Fiber skeleton impregnated material for rubber products and preparation and use method thereof

Through the combination of blocked isocyanate compound, water-based polyacrylate and rubber latex, the problem of insufficient environmental protection effect of fiber cord impregnated materials for rubber products in the existing technology is solved, achieving efficient environmental protection and adhesive performance, replacing the traditional Dip treatment by RFL method.

CN109371683BActive Publication Date: 2024-10-18江志平
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN201811087031.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-09-18
Publication Date
2024-10-18
Estimated Expiration
2038-09-18

AI Technical Summary

Technical Problem

The existing impregnating materials for fiber cords used in rubber products have insufficient environmental protection effects. They contain epoxy compounds that are harmful to the environment, and harmful chemicals such as resorcinol and formaldehyde are used, which affects the environment and human health.

Method used

A combination of blocked isocyanate compound, water-based polyacrylate and rubber latex is used for dipping treatment, avoiding the use of resorcinol, formaldehyde and epoxy resin. Through the combination of multi-functional isocyanate and water-based polyacrylate, a high cross-linking density is achieved of polymers to achieve good adhesive properties and environmental performance.

Benefits of technology

It has improved the environmental protection of the cord and reduced the harm to the environment. It has provided environmentally friendly impregnating materials and tires for organic fiber cords, improved the durability and adhesive performance of the cord, and replaced the traditional RFL impregnation method. deal with.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109371683B_ABST
    Figure CN109371683B_ABST
Patent Text Reader

Abstract

The invention discloses a fiber skeleton dipping material for rubber products and a preparation and use method thereof, and belongs to the technical field of rubber production. The invention contains a blocked isocyanate compound (A), a water-based polyacrylate (B) and a rubber latex (C). The dipping material of the invention is used to dip the cord, which can replace the RFL dipping process. The invention does not contain any one of resorcinol, formaldehyde or epoxy resin, thereby improving the environmental friendliness of the dipping material; and further provides an environmentally friendly dipping material adhesive for organic fiber cords, and a fiber skeleton material and tire using the same. The dipping material of the invention does not contain any one of resorcinol, formaldehyde or epoxy resin, thereby reducing the harm of the dipping material to the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a fiber skeleton impregnated material for rubber products and a preparation and use method thereof, belonging to the technical field of rubber production. The skeleton material of the organic fiber treated with the impregnated material and the rubber can achieve a good bonding effect. Background Art

[0002] The present invention relates to an adhesive composition for organic fiber cords (hereinafter, also referred to as "adhesive composition"), and a rubber skeleton material, tire and bonding method using the same. Specifically, it relates to an adhesive composition for organic fiber cords that does not contain resorcinol and formaldehyde, and has good adhesion and environment, especially working environment, and a rubber skeleton material, tire and bonding method using the same. So far, in the bonding of tire cords formed by polyester fibers and the like and tire rubber, an RFL (resorcinol-formaldehyde-latex) adhesive containing resorcinol, formaldehyde and rubber latex is used, and the bonding strength is ensured by thermal curing. RFL adhesive was invented by DuPont in 1938. RFL adhesive technology has good bonding effect and low cost, so it has been used since the invention of RFL technology. In addition, it is known that the bonding strength will be further improved by using a resorcinol-formaldehyde resin formed by condensing resorcinol and formaldehyde, or by pre-treating with an epoxy resin.

[0003] RFL adhesive technology has the advantages of stable structural characteristics and low cost, but RFL technology contains some chemicals that are harmful to the environment, among which resorcinol and formaldehyde are both chemicals with high risks to human and environmental health. Resorcinol is known to cause itching and rashes when it comes into contact with the skin, and is toxic to the liver and cardiovascular system; while formaldehyde is more toxic to human health than resorcinol; formaldehyde has the hazards of carcinogenicity and inducing gene mutations, that is, a small amount of formaldehyde can also cause irritation to the eyes, nose and throat. Therefore, with the rapid development of the economy and society, human awareness of environmental protection and their own health has gradually increased. Humans are eager to limit the use of high-risk chemicals and are increasingly eager to develop environmentally friendly alternatives to RFL technology to reduce environmental pollution and ensure people's health.

[0004] After searching, the name of the invention is: Adhesive composition for organic fiber cord, and rubber reinforcement material, tire and bonding method using the same (application number: 201080019100.9, application date: 2010.04.26). The patent provides an adhesive composition for organic fiber cord that does not contain resorcinol and formaldehyde, has good adhesion and environment, especially working environment, and a rubber reinforcement material, tire and bonding method using the same. An adhesive composition for organic fiber cord containing a (blocked) isocyanate compound and / or an amine curing agent (A), an epoxy compound (B), and a rubber latex (C), and a rubber reinforcement material, tire and bonding method using the same. The ratio of the mass a of the (blocked) isocyanate compound and / or the amine curing agent (A) to the mass b of the epoxy compound (B) (mass of the blocked) isocyanate compound and / or the amine curing agent / mass of the epoxy compound) a / b is greater than 0.1 and less than 30.

[0005] The invention is entitled: a cord impregnation solution free of formaldehyde and resorcinol and a method for producing the same (application number: 201580030320.4, application date: 2015.06.11). The method comprises the following steps: adding an acrylic polymer resin to water; adjusting the pH value, adding an epoxy resin to the composition; adding a polyisocyanate to the composition; and then adding latex to the composition; obtaining an impregnated material, which enables the organic fibers and rubber used in the production of cord reinforced rubber materials to bond to each other by providing an interface between the two materials, and is more environmentally friendly.

[0006] Japanese patent application JP 2011069020A (applicant: BRIEF SUNTON CO., LTD., application date: 2009-09-25) is prepared by mixing an acrylic resin, an epoxy compound, a latex and an epoxy curing agent, wherein isocyanate is not a main component of the dipping solution. Also, Japanese patent application JP 2012224962 A (applicant: BRIEF SUNTON CO., LTD., application date: 2011-04-20) discloses a formulation containing an epoxy resin, an amine curing agent, a blocked isocyanate, styrene-butadiene latex and styrene-butadiene-vinylpyridine latex. In addition, the impregnation solution of Japanese Patent Application JP 2013064037A (applicant: BRIEF SUTO CO., LTD., application date: 2009-09-25) is prepared by mixing a polyurethane resin having a blocked isocyanate group, an epoxy compound, an oxazoline functional polymer, polyethyleneimine, a copolymer containing maleic anhydride repeating units, and rubber latex.

[0007] Although the above-mentioned cord-reinforced rubber material does not contain formaldehyde in the impregnation solution, epoxy compounds are introduced into the components of the impregnation solution. Since epoxy compounds are harmful to the environment to a certain extent, the environmental protection effect of the above-mentioned solution needs to be improved. Summary of the invention

[0008] 1. Technical problem to be solved by the invention

[0009] The purpose of the present invention is to overcome the shortcomings of the prior art impregnation materials with poor environmental protection effects, and to provide a fiber skeleton impregnation material for rubber products and a preparation and use method thereof. The impregnation material of the present invention is used to impregnate the cord, which can reduce the harm to the environment.

[0010] Furthermore, an environmentally friendly impregnating material for organic fiber cords, and a carcass material and a tire using the same are provided, thereby reducing harm to the environment.

[0011] 2. Technical solution

[0012] In order to achieve the above object, the technical solution provided by the present invention is:

[0013] The fiber skeleton material dipping material for rubber products of the present invention contains a blocked isocyanate compound (A), a water-based polyacrylate (B) and a rubber latex (C).

[0014] Furthermore, it does not contain any of resorcinol, formaldehyde, or epoxy resin.

[0015] Furthermore, the dry weight percentage of the blocked isocyanate compound (A) is 5-25%, and the dry weight percentage of the waterborne polyacrylate (B) is 0.01%-5%.

[0016] Furthermore, the blocked isocyanate compound (A) is a multifunctional isocyanate blocked by a blocking agent, wherein the number of functional groups of the multifunctional isocyanate is n, and n≥2.

