Photomask blanks and photomasks

By using a light-shielding film containing molybdenum, silicon and nitrogen in the photomask blank to form a gradient layer structure, the pattern deterioration problem caused by the difference in etching rate of the light-shielding film in the photomask technology is solved, and high precision and stability are achieved. Photomask processing.

CN109212895BActive Publication Date: 2024-11-22SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201810683268.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-06-29
Filing Date
2018-06-28
Publication Date
2024-11-22
Estimated Expiration
2038-06-28

AI Technical Summary

Technical Problem

In lithography technology using 193nm ArF excimer laser, the difference in etching rate between the anti-reflection layer and the light-shielding layer of the MoSi-based light-shielding film results in deterioration of the cross-sectional shape and increase of roughness, making it difficult to maintain at high-precision nodes Pattern integrity.

Method used

A light-shielding film containing molybdenum, silicon and nitrogen is used to form a single or multi-layer constituent gradient layer structure to control the reflectivity and extinction coefficient of the exposed light to ensure the stability and fineness of the pattern shape in the etching process.

Benefits of technology

In the high-precision lithography process, the consistency of the etching rate of the light-shielding film and the integrity of the pattern shape are achieved, and the problems of deterioration of the mask pattern and increase reflectivity are avoided, and high-quality processing of the photomask is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109212895B_ABST
    Figure CN109212895B_ABST
Patent Text Reader

Abstract

The present invention relates to a photomask blank and a photomask. Specifically, it relates to a photomask blank for exposure light of ArF excimer laser, comprising: a transparent substrate and a light shielding film containing molybdenum, silicon and nitrogen. The light shielding film is formed into a single layer or a multilayer composed of a single composition layer or a composition gradient layer, the reflectivity of the light shielding film on the side away from the substrate is less than 40%, and the difference between the highest refractive index and the lowest refractive index at the surface of the substrate side and the side away from the substrate of all layers is less than 0.2, and the difference between the highest and lowest extinction coefficients at the surface is less than 0.5. The light shielding film presents a satisfactory and non-degraded cross-sectional shape of the mask pattern in the etching process or defect correction in mask processing.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This nonprovisional application claims priority under 35 U.S.C. §119(a) to Patent Application No. 2017-127637 filed in Japan on June 29, 2017, the entire contents of which are hereby incorporated herein by reference. Technical Field

[0003] The present invention relates to a photomask blank used as a material of a photomask for microfabrication of a semiconductor integrated circuit or the like, and to a photomask. Background Art

[0004] With respect to semiconductor integrated circuits for various purposes, in order to improve integration and reduce power consumption, more sophisticated circuit designs have been carried out. Therefore, in the photolithography technology using a photomask for forming a circuit, the development of micro-processing technology has developed from the 45nm node to the 32nm node, and then to the node below 20nm. In order to obtain a finer image, an exposure light source with a shorter wavelength has begun to be used, and in the most advanced actual processing technology at present, ArF excimer laser (193nm) is used for the exposure light source. Furthermore, in order to obtain a finer image, high-resolution technology is being developed, and liquid immersion exposure, deformation illumination, auxiliary patterns, etc. are used. With respect to the photomask used in photolithography, in addition to a binary photomask including a translucent portion and a light-shielding portion, as a phase-shift type photomask utilizing interference of light, a halftone phase-shift mask, a Levenson type phase-shift mask, a chrome-free type phase-shift mask, etc. have been developed.

[0005] A photomask blank used as a material of such a photomask is provided with an inorganic film, such as a light shielding film for shielding the exposure light and a phase shifting film for changing the phase of the exposure light, on a transparent substrate that transmits the exposure light. The photomask is prepared by patterning the inorganic film, such as the light shielding film and the phase shifting film, formed on the photomask blank. As the inorganic film, for example, as the light shielding film, a chromium-based film containing chromium or a molybdenum / silicon-based film containing molybdenum and silicon is generally used.

[0006] Reference List

[0007] Patent Document 1: JP-A 2012-32823 Summary of the invention

[0008] Typically, the MoSi-based light-shielding film includes an anti-reflection layer for reducing reflectivity and a light-shielding layer for ensuring a predetermined OD (optical density). In this case, in order to suppress the reflection of light in exposure using a mask, an anti-reflection layer with a high degree of oxidation or nitridation is provided on the light-shielding layer. However, in such an anti-reflection layer, the bonding performance of N, O and Si is high, so the layer has a slow etching rate. On the other hand, the light-shielding layer containing a large amount of unbonded Si has a fast etching rate. Therefore, when the stacked product of the two layers is etched, a level difference is generated between the two layers, and in an extreme example, an undercut is generated. Furthermore, when processing a transparent substrate, a difference in etching rate is generated between the anti-reflection layer and the light-shielding layer, so the cross-sectional shape of the mask pattern is degraded in the etching process in mask processing or defect correction.

[0009] In particular, in the generation of nodes below 20nm using 193nm ArF excimer laser, the roughness has a significant effect on the line width, for example, a difference in etching rate is generated at the interface between the anti-reflection layer and the light-shielding layer, so the cross-sectional shape of the mask pattern deteriorates and the roughness becomes larger. In extreme examples, if the anti-reflection layer is peeled off, the problem of not obtaining the desired pattern arises. At the same time, from the perspective of mask processing or exposure, a thinner film is preferred. However, if the film is thinned, the reflectivity increases to increase the influence of reflected light in exposure, so it is necessary to suppress the reflectivity to some extent.

