Process for preparing a zeolitic material comprising a metal M and having an AEI framework type

Through hydrothermal synthesis technology, combining zeolite materials with skeleton type other than AEI and tetravalent element Y, an AEI skeleton type zeolite material containing metal M was successfully prepared, solving the additional source and post-treatment steps of metal M in the prior art. Problem, efficient material preparation is achieved.

CN110621622BActive Publication Date: 2024-11-19BASF MOBILE EMISSIONS CATALYSTS LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201880032118.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-05-15
Filing Date
2018-05-15
Publication Date
2024-11-19
Estimated Expiration
2038-05-15

AI Technical Summary

Technical Problem

Prior art In preparing an AEI skeleton type zeolite material containing metal M, additional metal M source and post-treatment steps are required, and it is difficult to effectively contain the tetravalent elements Y and the trivalent element X.

Method used

Hydrothermal synthesis is performed to obtain a zeolite material with an AEI skeleton type and a metal M containing a metal M, by combining a zeolite material with a skeleton type other than AEI and a trivalent element X and oxygen, The use and post-treatment steps of additional metal M are avoided.

Benefits of technology

Zeolite materials with AEI skeleton type and skeleton structures of tetravalent elements Y, trivalent elements X and oxygen are achieved without additional metal M source and post-treatment steps, improving the preparation efficiency and purity of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110621622B_ABST
    Figure CN110621622B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a zeolite material containing a metal M, having an AEI framework type and having a framework structure containing a tetravalent element Y, a trivalent element X and oxygen, the method comprising: (i) providing a zeolite material containing a metal M, having a framework type other than AEI and having a framework structure containing a trivalent element X and oxygen; (ii) preparing a synthesis mixture comprising the zeolite material provided in (i), water, a source of a tetravalent element Y and an AEI framework structure directing agent; (iii) subjecting the synthesis mixture prepared in (ii) to hydrothermal synthesis conditions, comprising heating the synthesis mixture to a temperature of 100-200° C. and maintaining the synthesis mixture at a temperature within the range under autogenous pressure to obtain a zeolite material having an AEI framework type; wherein Y is one or more of Si, Ge, Sn, Ti and Zr; wherein X is one or more of Al, B, Ga and In; wherein M is a transition metal of Groups 7-12 of the periodic table.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for preparing a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen. In addition, the present invention relates to a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen obtainable or obtained by said method, and further to the use of said zeolitic material as a catalytically active material.

[0002] Zeolitic materials having an AEI framework type are known to be effective as catalysts for treating combustion exhaust gases in industrial applications, such as for converting nitrogen oxides (NO x ) of the catalyst or catalyst component. Synthetic AEI zeolite materials are usually prepared by precipitating crystals of zeolite materials from a synthesis mixture, the synthesis mixture containing a source of elements constituting the zeolite framework, such as a source of silicon and a source of aluminum. In addition, the AEI zeolite material may additionally contain one or more metals M, which are usually incorporated into the zeolite material by a suitable post-treatment step. Therefore, the object of the present invention is to provide a novel and advantageous method for preparing an AEI zeolite material comprising metal M. According to the present invention, it is found that this purpose can be achieved by zeolite framework transformation, according to which the starting material of a suitable zeolite material having a framework type other than AEI and comprising metal M is appropriately reacted to obtain a zeolite material having an AEI framework type and comprising metal M. According to this method, in the process of synthesizing the AEI zeolite material, it is not necessary to use a source of additional metal M, nor is it necessary to carry out post-treatment and incorporate metal M.

[0003] Therefore, the present invention relates to a method for preparing a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, the method comprising:

[0004] (i) providing a zeolitic material comprising a metal M, having a framework type other than AEI and having a framework structure comprising a trivalent element X and oxygen;

[0005] (ii) preparing a synthesis mixture comprising the zeolite material provided in (i), water, a source of a tetravalent element Y, and an AEI framework directing agent;

[0006] (iii) subjecting the synthesis mixture prepared in (ii) to hydrothermal synthesis conditions comprising heating the synthesis mixture to a temperature in the range of 100-200° C. and maintaining the synthesis mixture at a temperature in the range under autogenous pressure to obtain a zeolitic material having an AEI framework type;

[0007] Wherein Y is one or more of Si, Ge, Sn, Ti, and Zr;

[0008] Wherein X is one or more of Al, B, Ga, and In;

[0009] wherein M is a transition metal of Groups 7 to 12 of the Periodic Table of Elements.

[0010] Typically, M is a transition metal of Groups 7 to 12 of the Periodic Table of Elements. Preferably, M is one or more of Fe, Co, Ni, Cu and Zn, more preferably one or more of Fe and Cu. More preferably, M is Cu.

[0011] There is no specific limitation on the amount of metal M contained in the zeolite material provided in (i). For example, the zeolite material provided in (i) may contain 0.01-10 wt. % or 0.02-8 wt. % or 0.05-6 wt. % calculated as element M and based on the total weight of the zeolite material. Preferably, the zeolite material provided in (i) contains 0.1-5 wt. %, preferably 0.2-4 wt. %, more preferably 0.5-3 wt. % M calculated as element M and based on the total weight of the zeolite material.

[0012] Preferably, the zeolitic material provided in (i) has a framework structure which additionally comprises a tetravalent element Y. Preferably, at least 95 wt. %, more preferably at least 98 wt. %, more preferably at least 99 wt. %, more preferably at least 99.5 wt. % of the zeolitic material provided in (i) consists of Y, X, O, M and H.

[0013] Typically Y is one or more of Si, Ge, Sn, Ti, Zr. Preferably, Y is Si. Typically X is one or more of Al, B, Ga. Preferably, X is Al. More preferably, X is Al and Y is Si. More preferably, Y is Si and X is Al, and the molar ratio of Si to Al is 3:1-50:1, preferably 5:1-30:1, more preferably 8:1-25:1.

[0014] Section 1(i) of the AEI Regional Committee of the United States, ABW, ACO, AEI, AEL, etc. AEN、AET、AFG、AFI、AFN、AFO、AFR、AFS、AFT、AFV、AFX、AFY、AHT、ANA、APC、AP D、AST、ASV、ATN、ATO、ATS、ATT、ATV、AVL、AWO、AWW、BCT、BEA、BEC、BIK、BOF、 BOG、BOZ、BPH、BRE、BSV、CAN、CAS、CDO、CFI、CGF、CGS、CHA、-CHI、-CLO、CON、C SV、CZP、DAC、DDR、DFO、DFT、DOH、DON、EAB、EDI、EEI、EMT、EON、EPI、ERI、ESV 、ETR、EUO、*-EWT、EZT、FAR、FAU、FER、FRA、GIS、GIU、GME、GON、GOO、HEU、IFO 、IFR、-IFU、IFW、IFY、IHW、IMF、IRN、IRR、-IRY、ISV、ITE、ITG、ITH、*-ITN、I TR、ITT、-ITV、ITW、IWR、IWS、IWV、IWW、JBW、JNT、JOZ、JRY、JSN、JSR、JST、JSW 、KFI、LAU、LEV、LIO、-LIT、LOS、LOV、LTA、LTF、LTJ、LTL、LTN、MAR、MAZ、MEI、 MEL、MEP、MER、MFI、MFS、MON、MOR、MOZ、*MRE、MSE、MSO、MTF、MTN、MTT、MTW、M VY、MWF、MWW、NAB、NAT、NES、NON、NPO、NPT、NSI、OBW、OFF、OKO、OSI、OSO、OWE 、-PAR、PAU、PCR、PHI、PON、POS、PSI、PUN、RHO、-RON、RRO、RSN、RTE、RTH、RUT、 RWR, RWY, SAF, SAO, SAS, SAT, SAV, SBE, SBN, SBS, SBT, SEW, SFE, SFF, SFG, SF H、SFN、SFO、SFS、*SFV、SFW、SGT、SIV、SOD、SOF、SOS、SSF、*-SSO、SSY、STF、S TI、*STO、STT、STW、-SVR、SVV、SZR、TER、THO、TOL、TON、TSC、TUN、UEI、UFI、U OS、UOV、UOZ、USI、UTL、UWY、VET、VFI、VNI、VSV、WEI、-WEN、YUG、ZON.Preferably, the zeolitic material having a framework type other than AEI provided in (i) is of CHA, FAU, LTA, MOR, MFI or BEA, more preferably CHA or FAU framework type.

[0015] Therefore, the present invention further preferably relates to a method for preparing a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, preferably the method of any one of embodiments 1 to 10, the method comprising:

[0016] (i) providing a zeolitic material comprising a metal M, having a framework type other than AEI and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen;

[0017] (ii) preparing a synthesis mixture comprising the zeolite material provided in (i), water, a source of a tetravalent element Y, and an AEI framework directing agent;

[0018] (iii) subjecting the synthesis mixture prepared in (ii) to hydrothermal synthesis conditions (including a hydrothermal synthesis temperature of 100-200° C.) to obtain a mixture containing a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen;

[0019] wherein Y is Si, X is Al, M is Cu, and wherein the zeolitic material provided in (i) has a CHA or FAU framework type.

[0020] Generally, the zeolitic material comprising metal M, having a framework type other than AEI and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen may be provided in (i) according to any conceivable method. Preferably, providing the zeolitic material according to (i) comprises:

[0021] (i.1) providing a zeolitic material that does not contain a metal M, has a framework type other than AEI, and has a framework structure comprising a trivalent element X and oxygen;

[0022] (i.2) loading the metal M on the zeolite material provided in (i.1), preferably comprising

[0023] (i.2.1) preparing a mixture comprising the zeolite material provided according to (i.1), a source of metal M, a solvent for the source of metal M and optionally an acid, preferably an organic acid, wherein the solvent preferably comprises water, the source of metal M preferably comprises a salt of metal M, and the acid preferably comprises acetic acid;

[0024] (i.2.2) heating the mixture prepared in (i.2.1) to a temperature of 30-90°C, preferably 40-80°C;

[0025] (i.2.3) preferably cooling, more preferably rapidly cooling the mixture obtained by (i.2.2);

[0026] (i.2.4) separating the zeolitic material comprising the metal M from the mixture obtained by (i.2.2) or (i.2.3), preferably (i.2.4), said separation preferably comprising washing the zeolitic material comprising the metal M;

[0027] (i.2.5) drying the zeolitic material comprising the metal M obtained by (i.2.4) preferably in a gas atmosphere, preferably at a gas atmosphere temperature of 90-200° C., more preferably 100-150° C., wherein the gas atmosphere preferably comprises oxygen;

[0028] (i.2.6) The zeolitic material comprising metal M obtained by (i.2.4) or (i.2.5), preferably (i.2.5), is preferably calcined in a gas atmosphere, preferably at a gas atmosphere temperature of 350-600°C, more preferably 400-550°C, wherein the gas atmosphere preferably contains oxygen.

[0029] As described above, the zeolite material provided in (i) preferably has a CHA or FAU framework type. Therefore, it is preferred that the zeolite material that does not contain metal M and has a framework type other than AEI has a CHA or FAU framework type. In the case where it has a CHA framework type, it is preferred that the zeolite material provided in (i.1) that does not contain metal M, has a CHA framework type and has a framework structure containing a trivalent element X and oxygen is a template-free (TF)-CHA, wherein for example TF-CHA can be prepared according to a template-free synthesis method as described in WO 2013 / 068976A, for example, on page 6, lines 4-20, wherein some specific examples are also provided on pages 40-47 thereof, which are incorporated herein by reference. TF-CHA is more preferably prepared according to a template-free synthesis method as described in WO 2013 / 068976A, in Example 2, on page 43, line 29 to page 44, line 8.

[0030] Preferably, the zeolitic material provided in (i) is a calcined zeolitic material, more preferably a zeolitic material which has been calcined in a gas atmosphere at a gas atmosphere temperature of 350-600° C., preferably 400-550° C. Preferably, the gas atmosphere comprises oxygen. More preferably, the gas atmosphere comprises air, rarefied air or nitrogen such as industrial nitrogen, more preferably air. More preferably, the gas atmosphere is air.