[0017] Furthermore, the blocked isocyanate compound (A) is a mixture of one or more substances of crude MDI, MDI or TDI or HDI and its prepolymer or dimer or trimer, NDI or IPDI and its prepolymer or dimer or trimer blocked by a blocking agent, wherein the blocking agent is a mixture of one or more substances of caprolactam, phenol or oxime; the water-based polyacrylate (B) is a mixture of one or more substances of a copolymer or polymer of acrylic acid, a copolymer or polymer of methacrylic acid / ester / salt / amide; and the rubber latex (C) is a vinylpyridine-styrene-butadiene copolymer latex.

[0018] Furthermore, an alkaline solution (D) is also included.

[0019] Furthermore, the mass percentage of the blocked isocyanate compound (A) is 10-20%, and the mass percentage of the waterborne polyacrylate (B) is 0.01%-2%.

[0020] Furthermore, the number of functional groups of the multifunctional isocyanate is n, where n>2.

[0021] Furthermore, the alkaline solution (D) is aqueous ammonia, and the ratio of the dry weight of the aqueous polyacrylate (B) to the weight of the effective component of the alkaline solution (D) is B / D, and the value of B / D is 0.1 to 2.0.

[0022] Furthermore, the blocked isocyanate compound (A) is formed by blocking a multifunctional isocyanate monomer or a multifunctional prepolymer obtained by prepolymerization of a difunctional isocyanate.

[0023] Furthermore, the ratio of the dry weight of the aqueous polyacrylate (B) to the dry weight of the rubber latex (C) is B / C, and the value of B / C is 0.01% to 6.0%.

[0024] The method for preparing a fiber skeleton dipping material for rubber products of the present invention is characterized in that the dipping material is mixed and stirred with water to obtain the dipping material.

[0025] Furthermore, the alkaline solution, the water-based polyacrylate (B) and the blocked isocyanate compound (A) are mixed and stirred, and then the rubber latex (C) is added to the mixture and mixed and stirred to obtain the dipping material.

[0026] Furthermore, the alkaline solution and the polyacrylic acid emulsion (B) are mixed and stirred; the blocked isocyanate compound (A) is added and mixed and stirred, and then the rubber latex (C) is added and mixed and stirred to obtain the dipping material.

[0027] Furthermore, the rubber latex (C) is butylpyrrolidone latex, and after the butylpyrrolidone latex is added and mixed and stirred, an aging treatment is performed, and the aging treatment temperature is 5 to 35°C.

[0028] The invention discloses a method for dipping a fiber skeleton material for rubber products. The cord is treated with dipping by using the dipping material.

[0029] Furthermore, in the two-bath process: after the cord is treated with a first bath of dipping, the above-mentioned dipping material is treated with a second bath of dipping.

[0030] The fiber skeleton material for rubber products of the present invention is an organic fiber skeleton material which is treated by dipping in the above-mentioned dipping material.

[0031] A tire of the present invention is prepared using the above-mentioned fiber skeleton material for rubber products.

[0032] 3. Beneficial effects

[0033] Compared with the existing known technologies, the technical solution provided by the present invention has the following significant effects:

[0034] (1) A fiber skeleton dipping material for rubber products of the present invention and a preparation method thereof, wherein a blocked isocyanate compound (A), an aqueous polyacrylate (B) and a rubber latex (C) are mixed and stirred with water to obtain a dipping material, wherein the dipping material has excellent environmental performance, and at the same time, the H extraction of the cord treated with the dipping material is about 200N, which can replace the RFL dipping treatment, and the dipping material reduces the harm to the environment while ensuring that the cord has good durability;

[0035] (2) A fiber skeleton dipping material for rubber products of the present invention does not contain any of resorcinol, formaldehyde or epoxy resin, thereby improving the environmental friendliness of the dipping material; further providing an environmentally friendly dipping material for organic fiber cords, and a fiber skeleton material for rubber products and a tire using the same;

[0036] (3) In a fiber skeleton dipping material for rubber products of the present invention, the dry weight ratio of the water-based polyacrylate (B) to the dry weight ratio of the rubber latex (C) is B / C, and the value of B / C is 0.01% to 6.0%. While ensuring the stability of the dipping material, the rate of the competitive / substitution reaction of the chemical reaction in the dipping material is ensured, thereby forming appropriate bonds and cross-linking networks, so that the dipping material can achieve good cross-linking density and bonding performance;

[0037] (4) A method for dipping a fiber skeleton material for a rubber product of the present invention, wherein the cord is dipped with the above-mentioned dipping material, wherein the dipping material comprises a blocked isocyanate compound (A), an aqueous polyacrylate (B) and a rubber latex (C), and the H extraction of the cord after dipping is about 200N, which can replace the RFL dipping process and reduce the environmental hazards of the dipping process;

[0038] (5) A fiber skeleton material for rubber products of the present invention, wherein the organic fiber skeleton material is treated with the above-mentioned dipping material for dipping, wherein the dipping material comprises a blocked isocyanate compound (A), an aqueous polyacrylate (B) and a rubber latex (C), the preparation process of the fiber skeleton material is more environmentally friendly, and the fiber skeleton material has excellent durability;

[0039] (6) A tire of the present invention is prepared using the above-mentioned fiber skeleton material for rubber products. Since the tire uses the above-mentioned high-durability rubber skeleton material, the service life of the tire is increased. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 The present invention is a flow chart of a method for preparing a fiber skeleton impregnated material for rubber products. DETAILED DESCRIPTION

[0041] The following detailed description of exemplary embodiments of the present invention refers to the accompanying drawings. Although these exemplary embodiments are described in sufficient detail to enable those skilled in the art to implement the present invention, it should be understood that other embodiments may be implemented and various changes may be made to the present invention without departing from the spirit and scope of the present invention. The following more detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but is merely for illustration and does not limit the description of the features and characteristics of the present invention, in order to propose the best way to perform the present invention and to enable those skilled in the art to implement the present invention. Therefore, the scope of the present invention is limited only by the appended claims.

[0042] A fiber skeleton dipping material for rubber products of the present invention contains a blocked isocyanate compound (A), a water-based polyacrylate (B) and a rubber latex (C). The dipping material does not contain any of resorcinol, formaldehyde or epoxy resin, thereby reducing toxic chemical raw materials. The dry weight percentage of the blocked isocyanate compound (A) is 5-25%, and the dry weight percentage of the water-based polyacrylate (B) is 0.01%-5%; preferably, the mass percentage of the blocked isocyanate compound (A) is 10-20%, and the mass percentage of the water-based polyacrylate (B) is 0.01%-2%. The blocked isocyanate compound (A) is a multifunctional isocyanate blocked by a blocking agent, wherein the number of functional groups of the multifunctional isocyanate is n, and n≥2.

[0043] The blocked isocyanate compound (A) is a mixture of one or more substances of crude MDI, MDI or TDI or HDI and its prepolymer or dimer or trimer, NDI or IPDI and its prepolymer or dimer or trimer blocked by a blocking agent, wherein the blocking agent is a mixture of one or more substances selected from the group consisting of caprolactam, phenols and oximes; the waterborne polyacrylate (B) is a mixture of one or more substances selected from the group consisting of a copolymer or polymer of acrylic acid, a copolymer or polymer of methacrylic acid / ester / salt / amide; and the rubber latex (C) is a vinylpyridine-styrene-butadiene copolymer latex.

[0044] The above-mentioned dipping material also includes an alkaline solution (D), which can be a mixture of one or more substances such as NaOH solution, KOH solution or ammonia water; and the ratio of the dry weight mass of the water-based polyacrylate (B) to the mass of the effective component of the alkaline solution (D) is B / D, and the value of B / D is 0.1-2.0. The ratio of the dry weight mass of the above-mentioned water-based polyacrylate (B) to the dry weight mass of the rubber latex (C) is B / C, and the value of B / C is 0.01%-6.0%, thereby ensuring the uniformity of the dipping material. If the B / C value of the dipping material is too small, the bonding effect of the dipping material will be reduced, and the dipping material will not reach the required crosslinking density, and the dipping material cannot be stably dipping; if the B / C value is too large, the stability of the dipping material will be reduced, and the latex will precipitate from the dipping material solution, making it difficult to evenly coat the dipping material composition on the organic fiber cord.