[0010] An object of the present invention is to provide a photomask blank and a photomask having a MoSi-based light-shielding film which ensures necessary reflectivity and has a cross-sectional shape of a mask pattern which is satisfactory and does not deteriorate in an etching process in mask processing or defect correction.

[0011] The inventors have found that in a photomask blank including a transparent substrate and a light-shielding film and in which exposure light is ArF excimer laser, in a configuration in which the light-shielding film contains molybdenum, silicon and nitrogen and the reflectivity of the light-shielding film on the side away from the substrate with respect to the exposure light is 40% or less, the light-shielding film is formed into a single layer or a multilayer consisting of two or more layers, the layer consisting of a single composition layer having a constant composition in the thickness direction or a composition gradient layer having a composition continuously changing in the thickness direction, and in a case in which the light-shielding film is a single layer consisting of a composition gradient layer having a composition continuously changing in the thickness direction, the surface on the substrate side and the surface on the side away from the substrate are The difference in refractive index n for the exposure light between the surface on the substrate side and the surface on the side away from the substrate is 0.2 or less, and the difference in extinction coefficient k for the exposure light between the surface on the substrate side and the surface on the side away from the substrate is 0.5 or less. On the other hand, when the light-shielding film is a multilayer, the difference between the highest refractive index n and the lowest refractive index n for the exposure light at the surface on the substrate side and the surface on the side away from the substrate of all the layers of the multilayer is 0.2 or less, and the difference between the highest extinction coefficient k and the lowest extinction coefficient k for the exposure light at the surface on the substrate side and the surface on the side away from the substrate of all the layers of the multilayer is 0.5 or less. Thus, a photomask blank and a photomask having a MoSi-based light-shielding film having a satisfactory and non-degraded cross-sectional shape of a mask pattern in a mask processing or an etching process for defect correction can be provided, and the present invention is completed.

[0012] In one aspect, the present invention provides a photomask blank comprising:

[0013] a transparent substrate; and

[0014] A light-shielding film containing molybdenum, silicon and nitrogen, wherein

[0015] The exposure light is ArF excimer laser,

[0016] The light shielding film is formed into a single layer or a multilayer composed of two or more layers, the layer consisting of a single composition layer having a constant composition in the thickness direction or a composition gradient layer having a composition that continuously changes in the thickness direction,

[0017] The reflectivity of the light shielding film on the side away from the substrate to the exposure light is 40% or less,

[0018] In the case where the light-shielding film is a single layer composed of a composition gradient layer whose composition changes continuously in the thickness direction, the difference in refractive index n with respect to the exposure light between the surface on the substrate side and the surface on the side away from the substrate is 0.2 or less, and the difference in extinction coefficient k with respect to the exposure light between the surface on the substrate side and the surface on the side away from the substrate is 0.5 or less, and

[0019] In the case where the light-shielding film is a multilayer, among the refractive indices n for the exposure light at the surface on the substrate side of all the layers of the multilayer and the surface on the side away from the substrate, the difference between the highest refractive index n and the lowest refractive index n is less than 0.2, and among the extinction coefficients k for the exposure light at the surface on the substrate side of all the layers of the multilayer and the surface on the side away from the substrate, the difference between the highest extinction coefficient k and the lowest extinction coefficient k is less than 0.5.

[0020] In a preferred embodiment, the shading film is a single layer composed of a single composition layer with a constant composition in the thickness direction, the refractive index n of the shading film for the exposure light is less than 2.3 and the extinction coefficient k for the exposure light is greater than 1.3, and the thickness of the shading film is less than 80nm.

[0021] In a preferred embodiment, the light shielding film is a single layer composed of a composition gradient layer whose composition changes continuously in the thickness direction, in which the refractive index n at the surface on the substrate side is lower than the refractive index n at the surface on the side away from the substrate, and the extinction coefficient k at the surface on the substrate side is higher than the extinction coefficient k at the surface on the side away from the substrate. Typically, the refractive index n of the light shielding film for the exposure light is 2.3 or less and the extinction coefficient k for the exposure light is 1.3 or more, and the thickness of the light shielding film is 80 nm or less.

[0022] In a preferred embodiment, the light-shielding film is a multilayer, in which the refractive index n of the layer closest to the substrate is lower than the refractive index n of the layer farthest from the substrate, and the extinction coefficient k of the layer closest to the substrate is higher than the extinction coefficient k of the layer farthest from the substrate. Typically, i) the multilayer consists of only a single composition layer with a constant composition in the thickness direction, ii) in the light-shielding film, the refractive index n at the surface closest to the substrate is the lowest, and the layer closest to the substrate has the highest extinction coefficient k and has a thickness of 50 nm or less, or iii) the refractive index n is 2.3 or less and the extinction coefficient k is 1.3 or more, and the thickness of the light-shielding film is 80 nm or less.

[0023] In a preferred embodiment, in all compositions of the various layers of the light-shielding film, the total content of molybdenum and silicon is 55-75 atomic %, the content of nitrogen is 25-45 atomic %, and the ratio of molybdenum to the sum of molybdenum and silicon is less than 20 atomic %.

