A PTT continuous polymerization pre-crystallization process

Through the design of PTT continuous polymerization pre-crystallization process and cylindrical pre-crystallization device, the problems of adhesion, uneven heating and high energy consumption of mechanically stirred and fluidized bed pre-crystallizers are solved, and uniform pre-crystallization of PTT slices is achieved. Crystallization and drying simplify the process and reduce costs.

CN110370490BActive Publication Date: 2024-10-18ZHEJIANG HENGYI PETROCHEMICAL RES INST CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201910611140.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-07-08
Publication Date
2024-10-18
Estimated Expiration
2039-07-08

AI Technical Summary

Technical Problem

Existing mechanically stirred and fluidized bed pre-crystallizers have problems such as sticking, uneven heating, high energy consumption and complex operation during the pre-crystallization process of PTT slices, and are difficult to adapt to the different moisture contents and crystallization needs of the slices.

Method used

A PTT continuous polymerization pre-crystallization process is used, including slicing, coarse filtration, pre-crystallization and drying steps. A cylindrical pre-crystallization device is used for pre-crystallization and drying, through the staggered design of inner and outer cone baffles and steam counterflow. Heat exchange to achieve a semi-fluidized state and uniform temperature of the slices, simplify the process and reduce equipment costs.

Benefits of technology

It achieves the simultaneous completion of pre-crystallization and drying, shortens the process time, reduces energy consumption and equipment occupation, improves process efficiency and adaptability, and ensures uniform crystallinity and temperature of the slices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110370490B_ABST
    Figure CN110370490B_ABST
Patent Text Reader

Abstract

The present invention discloses a PTT continuous polymerization pre-crystallization process, including the following processes: (i) PTT material is sliced ​​by a slicer to form PTT slices; (ii) PTT slices are sent from a discharge hopper and a pelletizer pre-separator to a pelletizer water coarse filter for preliminary solid-liquid separation to screen out most of the water; (iii) wet PTT slices are sent to a pre-crystallization device for pre-crystallization, drying and treatment; (iv) dried PTT slices that have been pre-crystallized and dried are screened out of defective products by a vibrating screen; (v) stored in a warehouse. The beneficial effects of the present invention are: making the pre-crystallization and drying process short and adaptable, reducing investment, saving energy consumption and simplifying operation under the premise of meeting process requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical fiber production technology, in particular to a PTT continuous polymerization pre-crystallization technology. Background Art

[0002] Polytrimethylene terephthalate (PTT) is a new type of aromatic polyester material with excellent performance developed in the late 20th century. Compared with PET and PBT, its special "odd carbon effect" makes it have a unique spiral structure and very good elasticity. PTT has the softness of nylon, the fluffiness of acrylic and the stain resistance of polyester. It is also easy to dye and antistatic. Due to its excellent performance, PTT is widely used in clothing, industry, decoration and engineering plastics. The crystallization performance of PTT is between PBT and PET. Since the glass transition temperature of PTT is very low at 25-65℃, PTT needs to be pre-crystallized during industrial production to prevent agglomeration during the drying process. Common pre-crystallizers are mainly mechanical stirring type and fluidized bed type.

[0003] Chinese patent document CN2540269Y disclosed the "low melting point polyester chip pre-crystallization device" on March 19, 2003, which is a typical representative of the mechanical stirring type. The scheme includes a cylinder, a motor, a reducer and a conical head; the output shaft of the motor is connected to the input shaft of the reducer, the motor and the reducer are supported on the cylinder flat cover by a bracket, and the cylinder flat cover is fixedly connected to the cylinder through a flange, and is characterized in that there are multiple holes on the lower wall of the cylinder, and a feed pipe, an exhaust pipe and an intake pipe are fixed on the cylinder; there are multiple holes on the conical head, and the conical head is welded and connected to the cylinder; a stirring shaft is installed in the cylinder, and multiple stirring wings are installed on the stirring shaft. The lower part of the stirring shaft extends into the conical head, and its upper end passes through the cylinder flat cover and is connected to the output shaft of the reducer through a coupling.

