plastic materials that are recycled instead of being sent to landfills.

[0003] In Europe, plastic waste amounts to approximately 27 million tons per year; of this amount, in 2016, 7.4 million tons were disposed of in landfills, 11.27 million tons were incinerated (in order to produce energy), and about 8.5 million tons were recycled. Polypropylene-based materials are a particular problem, as these materials are extensively used in packaging. Considering the enormous amount of waste collected compared to the amount of waste recycled back into the stream (amounting to only about 30%), there is still great potential for intelligent reuse of plastic waste streams and for mechanical recycling of plastic waste.

[0004] Taking the automotive industry as an example. In Europe, the Petition 870250103521, dated 12 / 11 / 2025, page 11 / 238 EU states' End of Life Directive 2 / 45 stipulates that 85% to 95% of vehicle materials must be recyclable or recoverable. The current recycling rate of automotive components is significantly below this target. On average, vehicles consist of 9% by weight of plastics; of this 9% by weight, only 3% by weight is currently recycled. Therefore, there is still a need to be met for the recycling targets of plastics in the automotive industry to be achieved. This invention focuses particularly on mechanically recycled waste streams, as opposed to "energy recycling," where polyolefins are burned and used as energy.However, due to cost reasons, unsatisfactory mechanical properties, and inferior processing properties, waste streams containing cross-linked polyolefins are frequently used for energy recovery (e.g., incineration in a district heating plant or for heat generation in the cement industry) and are less frequently recycled into new products.

[0005] An important trend in the field of polyolefins is the use of recycled materials, which are derived from a wide variety of sources. Streams from durable goods, such as those derived from waste electrical equipment (WEEE) or end-of-life vehicles (ELVs), contain a wide variety of plastics. These materials can be processed to recover acrylonitrile butadiene styrene (ABS), high-impact polystyrene (HIPS), polypropylene (PP), and polyethylene (PE) plastics. Separation can be performed using density separation in water and then further separation based on fluorescence, near-infrared absorption, or Raman fluorescence. However, it is commonly quite difficult to obtain pure recycled polypropylene or pure recycled polyethylene.Generally, the recycled quantities of polypropylene on the market are mixtures of polypropylene (PP) and polyethylene (PE); this is especially true for post-consumer waste streams derived from household waste. It has been found that commercially recycled sources... Petition 870250103521, dated 12 / 11 / 2025, page 12 / 238 3 / 45 of post-consumer waste generally contains mixtures of PP and PE, with the smaller component reaching up to < 50% by weight.

[0006] The better the quality, that is, the higher the purity of the recycled polyolefin, the more expensive the material. Furthermore, recycled polyolefin materials frequently have cross-contamination with non-polyolefin materials such as polyethylene terephthalate, polyamide, polystyrene, or non-polymeric substances like wood, paper, glass, or aluminum. In addition, recycled polypropylene-rich materials typically have properties that are much worse than those of virgin materials, unless the amount of recycled polyolefin added to the final compound is extremely low. For example, these materials generally have unsatisfactory odor and taste performance, limited stiffness, limited impact resistance, and unsatisfactory mechanical properties (such as brittleness), therefore failing to meet customer requirements.

[0007] Unsatisfactory mechanical properties can be improved by blending recycled polyolefin with virgin polymers, or by using reinforcing fillers; however, this does not address the odor / taste issue.

[0008] The established method for removing volatile organic compounds from virgin and recycled polymers involves aeration of the polymers. This can be achieved, among other methods, through the use of air, inert gases, or steam.

[0009] Variants of this process have been known for many years and are described, among others, in documents EP 0 004 601 A1, EP 0 859 809 A1, EP 0 964 877 A1, EP 1 542 777 A2 and EP 3 647 328 A1.

[0010] Although these methods can be very efficient in removing a wide range of volatile compounds, they can consume a lot of energy, which can be counterproductive when seeking a recycling process that is as environmentally friendly as possible.

[0011] In addition, there are many known processes that result in the reduction Petition 870250103521, dated 12 / 11 / 2025, page 13 / 238 4 / 45 of the aldehyde content (aldehydes being an important odorant), with the aldehyde content increasing further in additional processing steps where more aldehyde is formed from decomposition reactions.

[0012] Thus, there is still a need for additional methods to reduce aldehyde content, where said methods are also capable of maintaining aldehyde levels at low values. Summary of the Invention

[0013] The present invention is based on the finding that mixing certain additives, especially anthranilamide and barbituric acid, with compositions containing post-consumer recycled materials has the effect of drastically reducing the aldehyde content of said compositions, helping to avoid unwanted odor.

[0014] Therefore, in a first aspect, the present invention relates to a polypropylene (PC) composition comprising: a) a blend of mixed polypropylene (PP) plastics with a quantity of black spot defects with a particle size in the range of 0.05 to 0.10 mm2 in the range of 0.10 to 4.0 particles / cm2; and b) one or more compounds that react with linear alkyl aldehydes.

[0015] In a second aspect, the present invention relates to a polypropylene (PC) composition comprising: a) a blend of polypropylene (PP) mixed plastics derived, at least partially, from post-consumer waste; and b) one or more compounds that react with linear alkyl aldehydes.

[0016] In a third aspect, the present invention relates to an article, preferably an injection-molded article, comprising the polypropylene (PC) composition of the first or second aspects in an amount of at least 95% by weight, more preferably at least 98% by weight, most preferably at least 99% by weight.

[0017] In a fourth aspect, the present invention relates to the use of a compound having a structure according to formula (I): Petition 870250103521, dated 12 / 11 / 2025, p. 14 / 238 5 / 45 wherein R1, R2 and R3 are each independently selected from the group consisting of a hydrogen atom, a linear or branched C1-C10 alkyl group, a hydroxyl group, an aryl group, a halogen atom, an acetyl group or a cyano group, to reduce the acetaldehyde and / or hexanal content of a polypropylene composition derived at least partially from post-consumer waste, without simultaneously increasing the acetone content by more than 30% and without simultaneously increasing the tert-butanol content by more than 10%.

[0018] In a final aspect, the present invention relates to the use of a compound having a structure according to formula (II): where RA represents from zero to four substitutions, each substitution being independently selected from the group consisting of a linear or branched C1-C10 alkyl group, a linear or branched C1-C10 alkoxy group, an aryl group or a halogen atom, wherein RB and RC is selected from the group consisting of hydrogen and a linear or branched C1-C10 alkyl group to reduce the acetaldehyde and / or hexanal content of a polypropylene composition derived, at least partially, from post-consumer waste, without simultaneously increasing the acetone content by more than 30% and without simultaneously increasing the tert-butanol content by more than 10%. Definitions

[0019] Unless otherwise defined, all technical and scientific terms Petition 870250103521, dated 12 / 11 / 2025, p. 15 / 238 6 / 45 used in this document have the same meaning as that commonly understood by an individual with ordinary skill in the art to which the invention pertains. Although any methods and materials similar or equivalent to those described herein may be used in practice for testing the present invention, preferred materials and methods are described herein. In describing and claiming the present invention, the following terminology shall be used in accordance with the definitions set forth below.

[0020] Unless clearly indicated otherwise, the use of the terms “a”, “an” and similar terms refers to one or more.

[0021] The following quantities are given as a % by weight (% by w), unless otherwise stated.

[0022] A propylene homopolymer is a polymer consisting essentially of propylene monomer units. Due to impurities, especially during commercial polymerization processes, a propylene homopolymer may comprise up to 0.1 mol% of comonomer units, preferably up to 0.05 mol% of comonomer units, and most preferably up to 0.01 mol% of comonomer units.

[0023] A propylene copolymer is a copolymer of propylene monomer units and comonomer units, preferably selected from ethylene and C4-C8 alpha-olefins. A random propylene copolymer is a propylene copolymer in which the comonomer units are randomly distributed along the polymer chain, while a propylene block copolymer comprises blocks of propylene monomer units and blocks of comonomer units. Random propylene copolymers may comprise comonomer units of one or more different comonomers in their carbon atom quantities.

[0024] Heterophasic propylene copolymers typically comprise: a) a crystalline propylene homopolymer or copolymer matrix (M); and Petition 870250103521, dated 12 / 11 / 2025, page 16 / 238 7 / 45 b) an elastomeric rubber, preferably a propylene-ethylene copolymer (E);

[0025] In the case of a random heterophasic propylene copolymer, said crystalline matrix phase is a random copolymer of propylene and at least one alpha-olefin comonomer.

[0026] The elastomeric phase can be a propylene copolymer with a high comonomer content that is not randomly distributed in the polymer chain, but is distributed in a comonomer-rich block structure and a propylene-rich block structure. A heterophasic polypropylene copolymer usually differs from a monophasic propylene copolymer by exhibiting two distinct glass transition temperatures Tg that are attributed to the matrix phase and the elastomeric phase.

[0027] For the purposes of this description and subsequent claims, the term “recycled waste” is used to indicate material recovered from both post-consumer waste and industrial waste, as opposed to virgin polymers. Post-consumer waste refers to objects that have completed at least one first use cycle (or life cycle), i.e., that have already served their first purpose; while industrial waste refers to manufacturing waste, which does not normally reach a consumer.

[0028] The term “virgin” denotes recently produced materials and / or objects before their first stage, which have not yet been recycled.

[0029] The term “recycled material” as used in this document denotes materials reprocessed from “recycled waste”.

[0030] A polymer blend denotes a mixture of two or more polymeric components. In general, the blend can be prepared by mixing the two or more polymeric components. Suitable blending procedures known in the art are post-polymerization blending procedures.

[0031] Post-polymerization blending can be the dry blending of polymeric components such as polymer powders and / or composite polymer pellets or Petition 870250103521, dated 12 / 11 / 2025, page 17 / 238 8 / 45 Fusion blending through fusion mixing of the polymeric components.

[0032] A blend of mixed polypropylene plastics indicates that the blend comprises predominantly polypropylene; however, small amounts of other plastics are present. Recycled blends, particularly post-consumer recycled blends, are almost always blends of mixed plastics, reflecting the efficiency of sorting in more advanced recycling processes.

[0033] The present invention will now be described in more detail. Detailed Description Polypropylene (PC) composition

[0034] The polypropylene (PC) composition of each of the first and second aspects includes: a) a blend of mixed polypropylene (PP) plastics; and b) one or more compounds that react with linear alkyl aldehydes.

