Ceramic blank injection molding product and sintering method thereof, ceramic blank injection molding mold

By setting up a support column cavity on the mold and performing low-temperature injection molding, the problem of collapse during the sintering process of ceramic blank injection molding products is solved, precise molding and efficient production are achieved, cost reduction and manufacturing accuracy are improved.

CN108297242BActive Publication Date: 2024-11-01LENS TECH CHANGSHA
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN201710023582.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2017-01-12
Publication Date
2024-11-01
Estimated Expiration
2037-01-12

AI Technical Summary

Technical Problem

The existing ceramic blank injection molded products have low product precision due to collapse during sintering, which cannot meet the needs of high precision and mass production.

Method used

The supporting column cavity is set on the mother mold kernel of the mold, and the low-temperature injection molding and process control are used to ensure that the injection molded ceramic blanks do not shrink or deform significantly during the sintering process. Use the burning plate for degreasing and sintering, and finally remove the support column. .

Benefits of technology

It realizes the precise molding of ceramic blank injection molded products, reduces processing allowance and cost, and improves the manufacturing accuracy and yield of products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN108297242B_ABST
    Figure CN108297242B_ABST
Patent Text Reader

Abstract

The present invention discloses a ceramic blank injection molded product and a sintering method thereof, and a ceramic blank injection mold, which relate to the field of ceramic manufacturing technology, in order to solve the technical problems of low product precision and other poor quality caused by collapse of existing ceramic blank injection molded products during the sintering process. The sintering method of the ceramic blank injection molded product described in the present invention comprises the following steps: a support column cavity is provided on the core of the mother mold of the mold; the aperture of the support column cavity is polished; the mold is mounted on an injection molding machine and a hard metal screw is used for low-temperature injection molding; the process is controlled so that the appearance of the ceramic blank injection molded product has no obvious shrinkage or pillar pulling and sticking phenomenon; after obtaining the embryo with the support column, it is loaded on a firing plate and then degreased and sintered; the support column on the ceramic blank injection molded product is removed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic manufacturing, and in particular to a ceramic blank injection-molded product and a sintering method thereof, and a ceramic blank injection-molded mold. Background Art

[0002] With the development of the times, the use of ceramic products is no longer limited to traditional fields such as utensils and decorations, but is gradually expanding to fields such as electronic product components. These fields have increasingly higher requirements for the precision of ceramic products. The existing ceramic sintering technology is difficult to meet the requirements of industrial technology upgrading.

[0003] The traditional sintering method of ceramic 3D blank injection molded products can easily cause the blank to deform and fail to ensure the contour and size requirements of the product, especially for products with an arched inner surface and a convex surface. Before sintering, the blank is loaded on the support plate with the inner surface facing down and the surface facing up. During the sintering process, the zirconia material softens at high temperature, causing the blank to collapse and deform, which can easily cause the outer and inner diameters, inner surface height and contour of the finished ceramic to exceed 0.1mm, thus seriously affecting the manufacturing accuracy of the product.

[0004] Therefore, how to provide a sintering method for ceramic blank injection molded products so that the products can be evenly supported, shrink uniformly and have a certain degree of mass production during the high-temperature sintering process, and can effectively improve the manufacturing accuracy of the products, reduce processing allowances and reduce manufacturing costs, has become a technical problem that technical personnel in this field urgently need to solve. Summary of the invention

[0005] The purpose of the present invention is to provide a ceramic blank injection molded product and a sintering method thereof, and a ceramic blank injection mold, so as to solve the technical problems of existing ceramic blank injection molded products such as low product precision and poor quality due to collapse during the sintering process.

[0006] The invention provides a sintering method for ceramic blank injection-molded products, comprising the following steps: arranging a support column cavity on a mold core of a mold; polishing the aperture of the support column cavity; placing the mold on an injection molding machine and using a hard metal screw to perform low-temperature injection molding; controlling the process so that the surface of the ceramic blank injection-molded product has no obvious shrinkage or pillar die pulling and mold sticking phenomena; after obtaining a blank with a support column, degreasing and sintering are performed after loading it with a firing plate; and removing the support column on the ceramic blank injection-molded product.

