Composite single crystal thin film

By combining the composite structure of lithium niobate or lithium tantalate single crystal film and silicon single crystal film in the field of optoelectronics, the problem of insufficient optical properties of silicon materials is solved, excellent optical and electrical properties are achieved, and the application prospects are expanded.

CN108565211BActive Publication Date: 2024-10-11JINAN JINGZHENG ELECTRONICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201810646430.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-06-21
Publication Date
2024-10-11
Estimated Expiration
2038-06-21

AI Technical Summary

Technical Problem

In the existing technology, the application of silicon materials in the field of optoelectronics is limited by its insufficient optical performance and its excellent electrical properties cannot be fully utilized.

Method used

It adopts a composite single crystal film structure, combining the optical properties of lithium niobate or lithium tantalate single crystal films with the electrical properties of silicon single crystal films, through the design of multi-layer structures and transition layers, including substrate, isolation layer, transition layer and The thin film layer uses plasma bonding and ion implantation technology to form a composite single crystal thin film with excellent properties.

Benefits of technology

It achieves stable and effective industrial production, improves the optical and electrical performance of the device, reduces scattering and transmission losses in signal propagation, and expands application prospects in fields such as optical signal processing and information storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN108565211B_ABST
    Figure CN108565211B_ABST
Patent Text Reader

Abstract

A composite single crystal film is provided, which may include the following seven-layer structure: a substrate; a first transition layer located on the substrate; a first isolation layer located on the first transition layer; a second transition layer located on the first isolation layer; a first thin film layer located on the second transition layer; a third transition layer located on the first thin film layer; and a second thin film layer located on the third transition layer, wherein the first transition layer, the second transition layer and the third transition layer may include H and Ar.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite single crystal thin film. Background Art

[0002] Lithium niobate and lithium tantalate single crystal films have excellent nonlinear optical, electro-optical, and acousto-optical properties, and are widely used in optical signal processing, information storage, etc. Silicon materials have become the most widely used material in the semiconductor industry due to their excellent electrical properties. However, the lack of optical properties of silicon materials limits their application in the optoelectronic field. Summary of the invention

[0003] In order to solve the above technical problems existing in the prior art, the purpose of the present invention is to provide a composite single crystal film that combines the advantages of lithium niobate or lithium tantalate single crystal film and silicon material, and the composite single crystal film can simultaneously utilize the optical properties of lithium niobate or lithium tantalate single crystal film and the electrical properties of silicon single crystal film to obtain a device with excellent performance. The composite single crystal film can achieve stable and effective industrial production and has a very broad application prospect.

[0004] According to the present invention, a composite single crystal thin film is provided, which may include the following seven-layer structure: a substrate; a first transition layer located on the substrate; a first isolation layer located on the first transition layer; a second transition layer located on the first isolation layer; a first thin film layer located on the second transition layer; a third transition layer located on the first thin film layer; and a second thin film layer located on the third transition layer, wherein the first transition layer, the second transition layer and the third transition layer may include H and Ar.

[0005] According to an embodiment of the present invention, the composite single crystal film may further include a second isolation layer between the first film layer and the second film layer, and the first isolation layer and the second isolation layer may both be silicon dioxide layers or silicon nitride layers, and their thicknesses may both be 0.005 μm to 4 μm.

[0006] According to an embodiment of the present invention, the concentration of H in the first transition layer, the second transition layer and the third transition layer may be 1×10 19 Atom / cc to 1×10 22 atoms / cc, the concentration of Ar in the first transition layer, the second transition layer, and the third transition layer can be 1×10 20 Atom / cc to 1×10 23 atoms / cc.

[0007] According to an embodiment of the present invention, the concentration of H in the second transition layer may be higher than the concentrations of H in the first isolation layer and the first thin film layer, respectively, and the concentration of H in the third transition layer may be higher than the concentrations of H in the first thin film layer and the second thin film layer, respectively.

[0008] According to an embodiment of the present invention, the thickness of the first transition layer may be 0.5 nm to 15 nm, the thickness of the second transition layer may be 0.5 nm to 10 nm, and the thickness of the third transition layer may be 0.5 nm to 15 nm.

[0009] According to an embodiment of the present invention, the third transition layer may include a first sub-transition layer adjacent to the first thin film layer and a second sub-transition layer adjacent to the second thin film layer. In the first sub-transition layer, the concentration of the element of the first thin film layer may be higher than the concentration of the element in the second thin film layer, and the concentration of the element of the first thin film layer may gradually decrease from the first sub-transition layer to the second sub-transition layer. In the second sub-transition layer, the concentration of the element of the second thin film layer may be higher than the concentration of the element of the first thin film layer, and the concentration of the element of the second thin film layer may gradually decrease from the second sub-transition layer to the first sub-transition layer.