[0024] In a preferred embodiment, the light shielding film is formed in contact with the substrate and has an optical density OD of 2.8 or more relative to the wavelength of the exposure light, or the light shielding film is formed on the substrate (with one or more other films inserted), and the light shielding film and other films as a whole have an optical density OD of 2.8 or more relative to the wavelength of the exposure light. Typically, the other film includes only an etching stopper film having an etching characteristic different from that of the light shielding film, only a phase shift film having the same etching characteristic as that of the light shielding film, or both the etching stopper film and the phase shift film.

[0025] In a preferred embodiment, the photomask blank includes a hard mask film in contact with the light shielding film on a side away from the substrate, and the hard mask film has an etching characteristic different from that of the light shielding film.

[0026] In another aspect, the present invention provides a photomask prepared by using the photomask blank.

[0027] Advantageous Effects of the Invention

[0028] A photomask blank and a photomask having a MoSi-based light-shielding film which exhibits a cross-sectional shape of a mask pattern that is satisfactory and does not deteriorate in an etching process in mask processing or defect correction can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 FIG. 1 is a cross-sectional view showing an example of the photomask blank of the present invention.

[0030] Figure 2 FIG. 1 is a cross-sectional view showing another example of the photomask blank of the present invention. DETAILED DESCRIPTION

[0031] The photomask blank of the present invention comprises a transparent substrate (a substrate transparent to exposure light) and a light-shielding film containing molybdenum, silicon and nitrogen. The photomask blank and the photomask of the present invention use ArF excimer laser (wavelength 193nm) as exposure light (light for exposure using a photomask).

[0032] As the transparent substrate, although there is no particular limitation on the type and size of the substrate, a quartz substrate transparent to the wavelength used as the exposure wavelength is used, and for example, a 6-inch square and 0.25-inch thick transparent substrate called a 6025 substrate specified in the SEMI standard is preferably used. In SI units, a 6025 substrate is also written as a 152 mm square and 6.35 mm thick transparent substrate.

[0033] The light shielding film is composed of a single layer or multiple layers (e.g., 2-10 layers). Figure 1As shown in , a single-layer photomask blank specifically includes a transparent substrate 1 and a light-shielding film 2 formed on the transparent substrate 1, and a multi-layer photomask blank includes a transparent substrate 1 and a light-shielding film 2, and the light-shielding film 2 includes a first layer 21 and a second layer 22 formed on the transparent substrate 1 in sequence from the transparent substrate 1 side. In the case of a light-shielding film composed of a single layer, the light-shielding film may be a single composition layer having a constant composition in the thickness direction or a composition gradient layer having a composition that continuously changes in the thickness direction. Meanwhile, in the case of a light-shielding film composed of a multilayer, the light-shielding film is composed of two or more layers selected from a single composition layer having a constant composition in the thickness direction and a composition gradient layer having a composition that continuously changes in the thickness direction, and may be any one of a combination of only a single composition layer, a combination of only a composition gradient layer, and a combination of a single composition layer and a composition gradient layer. The composition gradient layer may be a layer in which the constituent elements increase or decrease in the thickness direction, but from the viewpoint of reducing the reflectivity of the light-shielding film on the side away from the transparent substrate for the exposure light, a composition gradient in which the nitrogen content increases in the direction away from the transparent substrate is preferred.

[0034] The light shielding film contains molybdenum, silicon and nitrogen. The material of the light shielding film specifically includes molybdenum silicon nitride (MoSiN) composed of molybdenum, silicon and nitrogen, molybdenum silicon nitrogen compounds composed of molybdenum, silicon, nitrogen and one or both of oxygen and carbon such as molybdenum silicon oxynitride (MoSiNO), molybdenum silicon nitride carbide (MoSiNC), and transition metal silicon oxynitride carbide (MoSiNOC).

[0035] In any composition of each layer of the light-shielding film, the total content of molybdenum and silicon is preferably 55 atomic % or more, particularly 60 atomic % or more and 75 atomic % or less, particularly 70 atomic % or less. In addition, in any composition of each layer of the light-shielding film, the content of nitrogen is preferably 25 atomic % or more, particularly 28 atomic % or more, particularly 30 atomic % or more and 45 atomic % or less, particularly 35 atomic % or less. In addition, in any composition of each layer of the light-shielding film, the ratio of molybdenum to the sum of molybdenum and silicon is preferably 20 atomic % or less, particularly 18 atomic % or less. The ratio of molybdenum to the sum of molybdenum and silicon is usually 10 atomic % or more.

[0036] The reflectivity of the light-shielding film on the side away from the transparent substrate to the exposure light is 40% or less, and the reflectivity is preferably 38% or less, particularly 35% or less. In the light-shielding film of the present invention, in particular, the nitrogen content is increased, thereby suppressing the reflectivity of the light-shielding film on the side away from the transparent substrate to the exposure light to 40% or less, particularly 38% or less, particularly 35% or less, while ensuring the optical density OD (which is the light-shielding performance required for the photomask blank) and preventing the generation of ghost patterns. In addition, the content ratio of molybdenum is reduced to improve environmental resistance, washability and laser irradiation resistance.

