Polymer layer for protecting lithium anode of lithium metal secondary battery and manufacturing method
By using high elastic polymer as an anode protective layer in lithium metal batteries, the problem of lithium metal dendrites and lithium metal-electrolyte reactions is solved, and the cycle stability of lithium metal batteries is achieved with high specific capacity, high energy density and long life sex.
Patent Information
- Application Number
- CN201880038657.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2017-04-12
- Filing Date
- 2018-03-29
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing lithium metal batteries have internal short circuits and thermal runaway problems due to the formation of lithium metal dendrites, and the adverse reaction between lithium metal and electrolytes leads to rapid capacity attenuation, which lacks a simple and cost-effective solution.
Using high elastic polymer as the anode protective layer, with a recoverable tensile strain of no less than 2% and a lithium ion conductivity of no less than 10-6S/cm at room temperature, placed in lithium or lithium alloy foil/coating and electrolyte or between the membrane-electrolyte components, preventing uneven deposition of lithium ions and continuous reaction between the electrolyte and lithium metal.
It effectively prevents the formation of lithium metal dendrites, ensures uniform deposition of lithium ions and the cycle stability of the battery, and significantly improves the cycle life and safety of lithium metal batteries.
Smart Images

Figure CN110915049B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. Patent Application No. 15 / 485,934, filed on April 12, 2017, which is incorporated herein by reference. Technical Field
[0003] The present invention relates to the field of rechargeable lithium metal batteries having a lithium metal layer (in the form of a thin lithium foil, coating or sheet) as anode active material and methods for their manufacture. Background Art
[0004] Lithium-ion and lithium (Li) metal batteries (including lithium-sulfur batteries, Li-air batteries, etc.) are considered to be promising power sources for electric vehicles (EVs), hybrid electric vehicles (HEVs), and portable electronic devices such as laptop computers and mobile phones. 4.4 Compared with lithium metal (Si), lithium metal has the highest capacity (3,861 mAh / g). Therefore, in general, rechargeable Li metal batteries have significantly higher energy density than lithium ion batteries.
[0005] Historically, rechargeable lithium metal batteries were produced using non-lithiated compounds with high specific capacity such as TiS2, MoS2, MnO2, CoO2, and V2O5 as cathode active materials, which were coupled to a lithium metal anode. When the battery is discharged, lithium ions dissolve from the lithium metal anode and transfer to the cathode through the electrolyte, and the cathode thus becomes lithiated. Unfortunately, upon cycling, the lithium metal causes the formation of dendrites, ultimately causing unsafe conditions in the battery. As a result, the production of these types of secondary batteries was discontinued in the early 1990s, replaced by lithium-ion batteries.
[0006] Even now, cycling stability and safety issues remain the main factors hindering the further commercialization of Li metal batteries for EV, HEV and microelectronic device applications. These problems are mainly due to the high tendency of Li to form dendrite structures during repeated charge-discharge cycles or overcharge, resulting in internal electrical short circuits and thermal runaway. Many attempts have been made to solve the problems associated with dendrites, as briefly summarized below:
[0007] Fauteux et al. [D. Fauteux et al., "Secondary Electrolytic Cell and Electrolytic Process," U.S. Pat. No. 5,434,021, July 18, 1995] apply a protective surface layer (e.g., a mixture of polynuclear aromatic hydrocarbons and polyethylene oxide) to the metal anode, which enables metal ions to transfer from the metal anode to the electrolyte and back. The surface layer is also electronically conductive, so during electrodeposition (i.e., during battery recharging), the ions will be uniformly attracted back to the metal anode. Alamgir et al. [M. Alamgir et al., "Solid polymer electrolyte batteries containing metallocenes," U.S. Pat. No. 5,536,599, July 16, 1996] use ferrocene to prevent chemical overcharge and dendrite formation in rechargeable batteries based on solid polymer electrolytes.
[0008] Skotheim [TASkotheim, "Stabilized Anode for Lithium-Polymer Battery," U.S. Pat. No. 5,648,187 (July 15, 1997); U.S. Pat. No. 5,961,672 (October 5, 1999)] provides a Li metal anode that is stabilized against dendrite formation by using a vacuum evaporated thin film of a Li ion conducting polymer interposed between the Li metal anode and the electrolyte. Skotheim et al. [TASkotheim et al. "Lithium Anodes for Electrochemical Cells", U.S. Pat. No. 6,733,924 (May 11, 2004); U.S. Pat. No. 6,797,428 (September 28, 2004); U.S. Pat. No. 6,936,381 (August 30, 2005); and U.S. Pat. No. 7,247,408 (July 24, 2007)] further proposed a multilayer anode structure consisting of a first layer based on Li metal, a second layer of a temporary protective metal (such as Cu, Mg, and Al), and a third layer consisting of at least one layer (typically 2 or more layers) of a single ion conducting glass (such as lithium silicate and lithium phosphate) or a polymer. Obviously, such an anode structure consisting of at least 3 or 4 layers is too complicated and too expensive to manufacture and use.
[0009] Protective coatings for Li anodes, such as a glassy surface layer of LiI-Li3PO4-P2S5, can be obtained by plasma-assisted deposition [SJ Visco et al., "Protective Coatings for Negative Electrodes," U.S. Pat. No. 6,025,094 (Feb. 15, 2000). Complex multilayer protective coatings have also been proposed by Visco et al. [SJ Visco et al., "Protected Active Metal Electrode and Battery Cell Structures with Non-aqueous Interlayer Architecture," U.S. Pat. No. 7,282,295 (Oct. 16, 2007); U.S. Pat. No. 7,282,296 (Oct. 16, 2007); and U.S. Pat. No. 7,282,302 (Oct. 16, 2007)].
[0010] Despite these previous efforts, no rechargeable Li metal battery has yet achieved commercial success. This may be due to the view that these prior art approaches still have significant drawbacks. For example, in several cases, the anode structure or electrolyte structure is too complex. In other cases, the materials are too expensive, or the methods for making the materials are too laborious or difficult. Solid electrolytes typically have low lithium ion conductivity, are difficult to produce, and are difficult to implement into batteries.
[0011] Furthermore, solid electrolytes, either as the sole electrolyte in the cell or as an anode protection layer (interposed between the lithium membrane and the liquid electrolyte), do not have and cannot maintain good contact with the lithium metal. This effectively reduces the effectiveness of the electrolyte in supporting lithium ion dissolution (during battery discharge), transporting lithium ions, and allowing lithium ions to redeposit back into the lithium anode (during battery recharge).
[0012] Another major problem associated with lithium metal anodes is the continued reaction between the electrolyte and the lithium metal, resulting in the repeated formation of "dead lithium-containing species" that can no longer be deposited back into the anode and become isolated from the anode. These reactions continue to irreversibly consume the electrolyte and lithium metal, resulting in rapid capacity decay. In order to compensate for this continued loss of lithium metal, an excess of lithium metal (3-5 times more than what would be required) is typically implemented at the anode when manufacturing the battery. This not only increases cost, but also significantly increases the weight and volume of the battery, thereby reducing the energy density of the battery cell. This important issue has been largely ignored, and there has been no plausible solution to this problem in the battery industry.
[0013] Clearly, a simpler, more cost-effective, and easier to implement approach is urgently needed to prevent Li metal dendrite-induced internal short circuit and thermal runaway problems in Li metal batteries, as well as to reduce or eliminate the adverse reactions between Li metal and electrolyte.
[0014] Therefore, the object of the present invention is to provide an effective method to overcome the lithium metal dendrite and reaction problems in all types of Li metal batteries with lithium metal anodes. A specific object of the present invention is to provide a lithium metal battery cell that exhibits high specific capacity, high specific energy, high safety, and long and stable cycle life. Summary of the invention
[0015] Reported herein is a lithium secondary battery comprising a cathode, an anode and an electrolyte or a separator-electrolyte assembly arranged between the cathode and the anode, wherein the anode comprises: (a) a foil or coating of lithium or a lithium alloy as an anode active material; and (b) a thin layer of a highly elastic polymer having a recoverable tensile strain of not less than 2%, a tensile strength of not less than 10-100% at room temperature, and a strength of not less than 10-100% at room temperature. 6 S / cm lithium ion conductivity, and a thickness from 1nm to 10μm, wherein the highly elastic polymer is arranged between the lithium or lithium alloy foil / coating layer and the electrolyte or separator-electrolyte assembly layer. The lithium or lithium alloy foil or coating can be supported by a current collector (e.g., Cu foil, Ni foam, nanofilaments such as graphene sheets, carbon nanofibers, carbon nanotubes, etc.). If the electrolyte is a solid electrolyte, a porous separator may not be required.
[0016] Highly elastic polymers refer to polymers, typically lightly cross-linked polymers, which exhibit an elastic deformation of at least 2% (preferably at least 5%) when measured under uniaxial tension. In the field of materials science and engineering, "elastic deformation" is defined as the deformation of a material (when subjected to mechanical stress) that is substantially completely recoverable after the load is released, and the recovery process is substantially instantaneous (no or almost no time delay). The elastic deformation is more preferably greater than 10%, even more preferably greater than 30%, further more preferably greater than 50%, and still more preferably greater than 100%.
[0017] In some preferred embodiments, the highly elastic polymer contains a lightly cross-linked polymer chain network having ether bonds, nitrile-derived bonds, benzoyl peroxide-derived bonds, ethylene oxide bonds, propylene oxide bonds, vinyl alcohol bonds, cyano-resin bonds, triacrylate monomer-derived bonds, tetraacrylate monomer-derived bonds, or combinations thereof in the cross-linked polymer chain network. These networks or cross-linked polymers exhibit a unique combination of high elasticity (high elastic deformation strain) and high lithium ion conductivity.
[0018] In certain preferred embodiments, the elastomeric polymer contains a lightly cross-linked polymer chain network selected from nitrile-containing polyvinyl alcohol chains, cyanoresin chains, pentaerythritol tetraacrylate (PETEA) chains, pentaerythritol triacrylate chains, ethoxylated trimethylolpropane triacrylate (ETPTA) chains, ethylene glycol methyl ether acrylate (EGMEA) chains, or combinations thereof.
[0019] This highly elastic polymer layer can be a thin film arranged close to the surface of the lithium foil / coating layer or a thin coating deposited on the surface of the lithium foil / coating. It can be noted that as the lithium battery discharges, the thickness of the lithium foil / coating layer may decrease due to the dissolution of lithium into the electrolyte to become lithium ions. If the protective layer is not elastic, a gap is generated between the current collector and the protective layer. Such a gap will make it impossible to deposit lithium ions back to the anode. We have observed that the highly elastic polymer can expand or shrink accordingly or in unison with the anode layer. This ability helps to maintain good contact between the current collector (or the lithium film itself) and the protective layer, so that lithium ions can be deposited again without interruption.
