A composite metal friction disc of a grounding device and its production process
The composite metal friction disc made of double crystallizer continuous casting method and heat treatment process solves the reliability and safety of the friction disc of the grounding device under the vibration conditions of the EMU, and realizes a lighter and durable grounding device, avoiding the Defects of non-metallic materials.
Patent Information
- Application Number
- CN201911371064.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2039-12-26
AI Technical Summary
The friction discs of existing grounding devices are prone to loosening of installation bolts or cracks and melting of non-metallic materials under vibration conditions of the EMU, affecting safety and reliability.
The double crystallizer continuous casting method combines copper liquid and aluminum liquid metallurgy to form a composite blast material, and is mechanically processed through high-temperature and low-temperature heat treatment to make a composite metal friction disk. The friction disk core is a wear-resistant copper alloy and is coated The layer is a light metal aluminum alloy designed with raised and recessed structures to enhance bond strength and sealing.
Effectively reduce the weight of the friction disc, improve the reliability and safety of the grounding device, avoid the problems of non-metallic materials, and maintain the weight of the core structure of the non-metallic covered metal friction disc, and enhance the thermal conductivity and wear resistance of the friction disc.
Smart Images

Figure CN111009791B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of mechanical manufacturing and relates to a composite metal friction disc of a grounding device and a production process thereof. Background Art
[0002] The grounding device is a device that realizes the grounding return function of the EMU. The core components of the grounding device are the friction pairs, namely the carbon brushes and friction discs.
[0003] At present, the friction disc of the grounding device mainly has two structural forms: a single metal friction disc and a non-metallic material coated metal friction disc core; among them, the single metal friction disc is mainly a copper alloy and stainless steel friction disc, and the friction disc is heavy. Under the vibration conditions of the EMU, the grounding device is prone to loosening or even breaking of the mounting bolts, affecting the safety of the EMU operation. The non-metallic material coated metal friction disc core structure has a lighter weight, but the non-metallic material is prone to cracks on the surface of the non-metallic material and at the junction of the non-metal and the metal under the vibration of the EMU. The non-metallic material coating material has poor dimensional stability and may interfere with the assembly parts after being installed and running for a period of time; the non-metallic material has a low melting point, and when the grounding device is subjected to a large current shock, the non-metallic material may melt; compared with metal materials, non-metallic materials have poor thermal conductivity, and the grounding device has a high temperature rise after long-term use. Summary of the invention
[0004] Based on the above technical problems, the present invention provides a composite metal friction disc, which can effectively reduce the weight of the friction disc and improve the reliability of the grounding device during use compared with a single metal friction disc; compared with a metal friction disc core structure coated with a non-metallic material, the composite metal friction disc can avoid a series of problems caused by non-metallic materials, and at the same time can keep the weight of the friction disc equivalent to that of the metal friction disc core structure coated with a non-metallic material, thereby improving the safety of the grounding device during use.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0006] A production process of a composite metal friction disc of a grounding device, characterized in that the specific steps are as follows:
[0007] Step 1: metallurgically combining molten copper and molten aluminum by a double crystallizer continuous casting method to form a composite billet;
[0008] Step 2, heat treating the composite blank, including two stages of high temperature heat treatment and low temperature heat treatment;
[0009] Step three, cutting the composite blank and forming the composite metal friction disc by mechanical processing.
[0010] Among them, the specific method of step one is: using two coaxial crystallizers arranged along the direction of pulling the billet, first solidifying the prepared copper liquid in the upper crystallizer to form a core billet, the core billet enters the aluminum liquid in the lower insulation crucible, and then the aluminum liquid solidifies in the lower crystallizer to form a coating billet, and then the coating billet and the core billet are metallurgically combined to form a composite billet.
[0011] Specifically, the chemical composition of the copper liquid is Sn 8-11%, Zn 1-3%, Pb 0.5-2%, Ni 0.05-0.2%, P 0.01-0.04%, Ti 0.2-0.5%, and the rest is copper, and the total impurity content is less than 0.2%.
[0012] Furthermore, in step 2, the heat treatment process of the composite metal billet includes high-temperature heat treatment and low-temperature heat treatment. The high-temperature heat treatment process is first performed at 450-500°C / 2-8h, followed by air cooling, and the low-temperature heat treatment process is then performed at 25-200°C / 4-100h, followed by air cooling.