[0037] In the case where the light-shielding film is composed of a single layer, in the layer, or in the case where the light-shielding film is composed of multiple layers, in any of these layers, the refractive index of the light-shielding film for exposure light is preferably 2.3 or less, especially 2.2 or less. In the case where the light-shielding film is composed of a single layer, in the layer, or in the case where the light-shielding film is composed of multiple layers, in any of these layers, the extinction coefficient k of the light-shielding film for exposure light is preferably 1.3 or more, especially 1.5 or more. As the refractive index decreases, the reflectivity can be further reduced, and as the extinction coefficient k increases, the optical density OD per unit film thickness can be increased, that is, the film thickness can be further reduced. Regarding the thickness of the light-shielding film (the thickness of the entire light-shielding film), considering reducing the three-dimensional effect and shortening the time required for pattern formation, the thinner the better, and the thickness is preferably 80nm or less, more preferably 60nm or less. There is no particular restriction on the thickness of the light-shielding film (the thickness of the entire light-shielding film), but it is usually 40nm or more.

[0038] In the case where the light-shielding film is a single layer composed of a single composition layer having a constant composition in the thickness direction, it is advantageous in that the cross-sectional shape of the mask pattern after etching is satisfactory. At the same time, the light-shielding film can be formed as a single layer composed of a composition gradient layer having a composition that continuously changes in the thickness direction, but from the viewpoint of ensuring a satisfactory cross-sectional shape of the mask pattern, since it is necessary to make the difference in etching rate in the thickness direction of the light-shielding film small, the difference in refractive index n for exposure light between the surface on the transparent substrate side and the surface on the side away from the transparent substrate is made 0.2 or less, preferably 0.1 or less, and the difference in extinction coefficient k for exposure light between the surface on the transparent substrate side and the surface on the side away from the transparent substrate is made 0.5 or less, preferably 0.2 or less.

[0039] In this case, it is preferred that the refractive index n at the surface on the transparent substrate side is lower than the refractive index n at the surface on the side away from the transparent substrate, and the extinction coefficient k at the surface on the transparent substrate side is higher than the extinction coefficient k at the surface on the side away from the transparent substrate.

[0040] In addition, the light-shielding film can be formed as a multilayer consisting of two or more layers selected from a single composition layer having a constant composition in the thickness direction and a composition gradient layer having a composition that continuously changes in the thickness direction, and in this case, from the viewpoint of ensuring a satisfactory cross-sectional shape of the mask pattern, since it is necessary to make the difference in etching rate in the thickness direction of the light-shielding film small, the difference between the highest refractive index n and the lowest refractive index n for exposure light at the surface on the transparent substrate side of all layers of the multilayer and the surface on the side away from the transparent substrate is made to be less than 0.2, preferably less than 0.1, and the difference between the highest extinction coefficient k and the lowest extinction coefficient k for exposure light at the surface on the transparent substrate side of all layers of the multilayer and the surface on the side away from the transparent substrate is made to be less than 0.5, preferably less than 0.2.

[0041] In this case, it is preferred that the refractive index n of the layer closest to the transparent substrate is lower than the refractive index n of the layer farthest from the transparent substrate, and the extinction coefficient k of the layer closest to the transparent substrate is higher than the extinction coefficient k of the layer farthest from the transparent substrate.

[0042] In the case where the light-shielding film is a multilayer, in particular, in the light-shielding film, the refractive index n is preferably the lowest at the surface on the side closest to the transparent substrate (that is, the surface of the layer on the side closest to the transparent substrate closest to the transparent substrate). In addition, the layer with the highest extinction coefficient k has a thickness of preferably 50 nm or less, particularly 30 nm or less, especially 10 nm or less and 2 nm or more. The layer with the highest extinction coefficient k is preferably arranged on the side closest to the transparent substrate, and this arrangement facilitates the detection of the etching endpoint. In the layer with the highest extinction coefficient k, for example, the molybdenum content can be made higher than that of other layers, preferably by 1 atomic % or more, more preferably by 5 atomic % or more.

[0043] The light-shielding film may be formed in contact with the transparent substrate or on the transparent substrate, with one or more other layers interposed therebetween. In the case where the light-shielding film is formed in contact with the transparent substrate, the optical density OD of the light-shielding film relative to the wavelength of the exposure light is preferably 2.8 or more, particularly 2.9 or more, and especially 3 or more. At the same time, when the light-shielding film is formed together with other films such as a phase shift film and an etching stopper film interposed between the light-shielding film and the transparent substrate, the overall optical density OD of the light-shielding film and other films (all other films formed between the transparent substrate and the light-shielding film) relative to the wavelength of the exposure light is preferably 2.8 or more, particularly 2.9 or more, and especially 3 or more.

[0044] It is preferred that each layer of the monolayer or multilayer of the light-shielding film be formed by a sputtering method (a film with excellent uniformity can be easily obtained by this method), and any method of DC sputtering and RF sputtering can be used. The target and sputtering gas are appropriately selected according to the layer structure or composition. As a target, a molybdenum target, a target containing silicon (such as a molybdenum silicide target, a silicon target, a silicon nitride target), and a target containing both silicon and silicon nitride can be used. The nitrogen content can be adjusted by using a nitrogen-containing gas as a reactive gas for the sputtering gas and by performing reactive sputtering (appropriately adjusting the amount introduced). As a reactive gas, specifically, nitrogen (N2 gas), nitrogen oxide gas (NO gas, N2O gas, NO2 gas), etc. can be used, and oxygen (O2 gas), carbon oxide gas (CO gas, CO2 gas), etc. can be further used as needed. Furthermore, for the sputtering gas, as a rare gas, an inert gas such as helium, neon and argon can be used, and for the inert gas, argon is suitable. The sputtering pressure is usually 0.01 Pa or more, particularly 0.03 Pa or more and 10 Pa or less, particularly 0.1 Pa or less.

