A plug-in clutch housing structure and casting process thereof
By designing the plug-in clutch housing structure and adopting the casting process, we solve the problems of the existing clutch housing being simple in structure, resulting in easy wear of accessories and cumbersome disassembly and assembly, and achieve quick disassembly and assembly of the housing and products with high hardness and strength. , which meets the processing needs of complex-shaped parts.
Patent Information
- Application Number
- CN202010041175.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-01-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-01-15
AI Technical Summary
The existing forklift clutch housing has a simple structure, which makes the internal parts easy to wear and requires frequent replacement. The disassembly and assembly are cumbersome, time-consuming and labor-intensive.
A plug-in clutch housing structure is designed, using a casting process, including a hollow conical housing, positioning grooves, mounting bosses, operating ports and other features. The hardness and strength of the housing are improved through the casting process, and the shell is Preset operating holes on both sides of the body facilitate accessory replacement and maintenance.
It realizes the rapid disassembly and assembly of the clutch housing, improves the shape plasticity and usability of the product, reduces disassembly and assembly time and labor, ensures the hardness and strength of the product, meets the processing requirements of complex-shaped parts, and improves product quality.
Smart Images

Figure CN110985560B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of production and processing of a plug-in clutch housing, and mainly relates to a plug-in clutch housing structure and a casting process thereof. Background Art
[0002] With the development of the times, the blank production method of forklift clutch housing has changed from sand-bonded mold casting to composite sand casting or bubble film lost foam casting, etc. Sand-bonded mold casting can only make some simple-shaped products due to various reasons such as sand and soil, which limits the technical innovation of the housing blank. The existing clutch housing structure is simple, and the clutch housing is used for a long time. Its internal accessories such as friction discs and friction plates are easy to wear and need to be replaced frequently. Every time it is replaced, the entire clutch housing needs to be disassembled, which is troublesome, time-consuming and labor-intensive. Now a new clutch housing structure and its casting method are introduced to change the product's performance and improve the plasticity of the product shape. Therefore, some technical improvements and modifications are made to the clutch housing blank. Summary of the invention
[0003] The purpose of the present invention is to make up for the defects of the existing technology and provide a plug-in clutch housing structure and its casting process, which realizes the performance of quick disassembly and assembly of the housing, and through the casting molding method, it can meet the processing requirements of parts with more complex shapes, and ensure the hardness and strength of the product, thereby improving the product quality.
[0004] The present invention is achieved through the following technical solutions:
[0005] A plug-in clutch housing structure includes a hollow conical housing, an axial hole is provided in the middle of the upper end surface of the housing, and is characterized in that: a downwardly recessed positioning groove and a mounting hole are provided on the upper end surface at a circumferential position of the axial hole, a fixed mounting boss distributed along its circumference is provided on the outer side of the bottom end of the housing, mounting holes are distributed on the mounting boss, an opening is provided on one side of the housing, and an operating port for convenient disassembly and replacement of accessories in the clutch housing is provided on the side wall of the bottom end of the housing.
[0006] There are two operating ports, which are symmetrically arranged, and the outer ends of the operating ports are chamfered.
[0007] The operation port is rectangular, and its size is 30mm*25mm.
[0008] A boss protruding outward is provided at the bottom end of the shell side wall on the opening side, and an operation port is provided on the shell side wall directly opposite to the boss.
[0009] The trapezoidal opening has fixing holes at its four corners.
