A single slip soluble bridge plug
By designing a single-caliber structure and using a fast-dissolving high-strength high-elongation magnesium alloy and degradable water-soluble elastomer, the problems of large length, poor anchoring and incomplete dissolution of the double-caliber wall are solved, and the bridge is realized Compact, reliable anchoring and efficient re-discharge of plugs.
Patent Information
- Application Number
- CN201910437219.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-05-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2039-05-24
AI Technical Summary
The existing double-club bridge plug is long and large in size, which is inconvenient to enter, and the anchoring effect is poor. After layered fracturing, drilling and grinding are required to be released. The process is cumbersome and easy to block the wellbore, and it is soluble. Incomplete dissolution, slow dissolution rate and low intensity, resulting in low reflux efficiency.
Design a single cavities soluble bridge plug, using a single cavities structure, made of soluble metal materials and soluble elastic materials, including central tubes, upper joints, rubber cylinders, cones and cavities mechanisms, using rapid dissolution The high-strength high elongation magnesium alloy and degradable water-soluble elastomer achieve axial position anchoring and rapid dissolution of the bridge plug.
The bridge plug is shortened in length and compact in size, reliable anchoring effect, large inner diameter and high return discharge efficiency, and can quickly unblock, avoid residual solid material in the wellbore and improve construction efficiency.
Smart Images

Figure CN110067529B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tools for petroleum mining, and in particular relates to a single-slip soluble bridge plug. Background Art
[0002] In oilfield exploration and development, the lower well section needs to be plugged during the stratified fracturing, stratified acidizing and stratified oil testing of oil and water wells. Bridge plugs are safe, reliable and low-cost downhole plugging tools commonly used in oil development. Most of the bridge plugs in the prior art are double-slip bridge plugs, including a center tube, a rubber cylinder is sleeved on the middle section of the center tube, a cone is sleeved on each side of the rubber cylinder on the center tube, and a slip mechanism is sleeved behind each of the two cones. The small-diameter ends of the two cones are inserted into the gap between the slip mechanism and the center tube, and a joint is sleeved behind each of the two slip mechanisms. When sealing, the bridge plug is sent to the selected layer position in the casing, and the sealing tool is connected to the upper joint. The sealing tool is started, and the piston thrust of the sealing tool pushes the upper joint to slide along the center tube, squeeze the rubber cylinder, and make the rubber cylinder radially larger. The rubber cylinder seals the inside of the casing, and the upper joint continues to move to squeeze the cone. The small-diameter end of the cone is inserted into the inner wall of the slip mechanism so that the slip mechanism is stretched and expanded by the extrusion force until the slip mechanism breaks and separates, and the slip teeth are tightly anchored on the inner wall of the casing to complete the sealing.
[0003] However, the double-slip bridge plug in the prior art is relatively long and bulky, which makes it inconvenient to lower the bridge plug; and the slip structure in the bridge plug in the prior art has a poor breaking effect when it is set, and the anchoring effect is unreliable; in addition, after the layered fracturing is completed, the bridge plug needs to be released, and the drilling and grinding method is often used to wear the bridge plug away, but the processing process is cumbersome, and the remaining materials are easy to clog the wellbore. The prior art also uses soluble metal materials and soluble elastic materials to make bridge plugs, but the materials are usually not completely dissolved, the dissolution rate is slow, and the requirements of efficient construction cannot be met. In addition, the soluble materials in the prior art have low strength. In order to meet the strength requirements, the bridge plug can only be made into a very small inner diameter, which greatly reduces the backflow efficiency. Summary of the invention
[0004] The technical problem solved by the present invention is to provide a single-slip soluble bridge plug with short length, compact structure, easy lowering, reliable anchoring effect, good sealing effect, large inner diameter and high backflow efficiency. After sealing, the bridge plug can be dissolved by the backflow fluid to release the blockage.
[0005] In order to solve the above problems, the present invention provides a single-slip soluble bridge plug, including a center tube, on which an upper joint, a rubber cylinder, a cone, a slip mechanism and a lower joint are sequentially sleeved, and the upper joint, the rubber cylinder, the cone and the slip mechanism can slide axially along the center tube; the upper joint is connected to the center tube by a shear pin; the small diameter end of the cone is inserted into the gap between the slip mechanism and the center tube; the slip mechanism includes a first slip tooth and a second slip tooth, the tooth tip of the first slip tooth is inclined toward one side of the upper joint, and the tooth tip of the second slip tooth is inclined toward one side of the lower joint; the center tube, the upper joint, the lower joint, the cone and the slip mechanism are made of soluble metal material, and the rubber cylinder is made of soluble elastic material.
[0006] In the technical solution, preferably, the shear pins are evenly distributed in the circumferential direction of the upper joint.
[0007] In the technical solution, preferably, a first metal sealing ring is also sleeved on the central tube, the first metal sealing ring is arranged between the upper joint and the rubber sealing mechanism, and the first metal sealing ring is made of a soluble metal material.
[0008] In the technical solution, preferably, a second metal sealing ring is also sleeved on the central tube, the second metal sealing ring is arranged between the rubber sealing mechanism and the cone, and the second metal sealing ring is made of a soluble metal material.
[0009] In the technical solution, preferably, the cava mechanism includes a cava seat, a plurality of stress grooves are provided in the circumferential direction of the cava seat, and cava plates are formed between adjacent stress grooves on the cava seat. Each cava plate is provided with a plurality of first tooth grooves and second tooth grooves, a first cava tooth is provided in the first tooth groove, and a second cava tooth is provided in the second tooth groove.
[0010] In the technical solution, preferably, the inner wall of the slip seat on the side of the small diameter end close to the cone is a conical surface, and the large diameter end of the conical surface faces one side of the cone.
[0011] In the technical solution, preferably, the stress grooves are arranged at equal intervals in the circumferential direction of the slip seat. Further preferably, each stress groove is arranged in the axial direction on the slip seat.
[0012] In the technical solution, preferably, the number of first tooth grooves on each clap tile is the same and the arrangement is the same; the number of second tooth grooves on each clap tile is the same and the arrangement is the same.
[0013] In the technical solution, preferably, each tile is provided with 4 first tooth grooves and 1 second tooth groove, the 4 first tooth grooves are located at the 4 vertices of the rectangle, and the second tooth groove is located at the intersection of the diagonals of the rectangle.
[0014] In the technical solution, preferably, the highest point of the first slip tooth is higher than the highest point of the second slip tooth.
[0015] In the technical solution, preferably, the inner cavity of one end of the central tube close to the upper joint is provided with a reducing cavity, and the inner diameter of the reducing cavity decreases from the end of the central tube close to the upper joint to the end away from the upper joint.
[0016] In the technical solution, preferably, the inner wall of the central tube is provided with a plurality of grooves.
[0017] In the technical solution, preferably, the groove includes a plurality of circular grooves arranged in parallel, and the center of the circular groove is located on the axis of the central tube.
[0018] In the technical solution, preferably, the groove is a spiral groove arranged along the inner wall of the central tube and taking the axis of the central tube as the axis.