[0045] The photomask blank of the present invention may be subjected to heat treatment, which is performed at a temperature higher than the temperature applied in the patterning step of preparing a photomask from the photomask blank, for example, 150° C. or higher, after the light-shielding film is formed. The atmosphere of the heat treatment may be an atmosphere of an inert gas, such as helium and argon, an oxygen-containing atmosphere, such as an oxygen atmosphere, or may be under vacuum.

[0046] In addition, in order to suppress the change in the film quality of the light-shielding film, a surface oxide layer can be provided as the outermost layer of the surface side (the side away from the transparent substrate) of the light-shielding film. The oxygen content of the surface oxide layer can be 20 atomic % or more, and can be 50 atomic % or more. As a method for forming a surface oxide layer, specifically, in addition to oxidation by atmospheric oxidation (natural oxidation), the method of active oxidation treatment may include, for example, a method of treating a film of a silicon-based material with ozone gas or ozone water, a method of heating to 300°C or more in an oxygen-containing atmosphere such as an oxygen atmosphere by oven heating, lamp annealing, laser heating, etc., or a method of forming an oxide film by sputtering, etc. The thickness of the surface oxide layer is preferably less than 10 nm, particularly less than 5 nm, and especially less than 3 nm, and generally a thickness of more than 1 nm ensures the effect as an oxide film. The surface oxide layer can be formed by increasing the amount of oxygen in the sputtering process, but in order to form a layer with fewer defects, it is preferably formed by the above-mentioned atmospheric oxidation or oxidation treatment.

[0047] A surface oxide layer is formed on the side of the light shielding film farthest from the transparent substrate. When the light shielding film is a single layer, the surface oxide layer is formed as a part of the side farthest from the transparent substrate. When the light shielding film is a multilayer, the surface oxide layer is formed as a part of the side farthest from the transparent substrate of the layer farthest from the transparent substrate. The surface oxide layer is formed as a part of the light shielding film, the thickness of the surface oxide layer is included in the thickness of the entire light shielding film, and the entire light shielding film is the object of the optical density OD. However, the surface oxide layer itself does not need to satisfy the characteristics of the layers other than the surface oxide layer, such as the composition, refractive index and extinction coefficient k described above.

[0048] In the case where the light-shielding film is formed in contact with the transparent substrate or in the case where the light-shielding film is formed on the transparent substrate and an etching stopper film is inserted between them, the photomask blank of the present invention can apply a binary type photomask blank. In the case where the light-shielding film is formed on the transparent substrate and a phase-shift film or an etching stopper film and a phase-shift film are inserted between them, the photomask blank can apply a phase-shift type photomask blank. In the case where the light-shielding film is formed on the transparent substrate and an etching stopper film and a phase-shift film are inserted between them as other films, they can be formed in the order of an etching stopper film and a phase-shift film or in the order of a phase-shift film and an etching stopper film starting from the transparent substrate. A binary type photomask (binary mask) and a phase-shift type photomask (phase-shift mask) can be prepared from a binary type photomask blank and a phase-shift type photomask blank, respectively.

[0049] Etching can be precisely controlled by forming an etching barrier film. The etching barrier film can be any film having etching characteristics different from those of the light shielding film, and is preferably a film that withstands fluorine-based dry etching using fluorine-based gases applied to etching of silicon-containing materials, and is formed by a material that can be etched by chlorine-based dry etching using oxygen-containing chlorine-based gases (chlorine-oxygen). As such a film, a film containing chromium materials is preferred. The etching barrier film can be composed of a single layer or multiple layers. Chromium-containing materials specifically include chromium metal and chromium compounds, such as chromium oxide (CrO), chromium nitride (CrN), chromium carbide (CrC), chromium oxynitride (CrON), chromium oxycarbide (CrOC), chromium nitride (CrNC) and chromium oxynitride carbide (CrONC).

[0050] In the case where the etching stopper film is a film composed of a chromium compound, the chromium content is preferably 30 atomic % or more, particularly 35 atomic % or more and less than 100 atomic %, particularly 99 atomic % or less, particularly 90 atomic % or less. The nitrogen content is preferably 50 atomic % or less, particularly 40 atomic % or less, preferably 1 atomic % or more. The oxygen content is preferably 60 atomic % or less, particularly 55 atomic % or less, preferably 1 atomic % or more. The carbon content is preferably 30 atomic % or less, particularly 20 atomic % or less, preferably 1 atomic % or more. In this case, the total content of chromium, oxygen, nitrogen and carbon is preferably 95 atomic % or more, particularly 99 atomic % or more, particularly 100 atomic %. The thickness of the etching stopper film is generally 1 nm or more, particularly 2 nm or more and 20 nm or less, particularly 10 nm or less. In addition, the etching stopper film can function as an etching stopper film for a transparent substrate, or also as an etching stopper film for a phase shift film.

