Electrolyte for lithium secondary battery and lithium secondary battery containing the same
An electrolyte containing bis(trimethylsilyl)fumarate, bis(trimethylsilyl)thiophene-2,5-dicarboxylic acid ester and trimethylphenylsilane in a lithium secondary battery is used in a lithium secondary battery The composition forms a stable solid electrolyte contact layer, which solves the problems of increased resistance and short life of lithium secondary batteries under high temperature conditions, and improves output characteristics and life.
Patent Information
- Application Number
- CN201811177039.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-05-29
- Filing Date
- 2018-10-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2038-10-10
AI Technical Summary
The existing lithium secondary batteries have side reactions between the anode active substance and the electrolyte under high temperature conditions, resulting in an increase in resistance, a decrease in output characteristics, and a short life.
Using an electrolyte composition comprising lithium salts, solvents and specific additives, including bis(trimethylsilyl)fumarate, bis(trimethylsilyl)thiophene-2,5-dicarboxylic acid and tris Methylphenylsilane is used to form a stable solid electrolyte contact layer on the anode and cathode surfaces, reducing moisture and acidic substances, and inhibiting the dissolution and decomposition of the anode active substances.
It improves the output characteristics and life of lithium secondary batteries, reduces resistance, and extends the battery's cycle stability and high-temperature storage performance.
Smart Images

Figure CN110544792B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electrolyte for a lithium secondary battery, and more particularly to an electrolyte composition for medium-to-large lithium secondary batteries having improved output characteristics and life characteristics, and a lithium secondary battery comprising the composition. Background Art
[0002] Generally speaking, lithium secondary batteries have higher operating voltage and greater energy density than lead batteries and nickel / cadmium batteries by storing electrically active materials. As a result, lithium secondary batteries have attracted much attention as energy storage devices for electric vehicles (EVs) and hybrid electric vehicles (HEVs).
[0003] In order to extend the driving distance of electric vehicles, the most critical issue is to increase the energy density of batteries. In order to achieve high energy density of batteries, it is necessary to increase the energy density of the raw materials used. Currently, lithium secondary batteries using Ni, Co, Mn series anode raw materials and graphite cathodes have been developed, but it is necessary to develop electrolyte compositions that can improve output characteristics and life characteristics. Summary of the invention
[0004] [Technical problem to be solved by the invention]
[0005] The disclosed embodiments provide an electrolyte composition for a lithium secondary battery having improved output characteristics and life characteristics, and a lithium secondary battery including the composition.
[0006] [Technical solutions for solving technical problems]
[0007] As a technical solution for solving the above technical problems, a lithium secondary battery according to one aspect comprises: an anode containing an anode active material; a cathode containing a cathode active material; a separator located between the anode and the cathode; and an electrolyte.
[0008] The electrolyte comprises an electrolyte composition,
[0009] The electrolyte composition comprises a lithium salt, a solvent and an additive, wherein the additive comprises at least one of bis(trimethylsilyl)fumarate and bis(trimethylsilyl)thiophene-2,5-dicarboxylate.
[0010] In addition, the content of the above additives may be 10 wt % or less (excluding the case of 0 wt %) relative to the entire electrolyte composition.
[0011] In addition, the content of the above additives may be 0.2 wt % to 3 wt % relative to the total electrolyte composition.
[0012] In addition, the additive may further include trimethyl(phenyl)silane.
[0013] In addition, the content of the trimethylphenylsilane may be 10 wt % or less (excluding the case of 0 wt %) based on the total electrolyte composition.
[0014] In addition, the content of the trimethylphenylsilane may be 0.5 wt % to 5 wt % based on the total electrolyte composition.
[0015] In addition, the above-mentioned additives may further include VC (Vinylene Carbonate).
[0016] In addition, the total content of the additives including the above-mentioned bis(trimethylsilyl)fumarate, bis(trimethylsilyl)thiophene-2,5-dicarboxylate, VC (vinylene carbonate) and trimethylphenylsilane can be 10 wt% or less (excluding the case of 0 wt%) relative to the entire electrolyte composition.
