Laminating film for liquid crystal display and liquid crystal display backlight module

By designing a multi-layer structure and composite adhesive layer in the liquid crystal display bonding film, combined with microstructure forming technology, the problem of difficulty in taking into account both brightness and shielding in the prior art is solved, and an efficient application of liquid crystal display backlight modules is achieved.

CN109597243BActive Publication Date: 2024-11-29CCS (SHANGHAI) FUNCTIONAL FILMS IND CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN201811610827.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-12-27
Publication Date
2024-11-29
Estimated Expiration
2038-12-27

AI Technical Summary

Technical Problem

The existing LCD display bonding film is difficult to take into account both brightness and shielding, and is prone to scratching, making it impossible to directly contact the LCD screen, resulting in high costs and limited application.

Method used

A bonding film structure consisting of the first and second structural layer films, wherein the first structural layer film includes a first prism layer and a back coating, and the second structural layer film includes a second prism layer and a composite adhesive layer, and a composite adhesive The layer contains PBMA or PMMA microbeads, which improves shielding and brightness through microstructure molding technology, and is in direct contact with the LCD screen.

Benefits of technology

It achieves improving shielding, avoiding interference and glare while ensuring brightness, and meeting scratch resistance requirements. It is suitable for large-size LCD displays, reducing production and assembly costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109597243B_ABST
    Figure CN109597243B_ABST
Patent Text Reader

Abstract

The present invention discloses a laminating film for a liquid crystal display and a liquid crystal display backlight module. The laminating film for a liquid crystal display comprises, from bottom to top: a first structural layer film and a second structural layer film, wherein the first structural layer film comprises a first base film, a first prism layer and a back coating layer, wherein the first prism layer is formed by a plurality of first prisms arranged continuously; the first prism layer is arranged on the upper surface of the first base film; the back coating layer is arranged on the lower surface of the first base film; the second structural layer film comprises a second base film and a second prism layer, wherein the second prism layer is formed by a plurality of second prisms arranged continuously; the second prism layer is arranged on the upper surface of the second base film; a composite adhesive layer is arranged on the lower surface of the second base film; the composite adhesive layer contains PBMA or PMMA microbeads; the first prism is laminated to the second base film through the composite adhesive layer. The present invention ensures that the brightness meets the requirements of liquid crystal display products, and the shielding property meets the requirements, ensuring that there is no interference and no glare, and the visual effect meets the standards.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a laminating film for a liquid crystal display and a backlight module of the liquid crystal display. Background Art

[0002] With the popularization of TFT-LCD liquid crystal display technology, the demand for its backlight module and related optical films is also increasing. The four-film structure of lower diffusion, 90-degree light enhancement, 0-degree light enhancement, and upper diffusion used before has been gradually replaced by three or even two films. With the increasing size of liquid crystals, the requirements for stiffness have become higher, the products have been continuously thinned, and the assembly lines have become more and more simplified. DOP (light enhancement + diffusion) laminating films and POP (light enhancement + light enhancement) laminating films have also appeared on the market. However, the existing technology is not suitable for the use of many high-resolution LCD screens due to the low brightness of DOP, which leads to limited application scope. The existing POP products have poor shielding, easy scratches, and cannot directly contact the LCD screen. The covering film must be added, such as diffusion, which leads to high product costs and also affects the brightness. The industry is eager to solve the problem of optical laminating films that can improve brightness and ensure shielding and adaptability to LCD screens.

[0003] One of the existing technical solutions for POP laminating films is to use two mutually perpendicular high-transmittance prisms to laminate together. Although the brightness is high, it is easy to interfere, has poor shielding and is not scratch-resistant. Therefore, a diffusion-type protective sheet must be added between the film and the LCD screen. In this way, the brightness is significantly reduced. In addition, the scratch resistance and poor shielding lead to a decrease in production and assembly yield, which ultimately leads to high costs and cannot be widely used.

[0004] Another solution is to add protective films on the front and back and top and bottom of the two structural layers of the POP prism to solve the problem of easy scratches in the process and improve the production and assembly yield. However, due to poor anti-interference properties, it is still impossible to directly contact the LCD screen, and it is still necessary to add a diffusion-type protective film between the LCD screens. In addition, adding a protective film will also increase the process cost, so the cost of the entire solution is still relatively high and the fundamental problem has not been solved.

[0005] The third solution is to use a single-layer film. In order to save costs, two brightening methods are used: the lower brightening is mostly (high transmittance or high fog) brightening, and the upper brightening generally uses small pitch (16-25 microns) brightening to solve the interference problem. When cutting such small pitch brightening, it is necessary to turn different angles according to the matching with the LCD screen, generally 3-8 degrees, which not only increases material loss and causes cost increase, but also replaces the LCD screen to verify the matching work cumbersome, lengthens the introduction cycle and cost; in addition, due to the small structure and low brightness, the small pitch brightening needs to use high refractive index resin to improve the brightness, which leads to cost increase, and due to the small structure and poor scratch resistance of the small pitch, the production and assembly yield is low; in addition, a single brightening film, especially the small pitch brightening product that contacts the LCD screen above, has poor shielding and can be clearly seen with a slight deformation; and when applied to large sizes, the single film is not stiff enough and is prone to wrinkles, which is limited for large-size applications; in addition, cutting and assembling the two films separately will increase the risk of process defects, and the rework rate will increase, resulting in increased losses. Summary of the invention

[0006] The purpose of the present invention is to overcome the deficiencies in the prior art and to provide a laminating film for a liquid crystal display and a liquid crystal display backlight module with good shielding properties.

[0007] To achieve the above object, the present invention is implemented through the following technical solutions:

[0008] The laminating film for liquid crystal display is characterized by comprising, from bottom to top:

[0009] A first structural layer film, the first structural layer film comprising a first base film, a first prism layer and a back coating layer, the first prism layer is formed by a plurality of first prisms arranged continuously; the first prism layer is arranged on the upper surface of the first base film; the back coating layer is arranged on the lower surface of the first base film;

[0010] A second structural layer film, wherein the second structural layer film comprises a second base film and a second prism layer, wherein the second prism layer is formed by a plurality of second prisms arranged continuously; and the second prism layer is disposed on an upper surface of the second base film;

[0011] A composite adhesive layer is disposed on the lower surface of the second base film; the composite adhesive layer contains PBMA or PMMA microbeads; and the first prism is bonded to the second base film via the composite adhesive layer.

[0012] According to one embodiment of the present invention, the first prism has three edges, including two first bottom edges and one first top edge; the first top edge protrudes from the first base film; the spacing between the first top edges of two adjacent first prisms is 60-70 microns; the first prism layer also includes a first prism base, the two first bottom edges are arranged on the first prism base, and the first prism and the first prism base are integrally formed; the cross-section of the first prism is an isosceles triangle.

[0013] According to one embodiment of the present invention, in the cross section of the first prism, the vertex angle A is 88-92 degrees and / or the vertex angle B of the second prism is 89-93 degrees; or in the cross section of the second prism, the peak top of the vertex angle A is a rounded corner with a radius of 0-5 microns.

[0014] According to one embodiment of the present invention, the second prism has three edges, including two second bottom edges and one second top edge; the second top edge protrudes from the second base film; the spacing between the second top edges of two adjacent second prisms is 25-70 microns; the second prism layer also includes a second prism base, the two second bottom edges are arranged on the second prism base, and the second prism and the second prism base are integrally formed; the cross-section of the second prism is an isosceles triangle.

[0015] According to an embodiment of the present invention, the haze of the composite adhesive layer is 20%-60%.

[0016] According to one embodiment of the present invention, PMMA microbeads or PBMA microbeads are dispersed in the composite adhesive layer, and the PMMA microbeads or PBMA microbeads make the haze of the composite adhesive layer reach 20%-60%, or,

[0017] The composite adhesive layer adopts a microstructure molding method to make its haze reach 20%-60%; or,

[0018] Microbeads and spherical particles are dispersed in the composite adhesive layer, and the microbeads are PMMA microbeads or PBMA microbeads; the microbeads and the spherical particles make the haze of the composite adhesive layer reach 20%-60%; or

[0019] Spherical particles are dispersed in the composite adhesive layer, and a microstructure molding method is adopted to make its haze reach 20%-60%.

[0020] According to an embodiment of the present invention, the second prism layer is made of a resin material, or;

[0021] The second prism layer is made of a resin material, and spherical particles are dispersed in the resin.

[0022] According to one embodiment of the present invention, the spherical particles are selected from one or more of kaolin, aluminum hydroxide, magnesium hydroxide or powdered calcium carbonate.

[0023] According to one embodiment of the present invention, the particle size of the spherical particles is 0.1-1 micrometer.

[0024] According to one embodiment of the present invention, the first prism has a first top edge, and the second prism has a second top edge; an angle C between a top projection line of the first top edge and a top projection line of the second top edge is not 90 degrees.

[0025] According to one embodiment of the present invention, the first prism has a first top edge, and the second prism has a second top edge; the angle C between the top projection line of the first top edge and the top projection line of the second top edge is 45 degrees to 85 degrees or 95 degrees to 135 degrees.

[0026] According to an embodiment of the present invention, the first prism has a first top edge, and the second prism has a second top edge; the first top edge is inserted into the composite adhesive layer to a depth of 0.5-2 microns.

[0027] According to one embodiment of the present invention, the first prism has a first top edge, and the second prism has a second top edge; along the length direction of the second top edge, the second top edge has a height variation, and the height difference is 1.5-3 microns; the first prism is a straight prism or a high-low prism, and the height of each prism on its extension line remains unchanged, and adjacent prisms have the same height if they are straight prisms, or different heights if they are high-low prisms.

[0028] According to one embodiment of the present invention, the back coating composition comprises, by mass percentage:

[0029] 9%-12% of 6-functional aliphatic polyurethane acrylic prepolymer; 3%-6% of 3-functional aliphatic polyurethane acrylic prepolymer or 4-functional aliphatic polyurethane acrylic prepolymer; 6%-9% of active diluent; 1.2%-2.4% of photoinitiator; 0.3%-0.6% of dispersant; 0.3%-0.6% of antistatic agent; 0.2%-4% of 3-5 micron PBMA or PMMA microbeads; the rest is solvent, and the solvent is two or three of toluene, butanone and cyclohexanone.

[0030] According to one embodiment of the present invention, the components of the first prism layer include, by mass percentage:

[0031] OPPEA 25%-30%; epoxy acrylate prepolymer 10%-15%; EOEOEA 10%-15%; BPA (EO) 10DA 25%-30%; hydroxyethyl acrylate 3%-5%; photoinitiator 2%-6%; leveling agent 1%-3%.

[0032] According to one embodiment of the present invention, the components of the composite adhesive layer include, by mass percentage: 6%-8% of 2-functional aliphatic polyurethane acrylic prepolymer; 2%-4% of 4-functional aliphatic polyurethane acrylic prepolymer; 3%-5% of acryloyl morpholine; 0.2%-0.4% of methacrylate phosphate; 1%-2% of HDDA; 0.8%-1.6% of photoinitiator; 0.5%-2% of 3-5 micron PBMA microbeads or PMMA microbeads; the rest is solvent, which is one or both of butanone and toluene; or,

[0033] The components of the composite adhesive layer include, by mass percentage: 6%-8% of a difunctional aliphatic polyurethane acrylic prepolymer; 2%-4% of a tetrafunctional aliphatic polyurethane acrylic prepolymer; 3%-5% of acryloyl morpholine; 0.2%-0.4% of methyl methacrylate phosphate; 1%-2% of HDDA; 0.8%-1.6% of a photoinitiator; 0.5%-2% of 3-5 micron PBMA microbeads or PMMA microbeads; 0.5%-1.5% of spherical particles; and the rest is a solvent, which is one or both of butanone and toluene.

[0034] According to one embodiment of the present invention, the components of the composite adhesive layer include, by mass percentage: 6%-8% of a 2-functional aliphatic polyurethane acrylic prepolymer; 2%-4% of a 4-functional aliphatic polyurethane acrylic prepolymer; 3%-5% of acryloyl morpholine; 0.2%-0.4% of methacrylate phosphate; 1%-2% of HDDA; 0.5%-1.6% of a photoinitiator; 0.2%-0.6% of a phosphate monomer; and the rest is a solvent, which is one or both of butanone and toluene; or,

[0035] The components of the composite adhesive layer include, by mass percentage: 6%-8% of 2-functional aliphatic polyurethane acrylic prepolymer; 2%-4% of 4-functional aliphatic polyurethane acrylic prepolymer; 3%-5% of acryloyl morpholine; 0.2%-0.4% of methacrylate phosphate; 1%-2% of HDDA; 0.5%-1.6% of photoinitiator; 0.2%-0.6% of phosphate monomer; 0.5%-1.5% of spherical particles; the rest is solvent, which is one or both of butanone and toluene. More preferably, the composite adhesive layer manufactured according to the present formula adopts a microstructure molding method to achieve the required haze.