[0007] Among them, the step of "providing a support column cavity on the mother mold core of the mold" specifically includes: performing a first R angle treatment on the root of the support column cavity; performing a second R angle treatment on the head of the support column cavity; and performing a demoulding angle treatment on one side of the support column cavity.

[0008] Specifically, the core of the master mold is made of high-hardness steel and is heat-treated to achieve a Rockwell hardness of more than 50; the roughness of the support column cavity after polishing is less than 10nm.

[0009] In actual application, the step of "placing the mold on an injection molding machine and using a hard metal screw for low-temperature injection molding" specifically includes: spraying a layer of alloy with a thickness of 0.15-0.25 mm and a Rockwell hardness of more than 60 on the surface of the metal screw, so that the surface hardness of the metal screw reaches more than 60; during low-temperature injection molding, the temperature of the ceramic blank is 150-180°C, and the temperature of the mold is below 50°C.

[0010] The main material of the ceramic is zirconia material; the zirconia material includes: 80-85wt% of ceramic inorganic components and 15-20wt% of organic binder components; the ceramic inorganic components are composed of 92-98wt% of zirconia and 2-8wt% of colorant.

[0011] Specifically, the step of "through process control so that the surface of the ceramic blank injection molded product has no obvious shrinkage or pillar pulling and sticking film phenomenon" specifically includes: injection, pressure holding, cooling, and ejection. The injection pressure is 50-80MPa, the holding pressure is 40-70MPa, the holding time is controlled at 0.5-2s, the injection speed is 10-120mm / s, and the cooling time is 5-50s.

[0012] Furthermore, the step of "obtaining the embryo with support columns and then loading it with a firing plate for degreasing and sintering" specifically includes: during degreasing, using a 300mm*150mm*80mm firing plate for loading, the flatness of the firing plate is required to be within 0.1mm, and corundum sand is evenly sprinkled on each of the firing plates before loading. Each of the firing plates is loaded with 15-20 pcs of ceramic blank injection molded products, and the loading layers are 6-8 layers with a layer spacing of 1-3cm. The ceramic blank injection molded products are evenly placed on the firing plates, and the air flow in the kiln is maintained. The entire degreasing process is divided into 5-9 temperature zones, and the highest temperature is 700°C. The entire degreasing time is 35-50h.

[0013] Furthermore, the step of "obtaining the embryo with support columns and then loading it with a firing plate for degreasing and sintering" specifically includes: during sintering, using a 300mm*150mm*100mm firing plate for loading, the flatness of the firing plate is required to be within 0.1mm, and corundum sand is evenly sprinkled on each of the firing plates before loading. Each of the firing plates is loaded with 15-20 pcs of ceramic blank injection molded products, and the loading layers are 6-8 layers with a layer spacing of 1-3cm. The ceramic blank injection molded products are evenly placed on the firing plates, and the air flow in the kiln is maintained. The entire sintering process is divided into 5-8 temperature zones, and the highest temperature is 1600°C. The entire sintering time is 25-40h.

[0014] Compared with the prior art, the sintering method of the ceramic blank injection molded product of the present invention has the following advantages:

[0015] The sintering method of ceramic blank injection molded products provided by the present invention includes the following steps: a support column cavity is provided on the mold core of the mold; the aperture of the support column cavity is polished; the mold is mounted on an injection molding machine and a hard metal screw is used for low-temperature injection molding; the process is controlled so that the appearance of the ceramic blank injection molded products has no obvious shrinkage or pillar pulling and sticking phenomenon; after obtaining the embryo with the support column, it is degreased and sintered after loading with a firing plate; the support column on the ceramic blank injection molded product is removed. From this analysis, it can be seen that in the sintering method of ceramic blank injection molded products provided by the present invention, since a support column cavity is provided on the mold core of the mold, the support column after molding can effectively prevent the injection molded embryo from being deformed and collapsed due to high-temperature softening during the sintering process, so that the ceramic blank injection molded products can ensure that the ceramic size after sintering is more accurate, reduce the ceramic processing allowance, and achieve the purpose of reducing costs and improving yields.

[0016] The present invention also provides a ceramic blank injection-molded product, comprising: an injection-molded body, wherein the injection-molded body is preset with a support column, and the support column is removed after the ceramic blank injection-molded product is sintered.