[0045] When determining the above-mentioned ratio range and limit range, the relative rate of the competitive reaction must be considered, such as the specific reaction conditions of waterborne polyacrylate and polyisocyanate, waterborne polyacrylate and latex, polyisocyanate and latex, etc., so that the reaction of this process is that most of the active components participate in more than one of the above reactions, and the stoichiometric requirements of each reaction depend on the rate of the competitive / substitution reaction, which determines the different types of bonds and cross-linked networks formed, thereby determining the final microstructure and bonding performance. Therefore, when setting the above-mentioned ratio range and limit range, a large number of experimental verifications have been carried out, and the relative reaction rates and cross-linking processes between the various components have been fully considered when setting, so that any change in the above-mentioned range and ratio may affect the bonding effect of the dipping material.

[0046] In order to achieve better effects, the number of functional groups of the multifunctional isocyanate of the present invention is n, n>2; and the blocked isocyanate compound (A) is a multifunctional isocyanate monomer or a multifunctional prepolymer obtained by prepolymerization of a difunctional isocyanate.

[0047] The present invention discloses a method for preparing a fiber skeleton material dipping material for rubber products, wherein the dipping material is mixed with water to obtain the dipping material. The detailed steps are: mixing an alkaline solution, an aqueous polyacrylate (B) and a blocked isocyanate compound (A) and stirring them together, and then adding rubber latex (C) to the mixture and stirring them together to obtain the dipping material. Alternatively, the steps are: mixing an alkaline solution and a polyacrylic acid emulsion (B); then adding a blocked isocyanate compound (A) and stirring them together, and then adding rubber latex (C) and stirring them together to obtain the dipping material. Then, after adding butylpyrrolidone latex (C) and stirring them together, an aging treatment is performed, and the aging treatment temperature is 5 to 35°C.

[0048] The invention discloses a method for dipping a fiber skeleton material for rubber products, which comprises dipping a cord with the above-mentioned dipping material. The dipping material of the invention is applicable to cords dipped in one bath in the prior art, and is also applicable to the second bath treatment of cords dipped in two baths in the prior art. For example, polyester and aramid need to be dipped in one bath first and then in two baths, i.e., two bath treatment. In the two bath treatment, after the cords are dipped in the first bath, the above-mentioned dipping material is used for the second bath dipping.

[0049] It is worth noting that the present invention is also applicable to the cords that require two-bath dipping in the prior art, and enables the cords that require two-bath dipping to achieve relatively good performance by only dipping once in the present dipping material.

[0050] The cord is made of organic fiber cord, which may be a thermoplastic material, such as polyamide, polyester, and rayon. The polyamide may be nylon 6.6, nylon 6, aramid, and the like.

[0051] The fiber skeleton material for rubber products of the present invention is an organic fiber skeleton material that is dipped with the above-mentioned dipping material to obtain a fiber skeleton material after dipping. After the organic fiber cord is dipped, an adhesive layer is formed on the surface of the organic fiber cord, and then the organic fiber cord is dried and heated. The organic fiber cord is then buried in unvulcanized rubber, and the rubber is vulcanized, and the organic fiber cord and the rubber are bonded by an adhesive composition for the organic fiber cord. The organic fiber covering material of the present invention uses the above-mentioned dipping material to form an adhesive layer, and the organic fiber cord and the rubber are bonded by an adhesive composition for the organic fiber cord.

[0052] A fiber skeleton material for rubber products of the present invention can be used for general rubber products. As a rubber component, there is no particular limitation. For example, in addition to natural rubber, conjugated diene synthetic rubbers such as polyisoprene rubber (IR), polybutadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), acrylonitrile-butadiene rubber (NBR), chloroprene rubber (CR), and butyl rubber (IIR) can also be cited. Further, ethylene-propylene copolymer rubber (EPM), ethylene-propylene-diene copolymer rubber (EPDM), polysiloxane rubber, etc. can be cited; among them, natural rubber and conjugated diene synthetic rubber are preferred. In addition, these rubber components can be used alone or in combination of two or more.

[0053] The rubber components may be appropriately combined with fillers such as carbon black, silicon dioxide, aluminum hydroxide, vulcanization accelerators, antioxidants, softeners, etc. commonly used in the rubber industry. Furthermore, the rubber skeleton material of the present invention may also be made into a composite with particles, fibers, cloth, etc. of various materials.

[0054] A tire of the present invention is prepared using the above-mentioned rubber skeleton material, and the rubber skeleton material is preferably used for the tire cord layer and belt reinforcement layer. The tire of the present invention uses the above-mentioned highly durable rubber skeleton material, so it has excellent durability and increased service life.

[0055] Example 1

[0056] A fiber skeleton material dipping material for rubber products of the present embodiment comprises a blocked isocyanate compound (A), an aqueous polyacrylate (B) and a rubber latex (C); and the dipping material does not contain any of resorcinol, formaldehyde or epoxy resin, thereby reducing the introduction of toxic chemical raw materials and further improving the environmental friendliness of the dipping material.

[0057] The blocked isocyanate compound (A) used in this embodiment is caprolactam blocked MDI, or the blocked isocyanate compound (A) is blocked MDI or TDI or HDI or NDI or IPDI; the water-based polyacrylate (B) used is polyacrylic acid emulsion, and the rubber latex (C) used is butyl pyrrolidone latex. The dipping material also includes an alkaline solution (D), and the alkaline solution (D) is ammonia water, wherein the mass of caprolactam blocked MDI (dry weight content 50%) is 24g, the mass of polyacrylic acid emulsion (dry weight content 30%) is 2g, and the mass of butyl pyrrolidone latex (dry weight content 40%) is 170g. The mass of ammonia water (concentration of 25%) is 8g. MDI is diphenylmethane diisocyanate, and the number of its functional groups is n, n=2.

[0058] In this embodiment, the dry weight percentage of the blocked isocyanate compound (A) is 14.89%, and the dry weight percentage of the water-based polyacrylate (B) is 0.74%. The ratio of the dry weight of the water-based polyacrylate (B) to the dry weight of the rubber latex (C) is B / C, and the value of B / C is 0.88%. And the ratio of the dry weight of the water-based polyacrylate (B) to the mass of the effective component of ammonia water is B / D, and the value of B / D is 0.3.

[0059] The present embodiment provides a method for preparing a fiber skeleton impregnated material for rubber products. 190 g of water, 8 g of ammonia water (concentration of 25%) and 2 g of polyacrylic acid emulsion (dry weight content of 30%) are mixed and stirred for 20 minutes; 24 g of caprolactam-blocked MDI (dry weight content of 50%) is added to the mixed solution, and the mixing and stirring is continued for 15 minutes; 170 g of butylpyrrolidone latex (dry weight content of 40%) is added, and the mixture is mixed and stirred for 15 minutes to obtain a mixed solution of the impregnated material, and then the mixed solution of the impregnated material is aged for 12 hours, wherein the temperature of the maturation treatment is 5 to 35°C; a solution of the impregnated material is obtained.

[0060] In the production process of the dipped polyester cord, the first bath dip treatment is first carried out, and then the first bath dip treatment is carried out, followed by drying and reaction, and then the second bath dip treatment is carried out, and then the second bath dip treatment is carried out, followed by suction, drying and reaction to obtain the dipped cord. Among them, in the dip method of a fiber skeleton material for rubber products of this embodiment, the specification of the polyester cord is 1500D / 2, and after the cord is dipped in the first bath, the second bath dip treatment is carried out using the above-mentioned dipping material.