[0020] In certain embodiments, the highly elastic polymer contains a conductive material (i.e., an electronically conductive material) dispersed therein. The conductive material may be selected from electronically conductive polymers, metal particles or metal wires (or metal nanowires), graphene sheets, carbon fibers, graphite fibers, carbon nanofibers, graphite nanofibers, carbon nanotubes, graphite particles, expanded graphite flakes, acetylene black particles, or a combination thereof. The conductive material (e.g., metal nanowires, nanofibers, etc.) preferably has a thickness or diameter of less than 100 nm.
[0021] The lithium salt dispersed in the highly elastic polymer can be preferably selected from lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium fluoroborate (LiBF4), lithium hexafluoroarsenide (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethylsulfonyl)imide (LiN(CF3SO2)2), lithium bis(oxalate)borate (LiBOB), lithium difluorooxalatoborate (LiBF2C2O4), lithium difluorooxalatoborate (LiBF2C2O4), lithium nitrate (LiNO3), lithium fluoroalkyl phosphate (LiPF3(CF2CF3)3), lithium bisperfluoroethylsulfonyl imide (LiBETI), lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonyl imide (LiTFSI), ionic liquid-based lithium salts, or combinations thereof.
[0022] On the anode side, the highly elastic polymer used for the protective layer preferably and typically has a strength of not less than 10- 5 S / cm, more preferably not less than 10- 4S / cm, and most preferably not less than 10- 3 S / cm lithium ion conductivity. Some selected polymers exhibit greater than 10- 2 S / cm lithium ion conductivity. In some embodiments, the highly elastic polymer is a pure polymer without additives or fillers dispersed therein. In other embodiments, the highly elastic polymer is a polymer matrix composite containing from 0.1% to 50% by weight (preferably from 1% to 35% by weight) of lithium ion conductive additives dispersed in a polymer matrix material. In some embodiments, the highly elastic polymer contains from 0.1% by weight to 10% by weight of reinforced nanofilaments selected from carbon nanotubes, carbon nanofibers, graphene, or a combination thereof.
[0023] In some embodiments, the elastomeric polymer is mixed with an elastomer selected from the group consisting of natural polyisoprene (e.g., cis-1,4-polyisoprene natural rubber (NR) and trans-1,4-polyisoprene gutta-percha), synthetic polyisoprene (isoprene rubber, IR), polybutadiene (butadiene rubber, BR), chloroprene rubber (CR), polychloroprene (e.g., Neoprene, Baypren, etc.), butyl rubber (copolymer of isobutylene and isoprene, IIR), including halogenated butyl rubber (chlorobutyl rubber (CIIR) and bromobutyl rubber (BIIR)), styrene -Butadiene rubber (copolymer of styrene and butadiene, SBR), nitrile rubber (copolymer of butadiene and acrylonitrile, NBR), EPM (ethylene propylene rubber, copolymer of ethylene and propylene), EPDM rubber (ethylene propylene diene rubber, terpolymer of ethylene, propylene and diene components), epichlorohydrin rubber (ECO), polyacrylic rubber (ACM, ABR), silicone rubber (SI, Q, VMQ), fluorosilicone rubber (FVMQ), fluoroelastomers (FKM, and FEPM; such as Viton, Tecnoflon, Fluorel, Aflas and Dai-El), perfluoroelastomers (FFKM: Tecnoflon PFR, Kalrez, Chemraz, Perlast), polyether block amide (PEBA), chlorosulfonated polyethylene (CSM; such as Hypalon), and ethylene vinyl acetate (EVA), thermoplastic elastomers (TPE), protein elastin, protein elastin, ethylene oxide-epichlorohydrin copolymers, polyurethanes, urethane-urea copolymers, and combinations thereof.
[0024] In some embodiments, the elastomeric polymer is a composite containing a lithium ion conductive additive dispersed in a elastomeric polymer matrix material, wherein the lithium ion conductive additive is selected from Li2CO3, Li2O, Li2C2O4, LiOH, LiX, ROCO2Li, HCOLi, ROLi, (ROCO2Li)2, (CH2OCO2Li)2, Li2S, Li x SO y , or a combination thereof, wherein X=F, Cl, I, or Br, R=hydrocarbon, x=0-1, y=1-4.
[0025] The highly elastic polymer may form a mixture, blend, copolymer, or semi-IPN with an electronically conductive polymer selected from polyaniline, polypyrrole, polythiophene, polyfuran, bicyclic polymers, derivatives thereof (such as sulfonated versions), or combinations thereof.
[0026] In some embodiments, the highly elastic polymer may form a mixture, blend, or semi-IPN with a lithium ion conducting polymer selected from the group consisting of poly(ethylene oxide) (PEO), poly(propylene oxide) (PPO), poly(acrylonitrile) (PAN), poly(methyl methacrylate) (PMMA), poly(vinylidene fluoride) (PVdF), poly bis-methoxyethoxyethoxide-phosphazenex, polyvinyl chloride, polydimethylsiloxane, poly(vinylidene fluoride)-hexafluoropropylene (PVDF-HFP), sulfonated derivatives thereof, or combinations thereof. It is found herein that sulfonation imparts improved lithium ion conductivity to the polymer.
[0027] The cathode active material may be selected from inorganic materials, organic materials, polymer materials, or combinations thereof. The inorganic material may be selected from metal oxides, metal phosphates, metal silicides, metal selenides, metal sulfides, or combinations thereof.
[0028] The inorganic material may be selected from lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium vanadium oxide, lithium mixed metal oxide, lithium iron phosphate, lithium manganese phosphate, lithium vanadium phosphate, lithium mixed metal phosphate, lithium metal silicide, or a combination thereof.
[0029] In certain preferred embodiments, the inorganic material is selected from metal fluorides or metal chlorides, and the metal fluorides or metal chlorides include the group consisting of CoF3, MnF3, FeF3, VF3, VOF3, TiF3, BiF3, NiF2, FeF2, CuF2, CuF, SnF2, AgF, CuCl2, FeCl3, MnCl2, and combinations thereof. In certain preferred embodiments, the inorganic material is selected from lithium transition metal silicates, represented by Li2MSiO4 or Li2Ma x Mb y SiO4, wherein M and Ma are selected from Fe, Mn, Co, Ni, V, or VO; Mb is selected from Fe, Mn, Co, Ni, V, Ti, Al, B, Sn, or Bi; and x+y≤1.
[0030] In certain preferred embodiments, the inorganic material is selected from transition metal dichalcogenides, transition metal trichalcogenides, or combinations thereof. The inorganic material is selected from TiS2, TaS2, MoS2, NbSe3, MnO2, CoO2, iron oxides, vanadium oxides, or combinations thereof.
[0031] The cathode active material layer may contain a metal oxide containing a vanadium oxide selected from the group consisting of VO2, Li x VO2, V2O5, Li x V2O5, V3O8, Li x V3O8、Li x V3O7, V4O9, Li x V4O9, V6O 13 , Li x V6O 13 , its doping type, its derivatives, and combinations thereof, wherein 0.1 <x<5。
[0032] The cathode active material layer may contain a metal oxide or a metal phosphate, wherein the metal oxide or the metal phosphate is selected from a layered compound LiMO2, a spinel compound LiM2O4, an olivine compound LiMPO4, a silicate compound Li2MSiO4, a hydroxyphospholipid iron compound LiMPO4F, a borate compound LiMBO3, or a combination thereof, wherein M is a transition metal or a mixture of multiple transition metals.
[0033] In some embodiments, the inorganic material is selected from: (a) bismuth selenide or bismuth telluride, (b) dichalcogenides or trichalcogenides of transition metals, (c) niobium, zirconium, molybdenum, hafnium, tantalum, tungsten, titanium, cobalt, manganese, iron, nickel, or sulfides, selenides, or tellurides of transition metals; (d) boron nitride, or (e) combinations thereof.
[0034] For lithium-sulfur batteries, the cathode may contain sulfur, sulfur-containing molecules, sulfur compounds, lithium polysulfides, sulfur / carbon hybrids or composites, sulfur / graphite hybrids or composites, sulfur / graphene hybrids or composites, sulfur-polymer compounds, or combinations thereof. For lithium-selenium batteries, the cathode contains selenium (Se) or Se-containing compounds as cathode active materials.
[0035] The cathode active material layer may contain an organic material or a polymer material, wherein the organic material or the polymer material is selected from poly(anthraquinone sulfide) (PAQS), lithium oxycarbon, 3,4,9,10-perylenetetracarboxylic acid dianhydride (PTCDA), poly(anthraquinone sulfide), pyrene-4,5,9,10-tetraketone (PYT), polymer-bound PYT, quinone (triazene), redox-active organic material, tetracyanoquinodimethane (TCNQ), tetracyanoethylene (TCNE), 2,3,6,7,10,11-hexamethoxytriphenylene (HMTP), poly(5-amino-1,4-dihydroxyanthraquinone) (PADAQ), phosphazene disulfide polymer ([(NPS2)3]n), lithiated 1,4,5,8-naphthalene tetraol formaldehyde polymer, hexaazatrinaphthalene (HATN) , hexaazatriphenylene hexacarbonitrile (HAT(CN)6), 5-benzylidene hydantoin, isatin lithium salt, pyromellitic acid diimide lithium salt, tetrahydroxy-p-benzoquinone derivative (THQLi4), N,N'-diphenyl-2,3,5,6-tetraketopiperazine (PHP), N,N'-diallyl-2,3,5,6-tetraketopiperazine (AP), N,N'-dipropyl-2,3,5,6-tetraketopiperazine (PRP), thioether polymer, quinone compound, 1,4-benzoquinone, 5,7,12,14-pentacenetetraone (PT), 5-amino-2,3-dihydro-1,4-dihydroxyanthraquinone (ADDAQ), 5-amino-1,4-dihydroxyanthraquinone (ADAQ), quinone-type calixarene, Li4C6O6, Li2C6O6, Li6C6O6, or a combination thereof.
[0036] The thioether polymer is selected from poly[methylenethiocyanate-tetrakis(thiomethyl)] (PMTTM), poly(2,4-dithiopentene) (PDTP), a polymer containing poly(ethylene-1,1,2,2-tetrathiol) (PETT) as a main chain thioether polymer, a side chain thioether polymer having a main chain composed of a conjugated aromatic portion and having a thioether side chain as a side chain, poly(2-phenyl-1,3-dithiolane) (PPDT), poly(1,4-di(1,3-dithiolan-2-yl)benzene) (PDDTB), poly(tetrahydrobenzodithiophene) (PTHBDT), poly[1,2,4,5-tetrakis(propylthio)benzene] (PTKPTB) or poly[3,4(ethylenedithio)thiophene] (PEDTT).
[0037] In other embodiments, the cathode active material layer contains an organic material, and the organic material is selected from phthalocyanine compounds, such as copper phthalocyanine, zinc phthalocyanine, tin phthalocyanine, iron phthalocyanine, lead phthalocyanine, nickel phthalocyanine, vanadium phthalocyanine, fluorochromium phthalocyanine, magnesium phthalocyanine, manganese phthalocyanine, dilithium phthalocyanine, aluminum phthalocyanine chloride, cadmium phthalocyanine, chlorogallium phthalocyanine, cobalt phthalocyanine, silver phthalocyanine, metal-free phthalocyanine, their chemical derivatives, or combinations thereof.