[0036] According to one embodiment of the present invention, the components of the second prism layer include, by mass percentage: OPPEA 30%-35%;

[0037] Epoxy acrylate prepolymer 10%-15%; EOEOEA 5%-10%; BPA (EO) 20DA 5%-10%; BPA (EO) 3DA 10%-15%; DPHA 5%-10%; photoinitiator 3%-7%; leveling agent 1%-3%; or

[0038] The components of the second prism layer include, by mass percentage: OPPEA 30%-35%; epoxy acrylate prepolymer 10%-15%; EOEOEA 5%-10%; BPA (EO) 20DA 5%-10%; BPA (EO) 3DA 10%-15%; DPHA 5%-10%; photoinitiator 3%-7%; leveling agent 1%-3%; spherical particles 0.05%-0.15%.

[0039] A liquid crystal display backlight module is characterized by comprising the aforementioned laminating film for liquid crystal display.

[0040] The present invention proposes a complete set of solutions, which can effectively solve the problem of ensuring that the shielding property meets the requirements of the liquid crystal display module under the premise of ensuring that the brightness meets the requirements of the liquid crystal display product, and can be in direct contact with the liquid crystal display panel glass to ensure that there is no interference and no glare, the visual effect meets the standard, and the scratch resistance meets the assembly requirements. The product stiffness can meet the requirements of large-size modules, thereby effectively promoting the application and promotion of bonding products in the field of liquid crystal displays. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 Schematic diagram of the structure of the laminating film for liquid crystal display according to some embodiments of the present invention.

[0042] Figure 2 Schematic diagram of the membrane structure of the first structural layer in some embodiments of the present invention.

[0043] Figure 3 It is a schematic diagram of the angle between the first top edge and the second top edge when looking down at the laminating film.

[0044] Figure 4 Schematic diagram of the laminating film structure in some embodiments of the present invention.

[0045] Figure 5 Shown is a schematic structural diagram of Example 3, in which the composite adhesive layer is processed by a microstructure molding method.

[0046] Figure 6 Shown is a schematic diagram of the structure of Example 7, in which spherical particles are added to the second prism.

[0047] Figure 7 This is a schematic diagram of the structure of Example 8, in which spherical particles and microbeads are added to the composite adhesive layer.

[0048] Figure 8 Schematic diagram of the structure of Example 9, in which the composite adhesive layer is processed by a microstructure molding method and spherical particles are added. DETAILED DESCRIPTION

[0049] The second top edge spacing of the adjacent second prisms in the present invention is 25-70 microns, preferably 50-60 microns, and its specific value can be selected within this range, such as 26, 30, 34, 38, 42, 46, 50, 52, 55, 58, 60, 63, 66, 68, 70 microns. The second prism vertex angle is 89 degrees to 93 degrees, preferably 90 degrees to 92 degrees, and the cross section is an isosceles triangle shape. The specific angle of the vertex angle can be 89, 90, 91, 92 or 93 degrees. The peak top of the vertex angle can also adopt a radius of 0-5 microns, preferably 2-3 microns, such as 0, 0.5, 1, 1.6, 2, 2.3, 2.6, 3 microns. The composite film can achieve a suitable brightness and improve scratch resistance.

[0050] Along the length direction of the second top edge, the height of the second top edge varies, and the height difference is 1.5-3 microns, and the preferred height difference does not exceed 2 microns, such as 1.5, 1.7, 1.9, 2.1, 2.3, 2.5, 2.7, 3 microns. The height change of the second top edge can be either regular or irregular, as long as the height difference is within the above range. The projection line of the first top edge and the projection line of the second top edge form a non-90 degree angle, which can be 45-85 degrees or 95-135 degrees; preferably 69-76 degrees or 104-111 degrees; such as 69, 71, 73, 74, 75, 76 degrees or 104, 105, 106, 107, 109, 111 degrees. The angle size needs to be determined based on the matching effect with the LCD screen, so as to solve the interference problem with the LCD screen and improve the viewing angle. In addition, a pre-rotation angle solution is adopted, that is, the second prism and / or the first prism are pre-made to a required angle, and the pre-rotation is based on a line perpendicular or parallel to the film edge.

[0051] In the present invention, the first top edge spacing of adjacent first prisms is 60-70 microns, preferably 60 and 70 microns, and the specific value can be selected within this range, such as 60, 62, 64, 66, 68, 70 microns. The top angle of the first prism is 88 degrees to 92 degrees, preferably 89 degrees to 91 degrees, and the cross section is an isosceles triangle shape; the specific angle of the top angle can be 88, 89, 90, 91 or 92 degrees; the first prism is a straight prism or a high-low prism, and the height of each prism on its extension line remains unchanged, and the heights of adjacent prisms can be the same as straight prisms or different as high-low prisms.

[0052] The back coating resin of the first structural layer contains 3-5 micron PBMA or PMMA microbeads and is added with antistatic agent. The surface resistance is within 10 to the 12th power and the hardness is H-2H, which can solve the antistatic problem of the composite film and the anti-scratch problem on the back. In addition, the haze is continuously adjustable from 3 to 60%, preferably 3%, 15%, 18%, 20%, 24%, 30%, 34%, 40%, and 45%, ensuring that the different shielding requirements of the composite film are met to meet the needs of different modules.

[0053] The composite adhesive layer adopts a haze of 20-60%, thereby solving the shielding and glare problems of the composite film.

[0054] The first prism of the first structural film layer is inserted into the composite adhesive layer by 0.5-2 microns. If the insertion depth is insufficient, the bonding strength is poor and the bonding strength is affected. If the insertion depth is too deep, the brightness will be affected.

[0055] Both the first base film and the second base film can be made of transparent substrates such as PET film, PC film, PI film, PP film, etc. with chemically treated surfaces. The thickness is determined according to actual application needs, such as 36-250 microns, preferably 75, 100, 125, 188 microns.

[0056] Spherical particles can be added to the second prism structure of the second structural layer membrane. Since the spherical particles have a large optical specific surface area, they can have the best shielding property under the premise of ensuring brightness. The material of the spherical particles is one or more powder materials selected from kaolin, aluminum hydroxide, magnesium hydroxide or powdered calcium carbonate, preferably kaolin or powdered calcium carbonate; the particle size is 0.1-1 micron, preferably 0.4-0.6 micron. Too large a particle size affects the structure formation, and too small a particle size has poor shielding. The addition of spherical particles can improve the viewing angle, shielding property, and anti-glare while ensuring a small loss of brightness. At the same time, after adding spherical particles to the second prism structure of the second structural layer membrane, the haze of the composite adhesive layer can be appropriately reduced while ensuring the same viewing angle and shielding property, thereby reducing the amount of microbeads in the glue of the composite adhesive layer. Since the particle size of PMMA or PBMA microbeads is relatively large, a large number of them will have some influence on the fastness of the bonding adhesive, so the present invention can improve the bonding fastness.

[0057] The composite adhesive layer is dispersed with PMMA or PBMA microbeads, with a particle size of 3-5 microns and a haze of 20%-60%. The purpose is to increase the haze of the composite adhesive to solve the shielding and glare problems of the composite film. At the same time, spherical particles can be added. The spherical particles are made of one or more powder materials such as kaolin, aluminum hydroxide, magnesium hydroxide or powdered calcium carbonate, preferably kaolin or powdered calcium carbonate; the particle size is 0.1-1 micron, preferably 0.4-0.6 micron. Spherical particles with too large a particle size cannot complement PMMA & PBMA microbeads, and those with too small a particle size have poor shielding. Thus, the two kinds of microparticles cooperate with each other to solve the shielding and glare problems of the composite film, and can reduce the amount of PMMA or PBMA microbeads in the composite adhesive to improve the adhesion of the bonding. Because the particle size of PMMA or PBMA microbeads is relatively large, a large number of them will have some impact on the fastness of the bonding adhesive. In addition, after reducing the amount of PMMA or PBMA used, the depth of the first prism inserted into the composite adhesive layer during bonding can be appropriately reduced while ensuring the same bonding strength, thereby improving the optical brightness.

[0058] The composite adhesive layer between the first structural layer film and the second structural layer film adopts a microstructure molding method to produce a matte effect, reaching a haze of 20-60%, the purpose of which is to increase the haze of the composite adhesive to solve the shielding and glare problems of the composite film. At the same time, spherical particles can be added to achieve a haze of 20-60%, preferably 30-40% haze. The spherical particles are made of one or more powder materials such as kaolin, aluminum hydroxide, magnesium hydroxide or powdered calcium carbonate, preferably kaolin or powdered calcium carbonate; the particle size is 0.1-1 micron, preferably 0.4-0.6 micron. If the particle size of the spherical particles is too large, it will affect the adhesion fastness, and if the particle size is too small, the shielding is poor. Therefore, the spherical particles and the matte microstructure cooperate with each other to solve the shielding and glare problems of the composite film, and can reduce the haze when the matte structure is made, thereby reducing the ups and downs on the surface of the matte microstructure. Because the height difference of the convex and concave points of the matte structure is related to the haze, the higher the haze, the greater the height difference, and vice versa. Therefore, the present invention can improve the bonding adhesion of the composite adhesive layer; in addition, after reducing the haze of the matte structure, the depth of the first prism inserted into the composite adhesive layer during bonding can be appropriately reduced while ensuring the same bonding fastness, thereby improving the optical brightness.

[0059] The present invention is described in detail below in conjunction with the accompanying drawings:

[0060] Embodiment 1:

[0061] like Figure 1 , Figure 2 and Figure 3 As shown, the laminating film 100 for a liquid crystal display comprises a first structural layer film 110 and a second structural layer film 120 from bottom to top.

[0062] The first structural layer film 110 includes a first base film 111 and a first prism layer 112. The first base film 111 is a 125 micron optical grade chemically treated PET film. The first prism layer 112 includes a first prism base 119 and a plurality of first prisms 113. The plurality of first prisms 113 are arranged continuously and without intervals on the first prism base 119. The cross section of the first prism 113 is an isosceles triangle, and the vertex A is a right angle. The first prism 113 has three edges, including two first bottom edges 115 and a first top edge 116. The two first bottom edges 115 are arranged on the first prism base 119. The height H1 of the first top edge 116 is 30 microns, and the spacing D1 between adjacent first top edges 116 is 60 microns. The first prism layer 112 is arranged on the upper surface of the first base film 111. The first prism 113 is integrally formed with the first prism base 119, and the first prism base is arranged on the upper surface of the first base film. The first top ridge 116 protrudes from the first base film 111 .

[0063] The lower surface of the first base film 111 is provided with a back coating layer 118. The back coating layer 118 is a UV resin, and is dispersed with 3-5 micron PBMA micro beads and antistatic agents. The surface resistance is 10 to the 11th power, the hardness is 2H, the haze is 3%, and the thickness is 5 microns.

[0064] The second structural layer film 120 includes a second base film 121 and a second prism layer 122. The second base film 121 is a 125-micron optical grade chemically treated PET film. The second prism layer 122 includes a second prism base 129 and a plurality of second prisms 123. The plurality of second prisms 123 are continuously and uninterruptedly arranged on the second prism base 129. The second prism layer 122 is arranged on the upper surface of the second base film 121; the cross section of the second prism 123 is an isosceles triangle, and the vertex angle B is a right angle. The second prism 123 has three edges, including two second bottom edges 125 and a second top edge 126. The two second bottom edges 125 are arranged on the second prism base 129. The height H2 of the second top edge is 25 microns, and the second top edge 126 is 25 microns along the length direction of the second prism 123. Figure 1 As shown, the height of the second top edge 126 varies perpendicular to the paper surface. In this embodiment, the maximum height difference of the second top edge 126 is 2 microns. The spacing D2 between adjacent second top edges is 50 microns. The second prism 123 is integrally formed with the second prism substrate 129, and the second prism substrate 129 is disposed on the upper surface of the second base film 1211. The second top edge 126 protrudes from the second base film 121.

[0065] The lower surface of the second base film 1211 is provided with a composite adhesive layer 130. The composite adhesive layer 130 is glue, and PBMA micro beads of 3-5 microns are dispersed, reaching a haze of 40%.

[0066] The first prism 113 is attached to the second base film 121 through the composite adhesive layer 130. The first top edge is inserted into the composite adhesive layer by 0.5-2 microns. Figure 3 As shown, the included angle C between the projection line of the first top edge 116 and the projection line of the second top edge 126 is 76 degrees.

[0067] The back coating components of the first structural layer film include, by mass percentage:

[0068] Sartomer CN9006 (6-functional aliphatic polyurethane acrylic prepolymer) 12%; Sartomer CN9008 (3-functional aliphatic polyurethane acrylic prepolymer) 6%; reactive diluent-TMPTA 4.5%; reactive diluent-HDDA 4.5%; photoinitiator 184 1%; photoinitiator 1173 1%; Digo Chemical TEGO-688 (dispersant) 0.5%; antistatic agent 0.3%; 3-5 micron PBMA or PMMA microbeads 0.3%; the rest is solvent, the solvent is toluene, butanone and cyclohexanone, the ratio is 4:1:1.