[0061] (1) In the first bath dipping treatment, conventional blocked isocyanate and epoxy resin are used for dipping treatment;

[0062] (2) After the polyester cord is dipped in the first bath solution, it is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; then the polyester cord is dipped in the second bath solution for the second bath dipping treatment, and the second bath solution of this embodiment is a solution of the dipping material prepared as described above; after the second bath dipping treatment is completed, the polyester cord is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; a finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord, and the H extraction is measured to be 195.64N.

[0063] Comparative Example 1

[0064] The basic content of this comparative example is the same as that of Example 1, except that the dipping material of this comparative example does not contain polyacrylic acid emulsion, that is, the dipping material of this comparative example contains blocked isocyanate compound (A), rubber latex (C) and alkaline solution (D), but does not contain water-based polyacrylate (B), and the dosage of other reagents is the same as that of Example 1.

[0065] The preparation method of the dipping material of this comparative example is: mix 190g of water and 8g of ammonia water (concentration of 25%) and stir for 20min; then add 24g of caprolactam-blocked MDI (dry weight content of 50%) to the mixed solution, and continue mixing and stirring for 15min; then add 170g of butylpyrrolidone latex (dry weight content of 40%), mix and stir for 15min to obtain a mixed solution of the dipping material, and then mature the mixed solution of the dipping material for 12h to obtain a solution of the dipping material.

[0066] The dipping method of this comparative example is as follows:

[0067] (1) In the first bath, conventional blocked isocyanate and epoxy resin are used for dipping;

[0068] (2) After the polyester cord is treated with the first bath solution dipping, it is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; then the polyester cord is dipped in the second bath solution for the second bath dipping treatment, and the second bath solution of this comparative example is a solution of the dipping material prepared above (containing ammonia water, caprolactam-blocked MDI and butylpyrrolidone latex, but not containing water-based polyacrylate (B)); after the second bath dipping treatment, the polyester cord is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; a finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord, and the H extraction is measured to be 166.27N.

[0069] Comparative Example 2

[0070] The basic content of this comparative example is the same as that of Example 1, except that: this comparative example uses rosin (B1) instead of waterborne polyacrylate (B), the amount of rosin (B1, dry weight content is 40%) is 2g, and the amounts of other reagents are the same as those of Example 1. That is, the dipping material of this comparative example contains caprolactam-blocked MDI, rosin (dry weight content is 40%) and butylpyrrolidone latex. Water, rosin, ammonia water, caprolactam-blocked MDI and butylpyrrolidone latex are mixed and stirred to obtain a dipping material solution;

[0071] The dipping method of this comparative example is as follows:

[0072] (1) In the first bath dipping treatment, conventional blocked isocyanate and epoxy resin are used for dipping treatment;

[0073] (2) After the polyester cord is treated with the first bath solution dipping, it is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; then the polyester cord is dipped in the second bath solution for the second bath dipping treatment, and the second bath solution of this comparative example is a solution of the dipping material prepared above (comprising rosin, ammonia water, caprolactam-blocked MDI and butylpyrrolidone latex); after the second bath dipping treatment, the polyester cord is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; a finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord, and the H extraction is measured to be 156.42N.

[0074] Comparative Example 3

[0075] The basic content of this comparative example is the same as that of Example 1, except that: this comparative example uses polymaleic anhydride (B2) instead of waterborne polyacrylate (B), the amount of polymaleic anhydride (B2, dry weight content is 40%) is 2g, and the amounts of other reagents are the same as those of Example 1; that is, the dipping material of this comparative example contains caprolactam-blocked MDI, polymaleic anhydride (dry weight content is 40%) and butylpyrrolidone latex. Water, maleic anhydride, ammonia water, caprolactam-blocked MDI and butylpyrrolidone latex are mixed and stirred to obtain a dipping material solution;

[0076] The dipping method of this comparative example is as follows:

[0077] (1) In the first bath dipping treatment, conventional blocked isocyanate and epoxy resin are used for dipping treatment;

[0078] (2) After the polyester cord is dipped in the first bath solution, it is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; then the polyester cord is dipped in the second bath solution for the second bath dipping treatment, and the second bath solution of this comparative example is a solution of the dipping material prepared above (comprising polymaleic anhydride, ammonia water, caprolactam blocked MDI and butylpyrrolidone latex); after the second bath dipping treatment, the polyester cord is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; a finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord, and the H extraction is measured to be 153.23N.

[0079] Comparative Example 4

[0080] The basic contents of this comparative example are the same as those of Example 1, except that: this comparative example uses tragacanth resin (B3) instead of waterborne polyacrylate (B), the amount of tragacanth resin (B3, dry weight content is 100%) is 0.6 g, and the amounts of other reagents are the same as those of Example 1; that is, the dipping material of this comparative example contains caprolactam-blocked MDI, tragacanth resin and butylpyrrolidone latex. Water, tragacanth resin, ammonia water, caprolactam-blocked MDI and butylpyrrolidone latex are mixed and stirred to obtain a dipping material solution;

[0081] The dipping method of this comparative example is as follows:

[0082] (1) In the first bath, conventional blocked isocyanate and epoxy resin are used for dipping;

[0083] (2) After the polyester cord is treated with the first bath solution dipping, it is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; then the polyester cord is dipped in the second bath solution for the second bath dipping treatment, and the second bath solution of this comparative example is a solution of the dipping material prepared above (comprising tragacanth resin, ammonia water, caprolactam-blocked MDI and butylpyrrolidone latex); after the second bath dipping treatment, the polyester cord is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; a finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord, and the H extraction is measured to be 172.27N.

[0084] Comparative Example 5

[0085] The basic content of this comparative example is the same as that of Example 1, except that: polyvinyl alcohol (B4) is used instead of water-based polyacrylate (B), the amount of polyvinyl alcohol (B4) is 0.6 g (dry weight content is 100%), and the amounts of other reagents are the same as those of Example 1; that is, the dipping material of this comparative example contains caprolactam-blocked MDI, polyvinyl alcohol and butylpyrrolidone latex. Water, polyvinyl alcohol, ammonia water, caprolactam-blocked MDI and butylpyrrolidone latex are mixed and stirred to obtain a dipping material solution;

[0086] The dipping method of this comparative example is as follows:

[0087] (1) In the first bath, conventional blocked isocyanate and epoxy resin are used for dipping;

[0088] (2) After the polyester cord is treated with the first bath solution dipping, it is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; then the polyester cord is dipped in the second bath solution for the second bath dipping treatment, and the second bath solution of this comparative example is a solution of the dipping material prepared above (comprising polyvinyl alcohol, ammonia water, caprolactam-blocked MDI and butylpyrrolidone latex); after the second bath dipping treatment, the polyester cord is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; a finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord, and the H extraction is measured to be 155.56N.

[0089] Comparative Example 6

[0090] The basic content of this comparative example is the same as that of Example 1, except that: the dipping material of this comparative example is not subjected to aging treatment; that is, the preparation method of the dipping material of this comparative example is to mix and stir water, ammonia water and polyacrylic acid emulsion for 20 minutes; then add caprolactam-blocked MDI to the mixed solution, and continue to mix and stir for 15 minutes; then add butylpyrrolidone latex, mix and stir for 15 minutes to obtain a mixed solution of dipping material; obtain a solution of dipping material; it is worth noting that: the amount of reagents used is the same as that of Example 1.

[0091] The dipping method of this comparative example is as follows:

[0092] (1) In the first bath, conventional blocked isocyanate and epoxy resin are used for dipping;

[0093] (2) After the polyester cord is treated with the first bath solution for dipping, it is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; then the polyester cord is dipped in the second bath solution for the second bath dipping treatment, and the second bath solution of this comparative example is the solution of the dipping material prepared above (the solution of the dipping material that has not been aged); after the second bath dipping treatment is completed, the polyester cord is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; a finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord, and the H extraction is measured to be 180.99N.