[0004] The mechanical stirring pre-crystallizer is jacket heated, and the rod-shaped stirring blade rotates to mix the slices evenly. For example, the mechanical stirring pre-crystallizer is used for pre-crystallization of PTT slices. Because the PTT slices coming out of the pelletizer are easy to stick together, the slices entering the mechanical stirring pre-crystallizer are easy to stick together if they have less water content, and require a larger heat exchange area or heat exchange intensity if they have more water content. The mechanical stirring pre-crystallizer is heated by the hot jacket medium, and the jacket heating area cannot be adjusted, and the temperature of the heat medium is not easy to adjust, so it is not adaptable to the feeding slices. Before the mechanical stirring pre-crystallizer starts feeding, it is necessary to pre-fill about 1 / 3 to 1 / 2 of the cylinder volume with slices to prevent sticking and improve heat transfer efficiency. The slices must fill the pre-crystallizer cylinder to achieve the designed heat transfer effect. Since the stirring blades are mostly in the shape of steel bars, the characteristics of the slice particles make it impossible to achieve uniform heating, making the residence time of the slice particles uneven; and the heat conduction and heat transfer efficiency between solid particles is low, and the temperature of the slice particles is also prone to unevenness, resulting in uneven crystallinity of the slices. The mechanical stirring pre-crystallizer also needs to be equipped with a heat medium supply and circulation system, and its operation is relatively complicated.

[0005] On July 2, 2008, Chinese patent document CN101210772A disclosed "PTT slice drying method in PTT / PET composite fully drawn low-elastic network yarn", which is a typical representative of fluidized bed type. The PTT slices of this scheme adopt the following drying method: the first step, screening: the PTT slice raw material passes through the silo → vibrating screen → pulse generator → another silo; the second step, pre-crystallization: from another silo → vibrating feeder → fluidized bed → drying tower, the PTT slices stay in the fluidized bed pre-crystallizer for 5-15 minutes to complete the pre-crystallization process; the third step, drying: after 4-6 hours of high-temperature dry air drying, the moisture content of the uniformly crystallized PTT slices has reached the standard. The drying method of the present invention makes the PTT dry slices crystallize uniformly, with normal hue and no yellowing and degradation phenomenon; the slice moisture content is below 50ppm, which has met the production drying process requirements of PTT-POY pre-oriented yarns and the requirements of composite spinning with PET. The spinning of PTT dry slices is stable and there is no floating phenomenon.

[0006] The boiling fluidized bed pre-crystallizer is not suitable for materials with high water content and easy to stick together. The PTT slices from the pelletizer are easy to stick together after drying, and the water content is high if they are directly put into the pre-crystallizer without drying. At the same time, maintaining the fluidized state of the slices requires a large amount of hot air circulation, which consumes a lot of energy and the slice particles are also prone to high-speed collision. Summary of the invention

[0007] Based on the above problems, the present invention provides a PTT continuous polymerization pre-crystallization process, which makes the pre-crystallization and drying processes short and adaptable, reduces investment, saves energy consumption and simplifies operation while meeting process requirements.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical scheme: a PTT continuous polymerization pre-crystallization process, including the following process:

[0009] (1) The PTT material is sliced ​​by a slicer to form PTT slices;

[0010] (ii) PTT slices are sent from the discharge hopper and pelletizer pre-separator to the pelletizer water coarse filter for preliminary solid-liquid separation to remove most of the water;

[0011] (3) The wet PTT slices are sent to the pre-crystallization device for pre-crystallization and drying;

[0012] (IV) The dried PTT slices that have been pre-crystallized and dried are screened out with a vibrating screen to remove defective products;

[0013] (V) Storage in warehouse;

[0014] Among them, the pre-crystallization device includes a cylindrical tank body, which is longitudinally sealed, with a feed port at the upper end of the tank body, a discharge port at the lower end, a steam inlet at the lower side wall of the tank body, a steam outlet at the upper side wall of the tank body, and a slice pre-crystallization quick-drying structure is provided in the tank body between the height of the steam inlet and the height of the steam outlet; the slice pre-crystallization quick-drying structure is as follows: a central column is provided along the axis of the tank body; a plurality of inner cone baffles are provided on the central column, the inner cone baffles extend along the conical surface of a right cone, the inner end is fixed to the central column, and a gap is provided between the outer end and the inner wall of the tank body; a plurality of outer cone baffles are provided on the inner wall of the tank body, the outer cone baffles extend along the conical surface of an inverted cone, the outer end is fixed to the inner wall of the tank body, and a gap is provided between the inner end and the central column; the inner cone baffles and the outer cone baffles are staggered in a one-to-one correspondence in the height direction.

