Ceramic substrate, preparation method thereof, ceramic heating element, and electronic atomization device
A ceramic substrate composition with balanced silicon carbide, aluminum oxide, silicon dioxide, and glass powder, along with optional additives, addresses the strength-porosity trade-off in electronic atomization devices, maintaining e-liquid supply and thermal conductivity.
Patent Information
- Application Number
- CA3205713
- Authority / Receiving Office
- CA · CA
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-27
- Filing Date
- 2021-12-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2041-12-28
AI Technical Summary
The existing ceramic substrates used in electronic atomization devices face a trade-off between improving compressive strength and maintaining porosity and e-liquid guiding rate, as increasing sintering temperature to enhance strength often reduces porosity and affects e-liquid supply.
A ceramic substrate composition comprising specific weight percentages of silicon carbide, aluminum oxide, silicon dioxide, and glass powder, along with optional additives like calcium, sodium, potassium, boron, and zinc oxides, is formulated and processed through grinding, drying, granulating, and sintering to achieve balanced strength, porosity, and e-liquid guiding rate.
The solution maintains or enhances compressive strength while preserving porosity and e-liquid guiding rate, ensuring effective e-liquid supply and thermal conductivity within the ceramic heating body.
Abstract
Description
CERAMIC SUBSTRATE, PREPARATION METHOD THEREOF, CERAMIC HEATING ELEMENT, AND ELECTRONIC ATOMIZATION DEVICE
[0001] TECHNICAL FIELD
[0002] The present disclosure relates to the technical field of ceramic production, and in particular to a ceramic substrate and a preparation method thereof, a ceramic heating body, and an electronic atomization device. BACKGROUND
[0003] An electronic atomization device has an appearance and taste similar to those of a conventional cigarette, but usually does not include tar, suspended particulates, and other harmful ingredients in the cigarette. Therefore, the electronic atomization device is commonly used as a substitute for the cigarette.
[0004] The electronic atomization device generally includes a heating body, and currently, a ceramic heating body is widely used. The ceramic heating body includes a ceramic substrate. A sintering temperature is generally increased to improve compressive strength of the ceramic substrate. However, increasing the sintering temperature may reduce a porosity of a material, and the material may become brittle and deteriorate. In addition, the reduced porosity of the material may affect an e-liquid guiding rate, causing insufficient e-liquid supply. SUMMARY According to an aspect of the invention, there is provided a ceramic substrate, based on 2025-02-25 a mass percentage of each component, comprising the following components: 10 to 70 wt% of silicon carbide; 6 to 60 wt% of aluminum oxide; Date reçue / Received date 5 to 45 wt% of silicon dioxide; a glass powder comprising: 0.8 to 2.3 wt% of calcium oxide, 0.1 to 0.4 wt% of sodium oxide, 0.1 to 0.2 wt% of potassium oxide, 0.1 to 0.2 wt% of boron oxide, 0.1 to 0.4 wt% of barium oxide, and 0.2 to 0.5 wt% of zinc oxide. According to another aspect of the invention, there is provided a method for preparing the ceramic substrate as described above, comprising: sequentially grinding, drying, granulating, and molding mixed components to form a ceramic green body, and sintering the ceramic green body. According to another aspect of the invention, there is provided a ceramic heating body, wherein the ceramic heating body is configured to heat and atomize an aerosol-forming substance when powered on, and the ceramic heating body comprises: the ceramic substrate as described above; and a heating body, arranged on the ceramic substrate and configured to generate heat when powered on, wherein the ceramic substrate conducts heat generated by the heating body. According to another aspect of the invention, there is provided an electronic atomization device, comprising: the ceramic heating body as described above, and configured to heat and atomize an aerosol-forming substance when powered on; and a power supply component, wherein the ceramic heating body is connected to the power supply component, and the power supply component is configured to supply power to the ceramic heating body. According to another aspect of the invention, there is provided an electronic atomization device, comprising: a ceramic heating body wherein the ceramic heating body is configured to heat and atomize an aerosol-forming substance when powered on and the ceramic heating body comprises: the ceramic substrate according to as described above; and a heating body, arranged on the ceramic substrate and configured to generate heat when powered on, wherein the ceramic substrate conducts heat generated by the heating body; and a power supply component, wherein the ceramic heating body is connected to the power supply component, and the power supply component is configured to supply power to the ceramic heating body.
[0005] A technical problem to be resolved in the present disclosure is to overcome a defect in the related art that compressive strength of a ceramic substrate is improved while a porosity and an e-liquid guiding rate are reduced. In view of this, a ceramic substrate and a preparation method thereof, a ceramic heating body, and an electronic atomization device are provided. The ceramic . . . . substrate can improve the compressive strength of the ceramic substrate without reducing the porosity and the e-liquid guiding rate.
[0006] In order to resolve the foregoing technical problem, the present disclosure adopts the following technical solutions.
[0007] A ceramic substrate, based on a mass percentage of each component, includes the following raw materials: (a) 10 to 70 wt% of silicon carbide; (b) 6 to 60 wt% of aluminum oxide; (c) 5 to 45 wt% of silicon dioxide; and (d) 0 to 15 wt%, excluding 0, of glass powder.