[0094] Comparative Example 7

[0095] The basic content of this comparative example is the same as that of Example 1, except that the following differences exist: The dipping method of this comparative example is as follows:

[0096] The first bath dipping treatment is conventional blocked isocyanate and epoxy resin treatment;

[0097] The second bath uses RFL adhesive for dipping treatment; after the polyester cord is dipped in the first bath solution, it is dried at 160°C for 60s, and then heat-treated at 230°C for 60s; then the polyester cord is dipped in the second bath solution for the second bath dipping treatment, and the second bath solution of this comparative example is RFL adhesive solution; after the second bath dipping treatment is completed, the polyester cord is dried at 160°C for 60s, and then heat-treated at 230°C for 60s; the finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord. The measured H extraction is 205.18N.

[0098] By comparing Example 1 with Comparative Examples 1-7, it can be found that the solution prepared by first mixing the water-based polyacrylate (B) with ammonia water, then adding the blocked isocyanate compound (A), and then adding the rubber latex (C) is more stable, which greatly improves the stability of the solution, makes the solution less likely to stratify, and has better stability. The polyacrylate (B) can react with the fiber compound and the blocked isocyanate compound (A) to form a carboxyl group. The polyacrylate (B) can react with the chemical fiber itself, and the carboxyl group and the amide undergo a substitution reaction, which promotes chemical crosslinking and improves the bonding effect.

[0099] Polyester and aramid etc. need to be treated with a first bath of resin before being treated with a second bath of resin, which is a two-bath treatment process. This embodiment mainly focuses on the two-bath treatment process.

[0100] The blocked isocyanate compound (A) and the waterborne polyacrylate (B) form a high-strength polymer with a large crosslinking density. The present invention has found through long-term research that the H extraction of polymer materials such as rosin, polymaleic anhydride, tragacanth resin, and polyvinyl alcohol is low, and the effect of replacing the RFL dipping treatment is not achieved. However, a fiber skeleton dipping material for rubber products of the present invention includes a blocked isocyanate compound (A), a waterborne polyacrylate (B) and a rubber latex (C). The cord is dipped with the dipping material of the present invention, and the H extraction is measured to be 195.64N, which can replace the RFL dipping treatment.

[0101] Through many demonstrations, the applicant has not yet determined the reaction mechanism of the reaction. It may be believed that the reaction mechanism is as follows: the blocked isocyanate compound has the effect of increasing the crosslinking density of the adhesive composition. The present invention adopts a blocked isocyanate compound multifunctional isocyanate with a functional group number of n, n=2, and combines it with water-based polyacrylate (B). The ratio defined in the present invention can increase the crosslinking density of the bond, thereby improving the adhesion between the organic fiber cord and the adhesive composition; and overcomes the technical bias of the prior art, with outstanding substantial characteristics and significant progress.

[0102] The fiber skeleton dipping material for rubber products of the present invention comprises a blocked isocyanate compound (A), an aqueous polyacrylate (B) and a rubber latex (C). The dipping material of the present invention is used to dip a cord, which can replace the RFL dipping process and achieve substantially the same or better dipping effect. The present invention does not contain any one of resorcinol, formaldehyde or epoxy resin, thereby improving the environmental friendliness of the dipping material and reducing the harm to the environment. Furthermore, an adhesive composition for an organic fiber cord with good environment, a cord, a tire and a bonding method using the same are provided.

[0103] Example 2

[0104] The basic content of this embodiment is the same as that of embodiment 1, except that: the number of functional groups of the multifunctional isocyanate of the present invention in this embodiment is n, n>2; and the blocked isocyanate compound (A) is a multifunctional prepolymer obtained by prepolymerization of a multifunctional isocyanate monomer or a difunctional isocyanate, which can be a prepolymer or dimer or trimer of MDI, TDI or HDI, or a prepolymer or dimer or trimer of NDI or IPDI. The blocked isocyanate compound (A) in this embodiment is caprolactam-blocked PAPI, and the number of its functional groups is n, n=2.7.

[0105] That is, the blocked isocyanate compound (A) of the dipping material of this embodiment is caprolactam-blocked PAPI, the water-based polyacrylate (B) used is polyacrylic acid emulsion, and the rubber latex (C) used is butylpyrrolidone latex; PAPI can also be called crude MDI. The preparation method of the dipping material of this comparative example is: 190g of water, 8g of ammonia water (concentration of 25%) and 2g of polyacrylic acid emulsion (dry weight content of 30%) are mixed and stirred for 20min; then 24g of caprolactam-blocked PAPI (dry weight content of 50%) is added to the mixed solution, and the mixing and stirring is continued for 15min; then 170g of butylpyrrolidone latex (dry weight content of 40%) is added, and the mixing and stirring is continued for 15min to obtain a mixed solution of the dipping material, and then the mixed solution of the dipping material is subjected to a aging treatment for 12h, wherein the aging treatment temperature is 5-35°C; and a solution of the dipping material is obtained. The dipping method of this embodiment is as follows:

[0106] (1) In the first bath, conventional blocked isocyanate and epoxy resin are used for dipping;

[0107] (2) After the polyester cord is dipped in the first bath solution, it is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; then the polyester cord is dipped in the second bath solution for the second bath dipping treatment, and the second bath solution of this comparative example is a solution of the dipping material prepared above (the blocked isocyanate compound (A) is caprolactam blocked PAPI); after the second bath dipping treatment is completed, the polyester cord is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; a finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord, and the H extraction is measured to be 207.69N.

[0108] By comparing Example 2 with Comparative Example 7, it can be found that the blocked isocyanate compound (A) and the water-based polyacrylate (B) form a high-strength polymer with a large cross-linking density. A fiber skeleton dipping material for rubber products of the present invention comprises a blocked isocyanate compound (A), a water-based polyacrylate (B) and a rubber latex (C). The cord is dipped with the dipping material of the present invention. By using the blocked isocyanate compound (A) and the water-based polyacrylate (B) in the dipping material, the water-based polyacrylate (B) represents the main active component, which changes the final microstructure of the polymer network obtained after curing, that is, in the subsequent process of preparing the cord; the cross-linking density of the adhesive composition is improved, so that a good bonding effect is still maintained in the absence of an epoxy compound. The technical prejudice that those skilled in the art believe that it is difficult to achieve a good bonding effect without an epoxy compound in the prior art is broken. The RFL dipping process can be replaced and a better dipping effect can be achieved; and the harm to the environment is reduced, and the environmental friendliness of the dipping material binder is improved.

[0109] Example 3

[0110] The basic content of this embodiment is the same as that of embodiment 1, except that the functional group number of the multifunctional isocyanate of the present invention in this embodiment is n, where n>2; and the blocked isocyanate compound (A) is a multifunctional isocyanate monomer or a multifunctional prepolymer obtained by prepolymerization of a difunctional isocyanate. The blocked isocyanate compound (A) in this embodiment is a caprolactam-blocked HDI trimer. HDI is hexamethylene diisocyanate, and the functional group number is n, where n=3.

[0111] That is, the blocked isocyanate compound (A) of the dipping material of this embodiment is caprolactam-blocked HDI trimer, the water-based polyacrylate (B) used is polyacrylic acid emulsion, and the rubber latex (C) used is butylpyrrolidone latex. The preparation method of the dipping material of this comparative example is: mix 190g of water, 8g of ammonia water (concentration of 25%) and 2g of polyacrylic acid emulsion (dry weight content of 30%) for 20min; then add 24g of caprolactam-blocked HDI trimer (dry weight content of 50%) to the mixed solution, and continue mixing and stirring for 15min; then add 170g of butylpyrrolidone latex (dry weight content of 40%), mix and stir for 15min to obtain a mixed solution of the dipping material, and then mature the mixed solution of the dipping material for 12h, wherein the temperature of the maturation treatment is 5-35°C; to obtain a solution of the dipping material. The dipping method of this embodiment is as follows:

[0112] (1) In the first bath, conventional blocked isocyanate and epoxy resin are used for dipping;

[0113] (2) After the polyester cord is treated with the first bath solution, it is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; then the polyester cord is dipped in the second bath solution for the second bath dipping treatment, and the second bath solution of this comparative example is the solution of the dipping material prepared above (the blocked isocyanate compound (A) is caprolactam blocked TDI dimer); after the second bath dipping treatment is completed, the polyester cord is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; the finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord. The measured H extraction is 206.77N.