[0051] There is no particular limitation on the transmittance of the phase shift film, and even if the transmittance is almost 100%, a halftone phase shift film (for example, a transmittance of 5-30% for exposure light) can be used. The phase shift film is preferably formed of a material having the same etching characteristics as the light shielding film, specifically, a material that can be etched by fluorine-based dry etching using a fluorine-based gas, and more preferably, a film formed of a material that withstands chlorine-based dry etching using a chlorine-based gas containing oxygen (chlorine-oxygen).

[0052] The phase shift film may be composed of a single layer or a multilayer. The phase shift film is preferably a film formed of a silicon-containing material, and the silicon-containing material includes, for example, a silicon-containing compound, for example, a silicon-containing compound containing silicon and one or more selected from oxygen and nitrogen, specifically silicon oxide (SiO), silicon nitride (SiN), silicon oxynitride (SiON), etc., and a transition metal silicon compound, for example, a transition metal silicon compound containing a transition metal (Me), silicon and one or more selected from oxygen, nitrogen and carbon, specifically transition metal silicon oxide (MeSiO), transition metal silicon nitride (MeSiN), transition metal silicon carbide (MeSiC), transition metal silicon oxynitride (MeSiON), transition metal silicon oxycarbide (MeSiOC), transition metal silicon nitrogen carbide (MeSiNC), transition metal silicon oxynitride carbide (MeSiONC), etc. Suitable transition metals (Me) include one or more selected from titanium (Ti), vanadium (V), cobalt (Co), nickel (Ni), zirconium (Zr), niobium (Nb), molybdenum (Mo), hafnium (Hf), tantalum (Ta) and tungsten (W). From the perspective of dry etching processability, molybdenum (Mo) is particularly preferred.

[0053] The thickness of the phase shift film is adjusted to a thickness that shifts the phase by a predetermined amount (usually 150° or more, particularly 170° or more and 200° or less, particularly 190° or less, and generally about 180°) relative to the exposure light when using a photomask. Specifically, the suitable thickness is, for example, 50 nm or more, particularly 60 nm or more and 100 nm or less, and particularly 80 nm or less.

[0054] The photomask blank of the present invention may have a hard mask film having an etching characteristic different from that of a light shielding film, which contacts the light shielding film on the side away from the transparent substrate. The hard mask film can make the resist film thinner and accurately form a finer pattern. The hard mask film is used as an auxiliary film in the etching of the light shielding film and contributes to the improvement of density dependence (reduction of load effect), etc. The hard mask film is preferably a film that is particularly resistant to fluorine-based dry etching using fluorine-based gases applied to etching of silicon-containing materials, and is formed by a material that can be etched by chlorine-based dry etching using oxygen-containing chlorine-based gases (chlorine-oxygen). As such a film, a film containing chromium material is preferably used. The hard mask film can be composed of a single layer or a multilayer. Chromium-containing materials specifically include chromium metal and chromium compounds, such as chromium oxide (CrO), chromium nitride (CrN), chromium carbide (CrC), chromium oxynitride (CrON), chromium oxycarbide (CrOC), chromium nitride (CrNC) and chromium oxynitride carbide (CrONC).

[0055] In the case where the hard mask film is a film composed of a chromium compound, the chromium content is preferably 30 atomic % or more, particularly 35 atomic % or more and less than 100 atomic %, particularly 99 atomic % or less, particularly 90 atomic % or less. The nitrogen content is preferably 50 atomic % or less, particularly 40 atomic % or less, preferably 1 atomic % or more. The oxygen content is preferably 60 atomic % or less, particularly 40 atomic % or less, preferably 1 atomic % or more. The carbon content is preferably 30 atomic % or less, particularly 20 atomic % or less, more preferably 1 atomic % or more. In this case, the total content of chromium, oxygen, nitrogen and carbon is preferably 95 atomic % or more, particularly 99 atomic % or more, particularly 100 atomic %. The thickness of the hard mask film is generally 1 nm or more, particularly 2 nm or more and 30 nm or less, particularly 20 nm or less. The hard mask film may be completely removed after the pattern of the light-shielding film is formed, or may be partially or completely left after the pattern is formed to function as a film for compensating for the light-shielding performance or as a conductive film. The photomask blank of the present invention may include both an etch stopper film and a hard mask film.

[0056] By using, for example, a chromium target or a target consisting of chromium and any one or more selected from oxygen, nitrogen and carbon, and a sputtering gas containing a rare gas (inert gas) such as helium, neon and argon, and appropriately adding a reactive gas selected from, for example, an oxygen-containing gas, a nitrogen-containing gas and a carbon-containing gas according to the composition of the film to be formed, a film composed of a chromium-containing material can be formed by reactive sputtering.

[0057] By using a target selected from, for example, a silicon target, a transition metal target, a transition metal silicon target, and a sputtering gas containing a rare gas (inert gas) such as helium, neon, and argon, and appropriately adding a reactive gas selected from, for example, an oxygen-containing gas, a nitrogen-containing gas, and a carbon-containing gas according to the composition of the film to be formed, a film composed of a silicon-containing material can be formed by reactive sputtering.