[0008] That the porosity and the e-liquid guiding rate are not reduced means that the porosity and the e-liquid guiding rate at least remain unchanged, and optionally, the porosity and the e-liquid guiding rate are increased. An objective of the present disclosure is to make the porosity and e- liquid guiding rate not reduced, and improve the compressive strength of the ceramic substrate.
[0009] The foregoing content of each component is a mass percentage of each component, that is, a percentage of each component to a total mass of all components, where a sum of mass percentages of components is 100%. The raw materials of the ceramic substrate include silicon carbide, aluminum oxide, silicon dioxide, glass powder, and other components that can be optionally added. The other components may bring additional properties to the ceramic substrate.
[0010] In some embodiments, the content of the silicon carbide is, for example, 10 wt%, 12 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, or 70 wt%. When the content of the silicon carbide is excessively high, a sintering temperature may be excessively high, thermal conductivity of the ceramic substrate may be increased, and thermal efficiency of the ceramic heating body is reduced. When the content of the silicon carbide is excessively low, the compressive strength of the ceramic substrate may be reduced. Considering the compressive strength and thermal conductivity of the ceramic substrate, the content of the silicon carbide may optionally range from 20 wt% to 50 wt%.
[0011] In some embodiments, the content of the aluminum oxide is, for example, 6 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, or 60 wt%. When the content of the aluminum oxide is excessively high, a sintering temperature may be increased, increasing the thermal conductivity of the ceramic substrate and reducing the thermal efficiency of the ceramic heating body. When the content of the aluminum oxide is excessively low, the compressive strength of the ceramic substrate may be reduced. Considering the compressive strength and thermal conductivity of the ceramic substrate, the content of the aluminum oxide may optionally range from 10 wt% to 30 wt%.
[0012] In some embodiments, the content of the silicon dioxide is, for example, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, or 40 wt%. When the content of the silicon dioxide is excessively high, the e-liquid guiding rate of the ceramic substrate may be reduced. When the content of the silicon dioxide is excessively low, the compressive strength of the ceramic substrate may be affected. Considering the compressive strength and e-liquid guiding rate of the ceramic substrate, the content of the silicon dioxide may optionally range from 15 wt% to 25 wt%.
[0013] In some embodiments, the content of the glass powder is, for example, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, or 15 wt%. When the content of the glass powder is excessively high, the e-liquid guiding rate and porosity of the ceramic substrate may be reduced. When the content of the glass powder is excessively low, the compressive strength of the ceramic substrate may be affected. Considering the compressive strength, porosity, and e-liquid guiding rate of the ceramic substrate, the content of the glass powder may optionally range from 5 wt% to 12 wt%.
[0014] In an optional implementation of the present disclosure, the porosity of the ceramic substrate falls in the range from 50% to 60%, and the compressive strength of the ceramic substrate falls in the range from 15 MPa to 45 MPa.
[0015] It should be noted that, in the present disclosure, for a method for testing the porosity, it may refer to the ceramic open porosity and capacity test method in the GB / T1966-1996 of China, and for a method for testing the compressive strength, it may refer to the ceramic compressive strength test method in the GB / T1964-1996, where a size of a test sample is 9 mm <com:Math><semantics>×<annotation encoding="application / x-tex">\times< / annotation>< / semantics>< / com:Math> 3.2 mm <com:Math><semantics>×<annotation encoding="application / x-tex">\times< / annotation>< / semantics>< / com:Math> 2 mm, and a test contact area is <com:Math><semantics>3.2 mm×2 mm<annotation encoding="application / x-tex">3.2 \text{ mm} \times 2 \text{ mm}< / annotation>< / semantics>< / com:Math>.
[0016] In an optional implementation of the present disclosure, the thermal conductivity of the ceramic substrate falls in the range from 0.8 w / mk to 2.4 w / mk.
[0017] It should be noted that, in the present disclosure, a method for testing the thermal conductivity is a Hot Disk transient plane source method.
[0018] In an optional implementation of the present disclosure, the glass powder includes at least one of silicon dioxide, aluminum oxide, calcium oxide, sodium oxide, potassium oxide, barium oxide, boron oxide, or zinc oxide, and optionally includes silicon dioxide, aluminum oxide, calcium oxide, sodium oxide, potassium oxide, barium oxide, boron oxide, and zinc oxide.
[0019] The present disclosure further provides a ceramic substrate, based on a mass percentage of each component, including the following components: 10 to 70 wt% of silicon carbide, 6 to 65 wt% of aluminum oxide, 15 to 50 wt% of silicon dioxide, 0.8 to 2.3 wt% of calcium oxide, 0.1 to 0.4 wt% of sodium oxide, 0.1 to 0.2 wt% of potassium oxide, 0.1 to 0.2 wt% of boron oxide, 0.1 to 0.4 wt% of barium oxide, and 0.2 to 0.5 wt% of zinc oxide.
[0020] The foregoing content of each component is a mass percentage of each component, that is, a percentage of each component to a total mass of all components, where a sum of mass percentages of components is 100%.