[0038] The cathode active material is preferably in the form of nanoparticles (spherical, elliptical and irregular shapes), nanowires, nanofibers, nanotubes, nanosheets, nanobelts, nanoribbons, nanodisks, nanoplatelets, or nanohorns having a thickness or diameter of less than 100 nm. Unless otherwise specified or unless a specific type of the above substances is desired, these shapes can be collectively referred to as "particles". Further preferably, the cathode active material has a size of less than 50 nm, even more preferably less than 20 nm, and most preferably less than 10 nm. In some embodiments, a particle or a group of particles can be coated or surrounded by a carbon layer arranged between the one or more particles and / or the high elastic polymer layer (encapsulation shell).
[0039] The cathode layer may further contain graphite, graphene, or carbon material mixed with the cathode active material particles. The carbon or graphite material is selected from polymeric carbon, amorphous carbon, chemical vapor deposition carbon, coal tar pitch, petroleum pitch, mesophase pitch, carbon black, coke, acetylene black, activated carbon, fine expanded graphite particles with a size less than 100nm, artificial graphite particles, natural graphite particles, or a combination thereof. Graphene may be selected from native graphene, graphene oxide, reduced graphene oxide, fluorinated graphene, hydrogenated graphene, nitrided graphene, functionalized graphene, etc.
[0040] The cathode active material particles may be coated or surrounded by a conductive protective coating selected from a carbon material, graphene, an electronically conductive polymer, a conductive metal oxide or a conductive metal coating. Preferably, the cathode active material in the form of nanoparticles, nanowires, nanofibers, nanotubes, nanosheets, nanobelts, nanoribbons, nanodisks, nanoplatelets, or nanohorns is pre-intercalated or pre-doped with lithium ions to form a pre-lithiated anode active material having a lithium content of from 0.1% to 54.7% by weight of the pre-lithiated anode active material.
[0041] The present invention also provides a lithium metal-air battery comprising an air cathode, an anode comprising a protective layer based on a highly elastic polymer as defined above, and an electrolyte arranged between the anode and the air cathode or an electrolyte in combination with a separator. In the air cathode, oxygen from the open air (or from an oxygen supplier external to the battery) is the main cathode active material. The air cathode requires an inert material to support the lithium oxide material formed at the cathode. The applicants have surprisingly found that the integrated structure of conductive nanofilaments can be used as an air cathode intended to support discharge products (e.g., lithium oxide).
[0042] Therefore, another embodiment of the present invention is a lithium metal-air battery, wherein the air cathode comprises an integrated structure of conductive nanoscale filaments, the filaments are interconnected to form a porous network of electronic conduction paths containing interconnected pores, wherein the filaments have a lateral dimension of less than 500nm (preferably less than 100nm). These nanofilaments can be selected from carbon nanotubes (CNTs), carbon nanofibers (CNFs), graphene sheets, carbon fibers, graphite fibers, etc.
[0043] The present invention also provides a method for manufacturing a lithium battery, the method comprising: (a) providing a cathode active material layer and optionally a cathode current collector supporting the cathode active material layer; (b) providing an anode active material layer (containing lithium metal or lithium alloy foil or coating) and optionally an anode current collector supporting the lithium metal or lithium alloy foil or coating; (c) providing an electrolyte in contact with the anode active material layer and the cathode active material layer, and optionally a separator electrically separating the anode from the cathode; and (d) providing an anode protective layer of a highly elastic polymer, the highly elastic polymer having a recoverable tensile elastic strain of from 2% to 700% (preferably from 5% to 300%), a tensile strength of not less than 10-100% at room temperature, and a tensile strength of not less than 10-100% at room temperature. 6 S / cm, and a thickness from 0.5 nm to 10 μm. This anode protection layer is disposed between the lithium metal or lithium alloy foil or coating and the electrolyte or separator.
[0044] Preferably, the highly elastic polymer has a value ranging from 1×10- 5 S / cm to 5×10- 2 S / cm lithium ion conductivity. In some embodiments, the highly elastic polymer has a recoverable tensile strain from 10% to 300% (more preferably >30%, and even more preferably >50%).
[0045] In certain embodiments, the process of providing a highly elastic polymer includes providing a mixture / blend / composite of an ultra-high molecular weight polymer and an elastomer, an electronically conductive polymer (e.g., polyaniline, polypyrrole, polythiophene, polyfuran, a bicyclic polymer, a sulfonated derivative thereof, or a combination thereof), a lithium ion conductive material, a reinforcing material (e.g., carbon nanotubes, carbon nanofibers, and / or graphene), or a combination thereof.
[0046] In this mixture / blend / composite, the lithium ion conducting material is dispersed in the highly elastic polymer and is preferably selected from Li2CO3, Li2O, Li2C2O4, LiOH, LiX, ROCO2Li, HCOLi, ROLi, (ROCO2Li)2, (CH2OCO2Li)2, Li2S, Li x SO y , or a combination thereof, wherein X=F, Cl, I, or Br, R=hydrocarbon, x=0-1, y=1-4.
[0047] In some embodiments, the lithium ion conductive material is dispersed in the highly elastic polymer and is selected from lithium perchlorate LiClO4, lithium hexafluorophosphate LiPF6, lithium fluoroborate LiBF4, lithium hexafluoroarsenide LiAsF6, lithium trifluoromethanesulfonate LiCF3SO3, lithium bis(trifluoromethylsulfonyl)imide LiN(CF3SO2)2, lithium bis(oxalate)borate LiBOB, lithium difluorooxalatoborate LiBF2C2O4, lithium difluorooxalatoborate LiBF2C2O4, lithium nitrate LiNO3, lithium fluoroalkyl phosphate LiPF3(CF2CF3)3, lithium bis(perfluoroethylsulfonyl)imide LiBETI, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonylimide LiTFSI, ionic liquid-based lithium salts, or combinations thereof. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 Prior Art Schematic diagram of a lithium metal battery cell containing an anode layer (a thin Li foil or Li coating deposited on the surface of a current collector (Cu foil)), a porous separator, and a cathode active material layer consisting of cathode active material particles, a conductive additive (not shown), and a resin binder (not shown). A cathode current collector supporting the cathode active layer is also shown.
[0049] Figure 2Schematic diagram of a lithium metal battery cell of the present invention, the lithium metal battery cell contains an anode layer (a thin Li foil or Li coating deposited on the surface of a current collector (Cu foil)), an anode protective layer based on a highly elastic polymer, a porous separator, and a cathode active material layer, the cathode active material layer consisting of cathode active material particles, a conductive additive (not shown) and a resin binder (not shown). A cathode current collector supporting the cathode active layer is also shown.
[0050] FIG. 3 (A) Representative tensile stress-strain curves of lightly cross-linked ETPTA polymers.
[0051] Figure 3 (B) Intercalation specific capacity curves of four lithium batteries: 2 batteries each having a cathode containing V2O5 particles (one battery has an ETPTA polymer protective layer and the other does not) and 2 batteries each having a cathode containing V2O5 particles surrounded by graphene (one battery has an ETPTA polymer protective layer and the other does not).
[0052] Figure 4 (A) Representative tensile stress-strain curves of PVA-CN polymer films.
[0053] FIG. 4(B) Specific capacity values of two lithium-LiCoO2 cells (the cells initially contain no lithium) characterized by: (1) a highly elastic PVA-CN layer at the anode and (2) no polymer protective layer at the anode.
[0054] Figure 5 (A) Representative tensile stress-strain curves of PETEA polymer films.
[0055] FIG. 5(B) Discharge capacity curves of two coin cells with FeF3-based cathode active materials: (1) with anode protected by highly elastic PETEA; and (2) without anode protection layer.
[0056] Figure 6 Specific capacity of two lithium-FePc (organic) cells, each with Li foil as anode active material and FePc / RGO mixture particles as cathode active material (one cell contains ETPTA / EGMEA Semi-IPN protected anode and the other without anode protection layer).
[0057] Figure 7 Cathode specific capacity values of two Li-S cells with cathode active materials based on S-impregnated activated MCMB particles: one cell with an ETPTA-protected anode and the other without an anode protection layer.
[0058] Figure 8Cathode specific capacity values for two Li-S cells with cathode active materials based on S / graphene hybrids and (1) a highly elastic PETEA layer for anode protection and (2) no anode protection layer, respectively. DETAILED DESCRIPTION
[0059] The present invention relates to a lithium secondary battery, which is preferably based on an organic electrolyte, a polymer gel electrolyte, an ionic liquid electrolyte, a quasi-solid electrolyte, or a solid electrolyte. The shape of the lithium secondary battery can be cylindrical, square, button-shaped, etc. The present invention is not limited to any battery shape or configuration, or any type of electrolyte.
[0060] The present invention provides a lithium secondary battery, the lithium secondary battery comprising a cathode, an anode and an electrolyte or a separator-electrolyte assembly arranged between the cathode and the anode, wherein the anode comprises: (a) a foil or coating of lithium or a lithium alloy as an anode active material; and (b) a thin layer of a highly elastic polymer having a recoverable tensile strain of not less than 2%, a tensile strength of not less than 10-100% at room temperature, and a tensile strength of not less than 10-100% at room temperature. 6 S / cm lithium ion conductivity, and a thickness from 1nm to 10μm, wherein the highly elastic polymer is arranged (intercalated) between the lithium or lithium alloy foil / coating and the electrolyte or separator-electrolyte assembly. The lithium or lithium alloy foil or coating can be supported by a current collector (e.g., Cu foil, Ni foam, a porous layer of nanofilaments (such as graphene sheets, carbon nanofibers, carbon nanotubes, etc.) forming a 3D interconnected network of electronic conduction pathways).
[0061] Preferably, the composition of this anode protection layer is different from that of the electrolyte used in the lithium battery, and is maintained as a discrete layer (not dissolved in the electrolyte) disposed between the anode active material layer (e.g., Li foil or Li coating on the current collector) and the electrolyte (or electrolyte-separator layer).
[0062] We have discovered that this protective layer provides several unexpected benefits: (a) dendrite formation has been essentially eliminated; (b) uniform deposition of lithium back to the anode side is easily achieved; (c) the layer ensures smooth and uninterrupted transport of lithium ions from / to the lithium foil / coating and through the interface between the lithium foil / coating and the protective layer with minimal interfacial resistance; and (d) cycling stability can be significantly improved and cycle life increased.
[0063] In conventional lithium metal cells, as shown in FIG1 , the anode active material (lithium) is deposited directly on the anode current collector (e.g., Cu foil) in the form of a thin film or thin foil. The battery is a lithium metal battery, a lithium sulfur battery, a lithium-air battery, a lithium-selenium battery, etc. As previously discussed in the background technology section, these lithium secondary batteries have dendrite-induced internal short circuits and "dead lithium" problems at the anode.