[0015] The PTT continuous polymerization pre-crystallization process designed in this technical solution includes several major steps, including slicing, coarse filtration, pre-crystallization, drying and screening. Among them, the slicing is selected by a pelletizer. The PTT slices cut by the pelletizer are mixed with a large amount of water and cannot be directly pre-crystallized in the next step. Therefore, after slicing, they are coarsely filtered through the pelletizer water coarse filter to remove most of the water and reduce the working pressure of the subsequent drying step. After that, the wet PTT slices are sent to the pre-crystallization device, and the pre-crystallization and drying steps are completed simultaneously in the pre-crystallization device to improve efficiency. The feeding device for feeding the PTT slices into the pre-crystallization device can generally select a rotary feed valve, etc. After the PTT slices are discharged from the pre-crystallization device, pre-crystallization and drying have been achieved. At this time, the PTT slices only need to be sent to the vibrating screen for screening, and the defective products are removed. The good products can be stored in the warehouse, or directly sent to the subsequent processing steps. If the vibrating screen is directly placed at the discharge end of the pre-crystallization device, a rotary discharge valve can be installed at the discharge end of the pre-crystallization device, one is to act as a seal as the discharge port, and the other is to control the discharge speed. In this process, the core equipment is a pre-crystallization device, whose main structure is a longitudinally placed round tank with a sealed tank body, feeding at the upper end and discharging at the lower end. Steam is introduced into the lower end of the side wall of the tank body and discharged from the upper end. A central column is designed in the center of the tank body, extending along the axial direction of the tank body, and the height position is between the steam inlet and outlet. A number of inner cone baffles are fixed on the outer wall of the central column. The inner cone baffles extend along the conical surface of a right cone, with the inner end higher than the outer end, the inner end connected to the side wall of the central column, and the outer end is a free end, forming a gap between the inner wall of the tank body, which allows steam to go up and materials to go down. Correspondingly, a number of outer cone baffles are also fixed on the inner wall of the tank body, which extend along the conical surface of an inverted cone, with the outer end higher than the inner end, the outer end connected to the inner wall of the tank body, and the inner end is a free end, forming a gap between the outer wall of the central column, which allows steam to go up and materials to go down. Correspondingly, a number of outer cone baffles are also fixed on the inner wall of the tank body, which extend along the conical surface of an inverted cone, with the outer end higher than the inner end, the outer end connected to the inner wall of the tank body, and the inner end is a free end, forming a gap between the outer wall of the central column, which allows steam to go up and materials to go down. The inner cone baffle and the outer cone baffle are arranged alternately in the height direction, generally the highest is the inner cone baffle and the lowest is the outer cone baffle. The inner cone baffle and the outer cone baffle can be made of materials with stable chemical shape and sufficient rigidity, such as stainless steel. In the above structure, the material falls from above driven by gravity, and in the process of falling, it passes through the staggered inclined planes formed by the inner cone baffle and the outer cone baffle in turn, changing from free fall to step-by-step sliding, which significantly slows down the falling speed. During the falling process of the material, the countercurrent and cross-current heat exchange with the steam rising from below is realized to achieve pre-crystallization and drying of the slices. In this process, the slices are in a semi-fluidized state, achieving full contact with the steam, strong mixing and dispersion between gas and solid, high heat exchange efficiency, uniform slice temperature, and avoiding uneven crystallization. The conical surface design of the baffle can make the material flow stably along the upper surface of the baffle, without high-speed collision of pelletizing, which can prevent the agglomeration of the material.By using the pre-crystallization device, the two steps of pre-crystallization and drying can be completed at one time, which compresses the process flow, shortens the process time, reduces the space occupied by the equipment, improves the process efficiency, and saves the equipment cost and process cost.

