Electrode composite conductive agent for lithium battery, electrode for lithium battery, method for manufacturing the same, and lithium battery including the electrode
By using graphene-silicon composite as a conductive agent in lithium batteries, the problems of long charging time and short driving range of lithium batteries in electric vehicles have been solved, achieving higher battery performance and lifespan.
Patent Information
- Application Number
- CN201910846842.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-11-19
- Filing Date
- 2019-09-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-09-09
AI Technical Summary
Existing lithium batteries in electric vehicles suffer from short driving range and slow charging time. Furthermore, traditional carbon-based conductive materials in lithium batteries lead to reduced lithium-ion mobility and increased electrode expansion, affecting battery performance.
Graphene-silicon composite is used as an electrode composite conductive agent. By dry mixing the graphene-silicon composite with carbonaceous conductive materials and electrode active materials, a uniformly dispersed conductive network is formed, which reduces electrode voids and improves adhesion and conductivity.
It improves the electrolyte impregnation properties, initial efficiency, charge and discharge rate characteristics of lithium batteries, reduces electrode expansion rate, extends battery life, and increases lithium-ion mobility.
Smart Images

Figure CN111200130B_ABST
Abstract
Description
[0001] Cross-reference to related applications
[0002] This application claims the priority and benefit of Korean Patent Application No. 10-2018-0142512, filed on Nov. 19, 2018 with the Korean Intellectual Property Office, the content of which is incorporated herein by reference in its entirety. Technical field
[0003] The present disclosure relates to an electrode composite conductive agent for a lithium battery, an electrode for a lithium battery including the electrode composite conductive agent, a method of preparing the electrode, and a lithium battery including the electrode. Background art
[0004] Lithium ion batteries (LIBs) have been used as power sources for a variety of portable devices due to their high energy density and ease of design. With the recent growing trend of using LIBs as power sources for electric vehicles / energy storage rather than portable information technology (IT) devices, extensive research has been conducted on materials that can provide high energy density and long life.
[0005] Currently, commercially available electric vehicles have a low driving range and slow charging time, and thus have technical limitations in replacing existing petroleum-based energy sources. Therefore, there is an urgent need to develop battery materials for providing improved capacity and charging characteristics. Summary of the invention
[0006] Provided is an electrode composite conductive agent for a lithium battery.
[0007] Provided is an electrode for a lithium battery and a method of preparing the same, the electrode including the electrode composite conductive agent.
[0008] Provided is a lithium battery including the electrode and having improved output characteristics.
[0009] Additional aspects will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the provided embodiments.
[0010] According to an aspect of an embodiment, an electrode composite conductive agent for a lithium battery includes: a carbonaceous conductive material; and a graphene-silica composite, wherein the graphene-silica composite includes a matrix containing graphene, and a low-valent silicon oxide (silicon suboxide) of the formula SiO x where 0 < x < 2, or a combination of silica and a low-valent silicon oxide of the formula SiO x where 0 < x < 2, wherein the amount of the graphene-silica composite is 20 parts by weight or less based on the total weight of 100 parts by weight of the composite conductive agent.
[0011] According to an aspect of another embodiment, an electrode for a lithium battery includes the electrode composite conductive agent.
[0012] According to an aspect of another embodiment, a method of preparing an electrode for a lithium battery includes: dry-mixing an electrode active material, a carbonaceous conductive material, and a graphene-silica composite to obtain a mixture; adding a binder and a solvent to the dry-mixed mixture; and mixing the binder and the mixture to obtain an electrode active material composition, wherein the graphene-silica composite includes a matrix containing graphene, and a low-valent silicon oxide of the formula SiO x where 0 < x < 2, or a combination of silicon dioxide and a low-valent silicon oxide of the formula SiO x where 0 < x < 2, wherein the amount of the graphene-silica composite is 20 parts by weight or less, based on the total weight of 100 parts by weight of the carbonaceous conductive material and the graphene-silica composite constituting the composite conductive agent.