[0064] We have solved these challenging problems that have plagued battery designers and electrochemists alike for more than 30 years by developing and implementing a new anode protection layer between the lithium foil / coating and the electrolyte (or electrolyte / separator). This protection layer comprises a highly elastic polymer having a recoverable (elastic) tensile strain of not less than 2% (preferably not less than 5%) under uniaxial tension and a thermal conductivity of not less than 10- 6 S / cm (preferably and more typically from 1×10- 5 S / cm to 5×10- 2 S / cm) of lithium ion conductivity.
[0065] like Figure 2 As schematically shown in the figure, one embodiment of the present invention is a lithium metal battery cell, which contains an anode layer (a thin Li foil or Li coating deposited on the surface of a current collector (Cu foil)), an anode protection layer based on a highly elastic polymer, a porous separator and a cathode active material layer, wherein the cathode active material layer is composed of cathode active material particles, a conductive additive (not shown) and a resin binder (not shown). Figure 2 Also shown is a cathode current collector (eg, Al foil) supporting the cathode active layer.
[0066] A highly elastic polymer refers to a polymer that exhibits an elastic deformation of at least 2% when measured under uniaxial tension. In the field of materials science and engineering, "elastic deformation" is defined as the deformation of a material (when subjected to mechanical stress) that is substantially completely recoverable after the load is released and the recovery is substantially instantaneous. The elastic deformation is preferably greater than 5%, more preferably greater than 10%, further more preferably greater than 30%, and still more preferably greater than 100%.
[0067] It can be noted that although Figure 2 The lithium coating pre-existing at the anode when the lithium battery is manufactured is shown, but this is only one embodiment of the present invention. An alternative embodiment is a lithium battery that does not contain lithium foil or lithium coating at the anode (only the anode current collector, such as Cu foil or graphene / CNT felt) when the battery is manufactured. The lithium required to bounce back and forth between the anode and the cathode is first stored in the cathode active material (e.g., lithium vanadium oxide Li instead of vanadium oxide V2O5). xV2O5, or lithium polysulfide in place of sulfur). During the first charging procedure of the lithium battery (e.g., as part of the electrochemical formation process), lithium comes out of the cathode active material, migrates to the anode side, and is deposited on the anode current collector. The presence of the highly elastic polymer layer of the present invention enables the lithium ions to be uniformly deposited on the surface of the anode current collector. This alternative battery configuration avoids the need for a layer of lithium foil or coating during battery manufacturing. Bare lithium metal is highly sensitive to air moisture and oxygen, and is therefore more challenging to operate in an actual battery manufacturing environment. Lithium is pre-stored in a lithiated (lithium-containing) cathode active material (such as Li x V2O5 and Li2S x ) enables all materials to be safely handled in a practical manufacturing environment. x V2O5 and Li2S x ) are typically not air sensitive.
[0068] The lithium secondary battery of the present invention may contain a variety of cathode active materials. The cathode active material layer may contain a cathode active material selected from an inorganic material, an organic material, a polymer material, or a combination thereof. The inorganic material may be selected from a metal oxide, a metal phosphate, a metal silicide, a metal selenide, a transition metal sulfide, or a combination thereof.
[0069] The inorganic material may be selected from lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium vanadium oxide, lithium mixed metal oxide, lithium iron phosphate, lithium manganese phosphate, lithium vanadium phosphate, lithium mixed metal phosphate, lithium metal silicide, or a combination thereof.
[0070] In certain preferred embodiments, the inorganic material is selected from metal fluorides or metal chlorides, and the metal fluorides or metal chlorides include the group consisting of CoF3, MnF3, FeF3, VF3, VOF3, TiF3, BiF3, NiF2, FeF2, CuF2, CuF, SnF2, AgF, CuCl2, FeCl3, MnCl2, and combinations thereof. In certain preferred embodiments, the inorganic material is selected from lithium transition metal silicates, represented by Li2MSiO4 or Li2Ma x Mb y SiO4, wherein M and Ma are selected from Fe, Mn, Co, Ni, V, or VO; Mb is selected from Fe, Mn, Co, Ni, V, Ti, Al, B, Sn, or Bi; and x+y≤1.
[0071] In certain preferred embodiments, the inorganic material is selected from transition metal dichalcogenides, transition metal trichalcogenides, or combinations thereof. The inorganic material is selected from TiS2, TaS2, MoS2, NbSe3, MnO2, CoO2, iron oxides, vanadium oxides, or combinations thereof.
[0072] The cathode active material layer may contain a metal oxide containing a vanadium oxide selected from the group consisting of VO2, Li x VO2, V2O5, Li x V2O5, V3O8, Li x V3O8、Li x V3O7, V4O9, Li x V4O9, V6O 13 , Li x V6O 13 , its doping type, its derivatives, and combinations thereof, wherein 0.1 <x<5。
[0073] The cathode active material layer may contain a metal oxide or a metal phosphate, wherein the metal oxide or the metal phosphate is selected from a layered compound LiMO2, a spinel compound LiM2O4, an olivine compound LiMPO4, a silicate compound Li2MSiO4, a hydroxyphospholipid iron compound LiMPO4F, a borate compound LiMBO3, or a combination thereof, wherein M is a transition metal or a mixture of multiple transition metals.
[0074] In some embodiments, the inorganic material is selected from: (a) bismuth selenide or bismuth telluride, (b) dichalcogenides or trichalcogenides of transition metals, (c) niobium, zirconium, molybdenum, hafnium, tantalum, tungsten, titanium, cobalt, manganese, iron, nickel, or sulfides, selenides, or tellurides of transition metals; (d) boron nitride, or (e) combinations thereof.
[0075] The cathode active material layer may contain an organic material or a polymer material, wherein the organic material or the polymer material is selected from poly(anthraquinone sulfide) (PAQS), lithium oxycarbon, 3,4,9,10-perylenetetracarboxylic acid dianhydride (PTCDA), poly(anthraquinone sulfide), pyrene-4,5,9,10-tetraketone (PYT), polymer-bound PYT, quinone (triazene), redox-active organic material, tetracyanoquinodimethane (TCNQ), tetracyanoethylene (TCNE), 2,3,6,7,10,11-hexamethoxytriphenylene (HMTP), poly(5-amino-1,4-dihydroxyanthraquinone) (PADAQ), phosphazene disulfide polymer ([(NPS2)3]n), lithiated 1,4,5,8-naphthalene tetraol formaldehyde polymer, hexaazatrinaphthalene (HATN) , hexaazatriphenylene hexacarbonitrile (HAT(CN)6), 5-benzylidene hydantoin, isatin lithium salt, pyromellitic acid diimide lithium salt, tetrahydroxy-p-benzoquinone derivative (THQLi4), N,N'-diphenyl-2,3,5,6-tetraketopiperazine (PHP), N,N'-diallyl-2,3,5,6-tetraketopiperazine (AP), N,N'-dipropyl-2,3,5,6-tetraketopiperazine (PRP), thioether polymer, quinone compound, 1,4-benzoquinone, 5,7,12,14-pentacenetetraone (PT), 5-amino-2,3-dihydro-1,4-dihydroxyanthraquinone (ADDAQ), 5-amino-1,4-dihydroxyanthraquinone (ADAQ), quinone-type calixarene, Li4C6O6, Li2C6O6, Li6C6O6, or a combination thereof.
[0076] The thioether polymer is selected from poly[methylenethiocyanate-tetrakis(thiomethyl)] (PMTTM), poly(2,4-dithiopentene) (PDTP), a polymer containing poly(ethylene-1,1,2,2-tetrathiol) (PETT) as a main chain thioether polymer, a side chain thioether polymer having a main chain composed of a conjugated aromatic portion and having a thioether side chain as a side chain, poly(2-phenyl-1,3-dithiolane) (PPDT), poly(1,4-di(1,3-dithiolan-2-yl)benzene) (PDDTB), poly(tetrahydrobenzodithiophene) (PTHBDT), poly[1,2,4,5-tetrakis(propylthio)benzene] (PTKPTB) or poly[3,4(ethylenedithio)thiophene] (PEDTT).
[0077] In other embodiments, the cathode active material layer contains an organic material, and the organic material is selected from phthalocyanine compounds, such as copper phthalocyanine, zinc phthalocyanine, tin phthalocyanine, iron phthalocyanine, lead phthalocyanine, nickel phthalocyanine, vanadium phthalocyanine, fluorochromium phthalocyanine, magnesium phthalocyanine, manganese phthalocyanine, dilithium phthalocyanine, aluminum phthalocyanine chloride, cadmium phthalocyanine, chlorogallium phthalocyanine, cobalt phthalocyanine, silver phthalocyanine, metal-free phthalocyanine, their chemical derivatives, or combinations thereof.
[0078] The lithium secondary battery can be a lithium-sulfur battery, wherein the cathode comprises sulfur, sulfur-containing molecules, sulfur-containing compounds, metal sulfides, sulfur-carbon polymers, lithium polysulfides, sulfur / carbon hybrids or composites, sulfur / graphite hybrids or composites, sulfur / graphene hybrids or composites, sulfur-polymer compounds, or combinations thereof.
[0079] In the rechargeable lithium-sulfur battery, the metal sulfide may contain M x S y A material represented by wherein x is an integer from 1 to 3 and y is an integer from 1 to 10, and M is a metal element selected from an alkali metal, an alkaline earth metal selected from Mg or Ca, a transition metal, a metal from Group 13 to Group 17 of the periodic table, or a combination thereof. The metal element M is preferably selected from Li, Na, K, Mg, Zn, Cu, Ti, Ni, Co, Fe, or Al. In some preferred embodiments, the metal sulfide in the cathode layer contains Li2S1, Li2S2, Li2S3, Li2S4, Li2S5, Li2S6, Li2S7, Li2S8, Li2S9, Li2S 10 , or a combination thereof.
[0080] Preferably and typically, the highly elastic polymer has a 5 S / cm, more preferably not less than 10- 4 S / cm, preferably not less than 10- 3 S / cm, and most preferably not less than 10- 2 S / cm lithium ion conductivity. In some embodiments, the highly elastic polymer is a pure polymer without additives or fillers dispersed therein. In other embodiments, the highly elastic polymer is a polymer matrix composite containing from 0.1% to 50% (preferably 1% to 35%) by weight of lithium ion conductive additives dispersed in a highly elastic polymer matrix material. The highly elastic polymer must have high elasticity (elastic deformation strain value>2%). Elastic deformation is a fully recoverable deformation, and the recovery process is essentially instantaneous (without significant time delay). The highly elastic polymer can exhibit elastic deformation from 5% up to 1,000% (10 times its original length), more typically from 10% to 800%, and further more typically from 50% to 500%, and most typically and desirably from 70% to 300%. It can be noted that although metals typically have high ductility (i.e., can be extended to a large extent without breakage), most of the deformation is plastic deformation (irrecoverable) and there is only a small amount of elastic deformation (typically <1%, and more typically <0.2%).
[0081] In some preferred embodiments, the highly elastic polymer contains a lightly cross-linked polymer chain network having ether bonds, nitrile-derived bonds, benzoyl peroxide-derived bonds, ethylene oxide bonds, propylene oxide bonds, vinyl alcohol bonds, cyano-resin bonds, triacrylate monomer-derived bonds, tetraacrylate monomer-derived bonds, or combinations thereof in the cross-linked polymer chain network. These networks or cross-linked polymers exhibit a unique combination of high elasticity (high elastic deformation strain) and high lithium ion conductivity.