[0069] The components of the first prism layer include, by mass percentage:

[0070] OPPEA 30%; Allnex resin E3708 (epoxy acrylate prepolymer) 15%; EOEOEA 15%; BPA (EO) 10DA 30%; hydroxyethyl acrylate 5%; photoinitiator 184 2%; photoinitiator TPO 1%; Jintuan Chemical KEPERSURF-1577E (acrylate leveling agent) 2%.

[0071] The components of the composite adhesive layer include, by mass percentage:

[0072] Sartomer CN966H90 (2-functional aliphatic polyurethane acrylic prepolymer) 8%; Runao Chemical L8112 (4-functional aliphatic polyurethane acrylic prepolymer) 4%; acryloyl morpholine 5%; methacrylate phosphate 0.2%; HDDA 1%; photoinitiator 184 0.8%; photoinitiator 1173 0.8%; 3-5 micron PBMA or PMMA microbeads 1.7%; the rest is solvent, the solvent is toluene and butanone, toluene: butanone = 1:1.

[0073] The components of the second prism layer include, by mass percentage:

[0074] OPPEA 35%; Meiyuan Chemical E3708 (epoxy acrylate prepolymer) 14%; EOEOEA 10%; BPA (EO) 20DA 10%; BPA (EO) 3DA 14%; DPHA 10%; photoinitiator 184 3%; photoinitiator TPO 2%; BYK-371 (reactive silicone leveling agent) 2%.

[0075] Example 2

[0076] like Figure 4 , Figure 2 and Figure 3 As shown, the laminating film 100 for a liquid crystal display comprises a first structural layer film 110 and a second structural layer film 120 from bottom to top.

[0077] The first structural layer film 110 includes a first base film 111 and a first prism layer 112. The first base film 111 is a 125 micron optical grade chemically treated PET film. The first prism layer 112 is arranged on the upper surface of the first base film 111. The first prism layer 112 includes a first prism base 119 and a plurality of first prisms 113. The plurality of first prisms 113 are continuously arranged without spacing on the first prism base 119. The cross section of the first prism 113 is an isosceles triangle, and the vertex A is a right angle. The first prism 113 has three edges, including two first bottom edges 115 and a first top edge 116. The two first bottom edges 115 are arranged on the first prism base 119. The height H1 of the first top edge 116 is 30 or 35 microns. The first prisms 113 with a first top edge height H1 of 30 microns are spaced apart from the first prisms 113 with a first top edge height H1 of 35 microns. The spacing D1 between adjacent first top edges 116 is 70 or 60 microns. The spacing D1 between two adjacent first top edges 116 with a height H1 of 30 microns is 60 microns. The spacing D1 between two adjacent first top edges 116 with a height H1 of 35 microns is 70 microns. The first prism 113 is integrally formed with the first prism substrate 119, and the first prism substrate 119 is disposed on the upper surface of the first base film 110. The first top edge 116 protrudes from the first base film 111.

[0078] The lower surface of the first base film 111 is provided with a back coating layer 118. The back coating layer 118 is a UV resin, and is dispersed with 3-5 micron PBMA micro beads and antistatic agents. The surface resistance is 10 to the 11th power, the hardness is 2H, the haze is 3%, and the thickness is 5 microns.

[0079] The second structural layer film 120 includes a second base film 121 and a second prism layer 122. The second base film 121 is a 125-micron optical grade chemically treated PET film. The second prism layer 122 includes a second prism base 129 and a plurality of second prisms 123. The plurality of second prisms 123 are arranged on the second prism base 129. The second prism layer 122 is arranged on the upper surface of the second base film 121; the cross section of the second prism 123 is an isosceles triangle, and the vertex angle B is a fillet with a radius R of 2 microns. The second prism 123 has three edges, including two second bottom edges 125 and a second top edge 126. The two second bottom edges 125 are arranged on the second prism base 129. The height H2 of the second top edge is 30 microns, and the second prism 123 is 1.3 microns long. Figure 1 As shown, the height of the second top edge 126 varies perpendicular to the paper surface, and the maximum height difference of the second top edge 126 is 2 microns. The spacing D2 between adjacent second top edges is 60 microns. The second prism 123 is integrally formed with the second prism substrate 129, and the second prism substrate 129 is disposed on the upper surface of the second base film 121. The second top edge 126 protrudes from the second base film 121.

[0080] The lower surface of the second base film 121 is provided with a composite adhesive layer 130. The composite adhesive layer 130 is glue, and PBMA micro beads of 3-5 microns are dispersed, reaching a haze of 40%.

[0081] The first prism 113 is attached to the second base film 121 through the composite adhesive layer 130. The first top edge is inserted into the composite adhesive layer by 0.5-2 microns. Figure 3 As shown, the included angle C between the projection line of the first top edge 116 and the projection line of the second top edge 126 is 73 degrees.

[0082] The back coating components of the first structural layer film include, by mass percentage:

[0083] Allnex resin E1290N (6-functional aliphatic polyurethane acrylate prepolymer) 12%; Allnex resin E1258 (3-functional aliphatic polyurethane acrylate prepolymer) 6%; reactive diluent-TMPTA 4.5%; reactive diluent-HDDA 4.5%; photoinitiator 184 1%; photoinitiator 1173 1%; Silok771N (dispersant) 0.5%; antistatic agent 0.3%; 3-5 micron PBMA or PMMA microbeads 0.3%; the rest is solvent, the solvent is toluene, butanone and cyclohexanone, and the solvent ratio is 4:1:1.

[0084] The components of the first prism layer include, by mass percentage:

[0085] OPPEA 28%; Allnex resin E3708 (epoxy acrylate prepolymer) 15%; EOEOEA 15%; BPA (EO) 10DA 30%; Hydroxyethyl acrylate 5%; Photoinitiator 184 3%; Photoinitiator TPO 2%; Mo Neng Chemical UV1201 (acrylate leveling agent) 2%.

[0086] The components of the composite adhesive layer include, by mass percentage:

[0087] Lida Chemical U-8663 (2-functional aliphatic polyurethane acrylic prepolymer) 8%; Runao Chemical L8112 (4-functional aliphatic polyurethane acrylic prepolymer) 3.6%; acryloyl morpholine 4.8%; methyl methacrylate phosphate 0.4%; HDDA 1.5%; photoinitiator 184 0.8%; photoinitiator 1173 0.8%; 3-5 micron PBMA microbeads 1.6%; the rest is solvent, the solvent is toluene and butanone, the solvent ratio is 1:1.

[0088] The components of the second prism layer include, by mass percentage:

[0089] OPPEA 33%; Allnex resin E3708 (epoxy acrylate prepolymer) 15%; EOEOEA 10%; BPA (EO) 20DA 10%; BPA (EO) 3DA 15%; DPHA 10%; photoinitiator 184 3%; photoinitiator TPO 2%; Digao Chemical TEGO 2100 (reactive silicone leveling agent) 2%.

[0090] Example 3

[0091] like Figure 5 , Figure 2 and Figure 3 As shown, the laminating film 100 for a liquid crystal display comprises a first structural layer film 110 and a second structural layer film 120 from bottom to top.

[0092] The first structural layer film 110 includes a first base film 111 and a first prism layer 112. The first base film 111 is a 125 micron optical grade chemically treated PET film. The first prism layer 112 includes a first prism substrate 119 and a plurality of first prisms 113. The plurality of first prisms 113 are continuously arranged without spacing on the first prism substrate 119. The cross section of the first prism 113 is an isosceles triangle, and the vertex A is a right angle. The first prism 113 has three edges, including two first bottom edges 115 and a first top edge 116. The two first bottom edges 115 are arranged on the first prism substrate 119. The height H1 of the first top edge 116 is 30 or 35 microns. The first prism 113 with a first top edge height of 30 microns is spaced apart from the first prism 113 with a first top edge height of 35 microns. The spacing D1 between adjacent first top edges 116 is 70 or 60 microns. The spacing D1 between two adjacent first top edges 116 with a height of 30 microns is 60 microns. The distance D1 between two adjacent first top edges 116 with a height of 35 microns is 70 microns. The first prism layer 112 is disposed on the upper surface of the first base film 111. The first prism 113 is integrally formed with the first prism substrate 119, and the first prism substrate is disposed on the upper surface of the first base film. The first top edge 116 protrudes from the first base film 111.

[0093] The lower surface of the first base film 111 is provided with a back coating layer 118. The back coating layer 118 is a UV resin, and is dispersed with 3-5 micron PBMA micro beads and antistatic agents. The surface resistance is 10 to the 11th power, the hardness is 2H, the haze is 3%, and the thickness is 5 microns.

[0094] The second structural layer film 120 includes a second base film 121 and a second prism layer 122. The second base film 121 is a 125-micron optical grade chemically treated PET film. The second prism layer 122 includes a second prism base 129 and a plurality of second prisms 123. The plurality of second prisms 123 are continuously and uninterruptedly arranged on the second prism base 129. The second prism layer 122 is arranged on the upper surface of the second base film 121; the cross section of the second prism 123 is an isosceles triangle, and the vertex angle B is a right angle. The second prism 123 has three edges, including two second bottom edges 125 and a second top edge 126. The two second bottom edges 125 are arranged on the second prism base 129. The height H2 of the second top edge is 25 microns, and the second top edge 126 is 25 microns along the length direction of the second prism 123. Figure 1 As shown, the height of the second top edge 126 varies perpendicular to the paper surface, and the maximum height difference of the second top edge 126 is 2 microns. The spacing D2 between adjacent second top edges is 50 microns. The second prism 123 is integrally formed with the second prism substrate 129, and the second prism substrate 129 is disposed on the upper surface of the second base film 121. The second top edge 126 protrudes from the second base film 121.

[0095] The lower surface of the second base film 121 is provided with a composite adhesive layer 130. The composite adhesive layer 130 is glue. Figure 5 As shown, the composite adhesive layer 130 adopts a microstructure molding method to achieve a haze of 40%.

[0096] The first prism 113 is attached to the second base film 121 through the composite adhesive layer 130. The first top edge is inserted into the composite adhesive layer by 0.5-2 microns. The included angle C between the projection line of the first top edge 116 and the projection line of the second top edge 126 is 76 degrees.

[0097] The back coating components of the first structural layer film include, by mass percentage:

[0098] Allnex resin E1290N (6-functional aliphatic polyurethane acrylate prepolymer) 12%; Allnex resin E1258 (3-functional aliphatic polyurethane acrylate prepolymer) 6%; reactive diluent-TMPTA 4.5%; reactive diluent-HDDA 4.5%; photoinitiator 184 1%; photoinitiator 1173 1%; Sartomer epoxy acrylate CN 151 (dispersant) 0.5%; antistatic agent 0.3%; 3-5 micron PBMA or PMMA microbeads 0.3%; the rest is solvent, the solvent is toluene, butanone and cyclohexanone, and the solvent ratio is 4:1:1.

[0099] The components of the first prism layer include, by mass percentage:

[0100] OPPEA 29%; Meiyuan Chemical ME2100 (epoxy acrylate prepolymer) 14%; EOEOEA 14%; BPA (EO) 10DA 29%; hydroxyethyl acrylate 5%; photoinitiator 184 3%; photoinitiator TPO 3%; Jintuan Chemical KEPERSURF-1577E (acrylate leveling agent) 3%.

[0101] The components of the composite adhesive layer include, by mass percentage:

[0102] Lida Chemical U-8663 (2-functional aliphatic polyurethane acrylic prepolymer) 8%; Runao Chemical L8112 (4-functional aliphatic polyurethane acrylic prepolymer) 4%; acryloyl morpholine 4.8%; methyl methacrylate phosphate 0.4%; HDDA 1.5%; photoinitiator 184 0.5%; photoinitiator 1173 0.5%; photoinitiator TPO 0.4%; NTCADD FM30 Beijing Baiyuan Chemical Co., Ltd. (phosphate monomer) 0.5%; the rest is solvent, the solvent is toluene and butanone, and the solvent ratio is 2:1.

[0103] The components of the second prism layer include, by mass percentage:

[0104] OPPEA 35%; Meiyuan Chemical ME2100 (epoxy acrylate prepolymer) 12%; EOEOEA 10%; BPA (EO) 20DA 10%; BPA (EO) 3DA 15%; DPHA 9%; photoinitiator 184 3%; photoinitiator TPO 3%; BYK-371 (reactive silicone leveling agent) 3%.

[0105] Example 4

[0106] like Figures 1 to 3 As shown, the laminating film 100 for a liquid crystal display comprises a first structural layer film 110 and a second structural layer film 120 from bottom to top.