[0017] In addition, the total content of the additive including bis(trimethylsilyl)fumarate, bis(trimethylsilyl)thiophene-2,5-dicarboxylate, VC (vinylene carbonate) and trimethylphenylsilane may be 0.5 wt % to 1.5 wt % based on the total electrolyte composition.
[0018] In addition, the above lithium salts can be obtained from LiPF 6 , LiBF 4 、LiClO 4 、LiCl、LiBr、LiI、LiB 10 Cl 10 、LiCF 3 SO 3 、LiCF 3 CO 2 、LiAsF 6 、LiSbF 6 、LiAlCl 4 , CH 3 SO 3 Li, CF 3 SO 3 Li、LiN(SO 2 C 2 F 5 ) 2 、Li(CF 3 SO 2 )2 N、LiC 4 F 9 SO 3 、LiB(C 6 H 5 ) 4 、Li(SO 2 F) 2 N(LiFSI) and (CF 3 SO 2 ) 2 Select one or more from NLi.
[0019] In addition, the above-mentioned solvent can be one or more selected from ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) and ethyl methyl carbonate (EMC).
[0020] In addition, the anode active material may include an anode active material of a lithium nickel-manganese-cobalt three-component system, wherein the Ni content in the lithium nickel-manganese-cobalt three-component system is greater than 30 wt % and less than 100 wt %.
[0021] In addition, the above-mentioned diaphragm may include a ceramic coating diaphragm.
[0022] An electrolyte composition for a lithium secondary battery according to another aspect may include a lithium salt, a solvent, and an additive including bis(trimethylsilyl)fumarate or bis(trimethylsilyl)thiophene-2,5-dicarboxylate.
[0023] In addition, the content of the above additives may be 0.2 wt % to 3 wt % relative to the total electrolyte composition.
[0024] In addition, the above-mentioned additives may further contain trimethylphenylsilane.
[0025] In addition, the content of the trimethylphenylsilane may be 0.5 wt % to 5 wt % based on the total electrolyte composition.
[0026] In addition, the above-mentioned additives may further contain VC (vinylene carbonate).
[0027] In addition, the total content of the additive including bis(trimethylsilyl)fumarate, bis(trimethylsilyl)thiophene-2,5-dicarboxylate, VC (vinylene carbonate) and trimethylphenylsilane may be 1 wt % to 2.5 wt % based on the total electrolyte composition.
[0028] [Effects of the invention]
[0029] According to one aspect, an electrolyte for a lithium secondary battery can reduce the VC content in the prior art and improve the output of the lithium secondary battery by achieving low resistance characteristics by using at least one of bis(trimethylsilyl)fumarate and bis(trimethylsilyl)thiophene-2,5-dicarboxylate as an additive that forms a film on the cathode active material to increase the life. Therefore, it is useful for application in medium and large batteries.
[0030] In addition, by using trimethylphenylsilane as an additive, moisture vulnerability can be compensated and the life of the lithium secondary battery can be improved, wherein the above trimethylphenylsilane can suppress the generation of HF that reduces the life of the anode active material composed of Ni, Co, and Mn. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figures 1 to 5 is a graph showing life characteristics of a lithium secondary battery according to one embodiment. DETAILED DESCRIPTION
[0032] Throughout the specification, the same reference numerals refer to the same constituent elements. This specification does not describe all elements of the embodiments, and general contents in the technical field to which the present invention belongs or contents repeated between the embodiments are omitted.
[0033] Throughout the specification, when a part is described as “comprising” a certain constituent element, unless there is a particular description to the contrary, it does not exclude other constituent elements but means that other constituent elements may be further included.
[0034] In the case where it is not obvious that different meanings are indicated from the understanding of the context, an expression in the singular number includes an expression in the plural number.
[0035] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings and diagrams. First, a lithium secondary battery to which the electrolyte for lithium secondary batteries according to the present invention is applied will be described, and then the electrolyte for lithium secondary batteries will be described in detail.