[0031] Generally, it is envisaged that the zeolitic material is provided in its ammonium form, its hydrogen form (H form) or any other suitable cationic form (eg its sodium form).Preferably, the zeolitic material provided in (i) is in its hydrogen (H) form.

[0032] With regard to step (ii) of the process of the present invention, the synthesis mixture prepared in (ii) which is subjected to (iii) preferably does not contain a zeolitic material having an AEI framework type. More preferably, the synthesis mixture prepared in (ii) which is subjected to (iii) does not contain a zeolitic seed material having an AEI framework type.

[0033] Generally, according to (ii), any suitable source of the tetravalent element Y may be used. In particular, if Y is Si, the source of Y preferably includes, more preferably, one or more of wet process silica, dry process silica and colloidal silica. Colloidal silica, preferably colloidal silica as an alkali and / or ammonia solution, more preferably colloidal silica as an ammonia solution, is commercially available, especially as or Commercially available. "Wet process" silica is commercially available, especially as Hi- Valron- or Commercially available. "Dry process" silica is commercially available, especially as Cab-O- or Commercially available. In particular, an ammonia solution of colloidal silica may be used according to the present invention. More preferably, if Y is Si, the source of the tetravalent element Y according to (ii) comprises, preferably, colloidal silica.

[0034] According to (ii), the AEI framework directing agent may be any agent that results in the preparation of a zeolitic material having an AEI framework type according to (iii). Preferably, the AEI framework directing agent comprises one or more quaternary Cationic compounds and / or one or more compounds containing quaternary ammonium cations.

[0035] Preferably, one or more The cationic compound includes one or more R 1 R 2 R 3 R 4 P + A compound wherein R 1 , R 2 , R 3 and R 4 R is independently selected from optionally substituted and / or optionally branched (C1-C6)alkyl, more preferably (C1-C5)alkyl, more preferably (C1-C4)alkyl, more preferably (C2-C3)alkyl, preferably represents optionally substituted methyl or ethyl, more preferably R 1 , R 2 , R 3 and R 4 represents an optionally substituted ethyl group, preferably an unsubstituted ethyl group;

[0036] Preferably, the one or more compounds containing quaternary ammonium cations include one or more N,N-dialkyldialkylpiperidinyl Cationic compounds, more preferably one or more N,N-(C1-C3)dialkyl-(C1-C3)dialkylpiperidinyl Cationic compounds, more preferably one or more N,N-(C1-C2)dialkyl-(C1-C2)dialkylpiperidinyl Cationic compounds, wherein more preferably, one or more compounds containing quaternary ammonium cations are selected from N, N-(C1-C2) dialkyl-2,6-(C1-C2) dialkylpiperidinyl Cation and N,N-(C1-C2)dialkyl-3,5-(C1-C2)dialkylpiperidine The cationic compound is more preferably selected from N,N-dimethyl-2,6-(C1-C2) dialkylpiperidin Cation and N,N-dimethyl-3,5-(C1-C2)dialkylpiperidin The cationic compound is more preferably selected from N, N-dimethyl-2,6-dimethylpiperidinium Cation and N,N-dimethyl-3,5-dimethylpiperidinium Cationic compounds.

[0037] Preferably, one or more quaternary The compound containing a quaternary ammonium cation and / or one or more compounds containing a quaternary ammonium cation are salts, preferably selected from halides, more preferably chlorides and / or bromides, more preferably chlorides; hydroxides; sulfates; nitrates; phosphates; acetates and mixtures of two or more thereof, more preferably selected from chlorides, hydroxides, sulfates and mixtures of two or more thereof, wherein more preferably, one or more compounds containing a quaternary ammonium cation are salts, preferably selected from halides, more preferably chlorides and / or bromides, more preferably chlorides; hydroxides; sulfates; nitrates; phosphates; acetates and mixtures of two or more thereof The cationic compound and / or the one or more compounds containing a quaternary ammonium cation are hydroxides and / or chlorides, more preferably hydroxides.

[0038] More preferably, the AEI framework structure directing agent includes, preferably N,N-dimethyl-3,5-dimethylpiperidine hydroxide.

[0039] Preferably, in the synthesis mixture prepared in (ii) which is subjected to (iii), the weight ratio of the zeolitic material relative to the source of the tetravalent element Y (calculated as YO2) is 1.0: 1 to 3.0: 1, more preferably 1.5: 1 to 2.5, more preferably 2.0: 1 to 2.2: 1. According to one conceivable embodiment of the present invention, the weight ratio of the zeolitic material relative to the source of the tetravalent element Y may be infinite, which means that in addition to the zeolitic material comprising Y, no other source of the tetravalent element is contained in the synthesis mixture in (ii).

[0040] Preferably, the weight ratio of zeolitic material to water in the synthesis mixture prepared in (ii) which is subjected to (iii) is 0.005:1-0.030:1, more preferably 0.010:1-0.025:1, more preferably 0.015:1-0.020:1.

[0041] Preferably, the weight ratio of zeolitic material to AEI framework directing agent in the synthesis mixture prepared in (ii) which is subjected to (iii) is 0.1:1-0.9:1, preferably 0.3:1-0.7:1, more preferably 0.4:1-0.5:1.

[0042] The pH of the synthesis mixture prepared in (ii) is not limited to any particular value. Preferably, the synthesis mixture prepared in (ii) which is subjected to (iii) additionally comprises an alkali source, more preferably a hydroxide source.

[0043] Preferably, the synthesis mixture prepared in (ii) which is subjected to (iii) additionally comprises a source of one or more alkali metals such as sodium, lithium, potassium and alkaline earth metals such as magnesium, calcium, strontium, barium, more preferably alkali metals, more preferably sodium.

[0044] More preferably, the alkalinity source is a source of one or more of an alkali metal and an alkaline earth metal, preferably an alkali metal base, more preferably an alkali metal hydroxide, more preferably sodium hydroxide.

[0045] The synthesis mixture prepared in (ii) which is subjected to (iii) is not limited to any particular weight ratio of the components contained in the mixture. Preferably, the synthesis mixture prepared in (ii) which is subjected to (iii) has a weight ratio of zeolitic material relative to the alkaline source of 0.1:1 to 1.0:1, preferably 0.2:1 to 0.8:1, more preferably 0.3:1 to 0.6:1.

[0046] Preferably, the synthesis mixture prepared in (ii) and subjected to (iii) contains no source of metal M other than the zeolitic material comprising the metal M. Preferably, at least 95 wt.%, preferably at least 98 wt.%, more preferably at least 99 wt.% of the synthesis mixture prepared in (ii) and subjected to (iii) consists of the zeolitic material provided in (i), water, a source of the tetravalent element Y, an AEI framework structure directing agent and preferably a source of base and a source of one or more of an alkali metal and an alkaline earth metal.

[0047] Step (iii) of the process of the present invention comprises subjecting the synthesis mixture prepared in (ii) to hydrothermal synthesis conditions.

[0048] Preferably, the hydrothermal synthesis is carried out under autogenous pressure, preferably in an autoclave. Preferably, the synthesis mixture prepared in (ii) is heated to a hydrothermal synthesis temperature in an autoclave at a heating rate of 0.5-4K / min, more preferably 1-3K / min. Preferably, the hydrothermal synthesis temperature to which the mixture is heated is 110-175°C, preferably 120-150°C. Preferably, the hydrothermal synthesis conditions also include stirring the synthesis mixture during at least a portion of the synthesis time. Preferably, the hydrothermal synthesis conditions also include a hydrothermal synthesis time of 2-120h, more preferably 20-100h, more preferably 40-80h. Therefore, preferably according to (iii), the mixture provided in (ii) is heated to a temperature of 110-175°C, preferably 120-150°C, and maintained at this temperature for a period of 2-120h. Therefore, it is further preferred that according to (iii), the mixture provided in (ii) is heated to a temperature of 110-175°C, preferably 120-150°C, and maintained at this temperature for a period of 20-120h. Therefore, it is further preferred that according to (iii), the mixture provided in (ii) is heated to a temperature of 110-175°C, preferably 120-150°C, and maintained at this temperature for a period of 40-80h.

[0049] The hydrothermal synthesis according to (iii) obtains a mixture containing a zeolitic material having an AEI framework type suspended in its mother liquor at the hydrothermal synthesis temperature. Since the hydrothermal synthesis is carried out under autogenous pressure, preferably (iii) further comprises decompressing the mixture. Before, during or after decompression, the method of the present invention preferably further comprises:

[0050] (iv) cooling the mixture obtained in (iii).

[0051] Although not particularly limited, the mixture is preferably cooled to a temperature of 10-50°C, more preferably 20-35°C.

[0052] As mentioned above, since the mixture obtained from (iii) comprises a zeolitic material having an AEI framework type suspended in its mother liquor, it is further preferred that the process of the present invention further comprises:

[0053] (v) separating the zeolitic material comprising the metal M from the mixture obtained from (iii) or (iv), preferably from the mixture obtained from (iv).

[0054] There is no particular restriction on how the zeolitic material comprising the metal M can be separated. Preferably, the separation step (v) comprises

[0055] (v.1) subjecting the mixture obtained from (iii) or (iv) to a solid-liquid separation method, preferably comprising a filtration method or a spray method;

[0056] (v.2) preferably washing the zeolitic material comprising the metal M obtained in (v.1);

[0057] (v.3) Drying the zeolitic material comprising the metal M obtained by (v.1) or (v.2), preferably (v.2).

[0058] With regard to (v.1), the spraying method may comprise spray drying or spray granulation. If (v.2) is performed, the zeolitic material is preferably washed with water as a washing agent, preferably until the washing water has a conductivity of at most 500 microSiemens, preferably at most 200 microSiemens. With regard to (v.3), the zeolitic material is preferably dried in a gas atmosphere having a temperature of 80-175°C, more preferably 100-150°C. Preferably, the gas atmosphere comprises oxygen, more preferably comprises, more preferably is air, rarefied air or synthetic air.

[0059] Preferably, the method of the present invention further comprises:

[0060] (vi) calcining the zeolitic material comprising the metal M obtained in (v).

[0061] If step (vi) is performed, the zeolitic material comprising metal M is preferably calcined in a gas atmosphere having a temperature of 400-600° C., more preferably 450-550° C. Preferably, the gas atmosphere comprises oxygen, more preferably comprises, more preferably is air, rarefied air or synthetic air.

[0062] Therefore, the present invention further preferably relates to a method for preparing a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, the method comprising:

[0063] (i) providing a zeolitic material comprising a metal M, having a framework type other than AEI and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen;

[0064] (ii) preparing a synthesis mixture comprising the zeolite material provided in (i), water, a source of a tetravalent element Y, and an AEI framework directing agent;

[0065] (iii) subjecting the synthesis mixture prepared in (ii) to hydrothermal synthesis conditions (including a hydrothermal synthesis temperature of 100-200° C.) to obtain a mixture containing a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen;

[0066] (iv) cooling the mixture obtained from (iii), preferably to a temperature of 10-50°C, more preferably 20-35°C;

[0067] (v) separating the zeolitic material comprising the metal M from the mixture obtained in (iv), comprising

[0068] (v.1) subjecting the mixture obtained from (iv) to a solid-liquid separation method, preferably comprising a filtration method or a spray method;

[0069] (v.2) washing the zeolitic material containing the metal M obtained in (v.1);

[0070] (v.3) drying the zeolite material containing the metal M obtained in (v.2) in a gas atmosphere having a temperature of 80-175° C.;

[0071] (vi) calcining the zeolitic material containing the metal M obtained in (v) in a gas atmosphere having a temperature of 400-600°C.