[0107] The first structural layer film 110 includes a first base film 111 and a first prism layer 112. The first base film 111 is a 125 micron optical grade chemically treated PET film. The first prism layer 112 includes a first prism base 119 and a plurality of first prisms 113. The plurality of first prisms 113 are arranged continuously and without intervals on the first prism base 119. The cross section of the first prism 113 is an isosceles triangle, and the vertex A is a right angle. The first prism 113 has three edges, including two first bottom edges 115 and a first top edge 116. The two first bottom edges 115 are arranged on the first prism base 119. The height H1 of the first top edge 116 is 30 microns, and the spacing D1 between adjacent first top edges 116 is 60 microns. The first prism layer 112 is arranged on the upper surface of the first base film 111. The first prism 113 is integrally formed with the first prism base 119, and the first prism base is arranged on the upper surface of the first base film. The first top ridge 116 protrudes from the first base film 111 .

[0108] The lower surface of the first base film 111 is provided with a back coating layer 118. The back coating layer 118 is a UV resin, and is dispersed with 3-5 micron PBMA micro beads and antistatic agents. The surface resistance is 10 to the 11th power, the hardness is 2H, the fog is 40%, and the thickness is 5 microns.

[0109] The second structural layer film 120 includes a second base film 121 and a second prism layer 122. The second base film 121 is a 125-micron optical grade chemically treated PET film. The second prism layer 122 includes a second prism base 129 and a plurality of second prisms 123. The plurality of second prisms 123 are continuously arranged without spacing on the second prism base 129. The second prism layer 122 is arranged on the upper surface of the second base film 121; the cross section of the second prism 123 is an isosceles triangle, and the vertex angle B is a right angle. The second prism 123 has three edges, including two second bottom edges 125 and a second top edge 126. The two second bottom edges 125 are arranged on the second prism base 129. The height H2 of the second top edge is 25 microns, and the second top edge 126 is 25 microns along the length direction of the second prism 123. Figure 1 As shown, the height of the second top edge 126 changes perpendicular to the paper surface, and the maximum height difference of the second top edge 126 is 2 microns. The spacing D2 between adjacent second top edges is 50 microns. The second prism 123 is integrally formed with the second prism substrate 129, and the second prism substrate 129 is disposed on the upper surface of the second base film 121. The second top edge 126 protrudes from the second base film 121.

[0110] The lower surface of the second base film 121 is provided with a composite adhesive layer 130. The composite adhesive layer 130 is glue, and PBMA micro beads of 3-5 microns are dispersed, reaching a haze of 40%.

[0111] The first prism 113 is attached to the second base film 121 through the composite adhesive layer 130. The first top edge is inserted into the composite adhesive layer by 0.5-2 microns. The included angle C between the projection line of the first top edge 116 and the projection line of the second top edge 126 is 73 degrees.

[0112] The back coating components of the first structural layer film include, by mass percentage:

[0113] Sartomer CN9006 (6-functional aliphatic polyurethane acrylic prepolymer) 12%; Allnex resin E8210 (4-functional aliphatic polyurethane acrylic prepolymer) 6%; reactive diluent-TMPTA 4.5%; reactive diluent-HDDA 4.5%; photoinitiator 184 1.2%; photoinitiator 1173 1.2%; Silok771N (dispersant) 0.6%; antistatic agent 0.5%; 3-5 micron PBMA or PMMA microbeads 3.3%; the rest is solvent, the solvent is toluene, butanone and cyclohexanone, and the solvent ratio is 3:1:1.

[0114] The components of the first prism layer include, by mass percentage:

[0115] OPPEA 28%; Meiyuan Chemical ME2100 (epoxy acrylate prepolymer) 14.5%; EOEOEA 15%; BPA (EO) 10DA 29.5%; hydroxyethyl acrylate 5%; photoinitiator 184 3%; photoinitiator TPO 3%; Jintuan Chemical KEPERSURF-1577E (acrylate leveling agent) 2%.

[0116] The components of the composite adhesive layer include, by mass percentage:

[0117] Lida Chemical U-8663 (2-functional aliphatic polyurethane acrylic prepolymer) 7.8%; Runao Chemical L8112 (4-functional aliphatic polyurethane acrylic prepolymer) 3.8%; acryloyl morpholine 4.6%; methyl methacrylate phosphate 0.4%; HDDA 1.6%; photoinitiator 184 0.8%; photoinitiator 1173 0.8%; 3-5 micron PBMA or PMMA microbeads 1.8%; the rest is solvent, the solvent is toluene and butanone, the solvent ratio is 1:1.

[0118] The components of the second prism layer include, by mass percentage:

[0119] OPPEA 33%; Meiyuan Chemical ME2100 (epoxy acrylate prepolymer) 14%; EOEOEA 10%; BPA (EO) 20DA 10%; BPA (EO) 3DA 14%; DPHA 10%; photoinitiator 184 4%; photoinitiator TPO 2%; Digao Chemical TEGO 2100 (reactive silicone leveling agent) 3%.

[0120] Example 5

[0121] like Figure 4 , Figure 2 and Figure 3 As shown, the laminating film 100 for a liquid crystal display comprises a first structural layer film 110 and a second structural layer film 120 from bottom to top.

[0122] The first structural layer film 110 includes a first base film 111 and a first prism layer 112. The first base film 111 is a 125 micron optical grade chemically treated PET film. The first prism layer 112 includes a first prism substrate 119 and a plurality of first prisms 113. The plurality of first prisms 113 are continuously arranged without spacing on the first prism substrate 119. The cross section of the first prism 113 is an isosceles triangle, and the vertex A is a right angle. The first prism 113 has three edges, including two first bottom edges 115 and a first top edge 116. The two first bottom edges 115 are arranged on the first prism substrate 119. The height H1 of the first top edge 116 is 30 or 35 microns. The first prisms 113 with a first top edge height H1 of 30 microns are spaced apart from the first prisms 113 with a first top edge height of 35 microns. The spacing between adjacent first top edges 116 is 70 or 60 microns. The distance D1 between two adjacent first top edges 116 with a height of 30 microns is 60 microns. The distance D2 between two adjacent first top edges 116 with a height of 35 microns is 70 microns. The first prism layer 112 is disposed on the upper surface of the first base film 111. The first prism 113 is integrally formed with the first prism substrate 119, and the first prism substrate is disposed on the upper surface of the first base film. The first top edge 116 protrudes from the first base film 111.

[0123] The lower surface of the first base film 111 is provided with a back coating layer 118. The back coating layer 118 is a UV resin, and is dispersed with 3-5 micron PBMA micro beads and antistatic agents. The surface resistance is 10 to the 11th power, the hardness is 2H, the haze is 40%, and the thickness is 5 microns.

[0124] The second structural layer film 120 includes a second base film 121 and a second prism layer 122. The second base film 121 is a 125-micron optical grade chemically treated PET film. The second prism layer 122 includes a second prism base 129 and a plurality of second prisms 123. The plurality of second prisms 123 are continuously arranged without spacing on the second prism base 129. The second prism layer 122 is arranged on the upper surface of the second base film 121; the cross section of the second prism 123 is an isosceles triangle, and the vertex angle B is a fillet with a radius of 2 microns. The second prism 123 has three edges, including two second bottom edges 125 and a second top edge 126. The two second bottom edges 125 are arranged on the second prism base 129. The height H2 of the second top edge is 30 microns, and the second top edge is 126 along the length direction of the second prism 123. Figure 1 As shown, the height of the second top edge 126 varies perpendicular to the paper surface, and the maximum height difference of the second top edge 126 is 2 microns. The spacing D2 between adjacent second top edges is 60 microns. The second prism 123 is integrally formed with the second prism substrate 129, and the second prism substrate 129 is disposed on the upper surface of the second base film 121. The second top edge 126 protrudes from the second base film 121.

[0125] The lower surface of the second base film 121 is provided with a composite adhesive layer 130. The composite adhesive layer 130 is glue, and PBMA micro beads of 3-5 microns are dispersed, reaching a haze of 40%.

[0126] The first prism 113 is attached to the second base film 121 through the composite adhesive layer 130. The first top edge is inserted into the composite adhesive layer by 0.5-2 microns. The included angle C between the projection line of the first top edge 116 and the projection line of the second top edge 126 is 69 degrees.

[0127] The back coating components of the first structural layer film include, by mass percentage:

[0128] Sartomer CN9006 (6-functional aliphatic polyurethane acrylate prepolymer) 12%; Runao Chemical L8112 (4-functional aliphatic polyurethane acrylate prepolymer) 6%; reactive diluent-TMPTA 4.5%; reactive diluent-HDDA 4.5%; photoinitiator 184 1.2%; photoinitiator 1173 1.2%; Sartomer epoxy acrylate CN 151 (dispersant) 0.6%; antistatic agent 0.5%; 3-5 micron PBMA or PMMA microbeads 3.3%; the rest is solvent, the solvent is toluene, butanone and cyclohexanone, the solvent ratio is 3:1:1.

[0129] The components of the first prism layer include, by mass percentage:

[0130] OPPEA 30%; Meiyuan Chemical ME2100 (epoxy acrylate prepolymer) 15%; EOEOEA 14%; BPA (EO) 10DA 29.5%; Hydroxyethyl acrylate 4.5%; Photoinitiator 184 3%; Photoinitiator TPO 2%; Mo Neng Chemical UV1201 (acrylate leveling agent) 2%.

[0131] The components of the composite adhesive layer include, by mass percentage:

[0132] Lida Chemical U-8663 (2-functional aliphatic polyurethane acrylic prepolymer) 8%; Runao Chemical L8112 (4-functional aliphatic polyurethane acrylic prepolymer) 3.7%; acryloyl morpholine 4.9%; methyl methacrylate phosphate 0.4%; HDDA 1.9%; photoinitiator 184 0.8%; photoinitiator 1173 0.8%; 3-5 micron PBMA or PMMA microbeads 1.7%; the rest is solvent, the solvent is toluene and butanone, the solvent ratio is 1:1.

[0133] The components of the second prism layer include, by mass percentage:

[0134] OPPEA 32%; Allnex resin E3708 (epoxy acrylate prepolymer) 15%; EOEOEA 10%; BPA (EO) 20DA 10%; BPA (EO) 3DA 15%; DPHA 10%; photoinitiator 184 4%; photoinitiator TPO 2%; BYK-371 (reactive silicone leveling agent) 2%.

[0135] Example 6

[0136] like Figures 1 to 3 As shown, the laminating film 100 for a liquid crystal display comprises a first structural layer film 110 and a second structural layer film 120 from bottom to top.

[0137] The first structural layer film 110 includes a first base film 111 and a first prism layer 112. The first base film 111 is a 125 micron optical grade chemically treated PET film. The first prism layer 112 includes a first prism substrate 119 and a plurality of first prisms 113. The plurality of first prisms 113 are continuously arranged without spacing on the first prism substrate 119. The cross section of the first prism 113 is an isosceles triangle, and the vertex A is a right angle. The first prism 113 has three edges, including two first bottom edges 115 and a first top edge 116. The two first bottom edges 115 are arranged on the first prism substrate 119. The first prism 113 with a first top edge height H1 of 30 or 35 microns and the first prism 113 with a first top edge height H1 of 30 microns are spaced apart from each other. The spacing D1 between adjacent first top edges 116 is 70 or 60 microns. The distance D1 between two adjacent first top edges 116 with a height H1 of 30 microns is 60 microns. The distance D1 between two adjacent first top edges 116 with a height of 35 microns is 70 microns. The first prism layer 112 is arranged on the upper surface of the first base film 111, and the first prism layer 112 is arranged on the upper surface of the first base film 111. The first prism 113 is integrally formed with the first prism substrate 119, and the first prism substrate is arranged on the upper surface of the first base film. The first top edge 116 protrudes from the first base film 111. A back coating layer 118 is arranged on the lower surface of the first base film 111. The back coating layer 118 is a UV resin, and 3-5 micron PBMA microbeads and antistatic agents are dispersed. The surface resistance is 10 to the 11th power, the hardness is 2H, the haze is 40%, and the thickness is 5 microns.

[0138] The second structural layer film 120 includes a second base film 121 and a second prism layer 122. The second base film 121 is a 125-micron optical grade chemically treated PET film. The second prism layer 122 includes a second prism base 129 and a plurality of second prisms 123. The plurality of second prisms 123 are continuously arranged without spacing on the second prism base 129. The second prism layer 122 is arranged on the upper surface of the second base film 121; the cross section of the second prism 123 is an isosceles triangle, and the vertex angle B is a right angle. The second prism 123 has three edges, including two second bottom edges 125 and a second top edge 126. The two second bottom edges 125 are arranged on the second prism base 129. The height H2 of the second top edge is 25 microns, and the second top edge 126 is 25 microns along the length direction of the second prism 123. Figure 1 As shown, the height of the second top edge 126 varies perpendicular to the paper surface, and the maximum height difference of the second top edge 126 is 2 microns. The spacing D2 between adjacent second top edges is 50 microns. The second prism 123 is integrally formed with the second prism substrate 129, and the second prism substrate 129 is disposed on the upper surface of the second base film 121. The second top edge 126 protrudes from the second base film 121.