[0016] Preferably, the central column is a circular hollow tube, the upper end of which is closed, and the lower end is open outside the tank body and connected to the steam source; the hollow tube is provided with a number of turbulent holes that penetrate the tube wall. In this scheme, the central column is defined as a hollow tube, the lower end of which extends outside the tank body and is connected to the steam source, the upper end is closed, and turbulent holes are opened on the side wall of the hollow tube. Steam is ejected from the turbulent holes, which continuously turbulently disturb the material flow at a close distance, so that the material is dried more fully and the pre-crystallization effect is better. In actual applications, the steam inlet and the steam intake in the hollow tube can be adjusted to obtain the best process matching effect according to process requirements.

[0017] Preferably, the spoiler holes are divided into several groups, one group is arranged under the root of each inner cone baffle; the spoiler holes in each group are evenly arranged on the circumference of the cross section of the central tube. There are special requirements for the arrangement position of the spoiler holes, and it is better to arrange them in a ring below the root of each inner cone baffle. When the spoiler holes are arranged at this position, the airflow is restricted by the inner cone baffle, forming an outward and downward inclined airflow direction, and the material sliding down from the upper surface of the inner cone baffle continues to be disturbed by the steam ejected from the spoiler holes when falling at the end. By adjusting the spoiler steam flow rate, the flow speed and direction of the slice falling to the upper surface of the outer cone baffle below can be changed, so that it is in a semi-fluidized state, which is conducive to the dispersion, pre-crystallization and drying of the material.

[0018] Preferably, a circular gap is formed between the outer end of the inner cone baffle and the inner wall of the tank body at the same height, and the area of ​​the gap is S1; a circular gap is formed between the inner end of the outer cone baffle and the outer wall of the center column at the same height, and the area of ​​the gap is S2; the cross-sectional area of ​​the steam inlet is S3, and 20*S3≤S1≤50*S3, 10*S3≤S2≤40*S3. The area where S1 and S2 are located is the narrow position of the flow channel through which the material passes, and it is also the position where the steam passes when it rises. This position is the area where the material and steam are mixed and dispersed most intensely. By adjusting the flow rate of the rising steam, the descending speed of the slice can be easily adjusted, so the size of this area has a significant effect on the effect of pre-crystallization and drying of the material. The above parameters are the optimal numerical ranges obtained by the inventor based on process requirements and combined with multiple experiments.

[0019] Preferably, the upper end of the central column is an upwardly convex arc top, and the feed port is located directly above the arc top. The material falls freely from the feed port and lands on the arc top at the upper end of the central column, and can be evenly dispersed by its own gravity, without the need for a material disperser, thus saving costs and reducing equipment usage.

[0020] Preferably, the lower end of the tank body is inverted cone shape, and the discharge port is located at the end of the inverted cone; a bottom steam inlet is provided on the side wall of the inverted cone-shaped tank body. After the material passes through the slice pre-crystallization quick-drying structure above, most of the pre-crystallization and drying are completed, and then it falls into the lower end of the inverted cone-shaped tank body, and then stays at the lower end of the tank body for a period of time. During the stay period, the bottom steam inlet continues to introduce steam to help the material complete the final pre-crystallization and drying. The residence time is determined by technicians in this field according to the process requirements.

[0021] Preferably, there are several bottom steam inlets, which are evenly distributed along the circumference of the inverted conical tank side wall. This design ensures uniformity of steam distribution and avoids the occurrence of particle bridging.

[0022] Preferably, a steam distributor is connected to the inner side of the steam inlet, and the steam distributor is an annular tube type or a straight tube type, and a slot or hole is opened at the bottom of the steam distributor. Steam is ejected from the slot or hole at the bottom of the steam distributor and can be evenly distributed in the cylinder.

[0023] Preferably, the angle between the generatrix of the cone where the inner cone baffle and the outer cone baffle are located and the horizontal direction is 20°~55°. The inclination of the inner cone baffle and the outer cone baffle determines the sliding speed of the material on its inclined upper surface, and affects the length of time the material interacts with the ascending steam, and affects the dryness and crystallinity of the material.