[0021] The present disclosure further provides a method for preparing the ceramic substrate, including: sequentially grinding, drying, granulating, and molding mixed components to form a ceramic green body, and sintering the ceramic green body.
[0022] In an optional implementation of the present disclosure, the grinding includes: grinding the mixed components in the presence of water and a grinding medium, and the grinding includes at least one of the following process parameters: a temperature in the range from 20°C to 30°C, a grinding time in the range from 5 min to 30°C. min, and a grinded material to grinding media ratio in the range from 1:1 to 1:2.5.
[0023] The temperature for the grinding is, for example, <com:Math><semantics>21∘<annotation encoding="application / x-tex">21^{\circ}< / annotation>< / semantics>< / com:Math>C, <com:Math><semantics>22∘<annotation encoding="application / x-tex">22^{\circ}< / annotation>< / semantics>< / com:Math>C, <com:Math><semantics>23∘<annotation encoding="application / x-tex">23^{\circ}< / annotation>< / semantics>< / com:Math>C, <com:Math><semantics>24∘<annotation encoding="application / x-tex">24^{\circ}< / annotation>< / semantics>< / com:Math>C, <com:Math><semantics>25∘<annotation encoding="application / x-tex">25^{\circ}< / annotation>< / semantics>< / com:Math>C, <com:Math><semantics>26∘<annotation encoding="application / x-tex">26^{\circ}< / annotation>< / semantics>< / com:Math>C, <com:Math><semantics>27∘<annotation encoding="application / x-tex">27^{\circ}< / annotation>< / semantics>< / com:Math>C, 28°C, 29°C, or 30°C. The grinding time is, for example, 6 min, 10 min, 15 min, 20 min, 25 min, or 30 min.
[0024] A typical but non-restrictive grinding medium includes any one of an aluminum oxide grinding ball, a zirconia grinding ball, or an agate grinding ball.
[0025] In some embodiments, the grinding may be performed in a grinder. The grinded material to grinding media ratio refers to a ratio of a mass of a material to a mass of a grinding medium in the grinder, for example 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2, 1:2.2, 1:2.4, or 1:2.5.
[0026] In an optional implementation of the present disclosure, a drying temperature falls in the range from 60 to 90°C and a drying time falls in the range from 4h to 8h.
[0027] In an optional implementation of the present disclosure, a molding pressure falls in the range from 10 MPa to 40 MPa, for example, 10 MPa, 15 MPa, 20 MPa, 25 MPa, 30 MPa, 35 MPa, or 40 MPa, and a molding time falls in the range from 5s to 20s, for example, 5s, 8s, 11s, 14s, 17s, or 20s.
[0028] The molding may be performed through an automatic dry-pressing molding machine.
[0029] In an optional implementation of the present disclosure, a sintering temperature falls in the range from 1100°C to 1700°C, for example, 1150°C, 1200°C, 1250°C, 1300°C, 1350°C, 1400°C, 1450°C, 1500°C, 1550°C, 1600°C, or 1650°C. When the sintering temperature is lower than 1100°C, the ceramic substrate fails to meet a requirement for use due to insufficient sintering and low compressive strength. When the sintering temperature is higher than 1700°C, the ceramic substrate may have a problem of burning bubbles, greatly reducing the e-liquid guiding rate and porosity. A sintering time falls in the range from 2h to 8h, for example, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, or 7.5h. Optionally, the sintering temperature falls in the range from 1300°C to 1500°C, and the sintering time falls in the range from 2h to 4h.
[0030] In an optional implementation of the present disclosure, the method for preparing the heating body includes: grinding mixed components by adding water and a grinding medium, where the grinding medium is an aluminum oxide grinding ball, the temperature for the grinding falls in the range from 20°C to 30°C, the grinding time falls in the range from 5 min to 30 min, and the grinded material to grinding media ratio falls in the range from 1:1 to 1:2.5; drying the ground powder, where the drying temperature falls in the range from 60 to 90<com:Math><semantics>∘<annotation encoding="application / x-tex">^{\circ}< / annotation>< / semantics>< / com:Math>C. and the drying time falls in the range from 4h to 8h; granulating the dried powder; molding the granulated powder to form a ceramic green body, where the molding pressure falls in the range from 10 MPa to 40 MPa, and the molding time falls in the range from 5s to 20s; and sintering the ceramic green body, where the sintering temperature falls in the range from 1100°C to 1700°C, and the sintering time falls in the range from 2h to 8h.
[0031] The present disclosure further provides a ceramic heating body. The ceramic heating body is configured to heat and atomize an aerosol-forming substance when powered on. The ceramic heating body includes a ceramic substrate as described above and a heating body that is arranged on the ceramic substrate and is configured to generate heat when powered on. The ceramic substrate conducts heat generated by the heating body.