[0058] Phase-shift photomask blanks include, for example: a phase-shift photomask blank comprising a phase-shift film and a light-shielding film formed in sequence on a transparent substrate; a phase-shift photomask blank comprising a phase-shift film, a light-shielding film and a hard mask film formed in sequence on a transparent substrate; a phase-shift photomask blank comprising a phase-shift film, an etching stop film and a light-shielding film formed in sequence on a transparent substrate; and a phase-shift photomask blank comprising a phase-shift film, an etching stop film, a light-shielding film and a hard mask film formed in sequence on a transparent substrate.

[0059] The photomask of the present invention uses the photomask blank and can be prepared by conventional procedures. For example, in the case of a binary photomask, it can be prepared by the following process. First, a resist such as a chemically amplified resist is applied to a light-shielding film of a binary photomask blank in which a light-shielding film is formed on a transparent substrate in contact with the transparent substrate to form a resist film, and the resist film is drawn with an electron beam or the like, and then developed to form a predetermined resist pattern. Then, using the resist pattern as an etching mask, the light-shielding film is patterned by fluorine-based dry etching, and the resist pattern is removed by conventional procedures, thereby obtaining a binary photomask.

[0060] Example

[0061] The present invention will be specifically described below with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0062] Example 1

[0063] A 6025 quartz substrate of 152 mm square and 6.35 mm thick was installed in the chamber of the sputtering device, a MoSi target and a Si target were used as sputtering targets and argon gas and nitrogen (N2 gas) were used as sputtering gases, the power applied to the MoSi target was set to 150 W, the power applied to the Si target was set to 1,850 W, the flow rate of argon gas was set to 20 sccm, and the flow rate of nitrogen gas was set to 16 sccm, and a single-layer light-shielding film consisting of MoSiN and having a single composition layer with a constant composition in the thickness direction was formed. Thus, a binary photomask blank was obtained.

[0064] The light-shielding film had an optical density OD of 3.1 with respect to ArF excimer laser light, a film thickness of 54 nm, and in its composition, the contents of Si, Mo, and N were 62 atomic %, 8 atomic %, and 30 atomic %, respectively. In addition, with respect to ArF excimer laser light, the refractive index n was 1.7, the extinction coefficient k was 2.0, and the reflectivity on the side away from the quartz substrate was 37%. Next, the light-shielding film was etched in a defect correction device using XeF2 as an etching gas, so that the light-shielding film had a satisfactory cross-sectional shape without a roof-like portion that was not etched remaining on the outermost layer of the film.

[0065] Example 2

[0066] A 6025 quartz substrate of 152 mm square and 6.35 mm thick was installed in the chamber of the sputtering apparatus, a MoSi target and a Si target were used as sputtering targets and argon gas and nitrogen (N2 gas) were used as sputtering gases, the power applied to the MoSi target was set to 300 W, the power applied to the Si target was set to 1,850 W, the flow rate of the argon gas was set to 20 sccm, and the flow rate of the nitrogen gas was set to 16 sccm, a first layer (5 nm thick) of a single composition layer composed of MoSiN and having a constant composition in the thickness direction was formed, and then only the power applied to the MoSi target was changed to 150 W and a second layer (55 nm thick) of a single composition layer composed of MoSiN and having a constant composition in the thickness direction was formed to form a light-shielding film composed of two single composition layers each composed of MoSiN and having a constant composition in the thickness direction. Thus, a binary photomask blank was obtained.

[0067] The light-shielding film has an optical density OD of 3.2 with respect to ArF excimer laser light, a film thickness of 57 nm, and in the composition of the first layer, the contents of Si, Mo and N are 60 atomic %, 10 atomic % and 30 atomic %, respectively, and in the composition of the second layer, the contents of Si, Mo and N are 62 atomic %, 8 atomic % and 30 atomic %, respectively. In addition, with respect to ArF excimer laser light, the refractive index n is 1.7 in the first layer and the refractive index n is 1.7 in the second layer, the extinction coefficient k is 2.1 in the first layer and the extinction coefficient k is 1.9 in the second layer, and the reflectivity on the side away from the quartz substrate is 37%. Next, the light-shielding film is etched in a defect correction device using XeF2 as an etching gas, so that the light-shielding film has a satisfactory cross-sectional shape without a roof-like portion that is not etched remaining on the outermost layer of the film.

[0068] Comparative Example 1

[0069] A 6025 quartz substrate of 152 mm square and 6.35 mm thick was installed in the chamber of the sputtering apparatus, a MoSi target and a Si target were used as sputtering targets and argon gas and nitrogen gas (N2 gas) were used as sputtering gases, the power applied to the MoSi target was set to 575 W, the power applied to the Si target was set to 1,925 W, the flow rate of argon gas was set to 20 sccm, and the flow rate of nitrogen gas was set to 20 sccm, a first layer (42 nm thick) of a single composition layer composed of MoSiN and having a constant composition in the thickness direction was formed, then only the flow rate of nitrogen gas was changed to 70 sccm, and a second layer (18 nm thick) of a single composition layer composed of MoSiN and having a constant composition in the thickness direction was formed to form a light shielding film composed of two single composition layers each composed of MoSiN and having a constant composition in the thickness direction. Thus, a binary photomask blank was obtained.