[0017] The present invention further provides a ceramic blank injection mold, comprising: a mother mold core, a plurality of support column cavities are arranged on the mother mold core, and the support column cavities are used to mold ceramic blank injection molded products with support columns, so that each support column can evenly bear the self-weight of the product after molding.

[0018] The advantages of the ceramic blank injection molded product, the ceramic blank injection mold and the sintering method of the ceramic blank injection molded product are the same as those of the prior art, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 A schematic flow chart of a method for sintering a ceramic blank injection molded product provided in an embodiment of the present invention;

[0021] Figure 2 A schematic structural diagram of a ceramic blank injection molded product provided by an embodiment of the present invention;

[0022] Figure 3 A schematic structural diagram of a ceramic blank injection mold provided by an embodiment of the present invention;

[0023] Figure 4 A schematic cross-sectional structure diagram of a ceramic blank injection molded product and a ceramic blank injection mold provided in an embodiment of the present invention.

[0024] In the figure: 1 - mold; 11 - mother mold core; 12 - support column cavity; 2 - ceramic blank injection molded product; 21 - support column; 22 - injection molded embryo. DETAILED DESCRIPTION

[0025] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0027] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0028] Figure 1 A schematic flow chart of a method for sintering a ceramic blank injection molded product provided in an embodiment of the present invention; Figure 2 A schematic structural diagram of a ceramic blank injection molded product provided by an embodiment of the present invention; Figure 3 A schematic structural diagram of a ceramic blank injection mold provided by an embodiment of the present invention; Figure 4 A schematic cross-sectional structure diagram of a ceramic blank injection molded product and a ceramic blank injection mold provided in an embodiment of the present invention.

[0029] like Figure 1 Combination Figure 2 - Figure 4 As shown, an embodiment of the present invention provides a sintering method for a ceramic blank injection molded product, comprising the following steps: step S1, providing (multiple) support column cavities 12 on the mother mold core 11 of the mold 1; step S2, polishing the aperture of the support column cavity 12; step S3, placing the mold stand on an injection molding machine and using a hard metal screw for low-temperature injection molding; step S4, through process control, so that the appearance of the ceramic blank injection molded product 2 has no obvious shrinkage or pillar pulling and sticking phenomenon; step S5, after obtaining the embryo with the support column, it is loaded on a firing plate and then degreased and sintered; step S6, removing the support column 21 on the ceramic blank injection molded product.

[0030] Compared with the prior art, the sintering method of the ceramic blank injection molded product described in the embodiment of the present invention has the following advantages:

[0031] In the sintering method of the ceramic blank injection molded product provided by the embodiment of the present invention, Figure 1 Combination Figure 2 - Figure 4As shown, the following steps are included: step S1, providing (multiple) support column cavities 12 on the mother mold core 11 of the mold 1; step S2, polishing the aperture of the support column cavity 12; step S3, placing the mold on an injection molding machine and using a hard metal screw for low-temperature injection molding; step S4, through process control, so that the appearance of the ceramic blank injection molded product 2 has no obvious shrinkage or pillar pulling and sticking phenomenon; step S5, after obtaining the embryo with the support column, it is loaded on a firing plate and then degreased and sintered; step S6, removing the support column 21 on the ceramic blank injection molded product. From this analysis, it can be seen that in the sintering method of the ceramic blank injection molded product provided in the embodiment of the present invention, since a support column cavity 12 is provided on the mother mold core 11 of the mold 1, the support column 21 can effectively prevent the injection molded body 22 from deforming and collapsing due to high-temperature softening during the sintering process after molding. Therefore, it can ensure that the ceramic blank injection molded product 2 has a more precise ceramic size after sintering and reduces the ceramic processing allowance, thereby achieving the purpose of reducing costs and improving yields.

[0032] The above step S1 may specifically include: performing a first R angle treatment of 0.3mm-0.8mm on the root of the support column cavity 12; performing a second R angle treatment of 0.3mm-0.8mm on the head of the support column cavity 12; performing a demoulding angle treatment of 5-15° on one side of the support column cavity 12. Preferably, the first R angle treatment of 0.5mm is performed on the root of the support column cavity 12; the second R angle treatment of 0.5mm is performed on the head of the support column cavity 12; and the demoulding angle treatment of 10° is performed on one side of the support column cavity 12.