[0032] In an optional implementation of the present disclosure, the ceramic substrate includes a liquid absorbing surface and a atomization surface opposite to each other. The heating body is arranged on the atomization surface. The liquid absorbing surface is configured to absorb an aerosol-forming substance, the atomization surface is configured to atomize the aerosol-forming substance on the ceramic substrate, and the heating body is arranged on the atomization surface on the side of the ceramic substrate. The aerosol-forming substance is, for example, e-liquid. The ceramic substrate absorbs the e-liquid, and absorbs the e-liquid into the heating body through a capillary force, to atomize into aerosols.
[0033] The present disclosure further provides an electronic atomization device, including: a ceramic heating body as described above, configured to heat and atomize an aerosol-forming substance when powered on, and a power supply component, where the ceramic heating body is connected to the power supply component, and the power supply component is configured to supply power to the ceramic heating body.
[0034] The technical solution of the present disclosure includes the following advantages. In the present disclosure, the silicon carbide has advantages of high thermal conductivity, a low shrinkage rate, and high-temperature stability. However, a sintering temperature of the silicon carbide is relatively high. The aluminum oxide may assist in sintering and reduce the sintering temperature. Thermal conductivity may be controlled through coordination between the silicon carbide, the aluminum oxide, and the silicon dioxide of certain content. In addition, the silicon carbide, the aluminum oxide, and the silicon dioxide may form a skeleton of silicon carbide- corundum-mullite ternary phase at a high temperature, bringing high strength to the material. The glass powder is used as an adhesive that liquefies during the sintering and bonds components together after cooling, to improve anti-bending strength of the heating body. The glass powder is melted into a liquid phrase at a high temperature, to promote migration and sintering of aggregate grains. The aggregate grains are bonded together through the liquid phrase, thereby improving a bonding force between the grains and increasing the strength of the material. In addition, since the glass powder is formed into the liquid phrase at a high temperature and is wrapped the aggregate grains around, a pore originally filled by glass powder grains may enlarge with flowing of glass liquid, thereby improving overall e-liquid guide performance of the material.
[0035] In addition to the silicon dioxide and the aluminum oxide, the glass powder in the present disclosure further includes calcium oxide, sodium oxide, potassium oxide, barium oxide, boron oxide, and zinc oxide. A function of the foregoing components is to control a melting point of the glass powder, promote sintering of grains, and improve bonding strength of a glass phrase and bonding strength between the glass phrase and the aggregate grains, thereby bringing higher strength to the material. DETAILED DESCRIPTION
[0036] Embodiment 1
[0037] A ceramic substrate includes, based on a mass percentage of each component, the following raw materials: (a) 18% of silicon carbide; (b) 42% of aluminum oxide; (c) 25% of silicon dioxide; and (d) 15% of glass powder.
[0038] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 25°C, a grinding time is 10 min, and a grinded material to grinding media ratio is 1:2; drying the ground powder, where a drying temperature is 80°C, and a drying time is 5h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 15 MPa, and a molding time is 10s; and sintering the ceramic green body, where a sintering temperature is 1250°C, and a sintering time is 2.5h.
[0039] The ceramic substrate obtained by the method according to the first embodiment, based on a mass percentage of each component, includes the following components: 18 wt% of silicon carbide, 43.2 wt% of aluminum oxide, 34.9 wt% of silicon dioxide, 2.3 wt% of calcium oxide, 0.4 wt% of sodium oxide, 0.1 wt% of potassium oxide, 0.2 wt% of boron oxide, 0.4 wt% of barium oxide, and 0.5 wt% of zinc oxide.
[0040] Embodiment 2
[0041] A ceramic substrate includes, based on a mass percentage of each component, the following raw materials: (a) 28% of silicon carbide; (b) 32% of aluminum oxide; (c) 35% of silicon dioxide; and (d) 5% of glass powder.
[0042] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 24°C, a grinding time is 15min, and a grinded material to grinding media ratio is 1:1.2; drying the ground powder, where a drying temperature is 70°C, and a drying time is 6h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 16 MPa, and a molding time is 15s; and sintering the ceramic green body, where a sintering temperature is 1450°C, and a sintering time is 3h.
[0043] The ceramic substrate obtained by the method according to the second embodiment, based on a mass percentage of each component, includes the following components: 28 wt% of silicon carbide, 32.3 wt% of aluminum oxide, 38.2 wt% of silicon dioxide, 0.8 wt% of calcium oxide, 0.1 wt% of sodium oxide, 0.2 wt% of potassium oxide, 0.1 wt% of boron oxide, 0.1 wt% of barium oxide, and 0.2 wt% of zinc oxide.
[0044] Embodiment 3
[0045] A ceramic substrate includes, based on a mass percentage of each component, the following raw materials: (a) 64% of silicon carbide; (b) 16% of aluminum oxide; (c) 15% of silicon dioxide; and (d) 5% of glass powder.
[0046] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 16°C, a grinding time is 10 min, and a grinded material to grinding media ratio is 1:1.5; drying the ground powder, where a drying temperature is 75°C, and a drying time is 5h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 15 MPa, and a molding time is 12s; and sintering the ceramic green body, where a sintering temperature is 1500°C, and a sintering time is 3h.