[0035] Preferably, each polypropylene (PC) composition comprises, more preferably, consists of: a) from 98.0 to 99.99% by weight, relative to the total weight of the polypropylene (PC) composition, of the blend of polypropylene (PP) mixed plastics; and b) from 0.01 to 2.0% by weight, relative to the total weight of the polypropylene (PC) composition, of one or more compounds reactive with linear alkyl aldehydes.

[0036] More preferably, each polypropylene (PC) composition comprises, most preferably, consists of: a) from 98.5 to 99.99% by weight, relative to the total weight of the polypropylene (PC) composition, of the blend of polypropylene (PP) mixed plastics; and b) from 0.01 to 1.5% by weight, relative to the total weight of the polypropylene (PC) composition, of one or more compounds reactive with aldehydes of Petition 870250103521, dated 12 / 11 / 2025, page 18 / 238 9 / 45 linear alkyl groups.

[0037] More preferably, each polypropylene (PC) composition comprises, most preferably, consists of: a) from 99.0 to 99.99% by weight, relative to the total weight of the polypropylene (PC) composition, of the blend of polypropylene (PP) mixed plastics; and b) 0.01 to 1.0% by weight, relative to the total weight of the polypropylene (PC) composition, of one or more compounds reactive with linear alkyl aldehydes.

[0038] Preferably, the polypropylene (PC) composition of each of the first and second aspects has an acetaldehyde concentration determined by solid-phase microextraction (HS-SPME-GC-MS) in the range of 0 to 50% of the acetaldehyde concentration value of the polypropylene (PP) blended plastics, also determined by solid-phase microextraction (HS-SPME-GC-MS).

[0039] Preferably, the polypropylene (PC) composition of each of the first and second aspects has a hexanal concentration determined by solid-phase microextraction (HS-SPME-GC-MS) in the range of 0 to 60% of the hexanal concentration value of the polypropylene (PP) blended plastics, also determined by solid-phase microextraction (HSSPME-GC-MS).

[0040] An essential component of the polypropylene (PC) composition of each of the first and second aspects is the blend of mixed polypropylene (PP) plastics.

[0041] The blend of mixed polypropylene (PP) plastics from the first aspect has a quantity of black spot defects with a particle size in the range of 0.05 to 0.10 mm2 in the range of 0.10 to 4.0 particles / cm2.

[0042] The number of black spot defects in this band indicates that the blend of mixed polypropylene (PP) plastics in the first aspect is, at least partially, derived from post-consumer waste. Petition 870250103521, dated 12 / 11 / 2025, page 19 / 238 10 / 45

[0043] The blend of polypropylene (PP) mixed plastics in the second aspect is derived, at least partially, from post-consumer waste.

[0044] Therefore, it is preferable that the blend of mixed polypropylene (PP) plastics of the second aspect have a quantity of black spot defects with a particle size in the range of 0.05 to 0.10 mm2 in the range of 0.10 to 4.0 particles / cm2.

[0045] Other indications of the recycled nature of the blended polypropylene (PP) plastics of each of the first and second aspects include the presence of other polymers, such as polystyrene and polyamide-6, and the presence of limonene and / or fatty acids.

[0046] Consequently, it is preferable that the blend of mixed polypropylene (PP) plastics of each of the first and second aspects comprise one or more of polystyrene, polyamide-6, limonene and fatty acids, preferably comprising each of polystyrene, polyamide-6, limonene and fatty acids.

[0047] The blend of mixed polypropylene (PP) plastics of each of the first and second aspects preferably has a melt flow (MFR2), determined in accordance with ISO 1133 at 230 °C and 2.16 kg, in the range of 5.0 to 100 g / 10 min, more preferably in the range of 10.0 to 70 g / 10 min, and most preferably in the range of 15.0 to 40 g / 10 min.

[0048] The blend of mixed polypropylene (PP) plastics from each of the first and second aspects preferably has an ethylene content (C2(total)), determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy, in the range of 3.0 to 15.0 % by weight, more preferably in the range of 4.0 to 12.0 % by weight, with the highest preference in the range of 5.0 to 9.0 % by weight.

[0049] The blend of mixed polypropylene (PP) plastics of each of the first and second aspects preferably has a soluble fraction (SF) content, determined according to CRYSTEX QC analysis, in the range of 5.0 to 20.0% by weight, with greater preference Petition 870250103521, dated 12 / 11 / 2025, page 20 / 238 11 / 45 in the range of 8.0 to 15.0% by weight, with the highest preference in the range of 10.0 to 13.0% by weight.

[0050] The blend of mixed polypropylene (PP) plastics from each of the first and second aspects preferably has a crystalline fraction (CF) content, determined according to CRYSTEX QC analysis, in the range of 80.0 to 95.0 % by weight, more preferably in the range of 85.0 to 92.0 % by weight, with the highest preference in the range of 87.0 to 90.0 % by weight.

[0051] The blend of mixed polypropylene (PP) plastics from each of the first and second aspects preferably has an ethylene content in the soluble fraction (C2(SF)), according to CRYSTEX QC analysis, determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy, in the range of 15 to 60 wt%, more preferably in the range of 20 to 55 wt%, with the highest preference in the range of 25 to 50 wt%.

[0052] The blend of mixed polypropylene (PP) plastics from each of the first and second aspects preferably has an ethylene content in the crystalline fraction (C2(CF)), according to CRYSTEX QC analysis, determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy, in the range of 0.5 to 6.0 wt%, more preferably in the range of 0.8 to 5.5 wt%, with the highest preference in the range of 1.0 to 5.0 wt%.

[0053] The blend of mixed polypropylene (PP) plastics of each of the first and second aspects preferably has an intrinsic viscosity, determined in accordance with DIN ISO 1628 / 1, of the soluble fraction (iV(SF)), according to CRYSTEX QC analysis, in the range of 1.50 to 2.50 dl / g, more preferably in the range of 1.60 to 2.20 dl / g, with the highest preference in the range of 1.70 to 2.00 dl / g.

[0054] The blend of mixed polypropylene (PP) plastics from each of the first and second aspects preferably has an intrinsic viscosity, determined according to DIN ISO 1628 / 1, of the crystalline fraction (iV(CF)), according to CRYSTEX QC analysis, in the range of 1.00 to Petition 870250103521, dated 12 / 11 / 2025, page 21 / 238 12 / 45 2.00 dl / g, with a greater preference in the range of 1.25 to 1.85 dl / g, with the maximum preference in the range of 1.50 to 1.70 dl / g.

[0055] In a first embodiment, the blend of mixed polypropylene (PP) plastics from each of the first and second aspects originates from post-consumer waste. In other words, the blend of mixed polypropylene (PP) plastics from each of the first and second aspects is free of virgin polypropylene, more preferably free of virgin polymers.

[0056] In this first embodiment, the blend of mixed polypropylene (PP) plastics preferably has an acetaldehyde concentration, determined by solid-phase microextraction (HS-SPME-GC-MS) in a powder sample, in the range of 100 to 2000 mg / m3, more preferably in the range of 15 to 1800 mg / m3, with the highest preference in the range of 200 to 1700 mg / m3.

[0057] In this first embodiment, the blend of mixed polypropylene (PP) plastics preferably has a hexanal concentration, determined by solid-phase microextraction (HS-SPME-GC-MS) in a powder sample, in the range of 1 to 60 mg / m3, more preferably in the range of 5 to 50 mg / m3, with the highest preference in the range of 10 to 40 mg / m3.

[0058] Additionally, in this first embodiment, the blend of mixed polypropylene (PP) plastics preferably has a melt flow (MFR2), determined in accordance with ISO 1133 at 230 °C and 2.16 kg, in the range of 5.0 to 50 g / 10 min, more preferably in the range of 10.0 to 40 g / 10 min, and most preferably in the range of 15.0 to 30 g / 10 min.

[0059] In this first embodiment, the blend of mixed polypropylene (PP) plastics preferably has an ethylene content (C2(total)), determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy, in the range of 3.0 to 15.0 % by weight, more preferably in the range of 4.0 to 12.0 % by weight, with the maximum preference in the range of 5.0 to 9.0 % by weight.

[0060] In this first type, the blend of mixed polypropylene (PP) plastics preferably has a soluble fraction (SF) content, Petition 870250103521, dated 12 / 11 / 2025, page 22 / 238 13 / 45 determined according to the CRYSTEX QC analysis, in the range of 5.0 to 20.0% by weight, with greater preference in the range of 8.0 to 15.0% by weight, with maximum preference in the range of 10.0 to 13.0% by weight.

[0061] In this first embodiment, the blend of mixed polypropylene (PP) plastics preferably has a crystalline fraction (CF) content, determined according to CRYSTEX QC analysis, in the range of 80.0 to 95.0 % by weight, more preferably in the range of 85.0 to 92.0 % by weight, with the highest preference in the range of 87.0 to 90.0 % by weight.

[0062] In this first embodiment, the blend of mixed polypropylene (PP) plastics preferably has an ethylene content in the soluble fraction (C2(SF)), according to the CRYSTEX QC analysis, determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy, in the range of 15 to 50 wt%, more preferably in the range of 20 to 40 wt%, with the highest preference in the range of 25 to 35 wt%.

[0063] In this first embodiment, the blend of mixed polypropylene (PP) plastics preferably has an ethylene content in the crystalline fraction (C2(CF)), according to the CRYSTEX QC analysis, determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy, in the range of 1.0 to 6.0 wt%, more preferably in the range of 2.0 to 5.5 wt%, with the highest preference in the range of 3.0 to 5.0 wt%.

[0064] In this first embodiment, the blend of mixed polypropylene (PP) plastics preferably has an intrinsic viscosity, determined in accordance with the DIN ISO 1628 / 1 standard, of the soluble fraction (iV(SF)), according to the CRYSTEX QC analysis, in the range of 1.50 to 2.00 dl / g, more preferably in the range of 1.55 to 1.90 dl / g, with the maximum preference in the range of 1.60 to 1.80 dl / g.