[0114] Example 4

[0115] The basic content of this embodiment is the same as that of embodiment 1, except that: the number of functional groups of the multifunctional isocyanate of the present invention in this embodiment is n, where n>2; and the blocked isocyanate compound (A) is a multifunctional isocyanate monomer or a multifunctional prepolymer obtained by prepolymerization of a difunctional isocyanate. The blocked isocyanate compound (A) in this embodiment is a caprolactam-blocked TDI trimer, and the number of functional groups is n, where n=3.

[0116] That is, the blocked isocyanate compound (A) of the dipping material of this embodiment is caprolactam-blocked TDI trimer, the water-based polyacrylate (B) used is polyacrylic acid emulsion, and the rubber latex (C) used is butylpyrrolidone latex. The preparation method of the dipping material of this comparative example is: 190g of water, 8g of ammonia water (concentration of 25%) and 2g of polyacrylic acid emulsion (dry weight content of 30%) are mixed and stirred for 20min; then 24g of caprolactam-blocked TDI trimer (dry weight content of 50%) is added to the mixed solution, and the mixing and stirring is continued for 15min; then 170g of butylpyrrolidone latex (dry weight content of 40%) is added, and the mixing and stirring is continued for 15min to obtain a mixed solution of the dipping material, and then the mixed solution of the dipping material is subjected to a aging treatment for 12h, wherein the aging treatment temperature is 5-35°C; and a solution of the dipping material is obtained. The dipping method of this embodiment is as follows:

[0117] (1) In the first bath, conventional blocked isocyanate and epoxy resin are used for dipping;

[0118] (2) After the polyester cord is treated with the first bath solution dipping, it is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; then the polyester cord is dipped in the second bath solution for the second bath dipping treatment, and the second bath solution of this comparative example is a solution of the dipping material prepared above (the blocked isocyanate compound (A) is caprolactam blocked TDI dimer); after the second bath dipping treatment, the polyester cord is dried at 160°C for 60 seconds, and then heat-treated at 230°C for 60 seconds; a finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord, and the H extraction is measured to be 208.05N.

[0119] Example 5

[0120] The basic content of this embodiment is the same as that of embodiment 1, except that: the blocked isocyanate compound (A) used in this embodiment is caprolactam blocked MDI, the water-based polyacrylate (B) used is polyacrylic acid emulsion, and the rubber latex (C) used is butyl pyrrolidone latex. The dipping material also includes an alkaline solution (D), which is ammonia water; wherein the mass of caprolactam blocked MDI (dry weight content 50%) is 15.2g, the mass of polyacrylic acid emulsion (dry weight content 30%) is 0.7g, the mass of butyl pyrrolidone latex (dry weight content 40%) is 170g, and the mass of ammonia water (concentration 25%) is 8g.

[0121] In this embodiment, the dry weight percentage of the blocked isocyanate compound (A) is 10.03%, and the dry weight percentage of the water-based polyacrylate (B) is 0.28%. The ratio of the dry weight of the water-based polyacrylate (B) to the dry weight of the rubber latex (C) is B / C, and the value of B / C is 0.31%. The ratio of the dry weight of the water-based polyacrylate (B) to the mass of the effective component of ammonia water is B / D, and the value of B / D is 0.11.

[0122] In the dipping method of a fiber skeleton material for rubber products of the present embodiment, the specification of the polyester cord is 1500D / 2. After the cord is treated by dipping in a first bath, the cord is treated by dipping in a second bath using the above-mentioned dipping material.

[0123] (1) In the first bath dipping treatment, conventional blocked isocyanate and epoxy resin are used for dipping treatment;

[0124] (2) After the polyester cord is treated with the first bath solution, it is dipped in the second bath solution for the second bath dipping treatment. The specific dipping process is the same as that in Example 1. The finished dipped cord is obtained. The national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord. The measured H extraction is N=198.24.

[0125] Example 6

[0126] The basic content of this embodiment is the same as that of embodiment 1, except that the following differences are present: the blocked isocyanate compound (A) used in this embodiment is caprolactam blocked MDI, the water-based polyacrylate (B) used is polyacrylic acid emulsion, and the rubber latex (C) used is butyl pyrrolidone latex. The dipping material also includes an alkaline solution (D), which is ammonia water, wherein the mass of caprolactam blocked MDI is 34.9 g (dry weight content 50%), the mass of polyacrylic acid emulsion (dry weight content 30%) is 5.8 g, and the mass of butyl pyrrolidone latex (dry weight content 40%) is 170 g. The mass of ammonia water (concentration is 25%) is 50 g.

[0127] In this embodiment, the dry weight percentage of the blocked isocyanate compound (A) is 20.01%, and the dry weight percentage of the water-based polyacrylate (B) is 2.00%. The ratio of the dry weight of the water-based polyacrylate (B) to the dry weight of the rubber latex (C) is B / C, and the value of B / C is 2.56%. The ratio of the dry weight of the water-based polyacrylate (B) to the mass of the effective component of ammonia water is B / D, and the value of B / D is 0.14.

[0128] In the dipping method of a fiber skeleton material for rubber products of the present embodiment, the specification of the polyester cord is 1500D / 2. After the cord is treated by dipping in a first bath, the cord is treated by dipping in a second bath using the above-mentioned dipping material.

[0129] (1) In the first bath dipping treatment, conventional blocked isocyanate and epoxy resin are used for dipping treatment;

[0130] (2) After the polyester cord is treated with the first bath solution, it is dipped in the second bath solution for the second bath dipping treatment. The specific dipping process is the same as that in Example 1. The finished dipped cord is obtained. The national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord. The measured H extraction is N=196.06.

[0131] Example 7

[0132] The basic content of this embodiment is the same as that of embodiment 1, except that the following differences are present: the blocked isocyanate compound (A) used in this embodiment is caprolactam blocked MDI, the water-based polyacrylate (B) used is polyacrylic acid emulsion, and the rubber latex (C) used is butyl pyrrolidone latex. The dipping material also includes an alkaline solution (D), which is ammonia water, wherein the mass of caprolactam blocked MDI is 7.2g (dry weight content 50%), the mass of polyacrylic acid emulsion (dry weight content 30%) is 0.03g, and the mass of butyl pyrrolidone latex (dry weight content 40%) is 170g. The mass of ammonia water (concentration is 25%) is 0.35g.

[0133] In this embodiment, the dry weight percentage of the blocked isocyanate compound (A) is 5.03%, and the dry weight percentage of the water-based polyacrylate (B) is 0.01%. The ratio of the dry weight of the water-based polyacrylate (B) to the dry weight of the rubber latex (C) is B / C, and the value of B / C is 0.01%. And the ratio of the dry weight of the water-based polyacrylate (B) to the mass of the effective component of ammonia water is B / D, and the value of B / D is 0.10.

[0134] In the dipping method of a fiber skeleton material for rubber products of the present embodiment, the specification of the polyester cord is 1500D / 2. After the cord is treated by dipping in a first bath, the cord is treated by dipping in a second bath using the above-mentioned dipping material.

[0135] (1) In the first bath dipping treatment, conventional blocked isocyanate and epoxy resin are used for dipping treatment;

[0136] (2) After the polyester cord is treated with the first bath solution, it is dipped in the second bath solution for the second bath dipping treatment. The specific dipping process is the same as that in Example 1. The finished dipped cord is obtained, and the bonding effect of the finished dipped cord is tested using the national standard for cord testing (GBT-2942-2009). The measured H extraction is N=192.71.