[0036] Generally speaking, lithium secondary batteries use LiCoO 2 This lithium transition metal oxide is used as an anode active material, a graphite-based material is used as a cathode active material, and a carbonate-based organic solvent that is stable even at a relatively high voltage is used as an electrolyte that functions as a lithium ion transfer path.
[0037] During charging, lithium ions are deintercalated from the anode active material, which acts as a lithium ion source, and move to the interlayer of the carbon layered structure of the cathode, which acts as a storage place for lithium ions. During discharging, lithium ions return from the cathode to the anode and generate electricity. Therefore, the degree of lithium ion activation of the anode active material and whether there is sufficient space in the cathode active material to intercalate lithium ions will determine the performance of the battery.
[0038] However, there are the following problems: the active material reacts with the electrolyte to produce gas; during charging / discharging, manganese and other metals dissolve into the electrolyte and combine with other organic matter, thereby increasing resistance, ultimately resulting in the inability of lithium cations to move freely and reducing battery output characteristics.
[0039] Specifically, the precipitation of manganese components occurs more seriously during high-temperature storage. The dissolved manganese components are precipitated on the surface of the cathode active material, receive electrons from the cathode active material, and decompose the electrolyte on the cathode active material through a reduction reaction, thereby increasing the resistance of the battery.
[0040] Generally speaking, the electrolyte of a lithium secondary battery contacts the electrode and causes a redox reaction at the interface. As a result, LiF, Li 2 CO 3 、LiO 2 , LiOH and other substances to form a film on the surface of the cathode. This film is called a solid electrolyte interface (SEI) film.
[0041] Once the SEI film is formed during initial charging, it blocks the reaction of lithium ions with the cathode or other substances when the battery is subsequently used and repeatedly charged / discharged, and functions as an ion channel that allows only lithium ions to pass between the electrolyte and the cathode.
[0042] Therefore, attempts have been made to develop additives that can form a SEI film on the electrode surface.
[0043] According to the disclosed embodiment, a lithium secondary battery is provided, which includes an anode, a cathode, a separator and an electrolyte, wherein the electrolyte includes an electrolyte composition, and the electrolyte composition includes a lithium salt, a solvent and an additive.
[0044] As the anode, cathode, and separator constituting the electrode structure, any of those generally used in the production of lithium secondary batteries can be used.
[0045] As the cathode active material, generally, graphites capable of absorbing and releasing lithium ions can be used, but the material is not limited to any specific graphites.
[0046] In addition, as a diaphragm, a conventional porous polymer membrane can be used alone or in a laminated form, for example, a porous polymer membrane made of polyolefin polymers such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer and ethylene / methacrylate copolymer, or a ceramic coating can be used, but is not limited to this.
[0047] The electrolyte composition according to the disclosed embodiment is more preferably used in a lithium secondary battery using an anode containing a nickel-rich anode active material, so the anode may contain a lithium nickel-manganese-cobalt three-component system anode active material.
[0048] Specifically, the anode active material of the above-mentioned lithium nickel-manganese-cobalt three-component system may contain Ni as the main component. Ni is an element that improves the reversible capacity and life characteristics of the battery, and its content relative to the composition of the three-component system may be 30wt% or more and less than 100wt%, preferably the content of Ni is 60wt% or more, and more preferably 80wt% to 90wt%.
[0049] The components and composition ratios of the electrolyte solution for lithium secondary batteries according to the disclosed embodiment will be described in more detail below. Unless otherwise specified, the units are weight % (wt %).
[0050] The electrolyte composition for a lithium secondary battery according to one aspect of the present invention may include a lithium salt, a solvent, and an additive, wherein the additive includes at least one of bis(trimethylsilyl)fumarate and bis(trimethylsilyl)thiophene-2,5-dicarboxylate.
[0051] The above lithium salts can be prepared from LiPF 6 , LiBF 4 、LiClO 4 、LiCl、LiBr、LiI、LiB 10 Cl 10 、LiCF 3 SO 3 、LiCF 3 CO 2 、LiAsF 6 、LiSbF 6 、LiAlCl 4 , CH 3 SO 3 Li, CF 3 SO 3 Li、LiN(SO 2 C 2 F 5 ) 2 、Li(CF 3 SO 2 )2 N、LiC 4 F 9 SO 3 、LiB(C 6 H 5 ) 4 、Li(SO 2 F) 2 N(LiFSI) and (CF 3 SO 2 ) 2 Select one or more from NLi.