[0013] Preferably, in step three, the cutting length of the composite blank is 33 mm.
[0014] A composite metal friction disc for a grounding device is manufactured by the above-mentioned production process, and is composed of a friction disc core and a coating layer, wherein the friction disc core is a wear-resistant copper alloy, and the coating layer is a light metal aluminum alloy in the prior art, wherein the friction disc core at the center of the front side of the composite metal friction disc is a convex structure, and a circular disc core friction surface is formed at its top, and the friction disc core at the junction with the coating layer has a petal-shaped disc core flange, and the coating layer on the front side of the composite metal friction disc is provided with a coating layer outer edge, a coating layer groove, a coating layer inner edge and a coating layer transition surface in sequence from the periphery to the inside, and a mounting hole is provided on the coating layer transition surface; the friction disc at the center of the back side of the composite metal friction disc is also recessed inward to form a weight-reducing hole, and a circle of protruding coating layer back edge is provided on the coating layer on the back side of the composite metal friction disc corresponding to the position of the coating layer groove.
[0015] Preferably, three of the core flanges are connected into a group, and there are four groups in total that are evenly distributed around the outer side of the friction core.
[0016] Preferably, the mounting holes penetrate the transition surface of the coating layer and are arranged in a ring matrix, and four mounting holes are provided corresponding to the gaps between the flange groups of the disk core.
[0017] Furthermore, the outer edge of the coating layer and the inner edge of the coating layer are upright protruding circular ring structures, and the coating layer groove between the two is a sunken annular groove body, so that the outer edge of the coating layer, the coating layer groove, and the inner edge of the coating layer together form a frontal maze structure.
[0018] Preferably, the weight-reducing hole is a cylindrical slot.
[0019] The beneficial effects of the present invention are as follows:
[0020] (1) The present invention uses a copper-aluminum composite blank formed by a double crystallizer continuous casting method, and then heat treats the composite blank, and then performs machining after the heat treatment, thereby forming a composite metal friction disk of a grounding device. The composite metal friction disk can effectively reduce the weight of the friction disk and improve the reliability of the grounding device during use;
[0021] (2) The copper alloy material used in the present invention has good casting performance, high mechanical strength and good wear resistance and electrical conductivity;
[0022] (3) The composite metal friction disc produced by the present invention has a protrusion and a depression structure on the friction disc core to increase the bonding strength with the coating layer;
[0023] (4) The composite metal friction disc produced by the present invention has a friction surface on the friction disc core that is in sliding friction contact with the carbon brush of the grounding device to achieve the diversion function;
[0024] (5) The composite metal friction disc produced by the present invention, wherein a labyrinth structure and a mounting hole are provided on the coating layer, the labyrinth structure is used to seal the carbon powder of the grounding device, and the mounting hole is used to install the friction disc;
[0025] (6) The composite metal friction disc of the present invention can avoid a series of problems caused by non-metallic materials, while maintaining the weight of the friction disc comparable to that of a non-metallic material-coated metal friction disc core structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the front structure of the composite metal friction disk of the present invention;
[0027] Figure 2 It is a schematic diagram of the back structure of the composite metal friction disk of the present invention;
[0028] Figure 3 It is a schematic diagram of the cross-sectional structure of the composite metal friction disk of the present invention;
[0029] Figure 4 Schematic diagram of the present invention using a double crystallizer continuous casting method for production;
[0030] Figure 5 It is a schematic diagram of the structure of the composite blank in the present invention;
[0031] In the figure, 1-outer edge of coating layer, 2-groove of coating layer, 3-inner edge of coating layer, 4-transition surface of coating layer, 5-mounting hole, 6-disk core flange, 7-disk core friction surface, 8-weight reduction hole, 9-back edge of coating layer; 10-copper liquid, 11-disk core blank, 12-aluminum liquid, 13-wrapping layer blank, 14-composite blank. DETAILED DESCRIPTION
[0032] In order for those skilled in the art to better understand the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and the following embodiments.
[0033] like Figures 1 to 3 As shown, a grounding device composite metal friction disk consists of a friction disk core and a coating layer, wherein the friction disk core is a wear-resistant copper alloy, and the chemical composition of the copper alloy is Sn 8-11%, Zn 1-3%, Pb 0.5-2%, Ni 0.05-0.2%, P 0.01-0.04%, Ti 0.2-0.5%, and the rest is copper, and the total impurity content is less than 0.2%; the coating layer is a light metal aluminum alloy in the prior art.
