A technology of deepening agent and emulsifier, applied in the field of deepening agent and its preparation, can solve the problems of easily changing the physical index of the fabric, inconspicuous deepening effect, and difficult to control the deepening rate, etc., and achieves low scrub fastness, Small influence, small effect on washing fastness

CN106084120AActive Publication Date: 2016-11-09苏州联胜化学有限公司
2 Cites 6 Cited by

Patent Information

Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Publication Date
2016-11-09

Smart Images

  • Figure 1
    Figure 1
Patent Text Reader

Abstract

The invention provides a deepening agent for finishing a fabric. The deepening agent comprises the following components in percentage by mass: 12-66% of a monomer, 0.1-3% of a cross-linking agent, 0.05-2% of glacial acetic acid, 0.1-1% of an emulsifier and the balance of deionized water. By adopting the deepening agent, a covering membrane can be formed on the surface of fiber, a part of the deepening agent is embedded into the fiber to form diamond-like crystal, then diffuse reflection of light can be formed on the surface of fiber, and light can have multi-refraction and reflection, so that a deepening effect on a colored fabric can be achieved, and particularly a remarkable effect of deepening a fabric of a deep color can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

technical field

[0001] The invention relates to the field of textile auxiliaries, in particular to a darkening agent and a preparation method thereof. Background technique

[0002] Among the three major synthetic fibers, polyester has the simplest process, the largest output, the most widely used, and the cheapest price; because of its special molecular structure, there is no specific group that can be dyed on the molecular chain, and the polarity is also small. During the dyeing process, dye molecules are not easy to enter the fiber, so its dyeability is poor, which leads to poor dyeing depth of polyester.

[0003] Facing the dyeing problem of polyester, in the actual production process of the dyeing factory, a larger amount of disperse dyes will be added to increase the color depth; however, different customers have different requirements for the depth of fabrics. For example, in the black fabric market, "Arabian black "It is very representative of black style fabrics. T...

Examples

Embodiment 1

[0026] In this embodiment, a darkening agent is provided. The specific preparation is as follows:

[0027] Step S10. Pre-emulsification: Weigh 109g butyl acrylate, 30g methyl methacrylate, 3.5g hydroxyethyl methacrylate, 2.2g methacryloyloxyethyltrimethylammonium chloride, 0.6g cationic emulsifier 1831, 1.2g of non-ionic emulsifier EFS-630, 0.23g of ammonium persulfate, 1g of glacial acetic acid and 135g of deionized water were added to the reaction flask, and the stirring speed of the mixer was controlled at about 2000rpm at room temperature, and stirred for 30 minutes to prepare a milky white pre-emulsion.

[0028] Step S20. Preparation of seed emulsion: first weigh 40 g of the pre-emulsion obtained in step S10, then weigh 0.6 g of cationic emulsifier 1831, 1.2 g of nonionic emulsifier EFS-630, 0.23 g of ammonium persulfate and 210 g of deionized water Add them together into a reaction four-neck flask, then connect a thermometer, a condenser tube, and a nitrogen tube, and ...

Embodiment 2

[0031] In this embodiment, a darkening agent is provided. The specific preparation is as follows:

[0032] Step S10. Pre-emulsification: Weigh 80.5g butyl acrylate, 23.2g isooctyl acrylate, 35.8g methyl methacrylate, 3.5g hydroxyethyl methacrylate, 2.2g methacryloyloxyethyl trimethyl Add ammonium chloride, 0.6g cationic emulsifier 1831, 1.2g nonionic emulsifier EFS-630, 0.23g ammonium persulfate, 1g glacial acetic acid and 135g deionized water into the reaction flask, and control the stirring speed of the mixer at about 2000rpm at room temperature , and stirred for 30 minutes to prepare a milky white pre-emulsion.

[0033]Step S20. Preparation of seed emulsion: first weigh 40 g of the pre-emulsion obtained in step S10, then weigh 0.6 g of cationic emulsifier 1831, 1.2 g of nonionic emulsifier EFS-630, 0.23 g of ammonium persulfate and 210 g of deionized water Add them together into a reaction four-neck flask, then connect a thermometer, a condenser tube, and a nitrogen tube,...

Embodiment 3

[0036] In this embodiment, a darkening agent is provided. The specific preparation is as follows:

[0037] Step S10. Pre-emulsification: Weigh 80.5g butyl acrylate, 23.2g isooctyl acrylate, 35.8g methyl methacrylate, 3.7g 1,6-hexanediol diacrylate, 2.2g methacryloyloxyethyl Trimethylammonium chloride, 0.5g cationic emulsifier tallow trimethylammonium chloride, 1.0g nonionic emulsifier EFS-630, 0.23g ammonium persulfate, 1g glacial acetic acid and 138g deionized water were added to the reaction flask In the process, control the stirring speed of the stirrer at about 2000rpm at normal temperature, and stir for 30 minutes to prepare a milky white pre-emulsion.

[0038] Step S20. Preparation of seed emulsion: first weigh 40 g of the pre-emulsion obtained in step S10, then weigh 0.5 g of cationic emulsifier tallow trimethylammonium chloride, 1.0 g of nonionic emulsifier EFS-630, 0.23 g of Ammonium sulfate and 210 g of deionized water were added into the reaction four-necked flask...