[0024] Preferably, the roughness of the upper surface of the inner cone baffle and the outer cone baffle is Ra≤0.8. The upper surface of the inner cone baffle and the outer cone baffle should be smooth to prevent the material from being stuck on the surface and unable to slide down due to static friction.

[0025] Preferably, a plurality of cleaning holes are provided on the side wall of the tank body; each cleaning hole is divided into a plurality of layers in the height direction, each layer includes at least 3 cleaning holes, and is evenly distributed along the circumference; the opening position of the cleaning holes in the same layer on the inner side of the tank body is located between the heights of a group of adjacent inner cone baffles and outer cone baffles. If necessary, the operator manually cleans the inner cone baffles and outer cone baffles inside the tank body from outside the tank body.

[0026] As a preferred embodiment, each cleaning hole is provided with a sight glass, through which the operator can monitor the operation status in the tank at any time and take necessary treatment measures in time if any abnormality is found.

[0027] In summary, the beneficial effects of the present invention are: making the pre-crystallization and drying process short and adaptable, reducing investment, saving energy consumption and simplifying operation under the premise of meeting process requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is the process route diagram of the present invention.

[0029] Figure 2 It is a structural schematic diagram of the pre-crystallization device of the present invention.

[0030] Wherein: A pelletizer, B discharge hopper, C pelletizer pre-separator, D pelletizer water coarse filter, E rotary feed valve, F pre-crystallization device, G rotary discharge valve, H vibrating screen; 1 tank body, 2 feed port, 3 discharge port, 4 steam inlet, 5 steam outlet, 6 center column, 7 inner cone baffle, 8 outer cone baffle, 9 spoiler hole, 10 bottom steam inlet, 11 steam distributor, 12 manhole, 13 cleaning hole;

[0031] In the figure, the dotted arrows indicate the steam flow direction, and the solid arrows indicate the material flow direction. DETAILED DESCRIPTION

[0032] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0033] like Figure 1 The embodiment shown is a PTT continuous polymerization pre-crystallization process, which is applied to a 30,000 tons / year PTT polyester continuous production line of a PTT production enterprise.

[0034] The PTT continuous polymerization pre-crystallization process of this example has the following process flow: the PTT slices cut out from the pelletizer A pass through the discharge hopper B and the pelletizer pre-separator C, and most of the water is filtered out by the pelletizer water coarse filter D, and then sent to the pre-crystallization device F for pre-crystallization and drying through the rotary feed valve E; the PTT pellets that have completed pre-crystallization and drying are sent to the vibrating screen H through the rotary discharge valve G that can adjust the discharge speed, and the pellets that pass the screening are sent to the slice silo for storage through pneumatic conveying.

[0035] like Figure 2 As shown, the pre-crystallization device used in this process is provided with a cylindrical tank body 1, which is longitudinally placed and sealed. The upper end of the tank body is an arc-shaped top, and a feed inlet 2 is provided in the center of the top. The lower end is an inverted cone, and a discharge port 3 is provided at the bottom of the inverted cone. A steam inlet 4 is provided on the lower right side of the side wall of the tank body, and a steam outlet 5 is provided on the upper right side.

[0036] A slice pre-crystallization quick-drying structure is provided inside the tank body between the height of the steam inlet and the height of the steam outlet. The slice pre-crystallization quick-drying structure is as follows: a central column 6 is provided inside the tank body along the axis; a plurality of inner cone baffles 7 are provided on the central column, the inner cone baffles extend along the conical surface of a right cone, the inner end is fixed to the central column, and a gap is provided between the outer end and the inner wall of the tank body; a plurality of outer cone baffles 8 are provided on the inner wall of the tank body, the outer cone baffles extend along the conical surface of an inverted cone, the outer end is fixed to the inner wall of the tank body, and a gap is provided between the inner end and the central column; the inner cone baffles and the outer cone baffles are staggered and arranged one by one in the height direction. The central column is a circular hollow tube, the upper end of which is closed and provided with an upward convex arc top, and the arc top is located directly below the feed port. The lower end of the hollow tube opens outside the left side of the tank body and is connected to the steam source; the hollow tube is provided with a plurality of turbulent holes that penetrate the tube wall. In this example, the spoiler holes are divided into several groups, one group is set under the root of each inner cone baffle; the spoiler holes in each group are evenly arranged on the circumference of the cross section of the center tube. A circular gap is formed between the outer end of the inner cone baffle and the inner wall of the tank body of the same height, and the area of ​​the gap is S1; a circular gap is formed between the inner end of the outer cone baffle and the outer wall of the center column of the same height, and the area of ​​the gap is S2; the cross-sectional area of ​​the steam inlet is S3, and 20*S3≤S1≤50*S3, 10*S3≤S2≤40*S3. The values ​​in this example are: S1=35*S3, S2=25*S3.