[0010] According to an embodiment of the present invention, the first thin film layer and the second thin film layer may both be single crystal thin films with a nanometer-level thickness, and the thickness may be 10 nm to 2000 nm.

[0011] According to an embodiment of the present invention, the first thin film layer may be a lithium niobate single crystal thin film or a lithium tantalate single crystal thin film, and the second thin film layer may be a silicon single crystal thin film.

[0012] According to an embodiment of the present invention, the third transition layer may include: Si, which is distributed throughout the entire third transition layer, and the concentration of Si gradually decreases from the silicon single crystal thin film layer to the lithium niobate single crystal thin film layer or the lithium tantalate single crystal thin film layer; Ta or Nb, which is not distributed throughout the entire third transition layer, and the concentration of Ta or Nb gradually decreases from the lithium niobate single crystal thin film layer or the lithium tantalate single crystal thin film layer to the silicon single crystal thin film layer.

[0013] According to an embodiment of the present invention, the substrate may be a silicon substrate, a lithium niobate substrate or a lithium tantalate substrate, and the thickness of the substrate may be 0.1 mm to 1 mm. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] These and / or other aspects will become clear and more easily understood through the following description of the embodiments in conjunction with the accompanying drawings, in which:

[0015] Figure 1 is a schematic diagram showing the structure of a composite single crystal thin film according to an embodiment of the present invention;

[0016] Figure 2 is a transmission electron microscope (TEM) image showing a composite single crystal thin film according to an embodiment of the present invention;

[0017] Figure 3 yes Figure 2 An enlarged view of region A shown in FIG.

[0018] Figure 4 yes Figure 2 Element distribution diagram of region A shown in FIG.

[0019] Figure 5 yes Figure 2 An enlarged view of region B shown in FIG.

[0020] Figure 6 yes Figure 2 Element distribution diagram of region B shown in FIG.

[0021] Figure 7 yes Figure 2 An enlarged view of region C shown in FIG.

[0022] Figure 8 yes Figure 2 The element distribution diagram of region C shown in FIG.

[0023] Fig. 9 It shows Figure 2 Secondary ion mass spectrometry (SIMS) diagram of region A and region B shown in FIG. DETAILED DESCRIPTION

[0024] Embodiments of the present invention will now be described more fully with reference to the accompanying drawings, in which embodiments of the present invention are shown. However, the present invention can be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be thorough and complete, and these embodiments will fully convey the concept of the embodiments of the present invention to those of ordinary skill in the art. In the following detailed description, a number of specific details are set forth by way of example to provide a full understanding of the relevant teachings. However, it should be clear to those skilled in the art that the present teachings can be practiced without such details. In other cases, well-known methods, steps, and components are described at a relatively high level without details to avoid unnecessarily obscuring aspects of the present teachings. The same reference numerals in the accompanying drawings represent the same elements, and therefore their descriptions will not be repeated. In the accompanying drawings, the sizes and relative sizes of layers and regions may be exaggerated for clarity.

[0025] The present invention will now be described more fully hereinafter with reference to the accompanying drawings.

[0026] Figure 1 is a schematic diagram showing the structure of a composite single crystal thin film according to an embodiment of the present invention.

[0027] Reference Figure 1According to an embodiment of the present invention, the composite single crystal thin film may include: a substrate 110; a first transition layer 115, located on the substrate 110; a first isolation layer 120, located on the first transition layer 115; a second transition layer 125, located on the first isolation layer 120; a first thin film layer 130, located on the second transition layer 125; a third transition layer 135, located on the first thin film layer 130; and a second thin film layer 140, located on the third transition layer 135.

[0028] According to an embodiment of the present invention, the composite single crystal thin film may be prepared into a wafer, and the diameter of the wafer may be 2 inches to 12 inches.

[0029] According to an embodiment of the present invention, the substrate 110 of the composite single crystal thin film can mainly play a supporting role. According to an embodiment of the present invention, the substrate 110 can be a silicon substrate, a lithium niobate substrate or a lithium tantalate substrate, but the present invention is not limited thereto, but can be made of other suitable materials. In addition, the thickness of the substrate 110 according to an embodiment of the present invention can be 0.1mm to 1mm. Preferably, the thickness of the substrate 110 can be 0.1mm to 0.2mm, 0.3mm to 0.5mm or 0.2mm to 0.5mm.