[0065] In this first embodiment, the blend of mixed polypropylene (PP) plastics preferably has an intrinsic viscosity, determined in accordance with the DIN ISO 1628 / 1 standard, of the crystalline fraction (iV(CF)), according to the CRYSTEX QC analysis, in the range of 1.00 to 2.00 dl / g, Petition 870250103521, dated 12 / 11 / 2025, p. 23 / 238 14 / 45 with greater preference in the range of 1.25 to 1.85 dl / g, with maximum preference in the range of 1.50 to 1.70 dl / g.

[0066] In a second embodiment, the blend of polypropylene (PP) blended plastics can be obtained by blending a blend (B) of polypropylene blended plastics with one or more components.

[0067] Suitable components include, but are not limited to, virgin polymers, such as one or more heterophasic propylene-ethylene copolymers (HECO), one or more propylene homopolymers (h-PP), one or more elastomeric ethylene (E) copolymers, a polar group-modified polypropylene (PMP). Other suitable components include non-polymeric components such as fillers, for example, carbon and / or glass fibers (F1) or inorganic filler(s) (F2) other than carbon and / or glass fibers (F1). In addition, other additives known to those skilled in the art may be added.

[0068] The blend (B) of mixed polypropylene plastics is preferably derived from post-consumer waste and therefore has a quantity of black spot defects with a particle size in the range of 0.05 to 0.10 mm2 in the range of 0.10 to 4.0 particles / cm2.

[0069] In this second method, the blend of mixed polypropylene (PP) plastics can preferably be obtained by blending: a) from 0 to 50% by weight, in relation to the total weight of the blend of polypropylene (PP) mixed plastics, of one or more heterophasic propylene ethylene copolymers (HECO); b) from 0 to 50% by weight, in relation to the total weight of the blend of polypropylene (PP) mixed plastics, of one or more propylene homopolymers (h-PP); c) 0 to 10% by weight, relative to the total weight of the plastic mixture Petition 870250103521, dated 12 / 11 / 2025, page 24 / 238 15 / 45 blends of polypropylene (PP), of one or more elastomeric ethylene (E) copolymers; d) from 20 to 90% by weight, in relation to the total weight of the blend of polypropylene (PP) mixed plastics of a blend (B) of polypropylene mixed plastics with a quantity of black spot defects with a particle size in the range of 0.05 to 0.10 mm2 in the range of 0.10 to 4.0 particles / cm2; (e) from 0 to 30% by weight, in relation to the total weight of the blend of mixed polypropylene (PP), carbon fiber and / or glass fiber plastics (F1); f) from 0 to 30% by weight, in relation to the total weight of the blend of polypropylene (PP) mixed plastics, with inorganic filler(s) (F2) other than carbon and / or glass fibers (F1); (g) 0 to 10% by weight, relative to the total weight of the mixed polypropylene (PP) plastics blend, of a polar group modified polypropylene (PMP); and h) 0 to 5% by weight, relative to the total weight of the blend of mixed plastics of polypropylene (PP), other additives other than carbon and / or glass fibers (F1), inorganic filler(s) (F2) and polar group modified polypropylene (PMP).

[0070] More preferably, the blend of mixed polypropylene (PP) plastics of the second type can be obtained by blending: a) 5 to 30% by weight, relative to the total weight of the blend of polypropylene (PP) mixed plastics, of one or more heterophasic propylene ethylene copolymers (HECO); b) 5 to 30% by weight, in relation to the total weight of the blend of polypropylene (PP) mixed plastics, of one or more propylene homopolymers (h-PP); c) 1 to 5% by weight, relative to the total weight of the blend of polypropylene (PP) mixed plastics, of one or more elastomeric ethylene (E) copolymers; Petition 870250103521, dated 12 / 11 / 2025, page 25 / 238 16 / 45 d) from 20 to 70% by weight, in relation to the total weight of the blend of polypropylene (PP) mixed plastics of a blend (B) of polypropylene mixed plastics with a quantity of black spot defects with a particle size in the range of 0.05 to 0.10 mm2 in the range of 0.10 to 4.0 particles / cm2; e) 10 to 30% by weight, in relation to the total weight of the mixture of mixed polypropylene (PP) and glass fiber (F1) plastics; f) 0.5 to 5% by weight, relative to the total weight of the blend of polypropylene (PP) mixed plastics, of a polar group modified polypropylene (PMP); and (g) from 0 to 5% by weight, relative to the total weight of the blend of polypropylene (PP) mixed plastics, of other additives other than glass fibers (F1) and polar group modified polypropylene (PMP), wherein the combined amounts of one or more heterophasic propylene-ethylene copolymers (HECO), one or more propylene homopolymers (h-PP), one or more elastomeric ethylene copolymers (E), the blend (B) of polypropylene mixed plastics, glass fibers (F1), polar group modified polypropylene (PMP), additional additives and equal to 100% by weight, relative to the total weight of the blend of polypropylene (PP) mixed plastics.

[0071] Even more preferably, the blend of mixed polypropylene (PP) plastics of the second type can be obtained by blending: a) 8 to 15% by weight, relative to the total weight of the blend of polypropylene (PP) mixed plastics, of one or more heterophasic propylene ethylene copolymers (HECO); b) 20 to 30% by weight, in relation to the total weight of the blend of polypropylene (PP) mixed plastics, of one or more propylene homopolymers (h-PP); c) 1 to 3% by weight, relative to the total weight of the blend of polypropylene (PP) mixed plastics, of one or more ethylene (E) copolymers Petition 870250103521, dated 12 / 11 / 2025, page 26 / 238 17 / 45 elastomeric; d) 30 to 50% by weight, relative to the total weight of the blend of polypropylene (PP) mixed plastics of a blend (B) of polypropylene mixed plastics having a quantity of black spot defects with a particle size in the range of 0.05 to 0.10 mm2 in the range of 0.10 to 4.0 particles / cm2; e) 15 to 25% by weight, in relation to the total weight of the mixture of mixed polypropylene (PP) and glass fiber (F1) plastics; f) 0.5 to 2% by weight, relative to the total weight of the blend of polypropylene (PP) mixed plastics, of a polar group modified polypropylene (PMP); and (g) from 0 to 3% by weight, relative to the total weight of the blend of polypropylene (PP) mixed plastics, of other additives other than glass fibers (F1) and polar group modified polypropylene (PMP), wherein the combined amounts of one or more heterophasic propylene-ethylene copolymers (HECO), one or more propylene homopolymers (h-PP), one or more elastomeric ethylene copolymers (E), the blend (B) of polypropylene mixed plastics, glass fibers (F1), polar group modified polypropylene (PMP), additional additives and equal to 100% by weight, relative to the total weight of the blend of polypropylene (PP) mixed plastics.

[0072] In this second modality, the acetaldehyde concentration, determined by solid-phase microextraction (HS-SPME-GC-MS) in pellets, is in the range of 0 to 100 mg / m3, with a preference for the range of 5 to 75 mg / m3, with the maximum preference for the range of 10 to 50 mg / m3.

[0073] In this second modality, the hexanal concentration, determined by solid-phase microextraction (HS-SPME-GC-MS) in pellets, is in the range of 0 to 20 mg / m3, with a preference for the range of 0 to 10 mg / m3, with the maximum preference for the range of 0 to 5 mg / m3.

[0074] Additionally, in this second modality, it is preferable that the Petition 870250103521, dated 12 / 11 / 2025, page 27 / 238 18 / 45 blended polypropylene (PP) plastics preferably have a melt flux (MFR2), determined in accordance with ISO 1133 at 230 °C and 2.16 kg, in the range of 1 to 50 g / 10 min, more preferably in the range of 5 to 30 g / 10 min, and most preferably in the range of 8 to 25 g / 10 min.

[0075] In this second embodiment, the blend of mixed polypropylene (PP) plastics preferably has an ethylene content (C2(total)), determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy, in the range of 5.0 to 15.0 % by weight, more preferably in the range of 7.0 to 12.0 % by weight, with the maximum preference in the range of 8.0 to 10.0 % by weight.

[0076] In this second embodiment, the blend of mixed polypropylene (PP) plastics preferably has a soluble fraction (SF) content, determined according to CRYSTEX QC analysis, in the range of 5.0 to 20.0 % by weight, more preferably in the range of 8.0 to 15.0 % by weight, with the maximum preference in the range of 11.0 to 13.0 % by weight.

[0077] In this second embodiment, the blend of mixed polypropylene (PP) plastics preferably has a crystalline fraction (CF) content, determined according to CRYSTEX QC analysis, in the range of 80.0 to 95.0 % by weight, with more preference in the range of 85.0 to 92.0 % by weight, with maximum preference in the range of 87.0 to 89.0 % by weight.

[0078] In this second embodiment, the blend of mixed polypropylene (PP) plastics preferably has an ethylene content in the soluble fraction (C2(SF)), according to the CRYSTEX QC analysis, determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy, in the range of 30 to 60 % by weight, with more preference in the range of 35 to 55 % by weight, with maximum preference in the range of 40 to 50 % by weight.

[0079] In this second embodiment, the blend of mixed polypropylene (PP) plastics preferably has an ethylene content in the crystalline fraction (C2(CF)), according to the CRYSTEX QC analysis, determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy, in the range of 0.5 to 4.0 wt%, more preferably in the range of 0.8 to 3.5 wt%. Petition 870250103521, dated 12 / 11 / 2025, page 28 / 238 19 / 45 weight, with the maximum preference in the range of 1.0 to 2.0% by weight.

[0080] In this second embodiment, the blend of mixed polypropylene (PP) plastics preferably has an intrinsic viscosity, determined in accordance with the DIN ISO 1628 / 1 standard, of the soluble fraction (iV(SF)), according to the CRYSTEX QC analysis, in the range of 1.50 to 2.50 dl / g, more preferably in the range of 1.70 to 2.30 dl / g, with the maximum preference in the range of 1.90 to 2.10 dl / g.

[0081] In this second embodiment, the blend of mixed polypropylene (PP) plastics preferably has an intrinsic viscosity, determined in accordance with the DIN ISO 1628 / 1 standard, of the crystalline fraction (iV(CF)), according to the CRYSTEX QC analysis, in the range of 1.00 to 2.00 dl / g, more preferably in the range of 1.25 to 1.85 dl / g, with the maximum preference in the range of 1.50 to 1.70 dl / g.