[0019] In the technical solution, preferably, the center tube and / or the upper joint and / or the lower joint and / or the cone and / or the slip mechanism and / or the first metal sealing ring and / or the second metal sealing ring are made of a fast-dissolving high-strength and high-elongation magnesium alloy, and the fast-dissolving high-strength and high-elongation magnesium alloy is composed of the following elements in mass percentage: Gd 1.0%-22.0%, Y0.001%-5.0%, Al 0.001%-10%, Zn 0.001%-5.0%, Zr 0.01%-1.0%, Sc 0.0001%-1.0%, Cu 0.01%-10.0%, Li 0.01%-3.0%, Ni 0.01%-3.0%, Ga 0.01%-3.0%, In0.01%-3.0%, and the rest are Mg and impurity elements, and the total amount of Li, Ni, Ga and In is 0.1%-6.0%.
[0020] In the technical solution, preferably, the fast-dissolving high-strength and high-elongation magnesium alloy is composed of the following elements in mass percentage: Gd 1.5%-14.5%, Y 0.5%-2.0%, Al 0.1%-2.0%, Zn 0.1%-1.0%, Zr 0.2%-0.5%, Sc 0.001%-0.02%, Cu 0.1%-2.0%, Li 0.01%-1.0%, Ni 0.01%-1.0%, Ga0.01%-1.0%, In 0.01%-1.0%, and the rest are Mg and impurity elements, and the total amount of Li, Ni, Ga, and In is 0.5%-2.0%.
[0021] In the technical solution, preferably, the fast-dissolving high-strength and high-elongation magnesium alloy is composed of the following elements in mass percentage: Gd 2.5%, Y 1.0%, Al 1.0%, Zn 0.5%, Zr 0.4%, Sc 0.01%, Cu 1.5%, Li0.25%, Ni 0.25%, Ga 0.25%, In 0.25%, and the rest are Mg and impurity elements.
[0022] In the technical solution, preferably, the rubber cylinder is made of a degradable water-soluble elastomer, and the degradable water-soluble elastomer includes a block copolymer with a copolymer of polylactic acid and polyethylene glycol as a soft segment prepolymer and a copolymer of a sulfonic acid type hydrophilic monomer and isocyanate as a hard segment prepolymer, and the mass ratio of the soft segment prepolymer to the hard segment prepolymer is (25-120): (25-80).
[0023] In the technical solution, preferably, the mass ratio of the polylactic acid component to the polyethylene glycol in the soft segment prepolymer is (5-20): (20-100).
[0024] In the technical solution, preferably, the mass ratio of the sulfonic acid type hydrophilic monomer to the isocyanate in the hard segment prepolymer is (10-30): (15-50).
[0025] In the technical solution, preferably, the degradable water-soluble elastomer also includes a water-soluble functional additive, and the mass ratio of the water-soluble functional additive to the soft segment prepolymer is (5-50): (25-120), and the water-soluble functional additive is one or more of a polyhydroxy compound and a polyamide compound.
[0026] In the technical solution, preferably, the degradable water-soluble elastomer further comprises a dispersant, the mass ratio of the dispersant to the soft segment prepolymer is (5-50): (25-120), and the dispersant is sodium polyacrylate.
[0027] In the technical solution, preferably, the number average molecular weight of the polyethylene glycol in the degradable water-soluble elastomer is 1000-3000.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. The single-slip soluble bridge plug of the present invention is designed as a single-slip structure, and the axial position anchoring of the bridge plug is achieved through a slip mechanism. Compared with the double-slip bridge plug in the prior art, the length of the bridge plug can be shortened, the volume can be reduced, and the lowering of the bridge plug during plugging is convenient;
[0030] 2. The single-slip soluble bridge plug of the present invention has a first slip tooth and a second slip tooth of the slip mechanism that are respectively inclined toward the two ends of the central pipe and are bidirectionally distributed, so that after the axial position of the bridge plug is anchored, it can firmly resist the pressure from the upper part of the bridge plug during the upper layer fracturing operation, and can also resist the pressure from the lower part of the bridge plug during the flowback process, and the bridge plug anchoring reliability is strong;
[0031] 3. The single-slip soluble bridge plug of the present invention has a first metal sealing ring and a second metal sealing ring arranged on both sides of the rubber cylinder, which can further improve the sealing reliability of the bridge plug by cooperating with the deformation of the rubber cylinder through the compression deformation of the metal sealing ring, and further arranging stress grooves on the first metal sealing ring and the second metal sealing ring is conducive to the deformation of the metal sealing ring, which can further improve the sealing reliability of the bridge plug;
[0032] 4. The single slip soluble bridge plug of the present invention has a plurality of grooves on the inner wall of the central pipe. When the flowback liquid dissolves the central pipe during the flowback process, the contact area between the central pipe and the flowback liquid is larger, which can accelerate the reaction rate between the central pipe and the flowback liquid, accelerate the dissolution of the central pipe, and improve the flowback efficiency;
[0033] 5. The single slip soluble bridge plug of the present invention is made of soluble materials in all parts of the structure of the bridge plug. After the stratified fracturing is completed, the various parts of the bridge plug can be dissolved by the backflow fluid to release the blockage, and no solid materials will remain in the wellbore, so that the full diameter in the wellbore after fracturing is achieved;
[0034] 6. The single-slip soluble bridge plug of the present invention, the center pipe, the upper joint, the lower joint, the cone, the slip mechanism, the first metal sealing ring, and the second metal sealing ring adopt a fast-dissolving high-strength and high-elongation magnesium alloy. By adjusting the alloy composition and reasonably selecting the content of each element, the interaction between the alloy elements that is beneficial to the improvement of the alloy performance is obtained, so that the alloy has a very fast reaction rate with media such as water, and can be quickly dissolved by the return flow fluid during the return flow process, thereby improving the construction efficiency and achieving the full-diameter wellbore after fracturing; and the magnesium alloy material has both high-strength and high-elongation mechanical strength properties, and its strength can reach 400MPa. The inner diameter of the bridge plug made of the material can be increased by 65% compared with the inner diameter of the conventional bridge plug. For example, the inner diameter of the bridge plug used for 5.5 casing can reach an ultra-large inner diameter of 58mm, which can greatly improve the return flow efficiency;
[0035] 7. The single-slip soluble bridge plug of the present invention is made of a special degradable water-soluble elastomer. The degradable water-soluble elastomer has a copolymer of polylactic acid and polyethylene glycol as a soft segment and a copolymer of a sulfonic acid type hydrophilic monomer and isocyanate as a hard segment. A polyurethane structure of a block copolymer of the soft segment and the hard segment is generated through polymerization reaction. When the elastomer is in water, the ester bonds in the polylactic acid are hydrolyzed to break the macromolecules of the block copolymer polyurethane structure to form a molecular structure with a smaller molecular weight. Since the polylactic acid produces hydrophilic hydroxyl groups after the ester bonds are hydrolyzed, and the sulfonic acid type hydrophilic monomer in the molecular structure is not only an anionic group but also a strong hydrophilic group, the molecular structure with a smaller molecular weight produced after the breakage has strong water solubility, thereby making the elastomer have good water solubility. The solubility of the elastomer can also be regulated by regulating the proportion of polylactic acid in the molecule and the degree of polymerization of polylactic acid. It can be quickly dissolved in the return fluid, thereby significantly improving the return efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic diagram of the structure of a single slip soluble bridge plug according to an embodiment of the present invention;
[0037] Figure 2 is a cross-sectional schematic diagram of a single slip soluble bridge plug according to an embodiment of the present invention;
[0038] Figure 3 It is a structural schematic diagram of the slip mechanism in the single slip soluble bridge plug according to an embodiment of the present invention;
[0039] Figure 4 It is a schematic structural diagram of the slip seat in the single slip soluble bridge plug described in an embodiment of the present invention.