[0030] According to an embodiment of the present invention, the first isolation layer 120 of the composite single crystal film is used to separate the substrate 110 from the first film layer 130. Since the refractive index of the substrate 110 such as silicon is greater than the refractive index of the lithium niobate single crystal film or the lithium tantalate single crystal film, and the refractive index of these two materials is greater than the refractive index of silicon dioxide or silicon nitride, the first isolation layer 120 can be made of silicon dioxide or silicon nitride to separate the lithium niobate single crystal film or the lithium tantalate single crystal film from the substrate, thereby preventing the light field of the lithium niobate single crystal film or the lithium tantalate single crystal film from being erroneously coupled into the substrate 110. According to an embodiment of the present invention, the first isolation layer 120 can be made of a material (for example, silicon dioxide or silicon nitride) having a refractive index less than the refractive index of the substrate 110 and the refractive index of the first film layer 130, but the present invention is not limited thereto. According to an embodiment of the present invention, the thickness of the first isolation layer 120 can be 0.005 μm to 4 μm, preferably 100 nm to 2 μm.

[0031] According to another embodiment of the present invention, the composite single crystal film may further include a second isolation layer (not shown) located between the first film layer 130 and the second film layer 140, the second isolation layer may be a silicon dioxide layer or a silicon nitride layer, and the thickness of the second isolation layer may be 0.005 μm to 4 μm, preferably 100 nm to 2 μm, but the present invention is not limited thereto. The second isolation layer not only plays an optical isolation role for the first film layer 130 and the second film layer 140, but also prevents the mutual diffusion of elements of the first film layer 130 and the elements of the second film layer 140, avoids the first film layer 130 and the second film layer 140 from being contaminated by impurities, ensures the quality of the first film layer 130 and the second film layer 140, and thus ensures that the characteristics of the first film layer 130 and the second film layer 140 are not affected.

[0032] According to an embodiment of the present invention, the first isolation layer 120 and the second isolation layer may be respectively formed on the substrate 110 and the first thin film layer 130 or the second thin film layer 140 by methods such as deposition and oxidation, but the present invention is not limited thereto.

[0033] According to an embodiment of the present invention, the composite single crystal film includes a first film layer 130 and a second film layer 140 of different materials, the first film layer 130 may be a lithium niobate single crystal film or a lithium tantalate single crystal film having excellent optical properties, and the second film layer 140 may be a silicon single crystal film having excellent electrical properties. The first film layer 130 and the second film layer 140 may both have a nanometer-level thickness, and the thickness thereof is 10nm to 2000nm. Preferably, the thickness of the first film layer 130 and the second film layer 140 may be 10 to 200nm, 300nm to 900nm, or 1000nm to 1500nm. In addition, the upper surface of the second film layer 140 may be a polished surface or a rough surface having a micrometer or submicrometer level roughness.

[0034] According to an embodiment of the present invention, the first isolation layer 120 and the first thin film layer 130 and the first thin film layer 130 and the second thin film layer 140 may be bonded together by a plasma bonding method, but the present invention is not limited thereto.

[0035] According to an embodiment of the present invention, the composite single crystal thin film may include three transition layers, and each transition layer has its own characteristics.

[0036] According to an embodiment of the present invention, Figure 1 As shown in FIG. 1 , the first transition layer 115 may be located between the substrate 110 and the first isolation layer 120 , and the thickness thereof may be 0.5 nm to 15 nm.

[0037] According to an embodiment of the present invention, the first transition layer 115 may contain intrinsic elements in the substrate 110 and the first isolation layer 120. In the first transition layer 115, the concentration of the element of the substrate 110 may gradually decrease from the substrate 110 toward the first isolation layer 120, and the concentration of the element of the first isolation layer 120 may gradually decrease from the first isolation layer 120 toward the substrate 110.

[0038] According to an embodiment of the present invention, the second transition layer 125 may be located between the first isolation layer 120 and the first thin film layer 130 , and the thickness thereof may be 0.5 nm to 10 nm.

[0039] According to an embodiment of the present invention, the second transition layer 125 may include intrinsic elements in the first isolation layer 120 and the first thin film layer 130. In the second transition layer 125, the concentration of the element of the first isolation layer 120 may gradually decrease from the first isolation layer 120 toward the first thin film layer 130, and the concentration of the element of the first thin film layer 130 may gradually decrease from the first thin film layer 130 toward the first isolation layer 120.

[0040] According to an embodiment of the present invention, the third transition layer 135 may be located between the first thin film layer 130 and the second thin film layer 140 , and the thickness thereof may be 0.5 nm to 15 nm.

[0041] In addition, according to an embodiment of the present invention, the third transition layer 135 may include a first sub-transition layer 135a adjacent to the first thin film layer 130 and a second sub-transition layer 135b adjacent to the second thin film layer 140. The thickness of the first sub-transition layer 135a may be 0 to 5 nm, and the thickness of the second sub-transition layer 135b may be 0 to 10 nm, but the embodiment of the present invention is not limited thereto. For example, the thickness of the first sub-transition layer 135a and the second sub-transition layer 135b may change with the change of the subsequent process temperature (e.g., annealing temperature).