[0082] Another essential component of the polypropylene composition is one or more compounds that react with linear alkyl aldehydes.

[0083] In the broadest sense, this component can be any compound that, as understood by a person skilled in the art, reacts with linear alkyl aldehydes. Linear alkyl aldehydes are known to react in various ways, primarily with nucleophiles in addition and / or condensation reactions. Suitable nucleophilic compounds include primary amines (forming imines), secondary amines (forming imines), carbonyl-containing compounds with acidic α-protons (reacting via aldol processes and aldol derivatives (e.g., Knoevenagel condensation)). Alternatively, the aldehyde can react with various nucleophiles to form acetals, hemiacetals, amines or hemiamines, or Mannich reaction products.

[0084] However, certain compounds that react with linear alkyl aldehydes are preferred.

[0085] In one embodiment, one or more compounds reactive with linear aldehydes comprise at least one compound with a structure according to Petition 870250103521, dated 12 / 11 / 2025, page 29 / 238 20 / 45 using formula (I): wherein R1, R2 and R3 are each independently selected from the group consisting of a hydrogen atom, a linear or branched C1-C10 alkyl group, a hydroxyl group, an aryl group, a halogen atom, an acetyl group or a cyano group.

[0086] These barbituric acid-based compounds are particularly effective acid sequestrants.

[0087] It is preferred that each of R1 and R2 be independently selected from the group consisting of a hydrogen atom, a linear or branched C1-C10 alkyl group, an aryl group and an acetyl group.

[0088] It is preferable that R3 be selected from the group consisting of hydrogen, an acetyl group or a cyano group.

[0089] Most preferably, R3 is hydrogen.

[0090] In a particularly preferred embodiment, R1, R2 and R3 are all hydrogens, which means that the compound with a structure according to formula (I) is barbituric acid, that is, it has the following formula:

[0091] In another embodiment, one or more compounds reactive with linear aldehydes comprise at least one compound having a structure according to formula (II): Petition 870250103521, dated 12 / 11 / 2025, page 30 / 238 21 / 45 wherein RA represents from zero to four substitutions, each substitution being independently selected from the group consisting of a linear or branched C1-C10 alkyl group, a linear or branched C1-C10 alkoxy group, an aryl group and a halogen atom, wherein each of RB and RC is selected from the group consisting of hydrogen and a linear or branched C1-C10 alkyl group.

[0092] These anthranilamide-based compounds are also particularly effective acid scavengers.

[0093] It is preferable that each of RB and RC be selected from the group consisting of hydrogen and methyl. Most preferably, both RB and RC are hydrogen.

[0094] RA represents zero to four substitutions, that is, 0, 1, 2, 3 or 4 substitutions. Preferably, RA represents 0, 1 or 2 substitutions. More preferably, RA represents 0 or 1 substitution. Most preferably, RA represents zero substitutions.

[0095] Each RA substitution is preferably selected from the group consisting of a linear or branched C1-C10 alkyl group, a linear or branched C1-C10 alkoxy group, and a halogen atom. More preferably, each RA substitution is selected from the group consisting of a linear or branched C1-C10 alkyl group and a linear or branched C1-C10 alkoxy group. In one embodiment, at least one RA is methyl. In another embodiment, at least one RA is methoxy. In another embodiment, at least one RA is fluorine, chlorine, bromine, or iodine.

[0096] It is particularly preferable that RA represent zero substitutions and RBe RC be both hydrogens, that is, the compound with a structure according to formula (II) is anthranilamide, that is, it has the following formula: Petition 870250103521, dated 12 / 11 / 2025, page 31 / 238 22 / 45

[0097] Both compounds with a structure according to formula (I) (i.e., based on barbituric acid) and those with a structure according to formula (II) (i.e., based on anthranilamide) are not only able to reduce the amounts of aldehyde present in the polypropylene (PC) composition, but also to continue sequestering any additional aldehydes produced during further processing of the composition, for example, during extrusion or molding.

[0098] It is understood that the reactive compound(s) with linear alkyl aldehydes, according to the present invention, reduce(s) the content of linear alkyl aldehydes by several mechanisms besides the oxidation of linear alkyl aldehydes to corresponding linear alkylcarboxylic acids. Therefore, it is further preferred that the concentration of acetic acid, determined by solid-phase microextraction (HS-SPME-GC-MS), does not increase as a result of the addition of the reactive compound(s) with linear alkyl aldehydes.

[0099] The reactive compound(s) with linear alkyl aldehydes according to the present invention may be combined directly with the polypropylene (PP) blended plastics of the invention (i.e., added pure) or, alternatively, may be added via a standard mixture, such as a standard mixture containing anthranilamide.

[0100] If a standard mixture (SM), such as an anthranilamide-containing standard mixture (AAMB), is used, the reactive compound(s) with linear alkyl aldehydes will preferably be present in an amount in the range of 20 to 80% by weight, more preferably in the range of 25 to 75% by weight, most preferably in the range of 30 to 70% by weight, relative to the total weight of the standard mixture (SM).

[0101] The remainder of the standard mixture (SM) weight is comprised of a standard mixture carrier polymer. This standard mixture carrier polymer may be the same as one of the polymeric components of the composition. Petition 870250103521, dated 12 / 11 / 2025, page 32 / 238 23 / 45 of polypropylene (PC), for example, one or more heterophasic propylene-ethylene copolymers (HECO), one or more elastomeric ethylene copolymers (E), or a blend (B) of mixed polypropylene plastics of the second embodiment. Alternatively, the standard blend carrier polymer is different from the polymeric components of the polypropylene (PC) composition. In this case, the weight of the standard blend carrier polymer contributes to the total content of other additives (A) in the second embodiment.

[0102] Suitable carrier polymers may include polypropylene, polyethylene and polyethylene terephthalate).

[0103] If a standard blend (MB) is used, such as an anthranilamide-containing standard blend (AAMB), then the standard blend (MB) is preferably present in an amount in the range of 0.02 to 0.50% by weight, more preferably in the range of 0.06 to 0.40% by weight, most preferably in the range of 0.10 to 0.30% by weight, relative to the total weight of the polypropylene (PC) composition. The article

[0104] In a second aspect, the present invention relates to an article, preferably an injection-molded article, comprising the polypropylene composition according to the first aspect in an amount of at least 95% by weight, more preferably at least 98% by weight, most preferably at least 99% by weight.

[0105] Preferably, the article, more preferably the injection-molded article, is an external automotive article, more preferably selected from the group consisting of bumpers, side trims, running board supports, body panels and spoilers.

[0106] All preferred embodiments and alternative positions for the polypropylene composition of the first aspect apply mutatis mutandis to the article of the second aspect. Use

[0107] In a third aspect, the present invention relates to a use of Petition 870250103521, dated 12 / 11 / 2025, p. 33 / 238 24 / 45 a compound with a structure according to formula (I): wherein R1, R2 and R3 are each independently selected from the group consisting of a hydrogen atom, a linear or branched C1-C10 alkyl group, a hydroxyl group, an aryl group, a halogen atom, an acetyl group or a cyano group, to reduce the acetaldehyde and / or hexanal content of a polypropylene composition derived at least partially from post-consumer waste, without simultaneously increasing the acetone content by more than 30% and without simultaneously increasing the tert-butanol content by more than 10%.

[0108] In a final aspect, the present invention relates to a use of a compound having a structure according to formula (II): wherein RA represents from zero to four substitutions, each substitution being independently selected from the group consisting of a linear or branched C1-C10 alkyl group, a linear or branched C1-C10 alkoxy group, an aryl group or a halogen atom, wherein each of RBe and RC is selected from the group consisting of hydrogen and a linear or branched C1-C10 alkyl group to reduce the acetaldehyde and / or hexanal content of a polypropylene composition derived, at least partially, from post-consumer waste, without simultaneously increasing the acetone content by more than 30% and without simultaneously increasing the tert-butanol content by more than 10%.

[0109] In both the third and final aspects, it is further preferred Petition 870250103521, dated 12 / 11 / 2025, p. 34 / 238 25 / 45 that the concentration of acetic acid, determined by solid-phase microextraction (HS-SPME-GC-MS), of the polypropylene composition derived, at least partially, from post-consumer waste is not increased.

[0110] In both the third aspect and the final aspect, the polypropylene composition is preferably the polypropylene composition of the first aspect.

[0111] All preferred embodiments and alternative positions for compounds with structures conforming to formula (I) or (II) of the first aspect apply mutatis mutandis to the uses of the third aspect and the final aspect. EXAMPLES 1. Measurement methods

[0112] The following definitions of terms and methods of determination apply to the general description of the invention above, including claims, as well as to the examples below, unless otherwise defined. Microstructure quantification by NMR spectroscopy

[0113] Quantitative nuclear magnetic resonance (NMR) spectroscopy was used to quantify the comonomer content of the polymers.

[0114] Quantitative 13C{1H} NMR spectra were recorded in the molten state using a Bruker Avance III 500 NMR spectrometer operating at 500.13 and 125.76 MHz for 1H and 13C, respectively. All spectra were recorded using a 7 mm magic-angle spinning (MAS) optimized 13C probe head at 180 °C using nitrogen gas for all pneumatics. Approximately 200 mg of material were packed into a 7 mm outer diameter zirconia MAS rotor and spun at 4 kHz. This configuration was chosen primarily for the high sensitivity required for rapid identification and accurate quantification {klimke06, parkinson07, castignolles09}. Standard single-pulse excitation was employed using NOE in small recycle delays of 3 seconds {pollard04, klimke06} and the RS-HEPT decoupling scheme {fillip05, griffin07}. A total of 1024 Petition 870250103521, dated 12 / 11 / 2025, page 35 / 238 26 / 45 (1 k) variables were acquired by spectra.

[0115] Quantitative 13C{1H} NMR spectra were processed, integrated, and relevant quantitative properties were determined from the integrals. All chemical shifts are internally referenced to the methyl isotactic pentad (mmmm) at 21.85 ppm.

[0116] Characteristic signals corresponding to the incorporation of 1-butene {brandolini01} were observed and the comonomer content was quantified.