[0082] In certain preferred embodiments, the elastomeric polymer contains a lightly cross-linked polymer chain network selected from nitrile-containing polyvinyl alcohol chains, cyanoresin chains, pentaerythritol tetraacrylate (PETEA) chains, pentaerythritol triacrylate chains, ethoxylated trimethylolpropane triacrylate (ETPTA) chains, ethylene glycol methyl ether acrylate (EGMEA) chains, or combinations thereof.
[0083] Typically, the highly elastic polymer is initially in a monomer or oligomer state, which can be cured to form a highly elastic cross-linked polymer. Before curing, these polymers or oligomers are soluble in an organic solvent to form a polymer solution. An ion-conducting additive or an electron-conducting additive can be added to this solution to form a suspension. This solution or suspension can then be formed into a thin layer of a polymer precursor on the surface of the anode current collector. The polymer precursor (monomer or oligomer and initiator) is then polymerized and cured to form a slightly cross-linked polymer. This polymer thin layer can be temporarily deposited on a solid substrate (e.g., the surface of a polymer or glass), dried, and separated from the substrate to become a free-standing polymer layer. This free-standing layer is then laid on a lithium foil / coating or implemented between a lithium film / coating and an electrolyte or separator. The polymer layer formation can be completed by using one of several procedures well known in the art; for example, spraying, painting, printing, coating, extrusion-based film forming, casting, etc.
[0084] For example, ethoxylated trimethylolpropane triacrylate monomer (ETPTA, Mw=428, chemical formula given below) can be dissolved in an organic solvent such as ethylene carbonate (EC) or diethyl carbonate (DEC) together with an initiator. The ETPTA monomer / solvent / initiator solution can then be cast to form an ETPTA monomer / initiator layer on the glass surface. The layer can then be thermally cured to obtain a thin layer of a highly elastic polymer. The polymerization and crosslinking reactions of this monomer can be initiated by a free radical initiator derived from benzoyl peroxide (BPO) or AIBN through thermal decomposition of the initiator molecule. The ETPTA monomer has the following chemical formula:
[0085]
[0086] As another example, the highly elastic polymer for anode lithium foil / coating protection can be based on the cationic polymerization and cross-linking of cyanoethyl polyvinyl alcohol (PVA-CN, Formula 2) in succinonitrile (SN).
[0087]
[0088] The procedure can start with dissolving PVA-CN in succinonitrile (NCCH2CH2CN) to form a mixture solution. This is followed by adding an initiator to the mixture solution. For example, LiPF6 can be added to the PVA-CN / SN mixture solution at a certain weight ratio (selected from a preferred range of 20:1 to 2:1) to form a precursor solution. Then, the solution can be deposited to form a thin layer of the reaction material PVA-CN / LiPF6, and then the reaction material is heated at a certain temperature (e.g., from 75°C to 100°C) for 2 to 8 hours to obtain a highly elastic polymer. During this process, cationic polymerization and crosslinking of cyano groups on PVA-CN can be initiated by PF5 (which is produced by the thermal decomposition of LiPF6 at such a high temperature).
[0089] For these materials, it is necessary to form a lightly cross-linked polymer chain network. In other words, the network polymer or cross-linked polymer should have a relatively low degree of cross-linking or low cross-linking density to impart high elastic deformation.
[0090] The crosslink density of a crosslinked polymer chain network can be defined as the reciprocal of the molecular weight between crosslinks (Mc). The crosslink density can be determined by the following equation: Mc = ρRT / Ge, where Ge is the equilibrium modulus as determined by temperature sweep in dynamic mechanical analysis, ρ is the physical density, R is the universal gas constant in J / mol*K, and T is the absolute temperature in K. Once Ge and ρ are determined experimentally, Mc and the crosslink density can be calculated.
[0091] The size of Mc can be normalized by dividing the Mc value by the molecular weight of the characteristic repeating unit in the cross-linked chain or chain bond to obtain the numerical value Nc, which is the number of repeating units between two cross-linking points. We have found that the elastic deformation strain is very well related to Mc and Nc. The elasticity of cross-linked polymers comes from a large number of repeating units (large Nc) between cross-links. When the polymer is not stressed, the repeating unit can present a more relaxed conformation (such as random coil). However, when the polymer is subjected to mechanical stress, the bond chain unfolds or is stretched to provide a large deformation. The long chain bond (larger Nc) between the cross-linking points makes it possible to have a larger elastic deformation. After releasing the load, the bond chain returns to a more relaxed or curled state. During the mechanical loading of the polymer, cross-linking prevents the chain from sliding, otherwise plastic deformation (irrecoverable) will be formed.
[0092] Preferably, the Nc value in the highly elastic polymer is greater than 5, more preferably greater than 10, further more preferably greater than 100, and even more preferably greater than 200. These Nc values can be easily controlled and varied to obtain different elastic deformation values by using different cross-linking agents with different functional groups and by designing the polymerization and cross-linking reactions to be performed at different temperatures for different time periods.
[0093] Alternatively, the Mooney-Rilvin method can be used to determine the degree of crosslinking. Crosslinking can also be measured by swelling experiments. In swelling experiments, the crosslinked sample is placed in a good solvent for the corresponding linear polymer at a specific temperature, and mass change or volume change is measured. The higher the degree of crosslinking, the smaller the swelling that can be obtained. Based on the degree of swelling, Flory Interaction Parameter (Flory Interaction Parameter) (it relates to the interaction between the solvent and the sample, Flory-Huggins Eq.) and the density of the solvent, the theoretical degree of crosslinking can be calculated according to Flory's Network Theory. Flory-Rehner Equation can be used to determine crosslinking.
[0094] Highly elastic polymers may comprise simultaneous interpenetrating network (SIN) polymers (in which two cross-linked chains are entangled with each other) or semi-interpenetrating network polymers (semi-IPN) (which contain a cross-linked polymer and a linear polymer). An example of a semi-IPN is a UV-curable / polymerizable trivalent / monovalent acrylate mixture composed of ethoxylated trimethylolpropane triacrylate (ETPTA) and ethylene glycol methyl ether acrylate (EGMEA) oligomers. ETPTA with a trivalent vinyl group is a photo (UV) cross-linkable monomer capable of forming a cross-linked chain network. EGMEA with a monovalent vinyl group is also UV polymerizable, resulting in a linear polymer with high flexibility due to the presence of the oligomeric ethylene oxide unit. When the degree of cross-linking of ETPTA is moderate or low, the resulting ETPTA / EGMEA semi-IPN polymer provides good mechanical flexibility or elasticity and reasonable mechanical strength. The lithium ion conductivity of this polymer is 10 -4 S / cm to 5×10 -3 S / cm range.
[0095] The above-mentioned highly elastic polymer can be used alone to protect the lithium foil / coating layer at the anode. Alternatively, the highly elastic polymer can be mixed with various elastomers, conductive polymers, lithium ion conductive materials, and / or reinforcing materials (such as carbon nanotubes, carbon nanofibers or graphene sheets).
[0096] A variety of elastomers can be mixed with a highly elastic polymer to form a blend, copolymer or interpenetrating network that encapsulates the cathode active material particles. The elastomeric material can be selected from: natural polyisoprene (e.g., cis-1,4-polyisoprene natural rubber (NR) and trans-1,4-polyisoprene gutta-percha), synthetic polyisoprene (isoprene rubber, IR), polybutadiene (butadiene rubber, BR), chloroprene rubber (CR), polychloroprene (e.g., Neoprene, Baypren, etc.), butyl rubber (copolymer of isobutylene and isoprene, IIR), including halogenated butyl rubber (chlorobutyl rubber (CIIR) and bromobutyl rubber (BIIR)), styrene-butadiene rubber (copolymer of styrene and butadiene, IIR), and polyisoprene (isoprene rubber, IR). , SBR), nitrile rubber (copolymer of butadiene and acrylonitrile, NBR), EPM (ethylene propylene rubber, copolymer of ethylene and propylene), EPDM rubber (ethylene propylene diene rubber, terpolymer of ethylene, propylene and diene components), epichlorohydrin rubber (ECO), polyacrylic rubber (ACM, ABR), silicone rubber (SI, Q, VMQ), fluorosilicone rubber (FVMQ), fluoroelastomer (FKM, and FEPM; such as Viton, Tecnoflon, Fluorel, Aflas and Dai-El), perfluoroelastomer (FFKM: Tecnoflon PFR, Kalrez, Chemraz, Perlast), polyether block amide (PEBA), chlorosulfonated polyethylene (CSM; such as Hypalon), and ethylene vinyl acetate (EVA), thermoplastic elastomers (TPE), protein elastin, protein elastin, ethylene oxide-epichlorohydrin copolymers, polyurethanes, urethane-urea copolymers, and combinations thereof.
[0097] Urethane-urea copolymer films are typically composed of two types of domains, soft and hard domains. An entangled linear backbone consisting of poly(tetramethylene ether) glycol (PTMEG) units constitutes the soft domains, while repeating methylene diphenyl diisocyanate (MDI) and ethylenediamine (EDA) units constitute the hard domains. Lithium-ion conducting additives can be incorporated into the soft domains or other more amorphous regions.
[0098] In some embodiments, the elastomeric polymer can form a polymer matrix composite containing a lithium ion conductive additive dispersed in a elastomeric polymer matrix material, wherein the lithium ion conductive additive is selected from the group consisting of Li2CO3, Li2O, Li2C2O4, LiOH, LiX, ROCO2Li, HCOLi, ROLi, (ROCO2Li)2, (CH2OCO2Li)2, Li2S, Li x SO y , or a combination thereof, wherein X=F, Cl, I, or Br, R=hydrocarbon, x=0-1, y=1-4.
[0099] In some embodiments, the highly elastic polymer can be mixed with a lithium ion conductive additive, which contains a lithium salt selected from the following: lithium perchlorate LiClO4, lithium hexafluorophosphate LiPF6, lithium fluoroborate LiBF4, lithium hexafluoroarsenide LiAsF6, lithium trifluoromethanesulfonate LiCF3SO3, lithium bistrifluoromethylsulfonyl imide LiN(CF3SO2)2, lithium bis(oxalate)borate LiBOB, lithium difluorooxalatoborate LiBF2C2O4, lithium difluorooxalatoborate LiBF2C2O4, lithium nitrate LiNO3, lithium fluoroalkyl phosphate LiPF3(CF2CF3)3, lithium bisperfluoroethylsulfonyl imide LiBETI, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonyl imide LiTFSI, ionic liquid-based lithium salts, or combinations thereof.