[0013] According to an aspect of another embodiment, a lithium battery includes the electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] These and / or other aspects will become apparent and more readily appreciated from the following description of embodiments, taken in conjunction with the accompanying drawings, in which:
[0015] Figure 1 A schematic diagram for illustrating an embodiment of an electrode for a lithium battery;
[0016] Figure 2A A schematic diagram for illustrating the structure of an embodiment of a graphene-silica composite;
[0017] Figure 2B A schematic diagram for illustrating the structure of an embodiment of a silicon-containing composite;
[0018] Figure 3A A scanning electron microscope (SEM) image of the negative electrode of a full cell prepared according to Example 1;
[0019] Figure 3B Showing the results of energy dispersive spectroscopy (EDS) analysis of the negative electrode of a full cell prepared according to Example 1;
[0020] Figure 4 An SEM image of the negative electrode of a full cell prepared according to Comparative Example 1;
[0021] Figure 5 A graph of capacity retention (%) versus cycle number, illustrating the capacity retention of full cells prepared according to Example 1 and Comparative Examples 1 and 2;
[0022] Figures 6A to 6Dis a graph of voltage (volts, V) versus capacity (milliampere-hour / gram, mAh / g), which illustrates the rate characteristics of coin half-cell batteries prepared according to Example 4 and Comparative Examples 3 and 4 during charge and discharge tests;
[0023] Fig. 7A and 7B SEM images of the full unit cell prepared according to Example 1 before charge and discharge cycles and after 200 cycles, respectively;
[0024] Fig. 8A and 8B SEM images of the full-unit battery prepared according to Comparative Example 1 before charge and discharge cycles and after 200 cycles, respectively;
[0025] Fig.9A and 9B SEM images of the full-unit battery prepared according to Comparative Example 2 before charge and discharge cycles and after 200 cycles, respectively;
[0026] Fig.10 is a graph of capacity retention (percent) versus cycle number, illustrating the capacity retention of coin full-cell batteries prepared according to Examples 1, 2, and 3 and Comparative Examples 1 and 2;
[0027] Fig.11A is a graph of rate characteristics (percent, %) versus rate (C rate), which illustrates the rate characteristics of coin half-cell batteries prepared according to Examples 6a, 4, 5, and Comparative Example 3 during charge and discharge tests;
[0028] Fig. 11B is a graph of rate characteristics (percent, %) versus rate (C rate), which illustrates the rate characteristics of coin half-cell batteries prepared according to Example 4 and Comparative Example 3 during charge and discharge tests;
[0029] Fig.12 to illustrate a graph of rate performance (percent, %) versus rate (C-rate), which illustrates the rate performance of coin half-cell batteries prepared according to Examples 4, 6a, 5 and Comparative Example 3 during charge and discharge testing; and
[0030] Fig.13 A schematic diagram of an embodiment of a lithium battery. DETAILED DESCRIPTION
[0031] The present invention will now be described more fully hereinafter with reference to the accompanying drawings, wherein the same reference numerals refer to the same elements throughout. In this regard, the present embodiment may have different forms and should not be construed as being limited to the description set forth herein. Therefore, the disclosed embodiments are described below only by reference to the accompanying drawings to illustrate aspects. As used herein, the term "and / or" includes any and all combinations of one or more of the related enumerated items. Expressions such as "at least one (kind)" when before or after a list of elements modify the entire list of elements and do not modify the individual elements of the list.
[0032] It will be understood that when an element is referred to as being “on” another element, it can be directly on the other element or intervening elements may be present therebetween. In contrast, when an element is referred to as being “directly on” another element, there are no intervening elements present.
[0033] It will be understood that although the terms "first", "second", "third", etc. may be used herein to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings herein, the "first element", "component", "region", "layer" or "part" discussed below may be referred to as a second element, component, region, layer or part.