[0042] According to an embodiment of the present invention, the first sub-transition layer 135a mainly includes an element inherent in the first thin film layer 130, and in the first sub-transition layer 135a, the concentration of the element of the first thin film layer 130 can be gradually reduced from the first thin film layer 130 toward the second thin film layer 140. The second sub-transition layer 135b mainly includes an element inherent in the second thin film layer 140, and in the second sub-transition layer 135b, the concentration of the element of the second thin film layer 140 can be gradually reduced from the second thin film layer 140 toward the first thin film layer 130.

[0043] In addition, according to an embodiment of the present invention, when the first thin film layer 130 is a lithium niobate single crystal thin film or a lithium tantalate single crystal thin film, and the second thin film layer 140 is a silicon single crystal thin film, the third transition layer 135 may include Si element and Ta element or Nb element. In this case, the Si element is distributed throughout the entire third transition layer 135, that is, the Si element can be distributed throughout the entire first sub-transition layer 135a and the second sub-transition layer 135b, and the concentration of the Si element can be gradually reduced from the second thin film layer 140 toward the first thin film layer 130. The Ta element or the Nb element may not be distributed throughout the entire third transition layer 135, for example, the Ta element or the Nb element only exists in the sub-transition layer (first sub-transition layer 135a) adjacent to the first thin film layer 130, or a small amount of the Ta element or the Nb element exists in the partial thickness of the sub-transition layer (second sub-transition layer 135b) adjacent to the second thin film layer 140 close to the first thin film layer 130, and the concentration of the Ta element or the Nb element is gradually reduced from the first thin film layer 130 toward the second thin film layer 140. However, the embodiments of the present invention are not limited thereto.

[0044] According to an embodiment of the present invention, the first transition layer 115, the second transition layer 125 and the third transition layer 135 further include H element and Ar element. The Ar element in the second transition layer 125 and the third transition layer 135 originates from the plasma used when plasma bonding is performed between the first isolation layer 120 and the first thin film layer 130 or between the first thin film layer 130 and the second thin film layer 140, and the Ar element in the first transition layer 115 originates from the diffusion of the Ar element in the second transition layer 125 and the third transition layer 135. The reason why the second transition layer 125 and the third transition layer 135 have a higher concentration of H element is that when the surface of the first isolation layer 120, the first thin film layer 130 or the second thin film layer 140 is treated by plasma, the bombardment of the surface by the plasma will change its surface condition, so that a large number of active groups are formed on the surface, thereby making the surface have a higher activity. Therefore, when exposed to the air after the plasma treatment, a large amount of water molecules in the air will be adsorbed, so after the first isolation layer 120 and the first film layer 130 or the first film layer 130 and the second film layer 140 are bonded, there is a higher concentration of H element at their bonding interface. In addition, the H element in the first transition layer 115 comes from the diffusion of the H element in the second transition layer 125 and the third transition layer 135. In this case, the higher concentration of H element in the second transition layer 125 and the third transition layer 135 can form hydrogen bonds, thereby promoting bonding to enhance the bonding force of the bonding interface between the first isolation layer 120 and the first film layer 130 or the bonding interface between the first film layer 130 and the second film layer 140.

[0045] According to the embodiment of the present invention, in the first transition layer 115, the concentrations of the Ar element and the H element gradually decrease from their maximum concentrations in the direction toward the substrate 110 and the first isolation layer 120, respectively. This is because: the lattice constant of the material surface is generally slightly larger than the lattice constant of the material interior, that is, the density of the material surface is smaller than the density of the material interior. At the interface between the substrate 110 and the first isolation layer 120 having different materials (i.e., the first transition layer 115), the density is smaller than that inside the substrate 110 and the first isolation layer 120, that is, at the first transition layer 115, there are more gaps to accommodate impurity atoms, so the concentrations of H and Ar in the transition layer will be higher than those inside the substrate 110 and the first isolation layer 120. In the second transition layer 125, the concentrations of the Ar element and the H element gradually decrease from their maximum concentrations in the direction toward the first isolation layer 120 and the first thin film layer 130, respectively. In the third transition layer 135, the concentrations of the Ar element and the H element gradually decrease from their maximum concentrations in the direction toward the first thin film layer 130 and the second thin film layer 140, respectively. In the first transition layer 115, the second transition layer 125 and the third transition layer 135, the concentration of H element may be 1×10 19 Atom / cc to 1×10 22 atoms / cc, the concentration of Ar element is 1×10 20 Atom / cc to 1×10 23 atoms / cc, preferably, the concentration of Ar element is 1×10 20 Atom / cc to 1×10 22 Atom / cc, 1×10 21 Atom / cc to 1×10 22 atoms / cc and 1×10 22 Atom / cc to 1×10 23 atoms / cc.