[0040] Among them: 1-center tube; 2-upper joint; 3-rubber cylinder; 4-cone; 5-slip mechanism; 51-first slip tooth; 52-second slip tooth; 53-slip seat; 54-stress groove; 55-first tooth groove; 56-second tooth groove; 6-lower joint; 7-shear pin; 8-first metal sealing ring; 9-second metal sealing ring; 10-variable cavity; 11-groove. DETAILED DESCRIPTION
[0041] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] The double-cava bridge plug in the prior art is long and large in size, which makes it inconvenient to lower the bridge plug. The breaking effect of the cava structure is poor when it is sealed, and the anchoring effect is unreliable. After the layered fracturing is completed, the drilling and grinding method is required to wear out the bridge plug to release the blockage of the bridge plug. The processing process is cumbersome and it is easy to block the wellbore.
[0043] To solve the above problems, the present invention provides a single slip soluble bridge plug, such as Figure 1 , Figure 2As shown, it includes a central tube 1, on which an upper joint 2, a rubber cylinder 3, a cone 4, a slip mechanism 5 and a lower joint 6 are sequentially sleeved, and the upper joint 2, the rubber cylinder 3, the cone 4 and the slip mechanism 5 can slide along the axial direction of the central tube 1; the upper joint 2 is connected to the central tube 1 by a shear pin 7; the small diameter end of the cone 4 is inserted into the gap between the slip mechanism 5 and the central tube 1; the slip mechanism 5 includes a first slip tooth 51 and a second slip tooth 52, the tooth tip of the first slip tooth 51 is inclined toward one side of the upper joint 6, and the tooth tip of the second slip tooth 52 is inclined toward one side of the lower joint 2; the central tube 1, the upper joint 2, the lower joint 6 and the slip mechanism 5 are made of soluble metal materials, and the rubber cylinder 3 is made of soluble elastic materials.
[0044] When plugging downhole, a conveying device such as a cable or a pipe string is used to convey the single-slip soluble bridge plug and the sealing tool of the present invention to a predetermined position in the wellbore casing. The sealing tool generates a thrust acting on the upper joint 2 of the single-slip soluble bridge plug by means of gunpowder blasting, hydraulic sealing or mechanical sealing. The shear pin 7 at the connection between the upper joint 2 and the central pipe 1 is sheared by a certain shear force. The upper joint 2 moves along the central pipe 1 under the thrust, pushing the rubber tube 3 to move, so that the rubber tube 3 is squeezed and axially contracted, and the diameter increases. Thereby, it presses against the inner wall of the wellbore casing, realizes the locking of the radial position of the bridge plug, and at the same time seals the wellbore, and the upper joint 2 continues to move forward, pushing the cone 4 to move through the rubber tube 3, and the small diameter end of the cone 4 is inserted into the gap between the slip mechanism 5 and the central pipe 1. The slip mechanism 5 is expanded and stretched by the squeezing force of the cone 4 until the slip mechanism breaks and separates, and the first slip tooth 51 and the second slip tooth 52 on the slip mechanism 5 are anchored on the inner wall of the wellbore casing, realizing the axial position anchoring of the bridge plug and completing the sealing.
[0045] The single-slip soluble bridge plug described in the present invention is designed as a single-slip structure, and the axial position anchoring of the bridge plug is achieved through a slip mechanism. Compared with the double-slip bridge plug in the prior art, the length of the bridge plug can be shortened and the volume can be reduced, which is convenient for lowering the bridge plug during plugging; the first slip tooth 51 and the second slip tooth 52 of the slip mechanism 5 are respectively inclined toward the two ends of the central pipe 1, and are arranged in a bidirectional distribution, so that after the axial position of the bridge plug is anchored, it can firmly resist the pressure from the upper part of the bridge plug during the upper layer fracturing operation, and can also resist the pressure from the lower part of the bridge plug during the backflow process, and the bridge plug has strong anchoring reliability; the various structural parts of the bridge plug are made of soluble materials. After the layered fracturing is completed, the various structural parts of the bridge plug can be dissolved by the backflow fluid to release the plugging, and no solid material will remain in the wellbore, thereby achieving full diameter in the wellbore after fracturing.
[0046] In the technical solution, preferably, the shear pins 7 are evenly distributed in the circumferential direction of the upper joint 2 .
[0047] In the technical solution, preferably, the center tube 1 is also sleeved with a first metal sealing ring 8, which is arranged between the upper joint 1 and the rubber cylinder 3, and is made of a soluble metal material. Further preferably, the outer wall of the first metal sealing ring 8 is also provided with a plurality of stress grooves.
[0048] In the technical solution, preferably, the central tube 1 is also provided with a second metal sealing ring 9, which is provided between the rubber sleeve 3 and the cone 4 and is made of a soluble metal material. Further preferably, the outer wall of the second metal sealing ring 9 is provided with a plurality of stress grooves.
[0049] After the upper joint 1 is thrusted by the sealing tool, it moves backward to push the first metal sealing ring 8, the rubber tube 3 and the second metal sealing ring 9. The first metal sealing ring 8, the rubber tube 3 and the second metal sealing ring 8 are squeezed and deformed, and their diameters become larger, so that the inner pipe of the wellbore is blocked. The first metal sealing ring and the second metal sealing ring are arranged, and the sealing reliability of the bridge plug can be further improved through the compression deformation of the metal sealing ring and the deformation of the rubber tube. Further arranging stress grooves on the first metal sealing ring and the second metal sealing ring is beneficial to the deformation of the metal sealing rings, which can further improve the sealing reliability of the bridge plug.
[0050] The slip mechanism 5 may be a split type in which the petal-type slips in the prior art are fixed together by hoops, or may be an integral type slip.
[0051] As a preferred embodiment, Figure 3 , Figure 4 As shown, the cava mechanism 5 is an integral cava, and the cava mechanism 5 includes a cava seat 53. A plurality of stress grooves 54 are provided on the circumference of the cava seat 53. Cava pieces are formed between adjacent stress grooves 54 on the cava seat 53. Each cava piece is provided with a plurality of first tooth grooves 55 and second tooth grooves 56. A first cava tooth 51 is provided in the first tooth groove 55, and a second cava tooth 52 is provided in the second tooth groove 56.
[0052] Further preferably, the inner wall of the cava seat 53 on the side of the small diameter end close to the cone 4 is a conical surface, the large diameter end of the conical surface faces the side of the cone 4, and the small diameter end of the cone 4 is inserted into the gap between the conical surface of the cava seat 53 and the center tube 1, which makes it easier for the cone 4 to exert force on the expansion of the cava seat 53.
[0053] Preferably, the stress grooves 54 are arranged at equal intervals in the circumferential direction of the slip seat 53. This allows the slip seat 53 to be supported and broken more evenly by the force of the cone 4. Preferably, each stress groove 54 is arranged in the axial direction on the slip seat.
[0054] Further preferably, the number of first tooth grooves 55 on each cava piece is the same and the arrangement is the same; the number of second tooth grooves 56 on each cava piece is the same and the arrangement is the same, so that when the cava seat 53 is broken by the cone 4 and anchored on the inner wall of the wellbore, the forces in all directions are more uniform and the anchoring reliability is stronger.