[0034] The terms used herein are only for the purpose of describing specific embodiments and are not intended to be restrictive. As used herein, the singular forms "one (kind) (indefinite article, a, an)" and "the (the)" are intended to include plural forms, including "at least one (kind)", unless the content clearly indicates otherwise. "At least one (kind)" will not be interpreted as limiting "one (kind)". "Or" means "and / or". As used herein, the term "and / or" includes any and all combinations of one or more of the related enumerated items. It will be further understood that the term "include" or "comprising" when used in this specification indicates that there are stated features, regions, wholes, steps, operations, elements, and / or components, but does not exclude the presence or increase of one or more other features, regions, wholes, steps, operations, elements, components, and / or their sets.
[0035] For ease of description, spatially relative terms such as "under", "below", "lower", "above", "upper", etc. may be used herein to describe the relationship of one element or feature to another element or feature as shown in the figure. It will be understood that in addition to the orientation shown in the figure, the spatially relative terms are intended to include different orientations of the device in use or operation. For example, if the device in the figure is turned over, the elements described as "under" or "below" other elements or features will be oriented "above" other elements or features. Therefore, the exemplary term "under" can include both above and below. The device can be oriented in other ways (rotated 90 degrees or in other orientations), and the spatially relative descriptors used in this article are interpreted accordingly.
[0036] As used herein, "about" or "approximately" includes the stated value and means within an acceptable range of deviation for the particular value as determined by one of ordinary skill in the art taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" can mean that the deviation from the stated value is within one or more standard deviations, or within ±30%, 20%, 10%, or 5%.
[0037] Unless otherwise defined, all terms (including technical and scientific terms) used in this article have the same meaning as commonly understood by ordinary technicians in the field to which the present disclosure belongs. It will be further understood that terms, such as those defined in commonly used dictionaries, should be interpreted as having a meaning consistent with their meaning in the context of the relevant art and the present disclosure, and will not be interpreted in an idealized or overly formal sense unless clearly defined in this article.
[0038] Exemplary embodiments are described herein with reference to cross-sectional views as schematic diagrams of idealized embodiments. Thus, deviations from the shapes of the figures as a result of, for example, manufacturing techniques and / or tolerances are expected. Therefore, the embodiments described herein should not be construed as being limited to the specific shapes of the regions as shown herein, but rather include deviations in shape caused by, for example, manufacturing. For example, a region illustrated or described as flat may typically have rough and / or nonlinear features. In addition, the illustrated sharp corners may be rounded. Therefore, the regions shown in the figures are schematic in nature, and their shapes are not intended to illustrate the precise shapes of the regions and are not intended to limit the scope of the claims.
[0039] As used in this specification, the term "graphene" means a polycyclic aromatic molecule formed by multiple carbon atoms covalently bonded to each other. The covalently bonded carbon atoms can form six-membered rings as repeating units, and can further include at least one of five-membered rings and seven-membered rings. Thus, graphene includes a single layer of covalently bonded carbon atoms with sp2 hybridization. Multiple graphene layers are often referred to as graphite in the art. However, for convenience, "graphene" as used herein can be a single layer, or can also include multiple carbon layers, such as 1 - 100 carbon layers, or 1 - 30 carbon layers. Thus, graphene as used herein can have a multi-layer structure formed by stacking single layers of graphene.
[0040] Hereinafter, an electrode composite conductive agent for a lithium battery, an electrode including the same, a method for preparing the electrode, and a lithium battery including the electrode according to an embodiment will be described in further detail with reference to the accompanying drawings.
[0041] The electrode composite conductive agent for a lithium battery includes: a carbonaceous conductive material; and a graphene - silica composite, wherein the graphene - silica composite includes a matrix containing graphene, and a low - valent silicon oxide of the formula SiO x where 0 < x < 2, or silicon dioxide and a combination of a low - valent silicon oxide of the formula SiO x where 0 < x < 2, and the amount of the graphene - silica composite is 20 parts by weight or less based on the total weight of 100 parts by weight of the composite conductive agent. The silica, that is, a low - valent silicon oxide of the formula SiO x where 0 < x < 2, silicon dioxide (SiO 2 ), or a combination thereof can be located on the graphene matrix or can be within the graphene matrix.