[0052] On the other hand, the above-mentioned solvent can be one or more selected from ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) and ethyl methyl carbonate (EMC).
[0053] The above-mentioned bis(trimethylsilyl)fumarate is an additive for forming a stable SEI film on the surface of the cathode active material. When the content is too much, the resistance of the cathode electrode increases and the output characteristics deteriorate. Therefore, the upper limit can be limited to 10.0wt% in the present invention. The content of bis(trimethylsilyl)fumarate is preferably 0.2wt% to 3.0wt%, and more preferably 0.1wt% to 0.5wt%.
[0054] The above-mentioned bis(trimethylsilyl)thiophene-2,5-dicarboxylate is an additive for forming a stable SEI film on the surface of the cathode active material. When the content is too much, there is a problem that the resistance of the cathode electrode increases and the output characteristics of the battery cell deteriorate. Therefore, in the present invention, the upper limit can be limited to 10.0wt%. The content of bis(trimethylsilyl)thiophene-2,5-dicarboxylate is preferably 0.2wt% to 3.0wt%, and more preferably 0.1wt% to 0.5wt%.
[0055] The electrolyte composition for a lithium secondary battery according to the disclosed embodiment may further include trimethylphenylsilane as an additive.
[0056] Since trimethylphenylsilane contains silyl, it plays a role in removing water from the electrolyte and inhibiting the hydrolysis of lithium salts. Moreover, even if the lithium salts in the electrolyte hydrolyze to generate acidic substances (e.g., HF, etc.), the above acidic substances can be selectively removed by the neutralization reaction between the oxidative decomposition products of the above trimethylphenylsilane and the above acidic substances. Furthermore, if trimethylphenylsilane is added, it also has the additional effect of forming a stable SEI film on the surface of the anode.
[0057] As mentioned above, trimethylphenylsilane is an additive that inhibits the dissolution of transition metals from the anode active material. However, when the content is too high, the battery cell cost increases due to the excessive amount, and the energy density per unit weight is also adversely affected, so the upper limit can be limited to 10.0wt%. The content of trimethylphenylsilane is preferably 0.5wt% to 5.0wt%, and more preferably 0.2wt% to 1.5wt%.
[0058] The electrolyte composition for lithium secondary batteries according to another aspect of the present invention may further contain VC (vinylene carbonate) as an additive in addition to trimethylphenylsilane.
[0059] Generally speaking, VC (vinyl carbonate) with ring strain and vinyl structure within the five-membered structure has a lower LUMO (Lowest Unoccupied Molecular Orbital) energy than the organic solvent used for the electrolyte, so the tendency of reduction decomposition is relatively high, thereby playing a role in forming a stable SEI film on the cathode surface.
[0060] When VC (vinylene carbonate) and trimethylphenylsilane are added simultaneously, VC prevents the occurrence of electrolyte decomposition reaction, and even if the electrolyte decomposition reaction occurs, the above-mentioned trimethylphenylsilane can effectively remove acidic substances (such as HF, etc.) as its decomposition product, thereby compensating for moisture vulnerability.
[0061] Specifically, when the additive includes VC, trimethylphenylsilane, and at least one of bis(trimethylsilyl)fumarate and bis(trimethylsilyl)thiophene-2,5-dicarboxylate, the content of the additive can be less than 10wt% (excluding the case of 0wt%), preferably 0.5wt% to 1.5wt%, and more preferably 1wt% to 2.5wt%.
[0062] The output characteristics and life characteristics of the present invention are described below by using examples and comparative examples of the electrolyte composition for lithium secondary batteries according to one embodiment of the present invention. However, the following examples are only used to help understand the present invention, and the scope of the present invention is not limited to the following examples.