[0047] The ceramic substrate obtained by the method according to the third embodiment, based on a mass percentage of each component, includes the following components: 64 wt% of silicon carbide, 16.3 wt% of aluminum oxide, 18.2 wt% of silicon dioxide, 0.8 wt% of calcium oxide, 0.1 wt% of sodium oxide, 0.2 wt% of potassium oxide, 0.1 wt% of barium oxide, 0.1 wt% of boron oxide, and 0.2 wt% of zinc oxide.
[0048] Embodiment 4
[0049] A ceramic substrate includes, based on a mass percentage of each component, the following raw materials: (a) 50% of silicon carbide; (b) 6% of aluminum oxide; (c) 34% of silicon dioxide; and (d) 10% of glass powder.
[0050] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 25°C, a grinding time is 10 min, and a grinded material to grinding media ratio is 1:2; drying the ground powder, where a drying temperature is 80°C, and a drying time is 5h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 19 MPa, and a molding time is 10s; and sintering the ceramic green body, where a sintering temperature is 1400°C, and a sintering time is 2h.
[0051] The ceramic substrate obtained by the method according to the fourth embodiment, based on a mass percentage of each component, includes the following components: 50 wt% of silicon carbide, 6.7 wt% of aluminum oxide, 40.7 wt% of silicon dioxide, 1.5 wt% of calcium oxide, 0.3 wt% of sodium oxide, 0.1 wt% of potassium oxide, 0.1 wt% of boron oxide, 0.3 wt% of barium oxide, and 0.3 wt% of zinc oxide.
[0052] Embodiment 5
[0053] A ceramic substrate includes, based on a mass percentage of each component, the following raw materials: (a) 50% of silicon carbide; (b) 21% of aluminum oxide; (c) 17% of silicon dioxide; and (d) 12% of glass powder.
[0054] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 25°C, a grinding time is 15min, and a grinded material to grinding media ratio is 1:2; drying the ground powder, where a drying temperature is 80°C, and a drying time is 4h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 13 MPa, and a molding time is 10s; and sintering the ceramic green body, where a sintering temperature is 1320°C, and a sintering time is 4h.
[0055] The ceramic substrate obtained by the method according to the fifth embodiment, based on a mass percentage of each component, includes the following components: 50 wt% of silicon carbide, 21.8 wt% of aluminum oxide, 25.0 wt% of silicon dioxide, 1.8 wt% of calcium oxide, 0.4 wt% of sodium oxide, 0.1 wt% of potassium oxide, 0.1 wt% of barium oxide, 0.4 wt% of boron oxide, and 0.4 wt% of zinc oxide.
[0056] Embodiment 6
[0057] A ceramic substrate includes, based on a mass percentage of each component, the following raw materials: (a) 20% of silicon carbide; (b) 50% of aluminum oxide; (c) 20% of silicon dioxide; and (d) 10% of glass powder.
[0058] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 25°C, a grinding time is 15min, and a grinded material to grinding media ratio is 1:2; drying the ground powder, where a drying temperature is 85°C, and a drying time is 6h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 14 MPa, and a molding time is 15s; and sintering the ceramic green body, where a sintering temperature is 1375°C, and a sintering time is 2.5h.
[0059] The ceramic substrate obtained by the method according to the sixth embodiment, based on a mass percentage of each component, includes the following components: 20 wt% of silicon carbide, 50.7 wt% of aluminum oxide, 26.7 wt% of silicon dioxide, 1.5 wt% of calcium oxide, 0.3 wt% of sodium oxide, 0.1 wt% of potassium oxide, 0.1 wt% of barium oxide, 0.3 wt% of boron oxide, and 0.3 wt% of zinc oxide.
[0060] Embodiment 7
[0061] A ceramic substrate includes, based on a mass percentage of each component, the following raw materials: (a) 55% of silicon carbide; (b) 20% of aluminum oxide; (c) 10% of silicon dioxide; and (d) 15% of glass powder.
[0062] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 26°C, a grinding time is 20 min, and a grinded material to grinding media ratio is 1:2.5; drying the ground powder, where a drying temperature is 65°C, and a drying time is 8h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 20 MPa, and a molding time is 15s; and sintering the ceramic green body, where a sintering temperature is 1350°C, and a sintering time is 4h.
[0063] The ceramic substrate obtained by the method according to the seventh embodiment, based on a mass percentage of each component, includes the following components: 55 wt% of silicon carbide, 21.1 wt% of aluminum oxide, 20.0 wt% of silicon dioxide, 2.3 wt% of calcium oxide, 0.4 wt% of sodium oxide, 0.1 wt% of potassium oxide, 0.2 wt% of barium oxide, 0.4 wt% of boron oxide, and 0.5 wt% of zinc oxide.
[0064] Embodiment 8
[0065] A ceramic substrate includes, based on a mass percentage of each component, the following raw materials: (a) 55% of silicon carbide; (b) 19% of aluminum oxide; (c) 15% of silicon dioxide; and (d) 11% of glass powder.
[0066] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 25°C, a grinding time is 25 min, and a grinded material to grinding media ratio is 1:2; drying the ground powder, where a drying temperature is 80°C, and a drying time is 5h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 15 MPa, and a molding time is 15s; and sintering the ceramic green body, where a sintering temperature is 1500°C, and a sintering time is 2.5h.