[0042] As used in this specification, the term "silica" refers to a low - valent silicon oxide of the formula SiO x where 0 < x < 2, silicon dioxide, or a combination thereof.
[0043] In the case where the negative electrode includes a carbonaceous conductive agent such as graphite, with a porous silicon composite and a graphite-based material as the negative electrode active material, and although not wanting to be bound by theory, it is understood that voids are formed in the negative electrode because the porous silicon composite and the graphite-based material have a size of tens of microns. Therefore, the mobility of lithium ions can be reduced, and the ability to buffer volume changes, such as those caused by the circulation of lithium ions, can be deteriorated. In addition, since the carbonaceous conductive agent is located around the negative electrode active material, the migration of lithium ions toward the active material can be reduced, and due to the large number of voids formed between the particles, it can be difficult to maintain conductivity during the charge and discharge cycle. In addition, since graphite as a carbonaceous conductive material has a size of several microns to tens of microns and has a flake shape, it is difficult to evenly disperse graphite in the electrode in which the electrode active material is stacked.
[0044] In order to solve these problems, the present inventors have proposed an electrode composite conductive agent for a lithium battery, which includes a carbonaceous conductive material and a graphene-silica composite, wherein the amount of the graphene-silica composite is selected to be about 20 parts by weight or less, for example, in the range of about 0.5 parts by weight to about 20 parts by weight, for example, about 5 parts by weight to about 20 parts by weight, for example, about 5 parts by weight to about 10 parts by weight, based on 100 parts by weight of the composite conductive agent. 100 parts by weight of the composite conductive agent represents 100 parts by weight of the total weight of the carbonaceous conductive material and the graphene-silica composite.
[0045] The graphene-silica composite of the composite conductive agent with improved carbon crystallinity and a size of, for example, about 10 to about 1000 nanometers, or about 30 nanometers to about 500 nanometers can fill the voids of the electrode. Therefore, compared with when using different carbonaceous conductive materials as conductive agents, the adhesion between the components in the electrode is improved, thereby strengthening the three-dimensional conductive network. As a result, the electrode expansion rate is reduced and the surface-to-surface conductive path can be improved and maintained. By using a composite conductive agent including a graphene-silica composite according to an embodiment, the voids in the electrode can be reduced, thereby preventing the conductive path from being disconnected or short-circuited, and preventing the lithium ion mobility to the active material from being reduced.
[0046] When the composite conductive agent according to the embodiment is used, the expansion rate of the electrode and battery including the composite conductive agent is reduced, and the bonding force between the current collector and the electrode active material is increased, thereby preventing the electrode active material from being separated from the current collector, even after repeated charging and discharging processes. In addition, electrical short circuits are prevented during charging and discharging cycles. As a result, by using an electrode including the electrode composite conductive agent, a lithium battery having improved electrolyte impregnation properties, improved initial efficiency, and improved life and charge and discharge rate characteristics can be manufactured.
[0047] For example, the carbonaceous conductive material may include graphene, graphite, carbon black, carbon nanotubes, vapor grown carbon fiber (VGCF), metal-coated carbon fiber, or a combination thereof. The carbonaceous conductive material may have a carbon fiber density of about 10 m2 / g (m 2 / g)-about 1,000m 2 / g, for example, about 11m 2 / g-about 500m 2 / g, for example, about 12m 2 / g-about 300m 2 / g, for example, about 15m 2 / g-about 100m 2 / g specific surface area.
[0048] The graphene-silica composite may have a thickness of about 50 m 2 / g-about 800m 2 / g, for example, about 50m 2 / g-about 500m 2 / g, for example, about 50m 2 / g-about 300m 2 / g, for example, about 100m 2 / g-about 200m 2 / g specific surface area.