[0063] In order to perform tests for evaluating output characteristics and life characteristics, electrolyte compositions for lithium secondary batteries of Examples and Comparative Examples having the following compositions were prepared. The contents of additives in the Comparative Examples and Examples are summarized in Table 1 below.
[0064] Example 1 to Example 6
[0065] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 2:3:5, and 0.5 M LiPF 6 and 0.5 M lithium bis(trimethylsilyl) fumarate (LiFSI), as an additive of the following [Table 1], respectively, were mixed in amounts of 0.1 wt%, 0.5 wt%, 1.0 wt%, 1.5 wt%, 2.0 wt% and 5.0 wt% relative to the total weight of the electrolyte to produce an electrolyte.
[0066] 95 wt% of carbon powder as a cathode active material, 3 wt% of Styrene-Butadiene Rubber (SBR) / CarboxyMethyl Cellulose (CMC) as a binder, and 2 wt% of Super-P as a conductive material were added to water to prepare a cathode mixture slurry. The slurry was applied to both sides of a copper foil, dried, and compressed to prepare a cathode.
[0067] As the anode active material, Li(Ni 0.6 Co 0.2 Mn 0.2 ) 2 , polyvinylidene fluoride (PVdF) as a binder and carbon as a conductive material are mixed in a weight ratio of 93:4:3 and dispersed in N-methyl-2-pyrrolidone to produce an anode slurry. The anode slurry is coated on an aluminum foil, dried and crimped to produce an anode. A ceramic-coated polyolefin separator is placed between the produced cathode and anode to form an electrode assembly, and then the electrolyte prepared above is injected to produce a pouch-type lithium secondary battery.
[0068] Examples 7 to 12
[0069] The same procedures as in Examples 1 to 6 were carried out except that bis(trimethylsilyl)thiophene-2,5-dicarboxylate was used as an additive.
[0070] Comparative Example 1
[0071] The same procedures as in Example 1 to Example 6 were carried out except that 2% by weight of VC (vinylene carbonate) was used as an additive.
[0072] [Table 1]
[0073]
[0074] (Unit: weight %)
[0075] The output and life characteristics of the lithium secondary batteries produced under the conditions of [Table 1] were evaluated, and the evaluation results are shown in the following [Table 2].
[0076] The capacity retention rate related to the life characteristics was calculated according to the following calculation formula.
[0077] Capacity retention rate at the 100th cycle = discharge capacity at the 100th cycle / discharge capacity at the first cycle
[0078] [Table 2]
[0079]
[0080] Figure 1 is a graph showing the battery life characteristic results during 100 cycles according to the disclosed Example 2, Example 8 and Comparative Example 1.
[0081] As shown in Table 2 and Figure 1 As shown, the lithium secondary batteries of Examples 2 and 8 maintained a high capacity of 95% or more relative to the initial capacity even after 100 cycles, compared with the lithium secondary battery according to Comparative Example 1.
[0082] The electrolyte composition according to Example 1 includes 0.1 wt % of bis(trimethylsilyl)fumarate, and the measured initial resistance characteristic of the battery of Example 1 is 99%.
[0083] According to the electrolyte composition of Example 2, which contains 0.5% by weight of bis(trimethylsilyl)fumarate, the initial resistance characteristic of the battery of Example 2 is 86%, the resistance characteristic after 100 cycles is 90%, and the resistance characteristic after high-temperature storage is 96%, showing a more improved output characteristic compared with the battery of Comparative Example 1. In addition, compared with the battery of Comparative Example 1, the battery of Example 2 shows a more improved cycle characteristic and electrolyte ion conductivity.
[0084] The electrolyte composition according to Example 3 contains 1.0 wt % of bis(trimethylsilyl)fumarate, and the initial resistance characteristic of the battery of Example 3 is 87%, the resistance characteristic after 100 cycles is 91%, and the resistance characteristic after high temperature storage is 98%, showing a more improved output characteristic compared with the battery of Comparative Example 1. In addition, compared with the battery of Comparative Example 1, the battery of Example 3 shows a more improved cycle characteristic and electrolyte ion conductivity.