[0037] The inner cone baffle and the outer cone baffle are made of stainless steel plates. The angle between the generatrix of the cone where the inner cone baffle is located and the horizontal direction is 25°, and the angle between the generatrix of the cone where the outer cone baffle is located and the horizontal direction is 25°. The upper surfaces of the inner cone baffle and the outer cone baffle are polished to ensure that the roughness Ra≤0.8.

[0038] The inverted conical tank sidewall is provided with a bottom steam inlet 10, in this example, 8 bottom steam inlets are evenly distributed along the circumference of the inverted conical tank sidewall. A manhole 12 is also provided on the inverted conical tank sidewall for maintenance personnel to enter and exit the tank.

[0039] The inner side of the steam inlet is connected to a steam distributor 11. In this example, the steam distributor is a ring tube type, and a plurality of small holes are opened at equal intervals at the lower part of the steam distributor so that the steam can be evenly distributed in the tank body after entering.

[0040] A number of cleaning holes 13 are provided on the side wall of the tank body; each cleaning hole is divided into several layers in the height direction. In this example, each layer includes 3 cleaning holes, which are evenly distributed along the circumference; the opening position of the cleaning holes in the same layer on the inner side of the tank body is located between the heights of a group of adjacent inner cone baffles and outer cone baffles. Each cleaning hole is provided with a sight glass. The operator can observe the flow of materials inside the tank body through the sight glass, and can clean the inner cone baffle and outer cone baffle at the location through the cleaning hole when necessary to avoid material accumulation.

[0041] In this pre-crystallization device, the wet slices fall from top to bottom, and slide down step by step along the stepped slopes of the inner cone baffle and the outer cone baffle. During the sliding process, the slices and the steam from bottom to top have strong countercurrent and cross-current heat exchange, so that the slices are pre-crystallized and dried; in this process, the slices are in a semi-fluidized state, fully contacting with the steam, and there is strong mixing and dispersion between the gas and the solid, with high heat exchange efficiency, uniform slice temperature, and uneven crystallization. At the same time, the steam ejected from the hollow tube plays a role in strengthening heat exchange and affecting the flow rate of the slices. By adjusting the water vapor flow and temperature, it can well adapt to the change of the water content of the slices. When the slices fall to the lower end of the inverted cone tank, they stay for another 20 minutes, and are further dried by steam, and can avoid agglomeration and bridging. Finally, the steam is discharged from the steam outlet above, and the dried slices are discharged from the discharge port through the discharge rotary valve G below the tank.

[0042] In this example, the temperature of the steam introduced into the tank of the pre-crystallization device is controlled at 120-160° C., and the crystallinity of the PTT slices pre-crystallized and dried by the pre-crystallization device can reach 60% or higher.