[0100] The highly elastic polymer may form a mixture, a blend, or a semi-interpenetrating network with an electronically conductive polymer selected from polyaniline, polypyrrole, polythiophene, polyfuran, a bicyclic polymer, a derivative thereof (e.g., a sulfonated version), or a combination thereof. In some embodiments, the highly elastic polymer may form a mixture, a copolymer, or a semi-interpenetrating network with a lithium ion conductive polymer selected from poly(ethylene oxide) (PEO), polypropylene oxide (PPO), poly(acrylonitrile) (PAN), poly(methyl methacrylate) (PMMA), poly(vinylidene fluoride) (PVdF), polybismethoxyethoxyethanolate-phosphazene, polyvinyl chloride, polydimethylsiloxane, poly(vinylidene fluoride)-hexafluoropropylene (PVDF-HFP), a derivative thereof (e.g., a sulfonated version), or a combination thereof.
[0101] Unsaturated rubbers that can be mixed with high elastic polymers include natural polyisoprene (such as cis-1,4-polyisoprene natural rubber (NR) and trans-1,4-polyisoprene gutta-percha), synthetic polyisoprene (isoprene rubber, IR), polybutadiene (butadiene rubber, BR), chloroprene rubber (CR), polychloroprene (such as Neoprene, Baypren, etc.), butyl rubber (copolymer of isobutylene and isoprene, IIR), including halogenated butyl rubber (chlorobutyl rubber (CIIR) and bromobutyl rubber (BIIR)), styrene-butadiene rubber (copolymer of styrene and butadiene, SBR), and nitrile rubber (copolymer of butadiene and acrylonitrile, NBR).
[0102] Some elastomers are saturated rubbers that cannot be cured by sulfur vulcanization; they are made into rubbery or elastomeric materials by various means: for example, by having copolymer domains that hold otherwise linear chains together. Each of these elastomers can be used to bind particles of cathode active material by one of several means: for example, spray coating, dilute solution mixing (dissolving cathode active material particles in uncured polymer, monomer, or oligomer (with or without organic solvent)), followed by drying and curing.
[0103] Saturated rubbers and related elastomers in this category include EPM (ethylene propylene rubber, a copolymer of ethylene and propylene), EPDM rubber (ethylene propylene diene rubber, a terpolymer of ethylene, propylene and diene components), epichlorohydrin rubber (ECO), polyacrylic rubber (ACM, ABR), silicone rubber (SI, Q, VMQ), fluorosilicone rubber (FVMQ), fluoroelastomers (FKM, and FEPM; such as Viton, Tecnoflon, Fluorel, Aflas and Dai-El), perfluoroelastomers (FFKM: Tecnoflon PFR, Kalrez, Chemraz, Perlast), polyether block amides (PEBA), chlorosulfonated polyethylene (CSM; such as Hypalon) and ethylene-vinyl acetate (EVA), thermoplastic elastomers (TPE), protein elastin and protein elastin. Polyurethanes and their copolymers (e.g., urea-urethane copolymers) are particularly useful elastomeric shell materials for encapsulating anode active material particles.
[0104] Example 1: Lithium battery containing a lithium anode protected by a highly elastic polymer and a cathode containing V2O5 particles
[0105] The cathode active material layer is prepared by V2O5 particles and V2O5 particles surrounded by graphene, respectively. V2O5 particles are commercially available. V2O5 particles surrounded by graphene are prepared in-house. In a typical experiment, vanadium pentoxide gel is obtained by mixing V2O5 in a LiCl aqueous solution. The Li+ exchange gel obtained by interacting with a LiCl solution (Li:V molar ratio is kept at 1:1) is mixed with a GO suspension and then placed in a stainless steel 35ml autoclave lined with Teflon, sealed, and heated to a maximum of 180°C for 12h. After this hydrothermal treatment, the green solid is collected, thoroughly washed, ultrasonically treated for 2 minutes, and dried at 70°C for 12 hours, then mixed with another 0.1% of GO in water, ultrasonically treated to decompose the nanobelt size, and then spray-dried at 200°C to obtain V2O5 composite particles surrounded by graphene. A selected amount of V2O5 particles and graphene-surrounded V2O5 particles are then each separately formed into a cathode layer following a well-known slurry coating process.
[0106] Ethoxylated trimethylolpropane triacrylate monomer (ETPTA, Mw=428, Sigma-Aldrich) was dissolved in a solvent mixture of ethylene carbonate (EC) / diethyl carbonate (DEC) at a composition ratio of 3 / 97 (w / w) ETPTA / solvent on a weight basis. Subsequently, benzoyl peroxide (BPO, 1.0 wt.% relative to the ETPTA content) was added as a free radical initiator to allow a thermal crosslinking reaction after deposition on the lithium foil surface. This layer of ETPTA monomer / initiator was then thermally cured at 60° C. for 30 min to obtain a protective layer.
[0107] On a separate basis, a certain amount of ETPTA monomer / solvent / initiator solution was cast onto a glass surface to form a wet film, which was heat dried and then cured at 60°C for 30 minutes to form a cross-linked polymer film. In this experiment, the weight ratio of BPO / ETPTA was varied from 0.1% to 4% to change the degree of cross-linking of several different polymer films. Some of the cured polymer samples were subjected to dynamic mechanical testing to obtain the equilibrium dynamic modulus Ge to determine the number average molecular weight (Mc) and the corresponding number of repeating units (Nc) between two cross-linking points as a means of characterizing the degree of cross-linking. A typical and preferred number of repeating units (Nc) is from 5 to 5,000, more preferably from 10 to 1,000, further preferably from 20 to 500, and most preferably from 50 to 500.
[0108] Several tensile test specimens were cut from each crosslinked film and tested using a universal testing machine. Representative tensile stress-strain curves for four BPO-initiated crosslinked ETPTA polymers are shown in FIG. 3(A), which show that this series of network polymers have elastic deformations from about 230% to 700%. The above values are for pure polymers without any additives. Addition of up to 30% by weight of lithium salts typically reduces this elasticity to a reversible tensile strain in the range of 10% to 100%.
[0109] For electrochemical testing, the working electrode (cathode layer) was prepared by mixing 85wt.% of VO or 88% of graphene-surrounded VO particles, 5-8wt.% of CNTs, and 7wt.% of polyvinylidene fluoride (PVDF) binder dissolved in N-methyl-2-pyrrolidone (NMP) to form a slurry with a total solid content of 5wt.%. After coating the slurry on Al foil, the electrode was dried in vacuum at 120°C for 2h to remove the solvent before pressing. Then, the electrode was cut into discs (φ=12mm) and dried under vacuum at 100°C for 24h.
[0110] Electrochemical measurements were performed using CR2032 (3 V) coin cells with lithium metal as counter / reference electrode, Celgard 2400 membrane as separator, and 1 M LiPF6 electrolyte solution dissolved in a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) (EC-DEC, 1:1 v / v). Cell assembly was performed in an argon-filled glove box. CV measurements were performed using a CH-6 electrochemical workstation at a scan rate of 1 mV / s. The electrochemical performance of cells characterized by a highly elastic polymer binder and cells containing a PVDF binder were evaluated at a current density of 50 mA / g by constant current charge / discharge cycles using an Arbin electrochemical workstation.
[0111] Summarized in FIG3(B) are intercalation specific capacity curves for four lithium cells: two cells each having a cathode containing V2O5 particles (one cell having a lithium metal anode protection layer based on a cross-linked ETPTA polymer and the other not) and two cells each having a cathode containing V2O5 particles surrounded by graphene (one cell having a lithium anode protection layer based on a cross-linked ETPTA polymer and the other not). The specific capacity of the unprotected cell decreases at the fastest rate as the number of cycles increases. In contrast, the cross-linked ETPTA polymer protection layer of the present invention provides a battery cell with a significantly more stable and high specific capacity for many cycles. These data have clearly demonstrated the unexpected and superior performance of the cross-linked ETPTA polymer protection approach of the present invention.
[0112] The highly elastic cross-linked ETPTA polymer protective layer appears to be able to reversibly deform to a large extent without breakage when the thickness of the lithium foil is reduced during battery discharge. The protective polymer layer also prevents continued reaction between the liquid electrolyte and the lithium metal at the anode, thereby reducing the problem of continued loss of lithium and electrolyte. This also enables significantly more uniform deposition of lithium ions when they return from the cathode during battery recharge; therefore, there are no lithium dendrites. These were observed by examining the surface of electrodes recovered from battery cells after some number of charge-discharge cycles using SEM.
[0113] Example 2: Implementation of a highly elastic polymer in the anode of a lithium-LiCoO2 cell (the cell initially contains no lithium)
[0114] The highly elastic polymer for anode protection is based on the cationic polymerization and crosslinking of cyanoethyl polyvinyl alcohol (PVA-CN) in succinonitrile (SN). The procedure begins with dissolving PVA-CN in succinonitrile to form a mixture solution. This step is followed by adding an initiator to the solution. For the purpose of incorporating some lithium substances into the highly elastic polymer, we choose to use LiPF6 as an initiator. The ratio between LiPF6 and the PVA-CN / SN mixture solution varies from 1 / 20 to 1 / 2 by weight to form a series of precursor solutions. Subsequently, these solutions are spray-deposited onto the surface of lithium foil to form a thin layer of precursor reactive substances. The precursor reactive substances are then heated at a temperature of from 75°C to 100°C for 2 to 8 hours to obtain a layer of highly elastic polymer adhered to the surface of lithium foil.
[0115] Additionally, the reaction mass PVA-CN / LiPF6 was cast onto a glass surface to form several films, which were polymerized and cross-linked to obtain cross-linked polymers with different cross-linking degrees. These films were also subjected to tensile tests, and some of the test results are summarized in FIG4(a). This series of cross-linked polymers can be elastically stretched up to about 80% (higher cross-linking degree) to 400% (lower cross-linking degree).
[0116] Figure 4(B) shows that the cell with the polymer layer protecting the anode provides significantly more stable cycling behavior. The highly elastic polymer also serves to isolate the electrolyte from the lithium coating, while still allowing lithium ions to diffuse easily.
[0117] Example 3: Li metal cell with a cathode based on metal fluoride nanoparticles and a lithium anode protected by a highly elastic polymer based on PETEA
[0118] For the anode lithium metal protection layer, pentaerythritol tetraacrylate (PETEA) (Formula 3) was used as the monomer:
[0119]
[0120] In a representative procedure, the precursor solution consisted of 1.5 wt.% PETEA (C 17 H 20 O8) monomer and 0.1wt.% azobisisobutyronitrile (AIBN, C8H 12 N4) Initiator composition: The PETEA / AIBN precursor solution was cast onto the lithium metal layer pre-deposited on the Cu foil surface to form a precursor film, which was polymerized and cured at 70° C. for half an hour to obtain a lightly cross-linked polymer.
[0121] Additionally, the reaction mass PETEA / AIBN (without conductive additives) was cast onto a glass surface to form several films, which were polymerized and cured to obtain crosslinked polymers with different crosslinking degrees. These films were also subjected to tensile tests, and some of the test results are summarized in FIG5(A). This series of crosslinked polymers can be elastically stretched up to about 25% (higher crosslinking degree) to 80% (lower crosslinking degree).