[0085] According to the electrolyte composition of Example 4, which contains 1.5% by weight of bis(trimethylsilyl)fumarate, the initial resistance characteristic of the battery of Example 4 is 89%, and the resistance characteristic after 100 cycles is 94%, showing a more improved output characteristic compared with the battery of Comparative Example 1. In addition, compared with the battery of Comparative Example 1, the battery of Example 4 shows a more improved cycle characteristic.
[0086] The electrolyte composition according to Example 5 contains 2.0 wt % of bis(trimethylsilyl)fumarate, and the initial resistance characteristic of the battery of Example 5 is 92%, and the resistance characteristic after 100 cycles is 93%, showing a more improved output characteristic compared with the battery of Comparative Example 1. In addition, the battery of Example 5 shows a more improved cycle characteristic compared with the battery of Comparative Example 1.
[0087] The electrolyte composition according to Example 7 includes 0.1 wt % of bis(trimethylsilyl)thiophene-2,5-dicarboxylate, and the measured initial resistance characteristic of the battery of Example 7 is 99%.
[0088] According to the electrolyte composition of Example 8, 0.5 wt % of bis(trimethylsilyl)thiophene-2,5-dicarboxylate was included. The initial resistance characteristic of the battery of Example 8 was 91%, and the resistance characteristic after 100 cycles was 94%, showing a more improved output characteristic compared with the battery of Comparative Example 1. In addition, compared with the battery of Comparative Example 1, the battery of Example 8 showed a more improved cycle characteristic and electrolyte ion conductivity.
[0089] The electrolyte composition according to Example 9 includes 1.0 wt % of bis(trimethylsilyl)thiophene-2,5-dicarboxylate, and the initial resistance characteristic of the battery of Example 9 is 95%, and the resistance characteristic after 100 cycles is 95%, showing a more improved output characteristic compared with the battery of Comparative Example 1. In addition, the battery of Example 9 shows a more improved cycle characteristic compared with the battery of Comparative Example 1.
[0090] The electrolyte composition according to Example 10 contains 1.5 wt % of bis(trimethylsilyl)thiophene-2,5-dicarboxylate. The resistance characteristic of the battery of Example 10 after 100 cycles is 93%, which shows a more improved output characteristic than the battery of Comparative Example 1.
[0091] As a conclusion, it was confirmed that the use of bis(trimethylsilyl)fumarate or bis(trimethylsilyl)thiophene-2,5-dicarboxylate having lower resistance than conventional VC as the cathode coating additive has an effect of improving output characteristics.
[0092] Next, the output characteristics and life characteristics of the lithium secondary battery when VC (vinylene carbonate) is added simultaneously will be described.
[0093] Embodiment 13 to Example 14
[0094] The same procedures as in Example 1 to Example 6 were carried out except that either bis(trimethylsilyl)fumarate or bis(trimethylsilyl)thiophene-2,5-dicarboxylate was used together with VC as an additive for the electrolyte solution.
[0095] Embodiment 15 to Example 16
[0096] The same procedures as in Example 13 and Example 14 were carried out except that trimethylphenylsilane was further added as an additive to the electrolyte solution.
[0097] Comparative Example 2
[0098] The same procedure as in Comparative Example 1 was carried out except that the content of VC as an additive was set to 1% by weight.
[0099] The output characteristics and life characteristics of the lithium secondary batteries produced under the conditions of [Table 3] were evaluated, and the evaluation results are shown in the following [Table 4].
[0100] [Table 3]
[0101]
[0102] [Table 4]
[0103]
[0104] Figure 2 is a graph showing the battery life characteristics results during 100 cycles according to the disclosed Examples 13 to 16 and Comparative Example 2. Figure 3 is a graph showing the battery life characteristic results during 200 cycles according to the disclosed Example 15 and Comparative Example 2.
[0105] As shown in Table 2 and Figure 3 As shown, the lithium secondary battery of Example 15 also exhibits a high capacity of 94.5% or more relative to the initial capacity after 200 cycles, compared with the lithium secondary battery according to Comparative Example 2.
[0106] The resistance characteristic of the battery of Example 13 after 100 cycles was 92%, and the resistance characteristic after high-temperature storage was 96%, showing further improved output characteristics compared with the battery of Comparative Example 2.