[0034] Specifically, Figure 1 and 3 As shown, the friction disc core at the front center of the composite metal friction disc is a convex structure, and a circular disc core friction surface 7 is formed at the top, and the friction disc core at the junction with the coating layer has a petal-shaped disc core flange 6. Preferably, the disc core flanges 6 are connected in groups of three, and there are four groups evenly distributed around the outer side of the friction disc core to increase the bonding strength between the friction disc core and the coating layer; the friction surface 7 is in sliding friction contact with the carbon brush of the grounding device to achieve the diversion function.
[0035] Further, if Figure 1 and 3 As shown, the coating layer is arranged around the friction disc core on the front side of the composite metal friction disc, and the front side of the coating layer from the periphery to the inside are respectively the coating layer outer edge 1, the coating layer groove 2, the coating layer inner edge 3 and the coating layer transition surface 4, wherein the coating layer outer edge 1 and the coating layer inner edge 3 are upright raised circular ring structures, and the coating layer groove 2 between the two is a sunken annular groove body, so that the coating layer outer edge 1, the coating layer groove 2, and the coating layer inner edge 3 together form a front maze structure for sealing the carbon powder of the grounding device.
[0036] Among them, a plurality of mounting holes 5 in a ring matrix are provided on the transition surface 4 of the coating layer for installing the friction disc. The mounting holes 5 are arranged through the coating layer of the composite metal friction disc. Preferably, four mounting holes 5 are provided and are arranged corresponding to the gaps between the disc core flange groups.
[0037] Specifically, Figure 2 and 3 As shown, the friction disc core at the center of the back side of the composite metal friction disc is recessed inward to form a weight-reducing hole 8, and the weight-reducing hole 8 is a cylindrical groove body.
[0038] Furthermore, the coating layer on the back side of the composite metal friction disc corresponds to the position of the coating layer groove 2 and has a circle of protruding coating layer back side edge 9.
[0039] When the composite metal friction disc in the present invention is in use, the locomotive grounding device is installed on the front side of the composite metal friction disc of the present invention, and the locomotive grounding device is clamped in the maze structure on the front side, while the back side of the composite metal friction disc is connected to the adapter and fixedly connected through the corresponding mounting holes, thereby completing the installation of the grounding device for easy grounding use.
[0040] Example 1
[0041] The production process of producing the above-mentioned grounding device composite metal friction disc is as follows: Figure 4 and 5 As shown, the specific steps are as follows:
[0042] Step 1: The copper liquid 10 and the aluminum liquid 12 are compositely and continuously casted by a double crystallizer continuous casting method to form a composite billet 14; specifically, two coaxial crystallizers are arranged along the billet pulling direction, and the prepared copper liquid 10 is first solidified in the upper crystallizer to form a core billet 11, and the core billet 11 enters the aluminum liquid 12 in the lower insulation crucible, and then the aluminum liquid solidifies in the lower crystallizer to form a wrapping layer billet 13, and then the wrapping layer billet 13 is metallurgically combined with the core billet 11 to form a composite billet 14, such as Figure 5 shown.
[0043] The chemical composition of the copper liquid 10 is Sn 10%, Zn 3%, Pb 1%, Ni 0.15%, P 0.03%, Ti 0.5% by mass, the total impurity content is less than 0.2%, and the rest is copper.
[0044] Wherein, the aluminum liquid 12 is 7055 aluminum alloy.
[0045] Step 2: heat-treat the composite blank. The first high-temperature heat treatment process is 450 / 8h, followed by air cooling, and the second low-temperature heat treatment process is 120℃ / 8h, followed by air cooling.
[0046] Step 3: Cut the composite blank using a sawing machine according to the size of the friction disc, with the preferred cutting length being 33 mm, and then machine the friction disc blank to obtain the composite metal friction disc.
[0047] Through mechanical processing, the friction disc core at the center of the front side of the composite metal friction disc is made into a convex structure, and a circular disc core friction surface 7 is formed at the top, and the friction disc core at the junction with the coating layer has a petal-shaped disc core flange 6, and the coating layer on the front side of the composite metal friction disc is provided with a coating layer outer edge 1, a coating layer groove 2, a coating layer inner edge 3 and a coating layer transition surface 4 in sequence from the periphery to the inside, and a mounting hole is opened on the coating layer transition surface 4; the friction disc at the center of the back side of the composite metal friction disc is also recessed inward to form a weight reduction hole 8, and a circle of protruding coating layer back edge 9 is provided on the coating layer on the back side of the composite metal friction disc corresponding to the position of the coating layer groove 2.