[0122] Commercially available CoF3, MnF3, FeF3, VF3, VOF3, TiF3, and BiF3 powders were subjected to high intensity ball milling to reduce the particle size to approximately 0.5-2.3 μm. Each type of these metal fluoride particles was then added to a NMP and PVDF binder suspension along with graphene sheets (as a conductive additive) to form a multi-component slurry. The slurry was then slurried onto Al foil to form the cathode layer.
[0123] Shown in Figure 5(b) are the discharge capacity curves of two coin cells with the same cathode active material (FeF3), but one cell has a highly elastic polymer protected anode and the other has no protective layer. These results have clearly demonstrated that the highly elastic polymer protection strategy provides excellent protection against capacity fade of lithium metal batteries.
[0124] The highly elastic polymer appears to be able to deform reversibly without breakage when the anode layer expands and contracts during charge and discharge. The polymer also prevents continued reaction between the liquid electrolyte and the lithium metal. No dendrite-like features were found in the case where the anode was protected by the highly elastic polymer. This was confirmed by examining the surface of the electrodes recovered from the battery cells after some number of charge-discharge cycles using SEM.
[0125] Example 4: Li organic cell containing FePc / RGO hybrid microparticle cathode and highly elastic polymer protected Li foil anode
[0126] Particles of combined FePc / graphene sheets were obtained by ball milling a mixture of FePc and RGO in a milling chamber for 30 minutes. The resulting FePc / RGO mixture particles were potato-shaped. Some of these mixture particles were encapsulated by UHMW PAN polymer using a pan coating procedure. Two lithium batteries were prepared, each containing a Li foil anode, a porous separator, and a cathode layer of FePc / RGO particles (encapsulated or unencapsulated).
[0127] For the preparation of ETPTA semi-IPN polymer, ETPTA (Mw = 428 g / mol, trivalent acrylate monomer), EGMEA (Mw = 482 g / mol, monovalent acrylate oligomer), and 2-hydroxy-2-methyl-1-phenyl-1-propanone (HMPP, photoinitiator) were dissolved in a solvent (propylene carbonate, PC) to form a solution. The weight ratio between HMPP and the ETPTA / EGMEA mixture was varied from 0.2% to 2%. The ETPTA / EGMEA ratio in the solution was varied from 1% to 5% to produce different anode protection layer thicknesses. The ETPTA / EGMEA ratio in the acrylate mixture was varied from 10 / 0 to 1 / 9.
[0128] The cycling behavior of these two lithium batteries is Figure 6 , which shows that lithium-organic cells with a highly elastic polymer protective layer in the anode exhibit significantly more stable cycling response. This protective polymer reduces or eliminates the continuous contact between the lithium metal and the electrolyte, but the polymer layer itself is still in ionic contact with the lithium metal and is permeable to lithium ions. This approach has significantly increased the cycle life of all lithium-organic batteries.
[0129] Example 5: Li-S battery cell containing an anode protective layer and a cathode containing sulfur-impregnated activated carbon particles
[0130] One way to combine sulfur with conductive materials such as carbon / graphite particles is to use a solution or melt mixing process. Highly porous activated carbon particles, chemically etched mesocarbon microbeads (activated MCMB) and expanded graphite worms are mixed with sulfur melt at 117°C-120°C (slightly above the melting point of S (115.2°C)) for 10-60 minutes to obtain sulfur-impregnated carbon particles.
[0131] Figure 7 The cathode specific capacity values of two Li-S cells with cathode active materials based on S-impregnated activated MCMB are shown: one cell with a cross-linked ETPTA-protected anode and the other cell without an anode protection layer. Apparently, the lightly cross-linked ETPTA polymer layer implemented at the anode is highly beneficial for the cycling stability of Li-S cells.
[0132] Example 6: Li-S battery cell containing an anode protection layer and a cathode containing sulfur-coated graphene sheets
[0133] The cathode preparation procedure involves generating a vapor of elemental sulfur, causing the S vapor to be deposited on the surface of a monolayer or few-layer graphene sheet. As a first step, a graphene sheet suspended in a liquid medium (e.g., graphene oxide in water or graphene in NMP) is sprayed on a substrate (e.g., a glass surface) to form a thin layer of graphene sheets. This graphene thin layer is then exposed to physical vapor deposition produced by sublimation. The sublimation of solid sulfur occurs at temperatures greater than 40°C, but a meaningful and practically useful sublimation rate typically does not occur until the temperature is above 100°C. We typically use 117°C-160°C, with a vapor deposition time of 10-120 minutes, to deposit a thin film of sulfur on the graphene surface (sulfur thickness is about from 1nm to 10nm). This graphene thin layer with a thin film of sulfur deposited thereon is then easily broken into sheets of S-coated graphene sheets using an air jet mill. These S-coated graphene sheets were made into secondary particles of about 5-15 μm in diameter (e.g., by spray drying) and then encapsulated by UHMW PAN polymer. These encapsulated microparticles were made into cathode electrodes using conventional slurry coating procedures.
[0134] Figure 8 The cathode specific capacity values of two Li-S cells with cathode active materials based on S / graphene hybrids and lithium foil anodes with or without a highly elastic PETEA protective layer are summarized in . These data have further demonstrated the effectiveness of the highly elastic polymer layer protection approach.
[0135] Example 7: Effect of lithium ion conductive additives in highly elastic polymers
[0136] A variety of lithium ion conductive additives were added to several different polymer matrix materials to prepare anode protection layers. The lithium ion conductivity values of the resulting polymer / salt complex materials are summarized in Table 1 below. We have found that these polymer composites are suitable anode protection layer materials, provided that their lithium ion conductivity at room temperature is not less than 10- 6 S / cm. With these materials, lithium ions appear to be able to diffuse easily through a protective layer having a thickness of no more than 1 μm. For thicker polymer films (e.g., 10 μm), these highly elastic polymers would require a thermal conductivity of no less than 10-10 μm at room temperature. 4 Lithium ion conductivity of S / cm.
[0137] Table 1: Lithium ion conductivity of various highly elastic polymer composite compositions as shell materials for protecting anode active material particles.
[0138]
[0139]
[0140] Example 8: Cycling stability of various rechargeable lithium battery cells
[0141] In the lithium-ion battery industry, it is common practice to define the cycle life of a battery as the number of charge-discharge cycles at which the battery suffers 20% capacity fade based on the initial capacity measured after the desired electrochemical formation. Summarized in Table 2 below are cycle life data for various batteries featuring anodes with or without a polymer layer protecting the anode.
[0142] Table 2: Cycle life data for various lithium secondary (rechargeable) batteries.
[0143]
[0144]
[0145] In summary, the anode protection layer strategy based on highly elastic polymers is unexpectedly effective in alleviating the problems of lithium metal dendrite formation and lithium metal-electrolyte reaction, which otherwise lead to capacity decay and potential internal short circuits and explosions of lithium secondary batteries. The highly elastic polymer can expand or shrink accordingly or in unison with the anode layer. This ability helps maintain good contact between the current collector (or the lithium film itself) and the protective layer, so that lithium ions can be uniformly re-deposited without interruption.
Claims
1. A lithium secondary battery, comprising a cathode, an anode, and an electrolyte or a separator-electrolyte assembly arranged between the cathode and the anode, wherein the cathode comprises a cathode active material, the cathode active material is selected from an inorganic material, an organic material, and a combination thereof, and the inorganic material does not include sulfur or alkali metal polysulfide, The anode comprises: a) foil or coating of lithium or lithium alloy as anode active material; as well as b) a thin layer of a highly elastic polymer having a recoverable tensile strain of from 2% to 700%, a tensile strength of not less than 10 -6 S / cm, and a thickness from 1 nm to less than 10 nm, wherein the thin layer of highly elastic polymer comprises an ultra-high molecular weight polymer and an elastomer, and the thin layer of highly elastic polymer is disposed between the foil or coating of the lithium or lithium alloy and the electrolyte or separator-electrolyte assembly, wherein the formation of lithium metal dendrites is eliminated; The highly elastic polymer contains a cross-linked polymer chain network selected from nitrile-containing polyvinyl alcohol chains, cyanoresin chains, pentaerythritol tetraacrylate chains, pentaerythritol triacrylate chains, ethoxylated trimethylolpropane triacrylate (ETPTA) chains, ethylene glycol methyl ether acrylate (EGMEA) chains, and combinations thereof.
2. The lithium secondary battery according to claim 1, wherein The highly elastic polymer contains from 0.1% to 50% by weight of a lithium ion conductive additive dispersed therein, or contains from 0.1% by weight to 10% by weight of a reinforcing nanofilament selected from carbon nanotubes, carbon nanofibers, graphene, and combinations thereof.
3. The lithium secondary battery according to claim 1, wherein The highly elastic polymer is mixed with a lithium ion conductive additive to form a composite, wherein the lithium ion conductive additive is dispersed in the highly elastic polymer and is selected from Li2CO3, Li2O, Li2C2O4, LiOH, LiX, ROCO2Li, HCOLi, ROLi, (ROCO2Li)2, (CH2OCO2Li)2, Li2S, Li x SO y , and combinations thereof, wherein X=F, Cl, I, or Br, R=hydrocarbon group, 0≤x≤1, 1≤y≤4.
4. The lithium secondary battery according to claim 1, wherein The highly elastic polymer further contains a conductive material dispersed therein, and the conductive material is selected from electron conductive polymers, metal particles, metal wires, graphene sheets, carbon fibers, carbon nanotubes, graphite particles, expanded graphite flakes, acetylene black particles, and combinations thereof.
5. The lithium secondary battery according to claim 4, wherein: The conductive material has a thickness or diameter of less than 100 nm.
6. The lithium secondary battery according to claim 1, wherein The highly elastic polymer further contains a lithium salt dispersed therein, and the lithium salt is selected from lithium perchlorate LiClO4, lithium hexafluorophosphate LiPF6, lithium fluoroborate LiBF4, lithium hexafluoroarsenide LiAsF6, lithium trifluoromethanesulfonate LiCF3SO3, lithium bistrifluoromethylsulfonyl imide LiN(CF3SO2)2, lithium bis(oxalate)borate LiBOB, lithium difluorooxalatoborate LiBF2C2O4, lithium nitrate LiNO3, lithium fluoroalkyl phosphate LiPF3(CF2CF3)3, lithium bisperfluoroethylsulfonyl imide LiBETI, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonyl imide LiTFSI, ionic liquid-based lithium salts, and combinations thereof.
7. The lithium secondary battery according to claim 1, wherein The highly elastic polymer is mixed with an electron conductive polymer selected from the group consisting of polyaniline, polypyrrole, polythiophene, polyfuran, bicyclic polymers, sulfonated derivatives thereof, and combinations thereof.
8. The lithium secondary battery according to claim 1, wherein The highly elastic polymer forms a mixture or blend with a lithium ion conductive polymer, and the lithium ion conductive polymer is selected from poly(ethylene oxide) (PEO), polypropylene oxide (PPO), poly(acrylonitrile) (PAN), poly(methyl methacrylate) (PMMA), poly(vinylidene fluoride) (PVdF), polybismethoxyethoxyethanol salt-phosphazene, polyvinyl chloride, polydimethylsiloxane, poly(vinylidene fluoride)-hexafluoropropylene (PVDF-HFP), sulfonated derivatives thereof, and combinations thereof.