[0107] The resistance characteristic of the battery of Example 14 after 100 cycles was 93%, and the resistance characteristic after high-temperature storage was 97%, showing further improved output characteristics compared with the battery of Comparative Example 2.
[0108] The resistance characteristic of the battery of Example 15 after 100 cycles was 89%, and the resistance characteristic after high-temperature storage was 93%, showing further improved output characteristics compared with the battery of Comparative Example 2. In addition, the battery of Example 15 showed further improved cycle characteristics compared with the battery of Comparative Example 2.
[0109] The resistance characteristic of the battery of Example 16 after 100 cycles was 91%, and the resistance characteristic after high-temperature storage was 94%, showing further improved output characteristics compared with the battery of Comparative Example 2. In addition, the battery of Example 16 showed further improved cycle characteristics compared with the battery of Comparative Example 2.
[0110] As a conclusion, it can be confirmed that when bis(trimethylsilyl)fumarate or bis(trimethylsilyl)thiophene-2,5-dicarboxylate is used together with VC, it has the effect of reducing the VC content and improving the resistance of the battery cell. In addition, it can be confirmed from Examples 15 and 16 that when trimethylphenylsilane is further added, it has the effect of improving the life characteristics.
[0111] Next, the life characteristics when VC (vinylene carbonate) and trimethylphenylsilane are added together will be described.
[0112] Example 17 to Example 30
[0113] The same procedures as in Examples 1 to 6 were followed except that at least one of bis(trimethylsilyl)fumarate and bis(trimethylsilyl)thiophene-2,5-dicarboxylate was mixed together with VC and trimethylphenylsilane as electrolyte additives.
[0114] The life characteristics of lithium secondary batteries produced by changing the contents of VC, bis(trimethylsilyl)fumarate, bis(trimethylsilyl)thiophene-2,5-dicarboxylate, and trimethylphenylsilane were evaluated, and the evaluation results are shown in the following [Table 5]. [Table 5]
[0115]
[0116] Figure 4 and Figure 5 is a graph showing the battery life characteristics results during 200 cycles according to the disclosed Examples 17 to 30 and Comparative Example 2.
[0117] As shown in Table 5 and Figure 4 As shown, the lithium secondary batteries of Examples 17 to 20 in which VC, bis(trimethylsilyl)fumarate and trimethylphenylsilane were mixed maintained a high capacity of 93.9% or more relative to the initial capacity even after 200 cycles, compared with the lithium secondary battery of Comparative Example 2 in which only VC was added.
[0118] As shown in Table 5 and Figure 4 As shown, compared with the lithium secondary battery according to Comparative Example 2, the lithium secondary batteries of Examples 21 to 24 in which VC, bis(trimethylsilyl)thiophene-2,5-dicarboxylate and trimethylphenylsilane were mixed maintained a high capacity of 93.4% or more relative to the initial capacity even after 200 cycles.
[0119] As shown in Table 5 and Figure 5 As shown, compared with the lithium secondary battery according to Comparative Example 2, the lithium secondary batteries of Examples 25 to 30, which are mixed with VC, bis(trimethylsilyl)fumarate, bis(trimethylsilyl)thiophene-2,5-dicarboxylate and trimethylphenylsilane, also maintain a high capacity of more than 94.1% relative to the initial capacity after 200 cycles.
[0120] However, as shown in Tables 1 and 2 above, it can be confirmed that in the case of Example 6 and Example 12 where the addition amount of bis(trimethylsilyl)fumarate or bis(trimethylsilyl)thiophene-2,5-dicarboxylate is 5wt%, the output characteristics and life characteristics are reduced. Therefore, considering the utility of the battery cell, two or more additives are not mixed. Therefore, it is suitable that the content of the additive is 0.5wt% to 2.5wt% relative to the total electrolyte composition, preferably 1wt% to 2.5wt%.