[0139] The lower surface of the second base film 121 is provided with a composite adhesive layer 130. The composite adhesive layer 130 is glue. Figure 5 As shown, the composite adhesive layer 130 is formed by a microstructure method to achieve a haze of 40%.

[0140] The first prism 113 is attached to the second base film 121 through the composite adhesive layer 130. The first top edge is inserted into the composite adhesive layer by 0.5-2 microns. The included angle C between the projection line of the first top edge 116 and the projection line of the second top edge 126 is 73 degrees.

[0141] The back coating components of the first structural layer film include, by mass percentage:

[0142] Allnex resin E1290N (6-functional aliphatic polyurethane acrylate prepolymer) 12%; Allnex resin E8210 (4-functional aliphatic polyurethane acrylate prepolymer) 6%; reactive diluent-TMPTA 4.5%; reactive diluent-HDDA 4.5%; photoinitiator 184 1.2%; photoinitiator 1173 1.2%; Digo Chemical TEGO-688 (dispersant) 0.6%; antistatic agent 0.5%; 3-5 micron PBMA or PMMA microbeads 3.3%; the rest is solvent, the solvent is toluene, butanone and cyclohexanone, and the solvent ratio is 3:1:1.

[0143] The components of the first prism layer include, by mass percentage:

[0144] OPPEA 29%; Allnex resin E3708 (epoxy acrylate prepolymer) 15%; EOEOEA 14%; BPA (EO) 10DA 28%; Hydroxyethyl acrylate 5%; Photoinitiator 184 3%; Photoinitiator TPO 3%; Mo Neng Chemical UV1201 (acrylate leveling agent) 3%.

[0145] The components of the composite adhesive layer include, by mass percentage:

[0146] Lida Chemical U-8663 (2-functional aliphatic polyurethane acrylic prepolymer) 8%; Runao Chemical L8112 (4-functional aliphatic polyurethane acrylic prepolymer) 4%; acryloyl morpholine 4.8%; methyl methacrylate phosphate 0.4%; HDDA 1.5%; photoinitiator 184 0.5%; photoinitiator 1173 0.5%; photoinitiator TPO 0.4%; Dutch Tanextra MAP (phosphate monomer) 0.5%; the rest is solvent, the solvent is toluene and butanone, the solvent ratio is 2:1.

[0147] The components of the second prism layer include, by mass percentage:

[0148] OPPEA 34%; Meiyuan Chemical ME2100 (epoxy acrylate prepolymer) 13%; EOEOEA 10%; BPA (EO) 20DA 10%; BPA (EO) 3DA 14%; DPHA 10%; photoinitiator 184 3%; photoinitiator TPO 3%; BYK-371 (reactive silicone leveling agent) 3%.

[0149] Example 7

[0150] like Figure 6 , Figure 2 and Figure 3 As shown, the laminating film 100 for a liquid crystal display comprises a first structural layer film 110 and a second structural layer film 120 from bottom to top.

[0151] The first structural layer film 110 includes a first base film 111 and a first prism layer 112. The first base film 111 is a 125 micron optical grade chemically treated PET film. The first prism layer 112 includes a first prism base 119 and a plurality of first prisms 113. The plurality of first prisms 113 are arranged continuously and without intervals on the first prism base 119. The cross section of the first prism 113 is an isosceles triangle, and the vertex A is a right angle. The first prism 113 has three edges, including two first bottom edges 115 and a first top edge 116. The two first bottom edges 115 are arranged on the first prism base 119. The height H1 of the first top edge 116 is 30, and the spacing D1 between adjacent first top edges 116 is 60 microns. The first prism layer 112 is arranged on the upper surface of the first base film 111, and the first prism 113 is integrally formed with the first prism base 119, and the first prism base is arranged on the upper surface of the first base film. The first top ridge 116 protrudes from the first base film 111 .

[0152] The lower surface of the first base film 111 is provided with a back coating layer 118. The back coating layer 118 is a UV resin, and is dispersed with 3-5 micron PBMA micro beads and antistatic agents. The surface resistance is 10 to the 11th power, the hardness is 2H, the haze is 3%, and the thickness is 5 microns.

[0153] The second structural layer film 120 includes a second base film 121 and a second prism layer 122. The second base film 121 is a 125-micron optical grade chemically treated PET film. The second prism layer 122 includes a second prism base 129 and a plurality of second prisms 123. The plurality of second prisms 123 are continuously arranged without spacing on the second prism base 129. The second prism layer 122 is arranged on the upper surface of the second base film 121; the cross section of the second prism 123 is an isosceles triangle, and the vertex angle B is a right angle. The second prism 123 has three edges, including two second bottom edges 125 and a second top edge 126. The two second bottom edges 125 are arranged on the second prism base 129. The height H2 of the second top edge is 25 microns, and the second top edge 126 is 25 microns along the length direction of the second prism 123. Figure 1 As shown, the height of the second top edge 126 varies perpendicular to the paper surface, and the maximum height difference of the second top edge 126 is 2 microns. The spacing D2 between adjacent second top edges is 50 microns. The second prism 123 is integrally formed with the second prism substrate 129, and the second prism substrate 129 is disposed on the upper surface of the second base film 121. The second top edge 126 protrudes from the second base film 121. Figure 6 As shown, spherical particles are distributed in the second prism layer 122, and the spherical particles are used to make the second prism layer 122 reach the required haze. Manufacturing method: Powder material is added into the prism structure resin and ground, and ground in a sand mill with a diameter of 1-3mm pick beads for 20-40 minutes to ensure the particle size and spherical structure.

[0154] The lower surface of the second base film 121 is provided with a composite adhesive layer 130. The composite adhesive layer 130 is glue, and PBMA micro beads of 3-5 microns are dispersed, reaching a haze of 20%.

[0155] The first prism 113 is attached to the second base film 121 through the composite adhesive layer 130. The first top edge is inserted into the composite adhesive layer by 0.5-2 microns. The included angle C between the projection line of the first top edge 116 and the projection line of the second top edge 126 is 76 degrees.

[0156] The back coating components of the first structural layer film include, by mass percentage:

[0157] 12% of 6-functional aliphatic polyurethane acrylic prepolymer; 6% of 3-4-functional aliphatic polyurethane acrylic prepolymer; 4.5% of reactive diluent-TMPTA; 4.5% of reactive diluent-HDDA; 1% of photoinitiator 184; 1% of photoinitiator 1173; 0.5% of Silok771N (dispersant); 0.3% of antistatic agent; 0.3% of 3-5 micron PBMA or PMMA microbeads; the rest is solvent, which is toluene, butanone and cyclohexanone, and the solvent ratio is 4:1:1.

[0158] The components of the first prism layer include, by mass percentage:

[0159] OPPEA 28.5%; epoxy acrylate prepolymer 14.5%; EOEOEA 15%; BPA (EO) 10DA 29%; hydroxyethyl acrylate 5%; photoinitiator 184 3%; TPO 2%; Jintuan Chemical KEPERSURF-1577E (acrylate leveling agent) 3%.

[0160] The components of the composite adhesive layer include, by mass percentage:

[0161] Sartomer CN966H90 (2-functional aliphatic polyurethane acrylic prepolymer) 8%; Runao Chemical E8210 (4-functional aliphatic polyurethane acrylic prepolymer) 4%; acryloyl morpholine 5%; methacrylate phosphate 0.2%; HDDA 1%; photoinitiator 184 0.8%; photoinitiator 1173 0.8%; 3-5 micron PBMA or PMMA microbeads 0.9%; the rest is solvent, the solvent is toluene and butanone, and the solvent ratio is 1:1.

[0162] The components of the second prism layer include, by mass percentage:

[0163] OPPEA 34%; Allnex resin E3708 (epoxy acrylate prepolymer) 15%; EOEOEA 9%; BPA (EO) 20DA 10%; BPA (EO) 3DA 14%; DPHA 10%; photoinitiator 184 3%; photoinitiator TPO 3%; Digao Chemical TEGO 2100 (reactive silicone leveling agent) 2%; kaolin 0.07%.

[0164] Example 8

[0165] like Figure 7 , Figure 2 and Figure 3 As shown, the laminating film 100 for a liquid crystal display comprises a first structural layer film 110 and a second structural layer film 120 from bottom to top.

[0166] The first structural layer film 110 includes a first base film 111 and a first prism layer 112. The first base film 111 is a 125 micron optical grade chemically treated PET film. The first prism layer 112 includes a first prism base 119 and a plurality of first prisms 113. The plurality of first prisms 113 are arranged on the first prism base 119. The cross section of the first prism 113 is an isosceles triangle, and the vertex A is a right angle. The first prism 113 has three edges, including two first bottom edges 115 and a first top edge 116. The two first bottom edges 115 are arranged on the first prism base 119. The height H1 of the first top edge 116 is 30 microns. The spacing D1 between adjacent first top edges 116 is 60 microns. The first prism layer 112 is arranged on the upper surface of the first base film 111. The first prism 113 is integrally formed with the first prism base 119, and the first prism base is arranged on the upper surface of the first base film. The first top ridge 116 protrudes from the first base film 111 .

[0167] The lower surface of the first base film 111 is provided with a back coating layer 118. The back coating layer 118 is a UV resin, and is dispersed with 3-5 micron PBMA micro beads and antistatic agents. The surface resistance is 10 to the 11th power, the hardness is 2H, the haze is 3%, and the thickness is 5 microns.

[0168] The second structural layer film 120 includes a second base film 121 and a second prism layer 122. The second base film 121 is a 125-micron optical grade chemically treated PET film. The second prism layer 122 includes a second prism base 129 and a plurality of second prisms 123. The plurality of second prisms 123 are continuously arranged without spacing on the second prism base 129. The second prism layer 122 is arranged on the upper surface of the second base film 121; the cross section of the second prism 123 is an isosceles triangle, and the vertex angle B is a right angle. The second prism 123 has three edges, including two second bottom edges 125 and a second top edge 126. The two second bottom edges 125 are arranged on the second prism base 129. The height H2 of the second top edge is 25 microns, and the second top edge 126 is 25 microns along the length direction of the second prism 123. Figure 1 As shown, the height of the second top edge 126 changes perpendicular to the paper surface, and the maximum height difference of the second top edge 126 is 2 microns. The spacing D2 between adjacent second top edges is 50 microns. The second prism 123 is integrally formed with the second prism substrate 129, and the second prism substrate 129 is disposed on the upper surface of the second base film 121. The second top edge 126 protrudes from the second base film 121.

[0169] The lower surface of the second base film 121 is provided with a composite adhesive layer 130. Figure 7As shown, the composite adhesive layer 130 is glue, and 3-5 micron PBMA microbeads and spherical particles are dispersed, reaching 40% haze. Manufacturing method: Add powder material into composite adhesive solution (without PMMA or PBMA microbeads) and grind, grind in a sand mill with a diameter of 1-3mm pick beads for 20-40 minutes to ensure the particle size and spherical structure, and then add 3-5 micron PMMA or PBMA microbeads and stir evenly to obtain a coating liquid.

[0170] The first prism 113 is attached to the second base film 121 through the composite adhesive layer 130. The first top edge is inserted into the composite adhesive layer by 0.5-2 microns. The included angle C between the projection line of the first top edge 116 and the projection line of the second top edge 126 is 76 degrees.

[0171] The back coating components of the first structural layer film include, by mass percentage:

[0172] Allnex resin E1290N (6-functional aliphatic polyurethane acrylate prepolymer) 12%; Allnex resin E1258 (3-functional aliphatic polyurethane acrylate prepolymer) 6%; reactive diluent-TMPTA 4.5%; reactive diluent-HDDA 4.5%; photoinitiator 184 1%; photoinitiator 1173 1%; Sartomer epoxy acrylate CN 151 (dispersant) 0.5%; antistatic agent 0.3%; 3-5 micron PBMA or PMMA microbeads 0.3%; the rest is solvent, the solvent is toluene, butanone and cyclohexanone, and the solvent ratio is 4:1:1.

[0173] The components of the first prism layer include, by mass percentage:

[0174] OPPEA 29%; Allnex resin E3708 (epoxy acrylate prepolymer) 15%; EOEOEA 14%; BPA (EO) 10DA 29%; Hydroxyethyl acrylate 4%; Photoinitiator 184 3%; Photoinitiator TPO 3%; Mo Neng Chemical UV1201 (acrylate leveling agent) 3%.