[0046] The composite single crystal film according to the embodiment of the present invention has a first transition layer 115, a second transition layer 125 and a third transition layer 135, which can disperse the stress between the single crystal films. The dispersion of stress can reduce the defects of the single crystal film and improve the quality of the single crystal film, thereby reducing the transmission loss. In addition, the surfaces of the first transition layer 115, the second transition layer 125 and the third transition layer 135 are relatively flat, and the flat surface can reduce the scattering of the signal during the propagation process and reduce the transmission loss.

[0047] The following examples illustrate the present invention in more detail. However, these examples should not be interpreted as limiting the scope of the present invention in any sense.

[0048] Fabrication of composite single crystal thin films

[0049] Example 1: Silicon substrate / SiO 2Layer / Lithium Niobate Single Crystal Thin Film / Silicon Single Crystal Thin Film Composite Single Crystal Thin Film

[0050] A single crystal silicon substrate wafer with a size of 3 inches, a thickness of 0.4 mm and a smooth surface is prepared. After the silicon substrate is cleaned, a silicon dioxide layer with a thickness of 2 μm is formed on the smooth surface of the single crystal silicon substrate wafer by a thermal oxidation method.

[0051] Prepare a 3-inch lithium niobate wafer and use ion implantation to inject helium ions (He + ) is implanted into the lithium niobate wafer, the helium ion implantation energy is 200 KeV, and the dose is 4×10 16 ions / cm 2 A lithium niobate wafer having a three-layer structure of a thin film layer, a separation layer and a residual material layer is formed.

[0052] The thin film layer of the ion-implanted lithium niobate wafer is bonded to the silicon dioxide layer of the silicon substrate by plasma bonding to form a bonded body; the bonded body is then placed in a heating device and kept warm at 350°C until the residual material layer is separated from the bonded body to form a lithium niobate single crystal film. The lithium niobate single crystal film is then polished and thinned to 400nm to obtain a lithium niobate single crystal film with a nanometer-level thickness.

[0053] Prepare a 3-inch single crystal silicon wafer and use ion implantation to implant hydrogen ions (H + ) is implanted into the silicon wafer, the hydrogen ion implantation energy is 40KeV, and the dose is 6×10 16 ions / cm 2 A silicon wafer having a three-layer structure of a thin film layer, a separation layer and a residual material layer is formed.

[0054] The thin film layer of the ion-implanted silicon wafer is bonded to the lithium niobate single crystal thin film wafer obtained above by plasma bonding to obtain another bonded body. The bonded body is then placed in a heating device and kept warm at 400°C until the thin film layer of the silicon single crystal thin film wafer is separated from the bonded body to form a composite structure with a top layer of silicon single crystal thin film, and then the obtained composite structure is placed in an oven and kept warm at 500°C to eliminate the implantation damage; finally, the silicon single crystal thin film is polished and thinned to 220nm to obtain a composite single crystal thin film product with a double-layer nanometer-level thickness film.

[0055] Example 2: Silicon substrate / SiO 2 Layer / LiNbO3 single crystal thin film / SiO 2 Layer / Silicon single crystal film composite single crystal film

[0056] A single crystal silicon wafer with a size of 3 inches, a thickness of 0.4 mm and a smooth surface was prepared as a substrate. After the substrate wafer was cleaned, a silicon dioxide layer with a thickness of 2.5 μm was formed on the smooth surface of the substrate wafer by a thermal oxidation method.

[0057] Prepare a 3-inch lithium niobate wafer and use ion implantation to inject helium ions (He 2+ ) is implanted into the lithium niobate wafer, the helium ion implantation energy is 200 KeV, and the dose is 4×10 16 ions / cm 2 A lithium niobate wafer having a three-layer structure of a thin film layer, a separation layer and a residual material layer is formed.

[0058] The thin film layer of the lithium niobate wafer after ion implantation is bonded to the silicon dioxide layer of the silicon substrate by plasma bonding to form a bonded body. The bonded body is then placed in a heating device and heated at 350°C until the residual material layer is separated from the bonded body to form a lithium niobate single crystal film. The lithium niobate single crystal film is then polished and thinned to 300nm to obtain a bonded body of a lithium niobate single crystal film with a nanometer-level thickness.

[0059] Prepare a 3-inch single-crystal silicon wafer with a surface covered with a 50nm thick SiO 2 , using ion implantation to inject hydrogen ions (H + ) is injected into the SiO 2 The hydrogen ion implantation energy is 40 KeV and the dose is 6×10 16 ions / cm 2 , forming a silicon wafer with a three-layer structure of a thin film layer, a separation layer and a residual material layer.