[0121] Referring to Examples 1 to 30, according to the disclosed embodiments, the additive can be obtained in the following manner: that is, bis(trimethylsilyl)fumarate and bis(trimethylsilyl)thiophene-2,5-dicarboxylate are used alone in various ways; or, bis(trimethylsilyl)fumarate and bis(trimethylsilyl)thiophene-2,5-dicarboxylate are used in combination with VC and trimethylphenylsilane in various ways.
[0122] In conclusion, the electrolyte composition according to the disclosed embodiment can reduce the VC content and improve the initial output characteristics and high-temperature output characteristics. Moreover, by compensating for moisture vulnerability, the life characteristics of the lithium secondary battery can also be improved. Therefore, the lithium secondary battery containing the electrolyte composition according to the disclosed embodiment can be applied to medium and large batteries for vehicles that require high output characteristics and long life.
[0123] The disclosed embodiments are described above with reference to the accompanying drawings. It should be understood by those skilled in the art that the present invention can be implemented in a manner different from the disclosed embodiments without changing the technical concept and essential features of the present invention. The disclosed embodiments are merely illustrative and should not be construed as limiting the present invention.
Claims
1. A lithium secondary battery, It is characterized in that Include: an anode comprising an anode active material; a cathode comprising a cathode active material; a separator located between the anode and the cathode; and Electrolytes, The electrolyte comprises an electrolyte composition, The electrolyte composition comprises a lithium salt, a solvent and an additive. The additive comprises at least one of bis(trimethylsilyl)fumarate and bis(trimethylsilyl)thiophene-2,5-dicarboxylate, The additive further comprises trimethylphenylsilane and vinylene carbonate, The content of at least one of bis(trimethylsilyl)fumarate and bis(trimethylsilyl)thiophene-2,5-dicarboxylate is 0.2 wt % to 3 wt % relative to the total electrolyte composition, The content of trimethylphenylsilane is 0.5 wt % to 5 wt % relative to the total electrolyte composition, and The total content of the additives is 0.5 wt % to 1.5 wt % relative to the entire electrolyte composition.
2. The lithium secondary battery according to claim 1, Features: The lithium salt is selected from LiPF 6 , LiBF 4 、LiClO 4 、LiCl、LiBr、LiI、LiB 10 Cl 10 、LiCF 3 SO 3 、LiCF 3 CO 2 、LiAsF 6 、LiSbF 6 、LiAlCl 4 , CH 3 SO 3 Li, CF 3 SO 3 Li, LiN(SO 2 C 2 F 5 ) 2 、Li(CF 3 SO 2 ) 2 N, LiC 4 F 9 SO 3 、LiB(C 6 H 5 ) 4 、Li(SO 2 F) 2 N(LiFSI) and (CF 3 SO 2 ) 2 One or more of NLi.
3. The lithium secondary battery according to claim 1, Features: The solvent is at least one selected from the group consisting of ethylene carbonate, diethyl carbonate, dimethyl carbonate, propylene carbonate, dipropyl carbonate, butylene carbonate, methyl propyl carbonate, ethyl propyl carbonate and ethyl methyl carbonate.
4. The lithium secondary battery according to claim 1, Features: The anode active material comprises an anode active material of a lithium nickel-manganese-cobalt three-component system, wherein the Ni content of the lithium nickel-manganese-cobalt three-component system is greater than 30 wt % and less than 100 wt %.
5. The lithium secondary battery according to claim 1, Features: The diaphragm comprises a ceramic coated diaphragm.
6. An electrolyte composition for a lithium secondary battery, It is characterized in that Contains lithium salts, solvents and additives, The additive comprises bis(trimethylsilyl)fumarate or bis(trimethylsilyl)thiophene-2,5-dicarboxylate, The additive further comprises trimethylphenylsilane and vinylene carbonate, The content of bis(trimethylsilyl)fumarate or bis(trimethylsilyl)thiophene-2,5-dicarboxylate is 0.2 wt % to 3 wt % relative to the total electrolyte composition. The content of trimethylphenylsilane is 0.5 wt % to 5 wt % relative to the total electrolyte composition, and The total content of the additives is 1 wt % to 2.5 wt % relative to the entire electrolyte composition.