[0033] The purpose of making the R angle is to prevent the product from cracking during the degreasing / sintering process.

[0034] It should be additionally explained here that the above-mentioned mother mold core 11 is used to form the inner concave surface of the ceramic blank injection-molded product 2, and the head of the above-mentioned support column cavity 12 is used to form the support surface of the support column 21.

[0035] In addition, taking a ceramic blank injection molded product 2 with a blank diameter of 30 mm, a wall thickness of 1.5 mm, and an inner concave depth of 3.0 mm as an example, the above-mentioned support column cavities 12 can be provided with 1-8, preferably 4 are evenly provided; the height of the support column cavity 12 can be 3.0±0.05 mm, preferably 3.0±0.03 mm, and the diameter can be 2.0-4.0 mm, preferably 2.0 mm.

[0036] Specifically, in order to ensure the injection molding effect, the above-mentioned mother mold core 11 can be made of high-hardness steel and undergo heat treatment to make the Rockwell hardness reach above 50; the roughness of the above-mentioned support column cavity 12 after polishing should be less than 10nm.

[0037] In practical application, the above step S3 may specifically include: spraying a layer of alloy with a thickness of 0.15-0.25 mm and a Rockwell hardness of more than 60 on the surface of the metal screw to make the surface hardness of the metal screw reach more than 60; during low-temperature injection molding, the temperature of the ceramic blank can be 150-180°C, and the temperature of the mold 1 can be below 50°C.

[0038] It should be noted that low-temperature injection molding can effectively solve the root shrinkage and demoulding pulling phenomenon caused by the thickness and height of the support column 21 during molding. Specifically, the temperature of the ceramic blank is 150-180°C, which can ensure that the heat of the material is fully released within the effective time and the fluidity of the material is guaranteed; the temperature of the mold 1 is below 50°C, which can increase the shrinkage of the support column 21 in the mold cavity, thereby effectively reducing the pulling and breaking phenomenon of the support column 21 during demoulding.

[0039] In addition, the diameter of the metal screw can be 25mm; during injection molding, the mold (i.e., mold core) can be placed on a 100T horizontal injection molding machine; and the tonnage of the injection molding machine can be 50T-200T. It should be noted that the mold core here refers to the mold cavity required for molding the entire product, specifically including mold core inserts, mold boxes, ejector blocks, ejector pins, etc. The mold base refers to a cavity used to fix the mold core cavity, specifically including male / female mold fixing plates, pallets, ejector plates, ejector fixing plates, guide pillars, positioning pins, etc.

[0040] Among them, the main material of the above-mentioned ceramic can be zirconium oxide material; specifically, the zirconium oxide material can include: 80-85wt% ceramic inorganic component, 15-20wt% organic binder component; further, the ceramic inorganic component can be composed of 92-98wt% zirconium oxide and 2-8wt% colorant; specifically, it can be a black colorant.

[0041] Due to the increase of the support column 21, it is easy to cause the root to be thick and shrink or die pulling and sticking phenomenon, so it is necessary to increase the holding time appropriately on the basis of the original process; that is, the standard is that the appearance of the ceramic blank injection molded product 2 has no obvious shrinkage, and excessive pressure should be avoided. Specifically, the above step S4 can specifically include: injection, holding pressure, cooling, and ejection, the injection pressure is 50-80MPa, preferably 75-80MPa, the holding pressure is 40-70MPa, preferably 50-55MPa, the holding time is controlled at 0.5-2s, preferably 1.0-1.5s, the injection speed is 10-120mm / s, and the cooling time is 5-50s, preferably 25s.

[0042] Furthermore, the above step S5 may specifically include: during degreasing, a 300mm*150mm*80mm support plate is used for loading, the flatness of the support plate is required to be within 0.1mm, 300-mesh corundum sand is evenly sprinkled on each support plate before loading, and the thickness of the sand is within 0.1mm, each support plate is loaded with 15-20pcs of ceramic blank injection molded products 2, and the loading layers are 6-8 layers with a layer spacing of 1-3cm, the ceramic blank injection molded products 2 are evenly placed on the support plate, and the air flow in the kiln is kept permeable, the entire degreasing process is divided into 5-9 temperature zones, and the highest temperature is 700°C, and the entire degreasing time is 35-50h.