[0072] Usually, according to the inventive method, the above-mentioned conversion process of producing the zeolitic material comprising metal M and having AEI framework type can be a substantially complete conversion, and the resulting material is substantially composed of the zeolitic material comprising metal M and having AEI framework type. However, the conversion may also be partially incomplete, and in the resulting material, not only the zeolitic material comprising metal M and having AEI framework type is included, but also one or more other materials are included, preferably one or more zeolitic materials comprising metal M and having a framework type other than AEI, preferably FAU, LTA, MOR, MFI or BEA framework type, more preferably zeolitic materials with CHA or FAU framework type. Preferably, for the corresponding composition obtained, the composition comprising the zeolitic material comprising metal M and having AEI framework type and having a framework structure comprising tetravalent element Y, trivalent element X and oxygen, greater than 50% by weight, more preferably at least 60% by weight, more preferably at least 70% by weight, is composed of the zeolitic material comprising metal M and having AEI framework type and having a framework structure comprising tetravalent element Y, trivalent element X and oxygen. More preferably, at least 80% by weight, more preferably 80-100% by weight of the composition comprising a zeolite material comprising a metal M and having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen is composed of a zeolite material comprising a metal M and having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen. More preferably, at least 90% by weight, more preferably at least 95% by weight, more preferably at least 99% by weight of the composition is composed of a zeolite material comprising a metal M and having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen and a zeolite material comprising a metal M and having a CHA framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen. In a second preferred embodiment of the present invention, for example, relating to a method for preparing a composition, it is considered that the partial incomplete conversion of the composition comprising a zeolite material comprising a metal M and an AEI framework type is caused. For completeness, it is also mentioned that for these embodiments, in the case where the conversion is complete, the composition is understood to be composed of a zeolite material having an AEI framework type. In any case, even if the conversion is partially incomplete, the present invention still relates, for example, to a process for a zeolitic material comprising a metal M and having an AEI framework type, since this zeolitic material is compulsorily contained in the composition.

[0073] Depending on the intended use of the zeolitic material, the material can be used as is, preferably the material obtained by (vi). In addition, it is conceivable that the zeolitic material is subjected to one or more other post-processing steps. For example, the zeolitic material most preferably obtained in powder form can be suitably processed into a molded product or a molded body by any suitable method (including but not limited to extrusion, tabletting, spraying, etc.). Preferably, the molded body can have a rectangular, triangular, hexagonal, square, elliptical or circular cross-section, and / or preferably in the form of a star, sheet, sphere, cylinder, line or hollow cylinder. When preparing the molded body, one or more adhesives can be used, which can be selected according to the intended use of the molded body. Possible adhesive materials include but are not limited to a mixed oxide of two or more of graphite, silicon dioxide, titanium dioxide, zirconium oxide, aluminum oxide and silicon, titanium and zirconium. The weight ratio of the zeolitic material relative to the adhesive is generally not subject to any specific restrictions, and can be, for example, 10: 1-1: 10. According to another example of using the zeolite material, for example as a catalyst or catalyst component for treating an exhaust stream such as an engine exhaust stream, the zeolite material can be used as a component of a washcoat applied to a suitable substrate such as a wall flow filter or the like.

[0074] The present invention further relates to a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, obtainable or obtained or preparable or prepared by the above-described process.

[0075] Preferably, the zeolite material comprises 0.1-5 wt%, more preferably 0.2-4 wt%, more preferably 0.5-3 wt% of metal M, calculated as element M and based on the total weight of the zeolite material. M is a transition metal of Groups 7-12 of the Periodic Table, preferably M is Fe or Cu, more preferably Cu. Preferably, the zeolite material comprises metal M having a total amount of acid sites of 1.0-2.0 mmol / g, wherein the total amount of acid sites is defined as the total molar amount of ammonia desorbed per mass of the zeolite material as measured by the temperature programmed desorption of ammonia (NH3-TPD) as described in Reference Example 1.6 herein; wherein the zeolite material has an amount of medium acid sites of 0.1-0.8 mmol / g, wherein the amount of medium acid sites is defined as the amount of ammonia desorbed per mass of the zeolite material as measured by the temperature programmed desorption of ammonia (NH3-TPD) as described in Reference Example 1.6 herein in the temperature range of 250-500°C.

[0076] The zeolite material comprising metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen can be used for any conceivable purpose, including but not limited to absorbent, adsorbent, molecular sieve, catalyst, catalyst carrier or intermediate for preparing one or more thereof. Preferably, the zeolite material comprising metal M of the present invention is used as a catalytically active material, a catalyst or a catalyst component, more preferably as a catalytically active material, more preferably for selective catalytic reduction of nitrogen oxides in an exhaust gas stream (preferably an exhaust gas stream from a diesel engine). More preferably, it is used to convert a C1 compound into one or more olefins, preferably to convert methanol into one or more olefins or to convert a synthesis gas comprising carbon monoxide and hydrogen into one or more olefins.

[0077] Furthermore, the present invention relates to a method for the selective catalytic reduction of nitrogen oxides in an exhaust gas stream, preferably an exhaust gas stream from a diesel engine, the method comprising contacting a zeolite material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, obtainable or obtained or preparable or prepared by the method according to the invention with the exhaust gas stream, or a method for the catalytic conversion of a C1 compound into one or more olefins, preferably the conversion of methanol into one or more olefins or the conversion of a synthesis gas comprising carbon monoxide and hydrogen into one or more olefins, the method comprising contacting a zeolite material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, obtainable or obtained or preparable or prepared by the method according to the invention with the C1 compound.

[0078] The present invention is further illustrated by the following group of embodiments and the combinations of embodiments resulting from the indicated dependencies and back references. It should be particularly noted that in the case of referring to a range of embodiments, for example in the context of a term such as "a method according to any one of embodiments 1-4", it is intended that each embodiment within the range is explicitly disclosed to the skilled person, i.e. the wording of the term should be understood by the skilled person as being synonymous with "a method according to any one of embodiments 1, 2, 3 and 4".

[0079] 1. A method for preparing a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, the method comprising:

[0080] (i) providing a zeolitic material comprising a metal M, having a framework type other than AEI and having a framework structure comprising a trivalent element X and oxygen;

[0081] (ii) preparing a synthesis mixture comprising the zeolite material provided in (i), water, a source of a tetravalent element Y, and an AEI framework directing agent;

[0082] (iii) subjecting the synthesis mixture prepared in (ii) to hydrothermal synthesis conditions comprising heating the synthesis mixture to a temperature in the range of 100-200° C. and maintaining the synthesis mixture at a temperature in the range under autogenous pressure to obtain a zeolitic material having an AEI framework type;

[0083] Wherein Y is one or more of Si, Ge, Sn, Ti, and Zr;

[0084] Wherein X is one or more of Al, B, Ga, and In;

[0085] wherein M is a transition metal of Groups 7 to 12 of the Periodic Table of Elements.

[0086] 2. The method of embodiment 1, wherein M is one or more of Fe, Co, Ni, Cu and Zn, preferably one or more of Fe and Cu.

[0087] 3. The method of embodiment 1, wherein M is Cu.

[0088] 4. The process according to any of embodiments 1 to 3, wherein the zeolitic material provided in (i) comprises 0.1-5 wt.-%, preferably 0.2-4 wt.-%, more preferably 0.5-3 wt.-% M, calculated as element M and based on the total weight of the zeolitic material.

[0089] 5. The process according to any one of embodiments 1 to 4, wherein the zeolitic material provided in (i) has a framework structure which additionally comprises a tetravalent element Y.

[0090] 6. The process according to any one of embodiments 1 to 5, wherein at least 95% by weight, preferably at least 98% by weight, more preferably at least 99% by weight, more preferably at least 99.5% by weight of the zeolitic material provided in (i) consists of Y, X, O, M and H.

[0091] 7. The method of any one of embodiments 1 to 6, wherein X is Al.

[0092] 8. The method of any one of embodiments 1-7, wherein Y is Si.

[0093] 9. The process of any one of embodiments 1 to 8, wherein in the zeolitic material provided in (i), Y is Si, X is Al, and wherein the molar ratio Si:Al of Si calculated as elemental Si to Al calculated as elemental Al is 3:1-50:1, preferably 5:1-30:1, more preferably 8:1-25:1.

[0094] 10. The process according to any of embodiments 1 to 9, wherein the zeolitic material provided in (i) has a CHA, FAU, LTA, MOR, MFI or BEA, preferably a CHA or FAU framework type.

[0095] 11. A method for preparing a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, preferably the method of any one of embodiments 1 to 10, the method comprising:

[0096] (i) providing a zeolitic material comprising a metal M, having a framework type other than AEI and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen;

[0097] (ii) preparing a synthesis mixture comprising the zeolite material provided in (i), water, a source of a tetravalent element Y, and an AEI framework directing agent;

[0098] (iii) subjecting the synthesis mixture prepared in (ii) to hydrothermal synthesis conditions (including a hydrothermal synthesis temperature of 100-200° C.) to obtain a mixture comprising a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen;

[0099] wherein Y is Si, X is Al, M is Cu, and wherein the zeolitic material provided in (i) has a CHA or FAU framework type.

[0100] 12. The method of any one of embodiments 1-1, wherein providing a zeolite material according to (i) comprises:

[0101] (i.1) providing a zeolitic material that does not contain a metal M, has a framework type other than AEI, and has a framework structure comprising a trivalent element X and oxygen;

[0102] (i.2) loading the metal M on the zeolite material provided in (i.1), preferably comprising

[0103] (i.2.1) preparing a mixture comprising the zeolite material provided according to (i.1), a source of metal M, a solvent for the source of metal M and optionally an acid, preferably an organic acid, wherein the solvent preferably comprises water, the source of metal M preferably comprises a salt of metal M, and the acid preferably comprises acetic acid;

[0104] (i.2.2) heating the mixture prepared in (i.2.1) to a temperature of 30-90°C, preferably 40-80°C;

[0105] (i.2.3) preferably cooling, more preferably rapidly cooling the mixture obtained by (i.2.2);

[0106] (i.2.4) separating the zeolitic material comprising the metal M from the mixture obtained by (i.2.2) or (i.2.3), preferably (i.2.4), said separation preferably comprising washing the zeolitic material comprising the metal M;

[0107] (i.2.5) drying the zeolitic material comprising the metal M obtained by (i.2.4) preferably in a gas atmosphere, preferably at a gas atmosphere temperature of 90-200° C., more preferably 100-150° C., wherein the gas atmosphere preferably comprises oxygen;

[0108] (i.2.6) The zeolitic material comprising metal M obtained by (i.2.4) or (i.2.5), preferably (i.2.5), is preferably calcined in a gas atmosphere, preferably at a gas atmosphere temperature of 350-600°C, more preferably 400-550°C, wherein the gas atmosphere preferably contains oxygen.

[0109] 13. The method of any one of embodiments 1 to 12, wherein the zeolitic material provided in (i) is a calcined zeolitic material, preferably a zeolitic material calcined in a gas atmosphere at a gas atmosphere temperature of 350-600° C., preferably 400-550° C., wherein the gas atmosphere preferably comprises oxygen.

[0110] 14. The process according to any of embodiments 1 to 13, wherein the zeolitic material provided in (i) is in its H form.

[0111] 15. The process according to any of embodiments 1 to 14, wherein the synthesis mixture prepared in (ii) which is subjected to (iii) does not contain zeolitic material having an AEI framework type.

[0112] 16. The process according to any of embodiments 1 to 15, wherein the synthesis mixture prepared in (ii) which is subjected to (iii) does not contain zeolite seed material having an AEI framework type.

[0113] 17. The method of any one of embodiments 1 to 16, wherein Y is Si, and the source of the tetravalent element Y according to (ii) comprises one or more of wet-process silica, dry-process silica, and colloidal silica.

[0114] 18. The method of any one of embodiments 1 to 17, wherein the source of the tetravalent element according to (ii) comprises, preferably is, colloidal silica.