[0117] The amount of isolated 1-butene incorporated into PBP sequences was quantified using the integral of the aB2 sites at 43.6 ppm, which represents the number of reporting sites per comonomer: B = IαB2 / 2

[0118] The amount of 1-butene consecutively incorporated into PBBP sequences was quantified using the ααB2B2 site integral at 40.5 ppm, which represents the number of reporting sites per comonomer: BB = 2 * IααB2B2

[0119] In the presence of BB, the value of B must be corrected for the influence of the aB2 sites resulting from BB: B = (IαB2 / 2) - BB / 2

[0120] The total 1-butene content was calculated based on the sum of isolated and consecutively incorporated 1-butene: Btotal = B + BB

[0121] Characteristic signals corresponding to the incorporation of ethylene {brandolini01} were observed and the comonomer content was quantified.

[0122] The amount of isolated ethylene incorporated into PEP sequences was quantified using the integral of Sββ sites at 24.3 ppm, which represents the number of reporting sites per comonomer: E = Ispp

[0123] If characteristic signals corresponding to the consecutive incorporation of ethylene into the PEE sequence were observed, the Sβδ site at 27.0 ppm was used for quantification: Petition 870250103521, dated 12 / 11 / 2025, p. 36 / 238 27 / 45 EE = Isβδ

[0124] Characteristic signals corresponding to regiodefects were observed {resconi00}. The presence of isolated 2,1-erythro regiodefects was indicated by the presence of the two methyl sites at 17.7 and 17.2 ppm, by the methylene site at 42.4 ppm and confirmed by other characteristic sites. The presence of a 2,1-regiodefect adjacent to an ethylene unit was indicated by the two 8αβ inequivalent signals at 34.8 ppm and 34.4 ppm, respectively, and the Τγγ at 33.7 ppm.

[0125] The amount of isolated 2,1-erythro regiodefects (P21e alone) was quantified using the methylene site integral at 42.4 ppm (E9): P21e isolated = Ie9

[0126] If present, the amount of 2,1 regiodefects adjacent to ethylene (Pe2i) was quantified using the methine site at 33.7 ppm (Ityy): Pe21 = Ityy

[0127] The total ethylene content was then calculated based on the sum of ethylene from 2,1 isolated, consecutively incorporated and adjacent regiodefects: Etotal = E + EE + Pe21

[0128] The amount of propene was quantified based on methylene 8αα sites at 46.7 ppm, including all additional propene units not covered by 8αα, for example, the 3*P21e factor alone accounts for the three missing propene units in isolated 2,1-erythro regiodefects: Ptotal = I8aa + 3*P21e isolated + B + 0.5*BB + E + 0.5*EE + 2*Pe21

[0129] The total mole fraction of 1-butene and ethylene in the polymer was then calculated as: fB = Btotal / ( Etotal + Ptotal + Btotal ) fE = Etotal / ( Etotal + Ptotal + Btotal )

[0130] The comonomer incorporation percentage by mole was calculated from the mole fractions: B [% in mol] = 100 * fB E [% in mol] = 100 * fE Petition 870250103521, dated 12 / 11 / 2025, page 37 / 238 28 / 45

[0131] The incorporation of comonomer in weight percent was calculated from the mole fractions: B [% by weight] = 100 * (fB * 56.11) / ((fE * 28.05) + (fB * 56.11) + ((l-(fE+fB)) * 42.08)) E [% by weight] = 100 * (fE * 28.05) / ((fE * 28.05) + (fB * 56.11) + ((l - (fE + fB)) * 42.08))

[0132] The mole percentage of isolated 2,1-erythro regiodefects was quantified relative to the whole propylene: [21e] % in mol = 100 * Isolated P21e / Total P

[0133] The mole percentage of 2,1 regiodefects adjacent to ethylene was quantified relative to all propylene: [E21] % in mol = 100 * PE21 / Ptotal

[0134] The total number of 2.1 regiodefects was quantified as follows:

[21] % in mol = [21e] + [E21]

[0135] Characteristic signals corresponding to other types of regiodefects (insertion 2,1-treo, 3,1) were not observed {resconi00}. Literature (as mentioned above):

[0136] klimke06 Klimke, K., Parkinson, M., Piel, C., Kaminsky, W., Spiess, H. W., Wilhelm, M., Macromol. Chem. Phys. 2006;207:382. parkinson07 Parkinson, M., Klimke, K., Spiess, H. W., Wilhelm, M., Macromol. Chem. Phys. 2007;208:2128. pollard04 Pollard, M., Klimke, K., Graf, R., Spiess, H. W., Wilhelm, M., Sperber, O., Piel, C., Kaminsky, W., Macromolecules 2004;37:813. filip05 griffin07 Filip, Graf, R., Parkinson, M., Wilhelm, M., Petition 870250103521, dated 12 / 11 / 2025, p. 38 / 238 29 / 45 Gaborieau, M., Polymer 50 (2009) 2373. resconiOO Resconi, L., Cavallo, L., Fait, A., Piemontesi, F., Chem. Rev. 2000, 100, 1253. brandolini01 AJ Brandolini, DD Hills, “NMR Spectra of Polymers and Polymer Additives”, Marcel Deker Inc., 2000 CRYSTEX QC Review Method of crystalline and soluble fractions

[0137] The crystalline (CF) and soluble (SF) fractions of the polypropylene (PP) compositions, as well as the comonomer content and intrinsic viscosities of the respective fractions, were analyzed using the CRYSTEX instrument, Polymer Char (Valencia, Spain). Details of the technique and method can be found in the literature (Ljiljana Jeremic, Andreas Albrecht, Martina Sandholzer & Markus Gahleitner (2020) Rapid characterization of high-impact ethylene-propylene copolymer composition by crystallization extraction separation: comparability to standard separation methods, International Journal of Polymer Analysis and Characterization, 25:8, 581-596).

[0138] The crystalline and amorphous fractions are separated by dissolution temperature cycles at 160 °C, crystallization at 40 °C and redissolution in 1,2,4-trichlorobenzene at 160 °C. Quantification of SF and CF and determination of ethylene content (C2) are obtained by means of an integrated infrared detector (IR4) and for the determination of intrinsic viscosity (IV) an online 2-capillary viscometer is used.

[0139] The IR4 detector is a multi-wavelength detector that measures IR absorbance in two different bands (CH3 stretching vibration (centered at approx. 2960 cm-1) and CH stretching vibration (2700-3000 cm-1)) which serve for the determination of the concentration and content of ethylene in ethylene-propylene copolymers. The IR4 detector is calibrated with a series of 8 EP copolymers with known ethylene content in the range of 2 wt% to 69 wt% (determined by 13C-NMR) and each at various concentrations, in the range of 2 and 13 mg / ml. To consider both features, concentration and Petition 870250103521, dated 12 / 11 / 2025, page 39 / 238 30 / 45 ethylene content at the same time for various expected polymer concentrations during Crystex analyses, the following calibration equations were applied: Conc = a + b*Abs(CH) + c*(Abs(CH))2 + d*Abs(CH3) + e*(Abs(CH3)2+ f*Abs(CH)*Abs(CH3) (Equation 1) CH3 / 1000C = a + b*Abs(CH) + c*Abs(CH3) + d*(Abs(CH3) / Abs(CH)) + e*(Abs(CH3) / Abs(CH))2 (Equation 2)

[0140] The constants a up to and for equation 1 and a up to f for equation 2 were determined using least squares regression analysis.

[0141] CH3 / 1000C is converted to ethylene content in % by weight using the following relationship: % by weight (Ethylene in EP Copolymers) = 100 - CH3 / 1000TC * 0.3 (Equation 3)

[0142] The amounts of Soluble Fraction (SF) and Crystalline Fraction (CF) are correlated through XS calibration to the amount of “Cold Soluble in Xylene” (XCS) and, respectively, the Cold Insoluble in Xylene (XCI) fractions, determined according to the standard gravimetric method in accordance with ISO16152. The XS calibration is obtained by testing various EP copolymers with XS content in the range of 2-31% by weight. The determined XS calibration is linear: % by weight of XS = 1.01 * % by weight of SF (Equation 4)

[0143] The intrinsic viscosity (IV) of the parent EP copolymer and its soluble and crystalline fractions are determined using a 2-capillary in-line viscometer and correlated to the corresponding IVs determined by the standard decalin method according to ISO 1628-3. Calibration is achieved with several EP-PP copolymers with IV = 24 dl / g. The calibration curve determined is linear: IV (dl / g) = a* Vsp / c (equation 5)

[0144] The samples to be analyzed are weighed at concentrations of 10 mg / ml to 20 mg / ml. To avoid injecting possible gels and / or polymers that do not Petition 870250103521, dated 12 / 11 / 2025, page 40 / 238 31 / 45 dissolve in TCB at 160 °C, like PET and PA, the weighted sample was packed in a stainless steel mesh MW 0.077 / D 0.05 mm.

[0145] After automated filling of the flask with 1,2,4-TCB containing 250 mg / l of 2,6-tert-butyl-4-methylphenol (BHT) as an antioxidant, the sample is dissolved at 160 °C until complete dissolution is obtained, usually for 60 min, with constant stirring at 400 rpm. To prevent sample degradation, the polymer solution is covered with a N2 atmosphere during dissolution.

[0146] A defined volume of the sample solution is injected into the column packed with inert support where sample crystallization and separation of the soluble fraction from the crystalline part is occurring. This process is repeated twice. During the first injection, the entire sample is measured at high temperature, determining the IV[dl / g] and C2[% by weight] of the PP composition. During the second injection, the soluble fraction (at low temperature) and the crystalline fraction (at high temperature) with the crystallization cycle are measured (% by weight of SF, % by weight of C2, IV). Intrinsic viscosity

[0147] Intrinsic viscosity is measured according to DIN ISO 1628 / 1, October 1999 (in Decalina at 135 °C). Melt flow rate

[0148] The melt flow rate (MFR) is determined according to ISO 1133 and is indicated in g / 10 min. The MFR is an indication of the flowability and, therefore, the processability of the polymer.

[0149] The higher the melt flow rate, the lower the viscosity of the polymer. The MFR2 of polypropylene is determined at a temperature of 230 °C and a load of 2.16 kg. Density:

[0150] Density is measured according to ISO 1183-187. Sample preparation is done by compression molding according to Petition 870250103521, dated 12 / 11 / 2025, page 41 / 238 32 / 45 the ISO 1872-2:2007 standard.