[0067] The ceramic substrate obtained by the method according to the eighth embodiment, based on a mass percentage of each component, includes the following components: 55 wt% of silicon carbide, 20.0 wt% of aluminum oxide, 22.1 wt% of silicon dioxide, 1.7 wt% of calcium oxide, 0.3 wt% of sodium oxide, 0.1 wt% of potassium oxide, 0.1 wt% of barium oxide, 0.3 wt% of boron oxide, and 0.4 wt% of zinc oxide.
[0068] Embodiment 9
[0069] A ceramic substrate includes, based on a mass percentage of each component, the following raw materials: (a) 30% of silicon carbide; (b) 16% of aluminum oxide; (c) 44% of silicon dioxide; and (d) 10% of glass powder.
[0070] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 25°C, a grinding time is 10 min, and a grinded material to grinding media ratio is 1:2; drying the ground powder, where a drying temperature is 85°C, and a drying time is 4h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 25 MPa, and a molding time is 10s; and sintering the ceramic green body, where a sintering temperature is 1450°C, and a sintering time is 5h.
[0071] The ceramic substrate obtained by the method according to the ninth embodiment, based on a mass percentage of each component, includes the following components: 30 wt% of silicon carbide, 17.2 wt% of aluminum oxide, 49.1 wt% of silicon dioxide, 2.2 wt% of calcium oxide, 0.4 wt% of sodium oxide, 0.1 wt% of potassium oxide, 0.1 wt% of boron oxide, 0.4 wt% of barium oxide, and 0.5 wt% of zinc oxide.
[0072] Embodiment 10
[0073] A ceramic substrate includes, based on a mass percentage of each component, the following raw materials: (a) 10% of silicon carbide; (b) 60% of aluminum oxide; (c) 15% of silicon dioxide; and (d) 15% of glass powder.
[0074] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 25°C, a grinding time is 25 min, and a grinded material to grinding media ratio is 1:1; drying the ground powder, where a drying temperature is 90°C, and a drying time is 4h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 25 MPa, and a molding time is 15s; and sintering the ceramic green body, where a sintering temperature is 1200°C, and the sintering time is 6h.
[0075] The ceramic substrate obtained by the method according to the tenth embodiment, based on a mass percentage of each component, includes the following components: 10 wt% of silicon carbide, 61.0 wt% of aluminum oxide, 25.1 wt% of silicon dioxide, 2.3 wt% of calcium oxide, 0.4 wt% of sodium oxide, 0.1 wt% of potassium oxide, 0.2 wt% of boron oxide, 0.4 wt% of barium oxide, and 0.5 wt% of zinc oxide.
[0076] Embodiment 11
[0077] A ceramic substrate includes, based on a mass percentage of each component, the following raw materials: (a) 70% of silicon carbide; (b) 10% of aluminum oxide; (c) 5% of silicon dioxide; and (d) 15% of glass powder.
[0078] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 25°C, a grinding time is 25 min, and a grinded material to grinding media ratio is 1:2; drying the ground powder, where a drying temperature is 80°C, and a drying time is 7h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 30 MPa, and a molding time is 10s; and sintering the ceramic green body, where a sintering temperature is 1200°C, and the sintering time is 3h.
[0079] The ceramic substrate obtained by the method according to the eleventh embodiment, based on a mass percentage of each component, includes the following components: 70 wt% of silicon carbide, 11.1 wt% of aluminum oxide, 15.0 wt% of silicon dioxide, 2.3 wt% of calcium oxide, 0.4 wt% of sodium oxide, 0.1 wt% of potassium oxide, 0.2 wt% of barium oxide, 0.4 wt% of boron oxide, and 0.5 wt% of zinc oxide.
[0080] Comparative example 1
[0081] A ceramic substrate includes, based on a mass percentage of each component, the following raw materials: (a) 75% of silicon carbide; (b) 1% of aluminum oxide; (c) 4% of silicon dioxide; and (d) 20% of glass powder.
[0082] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 25°C, a grinding time is 10 min, and a grinded material to grinding media ratio is 1:2; drying the ground powder, where a drying temperature is 80°C, and a drying time is 5h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 20 MPa, and a molding time is 10s; and sintering the ceramic green body, where a sintering temperature is 1250°C, and the sintering time is 3h.
[0083] The ceramic substrate obtained by the method according to the first comparative example, based on a mass percentage of each component, includes the following components: 75 wt% of SiC, 4 wt% of Al<com:Sub>2< / com:Sub>O<com:Sub>3< / com:Sub>, 10 wt% of SiO<com:Sub>2< / com:Sub>, 5 wt% of CaO, 2 wt% of Na<com:Sub>2< / com:Sub>O, 1 wt% of K<com:Sub>2< / com:Sub>O, 1 wt% of B<com:Sub>2< / com:Sub>O<com:Sub>3< / com:Sub>, 1 wt% of BaO, and 1 wt% of ZnO.