[0115] 19. The method of any one of embodiments 1-18, wherein the AEI framework structuring agent comprises one or more quaternary Cationic compounds and / or one or more compounds containing quaternary ammonium cations;

[0116] One or more of which contain The cationic compound includes one or more compounds containing R1R2R3R4P+, wherein R 1 , R 2 , R 3 and R4 represents, independently of one another, an optionally substituted and / or optionally branched (C1-C6)alkyl group, preferably a (C1-C5)alkyl group, more preferably a (C1-C4)alkyl group, more preferably a (C2-C3)alkyl group, even more preferably an optionally substituted methyl or ethyl group, wherein even more preferably R 1 , R 2 , R 3 and R 4 represents an optionally substituted ethyl group, preferably an unsubstituted ethyl group;

[0117] The one or more compounds containing quaternary ammonium cations include one or more N,N-dialkyl-dialkylpiperidinyl Cationic compounds, preferably one or more N,N-(C1-C3)dialkyl-(C1-C3)dialkylpiperidinyl Cationic compounds, more preferably one or more N,N-(C1-C2)dialkyl-(C1-C2)dialkylpiperidinyl The compound containing quaternary ammonium cations, wherein more preferably one or more compounds containing quaternary ammonium cations are selected from N, N-(C1-C2) dialkyl-2,6-(C1-C2) dialkylpiperidin Cation and N,N-(C1-C2)dialkyl-3,5-(C1-C2)dialkylpiperidine Cationic compounds, more preferably N,N-dimethyl-2,6-(C1-C2) dialkylpiperidin Cation and N,N-dimethyl-3,5-(C1-C2)dialkylpiperidin Cationic compounds, more preferably N,N-dimethyl-2,6-dimethylpiperidinium Cation and N,N-dimethyl-3,5-dimethylpiperidinium Cationic compounds;

[0118] One or more of the following The compound containing the quaternary ammonium cation and / or the one or more compounds containing the quaternary ammonium cation are salts, preferably selected from halides, preferably chlorides and / or bromides, more preferably chlorides; hydroxides; sulfates; nitrates; phosphates; acetates; and mixtures of two or more thereof, more preferably selected from chlorides, hydroxides, sulfates and mixtures of two or more thereof, wherein one or more compounds containing the quaternary ammonium cation are more preferably selected from The cationic compound and / or the one or more compounds containing a quaternary ammonium cation are hydroxides and / or chlorides, even more preferably hydroxides.

[0119] 20. The method of any one of embodiments 1-19, wherein the AEI framework structure directing agent comprises, preferably N,N-dimethyl-3,5-dimethylpiperidine hydroxide.

[0120] 21. The process of any one of embodiments 1 to 20, wherein in the synthesis mixture prepared in (ii) which is subjected to (iii), the weight ratio of zeolitic material to the source of tetravalent element Y expressed as YO2 is 1.0:1-3.0:1, preferably 1.5:1-2.5, more preferably 2.0:1-2.2:1.

[0121] 22. The process according to any one of embodiments 1 to 21, wherein the weight ratio of zeolitic material to water in the synthesis mixture prepared in (ii) which is subjected to (iii) is 0.005:1-0.030:1, preferably 0.010:1-0.025:1, more preferably 0.015:1-0.020:1.

[0122] 23. The method of any one of embodiments 1-22, wherein in the synthesis mixture prepared in (ii) which is subjected to (iii), the weight ratio of zeolite material to AEI framework structure directing agent is 0.1:1-3:1, preferably 0.2:1-2:1, more preferably 0.3:1-0.7:1, more preferably 0.4:1-0.5:1.

[0123] 24. The process according to any of embodiments 1 to 23, wherein the synthesis mixture prepared in (ii) which is subjected to (iii) additionally comprises a base source, preferably a hydroxide source.

[0124] 25. The process according to any of embodiments 1 to 24, wherein the synthesis mixture prepared in (ii) which is subjected to (iii) additionally comprises a source of one or more of alkali metals and alkaline earth metals, preferably alkali metals, more preferably sodium.

[0125] 26. The process of embodiment 24 or 25, wherein the base source is a source of one or more of an alkali metal and an alkaline earth metal, preferably an alkali metal base, more preferably an alkali metal hydroxide, more preferably sodium hydroxide.

[0126] 27. The process according to any one of embodiments 24 to 26, wherein the weight ratio of zeolitic material to alkalinity source in the synthesis mixture prepared in (ii) which is subjected to (iii) is 0.1:1-1.0:1, preferably 0.2:1-0.8:1, more preferably 0.3:1-0.6:1.

[0127] 28. The process according to any of embodiments 1 to 27, wherein the synthesis mixture prepared in (ii) and subjected to (iii) contains no source of the metal M other than the zeolitic material comprising the metal M.

[0128] 29. The method of any one of embodiments 1-28, wherein at least 95% by weight, preferably at least 98% by weight, and more preferably at least 99% by weight of the synthesis mixture prepared in (ii) and subjected to (iii) consists of the zeolitic material provided in (i), water, a source of the tetravalent element Y, an AEI framework structure directing agent, and preferably a source of alkali and a source of one or more of alkali metals and alkaline earth metals.

[0129] 30. The process according to any of embodiments 1 to 29, wherein the hydrothermal synthesis is carried out under autogenous pressure, preferably in an autoclave.

[0130] 31. The process according to any of embodiments 1 to 30, wherein the synthesis mixture prepared in (ii) is heated to the hydrothermal synthesis temperature in an autoclave at a heating rate of 0.5 to 4 K / min, preferably 1 to 3 K / min.

[0131] 32. The method according to any one of embodiments 1 to 31, wherein the hydrothermal synthesis temperature is 110-175°C, preferably 120-150°C.

[0132] 33. The method of any one of embodiments 1 to 32, wherein the hydrothermal synthesis conditions comprise stirring the synthesis mixture.

[0133] 34. The method of any one of embodiments 1 to 33, wherein the hydrothermal synthesis conditions include a hydrothermal synthesis time of 2 to 120 hours, preferably 20 to 100 hours, more preferably 40 to 80 hours.

[0134] 35. The method of any one of embodiments 1-34, further comprising

[0135] (iv) cooling the mixture obtained from (iii), preferably to a temperature of 10-50°C, more preferably 20-35°C.

[0136] 36. The method of any one of embodiments 1-34, further comprising

[0137] (v) separating the zeolitic material comprising the metal M from the mixture obtained from (iii) or (iv).

[0138] 37. The method of embodiment 36, wherein (v) comprises

[0139] (v.1) subjecting the mixture obtained from (iii) or (iv) to a solid-liquid separation method, preferably comprising a filtration method or a spray method;

[0140] (v.2) preferably washing the zeolitic material comprising the metal M obtained in (v.1);

[0141] (v.3) Drying the zeolitic material comprising the metal M obtained by (v.1) or (v.2), preferably (v.2).

[0142] 38. The process according to embodiment 37, wherein according to (v.2), the zeolitic material comprising the metal M is washed with water, preferably until the wash water has a conductivity of at most 500 microSiemens, preferably at most 200 microSiemens.

[0143] 39. The process of embodiment 37 or 38, wherein according to (v.3), the zeolitic material comprising the metal M is dried in a gas atmosphere having a temperature of 80-175°C, preferably 100-150°C.

[0144] 40. The method according to embodiment 39, wherein the gas atmosphere comprises oxygen, preferably air, rarefied air or synthetic air.

[0145] 41. The method according to any one of embodiments 36-40, further comprising

[0146] (vi) calcining the zeolitic material comprising the metal M obtained in (v).

[0147] 42. The process of embodiment 41, wherein according to (vi), the zeolitic material comprising the metal M is calcined in a gas atmosphere having a temperature of 400-600°C, preferably 450-550°C.

[0148] 43. The method according to embodiment 42, wherein the gas atmosphere comprises oxygen, preferably air, rarefied air or synthetic air.

[0149] 44. A method for preparing a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, preferably the method of any one of embodiments 1-10, the method comprising:

[0150] (i) providing a zeolitic material comprising a metal M, having a framework type other than AEI and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen;

[0151] (ii) preparing a synthesis mixture comprising the zeolite material provided in (i), water, a source of a tetravalent element Y, and an AEI framework directing agent;

[0152] (iii) subjecting the synthesis mixture prepared in (ii) to hydrothermal synthesis conditions (including a hydrothermal synthesis temperature of 100-200° C.) to obtain a mixture comprising a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen;

[0153] (iv) cooling the mixture obtained from (iii), preferably to a temperature of 10-50°C, more preferably 20-35°C;

[0154] (v) separating the zeolitic material comprising the metal M from the mixture obtained in (iv), comprising

[0155] (v.1) subjecting the mixture obtained from (iv) to a solid-liquid separation method, preferably comprising a filtration method or a spray method;

[0156] (v.2) washing the zeolitic material containing the metal M obtained in (v.1);

[0157] (v.3) drying the zeolite material containing the metal M obtained in (v.2) in a gas atmosphere having a temperature of 80-175° C.;

[0158] (vi) calcining the zeolitic material containing the metal M obtained in (v) in a gas atmosphere having a temperature of 400-600°C.

[0159] 45. The process of embodiment 44, wherein Y is Si, X is Al, M is Cu, and the zeolitic material provided in (i) has a CHA or FAU framework type.

[0160] 46. ​​A zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, obtainable or obtained or preparable or prepared by the method of any one of embodiments 1-45.

[0161] 47. The zeolitic material comprising metal M according to embodiment 46, comprising 0.1-5 wt.-%, preferably 0.2-4 wt.-%, more preferably 0.5-3 wt.-% M, calculated as element M and based on the total weight of the zeolitic material.

[0162] 48. The zeolitic material of embodiment 47, wherein M is Cu.

[0163] 49. The zeolite material of any one of embodiments 46-48, having a total acid site amount of 1.0-2.0 mmol / g, wherein the total acid site amount is defined as the total molar amount of ammonia desorbed per mass of zeolite material measured according to the temperature-programmed desorption of ammonia (NH3-TPD) as described in Reference Example 1.6 herein; wherein the zeolite material has an intermediate acid site amount of 0.1-0.8 mmol / g, wherein the intermediate acid site amount is defined as the amount of ammonia desorbed per mass of zeolite material measured according to the temperature-programmed desorption of ammonia (NH3-TPD) as described in Reference Example 1.6 herein within a temperature range of 250-500°C.

[0164] 50. Use of the zeolitic material according to any of embodiments 46 to 49 as catalytically active material, catalyst or catalyst component.

[0165] 51. The use according to embodiment 50 for the selective catalytic reduction of nitrogen oxides in an exhaust gas stream, preferably an exhaust gas stream from a diesel engine.

[0166] 52. The use according to embodiment 50 for converting a C1 compound into one or more olefins, preferably converting methanol into one or more olefins or converting a synthesis gas comprising carbon monoxide and hydrogen into one or more olefins.

[0167] 53. A method for the selective catalytic reduction of nitrogen oxides in an exhaust gas stream, preferably an exhaust gas stream from a diesel engine, the method comprising contacting a zeolite material according to any one of embodiments 46-49 with the exhaust gas stream.

[0168] 54. A method for selective catalytic reduction of nitrogen oxides in an exhaust gas stream, preferably an exhaust gas stream from a diesel engine, the method comprising preparing a zeolite material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen by a method according to any one of embodiments 1-45, and contacting the exhaust gas stream with a catalyst comprising the zeolite material.

[0169] 55. A method for catalytically converting a C1 compound into one or more olefins, preferably converting methanol into one or more olefins or converting synthesis gas comprising carbon monoxide and hydrogen into one or more olefins, the method comprising contacting a zeolite material according to any one of embodiments 46-49 with the C1 compound.

[0170] 56. A method for catalytically converting a C1 compound into one or more olefins, preferably converting methanol into one or more olefins or converting synthesis gas comprising carbon monoxide and hydrogen into one or more olefins, the method comprising a zeolite material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, prepared by a method according to any one of embodiments 1-45, and contacting the C1 compound with a catalyst comprising the zeolite material.

[0171] 57. A catalyst, preferably for the selective catalytic reduction of nitrogen oxides in an exhaust gas stream, preferably an exhaust gas stream from a diesel engine, or for the catalytic conversion of a C1 compound into one or more olefins, preferably for the conversion of methanol into one or more olefins or for the conversion of a synthesis gas comprising carbon monoxide and hydrogen into one or more olefins, the catalyst comprising the zeolite material of any one of embodiments 58-60.

[0172] The present invention is further illustrated by the following group of embodiments and the combinations of embodiments resulting from the indicated dependencies and back references. It should be particularly noted that in the case of referring to a range of embodiments, for example in the context of a term such as "a method according to any one of embodiments 1-4", it is intended that each embodiment within the range is explicitly disclosed to the skilled person, i.e. the wording of the term should be understood by the skilled person as being synonymous with "a method according to any one of embodiments 1, 2, 3 and 4".