[0043] In this case, preferably: each firing plate is loaded with 20 pcs of ceramic green injection molded products 2, and the loading layers are 6 layers with a layer spacing of 2 cm. The ceramic green injection molded products 2 are evenly placed on the firing plate, and the air flow in the kiln is kept permeable. The entire degreasing process is divided into 7 temperature zones, and the highest temperature is 700°C. The entire degreasing time is 50 hours.

[0044] Furthermore, the above step S5 can also specifically include: during sintering, use a 300mm*150mm*100mm support plate for loading, the flatness of the support plate is required to be within 0.1mm, and before loading, 300-mesh corundum sand is evenly sprinkled on each support plate, and the thickness of the sand is within 0.05mm, each support plate is loaded with 15-20pcs of ceramic green injection molded products 2, and the loading layers are 6-8 layers with a layer spacing of 1-3cm. The ceramic green injection molded products 2 are evenly placed on the support plate, and the air flow in the kiln is kept permeable. The entire sintering process is divided into 5-8 temperature zones, and the highest temperature is 1600°C, and the entire sintering time is 25-40h.

[0045] In this case, preferably: each firing plate is loaded with 20 pcs of ceramic green injection molded products 2, and the loading layers are 8 layers with a layer spacing of 1.5 cm. The ceramic green injection molded products 2 are evenly placed on the firing plate, and the air flow in the kiln is kept permeable. The entire sintering process is divided into 5 temperature zones, and the highest temperature is 1600°C. The entire sintering time is 35 hours.

[0046] It should be noted here that if cracking, deformation, blistering and other defects occur in the blank after degreasing, they can be alleviated or improved by sprinkling sand on the support plate.

[0047] Furthermore, when removing the support column 21 corresponding to the support column cavity 12 on the ceramic blank injection molded product 2, the finished ceramic after leaving the kiln can be placed on a CNC machine tool and positioned by a fixture, and then the support column 21 can be directly removed using a 2.0mm-5.0mm grinding wheel rod.

[0048] The present invention also provides a ceramic blank injection molded product, such as Figure 2 As shown, it includes: an injection molded body 22, on which a support column 21 is preset, and the support column 21 needs to be removed after the ceramic blank injection molded product 2 is sintered.

[0049] Specifically, the above-mentioned injection molded body 22 can be a circular arch as a whole, with an inner surface arch height of 3.0mm, a platform with a diameter of 20mm at the center of the inner surface; the inner diameter is 30mm, and the outer diameter is 32.5mm. After sintering, the inner and outer diameters of the ceramic blank injection molded product 2 are controlled within ±0.08mm, and the height from the center platform to the bottom plane of the product is controlled within ±0.05mm.

[0050] The embodiment of the present invention further provides a ceramic blank injection mold, such as Figure 3 As shown, it includes: a mother mold core 11, on which a plurality of support column cavities 12 are arranged, and the support column cavities 12 are used to mold a ceramic blank injection molded product with support columns 21, so that each support column 21 can evenly bear the self-weight of the injection molded product after molding.

[0051] The ceramic blank injection molded product and its sintering method, as well as the ceramic blank injection mold provided in the embodiments of the present invention can effectively solve the sintering collapse problem. Specifically, the inner diameter and inner height can be controlled within ±0.06mm, the inner roundness is within 0.1mm, and the matching dimensions of the entire inner surface do not require CNC processing, thereby achieving the purpose of reducing costs, reducing processes, and improving efficiency.

[0052] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for sintering a ceramic blank injection molded product, characterized in that: The ceramic blank injection molded product comprises an injection molded body, and the sintering method comprises the following steps: A support column cavity is provided on the female mold core of the mold; Polishing the aperture of the support column cavity; Place the mold on the injection molding machine and use a hard metal screw for low-temperature injection molding; Through process control, the surface of the ceramic blank injection molded product has no obvious shrinkage, support die pulling, or sticking film phenomenon; After obtaining the injection molded body with support columns, it is loaded on a setter plate and then degreased and sintered; Removing the support column on the ceramic blank injection molded product; Wherein, in the step of "arranging a support column cavity on the mother mold core of the mold", the mother mold core is used to form the inner concave surface of the ceramic blank injection molded product, and the head of the support column cavity is used to form the support surface of the support column; In the step of "obtaining the injection molded body with the support column and then loading it on a firing plate for degreasing and sintering", during sintering, the ceramic blank injection molded product is loaded on the plane of the firing plate.