[0084] Comparative example 2
[0085] A ceramic substrate, based on a mass percentage of each component, includes the following raw materials: 55 wt% of silicon carbide, 25 wt% of aluminum oxide, and 20 wt% of silicon dioxide.
[0086] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 25°C, a grinding time is 15min, and a grinded material to grinding media ratio is 1:1.4; drying the ground powder, where a drying temperature is 80°C, and a drying time is 4h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 15 MPa, and a molding time is 15s; and sintering the ceramic green body, where a sintering temperature is 1600°C, and the sintering time is 6h. The obtained ceramic substrate, based on a mass percentage of each component, includes the following components: 55 wt% of silicon carbide, 25 wt% of aluminum oxide, and 20 wt% of silicon dioxide.
[0087] Comparative example 3
[0088] Comparative example 3 is a cCELL ceramic atomization core, and a manufacturer is Dongguan Mike New Material Technology Co., Ltd.
[0089] Comparative example 4
[0090] Comparative example 4 is an FFELM ceramic atomization core, and a manufacturer is Dongguan Mike New Material Technology Co., Ltd.
[0091] Comparative example 5
[0092] A ceramic substrate, based on a mass percentage of each component, includes the following raw materials: (a) 10% of silicon carbide; (b) 40% of aluminum oxide; (c) 50% of silicon dioxide; (d) 0% of glass powder (in other words, no glass powder is used as a raw material).
[0093] A method for preparing the ceramic substrate includes: mixing components, adding water and a grinding medium to grind the mixed components, where the grinding medium is an aluminum oxide grinding ball, a temperature for the grinding is 25°C, a grinding time is 10 min, and a grinded material to grinding media ratio is 1:2; drying the ground powder, where a drying temperature is 60°C, and a drying time is 8h; granulating the dried powder; molding the granulated powder to obtain a ceramic green body, where a molding pressure is 15 MPa, and a molding time is 15s; and sintering the ceramic green body, where a sintering temperature is 1600°C, and the sintering time is 4h.
[0094] The ceramic substrate obtained by the method according to the fifth comparative example, according to a mass percentage of each component, includes the following components: 10 wt% of silicon carbide, 40 wt% of aluminum oxide, and 50 wt% of silicon dioxide.
[0095] The porosity, the e-liquid guiding rate, the strength, and the thermal conductivity of the ceramic substrate according to Embodiments 1-11 and the ceramic substrate according to Comparative example 1-5 are tested, and a specific test method includes:
[0096] A method for testing the porosity is referred to the GB / T1966-1996 ceramic open porosity and capacity test method.
[0097] A method for testing the compressive strength is referred to the GB / T1964-1996 ceramic compressive strength test method, where a size of a test sample is 9 mm <com:Math><semantics>×<annotation encoding="application / x-tex">\times< / annotation>< / semantics>< / com:Math> 3.2 mm <com:Math><semantics>×<annotation encoding="application / x-tex">\times< / annotation>< / semantics>< / com:Math> 2 mm, and a test contact area is <com:Math><semantics>3.2 mm×2 mm<annotation encoding="application / x-tex">3.2 \text{ mm} \times 2 \text{ mm}< / annotation>< / semantics>< / com:Math>.
[0098] In a method for testing the e-liquid guiding rate, a porous ceramic is cut into a neat sample block with a size of 1 cm <com:Math><semantics>×<annotation encoding="application / x-tex">\times< / annotation>< / semantics>< / com:Math> 1 cm <com:Math><semantics>×<annotation encoding="application / x-tex">\times< / annotation>< / semantics>< / com:Math> 1 cm, a 10 ml precision injection sampler is used to drop 20- microlitre standard smoke e-liquid (the standard smoke is 50 mg of tobacco smoke e-liquid) on a surface of the sample block placed in a horizontal direction, a time required for the liquid to dip into the sample block is observed under an electron microscope, and the e-liquid guiding rate is obtained by calculating a ratio of the standard liquid volume of the e-liquid to the time required for the liquid to dip into the sample block.
[0099] A method for testing the thermal conductivity is a Hot Disk transient plane source method.
[00100] Performance evaluation of Embodiments 1-11, Comparative examples 1-2, and Comparative example 5 are shown in Table 2: [Image disponible dans le document PDF, Image available in the PDF document]
[00101] Three cCELL ceramic atomization cores manufactured by Dongguan Mike New Material Technology Co., Ltd. in Comparative example 3 are tested, the three samples have the same components, and performance evaluation of the three samples are shown in Table 3. Table 3 [Image disponible dans le document PDF, Image available in the PDF document]
[00102] Three FFELM ceramic atomization cores manufactured by Dongguan Mike New Material Technology Co., Ltd. in Comparative example 4 are tested, the three samples have the same components, and performance evaluation of the three samples are shown in Table 4. Table 4 [Image disponible dans le document PDF, Image available in the PDF document]
[00103] By comparing Embodiments 1-11 with Comparative examples 3-4, it can be learned that the porosity in Embodiments 1-11 is the same or close to the porosity in Comparative example 3 and Comparative example 4. However, the strength of the ceramic substrate in Embodiments 1-11 is apparently higher than the strength in Comparative examples 3-4.