[0060] The thin film layer of the ion-implanted silicon wafer is bonded to the lithium niobate single crystal thin film obtained above by plasma bonding to obtain another bonded body; the bonded body is then placed in a heating device and heated at 400°C until the residual material layer of the silicon wafer is separated from the bonded body to form a composite structure with the top layer being a silicon single crystal thin film, and then the obtained composite structure is placed in an oven and kept warm at 600°C to eliminate the implantation damage. Finally, the silicon single crystal thin film is polished and thinned to 220nm to obtain a composite single crystal thin film product with a double-layer nano-thickness film.

[0061] Example 3: Silicon substrate / SiO 2 Layer / Lithium Tantalate Single Crystal Thin Film / Silicon Single Crystal Thin Film Composite Single Crystal Thin Film

[0062] A single crystal silicon substrate wafer with a size of 3 inches, a thickness of 0.4 mm and a smooth surface was prepared. After the substrate wafer was cleaned, a silicon dioxide layer with a thickness of 600 nm was formed on the smooth surface of the substrate wafer by thermal oxidation.

[0063] Prepare a 3-inch lithium tantalate single crystal thin film wafer and use ion implantation to inject helium ions (He + ) is implanted into the lithium tantalate wafer, the helium ion implantation energy is 200 KeV, and the dose is 4×10 16 ions / cm 2 A lithium tantalate wafer having a three-layer structure of a thin film layer, a separation layer and a residual material layer is formed.

[0064] The thin film layer of the ion-implanted lithium tantalate wafer is bonded to the silicon dioxide layer of the silicon substrate wafer by plasma bonding to form a bonded body; the bonded body is then placed in a heating device and kept warm at 350°C until the residual material layer is separated from the bonded body to form a lithium tantalate single crystal film. The lithium tantalate single crystal film is then polished and thinned to 400nm to obtain a bonded body of a lithium tantalate single crystal film with a nanometer-level thickness.

[0065] Prepare a 3-inch single crystal silicon wafer and use ion implantation to implant hydrogen ions (H + ) is implanted into the silicon wafer, the hydrogen ion implantation energy is 80KeV, and the dose is 6×10 16 ions / cm 2 A silicon wafer having a three-layer structure of a thin film layer, a separation layer and a residual material layer is formed.

[0066] The thin film layer of the silicon wafer and the above-obtained lithium tantalate single crystal thin film are bonded by a plasma bonding method to obtain another bonded body; the bonded body is then placed in a heating device and kept warm at 400°C until the residual material layer of the silicon wafer is separated from the bonded body to form a composite structure with a top layer of the silicon single crystal thin film; the obtained composite structure is then placed in an oven and kept warm at 500°C to eliminate injection damage; finally, the silicon single crystal thin film is polished and thinned to 500nm to obtain a composite single crystal thin film product with a double-layer nanometer-level thickness film.

[0067] Example 4: Lithium Tantalate Substrate / SiO 2 Layer / Lithium Tantalate Single Crystal Thin Film / Silicon Single Crystal Thin Film Composite Single Crystal Thin Film

[0068] A lithium tantalate substrate wafer with a size of 3 inches, a thickness of 0.4 mm and a smooth surface was prepared. After the substrate wafer was cleaned, a silicon dioxide layer with a thickness of 1.0 μm was deposited on the smooth surface of the substrate wafer by a deposition method. The substrate wafer with the silicon dioxide layer was then annealed; the silicon dioxide layer was then polished to a target thickness of 600 nm.

[0069] Prepare a 3-inch lithium tantalate wafer and use ion implantation to implant helium ions (He 2+ ) is implanted into the lithium tantalate wafer, the helium ion implantation energy is 400 KeV, and the dose is 4×10 16 ions / cm 2 A lithium tantalate wafer having a three-layer structure of a thin film layer, a separation layer and a residual material layer is formed.

[0070] The thin film layer of the lithium tantalate wafer after ion implantation is bonded to the silicon dioxide layer of the silicon substrate wafer with a silicon dioxide layer deposited thereon by plasma bonding to form a bonded body; the bonded body is then placed in a heating device and kept warm at 350°C until the residual material layer is separated from the bonded body to form a lithium tantalate single crystal film. The lithium tantalate single crystal film is then polished and thinned to 800nm ​​to obtain a lithium tantalate single crystal film with a nanometer-level thickness.

[0071] Prepare a 3-inch single crystal silicon wafer and use ion implantation to implant hydrogen ions (H + ) is implanted into the silicon wafer, the hydrogen ion implantation energy is 80KeV, and the dose is 6×10 16 ions / cm 2 A silicon wafer having a three-layer structure of a thin film layer, a separation layer and a residual material layer is formed.