[0151] The xylene-soluble fraction at room temperature (XCS, % by weight): The amount of xylene-soluble polymer is determined at 25 °C according to ISO 16152; 5th edition; 01 / 07 / 2005.

[0152] DSC analysis, melting temperature (Tm) and heat of fusion (Hf), crystallization temperature (Tc) and heat of crystallization (Hc): measured with a TA Instrument Q200 differential scanning calorimetry (DSC) on samples of 5 to 7 mg. DSC operates according to ISO 11357 / part 3 / method C2 in a heat / cold / heat cycle with a scan rate of 10 °C / min in the temperature range of -30 to +225 °C. The crystallization temperature (Tc) and enthalpy of crystallization (Hc) are determined from the cooling step, while the melting temperature (Tm) and enthalpy of fusion (Hm) are determined from the second heating step.

[0153] The Flexural Modulus is determined according to the ISO 178 A method (3-point bending test) on specimens of 80 mm x 10 mm x 4 mm. Following the standard, a test speed of 2 mm / min and a span length of 16 times the thickness were used. The test temperature was 23 ± 2 °C. Injection molding was performed according to ISO 19069-2 using a melt temperature of 230 °C for all materials, regardless of the material melt flow rate. Notch impact resistance (NIS)

[0154] The Charpy impact resistance with notch (NIS) is measured according to ISO 179 1eA at +23 °C or -20 °C, using 80x10x4 mm3 injection molded bar test specimens prepared according to ISO 19069-2 using a melting temperature of 230 °C for all materials, regardless of the melt flow rate. Inorganic waste

[0155] Inorganic residues are quantified according to DIN ISO 1172:1996 using a Perkin Elmer TGA 8000. Approximately 1020 mg of material were placed in a platinum pan. The temperature was Petition 870250103521, dated 12 / 11 / 2025, page 42 / 238 33 / 45 equilibrated at 50 °C for 10 minutes, and then heated to 950 °C under nitrogen at a heating rate of 20 °C / min. The ash content was evaluated as a % by weight at 850 °C. Quantification of black spots (quantity of defects with specific particle sizes)

[0156] Digital images of 5 injection-molded plates were collected with a Canon EOS R6 camera. The settings were fixed so that a resolution of approximately 15 pixels / mm was obtained. After the image was converted to grayscale and the intensity normalized between 0 and 256, the exposure time was fixed so that a gray level of approximately 160 was obtained for the plates.

[0157] Image analysis was performed using Wavemetrics IgorPro software. A Region of Interest area was fixed inside the plates, with a size of 2100 x 1125 pixels2. A Prewitt edge detection algorithm, defined with a limit of 10, was used to identify particles on the surface. The edge image was then analyzed to collect information on the number and size of the detected particles, with a minimum area of ​​5 pixels and excluding particles that touched the edge of the analyzed area. This operation was repeated for the 5 photographed plates and a particle size distribution was created. The number of particles was normalized by the total area visualized on the 5 plates and, therefore, a particle frequency as n° / cm2 was obtained. The particles were grouped into compartments according to their size, with a compartment size of 0.05 mm2.As should be clear to anyone versed in the technique, the size of each black dot can be simply calculated from the number of pixels and the area of ​​each pixel. Quantity of iPP, polystyrene, polyethylene (and copolymers containing ethylene), polyethylene terephthalate) and quantity of polyamide-6

[0158] Calibration standards are prepared by mixing iPP and HDPE to generate a calibration curve. The thickness of the calibration standard films is 300 µm. For the quantification of iPP, PS and PA 6 content in Petition 870250103521, dated 12 / 11 / 2025, page 43 / 238 34 / 45 samples, quantitative IR spectra are recorded in the solid state using a Bruker Vertex 70 FTIR spectrometer. The spectra are recorded on 25x25 mm square films of 50-100 µm thickness prepared by compression molding at 190 °C and 4-6 mPa. Standard transmission FTIR spectroscopy is employed using a spectral range of 4000 cm⁻¹, an aperture of 6 mm, a spectral resolution of 2 cm⁻¹, 16 background scans, 16 spectrum scans, an interferogram with a zero-filling factor of 32 and strong Norton Beer apodization.

[0159] The absorption band at 1167 cm⁻¹ in iPP is measured, and the iPP content is quantified according to a calibration curve (absorption / thickness in cm versus iPP content in % by weight). The absorption band at 1601 cm⁻¹ (PS), 1513 cm⁻¹ (PET), and 3300 cm⁻¹ (PA6) is measured, and the PS, PET, and PA6 content is quantified according to the calibration curve (absorption / thickness in cm versus PS, PET, and PA content in % by weight). The content of copolymers containing polyethylene and ethylene is obtained by subtracting (iPP + PS + PET + PA6) from 100, considering the content of non-polymeric impurities as determined in the methods below. The analysis is performed as a double determination. Static headspace analysis for odorant content determination.

[0160] The parameters of the headspace gas chromatography mass spectrometry (HS / GC / MS) method applied are described in this document.

[0161] For the measurement of a standard solution, 5 pl of a standard solution containing 0.072 pg / ml acetaldehyde, 0.075 pg / ml hexanal, 0.081 pg / ml D-limonene, 1.499 pg / ml acetone and 0.078 pg / ml tert-butanol in 2-butanol solvent were injected into a 20 ml HS vial and tightly closed with a PTFE stopper. Each HS / GC / MS test sequence of sample measurements included the analysis of such a standard. Petition 870250103521, dated 12 / 11 / 2025, page 44 / 238 35 / 45

[0162] The samples were also analyzed by HS / GC / MS to determine acetaldehyde, hexanal, D-limonene, acetone, and tert-butanol. Therefore, 2.000 ± 0.100 g aliquots of a sample were weighed into a 20 ml HS vial and hermetically sealed with a PTFE cap. In samples CE1, CE2, IE1, IE2, approximately 10 g of the sample were cryo-ground before weighing into the aliquot. Otherwise, the sample pellet aliquot was weighed directly (CE3, CE4, CE5, IE3, IE4, IE5). When applicable, sequestrants were added according to the recipe shown in Table 4. Therefore, approximately 5 mg of sequestrant were weighed into a 20 ml vial with headspace (for cases with 0.25% sequestrant in the mixture). Approximately 20 mg of sequestrant were weighed in to make up 1% by weight in the final mixture.

[0163] Each of the sealed flasks was heated to 250 °C, held at that temperature for 10 minutes, and then cooled to room temperature.

[0164] Samples for CE6, IE6, and IE7 were cut from the middle of an injection-molded plate with dimensions of 148.5 x 210 x 3 mm. The plate was produced on an Engel ES 1050 / 250 HL injection molding machine with a melting temperature between 240 and 250 °C, using a holding pressure of 419 bar at 3.5 s. After production, the plates were stored at ambient conditions for 6 to 8 hours, subsequently packaged in A1 bags.

[0165] After heat treatment, for samples in CE1, CE2, IE1, IE2, CE3, CE4, CE5, IE3, IE4, IE5 or by cutting them directly from injection-molded plates in the case of CE6, IE6 and IE7, the samples were analyzed by HS / GC / MS at 100 °C / 2 h under isothermal headspace conditions.

[0166] The headspace parameters applied for standard and sample analyses differed in the flask equilibration time and HS oven temperature. Furthermore, the method parameters were kept the same for standard and sample runs. The mass spectrometer was operated in scanning mode and a total ion chromatogram (TIC) was recorded. Petition 870250103521, dated 12 / 11 / 2025, page 45 / 238 36 / 45 for each analysis. Substance identification was confirmed by deconvolution and by comparing the retention time with the respective marker substance in the standard. More detailed information on the method parameters and data evaluation software is provided below: > HS parameter (Headspace sampler Agilent G1888) Bulb equilibration time: 5 min (standard), 120 min (sample) Oven temperature: 200 °C (standard), 100 °C (sample) Cycle temperature: 205 °C Transfer line temperature: 210 °C Low agitation > GC parameter (Agilent 7890A GC system) Column: ZB-WAX 7HG-G007-22 (30 m x 250 pm x 1 pm) Carrier gas: Helium 5.0 Flow rate: 2 ml / min Ratio: 10:1 GC oven program: 35 °C for 0.1 min 10 °C / min up to 250 °C 250 °C for 1 min • MS parameter (Agilent 5975C inert XL MSD) Acquisition method: Scanning Scan parameters: Low mass: 20 High mass: 200 Threshold: 10 • Software / data evaluation MSD ChemStation F.01.03.2357 MSD ChemStation E.02.02.1431 AMDIS GC / MS Analysis Version 2.71 NIST Mass Spectral Library (2011 version) NIST11.L Petition 870250103521, dated 12 / 11 / 2025, page 46 / 238 37 / 45 Microsoft Excel Versions 2010 and 2016 Data evaluation

[0167] For further evaluation of the data, extracted ion chromatograms (EICs) of the marker compounds measured in the standard and samples were used. The corresponding target ions are described in Table 1. Table 1: Retention times and specific target ions for the selected marker substances. Substance | Retention time / min | Target ion (m / z) | Acetaldehyde | 1.6 | 44 | Acetone | 2.3 | 58 | tert-Butanol | 3.1 | 59 | Hexanal | 5.7 | 44 | D-limonene | 7.6 | 136

[0168] The standard concentration of a marker substance in the HS vial (cStandard™ [mg / m3]) was calculated according to equation 1, where the concentration of the marker substance in the liquid standard (CPad™ [pg / ml]) was multiplied by the injection volume (VInJeça0[pl]) of the standard and divided by the volume of the HS vial (vstandaHSrd[ml]). Here, an HS volume of 20 ml is used as standard. Standard Injection CPa drã0= _s-------- Equation 1

[0169] For each marker compound in the standard, a response factor (Rf) was calculated according to equation 2. çPa drãoR f= Are, db^--* Equation2

[0170] In this case, the concentration of the marker compound is divided by the integrated peak area of ​​the corresponding marker compound in the EIC (Standard Peak Area).