[0173] 1. A method for preparing a composition containing a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, the method comprising:

[0174] (i) providing a zeolitic material comprising a metal M, having a framework type other than AEI and having a framework structure comprising a trivalent element X and oxygen;

[0175] (ii) preparing a synthesis mixture comprising the zeolite material provided in (i), water, a source of a tetravalent element Y, and an AEI framework directing agent;

[0176] (iii) subjecting the synthesis mixture prepared in (ii) to hydrothermal synthesis conditions comprising heating the synthesis mixture to a temperature in the range of 100-200° C. and maintaining the synthesis mixture at a temperature in the range under autogenous pressure to obtain a mixture comprising a zeolitic material having an AEI framework type;

[0177] Wherein Y is one or more of Si, Ge, Sn, Ti, and Zr;

[0178] Wherein X is one or more of Al, B, Ga, and In;

[0179] wherein M is a transition metal of Groups 7 to 12 of the Periodic Table of Elements.

[0180] 2. The method of embodiment 1, wherein M is one or more of Fe, Co, Ni, Cu and Zn, preferably one or more of Fe and Cu.

[0181] 3. The method of embodiment 1, wherein M is Cu.

[0182] 4. The process according to any of embodiments 1 to 3, wherein the zeolitic material provided in (i) comprises 0.1-5 wt.-%, preferably 0.2-4 wt.-%, more preferably 0.5-3 wt.-% M, calculated as element M and based on the total weight of the zeolitic material.

[0183] 5. The process according to any one of embodiments 1 to 4, wherein the zeolitic material provided in (i) has a framework structure which additionally comprises a tetravalent element Y.

[0184] 6. The process according to any one of embodiments 1 to 5, wherein at least 95% by weight, preferably at least 98% by weight, more preferably at least 99% by weight, more preferably at least 99.5% by weight of the zeolitic material provided in (i) consists of Y, X, O, M and H.

[0185] 7. The method of any one of embodiments 1 to 6, wherein X is Al.

[0186] 8. The method of any one of embodiments 1-7, wherein Y is Si.

[0187] 9. The process of any one of embodiments 1 to 8, wherein in the zeolitic material provided in (i), Y is Si, X is Al, and wherein the molar ratio Si:Al of Si calculated as elemental Si to Al calculated as elemental Al is 3:1-50:1, preferably 5:1-30:1, more preferably 8:1-25:1.

[0188] 10. The process according to any of embodiments 1 to 9, wherein the zeolitic material provided in (i) has a CHA, FAU, LTA, MOR, MFI or BEA, preferably a CHA or FAU framework type.

[0189] 11. A method for preparing a composition containing a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, preferably the method of any one of embodiments 1 to 10, the method comprising:

[0190] (i) providing a zeolitic material comprising a metal M, having a framework type other than AEI and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen;

[0191] (ii) preparing a synthesis mixture comprising the zeolite material provided in (i), water, a source of a tetravalent element Y, and an AEI framework directing agent;

[0192] (iii) subjecting the synthesis mixture prepared in (ii) to hydrothermal synthesis conditions (including a hydrothermal synthesis temperature of 100-200° C.) to obtain a mixture comprising a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen;

[0193] wherein Y is Si, X is Al, M is Cu, and wherein the zeolitic material provided in (i) has a CHA or FAU framework type.

[0194] 12. The method of any one of embodiments 1-1, wherein providing a zeolite material according to (i) comprises:

[0195] (i.1) providing a zeolitic material that does not contain a metal M, has a framework type other than AEI, and has a framework structure comprising a trivalent element X and oxygen;

[0196] (i.2) loading the metal M on the zeolite material provided in (i.1), preferably comprising

[0197] (i.2.1) preparing a mixture comprising the zeolite material provided according to (i.1), a source of metal M, a solvent for the source of metal M and optionally an acid, preferably an organic acid, wherein the solvent preferably comprises water, the source of metal M preferably comprises a salt of metal M, and the acid preferably comprises acetic acid;

[0198] (i.2.2) heating the mixture prepared in (i.2.1) to a temperature of 30-90°C, preferably 40-80°C;

[0199] (i.2.3) preferably cooling, more preferably rapidly cooling the mixture obtained by (i.2.2);

[0200] (i.2.4) separating the zeolitic material comprising the metal M from the mixture obtained by (i.2.2) or (i.2.3), preferably (i.2.4), said separation preferably comprising washing the zeolitic material comprising the metal M;

[0201] (i.2.5) drying the zeolitic material comprising the metal M obtained by (i.2.4) preferably in a gas atmosphere, preferably at a gas atmosphere temperature of 90-200° C., more preferably 100-150° C., wherein the gas atmosphere preferably comprises oxygen;

[0202] (i.2.6) The zeolitic material comprising metal M obtained by (i.2.4) or (i.2.5), preferably (i.2.5), is preferably calcined in a gas atmosphere, preferably at a gas atmosphere temperature of 350-600°C, more preferably 400-550°C, wherein the gas atmosphere preferably contains oxygen.

[0203] 13. The method of any one of embodiments 1 to 12, wherein the zeolitic material provided in (i) is a calcined zeolitic material, preferably a zeolitic material calcined in a gas atmosphere at a gas atmosphere temperature of 350-600° C., preferably 400-550° C., wherein the gas atmosphere preferably comprises oxygen.

[0204] 14. The process according to any of embodiments 1 to 13, wherein the zeolitic material provided in (i) is in its H form.

[0205] 15. The process according to any of embodiments 1 to 14, wherein the synthesis mixture prepared in (ii) which is subjected to (iii) does not contain zeolitic material having an AEI framework type.

[0206] 16. The process according to any of embodiments 1 to 15, wherein the synthesis mixture prepared in (ii) which is subjected to (iii) does not contain zeolite seed material having an AEI framework type.

[0207] 17. The method of any one of embodiments 1 to 16, wherein Y is Si, and the source of the tetravalent element Y according to (ii) comprises one or more of wet-process silica, dry-process silica, and colloidal silica.

[0208] 18. The method of any one of embodiments 1 to 17, wherein the source of the tetravalent element according to (ii) comprises, preferably is, colloidal silica.

[0209] 19. The method of any one of embodiments 1-18, wherein the AEI framework structuring agent comprises one or more quaternary Cationic compounds and / or one or more compounds containing quaternary ammonium cations;

[0210] One or more of which contain The cationic compound includes one or more compounds containing R1R2R3R4P+, wherein R 1 , R 2 , R 3 and R 4 represents, independently of one another, an optionally substituted and / or optionally branched (C1-C6)alkyl group, preferably a (C1-C5)alkyl group, more preferably a (C1-C4)alkyl group, more preferably a (C2-C3)alkyl group, even more preferably an optionally substituted methyl or ethyl group, wherein even more preferably R 1 , R 2 , R 3 and R 4 represents an optionally substituted ethyl group, preferably an unsubstituted ethyl group;

[0211] The one or more compounds containing quaternary ammonium cations include one or more N,N-dialkyl-dialkylpiperidinyl Cationic compounds, preferably one or more N,N-(C1-C3)dialkyl-(C1-C3)dialkylpiperidinyl Cationic compounds, more preferably one or more N,N-(C1-C2)dialkyl-(C1-C2)dialkylpiperidinyl The compound containing quaternary ammonium cations, wherein more preferably one or more compounds containing quaternary ammonium cations are selected from N, N-(C1-C2) dialkyl-2,6-(C1-C2) dialkylpiperidin Cation and N,N-(C1-C2)dialkyl-3,5-(C1-C2)dialkylpiperidine Cationic compounds, more preferably N,N-dimethyl-2,6-(C1-C2) dialkylpiperidin Cation and N,N-dimethyl-3,5-(C1-C2)dialkylpiperidin Cationic compounds, more preferably N,N-dimethyl-2,6-dimethylpiperidinium Cation and N,N-dimethyl-3,5-dimethylpiperidinium Cationic compounds;

[0212] One or more of the following The compound containing the quaternary ammonium cation and / or the one or more compounds containing the quaternary ammonium cation are salts, preferably selected from halides, preferably chlorides and / or bromides, more preferably chlorides; hydroxides; sulfates; nitrates; phosphates; acetates; and mixtures of two or more thereof, more preferably selected from chlorides, hydroxides, sulfates and mixtures of two or more thereof, wherein one or more compounds containing the quaternary ammonium cation are more preferably selected from The cationic compound and / or the one or more compounds containing a quaternary ammonium cation are hydroxides and / or chlorides, even more preferably hydroxides.

[0213] 20. The method of any one of embodiments 1-19, wherein the AEI framework structure directing agent comprises, preferably N,N-dimethyl-3,5-dimethylpiperidine hydroxide.

[0214] 21. The process of any one of embodiments 1 to 20, wherein in the synthesis mixture prepared in (ii) which is subjected to (iii), the weight ratio of zeolitic material to the source of tetravalent element Y expressed as YO2 is 1.0:1-3.0:1, preferably 1.5:1-2.5, more preferably 2.0:1-2.2:1.

[0215] 22. The process according to any one of embodiments 1 to 21, wherein the weight ratio of zeolitic material to water in the synthesis mixture prepared in (ii) which is subjected to (iii) is 0.005:1-0.030:1, preferably 0.010:1-0.025:1, more preferably 0.015:1-0.020:1.

[0216] 23. The method of any one of embodiments 1-22, wherein in the synthesis mixture prepared in (ii) which is subjected to (iii), the weight ratio of zeolite material to AEI framework structure directing agent is 0.1:1-3:1, preferably 0.2:1-2:1, more preferably 0.3:1-0.7:1, more preferably 0.4:1-0.5:1.

[0217] 24. The process according to any of embodiments 1 to 23, wherein the synthesis mixture prepared in (ii) which is subjected to (iii) additionally comprises a base source, preferably a hydroxide source.

[0218] 25. The process according to any of embodiments 1 to 24, wherein the synthesis mixture prepared in (ii) which is subjected to (iii) additionally comprises a source of one or more of alkali metals and alkaline earth metals, preferably alkali metals, more preferably sodium.

[0219] 26. The process of embodiment 24 or 25, wherein the base source is a source of one or more of an alkali metal and an alkaline earth metal, preferably an alkali metal base, more preferably an alkali metal hydroxide, more preferably sodium hydroxide.

[0220] 27. The process according to any one of embodiments 24 to 26, wherein the weight ratio of zeolitic material to alkalinity source in the synthesis mixture prepared in (ii) which is subjected to (iii) is 0.1:1-1.0:1, preferably 0.2:1-0.8:1, more preferably 0.3:1-0.6:1.

[0221] 28. The process according to any of embodiments 1 to 27, wherein the synthesis mixture prepared in (ii) and subjected to (iii) contains no source of the metal M other than the zeolitic material comprising the metal M.

[0222] 29. The method of any one of embodiments 1-28, wherein at least 95% by weight, preferably at least 98% by weight, and more preferably at least 99% by weight of the synthesis mixture prepared in (ii) and subjected to (iii) consists of the zeolitic material provided in (i), water, a source of the tetravalent element Y, an AEI framework structure directing agent, and preferably a source of alkali and a source of one or more of alkali metals and alkaline earth metals.

[0223] 30. The process according to any of embodiments 1 to 29, wherein the hydrothermal synthesis is carried out under autogenous pressure, preferably in an autoclave.

[0224] 31. The process according to any of embodiments 1 to 30, wherein the synthesis mixture prepared in (ii) is heated to the hydrothermal synthesis temperature in an autoclave at a heating rate of 0.5 to 4 K / min, preferably 1 to 3 K / min.

[0225] 32. The method according to any one of embodiments 1 to 31, wherein the hydrothermal synthesis temperature is 110-175°C, preferably 120-150°C.

[0226] 33. The method of any one of embodiments 1 to 32, wherein the hydrothermal synthesis conditions comprise stirring the synthesis mixture.

[0227] 34. The method of any one of embodiments 1 to 33, wherein the hydrothermal synthesis conditions include a hydrothermal synthesis time of 2 to 120 hours, preferably 20 to 100 hours, more preferably 40 to 80 hours.