[0137] Example 8

[0138] The basic content of this embodiment is the same as that of Embodiment 1, except that the blocked isocyanate compound (A) of the dipping material of this embodiment is caprolactam-blocked PAPI, the water-based polyacrylate (B) used is polyacrylic acid emulsion, and the rubber latex (C) used is butylpyrrolidone latex; PAPI can also be called crude MDI, and the number of its functional groups is n, where n=2.7.

[0139] The preparation method of the dipping material of the present embodiment is: 190g of water, 8g of ammonia water (concentration of 25%) and 2g of polyacrylic acid emulsion (dry weight content of 30%) are mixed and stirred for 20min; then 24g of caprolactam-blocked PAPI (dry weight content of 50%) is added to the mixed solution, and the mixing and stirring is continued for 15min; then 170g of butylpyrrolidone latex (dry weight content of 40%) is added, and the mixture is mixed and stirred for 15min to obtain a mixed solution of the dipping material, and then the mixed solution of the dipping material is aged for 12h, wherein the temperature of the maturation treatment is 5-35°C; a solution of the dipping material is obtained.

[0140] The dipping method of this comparative example is as follows: the specification of the polyester cord is 1500D / 2, the cord is not pre-treated by dipping, and the cord is directly dipped in the solution of the above-mentioned dipping material; after the dipping treatment, the polyester cord is dried at 160°C for 60s, and then heat-treated at 230°C for 60s; the finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord. The H extraction is measured to be 169.29N.

[0141] Therefore, the cord wire that needs two-bath dipping can achieve good performance by using the dipping material of the present invention, even if the first dipping treatment is omitted and the dipping material is directly used for dipping treatment, so that the cord wire that originally needs two-bath dipping can achieve good results by only one dipping, thus breaking the technical prejudice of the prior art; it has an outstanding effect.

[0142] Comparative Example 8

[0143] The basic content of this comparative example is the same as that of Example 8, except that: RFL adhesive solution is used for dipping treatment; the polyester cord is dipped in RFL adhesive solution for dipping treatment; after the dipping treatment is completed, the polyester cord is dried at 160°C for 60s and heat-treated at 230°C for 60s; a finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord, and the H extraction is measured to be 76N.

[0144] By comparing Example 8 with Comparative Example 8, it can be found that directly using the solution of the dipping material of the present invention to dip the polyester cord once has an excellent dipping effect, and its H extraction is 169.29N, which is much greater than the dipping effect of using RFL for one-time dipping. Of course, for materials such as nylon that are only dipped in one bath, it also has excellent performance.

[0145] Example 9

[0146] The basic content of this embodiment is the same as that of embodiment 1, except that the following differences are present: the blocked isocyanate compound (A) used in this embodiment is caprolactam-blocked MDI, the water-based polyacrylate (B) used is polyacrylic acid emulsion, and the rubber latex (C) used is butyl pyrrolidone latex. The dipping material also includes an alkaline solution (D), which is ammonia water, wherein the mass of caprolactam-blocked MDI (dry weight content 50%) is 24g, the mass of polyacrylic acid emulsion (dry weight content 30%) is 2g, and the mass of butyl pyrrolidone latex (dry weight content 40%) is 170g. The mass of ammonia water (concentration 25%) is 8g.

[0147] The differences are as follows: This embodiment is directed to the dipping treatment of nylon (polyamide fiber) and rayon (artificial fiber) which are directly treated with one bath dipping in the prior art, that is, nylon and rayon are treated with the above-mentioned dipping materials.

[0148] In this embodiment, a rubber product fiber skeleton material dipping method is used. The specification of nylon is 1260 / 2. The nylon is directly dipped in the dipping material solution. The national standard (GBT-2942-2009) is used to detect the bonding effect of the finished dipped nylon. The H extraction is measured to be 158N.

[0149] Comparative Example 9

[0150] The basic content of this comparative example is the same as that of Example 9, except that: the nylon is dipped in the RFL adhesive solution, and the specification of the nylon is 1260 / 2; the nylon is dipped in the RFL adhesive solution for dipping, and after the dipping treatment, a finished dipped cord is obtained, and the national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped nylon, and the H extraction is measured to be 156N.

[0151] Example 10

[0152] The basic content of this embodiment is the same as that of embodiment 1, except that the following differences are present: the blocked isocyanate compound (A) used in this embodiment is caprolactam-blocked MDI, the water-based polyacrylate (B) used is polyacrylic acid emulsion, and the rubber latex (C) used is butyl pyrrolidone latex. The dipping material also includes an alkaline solution (D), which is ammonia water, wherein the mass of caprolactam-blocked MDI (dry weight content 50%) is 47.6g, the mass of polyacrylic acid emulsion (dry weight content 30%) is 11.3g, and the mass of butyl pyrrolidone latex (dry weight content 40%) is 170g. The mass of ammonia water (concentration is 25%) is 13g.

[0153] In this embodiment, the dry weight percentage of the blocked isocyanate compound (A) is 25.00%, and the dry weight percentage of the waterborne polyacrylate (B) is 3.56%. The ratio of the dry weight of the waterborne polyacrylate (B) to the dry weight of the rubber latex (C) is B / C, and the value of B / C is 4.99%. The ratio of the dry weight of the waterborne polyacrylate (B) to the mass of the effective component of ammonia water is B / D, and the value of B / D is 1.04.

[0154] In the dipping method of a fiber skeleton material for rubber products of the present embodiment, the specification of the polyester cord is 1500D / 2. After the cord is treated by dipping in a first bath, the cord is treated by dipping in a second bath using the above-mentioned dipping material.

[0155] (1) In the first bath dipping treatment, conventional blocked isocyanate and epoxy resin are used for dipping treatment;

[0156] (2) After the polyester cord is treated with the first bath solution, it is dipped in the second bath solution for the second bath dipping treatment. The specific dipping process is the same as that in Example 1. The finished dipped cord is obtained. The national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord. The measured H extraction is N=195.95.

[0157] Embodiment 11

[0158] The basic content of this embodiment is the same as that of embodiment 1, except that the following differences are present: the blocked isocyanate compound (A) used in this embodiment is caprolactam-blocked MDI, the water-based polyacrylate (B) used is polyacrylic acid emulsion, and the rubber latex (C) used is butyl pyrrolidone latex. The dipping material also includes an alkaline solution (D), which is ammonia water, wherein the mass of caprolactam-blocked MDI (dry weight content 50%) is 19g, the mass of polyacrylic acid emulsion (dry weight content 30%) is 13.6g, and the mass of butyl pyrrolidone latex (dry weight content 40%) is 170g. The mass of ammonia water (concentration is 25%) is 10.9g.

[0159] In this embodiment, the dry weight percentage of the blocked isocyanate compound (A) is 11.65%, and the dry weight percentage of the waterborne polyacrylate (B) is 5.00%. The ratio of the dry weight of the waterborne polyacrylate (B) to the dry weight of the rubber latex (C) is B / C, and the value of B / C is 6.00%. The ratio of the dry weight of the waterborne polyacrylate (B) to the mass of the effective component of ammonia water is B / D, and the value of B / D is 1.50.

[0160] In the dipping method of a fiber skeleton material for rubber products of the present embodiment, the specification of the polyester cord is 1500D / 2. After the cord is treated by dipping in a first bath, the cord is treated by dipping in a second bath using the above-mentioned dipping material.

[0161] (1) In the first bath dipping treatment, conventional blocked isocyanate and epoxy resin are used for dipping treatment;

[0162] (2) After the polyester cord is treated with the first bath solution, it is dipped in the second bath solution for the second bath dipping treatment. The specific dipping process is the same as that in Example 1. The finished dipped cord is obtained, and the bonding effect of the finished dipped cord is tested using the national standard for cord testing (GBT-2942-2009). The measured H extraction is N=197.23.