[0175] The components of the composite adhesive layer include, by mass percentage:

[0176] Lida Chemical U-8663 (2-functional aliphatic polyurethane acrylic prepolymer) 7.8%; Runao Chemical L8112 (4-functional aliphatic polyurethane acrylic prepolymer) 4%; acryloyl morpholine 5%; methacrylate phosphate 0.4%; HDDA 1.5%; photoinitiator 184 0.7%; photoinitiator 1173 0.8%; 3-5 micron PBMA or PMMA microbeads 0.9%; powdered calcium carbonate 1%; the rest is solvent, the solvent is toluene and butanone, the solvent ratio is 2:1. The components of the second prism layer include, by mass percentage:

[0177] OPPEA 33%; Meiyuan Chemical ME2100 (epoxy acrylate prepolymer) 15%; EOEOEA 10%; BPA (EO) 20DA 9%; BPA (EO) 3DA 14%; DPHA 10%; photoinitiator 184 3%; photoinitiator TPO 3%; Digao Chemical TEGO 2100 (reactive silicone leveling agent) 3%.

[0178] Example 9

[0179] like Figure 8 , Figure 2 and Figure 3 As shown, the laminating film 100 for a liquid crystal display comprises a first structural layer film 110 and a second structural layer film 120 from bottom to top.

[0180] The first structural layer film 110 includes a first base film 111 and a first prism layer 112. The first base film 111 is a 125 micron optical grade chemically treated PET film. The first prism layer 112 includes a first prism substrate 119 and a plurality of first prisms 113. The plurality of first prisms 113 are continuously arranged without spacing on the first prism substrate 119. The cross section of the first prism 113 is an isosceles triangle, and the vertex angle A is a right angle. The first prism 113 has three edges, including two first bottom edges 115 and a first top edge 116. The two first bottom edges 115 are arranged on the first prism substrate 119. The height H1 of the first top edge 116 is 30 or 35 microns. The first prism 113 with a first top edge height H1 of 30 microns is spaced from the first prism 113 with a first top edge height of 35 microns. The spacing D1 between adjacent first top edges 116 is 70 or 60 microns. The distance D1 between two adjacent first top edges 116 with a height H1 of 30 microns is 60 microns. The distance D1 between two adjacent first top edges 116 with a height H1 of 35 microns is 70 microns. The first prism layer 112 is disposed on the upper surface of the first base film 111. The first prism 113 is integrally formed with the first prism substrate 119, and the first prism substrate is disposed on the upper surface of the first base film. The first top edge 116 protrudes from the first base film 111.

[0181] The lower surface of the first base film 111 is provided with a back coating layer 118. The back coating layer 118 is a UV resin, and is dispersed with 3-5 micron PBMA micro beads and antistatic agents. The surface resistance is 10 to the 11th power, the hardness is 2H, the haze is 3%, and the thickness is 5 microns.

[0182] The second structural layer film 120 includes a second base film 121 and a second prism layer 122. The second base film 121 is a 125-micron optical grade chemically treated PET film. The second prism layer 122 includes a second prism base 129 and a plurality of second prisms 123. The plurality of second prisms 123 are continuously arranged without spacing on the second prism base 129. The second prism layer 122 is arranged on the upper surface of the second base film 121; the cross section of the second prism 123 is an isosceles triangle, and the vertex angle B is a fillet with a radius of 2 microns. The second prism 123 has three edges, including two second bottom edges 125 and a second top edge 126. The two second bottom edges 125 are arranged on the second prism base 129. The height H2 of the second top edge is 30 microns, and the second top edge is 126 along the length direction of the second prism 123. Figure 1 As shown, the height of the second top edge 126 varies perpendicular to the paper surface, and the maximum height difference of the second top edge 126 is 2 microns. The spacing D2 between adjacent second top edges is 60 microns. The second prism 123 is integrally formed with the second prism substrate 129, and the second prism substrate 129 is disposed on the upper surface of the second base film 121. The second top edge 126 protrudes from the second base film 121.

[0183] The lower surface of the second base film 121 is provided with a composite adhesive layer 130. Figure 8 As shown, spherical particles are dispersed in the composite adhesive layer 130, and a microstructure molding method is used to achieve a haze of 40%. Manufacturing method: Powder material is added to the composite adhesive and ground, and ground in a sand mill with a diameter of 1-3mm beads for 20-40 minutes to ensure the particle size and spherical structure.

[0184] The first prism 113 is attached to the second base film 121 through the composite adhesive layer 130. The first top edge is inserted into the composite adhesive layer by 0.5-2 microns. The included angle C between the projection line of the first top edge 116 and the projection line of the second top edge 126 is 69 degrees.

[0185] The back coating components of the first structural layer film include, by mass percentage:

[0186] Sartomer CN9006 (6-functional aliphatic polyurethane acrylate prepolymer) 12%; Sartomer CN9008 (3-functional aliphatic polyurethane acrylate prepolymer) 6%; reactive diluent-TMPTA 4.5%; reactive diluent-HDDA 4.5%; photoinitiator 184 1%; photoinitiator 1173 1%; Sartomer epoxy acrylate CN 151 (dispersant) 0.5%; antistatic agent 0.3%; 3-5 micron PBMA or PMMA microbeads 0.3%; the rest is solvent, the solvent is toluene, butanone and cyclohexanone, and the solvent ratio is 4:1:1.

[0187] The components of the first prism layer include, by mass percentage:

[0188] OPPEA 29%; Meiyuan Chemical ME2100 (epoxy acrylate prepolymer) 14.5%; EOEOEA 14.5%; BPA (EO) 10DA 28%; hydroxyethyl acrylate 5%; photoinitiator 184 3%; photoinitiator TPO 3%; Jintuan Chemical KEPERSURF-1577E (acrylate leveling agent) 3%.

[0189] The components of the composite adhesive layer include, by mass percentage:

[0190] Sartomer CN966H90 (2-functional aliphatic polyurethane acrylic prepolymer) 8%; Runao Chemical L8112 (4-functional aliphatic polyurethane acrylic prepolymer) 4%; acryloyl morpholine 4.8%; methacrylate phosphate 0.4%; HDDA 2%; photoinitiator 184 0.5%; photoinitiator 1173 0.6%; photoinitiator TPO 0.4%; NTCADD FM30 Beijing Baiyuan Chemical Co., Ltd. (phosphate monomer) 0.6%; powdered calcium carbonate 0.8%; the rest is solvent, the solvent is toluene and butanone, the solvent ratio is 1:1. The components of the second prism layer include, by mass percentage:

[0191] OPPEA 35%; allnex resin E3708 (epoxy acrylate prepolymer) 14%; EOEOEA 9%; BPA (EO) 20DA 9%; BPA (EO) 3DA 15%; DPHA 10%; photoinitiator 184 3%; photoinitiator TPO 3%; BYK-371 (reactive silicone leveling agent) 2%.

[0192] Embodiment 10:

[0193] like Figure 4 , Figure 2 and Figure 3 As shown, the laminating film 100 for a liquid crystal display comprises a first structural layer film 110 and a second structural layer film 120 from bottom to top.

[0194] The first structural layer film 110 includes a first base film 111 and a first prism layer 112. The first base film 111 is a 125 micron optical grade chemically treated PET film. The first prism layer 112 includes a first prism substrate 119 and a plurality of first prisms 113. The plurality of first prisms 113 are continuously arranged without spacing on the first prism substrate 119. The cross section of the first prism 113 is an isosceles triangle, and the vertex angle A is a right angle. The first prism 113 has three edges, including two first bottom edges 115 and a first top edge 116. The two first bottom edges 115 are arranged on the first prism substrate 119. The height H1 of the first top edge 116 is 30 or 35 microns. The first prism 113 with a first top edge height H1 of 30 microns is spaced from the first prism 113 with a first top edge height of 35 microns. The spacing D1 between adjacent first top edges 116 is 70 or 60 microns. The distance D1 between two adjacent first top edges 116 with a height H1 of 30 microns is 60 microns. The distance D1 between two adjacent first top edges 116 with a height H1 of 35 microns is 70 microns. The first prism layer 112 is disposed on the upper surface of the first base film 111. The first prism 113 is integrally formed with the first prism substrate 119, and the first prism substrate is disposed on the upper surface of the first base film. The first top edge 116 protrudes from the first base film 111.

[0195] The lower surface of the first base film 111 is provided with a back coating layer 118. The back coating layer 118 is a UV resin, and is dispersed with 3-5 micron PBMA micro beads and antistatic agents. The surface resistance is 10 to the 11th power, the hardness is 2H, the haze is 3%, and the thickness is 5 microns.

[0196] The second structural layer film 120 includes a second base film 121 and a second prism layer 122. The second base film 121 is a 125-micron optical grade chemically treated PET film. The second prism layer 122 includes a second prism base 129 and a plurality of second prisms 123. The plurality of second prisms 123 are continuously arranged without spacing on the second prism base 129. The second prism layer 122 is arranged on the upper surface of the second base film 121; the cross section of the second prism 123 is an isosceles triangle, and the vertex angle B is a fillet with a radius of 3 microns. The second prism 123 has three edges, including two second bottom edges 125 and a second top edge 126. The two second bottom edges 125 are arranged on the second prism base 129. The height H2 of the second top edge is 30 microns, and the second top edge is 126 along the length direction of the second prism 123. Figure 1 As shown, the height of the second top edge 126 varies in the direction perpendicular to the paper surface, and the maximum height difference of the second top edge 126 is 2 microns. The spacing D2 between adjacent second top edges is 60 microns. The second prism 123 is integrally formed with the second prism substrate 129, and the second prism substrate 129 is disposed on the upper surface of the second base film 121. The second top edge 126 protrudes from the second base film 121.

[0197] The lower surface of the second base film 121 is provided with a composite adhesive layer 130. The composite adhesive layer 130 is glue, and PBMA micro beads of 3-5 microns are dispersed, reaching a haze of 40%.

[0198] The first prism 113 is attached to the second base film 121 through the composite adhesive layer 130. The first top edge is inserted into the composite adhesive layer by 0.5-2 microns. The included angle C between the projection line of the first top edge 116 and the projection line of the second top edge 126 is 73 degrees.

[0199] The back coating components of the first structural layer film include, by mass percentage:

[0200] Sartomer CN9006 (6-functional aliphatic polyurethane acrylic prepolymer) 12%; Sartomer CN9008 (3-functional aliphatic polyurethane acrylic prepolymer) 6%; reactive diluent-TMPTA 4.5%; reactive diluent-HDDA 4.5%; photoinitiator 184 1%; photoinitiator 1173 1%; Silok771N (dispersant) 0.5%; antistatic agent 0.3%; 3-5 micron PBMA or PMMA microbeads 0.3%; the rest is solvent, the solvent is toluene, butanone and cyclohexanone. The solvent ratio is 4:1:1.

[0201] The components of the first prism layer include, by mass percentage:

[0202] OPPEA 29%; Meiyuan Chemical ME2100 (epoxy acrylate prepolymer) 14%; EOEOEA 14%; BPA (EO) 10DA 30%; Hydroxyethyl acrylate 5%; Photoinitiator 184 2%; Photoinitiator TPO 3%; Mo Neng Chemical UV1201 (acrylate leveling agent) 3%.

[0203] The components of the composite adhesive layer include, by mass percentage:

[0204] Lida Chemical U-8663 (2-functional aliphatic polyurethane acrylic prepolymer) 7.9%; Runao Chemical L8112 (4-functional aliphatic polyurethane acrylic prepolymer) 3.8%; acryloyl morpholine 4.6%; methacrylate phosphate 0.3%; HDDA 1.6%; photoinitiator 184 0.7%; photoinitiator 1173 0.8%; the rest is solvent, the solvent is toluene and butanone. The solvent ratio is 1:1.

[0205] The components of the composite adhesive layer also include, by mass percentage: 3-5 micron PBMA or PMMA microbeads 1.7%

[0206] The components of the second prism layer include, by mass percentage:

[0207] OPPEA 34%; allnex resin E3708 (epoxy acrylate prepolymer) 14%; EOEOEA 10%; BPA (EO) 20DA 10%; BPA (EO) 3DA 15%; DPHA 9%; photoinitiator 184 3%; photoinitiator TPO 2%; BYK-371 (reactive silicone leveling agent) 3%.

[0208] Embodiment 11:

[0209] like Figures 1 to 3 As shown, the laminating film 100 for a liquid crystal display comprises a first structural layer film 110 and a second structural layer film 120 from bottom to top.

[0210] The first structural layer film 110 includes a first base film 111 and a first prism layer 112. The first base film 111 is a 125 micron optical grade chemically treated PET film. The first prism layer 112 includes a first prism base 119 and a plurality of first prisms 113. The plurality of first prisms 113 are arranged continuously and without intervals on the first prism base 119. The cross section of the first prism 113 is an isosceles triangle, and the vertex A is a right angle. The first prism 113 has three edges, including two first bottom edges 115 and a first top edge 116. The two first bottom edges 115 are arranged on the first prism base 119. The height H1 of the first top edge 116 is 30 microns, and the spacing D1 between adjacent first top edges 116 is 60 microns. The first prism layer 112 is arranged on the upper surface of the first base film 111. The first prism 113 is integrally formed with the first prism base 119, and the first prism base is arranged on the upper surface of the first base film. The first top ridge 116 protrudes from the first base film 111 .