[0072] The thin film layer of the ion-implanted silicon wafer is bonded to the lithium tantalate single crystal thin film obtained above by plasma bonding to obtain another bonded body; the bonded body is then placed in a heating device and kept warm at 400°C until the residual material layer of the silicon wafer is separated from the bonded body to form a composite structure with a top layer of silicon single crystal thin film; finally, the silicon single crystal thin film is polished and thinned to 500nm to obtain a composite single crystal thin film product with a double-layer nanometer-level thickness film; finally, the composite single crystal thin film product is placed in an oven and kept warm at 500°C to eliminate injection damage.

[0073] Figure 2 is a transmission electron microscope (TEM) image showing the composite single crystal thin film according to Example 1 of the present invention.

[0074] Reference Figure 2According to an embodiment of the present invention, the substrate 110 of the composite single crystal film is a silicon substrate, the first isolation layer 120 is a silicon dioxide layer, the first film layer 130 is a lithium niobate single crystal film, and the second film layer 140 is a silicon single crystal film. Figure 2 It can be seen from the figure that the composite single crystal film according to the embodiment of the present invention includes a first transition layer 115 located between the substrate 110 and the first isolation layer 120, a second transition layer 125 located between the first isolation layer 120 and the first thin film layer 130, and a third transition layer 135 located between the first thin film layer 130 and the second thin film layer 140. The bonding interface in the composite single crystal film according to the embodiment of the present invention is clear and the boundary line is relatively flat, so the interface loss of acoustic waves and optical waves will be greatly reduced, thereby improving the performance of the device.

[0075] Figure 3 yes Figure 2 An enlarged view of region A is shown in FIG. Figure 4 yes Figure 2 Element distribution diagram of region A shown in FIG.

[0076] Reference Figure 3 The region A between the first film layer 130 and the second film layer 140 of the composite single crystal film includes four layers with clear interfaces, namely, the first film layer 130, the third transition layer 135 including the first sub-transition layer 135a and the second sub-transition layer 135b, and the second film layer 140. The first sub-transition layer 135a is adjacent to the first film layer 130, and the second sub-transition layer 135b is adjacent to the second film layer 140 and is located on the first sub-transition layer 135a. The thickness of the first sub-transition layer 135a and the second sub-transition layer 135b is related to the annealing temperature of the composite single crystal film.

[0077] Reference Figure 4 In the interface region A between the first film layer 130 and the second film layer 140 of the composite single crystal film, when the first film layer 130 is a lithium niobate single crystal film and the second film layer 140 is a silicon single crystal film, the Si element has the highest concentration in the second film layer 140, and the concentration of the Si element gradually increases from the first film layer 130 toward the second film layer 140, and the Si element is distributed throughout the third transition layer 135. The Nb element and the O element have the highest concentration in the first film layer 130, and the concentration of the Nb element and the O element gradually increases from the second film layer 140 toward the first film layer 130, and the Nb element does not distribute throughout the third transition layer 135. In addition, a small amount of Ar element exists in the third transition layer 135.

[0078] Figure 5 and Figure 7 They are Figure 2 The enlarged view of area B and area C shown in FIG. Figure 6 and Figure 8 They are Figure 2 Element distribution diagram of region B and region C shown in FIG.

[0079] Reference Figure 5 and Figure 7 There are transition layers with very thin thickness and clear and smooth interfaces between the first isolation layer 120 and the first thin film layer 130 and between the substrate 110 and the first isolation layer 120, namely, a second transition layer 125 between the first isolation layer 120 and the first thin film layer 130 and a first transition layer 115 between the substrate 110 and the first isolation layer 120.

[0080] Reference Figure 6 , when the first thin film layer 130 is a lithium niobate single crystal thin film and the first isolation layer 120 is a silicon dioxide layer, in the second transition layer 125 between the first isolation layer 120 and the first thin film layer 130, the Si element has a maximum concentration in the first isolation layer 120, and the concentration of the Si element gradually decreases from the first isolation layer 120 toward the first thin film layer 130. The Nb element has a maximum concentration in the first thin film layer 130, and the concentration of the Nb element gradually decreases from the first thin film layer 130 toward the first isolation layer 120. In addition, a relatively high concentration of the O element and a small amount of the Ar element also exist in the second transition layer 125.

[0081] Reference Figure 8 , when the first isolation layer 120 is a silicon dioxide layer and the substrate 110 is a silicon substrate, in the first transition layer 115 between the first isolation layer 120 and the substrate 110, the O element has a maximum concentration in the first isolation layer 120, and the concentration of the O element gradually decreases from the first isolation layer 120 toward the substrate 110. The Si element has a maximum concentration in the substrate 110, and the concentration of the Si element gradually decreases from the substrate 110 toward the first isolation layer 120. In addition, a small amount of Ar element also exists in the first transition layer 115.

[0082] Fig. 9 It shows Figure 2 Secondary ion mass spectrometry (SIMS) diagram of region A and region B shown in FIG.