[0163] Example 12

[0164] The basic content of this embodiment is the same as that of embodiment 1, except that the following differences are present: the blocked isocyanate compound (A) used in this embodiment is caprolactam-blocked MDI, the water-based polyacrylate (B) used is polyacrylic acid emulsion, and the rubber latex (C) used is butyl pyrrolidone latex. The dipping material also includes an alkaline solution (D), which is ammonia water, wherein the mass of caprolactam-blocked MDI (dry weight content 50%) is 19g, the mass of polyacrylic acid emulsion (dry weight content 30%) is 13.6g, and the mass of butyl pyrrolidone latex (dry weight content 40%) is 170g. The mass of ammonia water (concentration is 25%) is 8.1g.

[0165] In this embodiment, the dry weight percentage of the blocked isocyanate compound (A) is 11.65%, and the dry weight percentage of the water-based polyacrylate (B) is 5.00%. The ratio of the dry weight of the water-based polyacrylate (B) to the dry weight of the rubber latex (C) is B / C, and the value of B / C is 6.00%. The ratio of the dry weight of the water-based polyacrylate (B) to the mass of the effective component of ammonia water is B / D, and the value of B / D is 2.01.

[0166] In the dipping method of a fiber skeleton material for rubber products of the present embodiment, the specification of the polyester cord is 1500D / 2. After the cord is treated by dipping in a first bath, the cord is treated by dipping in a second bath using the above-mentioned dipping material.

[0167] (1) In the first bath dipping treatment, conventional blocked isocyanate and epoxy resin are used for dipping treatment;

[0168] (2) After the polyester cord is treated with the first bath solution, it is treated with the second bath solution. The specific dipping process is the same as that in Example 1. The finished dipped cord is obtained. The national standard for cord testing (GBT-2942-2009) is used to test the bonding effect of the finished dipped cord. The measured H extraction is N=195.17.

[0169] Table 1 Proportions of Examples and Comparative Examples and H Extraction

[0170]

[0171]

[0172] The present invention has been described in detail above in conjunction with specific exemplary embodiments. However, it should be understood that various modifications and variations may be made without departing from the scope of the present invention as defined by the appended claims. The detailed description and the accompanying drawings should be considered only as illustrative and not restrictive, and if there are any such modifications and variations, they will fall within the scope of the present invention described herein. In addition, the background art is intended to illustrate the current status and significance of the research and development of the present technology and is not intended to limit the present invention or the application field of the present application and the present invention.

[0173] More specifically, although exemplary embodiments of the present invention have been described herein, the present invention is not limited to these embodiments, but includes any and all embodiments that are modified, omitted, combined (e.g., between various embodiments), adaptively changed and / or replaced as can be recognized by a person skilled in the art based on the foregoing detailed description, and the various embodiments of the present invention can be combined as needed. The limitations in the claims are to be interpreted broadly according to the language used in the claims and are not limited to the examples described in the foregoing detailed description or during the implementation of the application, which examples should be considered non-exclusive. Any steps listed in any method or process claim may be performed in any order and are not limited to the order set forth in the claim. Therefore, the scope of the present invention should be determined solely by the attached claims and their legal equivalents, rather than by the description and examples given above.

Claims

1. A fiber skeleton impregnated material for rubber products, characterized in that: It contains a blocked isocyanate compound A, a water-based polyacrylate B, a rubber latex C and an alkaline solution D; it does not contain any of resorcinol, formaldehyde or epoxy resin; the alkaline solution D is ammonia water, and the ratio of the dry weight of the water-based polyacrylate B to the weight of the effective component of the alkaline solution D is B / D, and the value of B / D is 0.1 to 2.0; The dry weight percentage of the blocked isocyanate compound A is 5 to 25%, and the dry weight percentage of the waterborne polyacrylate B is 0.01 to 5%; The ratio of the dry weight of the waterborne polyacrylate B to the dry weight of the rubber latex C is B / C, and the value of B / C is 0.01% to 6.0%.

2. The fiber skeleton impregnated material for rubber products according to claim 1, characterized in that: The blocked isocyanate compound A is a multifunctional isocyanate blocked by a blocking agent, wherein the number of functional groups of the multifunctional isocyanate is n, and n≥2.

3. The fiber skeleton impregnated material for rubber products according to claim 1, characterized in that: The blocked isocyanate compound A is a mixture of one or more substances of crude MDI, MDI or TDI or HDI and its prepolymers or dimers or trimers, NDI or IPDI and its prepolymers or dimers or trimers blocked by a blocking agent, wherein the blocking agent is a mixture of one or more substances selected from the group consisting of caprolactams, phenols and oximes; The water-based polyacrylate B is a copolymer or polymer of acrylic acid, a copolymer or polymer of methacrylic acid / ester / salt / amide, or a mixture of one or more substances; The rubber latex C is a vinylpyridine-styrene-butadiene copolymer latex.

4. The fiber skeleton impregnated material for rubber products according to claim 2, characterized in that: The mass percentage of the blocked isocyanate compound A is 10-20%, and the mass percentage of the waterborne polyacrylate B is 0.01%-2%.

5. The fiber skeleton impregnated material for rubber products according to claim 3, characterized in that: The number of functional groups of a multifunctional isocyanate is n, where n>2.

6. The fiber skeleton impregnated material for rubber products according to claim 4, characterized in that: The blocked isocyanate compound A is formed by blocking a multifunctional isocyanate monomer or a multifunctional prepolymer obtained by prepolymerization of a difunctional isocyanate.

7. A method for preparing a fiber skeleton impregnated material for rubber products, characterized in that: The impregnated material according to any one of claims 1 to 6 is mixed and stirred with water to obtain the impregnated material.

8. The method for preparing a fiber skeleton impregnated material for rubber products according to claim 7, characterized in that: The alkaline solution, water-based polyacrylate B and blocked isocyanate compound A are mixed and stirred, and then rubber latex C is added to the mixed solution and mixed and stirred to obtain a dipping material.

9. The method for preparing a fiber skeleton impregnated material for rubber products according to claim 7, characterized in that: The alkaline solution and water-based polyacrylate B are mixed and stirred; the blocked isocyanate compound A is then added and mixed and stirred, and then the rubber latex C is added and mixed and stirred to obtain the dipping material.

10. The method for preparing a fiber skeleton impregnated material for rubber products according to any one of claims 7 to 9, characterized in that: The rubber latex C is butylpyrrolidone latex. After the butylpyrrolidone latex is added and mixed and stirred, an aging treatment is performed. The aging treatment temperature is 5 to 35°C.

11. A method for dipping a fiber skeleton material for rubber products, characterized in that: The cord is dipped in the dipping material according to any one of claims 1 to 6.

12. The method for dipping a fiber skeleton material for rubber products according to claim 11, characterized in that: In the two-bath treatment, after the cord is treated with the first bath dipping treatment, the second bath dipping treatment is carried out using the dipping material described in any one of claims 1 to 6.

13. A fiber skeleton material for rubber products, characterized in that: The organic fiber skeleton material is impregnated with the impregnated material described in any one of claims 1 to 6.

14. A tire, characterized in that: The rubber product is prepared using the fiber skeleton material according to claim 13.

Citation Information

Patent Citations

  • Adhesive composition for organic fiber cords, rubber-reinforcing material using same, tire and bonding method

    CN102414362A

  • Adhesive composition for organic fiber cord, and rubber reinforcing material and tire as well as method of adhesion using the same

    JP2011069020A

  • Adhesive composition for organic fiber cord, and rubber reinforcing material, tire and adhering method using the same

    JP2012224962A

  • Adhesive composition for organic fiber cord, adhesive process using the composition, rubber-reinforcing member, and tire

    JP2013064037A

  • Closed isocyanate adhesive for gumming fiber framework materials of rubber products, composition of closed isocyanate adhesive, preparation method and application

    CN102634985A