[0055] As a preferred embodiment, each cava piece on the cava seat 53 is provided with four first tooth grooves 55 and one second tooth groove 56, the four first tooth grooves 55 are located at the four vertices of the rectangle, and the second tooth groove 56 is located at the intersection of the diagonals of the rectangle.
[0056] Furthermore, the highest point of the first slip teeth 51 in the first tooth groove 55 is higher than the highest point of the second slip teeth 52 in the second tooth groove 56, so as to minimize the influence of the second slip teeth 52 in the middle reverse direction during the setting process.
[0057] Further preferably, the top surface of the first cava tooth 51 is inclined toward one side of the upper joint 2, and the angle between the top surface of the first cava tooth 51 and the outer wall surface of the cava seat 53 is 75°-85°, and the top surface of the second cava tooth 52 is inclined toward one side of the lower joint 6, and the angle between the top surface of the second cava tooth 52 and the outer wall surface of the cava seat 53 is 75°-85°.
[0058] Among them, the plugging method of the single-slip soluble bridge plug of the present invention can be a ball-dropping type, a check valve type or a blind plugging type. As a preferred method, the single-slip soluble bridge plug of the present invention is a ball-dropping type, and the ball is also made of a soluble metal material. The inner cavity of the end of the central tube 1 close to the upper joint 2 is provided with a variable diameter cavity 10. The inner diameter of the variable diameter cavity 10 decreases from the end of the central tube 1 close to the upper joint 2 to the end away from the upper joint 2. The inner diameter of the inner cavity of the central tube 1 is smaller than the outer diameter of the ball. After the sealing is completed, when the lower layer needs to be sealed, the ball is dropped from the wellhead, and the ball will fall into the variable diameter cavity 10 to achieve the isolation of the lower layer. When the lower pressure is greater than the upper pressure of the ball, the ball will be separated from the variable diameter cavity 10, and backflow can be achieved. The single-slip soluble bridge plug of the embodiment of the present invention is a ball-dropping type, and the sealing method is adopted from the upper part of the bridge plug. In the process of lowering the bridge plug, the ball can be pumped in together with the bridge plug, saving the amount of water pumped into the conveying ball.
[0059] In the technical solution, preferably, the inner wall of the central tube 1 is provided with a plurality of grooves 11. The inner wall of the central tube 1 is set as a non-smooth surface, but has a plurality of grooves. When the return liquid dissolves the central tube 1 during the return flow process, the contact area between the central tube 1 and the return liquid is larger, which can speed up the reaction rate between the central tube 1 and the return liquid, accelerate the dissolution of the central tube 1, and improve the return flow efficiency.
[0060] As a preferred embodiment, the groove 11 includes a plurality of circular grooves arranged in parallel, and the center of the circular groove is located on the axis of the central tube.
[0061] As another preferred embodiment, the groove 11 is a spiral groove arranged along the inner wall of the central tube and taking the axis of the central tube as its axis.
[0062] The operation of the single slip soluble bridge plug of the present invention when plugging the lower layer is as follows:
[0063] 1) Connect the single slip soluble bridge plug to the adapter, and connect the perforating gun and the sealing tool to the adapter; 2) The cable car transfers the pipe string to the designed layer; 3) Set the bridge plug; 4) Release the hand; 5) Lift the perforating gun to the designed layer to complete the perforation; 6) Lift the cable out of the wellhead; 7) Throw the ball to perform fracturing construction; 8) Repeat steps 1-6 to achieve multi-layer fracturing construction; 9) After the fracturing is completed, the soluble bridge plug is dissolved in the flowback fluid to achieve full diameter.
[0064] The single-slip soluble bridge plug of the present invention, wherein the soluble metal material refers to a metal material that can react with water or return fluid containing salt and thereby dissolve in water or return fluid. The soluble metal material belongs to the prior art. The center pipe, the upper joint, the lower joint, the cone, the slip mechanism, the first metal sealing ring, and the second metal sealing ring can be made of various metal materials in the prior art that can be dissolved in water or a salt solution with a composition similar to that of the return fluid. For example, soluble magnesium alloys and soluble aluminum alloys in the prior art can be used. Although a large number of soluble metals of the above-mentioned structure that can be used to make bridge plugs have been disclosed in the prior art, the overall performance of most materials is poor. Some have poor solubility, incomplete dissolution and too slow dissolution rate, and some materials have good solubility but poor mechanical properties. Therefore, as a preferred solution, the center tube 1 and / or the upper joint 2 and / or the lower joint 6 and / or the slip mechanism 5 and / or the first metal sealing ring 8 and / or the second metal sealing ring 9 are made of a fast-dissolving high-strength and high-elongation magnesium alloy, and the fast-dissolving high-strength and high-elongation magnesium alloy is composed of the following elements in mass percentage: Gd 1.0%-22.0%, Y 0.001%-5.0%, Al 0.001%-10%, Zn0.001%-5.0%, Zr 0.01%-1.0%, Sc 0.0001%-1.0%, Cu 0.01%-10.0%, Li 0.01%-3.0%, Ni 0.01%-3.0%, Ga 0.01%-3.0%, In 0.01%-3.0%, the rest is Mg and impurity elements, and the total amount of Li, Ni, Ga and In is 0.1%-6.0%.
[0065] Further preferably, the fast-dissolving high-strength and high-elongation magnesium alloy is composed of the following elements in mass percentage: Gd 1.5%-14.5%, Y 0.5%-2.0%, Al 0.1%-2.0%, Zn 0.1%-1.0%, Zr 0.2%-0.5%, Sc 0.001%-0.02%, Cu 0.1%-2.0%, Li 0.01%-1.0%, Ni 0.01%-1.0%, Ga0.01%-1.0%, In 0.01%-1.0%, and the rest are Mg and impurity elements, and the total amount of Li, Ni, Ga and In is 0.5%-2.0%.
[0066] Still further preferably, the fast-dissolving high-strength and high-elongation magnesium alloy is composed of the following elements in mass percentage: Gd 2.5%, Y 1.0%, Al 1.0%, Zn 0.5%, Zr 0.4%, Sc 0.01%, Cu 1.5%, Li 0.25%, Ni 0.25%, Ga 0.25%, In 0.25%, and the rest are Mg and impurity elements.
[0067] Herein, impurity elements refer to inevitable impurity elements introduced from the raw materials used to prepare the alloy during the preparation of the alloy, i.e., metal or non-metal elements present in the metal but not intentionally added or retained. Preferably, the mass percentage of the inevitable impurity elements is 0%-0.15%.
[0068] Among them, Cu, Li, Ni, Ga, and In are mixed reaction promoting elements. During the smelting process, these elements form new crystal phases with magnesium. These crystal phases can destroy the continuity of the generated magnesium hydroxide during the reaction of magnesium with the aqueous medium, thereby reducing the barrier of magnesium hydroxide to the contact between magnesium and the aqueous medium, promoting the reaction of magnesium with media such as water, and increasing the reaction rate of magnesium with the aqueous medium; in addition, Cu, Li, Ni, Ga, and In cooperate with each other, and adding them in the above proportion can eliminate the intracrystalline segregation of magnesium alloys to the greatest extent, refine the grains, and thus improve the elongation. Cu, Li, Ni, Ga, and In cooperate with each other and add them in the above proportion, which can reduce the upper limit of the solid solubility of magnesium alloys to the greatest extent, make the alloy composition homogenized, reduce casting defects, and maximize the alloy effect; Cu, Li, Ni, Ga, and In can also promote the precipitation strengthening of Gd and Zn elements in the subsequent heat treatment process, further improving the strength of the alloy.