[0048] As shown in the following table, a weight comparison between the composite metal friction disc produced by the present invention and friction discs of other structures shows that the composite metal friction disc of the present invention has a better weight reduction effect than the friction plate of a single metal.
[0049]
[0050]
[0051] Then, the composite metal friction disc was subjected to vibration and impact tests according to the severe level 3 test in GB / T21563. After the test, the composite metal friction disc was subjected to X-ray flaw detection, and the joints between the two metals were well bonded without defects such as cracks.
[0052] The composite metal friction disc was subjected to a current-carrying wear temperature rise test on the experimental bench (test current 470A, test speed 350Km / h). The wear of the composite metal friction disc was less than 0.1mm / 100,000 kilometers, meeting the wear requirements. During the test, the maximum temperature of the composite metal friction disc was 83°C, which was lower than the temperature of the friction disc with a metal friction disc core coated with non-metallic materials.
[0053] Example 2
[0054] The production process of producing the composite metal friction disc of the grounding device is as follows: Figure 4 and 5 As shown, the specific steps are as follows:
[0055] Step 1: metallurgically combine the copper liquid 10 and the aluminum liquid 12 by a double crystallizer continuous casting method to form a composite billet 14; specifically, using two coaxial crystallizers arranged along the billet pulling direction, first solidify the prepared copper liquid 10 in the upper crystallizer to form a core billet 11, and the core billet 11 enters the aluminum liquid 12 in the lower insulation crucible, and then the aluminum liquid solidifies in the lower crystallizer to form a wrapping layer billet 13, and then the wrapping layer billet 13 is metallurgically combined with the core billet 11 to form a composite billet 14, such as Figure 5 shown.
[0056] The chemical composition of the copper liquid 10 is Sn 8%, Zn 2%, Pb 1.5%, Ni 0.1%, P 0.04%, Ti 0.3% by mass fraction, the total impurity content is less than 0.2%, and the rest is copper.
[0057] Wherein, the aluminum liquid 12 is 2024 aluminum alloy.
[0058] Step 2: heat-treating the composite blank. The first high-temperature heat treatment process is 500°C / 6h, followed by air cooling, and the second low-temperature heat treatment process is 25°C / 96h, followed by air cooling.
[0059] Step 3: Cut the composite blank using a sawing machine according to the size of the friction disc, with the preferred cutting length being 33 mm, and then machine the friction disc blank to obtain the composite metal friction disc.
[0060] Through mechanical processing, the friction disc core at the center of the front side of the composite metal friction disc is made into a convex structure, and a circular disc core friction surface 7 is formed at the top, and the friction disc core at the junction with the coating layer has a petal-shaped disc core flange 6, and the coating layer on the front side of the composite metal friction disc is provided with a coating layer outer edge 1, a coating layer groove 2, a coating layer inner edge 3 and a coating layer transition surface 4 in sequence from the periphery to the inside, and a mounting hole is opened on the coating layer transition surface 4; the friction disc at the center of the back side of the composite metal friction disc is also recessed inward to form a weight reduction hole 8, and a circle of protruding coating layer back edge 9 is provided on the coating layer on the back side of the composite metal friction disc corresponding to the position of the coating layer groove 2.
[0061] As shown in the following table, a weight comparison between the composite metal friction disc produced by the present invention and friction discs of other structures shows that the composite metal friction disc of the present invention has a better weight reduction effect than the friction plate of a single metal.
[0062]
[0063]
[0064] Then, the composite metal friction disc was subjected to vibration and impact tests according to the severe level 3 test in GB / T21563. After the test, the composite metal friction disc was subjected to X-ray flaw detection, and the joints between the two metals were well bonded without defects such as cracks.
[0065] The composite metal friction disc was subjected to a current-carrying wear temperature rise test on the experimental bench (test current 470A, test speed 350Km / h). The wear of the composite metal friction disc was less than 0.1mm / 100,000 kilometers, meeting the wear requirements. During the test, the maximum temperature of the composite metal friction disc was 82°C, which was lower than the temperature of the friction disc with a metal friction disc core coated with non-metallic materials.