[0228] 35. The method of any one of embodiments 1-34, further comprising

[0229] (iv) cooling the mixture obtained from (iii), preferably to a temperature of 10-50°C, more preferably 20-35°C.

[0230] 36. The method of any one of embodiments 1-34, further comprising

[0231] (v) isolating a composition comprising a zeolitic material comprising a metal M from the mixture obtained from (iii) or (iv).

[0232] 37. The method of embodiment 36, wherein (v) comprises

[0233] (v.1) subjecting the mixture obtained from (iii) or (iv) to a solid-liquid separation method, preferably comprising a filtration method or a spraying method, to obtain a composition containing a zeolitic material comprising a metal M;

[0234] (v.2) preferably washing the composition containing the zeolitic material comprising the metal M obtained in (v.1);

[0235] (v.3) Drying the composition containing the zeolitic material comprising the metal M obtained by (v.1) or (v.2), preferably (v.2).

[0236] 38. The process of embodiment 37, wherein according to (v.2), the composition is washed with water, preferably until the wash water has a conductivity of at most 500 microSiemens, preferably at most 200 microSiemens.

[0237] 39. The method of embodiment 37 or 38, wherein according to (v.3), the composition is dried in a gas atmosphere having a temperature of 80-175°C, preferably 100-150°C.

[0238] 40. The method according to embodiment 39, wherein the gas atmosphere comprises oxygen, preferably air, rarefied air or synthetic air.

[0239] 41. The method of any one of embodiments 36-40, further comprising (vi) calcining the composition obtained from (v).

[0240] 42. The process of embodiment 41, wherein according to (vi), the composition is calcined in a gas atmosphere having a temperature of 400-600°C, preferably 450-550°C.

[0241] 43. The method according to embodiment 42, wherein the gas atmosphere comprises oxygen, preferably air, rarefied air or synthetic air.

[0242] 44. A method for preparing a composition containing a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, preferably the method of any one of embodiments 1-10, the method comprising:

[0243] (i) providing a zeolitic material comprising a metal M, having a framework type other than AEI and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen;

[0244] (ii) preparing a synthesis mixture comprising the zeolite material provided in (i), water, a source of a tetravalent element Y, and an AEI framework directing agent;

[0245] (iii) subjecting the synthesis mixture prepared in (ii) to hydrothermal synthesis conditions (including a hydrothermal synthesis temperature of 100-200° C.) to obtain a mixture comprising a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen;

[0246] (iv) cooling the mixture obtained from (iii), preferably to a temperature of 10-50°C, more preferably 20-35°C;

[0247] (v) separating a composition comprising a zeolitic material comprising a metal M from the mixture obtained from (iv), comprising

[0248] (v.1) subjecting the mixture obtained from (iv) to a solid-liquid separation method, preferably comprising a filtration method or a spraying method, to obtain a composition containing a zeolitic material comprising a metal M;

[0249] (v.2) washing the composition obtained in (v.1);

[0250] (v.3) drying the composition obtained in (v.2) in a gas atmosphere having a temperature of 80-175° C.;

[0251] (vi) calcining the composition obtained in (v) in a gas atmosphere having a temperature of 400-600°C.

[0252] 45. The process of embodiment 44, wherein Y is Si, X is Al, M is Cu, and the zeolitic material provided in (i) has a CHA or FAU framework type.

[0253] 46. ​​The method of any of embodiments 1-45, wherein greater than 50 wt.%, preferably at least 60 wt.%, more preferably at least 70 wt.%, of the composition containing zeolitic material comprising metal M, having an AEI framework type, and having a framework structure comprising a tetravalent element Y, a trivalent element X, and oxygen consists of zeolitic material comprising metal M, having an AEI framework type, and having a framework structure comprising a tetravalent element Y, a trivalent element X, and oxygen.

[0254] 47. The method of embodiment 46, wherein at least 80 weight percent, preferably 80-100 weight percent, of the composition containing a zeolite material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen consists of a zeolite material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen.

[0255] 48. The method of embodiment 46 or 47, wherein at least 90% by weight, preferably at least 95% by weight, and more preferably at least 99% by weight of the composition consists of zeolitic material comprising metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X, and oxygen, and zeolitic material comprising metal M, having a framework type other than AEI and having a framework structure comprising a tetravalent element Y, a trivalent element X, and oxygen.

[0256] 49. A composition comprising a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, obtainable or obtained or preparable or prepared by the method of any one of embodiments 1-48.

[0257] 50. The composition of embodiment 49, comprising 0.1-5 wt.-%, preferably 0.2-4 wt.-%, more preferably 0.5-3 wt.-% of M, calculated as element M and based on the total weight of the zeolitic material.

[0258] 51. The composition of embodiment 50, wherein M is Cu.

[0259] 52. A composition of any one of embodiments 49-51, having a total acid site amount of 1.0-2.0 mmol / g, wherein the total acid site amount is defined as the total molar amount of ammonia desorbed per mass of zeolite material measured according to the temperature-programmed desorption of ammonia (NH3-TPD) as described in Reference Example 1.6 herein; wherein the zeolite material has an intermediate acid site amount of 0.1-0.8 mmol / g, wherein the intermediate acid site amount is defined as the amount of ammonia desorbed per mass of zeolite material measured according to the temperature-programmed desorption of ammonia (NH3-TPD) as described in Reference Example 1.6 herein within a temperature range of 250-500°C.

[0260] 53. Use of the composition according to any of embodiments 49 to 52 as catalytically active material, catalyst or catalyst component.

[0261] 54. The use according to embodiment 53 for the selective catalytic reduction of nitrogen oxides in an exhaust gas stream, preferably an exhaust gas stream from a diesel engine.

[0262] 55. The use according to embodiment 53 for converting a C1 compound into one or more olefins, preferably converting methanol into one or more olefins or converting a synthesis gas comprising carbon monoxide and hydrogen into one or more olefins.

[0263] 56. A method for the selective catalytic reduction of nitrogen oxides in an exhaust gas stream, preferably an exhaust gas stream from a diesel engine, the method comprising contacting a composition according to any one of embodiments 49-52 with the exhaust gas stream.

[0264] 57. A method for the selective catalytic reduction of nitrogen oxides in an exhaust stream, preferably an exhaust stream from a diesel engine, the method comprising preparing a composition by the method according to any one of embodiments 1-48, and contacting the exhaust stream with a catalyst comprising the composition.

[0265] 58. A method for catalytically converting a C1 compound into one or more olefins, preferably converting methanol into one or more olefins or converting synthesis gas comprising carbon monoxide and hydrogen into one or more olefins, the method comprising contacting a composition according to any one of embodiments 49-52 with the C1 compound.

[0266] 59. A method for catalytically converting a C1 compound into one or more olefins, preferably converting methanol into one or more olefins or converting synthesis gas comprising carbon monoxide and hydrogen into one or more olefins, the method comprising preparing a composition by a method according to any one of embodiments 1-48, and contacting the C1 compound with a catalyst comprising the composition.

[0267] 60. A catalyst, preferably for the selective catalytic reduction of nitrogen oxides in an exhaust gas stream, preferably an exhaust gas stream from a diesel engine, or for the catalytic conversion of a C1 compound into one or more olefins, preferably for the conversion of methanol into one or more olefins or for the conversion of a synthesis gas comprising carbon monoxide and hydrogen into one or more olefins, the catalyst comprising a composition according to any one of embodiments 49-52.

[0268] The present invention is further illustrated by the following examples, comparative examples and reference examples. Example

[0269] Reference Example 1.1: Determination of crystallinity

[0270] The crystallinity of the zeolite material of the present invention is determined by XRD analysis. Data are collected using a standard Bragg-Brentano diffractometer with a Cu-X-ray source and an energy dispersion point detector. The angular range of 2-70° (2θ) is scanned with a step size of 0.02°, while the variable divergence slit is set to a constant opening angle of 0.3°. The data are then analyzed using TOPAS V5 software, in which the sharp diffraction peaks are modeled using the PONKCS phase (for AEI and FAU) and the crystal structure (for CHA). The model is prepared as described by Madsen, IC, etc. It is refined to fit the data. An independent peak is inserted at an angular position of 28°. This is used to describe the amorphous content. The crystal content describes the crystal signal intensity relative to the total scattering intensity. Linear background, Lorentz and polarization corrections, lattice parameters, space groups and crystallite size are also included in the model.

[0271] Reference Example 1.2: Determination of BET specific surface area

[0272] The BET specific surface area is determined by nitrogen physical adsorption at 77K according to ISO 9277 (2nd edition 2010).

[0273] Reference Example 1.3: Determination of C value

[0274] The C value (BET parameter) was determined as described in ISO 9277 (2nd edition 2010), section 7.2.

[0275] Reference Example 1.4: Determination of XRD pattern

[0276] The XRD diffractogram was determined as described in Reference Example 1.1.

[0277] Reference Example 1.5: Scanning Electron Microscopy

[0278] SEM (scanning electron microscope) images (secondary electron (SE) images at 15 kV (kilovolts)) were prepared using Hitachi TM3000.

[0279] Reference Example 1.6: Temperature Programmed Desorption of Ammonia (NH3-TPD)

[0280] The temperature program desorption (NH3-TPD) of ammonia is carried out in the automatic chemisorption analysis unit (Micromeritics AutoChem II 2920) with thermal conductivity detector. The continuous analysis of desorbed material is completed using an online mass spectrometer (OmniStar QMG200 from Pfeiffer Vacuum). Sample (0.1g) is introduced into a quartz tube and analyzed using the following program. Temperature is measured by the Ni / Cr / Ni thermocouple above the sample in the quartz tube. For analysis, the He of purity 5.0 is used. Before any measurement, a blank sample is analyzed for calibration.

[0281] 1. Preparation: Start recording; measure once per second. At 25℃ and 30cm 3 / min He flow rate (room temperature (about 25 ° C) and 1 atm); heat to 600 ° C at a heating rate of 20 K / min; hold for 10 minutes. Cool at a cooling rate of 20 K / min in He flow (30 cm 3 / min) to 100 °C (the furnace is cooled along the slope); at a cooling rate of 3 K / min in a He gas flow (30 cm 3 / min) to 100°C (the sample is cooled along the slope).

[0282] 2. Saturation with NH3: Start recording; measure once per second. Change the gas flow to a 10% NH3 mixture in He (75 cm 3 / min; 100°C and 1atm); hold for 30 minutes.

[0283] 3. Remove excess material: Start recording; measure once per second. Change the air flow to 75 cm at 100 °C. 3 / min He flow rate (100°C and 1 atm); maintained for 60 minutes.

[0284] 4. NH3-TPD: Start recording; measure once per second. Heat at 10K / min in He gas flow (flow rate: 30cm 3 / min) to 600°C; hold for 30 minutes.

[0285] 5. The measurement is completed.

[0286] The desorbed ammonia was measured by means of an online mass spectrometer, which showed that the signal from the thermal conductivity detector was caused by the desorbed ammonia. This involved using the m / z=16 signal from ammonia to monitor the desorption of ammonia. The amount of ammonia adsorbed (mmol / g sample) was determined by integrating the TPD signal into the horizontal baseline with the aid of Micromeritics software.

[0287] Reference Example 2.1: Preparation of CuCHA

[0288] a) CHA zeolitic material (sodium form) was prepared according to a template-free synthesis method as described in WO 2013 / 068976 A, Example 2, page 43, line 29 to page 44, line 8.

[0289] b) 4,000 g of deionized water are charged into a container. 590 g of ammonium nitrate are dissolved therein under stirring, followed by 590 g of the zeolite material (sodium form) obtained according to a) being mixed under stirring and then rinsed with 190 g of deionized water. The resulting suspension is heated to 80° C. and maintained at this temperature for 2 hours. The resulting zeolite material in ammonium form is separated from the suspension by filtration and washed until the washing water is free of nitrates. The zeolite material thus separated is dried overnight at 120° C. in a convection oven.

[0290] b) 130 g of the zeolite material of a) was heated from room temperature to 450° C. in air at a heating rate of 2 K / min, and calcined at this temperature in air for 10 h to obtain an H-type zeolite material.