[0070] The light-shielding film has an optical density OD of 3.1 with respect to ArF excimer laser light, a film thickness of 60 nm, and in the composition of the first layer, the contents of Si, Mo, and N are 56 atomic %, 17 atomic %, and 27 atomic %, respectively, and in the composition of the second layer, the contents of Si, Mo, and N are 46 atomic %, 10 atomic %, and 44 atomic %, respectively. In addition, with respect to ArF excimer laser light, the refractive index n in the first layer is 2.0 and the refractive index n in the second layer is 2.2, the extinction coefficient k in the first layer is 2.0 and the extinction coefficient k in the second layer is 0.94, and the reflectivity on the side away from the quartz substrate is 11%. Next, the light-shielding film is etched in a defect correction device using XeF2 as an etching gas, so that the light-shielding film has an eaves-like portion on the side of the second layer away from the quartz substrate and has a defective cross-sectional shape.

Claims

1. Photomask blanks, including: Transparent substrate; and A light shielding film comprising molybdenum, silicon and nitrogen, wherein The exposure light is ArF excimer laser, The light-shielding film is composed of a single layer, which is composed of a single composition layer having a constant composition in the thickness direction, The reflectivity of the shading film on the side away from the substrate for the exposure light is less than 40%, the refractive index n of the shading film for the exposure light is less than 2.3 and the extinction coefficient k for the exposure light is greater than 1.3, and the thickness of the shading film is less than 80nm.

2. The photomask blank according to claim 1, wherein in the light-shielding film, the total content of molybdenum and silicon is 55-75 atomic %, the content of nitrogen is 25-45 atomic %, and the ratio of molybdenum to the sum of molybdenum and silicon is 20 atomic % or less.

3. The photomask blank according to claim 1, wherein the light-shielding film is formed in contact with the substrate and has an optical density OD of 2.8 or more relative to the wavelength of the exposure light, or the light-shielding film is formed on the substrate and one or more other films are inserted, and the overall optical density OD of the light-shielding film and other films relative to the wavelength of the exposure light is 2.8 or more.

4. The photomask blank according to claim 3, wherein the other film includes only an etching stopper film having an etching characteristic different from that of the light shielding film, only a phase shift film having the same etching characteristic as that of the light shielding film, or both the etching stopper film and the phase shift film.

5. The photomask blank according to claim 1, comprising a hard mask film in contact with the light shielding film on a side remote from the substrate, and having an etching characteristic different from that of the light shielding film.

6. Photomask blanks, including: Transparent substrate; and A light shielding film comprising molybdenum, silicon and nitrogen, wherein The exposure light is ArF excimer laser, The light shielding film is composed of a single layer, the layer being composed of a composition gradient layer having a composition that changes continuously in the thickness direction, The reflectivity of the light shielding film on the side away from the substrate to the exposure light is 40% or less, In the light-shielding film, a difference in refractive index n with respect to the exposure light between the surface on the substrate side and the surface on the side away from the substrate is 0.2 or less, and a difference in extinction coefficient k with respect to the exposure light between the surface on the substrate side and the surface on the side away from the substrate is 0.5 or less, and In the light-shielding film, the refractive index n at the surface on the substrate side is lower than the refractive index n at the surface on the side away from the substrate, and the extinction coefficient k at the surface on the substrate side is higher than the extinction coefficient k at the surface on the side away from the substrate. 7 . The photomask blank according to claim 6 , wherein a refractive index n of the light-shielding film with respect to the exposure light is 2.3 or less, an extinction coefficient k of the light-shielding film with respect to the exposure light is 1.3 or more, and a thickness of the light-shielding film is 80 nm or less.

8. Photomask blanks, including: Transparent substrate; and A light shielding film comprising molybdenum, silicon and nitrogen, wherein The exposure light is ArF excimer laser, The light shielding film is formed into a multilayer composed of two or more layers, the layers being composed of a single composition layer having a constant composition in the thickness direction or a composition gradient layer having a composition that continuously changes in the thickness direction, The reflectivity of the light shielding film on the side away from the substrate to the exposure light is 40% or less, In the light-shielding film, among the refractive indices n at the substrate side surface and the surface on the side away from the substrate of all the layers of the multilayer with respect to the exposure light, the difference between the highest refractive index n and the lowest refractive index n is 0.2 or less, and among the extinction coefficients k at the substrate side surface and the surface on the side away from the substrate of all the layers of the multilayer with respect to the exposure light, the difference between the highest extinction coefficient k and the lowest extinction coefficient k is 0.5 or less, and In the light-shielding film, the refractive index n of the layer closest to the substrate is lower than the refractive index n of the layer farthest from the substrate, and the extinction coefficient k of the layer closest to the substrate is higher than the extinction coefficient k of the layer farthest from the substrate.

9. The photomask blank according to claim 8, wherein the multilayer consists of only a single composition layer having a constant composition in a thickness direction.

10. The photomask blank according to claim 8, wherein in the light-shielding film, a refractive index n is lowest at a face closest to the substrate, and a layer closest to the substrate has a highest extinction coefficient k and has a thickness of 50 nm or less.

11. The photomask blank according to claim 8, wherein in the multiple layers of the light-shielding film, any refractive index n of each layer is 2.3 or less and any extinction coefficient k of each layer is 1.3 or more, and the thickness of the light-shielding film is 80 nm or less.

12. A photomask manufactured by using the photomask blank according to claim 1.