9. The lithium secondary battery according to claim 1, wherein: The highly elastic polymer has a -4 S / cm to 10 -2 Lithium ion conductivity of S / cm.
10. The lithium secondary battery according to claim 1, wherein The inorganic material is selected from metal oxides, metal phosphates, metal silicides, metal selenides, transition metal sulfides, and combinations thereof.
11. The lithium secondary battery according to claim 1, wherein The inorganic material is selected from lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium vanadium oxide, lithium mixed metal oxide, lithium iron phosphate, lithium manganese phosphate, lithium vanadium phosphate, lithium mixed metal phosphate, lithium metal silicide, and combinations thereof.
12. The lithium secondary battery according to claim 1, wherein The inorganic material is selected from metal fluorides or metal chlorides, and the metal fluorides or metal chlorides include the group consisting of: CoF3, MnF3, FeF3, VF3, VOF3, TiF3, BiF3, NiF2, FeF2, CuF2, CuF, SnF2, AgF, CuCl2, FeCl3, MnCl2, and combinations thereof.
13. The lithium secondary battery according to claim 1, wherein: The inorganic material is selected from lithium transition metal silicates, represented by Li2MSiO4 or Li2Ma x Mb y SiO4, wherein M and Ma are selected from Fe, Mn, Co, Ni, V, or VO; Mb is selected from Fe, Mn, Co, Ni, V, Ti, Al, B, Sn, or Bi; and x+y≤1.
14. The lithium secondary battery according to claim 1, wherein The inorganic material is selected from transition metal dichalcogenides, transition metal trichalcogenides, and combinations thereof.
15. The lithium secondary battery according to claim 1, wherein: The inorganic material is selected from TiS2, TaS2, MoS2, NbSe3, MnO2, CoO2, iron oxide, vanadium oxide, and combinations thereof.
16. The lithium secondary battery according to claim 10, wherein: The metal oxide contains vanadium oxide selected from the group consisting of VO2, Li x VO2, V2O5, Li x V2O5, V3O8, Li x V3O8、Li x V3O7, V4O9, Li x V4O9, V6O 13 , Li x V6O 13 , and their combinations, where 0.1 <x<5。 17. The lithium secondary battery according to claim 10, wherein: The metal oxide or metal phosphate is selected from layered compounds LiMO2, spinel compounds LiM2O4, olivine compounds LiMPO4, silicate compounds Li2MSiO4, hydroxyphosphite compounds LiMPO4F, borate compounds LiMBO3, and combinations thereof, wherein M is a transition metal or a mixture of multiple transition metals.
18. The lithium secondary battery according to claim 10, wherein: The inorganic material is selected from: (a) bismuth selenide or bismuth telluride, (b) dichalcogenides or trichalcogenides of transition metals, (c) selenides or tellurides of niobium, zirconium, molybdenum, hafnium, tantalum, tungsten, titanium, cobalt, manganese, iron, or nickel; (d) boron nitride, and (e) combinations thereof.
19. The lithium secondary battery according to claim 1, wherein: The organic material is selected from poly(anthraquinone sulfide) (PAQS), 3,4,9,10-perylenetetracarboxylic dianhydride (PTCDA), pyrene-4,5,9,10-tetraketone (PYT), quinone (triazene), redox-active organic material, tetracyanoquinodimethane (TCNQ), tetracyanoethylene (TCNE), 2,3,6,7,10,11-hexamethoxytriphenylene (HMTP), poly(5-amino-1,4-dihydroxyanthraquinone) (PADAQ), phosphazene disulfide polymer ([(NPS2)3]n), lithiated 1,4,5,8-naphthalene tetraol formaldehyde polymer, hexaazatrinaphthalene (HATN), hexaazatriphenylene hexanitrile (HAT(CN)6), 5 -benzylidene hydantoin, isatin lithium salt, pyromellitic acid diimide lithium salt, tetrahydroxy-p-benzoquinone derivative (THQLi4), N,N'-diphenyl-2,3,5,6-tetraketopiperazine (PHP), N,N'-diallyl-2,3,5,6-tetraketopiperazine (AP), N,N'-dipropyl-2,3,5,6-tetraketopiperazine (PRP), 1,4-benzoquinone, 5,7,12,14-pentacenetetraone (PT), 5-amino-2,3-dihydro-1,4-dihydroxyanthraquinone (ADDAQ), 5-amino-1,4-dihydroxyanthraquinone (ADAQ), quinone-type calixarene, Li4C6O6, Li2C6O6, Li6C6O6, and combinations thereof.
20. The lithium secondary battery according to claim 1, wherein The organic material is selected from thioether polymers, and the thioether polymer is selected from poly[methylenethiocyanate-tetrakis(thiomethylene)] (PMTTM), poly(2,4-dithiopentene) (PDTP), a polymer containing poly(ethylene-1,1,2,2-tetrathiol) (PETT) as a main chain thioether polymer, a side chain thioether polymer having a main chain composed of a conjugated aromatic portion and having a thioether side chain as a side chain, poly(2-phenyl-1,3-dithiolane) (PPDT), poly(1,4-di(1,3-dithiolan-2-yl)benzene) (PDDTB), poly(tetrahydrobenzodithiophene) (PTHBDT), poly[1,2,4,5-tetrakis(propylthio)benzene] (PTKPTB), or poly[3,4(ethylenedithio)thiophene] (PEDTT).
21. The lithium secondary battery according to claim 1, wherein The organic material contains a phthalocyanine compound selected from the group consisting of copper phthalocyanine, zinc phthalocyanine, tin phthalocyanine, iron phthalocyanine, lead phthalocyanine, nickel phthalocyanine, vanadium phthalocyanine, fluorochromium phthalocyanine, magnesium phthalocyanine, manganese phthalocyanine, dilithium phthalocyanine, aluminum phthalocyanine chloride, cadmium phthalocyanine, chlorogallium phthalocyanine, cobalt phthalocyanine, silver phthalocyanine, metal-free phthalocyanine, and combinations thereof.
22. The lithium secondary battery according to claim 1, wherein: The cathode active material is in the form of nanoparticles, nanowires, nanofibers, nanotubes, nanosheets, nanobelts, nanodisks, nanoplatelets, or nanohorns having a thickness or diameter of from 0.5 nm to 100 nm.
23. The lithium secondary battery according to claim 22, wherein: The nanoparticles, nanowires, nanofibers, nanotubes, nanosheets, nanobelts, nanodisks, nanoplatelets, or nanohorns are coated or surrounded by a conductive protective coating selected from a carbon material, an electronically conductive polymer, a conductive metal oxide, or a conductive metal coating.
24. The lithium secondary battery according to claim 1, wherein: The highly elastic polymer is a pure polymer without additives or fillers dispersed therein.
25. The lithium secondary battery of claim 1, wherein the lithium secondary battery is a lithium-sulfur battery, wherein the cathode comprises sulfur, sulfur-containing molecules, metal sulfides, sulfur-carbon polymers, lithium polysulfides, sulfur / carbon hybrids or composites, sulfur-polymer compounds, and combinations thereof. 26 . The lithium secondary battery of claim 1 , wherein the lithium secondary battery is a lithium metal battery, a lithium-sulfur battery, a lithium-selenium battery, or a lithium-air battery.
27. A method for manufacturing a lithium battery, the method comprising: (a) providing a cathode active material layer; (b) providing lithium metal or lithium alloy foil or coating; (c) providing electrolytes; as well as (d) providing an anode protective layer of a highly elastic polymer disposed between the lithium metal or lithium alloy foil or coating and the electrolyte, wherein providing the anode protective layer of the highly elastic polymer comprises providing an ultra-high molecular weight polymer and an elastomer; wherein the cathode active material is selected from inorganic materials, organic materials, and combinations thereof, and the inorganic material does not include sulfur or alkali metal polysulfide, The highly elastic polymer has a recoverable tensile elastic strain of 2% to 700%, a tensile strength of not less than 10 -6 S / cm, and a thickness from 0.5 nm to less than 10 nm, wherein the formation of lithium metal dendrites is eliminated; The highly elastic polymer contains a cross-linked polymer chain network selected from nitrile-containing polyvinyl alcohol chains, cyanoresin chains, pentaerythritol tetraacrylate chains, pentaerythritol triacrylate chains, ethoxylated trimethylolpropane triacrylate (ETPTA) chains, ethylene glycol methyl ether acrylate (EGMEA) chains, and combinations thereof.
28. The method of claim 27, wherein: The highly elastic polymer contains from 0.1% to 50% by weight of a lithium ion conductive additive dispersed therein, or contains from 0.1% by weight to 10% by weight of a reinforcing nanofilament selected from carbon nanotubes, carbon nanofibers, graphene, or a combination thereof.
29. The method of claim 27, wherein: The highly elastic polymer is mixed with a lithium ion conductive additive to form a composite, wherein the lithium ion conductive additive is dispersed in the highly elastic polymer and is selected from Li2CO3, Li2O, Li2C2O4, LiOH, LiX, ROCO2Li, HCOLi, ROLi, (ROCO2Li)2, (CH2OCO2Li)2, Li2S, Li x SO y , or a combination thereof, wherein X=F, Cl, I, or Br, R=hydrocarbon, 0≤x≤1, and 1≤y≤4.
30. The method of claim 27, wherein: The highly elastic polymer further contains a conductive material dispersed therein, and the conductive material is selected from electron conductive polymers, metal particles, metal wires, graphene sheets, carbon fibers, carbon nanotubes, graphite particles, expanded graphite flakes, acetylene black particles, and combinations thereof.
31. The method of claim 28, wherein: The lithium ion conductive material is dispersed in the highly elastic polymer and is selected from lithium perchlorate LiClO4, lithium hexafluorophosphate LiPF6, lithium fluoroborate LiBF4, lithium hexafluoroarsenide LiAsF6, lithium trifluoromethanesulfonate LiCF3SO3, lithium bistrifluoromethylsulfonyl imide LiN(CF3SO2)2, lithium bis(oxalate)borate LiBOB, lithium difluorooxalatoborate LiBF2C2O4, lithium nitrate LiNO3, lithium fluoroalkyl phosphate LiPF3(CF2CF3)3, lithium bisperfluoroethylsulfonyl imide LiBETI, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonyl imide LiTFSI, ionic liquid-based lithium salts, and combinations thereof.
32. The method of any one of claims 27 to 31, wherein: Step (a) also provides a cathode current collector supporting the cathode active material layer; Step (b) also provides an anode current collector supporting the foil or coating; Step (c) also provides a separator for electrically separating the anode from the cathode; as well as Step (d) also provides an anode-protective layer of a highly elastic polymer disposed between the lithium metal or lithium alloy foil or coating and the electrolyte or the separator.
33. The method of claim 32, wherein: The step of providing a lithium metal coating supported by the anode current collector is performed during a first charging operation of the battery.