[0291] c) Preparation of CuCHA

[0292] Materials used:

[0293]

[0294] 700 g of deionized water were transferred to a container and zeolite CHA was added under stirring, followed by 30 g of deionized water. The resulting suspension was heated to 60° C., and acetic acid was added at this temperature, followed by copper (II) acetate monohydrate. Then, 50 g of water was added. The resulting mixture was kept at a temperature of 60° C. for 2 hours. The resulting suspension was rapidly cooled by adding 586 g of cold distilled water. The resulting suspension was subjected to filtration with a vacuum suction filter, and the filter cake was washed with deionized water until the conductivity of the washing water was less than 20 micro-Siemens. The zeolite material thus washed was dried overnight at 120° C. in a convection oven in air, subsequently heated to a temperature of 500° C. at a heating rate of 2 K / min, and calcined at this temperature for 5 h. 124 g of zeolite material CuCHA was obtained. Elemental analysis of the zeolite material (in weight %): Si=29.3; Al=6.5; Na=0.07; Cu=3.1.

[0295] Reference Example 2.2: Preparation of CuY

[0296] a) 50 g of zeolite Y (CBV-500 from Zeolyst) in its ammonium form were provided. Characteristics of zeolite Y: silica:alumina ratio (SAR) = 5.2; unit cell size = 24.53 angstroms; BET specific surface area = 750 m 3 / g. Na2O content = 0.2 wt%.

[0297] b) The zeolitic material of a) was converted into its H form by heating from room temperature to 500° C. in air at a heating rate of 2 K / min and calcining at this temperature for 5 h in air.

[0298] c) Preparation of CuY

[0299] Materials used:

[0300]

[0301] 250g of deionized water is transferred to a container and zeolite Y is added under stirring, followed by 30g of deionized water. The resulting suspension is heated to 60°C, and acetic acid is added at this temperature, followed by copper acetate (II) monohydrate. Then, the remaining amount of water is added. The resulting mixture is kept at a temperature of 60°C for 2 hours. The resulting suspension is rapidly cooled by adding 200g of cold distilled water. The resulting suspension is subjected to filtration with a vacuum suction filter, and the filter cake is washed with deionized water until the conductivity of the washing water is less than 20 micro-Siemens. The zeolite material thus washed is dried overnight at 120°C in a convection oven in air, then heated to a temperature of 500°C at a heating rate of 2K / min, and calcined at this temperature for 5h. 48.6g of zeolite material CuY is obtained.

[0302] Elemental analysis of the zeolitic material (in wt. %): Si=27.2; Al=9.2; Na=0.11; Cu=1.7.

[0303] Example 1: Preparation of CuAEI from CuCHA

[0304] Materials used:

[0305] NaOH (aqueous solution; 50 wt%): 70.73 g

[0306] Deionized water: 770.71 g 1,1,3,5-tetramethylpiperidine Hydroxide (Sachem; aqueous mixture, 19.77 wt%):

[0307] 196.18g AS40 (Grace; colloidal silica; aqueous solution, 40 wt%): 19.80 g CuCHA zeolite material according to the above Reference Example 2.1: 16.40 g

[0308] Fill a beaker with 670.71 g of deionized water and add the NaOH solution under stirring. Then, add the template compound (1,1,3,5-tetramethylpiperidin Hydroxide) was added, followed by the addition of CuCHA zeolite material under stirring. The mixture was stirred for another 1 h. Then, the colloidal silica solution was added under stirring, and the resulting mixture was stirred for another 0.5 h. The resulting suspension was transferred to a 2.5 L autoclave, and the remaining 100 g of deionized water was used to rinse the involved pipelines. The autoclave was then sealed.

[0309] Within 1 h, the mixture in the autoclave was heated to a temperature of 140° C. and maintained at this crystallization temperature for 72 h with stirring at 250 rpm. After depressurization and cooling to room temperature, the resulting suspension was subjected to filtration with a vacuum suction filter and the filter cake was washed with deionized water until the conductivity of the washing water was less than 200 microsiemens. The zeolite material thus washed was dried in air in a convection oven at 120° C. overnight and then heated to a temperature of 500° C. at a heating rate of 2 K / min and calcined at this temperature for 5 h. 24.0 g of zeolite material were obtained with a space-time yield of 6.15 kg / m 3 / d.

[0310] Elemental analysis of the zeolitic material (in wt. %): Si=32; Al=4.6; Na=3.4; Cu=2.0.

[0311] The crystallinity was measured as described in Reference Example 1.1 and was 65%. The BET specific surface area was measured as described in Reference Example 1.2 and was 501 m 3 / g. The C value measured as described in Reference Example 1.3 was -62. The XRD pattern measured as described in Reference Example 1.4 showed Figure 1 The SEM images measured as described in Reference Example 1.5 are shown in Figure 2 middle.

[0312] 82% of the crystalline material was CuAEI and 18% of the material was CuCHA.

[0313] Example 2: Preparation of CuAEI starting from CuY

[0314] Materials used:

[0315] NaOH (aqueous solution; 50 wt%): 70.73 g

[0316] Deionized water: 770.71 g 1,1,3,5-tetramethylpiperidine Hydroxide (Sachem; aqueous mixture, 19.77 wt%): 196.18 g

[0317] AS40 (Grace; colloidal silica; aqueous solution, 40 wt%): 19.80 g CuY zeolite material according to the above Reference Example 2.2: 16.40 g

[0318] Fill a beaker with 670.71 g of deionized water and add the NaOH solution under stirring. Then, add the template compound (1,1,3,5-tetramethylpiperidin Hydroxide), followed by the addition of CuCHA zeolite material under stirring. The mixture was stirred for another 1h. Then, the colloidal silica solution was added under stirring, and the resulting mixture was stirred for another 0.5h. The resulting suspension was transferred to a 2.5L autoclave, and the remaining 100g of deionized water was used to rinse the pipeline involved. Then, the autoclave was sealed. Within 1h, the mixture in the autoclave was heated to a temperature of 140°C and maintained at the crystallization temperature for 72h under stirring at 250rpm. After depressurization and cooling to room temperature, the resulting suspension was subjected to filtration with a vacuum suction filter, and the filter cake was washed with deionized water until the conductivity of the washing water was less than 200 micro-Siemens. The zeolite material thus washed was dried overnight at 120°C in a convection oven in air, then heated to a temperature of 500°C at a heating rate of 2K / min, and calcined at this temperature for 5h. 28.1g of zeolite material was obtained, with a space-time yield of 7.21kg / m 3 / d.

[0319] Elemental analysis of the zeolitic material (in wt. %): Si=35; Al=4.2; Na=1.4; Cu=0.71.

[0320] The crystallinity was measured as described in Reference Example 1.1 and was 94%. The BET specific surface area was measured as described in Reference Example 1.2 and was 583 m 3 / g. The C value measured as described in Reference Example 1.3 was -52. The XRD pattern measured as described in Reference Example 1.4 showed Figure 3 middle.

[0321] 85% of the crystalline material consisted of CuAEI and 15% of the material consisted of CuY.

[0322] Example 3: Use of a zeolite material having an AEI framework type and containing a metal M (Cu) in the selective catalytic reduction of nitrogen oxides

[0323] The zeolite materials obtained from Example 1 (powder) and Example 2 (powder) were prepared by mixing the corresponding materials with a ground alumina slurry ( The molded article was prepared by mixing with 100% TM100 / 150 (weight ratio of zeolite material: alumina = 70:30). The molded article was dried and calcined at 550°C for 1 h under stirring. The molded article was then crushed and sieved to a particle size of 250-500 microns. For subsequent tests, the corresponding aged material was used. For aging, the crushed and sieved particles were subjected to air containing 10% by weight of water at 650°C for 50 h, optionally followed by air containing 10% by weight of water at 800°C for 16 h. These crushed and aged materials were subjected to a selective catalytic reduction test. For this purpose, the corresponding aged samples (170 mg each) were diluted with 1 mL of corundum having the same particle size as the sample. The given sample was heated to 80,000 h. -1 The samples were exposed to a feed stream (500 ppm NO, 500 ppm NH3, 5% H2O, 10% O2, balance N2) at a gas hourly space velocity of 200°C and 575°C feed stream temperature. The results are shown in Figure 4 and 5 In. Figure 4 and 5 In the figure, the test results of the reference material are also shown.

[0324] The reference material is a zeolitic material having a CHA framework type, which was prepared as described in Example 1 of WO 2013 / 182974 A1, page 47, lines 1-18. This material was shaped, crushed, aged and tested as the material according to the invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0325] Figure 1 : shows the XRD pattern of the Cu-containing zeolite material according to Example 1.

[0326] Figure 2 : shows the SEM picture of the Cu-containing zeolite material according to Example 1.

[0327] Figure 3 : shows the XRD pattern of the Cu-containing zeolite material according to Example 2.

[0328] Figure 4 : shows the test results according to Example 3, in particular the results of the corresponding material aged at 650°C (simulating heavy-duty diesel engine application). The x-axis represents the NOx conversion rate of the corresponding material at a conversion temperature of 200°N, and the y-axis represents the NOx conversion rate of the corresponding material at a conversion temperature of 200°C. The empty triangle symbol represents the reference material (CHA zeolite without template), the black square represents the zeolite material of Example 1, and the black circle represents the zeolite material of Example 2.

[0329] Figure 5: shows the test results according to Example 3, in particular the results of the corresponding material aged at 800° C. (simulating a light-duty diesel engine application). The x-axis represents the NOx conversion of the corresponding material at a conversion temperature of 200° N, and the y-axis represents the NOx conversion of the corresponding material at a conversion temperature of 200° C. The empty triangle symbol represents the reference material (CHA zeolite without template), the black square represents the zeolite material of Example 1, and the black circle represents the zeolite material of Example 2.

[0330] Citations

[0331] - WO 2013 / 068976 A

[0332] - Madsen, IC, Scarlett, NVY (2008) "Quantitative phase analysis", in Dinnebier, RE, Billinge SJL (eds.) "Powder diffraction: theory and practice", The Royal Society of Chemistry, Cambridge, pp. 298-331.

[0333] - WO 2013 / 182974 A

Claims

1. A method for preparing a zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, the method comprising: (i) providing a zeolite material comprising a metal M, having a CHA framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen; (ii) preparing a synthesis mixture comprising the zeolite material provided in (i), water, a source of a tetravalent element Y, and an AEI framework directing agent; wherein Y is Si and the source of Y comprises colloidal silica; (iii) subjecting the synthesis mixture prepared in (ii) to hydrothermal synthesis conditions comprising heating the synthesis mixture to a temperature in the range of 100-200° C. and maintaining the synthesis mixture at a temperature in the range under autogenous pressure to obtain a zeolitic material having an AEI framework type; wherein X is Al; Wherein M is Cu; wherein the zeolitic material provided in (i) comprises 0.5-4 wt. % M, calculated as element M and based on the total weight of the zeolitic material; Wherein the AEI framework structuring agent comprises one or more compounds containing quaternary ammonium cations; The hydrothermal synthesis conditions include a hydrothermal synthesis time of 2 to 120 hours; The synthesis mixture prepared in (ii) which is subjected to (iii) additionally comprises an alkali source.

2. The process of claim 1, wherein the zeolitic material provided in (i) comprises 3 to 4 wt. % M, calculated as element M and based on the total weight of the zeolitic material.

3. The process of claim 1, wherein at least 95 wt. % of the zeolitic material provided in (i) consists of Y, X, O, M and H.

4. The process of claim 2, wherein at least 95 wt. % of the zeolitic material provided in (i) consists of Y, X, O, M and H.

5. The process of claim 4, wherein at least 98 wt. % of the zeolitic material provided in (i) consists of Y, X, O, M and H.

6. The process of claim 4, wherein at least 99 weight percent of the zeolitic material provided in (i) consists of Y, X, O, M and H.

7. The process of claim 4, wherein at least 99.5 wt. % of the zeolitic material provided in (i) consists of Y, X, O, M and H.