[0069] Among them, Gd and Y can form a solid solution with Mg during the smelting process, and the strength of the obtained alloy can be significantly improved through solid solution or aging strengthening. Gd and Y have a large solid solubility with Mg, and Gd can be dissolved into the magnesium alloy with a high solid solubility. And as the temperature decreases, the solid solubility decreases significantly, so the strength and other properties of the alloy can be greatly improved through solid solution strengthening or aging strengthening. The role of Y is similar to that of Gd. At the same time, the addition of a small amount of Y can also refine the grains and improve the mechanical properties of the alloy. Since the maximum solid solubility of Gd and Y in magnesium alloys is 23.5% and 12.6% respectively, the present invention adds the above-mentioned Gd and Y in appropriate amounts to ensure that Gd and Y can form a solid solution of a single lattice structure with Mg, thereby achieving high strength and high elongation of the magnesium alloy. Gd and Y can also improve the stability of the melt during the smelting process, improve the stability of the oxide film, and reduce the burning loss of other elements.
[0070] Among them, Zr and Sc elements can significantly refine the ingot grains of the material. According to the Hall-Petch formula, grain refinement can improve the strength and plasticity of magnesium alloy molded parts; in addition, the refinement of ingot grains can also promote the mixed reaction of Li, Ni, Ga, and In to promote the uniformity of dispersion of elements in the alloy, further improve the reaction rate of magnesium with water-soluble media, and promote the uniformity of dispersion of Gd and Y in the alloy, so that the Gd and Y elements in the alloy are more evenly dispersed, further improving the high strength and high elongation of magnesium alloys. Among them, the price of Sc is relatively expensive, and although the grain refining effect of Zr is not as good as that of Sc, its price is cheap. Adding the two to the raw materials in the above mass percentage can obtain the best grain refining effect and greatly reduce the material cost.
[0071] The fast-dissolving high-strength and high-elongation magnesium alloy obtains the interaction between the alloy elements that is beneficial to the improvement of alloy performance by regulating the alloy composition and reasonably selecting the content of each element, and obtains a magnesium alloy with a fast reaction rate with water and other media. The center pipe, upper joint, lower joint, cone, slip mechanism, first metal sealing ring, and second metal sealing ring are made of the magnesium alloy material, which can be quickly dissolved by the return fluid during the return flow process, improve the construction efficiency, and achieve full bore in the wellbore after fracturing; and the magnesium alloy material has high strength and high elongation mechanical strength properties at the same time, and its strength can reach 400MPa, which can increase the inner diameter of the conventional bridge plug by 65%. For example, the inner diameter of the bridge plug used in 5.5 casing can reach an ultra-large inner diameter of 58mm, which can greatly improve the return efficiency. The specific composition examples and performance tests of the fast-dissolving high-strength and high-elongation magnesium alloy are shown in the embodiments.
[0072] Wherein, the soluble elastic material refers to an elastic material that can be gradually decomposed and dissolved in water or backflow liquid, and the soluble elastic material belongs to the prior art. The rubber tube can be made of any elastic material that can be dissolved in water or a salt solution similar to the backflow liquid composition in the prior art, such as soluble polyurethane, soluble rubber, etc. However, the process of dissolving the soluble polyurethane and soluble rubber in water in the prior art is usually swelling first, and then the macromolecules gradually break to form small molecules and then dissolve, and the water solubility is not good, and rapid dissolution cannot be achieved. Therefore, as a preferred solution, the rubber tube 3 is made of a degradable water-soluble elastomer, and the degradable water-soluble elastomer includes a block copolymer with a copolymer of polylactic acid and polyethylene glycol as a soft segment prepolymer and a copolymer of a sulfonic acid type hydrophilic monomer and isocyanate as a hard segment prepolymer, and the mass ratio of the soft segment prepolymer to the hard segment prepolymer is (25-120): (25-80).
[0073] The degradable water-soluble elastomer has a copolymer of polylactic acid and polyethylene glycol as a soft segment and a copolymer of a sulfonic acid type hydrophilic monomer and isocyanate as a hard segment, and a polyurethane structure of a block copolymer of the soft segment and the hard segment is generated through a polymerization reaction. When the elastomer is in water, the ester bonds in the polylactic acid are hydrolyzed to break the macromolecules of the block copolymer polyurethane structure to form a molecular structure with a smaller molecular weight. Since the polylactic acid generates hydrophilic hydroxyl groups after the ester bonds are hydrolyzed, and the sulfonic acid type hydrophilic monomer in the molecular structure is not only an anionic group but also a strong hydrophilic group, the molecular structure with a smaller molecular weight generated after the break can have strong water solubility, thereby making the elastomer have good water solubility. When the elastomer is in water, it is different from other elastomers in which the macromolecular chains swell first and then dissolve. The macromolecular chains of the elastomer are first broken into small molecules and then dispersed in water, so that swelling does not occur first and the solubility is better. In addition, the solubility of the elastomer can be regulated by regulating the proportion of polylactic acid in the molecule and the degree of polymerization of the polylactic acid. In addition, the elastomer is also environmentally friendly. The polypropionic acid in the block copolymer is a recognized material with good biodegradability. After the ester bond in the molecule is broken, it can be hydrolyzed and degraded to form lactic acid, and then the lactic acid can be completely degraded by microorganisms into carbon dioxide and water; polyethylene glycol is a water-soluble polymer. Studies have shown that polyethylene glycol with a molecular weight of more than 2000 can be metabolized by humans through the kidneys and is relatively safe for the human body; although the isocyanate structure has certain toxicity, the NCO group has a high reactivity and will react to form a non-toxic urea bond when it comes into contact with water or humid air. Therefore, the elastomer has certain environmental protection.
[0074] Among them, the sulfonic acid type hydrophilic monomer refers to a monomer having hydrophilic groups such as hydroxyl groups and amino groups and having a sulfonate, for example, sodium 1,4-butanediol-2-sulfonate, sodium N,N-di(2-hydroxyethyl)-2-aminoethanesulfonate, etc. Preferably, the sulfonic acid type hydrophilic monomer is sodium 1,4-butanediol-2-sulfonate.
[0075] Wherein, the isocyanate can be selected from one or more of diisocyanate and polyisocyanate. Preferably, the isocyanate is diisocyanate, and more preferably, the diisocyanate is selected from isophorone diisocyanate.
[0076] Among them, the polyethylene glycol preferably has a number average molecular weight of 1000-3000.
[0077] More preferably, the mass ratio of the polylactic acid component to the polyethylene glycol in the soft segment prepolymer is (5-20): (20-100).
[0078] More preferably, the mass ratio of the sulfonic acid type hydrophilic monomer to the isocyanate in the hard segment prepolymer is (10-30):(15-50).