Claims

1. A PTT continuous polymerization pre-crystallization process, characterized in that it includes The following process: (i) The PTT material is sliced ​​by a slicer (A) to form PTT slices; (ii) The PTT slices are sent from the discharge hopper (B) and the pelletizer pre-separator (C) to the pelletizer water coarse filter (D) for preliminary solid-liquid separation to remove most of the water; (iii) The wet PTT slices are sent to the pre-crystallization device (F) for pre-crystallization and drying; (iv) The dried PTT slices after pre-crystallization and drying are screened through a vibrating screen (G) to remove defective products; (V) Storage in warehouse; The pre-crystallization device comprises a cylindrical tank body (1), which is longitudinally sealed, has a feed port (2) at the upper end of the tank body, a discharge port (3) at the lower end, a steam inlet (4) at the lower side wall of the tank body, a steam outlet (5) at the upper side wall of the tank body, and a slice pre-crystallization quick-drying structure is provided in the tank body between the height of the steam inlet and the height of the steam outlet; the slice pre-crystallization quick-drying structure comprises: a central column (6) is provided in the tank body along the axis; a plurality of inner cone baffles (7) are provided on the central column, the inner cone baffles extend along the conical surface of a right cone, the inner ends are fixed to the central column, and a gap is provided between the outer ends and the inner wall of the tank body; a plurality of outer cone baffles (8) are provided on the inner wall of the tank body, the outer cone baffles extend along the conical surface of an inverted cone, the outer ends are fixed to the inner wall of the tank body, and a gap is provided between the inner ends and the central column; the inner cone baffles and the outer cone baffles are staggered and arranged one by one in the height direction; The central column is a circular hollow tube, the upper end of which is closed and the lower end of which is open outside the tank body and connected to the steam source; a group of flow-disturbing holes (9) penetrating the tube wall are respectively provided under the root of each inner cone baffle on the hollow tube.

2. A PTT continuous polymerization pre-crystallization process according to claim 1, characterized in that: The spoiler holes arranged under the roots of the inner cone baffles are evenly arranged on the circumference of the cross section of the central tube.

3. A PTT continuous polymerization pre-crystallization process according to claim 1 or 2, characterized in that: A circular gap is formed between the outer end of the inner cone baffle and the inner wall of the tank body of the same height, and the area of ​​the gap is S1; a circular gap is formed between the inner end of the outer cone baffle and the outer wall of the center column of the same height, and the area of ​​the gap is S2; the cross-sectional area of ​​the steam inlet is S3, and 20*S3≤S1≤50*S3, 10*S3≤S2≤40*S3.

4. A PTT continuous polymerization pre-crystallization process according to claim 1 or 2, characterized in that: The upper end of the central column is an upwardly convex arc-shaped top, and the feed inlet is located directly above the arc-shaped top.

5. A PTT continuous polymerization pre-crystallization process according to claim 1 or 2, characterized in that: The lower end of the tank body is in an inverted cone shape, and the discharge port is located at the end of the inverted cone; a bottom steam inlet (10) is provided on the side wall of the inverted cone-shaped tank body.

6. A PTT continuous polymerization pre-crystallization process according to claim 5, characterized in that: There are several bottom steam inlets, which are evenly distributed along the circumference on the side wall of the inverted cone-shaped tank body.

7. A PTT continuous polymerization pre-crystallization process according to claim 1 or 2, characterized in that: The inner side of the steam inlet is connected to a steam distributor (11), which is a ring tube type or a straight tube type, and has grooves or holes at the bottom.

8. A PTT continuous polymerization pre-crystallization process according to claim 1 or 2, characterized in that: The included angle between the generatrix of the cone where the inner cone baffle and the outer cone baffle are located and the horizontal direction is 20°~55°.

9. A PTT continuous polymerization pre-crystallization process according to claim 1 or 2, characterized in that: The roughness of the upper surfaces of the inner cone baffle and the outer cone baffle is Ra≤0.

8.

10. A PTT continuous polymerization pre-crystallization process according to claim 1 or 2, characterized in that: A plurality of cleaning holes are arranged on the side wall of the tank body; each cleaning hole is divided into a plurality of layers in the height direction, each layer includes at least 3 cleaning holes, and is evenly distributed along the circumference; the opening position of the cleaning holes in the same layer on the inner side of the tank body is located between the heights of an adjacent set of inner cone baffles and outer cone baffles.

Citation Information

Patent Citations

  • PTT slicing drying method for PTT / PET composite full drafting low-elasticity network thread

    CN101210772A

  • Low melting point polyester slice pre-crystallization device

    CN2540269Y

  • PTT continuous polymerization pre-crystallization device

    CN210477469U