[0211] The lower surface of the first base film 111 is provided with a back coating layer 118. The back coating layer 118 is a UV resin, and is dispersed with 3-5 micron PBMA micro beads and antistatic agents. The surface resistance is 10 to the 11th power, the hardness is 2H, the haze is 3%, and the thickness is 5 microns.

[0212] The second structural layer film 120 includes a second base film 121 and a second prism layer 122. The second base film 121 is a 125-micron optical grade chemically treated PET film. The second prism layer 122 includes a second prism base 129 and a plurality of second prisms 123. The plurality of second prisms 123 are continuously arranged without spacing on the second prism base 129. The second prism layer 122 is arranged on the upper surface of the second base film 121; the cross section of the second prism 123 is an isosceles triangle, and the vertex angle B is a right angle. The second prism 123 has three edges, including two second bottom edges 125 and a second top edge 126. The two second bottom edges 125 are arranged on the second prism base 129. The height H2 of the second top edge is 25 microns, and the second top edge 126 is 25 microns along the length direction of the second prism 123. Figure 1 As shown, the height of the second top edge 126 varies in the direction perpendicular to the paper surface, and the maximum height difference of the second top edge 126 is 2 microns. The spacing D2 between adjacent second top edges is 50 microns. The second prism 123 is integrally formed with the second prism substrate 129, and the second prism substrate 129 is disposed on the upper surface of the second base film 121. The second top edge 126 protrudes from the second base film 121.

[0213] The lower surface of the second base film 121 is provided with a composite adhesive layer 130. The composite adhesive layer 130 is glue, and PBMA micro beads of 3-5 microns are dispersed, reaching a haze of 50%.

[0214] The first prism 113 is attached to the second base film 121 through the composite adhesive layer 130. The first top edge is inserted into the composite adhesive layer by 0.5-2 microns. The included angle C between the projection line of the first top edge 116 and the projection line of the second top edge 126 is 76 degrees.

[0215] The back coating components of the first structural layer film include, by mass percentage:

[0216] Allnex resin E1290N (6-functional aliphatic polyurethane acrylate prepolymer) 12%; Allnex resin E1258 (3-functional aliphatic polyurethane acrylate prepolymer) 6%; reactive diluent-TMPTA 4.5%; reactive diluent-HDDA 4.5%; photoinitiator 184 1%; photoinitiator 1173 1%; Sartomer epoxy acrylate CN 151 (dispersant) 0.5%; antistatic agent 0.3%; 3-5 micron PBMA or PMMA microbeads 0.3%; the rest is solvent, the solvent is toluene, butanone and cyclohexanone. The solvent ratio is 4:1:1.

[0217] The components of the first prism layer include, by mass percentage:

[0218] OPPEA 28%; Meiyuan Chemical ME2100 (epoxy acrylate prepolymer) 15%; EOEOEA 14%; BPA (EO) 10DA 30%; hydroxyethyl acrylate 4.5%; photoinitiator 184 3%; photoinitiator TPO 2.5%; Jintuan Chemical KEPERSURF-1577E (acrylate leveling agent) 3%.

[0219] The components of the composite adhesive layer include, by mass percentage:

[0220] Sartomer CN966H90 (2-functional aliphatic polyurethane acrylic prepolymer) 7.8%; Runao Chemical L8112 (4-functional aliphatic polyurethane acrylic prepolymer) 3.8%; acryloyl morpholine 4.9%; methacrylate phosphate 0.4%; HDDA 1.8%; photoinitiator 184 0.7%; photoinitiator 1173 0.8%; the rest is solvent, the solvent is toluene and butanone. The solvent ratio is 1:1.

[0221] The components of the composite adhesive layer also include, by mass percentage: 3-5 micron PBMA or PMMA microbeads 2%

[0222] The components of the second prism layer include, by mass percentage:

[0223] OPPEA 34%; Meiyuan Chemical ME2100 (epoxy acrylate prepolymer) 14%; EOEOEA 9%; BPA (EO) 20DA 10%; BPA (EO) 3DA 15%; DPHA 10%; photoinitiator 184 3%; photoinitiator TPO 3%; BYK-371 (reactive silicone leveling agent) 2%.

[0224] Embodiment 12:

[0225] like Figures 1 to 3 As shown, the laminating film 100 for a liquid crystal display comprises a first structural layer film 110 and a second structural layer film 120 from bottom to top.

[0226] The first structural layer film 110 includes a first base film 111 and a first prism layer 112. The first base film 111 is a 125 micron optical grade chemically treated PET film. The first prism layer 112 includes a first prism base 119 and a plurality of first prisms 113. The plurality of first prisms 113 are arranged continuously and without intervals on the first prism base 119. The cross section of the first prism 113 is an isosceles triangle, and the vertex A is a right angle. The first prism 113 has three edges, including two first bottom edges 115 and a first top edge 116. The two first bottom edges 115 are arranged on the first prism base 119. The height H1 of the first top edge 116 is 30 microns, and the spacing D1 between adjacent first top edges 116 is 60 microns. The first prism layer 112 is arranged on the upper surface of the first base film 111. The first prism 113 is integrally formed with the first prism base 119, and the first prism base is arranged on the upper surface of the first base film. The first top ridge 116 protrudes from the first base film 111 .

[0227] The lower surface of the first base film 111 is provided with a back coating layer 118. The back coating layer 118 is a UV resin, and is dispersed with 3-5 micron PBMA micro beads and antistatic agents. The surface resistance is 10 to the 11th power, the hardness is 2H, the haze is 3%, and the thickness is 5 microns.

[0228] The second structural layer film 120 includes a second base film 121 and a second prism layer 122. The second base film 121 is a 125-micron optical grade chemically treated PET film. The second prism layer 122 includes a second prism base 129 and a plurality of second prisms 123. The plurality of second prisms 123 are continuously arranged without spacing on the second prism base 129. The second prism layer 122 is arranged on the upper surface of the second base film 121; the cross section of the second prism 123 is an isosceles triangle, and the vertex angle B is a right angle. The second prism 123 has three edges, including two second bottom edges 125 and a second top edge 126. The two second bottom edges 125 are arranged on the second prism base 129. The height H2 of the second top edge is 20 microns, and the second top edge 126 is 1.2 microns along the length direction of the second prism 123. Figure 1 As shown, the height of the second top edge 126 varies perpendicular to the paper surface, and the maximum height difference of the second top edge 126 is 2 microns. The spacing D2 between adjacent second top edges is 40 microns. The second prism 123 is integrally formed with the second prism substrate 129, and the second prism substrate 129 is disposed on the upper surface of the second base film 121. The second top edge 126 protrudes from the second base film 121.

[0229] The lower surface of the second base film 121 is provided with a composite adhesive layer 130. The composite adhesive layer 130 is glue, and PBMA micro beads of 3-5 microns are dispersed, reaching a haze of 40%.

[0230] The first prism 113 is attached to the second base film 121 through the composite adhesive layer 130. The first top edge is inserted into the composite adhesive layer by 0.5-2 microns. The included angle C between the projection line of the first top edge 116 and the projection line of the second top edge 126 is 73 degrees.

[0231] The back coating components of the first structural layer film include, by mass percentage:

[0232] Allnex resin E1290N (6-functional aliphatic polyurethane acrylic prepolymer) 12%; Allnex resin E1258 (3-functional aliphatic polyurethane acrylic prepolymer) 6%; reactive diluent-TMPTA 4.5%; reactive diluent-HDDA 4.5%; photoinitiator 184 1%; photoinitiator 1173 1%; Digo Chemical TEGO-688 (dispersant) 0.5%; antistatic agent 0.3%; 3-5 micron PBMA or PMMA microbeads 0.3%; the rest is solvent, the solvent is toluene, butanone and cyclohexanone. The solvent ratio is 4:1:1.

[0233] The components of the first prism layer include, by mass percentage:

[0234] OPPEA 28%; Allnex resin E3708 (epoxy acrylate prepolymer) 14%; EOEOEA 15%; BPA (EO) 10DA 29%; Hydroxyethyl acrylate 5%; Photoinitiator 184 3%; Photoinitiator TPO 3%; Mo Neng Chemical UV1201 (acrylate leveling agent) 3%.

[0235] The components of the composite adhesive layer include, by mass percentage:

[0236] Lida Chemical U-8663 (2-functional aliphatic polyurethane acrylic prepolymer) 7.7%; Runao Chemical L8112 (4-functional aliphatic polyurethane acrylic prepolymer) 3.9%; acryloyl morpholine 4.5%; methacrylate phosphate 0.4%; HDDA 1.7%; photoinitiator 184 0.7%; photoinitiator 1173 0.8%; the rest is solvent, the solvent is toluene and butanone. The solvent ratio is 1:1.

[0237] The components of the composite adhesive layer also include, by mass percentage: 3-5 micron PBMA or PMMA microbeads 1.7%

[0238] The components of the second prism layer include, by mass percentage:

[0239] OPPEA 34%; Meiyuan Chemical ME2100 (epoxy acrylate prepolymer) 15%; EOEOEA 10%; BPA (EO) 20DA 9%; BPA (EO) 3DA 15%; DPHA 9%; photoinitiator 184 3%; photoinitiator TPO 3%; Digao Chemical TEGO2100 (reactive silicone leveling agent) 2%.

[0240] Process steps of embodiments 1-2, 4-5, 7-8, 10-12

[0241] 1) First, apply a back coating layer on the back of the first base film, then dry it at 80-130°C for 30 seconds to 1 minute, and then UV cure it at 200-400mj of UV light.

[0242] 2) Then, a first prism layer is coated on the front side of the first base film, with a UV light dosage of 30-100 mj.

[0243] 3) Apply composite glue on the back of the second base film, and dry it at 80-130°C for 30 seconds to 1 minute; then laminate it with the first prism layer in step 2), and then UV cure it with a UV light of 600-800mj.

[0244] 4) Coat the second prism layer on the upper surface of the laminated second base film, and then UV cure it with UV light of 50-100mj and 300-500mj.

[0245] Embodiment 3, 6, 9 process steps:

[0246] 1) First, apply a back coating layer on the back of the first base film, then dry it at a temperature of 80-130°C for 30 seconds to 1 minute, and then UV cure it at a UV light of 200-400mj.

[0247] 2) Coating the first prism layer on the upper surface of the first base film, and then UV curing, with the UV light amount of 30-100mj.

[0248] 3) Apply composite glue-matt on the back of the second base film, and then use microstructure molding technology to make the composite glue reach the required haze; UV curing, UV light 30-100mj. Then adhere to the first prism layer in 2); UV curing again, UV light 600-800mj.

[0249] 4) Coat the second prism layer on the upper surface of the laminated second base film, and then UV cure it with UV light 50-100mj+300-500mj.

[0250] The pre-rotation angle described in the present invention means that when the second prism layer is produced, the second base film is in a rectangular shape, and the second top edge of the second prism is pre-set to an acute angle or an obtuse angle with the edge of the second base film. If the first prism layer does not use a pre-rotation angle, the first top edge of the first prism is perpendicular or parallel to the edge of the first base film. When the first prism layer and the second prism layer are attached, the edges of the first base film and the second base film are aligned, so that the first top edge and the second top edge are set at an angle C (such as Figure 3 The first prism layer may also be pre-rotated.

[0251] 1. Comparative Example 1: From bottom to top in the backlight, the high-transmittance increases by 93 degrees, and the high-fog small-pitch increases by 3 degrees.

[0252] 1) High transmittance increased by 93 degrees: the prism base film is a 250-micron optical-grade chemically treated PET film; the distance between adjacent top edges is 50 microns, the top edge height is 25 microns, the prism cross-section is an isosceles triangle, the top angle is a right angle, the top of the peak of the top angle is a sharp angle, and a back coating is provided on the lower surface of the base film, and the back coating haze is 3%.

[0253] 2) High fog and small spacing increase by 3 degrees: the prism base film is a 250-micron optical grade chemically treated PET film; the spacing between adjacent top edges is 20 microns, the top edge height is 10 microns, the prism cross-section is an isosceles triangle, the top angle is a right angle, the peak of the top angle is a sharp angle, and a back coating is provided on the lower surface of the base film, and the back coating haze is 40%.

[0254] 2. Comparative Example 2: From bottom to top, the backlight is ordinary POP and high-transmittance diffusion

[0255] 1) Ordinary POP:

[0256] The second structural layer base film is a 125 micron optical grade chemically treated PET film; the spacing between adjacent top edges is 60 microns, the prism is straight (the spacing remains unchanged), the top edge height is 30 microns, the prism cross section is an isosceles triangle, the top angle is a right angle, and the top of the peak of the top angle is a sharp angle;

[0257] The back side of the second structural layer and the front side of the first structural layer are bonded together by a composite glue, the composite glue does not contain micro beads and spherical particles, and no micro-structure molding method is used to achieve haze;

[0258] The first structural layer base film is a 125-micron optical-grade chemically treated PET film, with a spacing of 60 microns between adjacent top edges, a straight prism (spacing remains unchanged), a top edge height of 30 microns, an isosceles triangle cross section, a right angle, and a sharp corner at the top of the peak;

[0259] The first structural layer is provided with a back coating layer on the lower surface of the base film, and the back coating haze is 3%.