[0079] Further preferably, the degradable water-soluble elastomer also includes a water-soluble functional additive, the mass ratio of the water-soluble functional additive to the soft segment prepolymer is (5-50): (25-120), and the water-soluble functional additive is one or more of a polyhydroxy compound and a polyamide compound. A water-soluble functional additive refers to a functional additive that can improve the mechanical properties of an elastomer material and has a certain water solubility. Preferably, the water-soluble functional additive is one or more of a polyhydroxy compound and a polyamide compound. A polyhydroxy compound refers to a compound containing a large number of hydroxyl groups in the molecule, and a polyamide compound refers to a compound containing a large number of amide groups in the molecule. The water-soluble functional additives are selected from polyhydroxy compounds or polyamide compounds. The hydroxyl and amide groups in the water-soluble functional additives can form hydrogen bonds with the urethane bonds in the polyurethane structure of the block copolymer in the elastomer, so that the two are attracted to each other due to hydrogen bonding, and the good mechanical properties of the elastomeric material are guaranteed. When water is present, the hydrogen bonds between water molecules and polyurethane, the hydrogen bonds between water molecules and polyhydroxy and polyamide water-soluble functional additives are greater than the hydrogen bonds between the two, so that the polyurethane structure and the water-soluble functional additives are both dissolved in water, thereby not affecting the water solubility of the elastomer. In addition, when the water-soluble functional additive in the elastomer is dissolved in water, a large number of pores are generated in the elastomer, which makes it easier for water molecules to enter the inside of the elastomer, promote the hydrolysis of the polylactic acid ester bonds in the block copolymer macromolecules, and promote the degradation and dissolution of the material. Further preferably, the water-soluble functional additive is one or more of polyacrylamide, polyvinyl alcohol, and guar gum.
[0080] Further preferably, the degradable water-soluble elastomer further comprises a dispersant, wherein the mass ratio of the dispersant to the soft segment prepolymer is (5-50): (25-120), and after the block copolymer of the polyurethane structure of the elastomer is degraded, the dispersant can enhance the dispersibility of each small molecule compound obtained by degradation in water. Among them, the dispersant is preferably sodium polyacrylate.
[0081] The degradable water-soluble elastomer has good mechanical strength and good dispersibility in water, and can be quickly dissolved in the flowback fluid, significantly improving the flowback efficiency. The specific composition examples and performance tests of the degradable water-soluble elastomer are shown in the examples.
[0082] The following is a further introduction to the specific implementation methods of the fast-dissolving high-strength and high-elongation magnesium alloy used in the center tube, the upper joint, the lower joint, the cone, the slip mechanism, the first metal sealing ring, and the second metal sealing ring and the degradable water-soluble elastomer used in the rubber cartridge in combination with several specific embodiments of the present invention:
[0083] Example 1
[0084] The fast-dissolving, high-strength and high-elongation magnesium alloy described in this embodiment is composed of the following elements in mass percentage: Gd 2.5%, Y 1.0%, Al 1.0%, Zn 0.5%, Zr 0.4%, Sc 0.01%, Cu 1.5%, Li 0.25%, Ni 0.25%, Ga 0.25%, In 0.25%, and the rest is Mg.
[0085] The method for preparing the fast-dissolving high-strength and high-elongation magnesium alloy described in this embodiment comprises the following specific steps:
[0086] S1. Weigh pure Mg, pure Al, pure Zn, pure Ga, pure In, Mg-Gd master alloy, Mg-Y master alloy, Mg-Zr master alloy, Mg-Sc master alloy, Mg-Cu master alloy, Mg-Li master alloy, Mg-Ni master alloy according to the selected mass percentage;
[0087] S2. Preheat the raw materials except pure Ga in step S1 at 150°C for 2h;
[0088] S3. All raw materials are mixed, and the mixed raw materials are heated to 720°C using a crucible resistance furnace, melted for 30 minutes, and a first refining agent is added, and refined for 30 minutes to remove inclusions in the melt, and then the refined material is covered with a covering agent to obtain a melt;
[0089] S4. Casting the above melt at 680°C to obtain an ingot;
[0090] S5. The ingot is homogenized, the ingot is kept at 420°C for 24h, and then the homogenized ingot is forged at 350°C to obtain a forging;
[0091] S6. Perform aging strengthening treatment on the forgings, keep the forgings at 150° C. for 32 hours, and obtain the fast-dissolving high-strength and high-elongation magnesium alloy described in this embodiment.
[0092] The first refining agent is composed of the following components by weight: MgCl 2 24-30 parts, KCl 20-26 parts, BaCl 2 28-31 parts, CaF 2 13-15 parts, NaCl 1-7 parts, CaCl 2 1-7 parts, insoluble matter ≤1.5 parts, MgO ≤1.5 parts, water ≤2 parts.
[0093] The covering agent is composed of the following components in mass percentage: MgCl 2 35-41 parts, KCl 25-29 parts, NaCl 24-28 parts, CaCl 2 6-10 parts, insoluble matter ≤ 1.5 parts, MgO ≤ 1.5 parts, H 2 O≤2 copies.
[0094] Example 2
[0095] The fast-dissolving, high-strength and high-elongation magnesium alloy described in this embodiment is composed of the following elements in mass percentage: Gd 1.5%, Y 0.5%, Al 0.1%, Zn 0.1%, Zr 0.2%, Sc 0.001%, Cu 0.1%, Li 0.01%, Ni 0.01%, Ga 0.01%, In 0.01%, and the rest is Mg.
[0096] The method for preparing the fast-dissolving high-strength and high-elongation magnesium alloy described in this embodiment is the same as that in Example 1.
[0097] Example 3
[0098] The fast-dissolving, high-strength and high-elongation magnesium alloy described in this embodiment is composed of the following elements in percentage by mass: Gd 14.5%, Y 2.0%, Al 2.0%, Zn 1.0%, Zr 0.5%, Sc 0.02%, Cu 2.0%, Li 0.5%, Ni 0.5%, Ga 0.5%, In 0.5%, and the rest is Mg.
[0099] The method for preparing the fast-dissolving high-strength and high-elongation magnesium alloy described in this embodiment is the same as that in Example 1.
[0100] Example 4
[0101] The fast-dissolving, high-strength and high-elongation magnesium alloy described in this embodiment is composed of the following elements in mass percentage: Gd 1.0%, Y 0.001%, Al 0.001%, Zn 0.001%, Zr 0.01%, Sc 0.0001%, Cu 0.01%, Li 0.01%, Ni 0.01%, Ga 0.01%, In 0.01%, and the rest is Mg.
[0102] The method for preparing the fast-dissolving high-strength and high-elongation magnesium alloy described in this embodiment is the same as that in Example 1.
[0103] Example 5
[0104] The fast-dissolving, high-strength and high-elongation magnesium alloy described in this embodiment is composed of the following elements in percentage by mass: Gd 12%, Y 4.0%, Al 1.0%, Zn 2.5%, Zr 0.5%, Sc 0.005%, Cu 0.8%, Li, Ni, Ga, In 0.4% each, and the rest is Mg.
[0105] The method for preparing the fast-dissolving high-strength and high-elongation magnesium alloy described in this embodiment is the same as that in Example 1.
[0106] Comparative Example 1
[0107] The magnesium alloy of this comparative example is composed of the following elements in percentage by mass:
[0108] The magnesium alloy is prepared in the same manner as in Example 1: Gd 2.5%, Y 1.0%, Al 1.0%, Zn 0.5%, Zr 0.4%, Sc 0.01%, and the remainder is Mg.