[0171] To estimate the respective concentration of marker compound in Petition 870250103521, dated 12 / 11 / 2025, page 47 / 238 38 / 45 headspace of a sample (c£sample[mg / m3]), equation 3 was used. Therefore, the response factor obtained from equation 2 is multiplied by the peak area of ​​the corresponding marker compound in the EIC of the sample run (Sample Peak Area). C^sample = ff * Peak Area Sample Equation 3 2. Examples 2.1 Synthesis of heterophasic propylene-ethylene copolymers (HECO)

[0172] The catalyst used to produce HECO was a Borealis ZieglerNatta catalyst with a Ti content of 1.9 wt% (as described in document EP 591 224). Prior to polymerization, the catalyst was prepolymerized with vinylcyclohexane (VCH) as described in documents EP 1 028 984 and EP 1 183 307. A VCH to catalyst ratio of 1:1 was used in the preparation, thus the final poly-VCH content was less than 100 ppm.

[0173] Subsequent polymerization was carried out under the following conditions. Table 1 Polymerization conditions for HECOs HECO Pre-polymerization [Co] / [ED] [mol / mol] 40 [Co] / [Ti] [mol / mol] 230 Temperature [°C] 30 Residence time [min] 5 Cycle reactor Temperature [°C] 72 Division [% by weight] 30 H2 / C3 [kg / ton] 18.8 MFR2 [g / 10 min] 110 1st gas phase reactor Temperature [°C] 80 Petition 870250103521, dated 12 / 11 / 2025, page 48 / 238 39 / 45 HECO Division [% by weight] 35 H2 / C3 [mol / kmol] 137 MFR2 [g / 10 min] 80 MFR2 (1st fraction GPR) [g / 10 min] 62 XCS [% by weight] 2.0 2nd gas phase reactor Temperature [°C] 70 Division [% by weight] 17 H2 / C3 [mol / kmol] 119 C2 / C3 [mol / kmol] 515 MFR2 [g / 10 min] 15 C2 [% by weight] 7.9 3rd gas phase reactor Temperature [°C] 85 Division [% by weight] 18 H2 / C3 [mol / kmol] 285 C2 / C3 [mol / kmol] 1429 MFR2 [g / 10 min] 18 C2 [% by weight] 18.9 Final Properties (pellet) MFR2 [g / 10 min] 18 C2 [% by weight] 20 SF [% by weight] 30 C2(SF) [% by weight] 45 iV(SF) [dF / g] 2.40 CF [% by weight] 70 C2(CF) [% by weight] 9 Petition 870250103521, dated 12 / 11 / 2025, p. 49 / 238 40 / 45 HECO iV(CF) [dF / g] 1.44 Tm [°C] 165 Tc [°C] 115

[0174] The heterophasic propylene-ethylene copolymer HECO was compounded in a Coperion ZSK 47 co-rotating twin-screw extruder at 220 °C with 0.15 wt% antioxidant (Irganox B215 FF together with BASF AG, Germany; this is a 1:2 mixture of pentaerythryl-tetrakis(3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate, CAS No. 6683-19-8 and Tris(2,4-di-t-butylphenyl)phosphite, CAS No. 31570-04-4); Faci, Italy). 2.2 Blends (B) of mixed polypropylene plastics

[0175] The properties of the mixed polypropylene plastic blends (B1 and B2) are given in Table 2 Table 2 Properties of blends (B) of polypropylene blended plastics B1 B2 Density [kg / m3] 917 920 MFR2 [g / 10 min] 25 17 C2(total) [% by weight] 5 8 SF [% by weight] 11 11 C2(SF) [% by weight] 28 29 iV(SF) [dF / g] 1.71 1.70 CF [% by weight] 89 89 C2(CF) [% by weight] 3 5 iV(CF) [dF / g] 1.55 1.69 Inorganic residues [% by weight] 1 1 Flexural modulus [MPa] 1344 1247 Charpy NIS (23 °C) [kJ / m2] 5.14 5.50 Petition 870250103521, dated 12 / 11 / 2025, page 50 / 238 41 / 45 Defect content (0.05 to 0.10 mm2) [particles / cm2] 0.2 3.0

[0176] The blend of mixed polypropylene plastics (B1) additionally comprises smaller amounts of polystyrene, polyamide-6 and fatty acids. 2.3 Composition of inventive and comparative compositions

[0177] In addition to the HECOs and the polypropylene blended plastics described above, the following commercially available components were also used: h-PP is a commercial propylene homopolymer HF955MO, commercially available from Borealis AG (Austria), with an MFR2 (230 °C) of 20 g / 10 min, a density of 905 kg / m3, a flexural modulus of 2000 MPa and a Charpy NIS (+23 °C) of 2.5 kJ / m2. EC is an ethylene-octene elastomeric copolymer with the trade name Engage 8842, commercially available from Dow Chemicals (USA), with an MFR2 (190 °C) of 1.0 g / 10 min and a density of 857 kg / m3. PMP is a commercially available maleic anhydride grafted polypropylene (MAH-PP) Scona TPPP 8112 GA from BYK Chemie (Germany), with an MFR2 (190 °C) of 100 g / 10 min and a MAH content of 1.2% by weight. F1 cut fiberglass DS 2200-13P from 3B Fibreglass (Belgium), with a diameter of 13 µm and a fiber length of 4 mm. CBMB is a standard blend based on FDPE CMB520 Black 7PE-30 from QolorTech BV (Netherlands) containing 30% carbon black by weight. Petition 870250103521, dated 12 / 11 / 2025, p. 51 / 238 42 / 45 A1 is a sulfur-based antioxidant with the trade name Irganox PS-802 FF, commercially available from BASF AG (Germany). A2 is an antioxidant blend with the trade name Irganox B215 FF, commercially available from BASF AG (Germany), being a 1:2 mixture of pentaerythrityl-tetrakis(3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate, CAS no. 6683-19-8, and tris-(2,4-di-tert-butylphenyl)phosphite, CAS no. 31570-04-4); MB is a standard blend propylene homopolymer carrier with the trade name HC001 A, commercially available from Borealis AG (Austria). Alpha-cyclodextrin CAS no. 10016-20-3, commercially available from Sigma Aldrich (Germany). Antranilamide CAS no. 88-68-6, commercially available from Sigma Aldrich (Germany). Barbituric acid CAS no. 67-52-7, commercially available from Sigma Aldrich (Germany). m-Xylylenediamine CAS no. 1477-55-0, commercially available from Sigma Aldrich (Germany).AAMB A standard mixture containing anthranilamide with 30 to 70% by weight of anthranilamide, commercially available from Holland Colours NV (NE) under the trade name TasteGuard Ultramax.

[0178] In a first step, a representative recycled-containing polypropylene (PP) composition suitable for automotive applications was produced by blending according to the recipe presented in Table 3. The recycled-containing polypropylene (PP) composition used for CE3 to CE5 and IE3 to IE5 was prepared by blending in a Coperion ZSK 40 co-rotating twin-screw extruder at 220 °C. The polypropylene (PP) composition Petition 870250103521, dated 12 / 11 / 2025, page 52 / 238 43 / 45 containing recycled material used for CE6, IE6 and IE7 was prepared by composition in a Coperion ZSK 32 co-rotating twin-screw extruder at 220 °C. Table 3 Suitable polypropylene (PC) composition for automotive applications PP Ingredients B2 [% by weight] 39.30 HECO [% by weight] 10.00 h-PP [% by weight] 25.00 EC [% by weight] 2.00 PMP [% by weight] 1.00 F1 [% by weight] 20.00 CBMB [% by weight] 0.70 A1 [% by weight] 0.40 A2 [% by weight] 0.25 Vehicle MB [% by weight] 1.35 Properties MFR2 [g / 10 min] 10 C2(total) [% by weight] 9 SF [% by weight] 12 C2(SF) [% by weight] 44 iV(SF) [dl / g] 1.96 CF [% by weight] 88 C2(CF) [% by weight] 1.2 iV(CF) [dF / g] 1.63 Defect content (0.05 to 0.10 mm2) [particles / cm2] 1.2

[0179] The B1 and B2 recycled blends, as well as the recycled-containing (PC) composition, were additionally blended with various compounds. Petition 870250103521, dated 12 / 11 / 2025, page 53 / 238 44 / 45 additional compounds (pure compounds for CE4, CE5 and IE3 to IE5 or in standard mixture form for IE6 and IE7) were used to test the potential of said compounds as aldehyde scavengers. The recipes for these comparative and inventive examples are presented in Table 4, as well as their odorant contents. The odorant contents of CE1-CE2 and IE1-IE2 were measured in powder samples (formed by cryogenic milling of pellets), while the odorant contents of CE3-CE5 and IE3-IE5 were measured in pelletized samples. The odorant contents of CE6, IE6 and IE7 were measured in injection-molded plates, as described in the determination methods.

[0180] In all cases, the MFR2 and CRYSTEX properties of the compositions were not altered by the addition of aldehyde scavengers, i.e., the properties of the inventive and comparative examples in this respect are simply the same as those of the base resin employed (i.e., the same as CE1, CE2 or CE3).