[0066] The above is an embodiment of the present invention. The above embodiments and the specific parameters in the embodiments are only for the purpose of clearly describing the verification process of the present invention, and are not intended to limit the patent protection scope of the present invention. The patent protection scope of the present invention is still subject to its claims, and any equivalent structural changes made by using the description and drawings of the present invention should be included in the protection scope of the present invention.
Claims
1. A production process for a composite metal friction disc of a grounding device, It is characterized in that The specific steps are as follows: Step 1: metallurgically combining molten copper and molten aluminum by a double crystallizer continuous casting method to form a composite billet; Step 2, heat treating the composite blank, including two stages of high temperature heat treatment and low temperature heat treatment; Step 3, cutting the composite blank and forming the composite metal friction disc by mechanical processing; The specific method of step 1 is as follows: using two coaxial crystallizers arranged along the direction of billet pulling, first solidifying the prepared copper liquid in the upper crystallizer to form a core billet, the core billet enters the aluminum liquid in the lower insulation crucible, and then solidifying the aluminum liquid in the lower crystallizer to form a wrapping billet, and then metallurgically combining the wrapping billet with the core billet to form a composite billet; The composite metal friction disc is composed of a friction disc core and a coating layer, wherein the friction disc core is a wear-resistant copper alloy, and the coating layer is a light metal aluminum alloy in the prior art, wherein the friction disc core at the center of the front side of the composite metal friction disc is a convex structure, and a circular disc core friction surface is formed at the top thereof, and the friction disc core at the junction with the coating layer has a disc core flange in the shape of a petal, and the coating layer at the front side of the composite metal friction disc is provided with a coating layer outer edge, a coating layer groove, a coating layer inner edge and a coating layer transition surface in sequence from the periphery to the inside, and a mounting hole is provided on the coating layer transition surface; the friction disc at the center of the back side of the composite metal friction disc is also recessed inward to form a weight-reducing hole, and a circle of protruding coating layer back edge is provided on the coating layer at the back side of the composite metal friction disc corresponding to the position of the coating layer groove; The outer edge of the coating layer and the inner edge of the coating layer are upright protruding circular ring structures, and the coating layer groove therebetween is a sunken annular groove body, so that the outer edge of the coating layer, the coating layer groove, and the inner edge of the coating layer together form a frontal maze structure.
2. The production process of a composite metal friction disc for a grounding device according to claim 1, It is characterized in that The chemical composition of the copper liquid is Sn 8-11%, Zn 1-3%, Pb 0.5-2%, Ni 0.05-0.2%, P0.01-0.04%, Ti 0.2-0.5%, and the rest is copper. The total impurity content is less than 0.2%.
3. The production process of a composite metal friction disc for a grounding device according to claim 1, It is characterized in that In step 2, the heat treatment process of the composite metal billet includes high-temperature heat treatment and low-temperature heat treatment. The high-temperature heat treatment process is first performed at 450-500°C / 2-8h, followed by air cooling, and the low-temperature heat treatment process is then performed at 25-200°C / 4-100h, followed by air cooling.
4. The production process of a composite metal friction disc for a grounding device according to claim 1, It is characterized in that In step three, the cutting length of the composite blank is 33 mm.
5. The production process of a composite metal friction disc for a grounding device according to claim 1, It is characterized in that The disc core flanges are connected into a group of three, and there are four groups in total, which are evenly distributed around the outer side of the friction disc core.
6. The production process of a composite metal friction disc for a grounding device according to claim 5, It is characterized in that The mounting holes penetrate the transition surface of the coating layer and are arranged in a ring matrix, and four mounting holes are provided, which are arranged corresponding to the gaps between the flange groups of the disk core.
7. The production process of a composite metal friction disc for a grounding device according to claim 1, It is characterized in that The weight-reducing hole is a cylindrical slot.
Citation Information
Patent Citations
Self-repair conductive abrasion-resistant copper alloy for high-speed rail grounding device and preparation method for self-repair conductive abrasion-resistant copper alloy
CN106756215A
Bimetal railway through ground wire and short-flow production method thereof
CN108320835A
Motor friction disk material used for high speed train, and preparation method thereof
CN108754221A
Method for casting aluminum-steel composite brake disc through solid-liquid composite extrusion