[0109] The fast-dissolving high-strength and high-elongation magnesium alloy of the above embodiment and the magnesium alloy of the comparative example were subjected to mechanical property tests and dissolution performance tests. The mechanical property test method was performed in accordance with GB T 228.1-2010. The dissolution performance test conditions were: The sample is placed in a 3% KCl aqueous solution at 93°C, and the weight dissolved per hour is tested. The dissolution rate is: dissolved weight / (sample surface area×time). The mechanical properties and dissolution performance indicators of the fast-dissolving high-strength and high-elongation magnesium alloy of this embodiment are shown in Table 1.
[0110] It can be seen from the mechanical properties test results that the tensile strength of the fast-dissolving high-strength and high-elongation magnesium alloy of the present application is ≥220MPa, the yield strength is ≥150MPa, and the elongation is ≥16%; the dissolution rate in 93°C, 3% KCl solution is 40-100mg·cm -2 h -1 .
[0111] Table 1 Room temperature mechanical properties and high temperature dissolution rate of magnesium alloys
[0112]
[0113] Example 6
[0114] The degradable water-soluble elastomer described in this embodiment includes the following components in parts by weight:
[0115] 185 parts of a block copolymer with a copolymer of polylactic acid and polyethylene glycol as a soft segment prepolymer and a copolymer of 1,4-butanediol-2-sodium sulfonate and isophorone diisocyanate as a hard segment prepolymer, wherein the mass ratio of the soft segment prepolymer to the hard segment prepolymer in the block copolymer is 105:80; 30 parts of polyacrylamide; 20 parts of polyvinyl alcohol; 5 parts of hydroxy silicone oil; and 5 parts of sodium polyacrylate.
[0116] The mass ratio of polylactic acid to polyethylene glycol in the soft segment prepolymer is 5:100; the number average molecular weight of polyethylene glycol is 1000;
[0117] The mass ratio of sodium 1,4-butanediol-2-sulfonate to isophorone diisocyanate in the hard segment prepolymer is 30:50.
[0118] The preparation method of the degradable water-soluble elastomer described in this embodiment is as follows:
[0119] S1. 100 parts of polyethylene glycol 1000, 5 parts of lactide and 0.5 parts of bismuth isooctanoate catalyst were put into a reactor, stirred and reacted at 180-200°C for 2 hours under a nitrogen protection environment, and then the reactor was evacuated to -0.098Mpa, and the stirring reaction was continued for 1h to prepare a copolymer polyol of polylactic acid and polyethylene glycol, which is a soft segment prepolymer;
[0120] S2. 30 parts of sodium 1,4-butanediol-2-sulfonate and 50 parts of isophorone diisocyanate were put into a reactor together, and stirred at 60 ° C for 4 hours under a nitrogen atmosphere to prepare a copolymer of sodium 1,4-butanediol-2-sulfonate and isophorone diisocyanate, which is a hard segment prepolymer;
[0121] S3. Put the soft segment prepolymer in step S1, the hard segment prepolymer in step S2, 30 parts of polyacrylamide, 20 parts of polyvinyl alcohol, 5 parts of hydroxy silicone oil, and 5 parts of sodium polyacrylate into a storage tank, stir and mix, and then extrude and granulate through a reactive twin-screw extruder at 170-200°C to obtain the degradable water-soluble elastomer of this embodiment.
[0122] Example 7
[0123] The degradable water-soluble elastomer described in this embodiment includes the following components in parts by weight:
[0124] 100 parts of a block copolymer with a copolymer of polylactic acid and polyethylene glycol as a soft segment prepolymer and a copolymer of 1,4-butanediol-2-sodium sulfonate and isophorone diisocyanate as a hard segment prepolymer, wherein the mass ratio of the soft segment prepolymer to the hard segment prepolymer in the block copolymer is 40:60; 50 parts of guar gum; 5 parts of amino silicone oil; and 50 parts of sodium polyacrylate.
[0125] The mass ratio of polylactic acid to polyethylene glycol in the soft segment prepolymer is 1:1; the number average molecular weight of polyethylene glycol is 2000;
[0126] The mass ratio of sodium 1,4-butanediol-2-sulfonate to isophorone diisocyanate in the hard segment prepolymer is 1:1.
[0127] The preparation method of the degradable water-soluble elastomer described in this embodiment is the same as that of Example 6.
[0128] Example 8
[0129] The degradable water-soluble elastomer described in this embodiment includes the following components in parts by weight:
[0130] 165 parts of a block copolymer with a copolymer of polylactic acid and polyethylene glycol as a soft segment prepolymer and a copolymer of 1,4-butanediol-2-sodium sulfonate and isophorone diisocyanate as a hard segment prepolymer; the mass ratio of the soft segment prepolymer to the hard segment prepolymer in the block copolymer is 105:60; 30 parts of polyacrylamide; 20 parts of polyvinyl alcohol; 5 parts of hydroxy silicone oil; and 5 parts of sodium polyacrylate.
[0131] The mass ratio of polylactic acid to polyethylene glycol in the soft segment prepolymer is 5:100; the number average molecular weight of polyethylene glycol is 1000;
[0132] The mass ratio of 1,4-butanediol-2-sulfonate sodium to isophorone diisocyanate in the hard segment prepolymer is 10:50.
[0133] The preparation method of the degradable water-soluble elastomer described in this embodiment is the same as that in Example 6.
[0134] Example 9
[0135] The degradable water-soluble elastomer described in this embodiment includes the following components in parts by weight:
[0136] 150 parts of a block copolymer with a copolymer of polylactic acid and polyethylene glycol as a soft segment prepolymer and a copolymer of 1,4-butanediol-2-sodium sulfonate and isophorone diisocyanate as a hard segment prepolymer; the mass ratio of the soft segment prepolymer to the hard segment prepolymer in the block copolymer is 105:45; 30 parts of polyacrylamide; 20 parts of polyvinyl alcohol; 5 parts of hydroxy silicone oil; and 5 parts of sodium polyacrylate.
[0137] The mass ratio of polylactic acid to polyethylene glycol in the soft segment prepolymer is 5:100; the number average molecular weight of polyethylene glycol is 1000;
[0138] The mass ratio of sodium 1,4-butanediol-2-sulfonate to isophorone diisocyanate in the hard segment prepolymer is 30:15.
[0139] The preparation method of the degradable water-soluble elastomer described in this embodiment is the same as that in Example 6.
[0140] Example 10
[0141] The degradable water-soluble elastomer described in this embodiment includes the following components in parts by weight:
[0142] 105 parts of a block copolymer with a copolymer of polylactic acid and polyethylene glycol as a soft segment prepolymer and a copolymer of 1,4-butanediol-2-sodium sulfonate and isophorone diisocyanate as a hard segment prepolymer; the mass ratio of the soft segment prepolymer to the hard segment prepolymer in the block copolymer is 25:80; 30 parts of polyacrylamide; 20 parts of polyvinyl alcohol; 5 parts of hydroxy silicone oil; and 5 parts of sodium polyacrylate.
[0143] The mass ratio of polylactic acid to polyethylene glycol in the soft segment prepolymer is 5:20; the number average molecular weight of polyethylene glycol is 1000;
[0144] The mass ratio of sodium 1,4-butanediol-2-sulfonate to isophorone diisocyanate in the hard segment prepolymer is 30:50.
[0145] The preparation method of the degradable water-soluble elastomer described in this embodiment is the same as that in Example 6.