[0010] The plug-in clutch housing of the above structure is integrally formed by casting, and the specific casting process is as follows:
[0011] (1) Production of casting mold
[0012] Selecting molding sand according to the molding sand binder, mixing it with the molding sand binder and additives after screening, preparing a corresponding imitation mold according to the shape and contour characteristics of the shell, imitating the mixed sand into the molding sand mold by air pressure compaction, and then putting the lower core into the mold after compaction to obtain a corresponding casting mold. The molding sand can be divided into clay sand, water glass sand, cement sand, and resin sand according to the different binders used;
[0013] The casting mold comprises an upper flask and a lower flask, the upper flask is provided with at least one boss, the lower flask is provided with a groove matched with the boss of the upper flask, the joint surface of the upper flask and the lower flask constitutes a parting surface, the internal space formed by the upper flask and the lower flask constitutes a mold cavity, and a horizontal runner is arranged at the parting surface;
[0014] (2) Melting of cast iron raw materials
[0015] The cast iron raw materials include the following raw materials and their weight percentages: carbon 10-18%, silicon 0.3-0.6%, copper 0.5-1.5%, manganese 0.3-1%, chromium 25-32%, nickel 2-4%, molybdenum 3-7%, titanium 0.25-0.58%, silicon 3-6%, phosphorus 0.03-0.06%, vanadium 0.04-0.07%, and the balance is iron; the above components are added into a smelting furnace in the above proportions, and then the air in the smelting furnace is exhausted by argon gas to make the gas pressure in the smelting furnace constant at 1-3 standard atmospheres, and then the smelting furnace is heated to 1300°C-1500°C until the raw materials in the furnace are molten and stirred evenly, and then kept warm for 20-40 minutes;
[0016] (3) Casting
[0017] The molten cast iron raw material is poured into the casting mold to form the mold. During the injection process, the air pressure inside and outside the casting mold is kept synchronous. After the injection is completed, the casting mold is closed and the sand is removed after natural cooling for 1-3 hours.
[0018] (4) Heat treatment
[0019] The blank after casting is heat treated, the blank is placed in a heat treatment furnace, heated to 500°C for about 2 hours, kept warm for 5-7 hours, taken out of the furnace, quenched in water at about 30°C, and then aging treated at 150°C for 6 hours to obtain a plug-in clutch housing;
[0020] (5) Shot blasting
[0021] The high-speed projectile 60-110m / s stream continuously impacts the surface of the workpiece to be strengthened, forcing the target surface and the surface layer 0.10-0.85mm to change during the cyclic deformation process, thereby strengthening the surface.
[0022] (6) Qualified for storage
[0023] Check whether the surface of the shot blasted blank is damaged. If not, it will be placed in the qualified parts area. If not, it will be placed in the scrap area. Qualified parts will be put into storage after being polished and sprayed with paint, and unqualified parts will be placed in the scrap area.
[0024] The principle is: operation holes are pre-opened on both sides of the clutch housing to facilitate the replacement and maintenance of the friction disc and friction plate installed in the clutch housing during use. When replacing and maintaining, there is no need to disassemble, and the metal sleeve can be directly inserted into the operation hole to replace and adjust the internal accessories of the housing, which reduces the overall disassembly and assembly of the housing, saves time and effort, and has high disassembly and replacement efficiency, meeting the replacement requirements.
[0025] By casting the clutch housing, parts with more complex shapes can be manufactured, and are often used in the manufacture of supports and housings that do not require high mechanical properties. The casting process can improve the accuracy of the blank, reduce processing allowances, and have good comprehensive performance. In addition, alloy elements such as copper, manganese, chromium, nickel, molybdenum, and titanium are added to the casting raw materials in this application, and the control of relevant process parameters ensures that defects such as pores will not be generated in the product, thereby ensuring the hardness and strength of the product and improving the product quality.
[0026] The advantages of the present invention are:
[0027] The invention has reasonable structural design, and is convenient for disassembly and adjustment by opening the operating hole. It adopts the casting molding process, can manufacture parts with more complicated shapes, and can improve the precision of the blank, reduce the processing allowance, and has good comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a structural schematic diagram of the present invention.
[0029] Figure 2 for Figure 1 sectional view of .
[0030] Figure 3 It is a casting process flow chart of the present invention. DETAILED DESCRIPTION
[0031] See attached picture.
[0032] A plug-in clutch housing structure includes a hollow conical housing 1, an axial hole 2 is provided in the middle of the upper end surface of the housing 1, and is characterized in that: a downwardly recessed positioning groove 3 and a mounting hole 4 are provided on the upper end surface at a circumferential position of the axial hole 2, a fixed mounting boss 5 distributed along its circumference is provided on the outer side of the bottom end of the housing 1, and mounting holes are distributed on the mounting boss 5, an opening 6 is provided on one side of the housing 1, and an operating port 7 for convenient disassembly and replacement of accessories in the clutch housing is provided on the side wall of the bottom end of the housing 6.