[0181] As can be seen in Table 4, anthranilamide and barbituric acid are effective in reducing the acetaldehyde and hexanal content in recycled materials (IE1 vs. CE1 and IE2 vs. CE2) and in compositions containing recycled materials (IE3 to IE5 vs. CE3), with low amounts, such as 0.25% by weight of aldehyde scavenger, sufficient to obtain a considerable effect (while higher amounts, such as 1.00% by weight, may further enhance the effect). The content of non-aldehyde odorants is not significantly altered by the presence of anthranilamide or barbituric acid. Alpha-cyclodextrin, on the other hand, is ineffective in reducing aldehyde content (CE4 vs. CE3), and although m-xylylenediamine is able to reduce aldehyde content, it simultaneously increases acetone and tert-butanol content to almost double their initial levels (CE5 vs. CE3).IE6 and IE7 show that small amounts of anthranilamide, introduced through the use of a standard mixing composition, are also highly effective (vs. CE6). Petition 870250103521, dated 12 / 11 / 2025, page 54 / 238 45 / 45 Table 4 Recipes for inventive and comparative examples and odorant content IE7 Components ii 99.90 i 1 1 i 0.10 Odorant contents nmnm CO 58 00 x— IE6 ii 99.95 i 1 1 i 0.05 nmnm 67 00 1 0.25 i 25 nd* nd* 434 118 IE5 ii 99.00 i 1 1.00 ii 25 nd* 14 220 65 IE4 ii 9Z'66 i 1 0.25 ii 25 nd* 33 213 65 IE3 ii 99.75 i 0.25 1 ii 25 nd* 47 170 69 CE4 ii 99.75 0.25 1 1 ii 25 nd* 287 154 46 CE3 ii 100 i 1 1 ii 25 nd* 300 174 64 IE2 i 99.75 1 i 1 0.25 ii 55 36 1646 4750 139 CE2 i 100 1 i 1 1 ii 55 63 3328 5433 148 IE1 99.75 1 1 1 1 0.25 1 1 r- 14 259 3102 375 CE1 100 i 1 i 1 1 ii CO 55 3060 4650 456 [% by weight] [% by weight] [% [by weight] [% by weight] [% by weight] [% by weight] [% by weight] [% by weight] E ~δ> E, [εω / 6ιυ] [mg / m3] [mg / m3] E £ B1 B2 dd Alphacyclodextrin Antranilamide Barbituric acid xylylenediamine AAMB D-limonene Hexanal Acetaldehyde Acetone tert-Butanol nd = not detected, i.e., below the detection limit, nm = not measured. Petition 870250103521, dated 12 / 11 / 2025, p. 55 / 238

Claims

1 / 7 CLAIMS 1. Polypropylene (PC) composition characterized by comprising: a) a blend of mixed polypropylene (PP) plastics with a quantity of black spot defects with a particle size in the range of 0.05 to 0.10 mm2 in the range of 0.10 to 4.0 particles / cm2; and b) one or more compounds reactive with linear alkyl aldehydes.

2. Polypropylene (PC) composition characterized by comprising: a) a blend of polypropylene (PP) mixed plastics derived, at least partially, from post-consumer waste; and b) one or more compounds reactive with linear alkyl aldehydes.

3. Polypropylene (PC) composition according to claim 1 or 2, characterized in that one or more compounds reactive with linear aldehydes comprise at least one compound having a structure according to formula (I): wherein R1, R2 and R3 are each independently selected from the group consisting of a hydrogen atom, a linear or branched C1-C10 alkyl group, a hydroxyl group, an aryl group, a halogen atom, an acetyl group or a cyano group.

4. Polypropylene (PC) composition according to any of the preceding claims, characterized in that one or more compounds reactive with linear aldehydes comprise at least one compound having a structure according to formula (II): Petition 870250103521, 12 / 11 / 2025, p. 56 / 238 2 / 7 wherein RA represents from zero to four substitutions, each substitution being independently selected from the group consisting of a linear or branched C1-C10 alkyl group, a linear or branched C1-C10 alkoxy group, an aryl group or a halogen atom, wherein each of RB and RC is selected from the group consisting of hydrogen and a linear or branched C1-C10 alkyl group.

5. Polypropylene (PC) composition, according to any of the preceding claims, characterized in that the blend of polypropylene (PP) mixed plastics has one or more of the following properties, preferably all: a) a melt flow rate (MFR2), determined according to ISO 1133 at 230 °C and 2.16 kg, in the range of 5.0 to 100 g / 10 min; b) an ethylene content (C2(total)), determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy, in the range of 3.0 to 15.0 % by weight; c) a soluble fraction (SF) content, determined according to CRYSTEX QC analysis, in the range of 5.0 to 20.0 wt% and a crystalline fraction (CF) content, determined according to CRYSTEX QC analysis, in the range of 80.0 to 95.0 wt%; d) an ethylene content of the soluble fraction (C2(SF)), according to CRYSTEX QC analysis, determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy, in the range of 15 to 60 wt%;e) an ethylene content of the crystalline fraction (C2(CF)), according to CRYSTEX QC analysis, determined by FT-IR spectroscopy calibrated by quantitative 13C-NMR spectroscopy, in the range of 0.5 to 6.0 % by weight; Petition 870250103521, dated 12 / 11 / 2025, page 57 / 238 3 / 7 f) an intrinsic viscosity of the soluble fraction (iV(SF)), according to CRYSTEX QC analysis, determined according to DIN ISO 1628 / 1, in the range of 1.50 to 2.50 dl / g; (g) an intrinsic viscosity of the crystalline fraction (iV(CF)), according to CRYSTEX QC analysis, determined in accordance with DIN ISO 1628 / 1, in the range of 1.00 to 2.00 dl / g.; 6. Polypropylene (PC) composition, according to any of the preceding claims, characterized in that the polypropylene (PP) blended plastics are obtainable by blending: a) from 0 to 50% by weight, relative to the total weight of the polypropylene (PP) blended plastics, of one or more heterophasic propylene ethylene copolymers (HECO); b) from 0 to 50% by weight, relative to the total weight of the polypropylene (PP) blended plastics, of one or more propylene homopolymers (h-PP); c) from 0 to 10% by weight, relative to the total weight of the polypropylene (PP) blended plastics, of one or more elastomeric ethylene (E) copolymers; d) from 20 to 90% by weight, in relation to the total weight of the blend of polypropylene (PP) mixed plastics of a blend (B) of polypropylene mixed plastics with a quantity of black spot defects with a particle size in the range of 0.05 to 0.10 mm2 in the range of 0.10 to 4.0 particles / cm2;e) 0 to 30% by weight, relative to the total weight of the blend of polypropylene (PP), carbon and / or glass fibers (F1); f) 0 to 30% by weight, relative to the total weight of the blend of polypropylene (PP) plastics, of inorganic filler(s) (F2) other than carbon and / or glass fibers (F1); g) 0 to 10% by weight, relative to the total weight of the blend of polypropylene (PP) plastics, of a polar group modified polypropylene (PMP); eh) from 0 to 5% by weight, relative to the total weight of the blend of mixed plastics of polypropylene (PP), other additives other than carbon and / or glass fibers (F1), inorganic filler(s) (F2) and polar group modified polypropylene (PMP).; 7. Polypropylene (PC) composition according to claim 6, characterized in that the polypropylene (PP) blended plastics are obtainable by blending: a) 5 to 30% by weight, relative to the total weight of the polypropylene (PP) blended plastics, of one or more heterophasic propylene ethylene copolymers (HECO); b) 5 to 30% by weight, relative to the total weight of the polypropylene (PP) blended plastics, of one or more propylene homopolymers (h-PP); c) 1 to 5% by weight, relative to the total weight of the polypropylene (PP) blended plastics, of one or more elastomeric ethylene (E) copolymers; d) from 20 to 70% by weight, in relation to the total weight of the blend of polypropylene (PP) mixed plastics of a blend (B) of polypropylene mixed plastics with a quantity of black spot defects with a particle size in the range of 0.05 to 0.10 mm2 in the range of 0.10 to 4.0 particles / cm2;e) 10 to 30% by weight, relative to the total weight of the blend of polypropylene (PP) and glass fiber (F1) plastics; f) 0.5 to 5% by weight, relative to the total weight of the blend of polypropylene (PP) plastics, of a polar group modified polypropylene (PMP); g) 0 to 5% by weight, relative to the total weight of the blend of polypropylene (PP) plastics, of other additives different from glass fiber (F1) and polar group modified polypropylene (PMP). Petition 870250103521, dated 12 / 11 / 2025, page 59 / 238 5 / 7; 8. Polypropylene (PC) composition according to claim 6 or 7, characterized in that the blend (B) of mixed polypropylene plastics originates from post-consumer waste.

9. Polypropylene (PC) composition, according to any one of claims 6 to 8, characterized by having an acetaldehyde concentration, determined by solid-phase microextraction (HS-SPME-GC-MS), in the range of 0 to 100 mg / m3.

10. Polypropylene (PC) composition, according to any one of claims 1 to 5, characterized in that the blend of mixed polypropylene (PP) plastics originates from post-consumer waste.

11. Polypropylene (PC) composition according to claim 10, characterized by having an acetaldehyde concentration, determined by solid-phase microextraction (HS-SPME-GC-MS), in the range of 100 to 2000 mg / m3.

12. Polypropylene (PC) composition, according to any of the preceding claims, characterized by having an acetaldehyde concentration determined by solid-phase microextraction (HS-SPME-GC-MS) in the range of 0 to 50% of the acetaldehyde concentration value of the polypropylene (PP) blended plastics, also determined by solid-phase microextraction (HS-SPME-GC-MS).

13. Polypropylene (PC) composition, according to any of the preceding claims, characterized by comprising, more preferably, consisting of: a) 98.0 to 99.99% by weight, relative to the total weight of the polypropylene (PC) composition, of a blend of mixed polypropylene (PP) plastics; and b) 0.01 to 2.0% by weight, relative to the total weight of the polypropylene (PC) composition, of one or more compounds reactive with linear alkyl aldehydes.

14. Article, preferably an injection-molded article, Petition 870250103521, dated 12 / 11 / 2025, page 60 / 238 6 / 7 characterized by comprising the polypropylene (PC) composition as defined in any of the preceding claims in an amount of at least 95% by weight, more preferably at least 98% by weight, most preferably at least 99% by weight.

15. Use of a compound characterized by having a structure according to formula (I): wherein R1, R2 and R3 are each independently selected from the group consisting of a hydrogen atom, a linear or branched C1-C10 alkyl group, a hydroxyl group, an aryl group, a halogen atom, an acetyl group or a cyano group, to reduce the acetaldehyde content and / or the hexanal content of a polypropylene composition derived at least partially from post-consumer waste, without simultaneously increasing the acetone content by more than 30% and without simultaneously increasing the tert-butanol content by more than 10%.

16. Use of a compound characterized by having a structure according to formula (II): wherein RA represents from zero to four substitutions, each substitution being independently selected from the group consisting of a linear or branched C1-C10 alkyl group, a linear or branched C1-C10 alkoxy group, an aryl group or a halogen atom, wherein each of RB and RC is selected from the group consisting of hydrogen and a linear or branched C1-C10 alkyl group Petition 870250103521, 12 / 11 / 2025, p. 61 / 238 7 / 7 to reduce the acetaldehyde content and / or the hexanal content of a polypropylene composition derived, at least partially, from post-consumer waste, without simultaneously increasing the acetone content by more than 30% and without simultaneously increasing the tert-butanol content by more than 10%. Petition 870250103521, dated 12 / 11 / 2025, p. 62 / 238