[0146] Embodiment 11
[0147] The degradable water-soluble elastomer described in this embodiment includes the following components in parts by weight:
[0148] 145 parts of a block copolymer with a copolymer of polylactic acid and polyethylene glycol as a soft segment prepolymer and a copolymer of 1,4-butanediol-2-sodium sulfonate and isophorone diisocyanate as a hard segment prepolymer; the mass ratio of the soft segment prepolymer to the hard segment prepolymer in the block copolymer is 120:25; 30 parts of polyacrylamide; 20 parts of polyvinyl alcohol; 5 parts of hydroxy silicone oil; and 5 parts of sodium polyacrylate.
[0149] The mass ratio of polylactic acid to polyethylene glycol in the soft segment prepolymer is 20:100; the number average molecular weight of polyethylene glycol is 1000;
[0150] The mass ratio of sodium 1,4-butanediol-2-sulfonate to isophorone diisocyanate in the hard segment prepolymer is 10:15.
[0151] The preparation method of the degradable water-soluble elastomer described in this embodiment is the same as that in Example 6.
[0152] Comparative Example 2
[0153] The elastomer described in this comparative example comprises the following components in parts by weight:
[0154] 125 parts of block copolymer with polyethylene glycol 3000 homopolymer as soft segment prepolymer and copolymer of 1,4-butanediol-2-sodium sulfonate and isophorone diisocyanate as hard segment prepolymer; 10 parts of guar gum, 5 parts of amino silicone oil and 30 parts of sodium polyacrylate.
[0155] The mass ratio of sodium 1,4-butanediol-2-sulfonate to isophorone diisocyanate in the hard segment prepolymer is 10:15.
[0156] The preparation method of the elastomer of this comparative example is the same as that of Example 6.
[0157] The mechanical properties, injection molding properties and solubility properties of the elastomers of the above-mentioned embodiments and comparative examples were tested.
[0158] Preparation of test specimens and injection molding performance evaluation: The injection molding temperature is 170-200°C, and the specimens required for injection molding tensile properties, hardness and solubility performance tests are made by the injection molding machine KS-8502R from Jiaxing Kesu Machinery Co., Ltd.
[0159] The tensile properties of the elastomer were tested on an RG1-5 electronic universal testing machine (produced by Shenzhen Rigel Instrument Co., Ltd.) according to GB / T528-1998 standard; the hardness of the elastomer was tested on a Shaw A durometer (produced by Yangzhou Derui Instrument Co., Ltd.) according to GB / T531 standard.
[0160] Solubility test: Weigh the GB / T528-1998 standard dumbbell specimen obtained by injection molding (the weight of the dumbbell specimen before the dissolution test is recorded as m 1 ) into a 100ml beaker, add 800ml of water, and place the entire flask in a hot water bath at different temperatures to dissolve for 120h. Then, all the materials in the flask are passed through a 20-mesh sieve, and the components that do not pass through the sieve are scraped and dried in an oven at 130℃ for 5h and weighed (the mass is recorded as m 2 ). The solubility rate of the elastomer is (m 1 -m 2 ) / m 1 .
[0161] The test results of mechanical properties, injection molding properties and solubility properties of the elastomers of various embodiments and comparative examples are shown in Table 2 below.
[0162] It can be seen from the above experimental data that the degradable water-soluble elastomer of the present application has high tensile strength, high elongation at break and high hardness, and therefore has high mechanical strength; and the degradable water-soluble elastomer of the present application has good water solubility and a fast dissolution rate in the return fluid, which greatly improves the return efficiency; in addition, the degradable water-soluble elastomer of the present application also has good processing performance and good thermoplasticity.
[0163] Table 2
[0164]
[0165] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A single slip soluble bridge plug, characterized in that: The invention comprises a central tube, on which an upper joint, a rubber tube, a cone, a slip mechanism and a lower joint are sleeved in sequence, and the upper joint, the rubber tube, the cone and the slip mechanism can slide axially along the central tube; the upper joint is connected to the central tube by a shear pin; the small diameter end of the cone is inserted into the gap between the slip mechanism and the central tube; the slip mechanism comprises a first slip tooth and a second slip tooth, the tooth tip of the first slip tooth is inclined toward one side of the upper joint, and the tooth tip of the second slip tooth is inclined toward one side of the lower joint; the central tube, the upper joint, the lower joint, the cone and the slip mechanism are made of soluble metal materials, and the rubber tube is made of soluble elastic materials; the central tube and / or the upper joint and / or the lower joint and / or the cone and / or the slip mechanism are made of a fast-dissolving high-strength and high-elongation magnesium alloy, and the fast-dissolving high-strength and high-elongation magnesium alloy is composed of the following elements in percentage by mass: Gd 1.0%-22.0%, Y0.001%-5.0%, Al 0.001%-10%, Zn 0.001%-5.0%, Zr 0.01%-1.0%, Sc 0.0001%-1.0%, Cu 0.01%-10.0%, Li0.01%-3.0%, Ni 0.01%-3.0%, Ga 0.01%-3.0%, In0.01%-3.0%, and the rest are Mg and impurity elements, and the total amount of Li, Ni, Ga and In is 0.1%-6.0%.
2. The single slip soluble bridge plug according to claim 1, characterized in that: The central tube is also sleeved with a first metal sealing ring, which is arranged between the upper joint and the rubber cylinder and is made of a soluble metal material.
3. The single slip soluble bridge plug according to claim 2, characterized in that: The central tube is also sleeved with a second metal sealing ring, which is arranged between the rubber tube and the cone, and is made of a soluble metal material.
4. The single slip soluble bridge plug according to claim 1 or 2, characterized in that: The cava mechanism includes a cava seat, a plurality of stress grooves are arranged in the circumferential direction of the cava seat, and cava plates are formed between adjacent stress grooves on the cava seat. Each cava plate is provided with a plurality of first tooth grooves and second tooth grooves, the first cava teeth are arranged in the first tooth grooves, and the second cava teeth are arranged in the second tooth grooves.
5. The single slip soluble bridge plug according to claim 1 or 2, characterized in that: The highest point of the first slip tooth is higher than the highest point of the second slip tooth.
6. The single slip soluble bridge plug according to claim 1 or 2, characterized in that: The inner cavity of one end of the central tube close to the upper joint is provided with a diameter-changing cavity, and the inner diameter of the diameter-changing cavity decreases from the end of the central tube close to the upper joint to the end away from the upper joint.
7. The single slip soluble bridge plug according to claim 1 or 2, characterized in that: The inner wall of the central tube is provided with a plurality of grooves.
8. The single slip soluble bridge plug according to claim 3, characterized in that: The first metal sealing ring and / or the second metal sealing ring are made of the fast-dissolving high-strength and high-elongation magnesium alloy.
9. The single slip soluble bridge plug according to claim 1 or 2, characterized in that: The rubber cylinder is made of a degradable water-soluble elastomer, which includes a block copolymer with a copolymer of polylactic acid and polyethylene glycol as a soft segment prepolymer and a copolymer of a sulfonic acid type hydrophilic monomer and isocyanate as a hard segment prepolymer, and the mass ratio of the soft segment prepolymer to the hard segment prepolymer is (25-120): (25-80).
10. The single slip soluble bridge plug according to claim 9, characterized in that: The degradable water-soluble elastomer also includes a water-soluble functional additive, the mass ratio of the water-soluble functional additive to the soft segment prepolymer is (5-50): (25-120), and the water-soluble functional additive is one or more of a polyhydroxy compound and a polyamide compound.
Citation Information
Patent Citations
Single-slips fully-soluble bridge plug