[0033] Furthermore, there are two operating ports 7, which are symmetrically arranged, and the outer ends of the operating ports are chamfered.
[0034] Furthermore, the operation port 7 is rectangular, and its size is 30mm*25mm.
[0035] Furthermore, a boss 8 protruding outward is provided at the bottom end of the shell side wall on one side of the opening 6 , and an operation port 7 is provided on the shell side wall directly opposite to the boss 8 .
[0036] Furthermore, the trapezoidal opening 6 has four corners with fixing holes.
[0037] The plug-in clutch housing of the above structure is integrally formed by casting, and the specific casting process is as follows:
[0038] (1) Production of casting mold
[0039] Selecting molding sand according to the molding sand binder, mixing it with the molding sand binder and additives after screening, preparing a corresponding imitation mold according to the shape and contour characteristics of the shell, imitating the mixed sand into the molding sand mold by air pressure compaction, and then putting the lower core into the mold after compaction to obtain a corresponding casting mold. The molding sand can be divided into clay sand, water glass sand, cement sand, and resin sand according to the different binders used;
[0040] The casting mold comprises an upper flask and a lower flask, the upper flask is provided with at least one boss, the lower flask is provided with a groove matched with the boss of the upper flask, the joint surface of the upper flask and the lower flask constitutes a parting surface, the internal space formed by the upper flask and the lower flask constitutes a mold cavity, and a horizontal runner is arranged at the parting surface;
[0041] (2) Melting of cast iron raw materials
[0042] The cast iron raw materials include the following raw materials and their weight percentages: carbon 15%, silicon 0.4%, copper 1%, manganese 0.6%, chromium 29%, nickel 3%, molybdenum 5%, titanium 0.42%, silicon 4.5%, phosphorus 0.49%, vanadium 0.0.56%, and the balance is iron; the above components are added into a smelting furnace in the above proportions, and then the air in the smelting furnace is exhausted by argon gas and the gas pressure in the smelting furnace is kept constant at 2 standard atmospheres, and then the smelting furnace is heated to 1400°C until the raw materials in the furnace are molten and stirred evenly, and then kept warm for 30 minutes;
[0043] (3) Casting
[0044] The molten cast iron raw material is poured into the casting mold to form the mold. During the injection process, the air pressure inside and outside the casting mold is kept synchronous. After the injection is completed, the casting mold is closed and the sand is removed after natural cooling for 2 hours.
[0045] (4) Heat treatment
[0046] The blank after casting is heat treated, the blank is placed in a heat treatment furnace, heated to 500°C for about 2 hours, kept warm for 6 hours, taken out of the furnace, and quenched in water at about 30°C; then an aging treatment is performed at 150°C for 6 hours to obtain a plug-in clutch housing;
[0047] (5) Shot blasting
[0048] The high-speed projectile 60-110m / s stream continuously impacts the surface of the workpiece to be strengthened, forcing the target surface and the surface layer 0.10-0.85mm to change during the cyclic deformation process, thereby strengthening the surface.
[0049] (6) Qualified for storage
[0050] Check whether the surface of the shot blasted blank is damaged. If not, it will be placed in the qualified parts area. If not, it will be placed in the scrap area. Qualified parts will be put into storage after being polished and sprayed with paint, and unqualified parts will be placed in the scrap area.
[0051] The castings are tested by physical sampling. The macroscopic pinhole grade is level one (refer to GB10851-89), the tensile strength is greater than 310MPa, the yield strength is 140MPa, and the average hardness is HB108, which meets the use requirements and improves the product quality.
[0052] In the description of the present invention, it should be noted that the terms "vertical", "upper", "lower", "horizontal", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, "first", "second", "third", and "fourth" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.
[0053] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection, it can be a mechanical connection, it can be an electrical connection, it can be a direct connection, it can be connected through an intermediate medium, and it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this utility model can be understood according to specific circumstances.