[00104] Apparently, the foregoing embodiments are merely examples for a clear description, and are not intended to limit the implementations. A person of ordinary skill in the art may further make different other changes or variations of various forms based on the foregoing descriptions. It is neither necessary nor possible to exhaust all the implementations herein. The apparent changes or variations derived from the foregoing descriptions shall still fall within the protection scope of the present disclosure.
Claims
CLAIMS 1. A ceramic substrate, based on a mass percentage of each component, comprising the following components: 10 to 70 wt% of silicon carbide; 6 to 60 wt% of aluminum oxide; 5 to 45 wt% of silicon dioxide; a glass powder comprising 0.8 to 2.3 wt% of calcium oxide, 0.1 to 0.4 wt% of sodium oxide, 0.1 to 0.2 wt% of potassium oxide, 0.1 to 0.2 wt% of boron oxide, 0.1 to 0.4 wt% of barium oxide, and 0.2 to 0.5 wt% of zinc oxide.
2. The ceramic substrate according to claim 1, wherein content of the silicon carbide falls in the range from 20 wt% to 50 wt%.
3. The ceramic substrate according to claim 1, wherein content of the aluminum oxide falls in the range from 10 wt% to 30 wt%.
4. The ceramic substrate according to claim 1, wherein content of the silicon dioxide falls in the range from 15 wt% to 25 wt%.
5. The ceramic substrate according to claim 1, wherein content of the glass powder falls in the range from 5 wt% to 12 wt%.
6. The ceramic substrate according to any one of claims 1 to 5, wherein a porosity of the ceramic substrate falls in the range from 50% to 60%, and compressive strength of the ceramic substrate falls in the range from 15 MPa to 45 MPa.
7. The ceramic substrate according to any one of claims 1 to 5, wherein thermal conductivity of the ceramic substrate falls in the range from 0.8 w / mk to 2.4 w / mk.
8. A method for preparing the ceramic substrate according to any one of claims 1 to 7, comprising: sequentially grinding, drying, granulating, and molding mixed components to form a ceramic green body, and sintering the ceramic green body.
9. The method according to claim 8, wherein the grinding mixed components comprises: grinding the mixed components in the presence of water and a grinding medium, and the grinding comprises at least one of the following process parameters: a temperature for the grinding in the range from 20°C to 30°C, a grinding time in the range from 5 min to 30 min, and a grinded material to grinding media ratio in the range from 1:1 to 1:2.
5.
10. The method according to claim 8, wherein a molding pressure falls in the range from 10 MPa to 40 MPa, and a molding time falls in the range from 5s to 20s.
11. The method according to claim 8, wherein a sintering temperature falls in the range from 1100°C to 1700°C, and a sintering time falls in the range from 2h to 8h.
12. The method according to claim 11, wherein the sintering temperature falls in the range from 1300°C to 1500°C, and the sintering time falls in the range from 2h to 4h.
13. The method according to claim 8, wherein the method for preparing the ceramic substrate comprises: grinding mixed components by adding water and a grinding medium, wherein the grinding medium is an aluminum oxide grinding ball, the grinding temperature falls in the range from 20°C to 30°C, the grinding time falls in the range from 5 min to 30 min, and the grinded material to grinding media ratio falls in the range from 1:1 to 1:2.5; drying the ground powder, wherein the drying temperature falls in the range from 60 to 90°C, and the drying time falls in the range from 4h to 8h; granulating the dried powder; molding the granulated powder to form the ceramic green body, wherein the molding pressure falls in the range from 10 MPa to 40 MPa, and the molding time falls in the range from 5s to 20s; and sintering the ceramic green body, wherein the sintering temperature falls in the range from 1100°C to 1700°C, and the sintering time falls in the range from 2h to 8h.
14. The method according to claim 9, wherein the grinding medium is a zirconia grinding ball, or an agate grinding ball.
15. A ceramic heating body, wherein the ceramic heating body is configured to heat and atomize an aerosol-forming substance when powered on, and the ceramic heating body comprises: the ceramic substrate according to any one of claims 1 to 7; and a heating body, arranged on the ceramic substrate and configured to generate heat when powered on, wherein the ceramic substrate conducts heat generated by the heating body.
16. The ceramic heating body according to claim 15, wherein the ceramic substrate comprises a liquid absorbing surface and an atomization surface opposite to each other, and the heating body is arranged on the atomization surface.
17. An electronic atomization device, comprising: a ceramic heating body wherein the ceramic heating body is configured to heat and atomize an aerosol-forming substance when powered on and the ceramic heating body comprises: the ceramic substrate according to any one of claims 1 to 7; and a heating body, arranged on the ceramic substrate and configured to generate heat when powered on, wherein the ceramic substrate conducts heat generated by the heating body; and a power supply component, wherein the ceramic heating body is connected to the power supply component, and the power supply component is configured to supply power to the ceramic heating body. .
18. The electronic atomization device according to claim 17, wherein the ceramic substrate comprises a liquid absorbing surface and an atomization surface opposite to each other, and the heating body is arranged on the atomization surface. . • •