[0083] Reference Fig. 9 The second transition layer 125 and the third transition layer 135 contain a high concentration of H element, and the concentration of H element is 1×10 20 Atom / cc to 1×10 21atoms / cc, the H concentration in the second transition layer 125 may be higher than the H concentration in the first isolation layer 120 and the first thin film layer 130, respectively, and the H concentration in the third transition layer 135 may be higher than the H concentration in the first thin film layer 130 and the second thin film layer 140, respectively. The high concentration of H element improves the bonding force of the bonding interface.

[0084] The present invention provides a composite single crystal film, which combines the excellent optical properties of lithium niobate or lithium tantalate single crystal films with the excellent electrical properties of silicon materials, thereby improving the performance of the composite single crystal film. In addition, the composite single crystal film has a transition layer with a relatively flat surface, which can disperse the stress between the single crystal films and reduce the scattering of signals during propagation, so as to reduce the defects of the single crystal film and improve the quality of the single crystal film, thereby playing a role in reducing transmission loss.

[0085] Although the present invention has been specifically shown and described with reference to exemplary embodiments of the present invention, it will be understood by those skilled in the art that various changes in form and detail may be made herein without departing from the spirit and scope of the present invention as defined by the appended claims and their equivalents. The embodiments should be considered in a descriptive sense only and not for the purpose of limitation. Therefore, the scope of the present invention is not limited by the specific embodiments of the present invention, but by the claims, and all differences within the scope will be interpreted as included in the present invention.

Claims

1. A composite single crystal thin film, comprising: substrate; A first transition layer, located on the substrate; A first isolation layer, located on the first transition layer; A second transition layer, located on the first isolation layer; a first film layer, disposed on the second transition layer; A third transition layer, located on the first film layer; and The second film layer is located on the third transition layer. The first transition layer, the second transition layer and the third transition layer include H and Ar. The third transition layer includes a first sub-transition layer adjacent to the first thin film layer and a second sub-transition layer adjacent to the second thin film layer. The first film layer is a lithium niobate single crystal film or a lithium tantalate single crystal film, and the second film layer is a silicon single crystal film. The third transition layer comprises: Si, which is distributed throughout the first sub-transition layer and the second sub-transition layer; and Ta or Nb, which is only present in the first sub-transition layer, or in the first sub-transition layer and a portion of the second sub-transition layer close to the first thin film layer. The concentration of H in the first transition layer, the second transition layer, and the third transition layer is 1×10 19 Atom / cc to 1×10 22 atoms / cc.

2. The composite single crystal thin film according to claim 1, wherein: The composite single crystal film further includes a second isolation layer located between the first film layer and the second film layer, and the first isolation layer and the second isolation layer are silicon dioxide layers or silicon nitride layers, and the thickness thereof is 0.005 μm to 4 μm.

3. The composite single crystal thin film according to claim 1, wherein: The concentration of Ar in the first transition layer, the second transition layer, and the third transition layer is 1×10 20 Atom / cc to 1×10 23 atoms / cc.

4. The composite single crystal thin film according to claim 1, wherein: The concentration of H in the second transition layer is higher than the concentrations of H in the first isolation layer and the first thin film layer, respectively. The concentration of H in the third transition layer is higher than the concentrations of H in the first thin film layer and the second thin film layer, respectively.

5. The composite single crystal thin film according to claim 1, wherein: The thickness of the first transition layer is 0.5 nm to 15 nm, the thickness of the second transition layer is 0.5 nm to 10 nm, and the thickness of the third transition layer is 0.5 nm to 15 nm.

6. The composite single crystal thin film according to claim 1, in, In the first sub-transition layer, the concentration of the element in the first thin film layer is higher than the concentration of the element in the second thin film layer, and the concentration of the element in the first thin film layer gradually decreases from the first sub-transition layer to the second sub-transition layer. In the second sub-transition layer, the concentration of the element of the second thin film layer is higher than that of the first thin film layer, and the concentration of the element of the second thin film layer gradually decreases from the second sub-transition layer to the first sub-transition layer.

7. The composite single crystal thin film according to claim 1, wherein: Both the first thin film layer and the second thin film layer are single crystal thin films with a nanometer-level thickness, and the thickness thereof is 10 nm to 2000 nm.

8. The composite single crystal thin film according to claim 1, wherein: The concentration of Si gradually decreases from the silicon single crystal thin film layer to the lithium niobate single crystal thin film layer or the lithium tantalate single crystal thin film layer; The concentration of Ta or Nb gradually decreases from the lithium niobate single crystal thin film or the lithium tantalate single crystal thin film layer to the silicon single crystal thin film layer.

9. The composite single crystal thin film according to claim 1 or 2, wherein: The substrate is a silicon substrate, a lithium niobate substrate or a lithium tantalate substrate, and the thickness of the substrate is 0.1 mm to 1 mm.