[0054] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A casting process for a plug-in clutch housing, characterized in that: The plug-in clutch housing is integrally formed by casting, and the specific casting process is as follows: (1) Production of casting mold Selecting molding sand according to the molding sand binder, mixing it with the molding sand binder and additives after screening, preparing a corresponding imitation mold according to the shape and contour characteristics of the shell, imitating the mixed sand into the molding sand mold with air pressure compaction, and then putting the lower core into it after compaction to obtain a corresponding casting mold. The molding sand is divided into clay sand, water glass sand, cement sand, and resin sand according to the different binders used; The casting mold comprises an upper flask and a lower flask, the upper flask is provided with at least one boss, the lower flask is provided with a groove matched with the boss of the upper flask, the joint surface of the upper flask and the lower flask constitutes a parting surface, the internal space formed by the upper flask and the lower flask constitutes a mold cavity, and a horizontal runner is arranged at the parting surface; (2) Melting of cast iron raw materials The cast iron raw materials include the following raw materials and their weight percentages: carbon 10-18%, silicon 0.3-0.6%, copper 0.5-1.5%, manganese 0.3-1%, chromium 25-32%, nickel 2-4%, molybdenum 3-7%, titanium 0.25-0.58%, silicon 3-6%, phosphorus 0.03-0.06%, vanadium 0.04-0.07%, and the balance is iron; the above components are added into a smelting furnace in the above proportions, and then the air in the smelting furnace is exhausted by argon gas and the air pressure in the smelting furnace is kept constant at 1-3 standard atmospheres, and then the smelting furnace is heated to 1300°C-1500°C until the raw materials in the furnace are molten and stirred evenly, and then kept warm for 20-40 minutes; (3) Casting The molten cast iron raw material is poured into the casting mold to form the mold. During the injection process, the air pressure inside and outside the casting mold is kept synchronous. After the injection is completed, the casting mold is closed and the sand is removed after natural cooling for 1-3 hours. (4) Heat treatment The blank after casting is heat treated, the blank is placed in a heat treatment furnace, heated to 500°C for about 2 hours, kept warm for 5-7 hours, taken out of the furnace, quenched in water at about 30°C, and then aging treated at 150°C for 6 hours to obtain a plug-in clutch housing; (5) Shot blasting Use high-speed projectiles at a flow rate of 60-110m / s to continuously impact the surface of the workpiece to strengthen its surface; (6) Qualified for storage Check whether the surface of the shot blasted blank is damaged. If not, it will be sent to the qualified parts area. If not, it will be sent to the scrap area. The qualified parts will be put into storage after being polished and sprayed with paint, and the unqualified parts will be put into the scrap area. The plug-in clutch housing structure comprises a hollow conical housing (1), an axial hole (2) is provided in the middle of the upper end surface of the housing (1), a downwardly recessed positioning groove (3) and a mounting hole (4) are provided on the upper end surface of the axial hole (2) at a circumferential position, a mounting boss (5) distributed along the circumference of the housing (1) is provided on the outer side of the bottom end, and mounting holes are distributed on the mounting boss (5), an opening (6) is provided on one side of the housing (1), and an operating port (7) for convenient disassembly and replacement of accessories in the clutch housing is provided on the side wall of the bottom end of the housing (1).
2. The casting process of the plug-in clutch housing according to claim 1 is characterized in that: There are two operating ports (7), which are symmetrically arranged, and the outer ends of the operating ports are provided with chamfers.
3. The casting process of the plug-in clutch housing according to claim 1 is characterized in that: The operation port (7) is rectangular, and its size is 30mm*25mm.
4. The casting process of the plug-in clutch housing according to claim 1 is characterized in that: A boss (8) protruding outward is provided at the bottom end of the shell side wall on one side of the opening (6), and an operating port (7) is provided on the shell side wall directly opposite to the boss (8).
5. The casting process of the plug-in clutch housing according to claim 1, characterized in that: The trapezoidal operating opening (7) has fixing holes at its four corners.