2. The sintering method of ceramic green material injection molded product according to claim 1, characterized in that: The step of "arranging a support column cavity on the female mold core of the mold" specifically includes: The root of the support column cavity is subjected to a first R angle treatment; The head of the support column cavity is subjected to a second R angle treatment; One side of the support column cavity is subjected to demoulding angle treatment.

3. The sintering method of the ceramic green material injection molded product according to claim 1 or 2, characterized in that: The cores of male and female molds are made of high-hardness steel and heat-treated to achieve a Rockwell hardness of more than 50; The roughness of the support column cavity after polishing is less than 10 nm.

4. The sintering method of ceramic green material injection molded product according to claim 2, characterized in that: The step of "placing the mold on an injection molding machine and using a hard metal screw for low temperature injection molding" specifically includes: The surface of the metal screw is sprayed with a layer of alloy with a thickness of 0.15-0.25 mm and a Rockwell hardness of more than 60, so that the surface hardness of the metal screw reaches more than 60; During low-temperature injection molding, the temperature of the ceramic blank is 150-180°C, and the temperature of the mold is below 50°C.

5. The sintering method of ceramic green material injection molded product according to claim 1, characterized in that: The main material of the ceramic is zirconium oxide material; The zirconium oxide material comprises: 80-85wt% of a ceramic inorganic component and 15-20wt% of an organic binder component; The ceramic inorganic component consists of 92-98 wt % of zirconium oxide and 2-8 wt % of a colorant.

6. The sintering method of ceramic green material injection molded product according to claim 4, characterized in that: The step of "controlling the process so that the ceramic blank injection molded product has no obvious shrinkage or pillar pulling or sticking phenomenon on the surface" specifically includes: Injection, holding pressure, cooling, ejection, the injection pressure is 50-80MPa, the holding pressure is 40-70MPa, the holding time is controlled at 0.5-2s, the injection speed is 10-120mm / s, and the cooling time is 5-50s.

7. The sintering method of ceramic green material injection molded product according to claim 6, characterized in that: The step of "obtaining the embryo with the support column and then loading it on a setter plate for degreasing and sintering" specifically includes: During degreasing, a 300mm*150mm*80mm support plate is used for loading. The flatness of the support plate is required to be within 0.1mm. Corundum sand is evenly sprinkled on each support plate before loading. Each support plate is loaded with 15-20pcs of ceramic blank injection molded products, and the loading layers are 6-8 layers with a layer spacing of 1-3cm. The ceramic blank injection molded products are evenly placed on the support plate, and the air flow in the kiln is kept permeable. The entire degreasing process is divided into 5-9 temperature zones, and the highest temperature is 700°C. The entire degreasing time is 35-50h.

8. The sintering method of ceramic green material injection molded product according to claim 6, characterized in that: The step of "obtaining the embryo with the support column and then loading it on a setter plate for degreasing and sintering" specifically includes: During sintering, a 300mm*150mm*100mm support plate is used for loading. The flatness of the support plate is required to be within 0.1mm. Corundum sand is evenly sprinkled on each support plate before loading. Each support plate is loaded with 15-20pcs of ceramic green injection molded products, and the loading layers are 6-8 layers with a layer spacing of 1-3cm. The ceramic green injection molded products are evenly placed on the support plate, and the air flow in the kiln is kept permeable. The entire sintering process is divided into 5-8 temperature zones, and the highest temperature is 1600°C. The entire sintering time is 25-40h.

Citation Information

Patent Citations

  • Large-sized injection mold cutting-up board supporting structure

    CN103707470A

  • Forming and processing method for fine ceramic accessories

    CN104045360A

  • Magnetron ceramic sintering method and device thereof

    CN105084909A

  • Manufacturing method of zirconia ceramic large-scale thin-wall device

    CN105837206A

  • Ceramic blank injection molding , ceramic blank injection mold

    CN206703228U