8. The process according to any one of claims 1 to 7, wherein the zeolitic material is provided according to (i) include: (i.1) providing a zeolitic material that does not contain a metal M, has a framework type other than AEI, and has a framework structure comprising a tetravalent element Y, a trivalent element X, and oxygen; (i.2) The metal M is loaded on the zeolite material provided in (i.1).

9. The method of claim 8, wherein loading the metal M on the zeolite material provided in (i.1) comprises (i.2.1) preparing a mixture comprising the zeolite material provided according to (i.1), a source of the metal M, a solvent for the source of the metal M, and optionally an acid; (i.2.2) heating the mixture prepared in (i.2.1) to a temperature of 30-90°C; (i.2.3) cooling the mixture obtained in (i.2.2); (i.2.4) separating the zeolitic material comprising the metal M from the mixture obtained in (i.2.3); (i.2.5) drying the zeolite material containing the metal M obtained in (i.2.4) in a gas atmosphere; (i.2.6) The zeolite material containing the metal M obtained in (i.2.5) is calcined in a gas atmosphere.

10. The method of claim 9, wherein in (i.2.1), the solvent comprises water.

11. The method of claim 9, wherein in (i.2.1), the source of metal M comprises a salt of metal M.

12. The method of claim 9, wherein in (i.2.1), the acid comprises acetic acid.

13. The method of claim 9, wherein in (i.2.2), the mixture prepared in (i.2.1) is heated to a temperature of 40-80°C.

14. The method of claim 9, wherein in (i.2.3), the mixture obtained in (i.2.2) is rapidly cooled.

15. The process of claim 9, wherein the separating in (i.2.4) comprises washing the zeolitic material comprising the metal M.

16. The process of claim 9, wherein in (i.2.5), the zeolitic material comprising the metal M obtained from (i.2.4) is dried in a gas atmosphere at a gas atmosphere temperature of 90-200°C.

17. The process of claim 9, wherein in (i.2.5), the zeolitic material comprising the metal M obtained from (i.2.4) is dried in a gas atmosphere at a gas atmosphere temperature of 100-150°C.

18. The method of claim 9, wherein in (i.2.5), the gas atmosphere comprises oxygen.

19. The method of claim 9, wherein in (i.2.6), the zeolitic material comprising the metal M obtained from (i.2.5) is calcined in a gas atmosphere at a gas atmosphere temperature of 350-600°C.

20. The process of claim 9, wherein in (i.2.6), the zeolitic material comprising the metal M obtained from (i.2.5) is calcined in a gas atmosphere at a gas atmosphere temperature of 400-550°C.

21. The method of claim 9, wherein in (i.2.6), the gas atmosphere comprises oxygen.

22. The method of any one of claims 1 to 7, wherein the one or more compounds containing quaternary ammonium cations include one or more N,N-dialkyl-dialkylpiperidinyl A compound containing a quaternary ammonium cation; wherein one or more compounds containing a quaternary ammonium cation are salts.

23. The method of any one of claims 9 to 21, wherein the one or more compounds containing quaternary ammonium cations include one or more N,N-dialkyl-dialkylpiperidinyl and wherein the one or more compounds containing quaternary ammonium cations are salts.

24. The method of claim 23, wherein the one or more compounds containing quaternary ammonium cations include one or more compounds containing N,N-(C 1 -C 3 )dialkyl-(C 1 -C 3 )Dialkylpiperidine Cationic compounds.

25. The method of claim 23, wherein the one or more compounds containing quaternary ammonium cations include one or more compounds containing N,N-(C 1 -C 2 )dialkyl-(C 1 -C 2 )Dialkylpiperidine Cationic compounds.

26. The method of claim 23, wherein the one or more compounds containing quaternary ammonium cations are selected from the group consisting of N,N-(C 1 -C 2 )dialkyl-2,6-(C 1 -C 2 )Dialkylpiperidine Cations and N,N-(C 1 -C 2 )dialkyl-3,5-(C 1 -C 2 )Dialkylpiperidine Cationic compounds.

27. The method of claim 23, wherein the one or more compounds containing quaternary ammonium cations are selected from the group consisting of N,N-dimethyl-2,6-(C 1 -C 2 )Dialkylpiperidine Cations and N,N-dimethyl-3,5-(C 1 -C 2 )Dialkylpiperidine Cationic compounds.

28. The method of claim 23, wherein the one or more compounds containing a quaternary ammonium cation are selected from the group consisting of N,N-dimethyl-2,6-dimethylpiperidinium Cation and N,N-dimethyl-3,5-dimethylpiperidinium Cationic compounds.

29. The method of claim 23, wherein the one or more quaternary ammonium cation-containing compounds are selected from the group consisting of halides; hydroxides; sulfates; nitrates; phosphates; acetates; and mixtures of two or more thereof.

30. The method of claim 23, wherein the one or more quaternary ammonium cation-containing compounds are selected from chlorides and / or bromides.

31. The method of claim 23, wherein the AEI framework structure directing agent is N,N-dimethyl-3,5-dimethylpiperidine hydroxide.

32. The process of any one of claims 1 to 7, wherein in the synthesis mixture prepared in (ii) which is subjected to (iii), the zeolitic material is present in an amount relative to the amount of YO 2 The weight ratio of the source of the tetravalent element Y is 1.0:1-3.0:1; the weight ratio of the zeolite material to water is 0.005:1-0.030:1; and the weight ratio of the zeolite material to the AEI framework structure directing agent is 0.1:1-3:

1.

33. A process according to any one of claims 24 to 31, wherein in the synthesis mixture prepared in (ii) which is subjected to (iii), the zeolitic material is present in an amount relative to YO 2 The weight ratio of the source of the tetravalent element Y is 1.0:1-3.0:1; the weight ratio of the zeolite material to water is 0.005:1-0.030:1; and the weight ratio of the zeolite material to the AEI framework structure directing agent is 0.1:1-3:

1.

34. The process of claim 33, wherein in the synthesis mixture prepared in (ii) which is subjected to (iii), the zeolitic material is present relative to YO 2 The weight ratio of the source of the tetravalent element Y is 1.5:1-2.

5.

35. The process of claim 33, wherein in the synthesis mixture prepared in (ii) which is subjected to (iii), the zeolitic material is present relative to YO 2 The weight ratio of the source of the tetravalent element Y is 2.0:1-2.2:

1.

36. The process of claim 33, wherein the weight ratio of the zeolite material to water in the synthesis mixture prepared in (ii) which is subjected to (iii) is from 0.010:1 to 0.025:

1.

37. The process of claim 33, wherein the weight ratio of the zeolite material to water in the synthesis mixture prepared in (ii) which is subjected to (iii) is from 0.015:1 to 0.020:

1.

38. The method of claim 33, wherein the weight ratio of zeolitic material to AEI framework directing agent in the synthesis mixture prepared in (ii) which is subjected to (iii) is from 0.2:1 to 2:

1.

39. The method of claim 33, wherein the weight ratio of zeolitic material to AEI framework directing agent in the synthesis mixture prepared in (ii) which is subjected to (iii) is from 0.3:1 to 0.7:

1.

40. The method of claim 33, wherein the weight ratio of zeolitic material to AEI framework directing agent in the synthesis mixture prepared in (ii) which is subjected to (iii) is from 0.4:1 to 0.5:

1.

41. The method of any one of claims 1-7, wherein the base source is a hydroxide source.

42. The method of any one of claims 34-40, wherein the base source is a hydroxide source.

43. The process of claim 42, wherein the weight ratio of the zeolitic material to the alkaline source in the synthesis mixture prepared in (ii) which is subjected to (iii) is from 0.1:1 to 1.0:

1.

44. The process of claim 42, wherein the weight ratio of the zeolitic material to the alkaline source in the synthesis mixture prepared in (ii) which is subjected to (iii) is from 0.2:1 to 0.8:

1.

45. The process of claim 42, wherein the weight ratio of the zeolitic material to the alkaline source in the synthesis mixture prepared in (ii) which is subjected to (iii) is from 0.3:1 to 0.6:

1.

46. ​​The method of any one of claims 1 to 7, wherein the hydrothermal synthesis temperature is 110-175°C.

47. The method of any one of claims 43 to 45, wherein the hydrothermal synthesis temperature is 110 to 175°C.

48. The method of claim 47, wherein the hydrothermal synthesis temperature is 120-150°C.

49. The method of claim 47, wherein the hydrothermal synthesis conditions include a hydrothermal synthesis time of 20 to 100 hours.

50. The method of claim 47, wherein the hydrothermal synthesis conditions include a hydrothermal synthesis time of 40-80 hours.

51. The method of any one of claims 1 to 7, further comprising (iv) cooling the mixture obtained in (iii); (v) separating the zeolitic material comprising the metal M from the mixture obtained in (iv); (vi) calcining the zeolitic material comprising the metal M obtained in (v).

52. The method of any one of claims 48-50, further comprising (iv) cooling the mixture obtained in (iii); (v) separating the zeolitic material comprising the metal M from the mixture obtained in (iv); (vi) calcining the zeolitic material comprising the metal M obtained in (v).

53. The process of claim 52, wherein in (iv), the mixture obtained from (iii) is cooled to a temperature of 10-50°C.

54. The process of claim 52, wherein in (iv), the mixture obtained from (iii) is cooled to a temperature of 20-35°C.

55. The process of claim 52, wherein in (vi), the zeolitic material comprising the metal M obtained from (v) is calcined in a gas atmosphere having a temperature of 400-600°C.

56. The process of claim 52, wherein in (vi), the zeolitic material comprising the metal M obtained from (v) is calcined in a gas atmosphere having a temperature of 450-550°C.

57. The method of claim 52, wherein (v) comprises (v.1) subjecting the mixture obtained from (iv) to a solid-liquid separation process; (v.2) washing the zeolitic material containing the metal M obtained in (v.1); (v.3) Drying the zeolitic material containing the metal M obtained in (v.2).

58. The method of claim 57, wherein in (v.1), the solid-liquid separation method comprises a filtration method or a spray method.

59. The process of claim 57, wherein in (v.3), the zeolitic material containing the metal M obtained from (v.2) is dried in a gas atmosphere having a temperature of 80-175°C.

60. The process of claim 57, wherein in (v.3), the zeolitic material containing the metal M obtained from (v.2) is dried in a gas atmosphere having a temperature of 100-150°C.

61. A zeolitic material comprising a metal M, having an AEI framework type and having a framework structure comprising a tetravalent element Y, a trivalent element X and oxygen, obtainable or obtained or preparable or prepared by a process according to any one of claims 1 to 60, and comprising 0.1 to 5 wt.-% M, calculated as element M and based on the total weight of the zeolitic material; wherein X is Al; wherein M is Cu.

62. The zeolitic material according to claim 61, comprising 0.2 to 4 wt.-% M, calculated as element M and based on the total weight of the zeolitic material.

63. The zeolitic material according to claim 61, comprising 0.5 to 3 wt.-% M, calculated as element M and based on the total weight of the zeolitic material.

64. The zeolite material of any one of claims 61-63, having a total acid site amount of 1.0-2.0 mmol / g, wherein the total acid site amount is defined as the total molar amount of ammonia desorbed per mass of zeolite material measured according to the temperature-programmed desorption of ammonia; wherein the zeolite material has an intermediate acid site amount of 0.1-0.8 mmol / g, wherein the intermediate acid site amount is defined as the amount of ammonia desorbed per mass of zeolite material measured according to the temperature-programmed desorption of ammonia in the temperature range of 250-500°C.

65. Use of a zeolitic material according to any of claims 61 to 64 as catalytically active material, catalyst or catalyst component.

66. Use of a zeolitic material according to any of claims 61 to 64 as catalytically active material, catalyst or catalyst component for the selective catalytic reduction of nitrogen oxides in exhaust gas streams, or for the conversion of C1 compounds into one or more olefins, or for the conversion of synthesis gas comprising carbon monoxide and hydrogen into one or more olefins.

67. Use of a zeolitic material according to any of claims 61 to 64 as catalytically active material, catalyst or catalyst component for the selective catalytic reduction of nitrogen oxides in exhaust gas streams from diesel engines.

68. Use of a zeolitic material according to any one of claims 61 to 64 as catalytically active material, catalyst or catalyst component in the conversion of methanol to one or more olefins.