[0260] The angle formed by the extension lines of the second prism structure layer and the first prism structure layer is 90°.

[0261] 2) High transparency diffusion:

[0262] Haze and light transmittance both reach 89%

[0263] 3. Comparative Example 3: From bottom to top in the backlight, the high fog increases by 93 degrees, and the high fog small spacing increases by 3 degrees

[0264] 1) Increase of 93 degrees under high fog: the prism base film is a 250-micron optical-grade chemically treated PET film; the distance between adjacent top edges of the prism structure is 50 microns, the top edge height is 25 microns, the prism cross-section is an isosceles triangle, the top angle is a right angle, the top of the peak of the top angle is a sharp angle, and a back coating is provided on the lower surface of the base film, and the back coating haze is 40%.

[0265] 2) High fog and small spacing increase by 3 degrees: the prism base film is a 250-micron optical grade chemically treated PET film; the spacing between adjacent top edges of the prism structure is 20 microns, the top edge height is 10 microns, the prism cross-section is an isosceles triangle, the top angle is a right angle, the peak of the top angle is a sharp angle, and a back coating is provided on the lower surface of the base film, and the back coating haze is 40%.

[0266] Comparison between Examples 1-3, 7-12 and Comparative Example 1: Direct backlight. Backlight film test structure (from bottom to top): reflector, lamp beads, diffuser, test film.

[0267]

[0268]

[0269] Comparison between Examples 1-3, 7-12 and Comparative Example 2: Direct backlight, backlight film test structure (from bottom to top): reflector, lamp beads, diffuser, test film.

[0270]

[0271]

[0272] Comparison between Examples 4-6 and Comparative Example 3: Edge-type backlight, backlight film test architecture (from bottom to top): reflector, light bar, light guide plate, test film.

[0273]

[0274]

[0275] The formula of each raw material of the present invention can be freely selected within the aforementioned content range to replace the above embodiments. After experimental detection, the following effects of the present invention can be achieved.

[0276] Description of the test method:

[0277] 1. Backlight module brightness test: Turn on the backlight, wait for the backlight source to stabilize, put in the test film under normal working current and voltage, use SR-3A equipment to test the brightness of 9 points, and take the average value.

[0278] 2. Backlight module viewing angle test: Turn on the backlight, wait for the backlight source to stabilize, then put in the test film. Under normal working current and voltage, use the SR-3A device to test the single-point brightness and the brightness at different angles. The angle that is higher than and closest to one-third of the single-point brightness is taken as the viewing angle value.

[0279] 3. Visual effect after the backlight module covers the LCD screen: LCD screen normal working brightness, WRGB four colors (main white field) visual observation at different angles.

[0280] 4. Upper prism scratch resistance test: Use 40% haze back coating as friction material, fix the friction surface upward on the flat glass, place the test object with the surface coating facing downward on the friction material, and make the prism peak direction perpendicular to the moving direction. Place a protective film on the back of the test object, and place a load weight on the protective film. Pull out the test object at a uniform speed and observe it under a three-wavelength lamp or a microscope. The maximum weight without obvious scratches is the test data.

[0281] Based on the comparative data of the above embodiments, the laminating film of the present invention has the following effects:

[0282] 1. Under DLED backlight, compared with the two enhanced brightness images (Comparative Example 1), the viewing angle and scratch resistance of Examples 1-12 of the present invention are greatly improved under the premise of equivalent or slightly higher brightness, and there is no interference problem.

[0283] 2. Under DLED backlight, compared with ordinary POP plus a high-transmittance top expansion (Comparative Example 2), Examples 2, 9 and 10 of the present invention are superior to Comparative Example 2 in terms of brightness, viewing angle and scratch resistance; the brightness and scratch resistance of other comparative examples are greatly improved under the premise that the viewing angle can meet the requirements of conventional products.

[0284] 3. Under ELED backlight, compared with increasing high haze under high haze (Comparative Example 3), Examples 4 and 6 of the present invention are slightly greater than Comparative Example 3 in terms of brightness and viewing angle. Example 5 has the same brightness as Comparative Example 3, and the viewing angle is significantly greater than Comparative Example 3. At the same time, Examples 4-6 have significantly improved scratch resistance, and there is no interference problem.

[0285] With the popularization of TFT-LCD liquid crystal display technology, the demand for optical films for backlight modules is increasing. As the size continues to increase, the stiffness requirements are increased, the overall thickness is gradually reduced, and the assembly requirements are becoming increasingly simplified and automated. Laminating films have become a major trend in the optical film industry. However, the problems of poor shielding, easy scratching and inability to directly contact the LCD screen of laminating films, especially POP laminating films with higher brightness, have not been effectively solved, which has affected the application and promotion of laminating products. The technical solution of the present invention proposes a complete set of solutions, which can effectively solve the problem of ensuring that the brightness basically meets the requirements of liquid crystal display products, the shielding meets the requirements of liquid crystal display modules, and can be in direct contact with the liquid crystal display panel glass to ensure that there is no interference and no glare, the visual effect meets the standard, and the scratch resistance meets the assembly requirements. The product stiffness can meet the requirements of large-size modules, thereby effectively promoting the application and promotion of laminating products in the field of liquid crystal display.

[0286] Microbeads or spherical particles are added to the composite adhesive layer of the present invention. Due to the use of appropriate resin and formula combination, the leveling property is good, so that the bonding fastness meets the requirements, and the problem that adding microbeads or spherical particles to conventional composite adhesives will lead to poor leveling or poor bonding fastness is solved.

[0287] The composite adhesive layer of the present invention uses microstructure molding technology to achieve the required haze, and because of the selection of appropriate resin and formula combination, it can also be bonded to the first prism layer after the first UV curing. This solves the problem that conventional composite glue cannot be bonded to the first prism smoothly due to loss of viscosity after microstructure molding UV curing.

[0288] The embodiments of the present invention are only used to illustrate the present invention and do not constitute a limitation on the scope of the claims. Other substantially equivalent substitutes that can be thought of by those skilled in the art are all within the protection scope of the present invention.

Claims

1. A laminating film for a liquid crystal display, characterized in that: From bottom to top, it includes: A first structural layer film, the first structural layer film comprising a first base film, a first prism layer and a back coating layer, the first prism layer is formed by a plurality of first prisms arranged continuously; the first prism layer is arranged on the upper surface of the first base film; the back coating layer is arranged on the lower surface of the first base film; A second structural layer film, wherein the second structural layer film comprises a second base film and a second prism layer, wherein the second prism layer is formed by a plurality of second prisms arranged continuously; and the second prism layer is disposed on an upper surface of the second base film; The lower surface of the second base film is provided with a composite adhesive layer; the composite adhesive layer contains PBMA or PMMA microbeads; the first prism is attached to the second base film through the composite adhesive layer, The haze of the composite adhesive layer is 20%-60%. In the cross section of the second prism, the top of the peak of the vertex angle A is a rounded corner with a radius of 0-5 microns, The components of the second prism layer include, by mass percentage: OPPEA 30%-35%; epoxy acrylate prepolymer 10%-15%; EOEOEA 5%-10%; BPA (EO) 20DA 5%-10%; BPA (EO) 3DA 10%-15%; DPHA 5%-10%; photoinitiator 3%-7%; leveling agent 1%-3%; or The components of the second prism layer include, by mass percentage: OPPEA 30%-35%; epoxy acrylate prepolymer 10%-15%; EOEOEA 5%-10%; BPA (EO) 20DA 5%-10%; BPA (EO) 3DA 10%-15%; DPHA 5%-10%; photoinitiator 3%-7%; leveling agent 1%-3%; spherical particles 0.05%-0.15%, The back coating components include, by mass percentage: 9%-12% of 6-functional aliphatic polyurethane acrylic prepolymer; 3%-6% of 3-functional aliphatic polyurethane acrylic prepolymer or 4-functional aliphatic polyurethane acrylic prepolymer; 6%-9% of active diluent; 1.2%-2.4% of photoinitiator; 0.3%-0.6% of dispersant; 0.3%-0.6% of antistatic agent; 0.2%-4% of 3-5 micron PBMA or PMMA microbeads; the rest is solvent, which is two or three of toluene, butanone and cyclohexanone; The surface resistance of the back coating is within 10 to the 12th power, and the hardness is H-2H; Microbeads and spherical particles with a particle size of 3-5 microns are dispersed in the composite adhesive layer, and the microbeads are PMMA microbeads or PBMA microbeads; the microbeads and spherical particles make the haze of the composite adhesive layer reach 20%-60%; or Spherical particles are dispersed in the composite adhesive layer, and a microstructure molding method is used to make its haze reach 20%-60%; Spherical particles are dispersed in the composite adhesive layer or the second prism layer, and the spherical particles are selected from one or more of kaolin, aluminum hydroxide, magnesium hydroxide or powdered calcium carbonate; The particle size of the spherical particles is 0.1-1 micrometer; The first prism has a first top edge, and the second prism has a second top edge; an included angle C between a top projection line of the first top edge and a top projection line of the second top edge is 45 degrees to 85 degrees or 95 degrees to 135 degrees; The first prism has a first top edge, and the second prism has a second top edge; the first top edge is inserted into the composite adhesive layer to a depth of 0.5-2 microns.

2. The laminating film for a liquid crystal display according to claim 1, characterized in that: The first prism has three edges, including two first bottom edges and one first top edge; the first top edge protrudes from the first base film; the spacing between the first top edges of two adjacent first prisms is 60-70 microns; the first prism layer also includes a first prism base, the two first bottom edges are arranged on the first prism base, and the first prism and the first prism base are integrally formed; the cross-section of the first prism is an isosceles triangle.

3. The laminating film for a liquid crystal display according to claim 1, characterized in that: The second prism has three edges, including two second bottom edges and one second top edge; the second top edge protrudes from the second base film; the spacing between the second top edges of two adjacent second prisms is 25-70 microns; the second prism layer also includes a second prism base, the two second bottom edges are arranged on the second prism base, and the second prism and the second prism base are integrally formed; the cross-section of the second prism is an isosceles triangle.

4. The laminating film for a liquid crystal display according to claim 1, characterized in that: The first prism has a first top edge, and the second prism has a second top edge; along the length direction of the second top edge, the second top edge has a height change, and the height difference is 1.5-3 microns. The first prism is a straight prism or a high-low prism, and the height of each prism on its extension line remains unchanged. Adjacent prisms have the same height if they are straight prisms, or have different heights if they are high-low prisms.

5. The laminating film for a liquid crystal display according to claim 1, characterized in that: The components of the first prism layer include, by mass percentage: OPPEA 25%-30%; epoxy acrylate prepolymer 10%-15%; OEOEA 10%-15%; BPA (EO) 10DA 25%-30%; hydroxyethyl acrylate 3%-5%; photoinitiator 2%-6%; leveling agent 1%-3%.

6. The laminating film for a liquid crystal display according to claim 1, characterized in that: The components of the composite adhesive layer include, by mass percentage: 6%-8% of a difunctional aliphatic polyurethane acrylic prepolymer; 2%-4% of a tetrafunctional aliphatic polyurethane acrylic prepolymer; 3%-5% of acryloyl morpholine; 0.2%-0.4% of methyl methacrylate phosphate; 1%-2% of HDDA; 0.8%-1.6% of a photoinitiator; 0.5%-2% of 3-5 micron PBMA microbeads or PMMA microbeads; 0.5%-1.5% of spherical particles; and the rest is a solvent, which is one or both of butanone and toluene.

7. The laminating film for a liquid crystal display according to claim 1, characterized in that: The components of the composite adhesive layer include, by mass percentage: 6%-8% of difunctional aliphatic polyurethane acrylic prepolymer; 2%-4% of tetrafunctional aliphatic polyurethane acrylic prepolymer; 3%-5% of acryloyl morpholine; 0.2%-0.4% of methyl methacrylate phosphate; 1%-2% of HDDA; 0.5%-1.6% of photoinitiator; 0.2%-0.6% of phosphate monomer; 0.5%-1.5% of spherical particles; and the rest is solvent, which is one or both of butanone and toluene.

8. A liquid crystal display backlight module, characterized in that: The present invention comprises the laminating film for liquid crystal display according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Prism sheet, backlight unit and liquid crystal display

    CN101071221A

  • An optical projection screen for display and a manufacturing method thereof

    CN106226988A

  • Preparing method of non-obstructing quantum dot film

    CN108089370A

  • Compound brightness enhancement film and preparing method and application thereof

    CN108205218A

  • Novel hold light membrane

    CN207216069U