[0049] The amount of the graphene-silica composite is selected to be about 20 parts by weight or less, such as about 0.5 parts by weight to about 20 parts by weight, such as about 5 parts by weight to about 20 parts by weight, such as about 5 parts by weight to about 10 parts by weight, based on 100 parts by weight of the composite conductive agent. When the amount of the graphene-silica composite is within the above range, adhesion between structures in the electrode can be improved and voids can be reduced.
[0050] The electrode active material may be any suitable electrode active material for a lithium battery. For example, a porous silicon composite, or a combination of a porous silicon composite and a carbonaceous negative electrode active material may be used. The porous silicon composite and the carbonaceous negative electrode active material may constitute a carbonaceous composite. The porous silicon composite is a composite containing silicon.
[0051] The carbonaceous negative electrode active material may include natural graphite, artificial graphite, expanded graphite, graphene, carbon black, fullerene soot, carbon nanotubes, graphite carbon, carbon fiber, or a combination thereof. However, the carbonaceous negative electrode active material is not limited thereto, and any suitable material available in the art may also be used.
[0052] The carbonaceous conductive material may have a flake shape, a plate shape, a rod shape, an irregular shape, or a combination thereof.
[0053] The size of the carbonaceous conductive material may be from about 1 nm to about 99 μm. The size of the carbonaceous conductive material may be from about 1 μm to about 99 μm, such as from about 1 μm to about 50 μm, such as from about 1 μm to about 10 μm, such as from about 1 μm to about 5 μm. When the carbonaceous conductive material is used, voids may exist between the structures in the electrode, and although not wishing to be bound by theory, it is understood that such voids may cause deterioration of charge and discharge characteristics such as life characteristics and high rate characteristics, and an increase in the electrode swelling rate. Throughout the specification, the size of the carbonaceous conductive material represents the average particle diameter in the case where the carbonaceous conductive material is spherical, and represents the length of the major axis in the case where the carbonaceous conductive material is not spherical.
[0054] Figure 1 Schematic diagram for explaining the structure of an electrode for a lithium battery including an electrode composite conductive agent according to an embodiment. The electrode may be, for example, a negative electrode.
[0055] As Figure 1 shown, the electrode has such a structure: an electrode active material layer including a first electrode active material 11, a second electrode active material 14, and a composite conductive agent including a carbonaceous conductive material 13 and a graphene-silica composite 12 is provided on a current collector 10.
[0056] For example, each of the first electrode active material 11 and the second electrode active material 14 may include a carbonaceous material, a silicon-based material, a silicon oxide, a silicon-based alloy, a silicon-carbonaceous material composite, tin, a tin-based alloy, a tin-carbon composite, a metal oxide, and a porous silicon composite. Combinations including at least two of the foregoing may be used. According to an embodiment, the first electrode active material 11 may be, for example, Figure 2B the porous silicon composite shown. The graphite may be natural graphite or artificial graphite. In addition, since the graphene-silica composite 12 is uniformly dispersed around the first electrode active material 11, the second electrode active material 14, and the carbonaceous conductive material 13, and in the voids, as Figure 1 shown, voids in the electrode can be reduced and surface-to-surface conductive channels can be formed. Although Figure 1 two types of electrode active materials are shown, a single type may also be used.
[0057] The graphene-silica composite includes silica 321 and graphene 312, as Figure 2A shown. The silica 321 may be: a low-valence silicon oxide of the formula SiO x where 0 < x < 2; or a combination of the low-valence silicon oxide and silicon dioxide (SiO 2 ).
[0058] As used herein, the term "low-valence silicon oxide" is represented by the formula SiOx (where 0 < x < 2) represents the composition. Alternatively, the low-valence silica may be, for example, a combination including Si and SiO x (where 0 < x < 2) representing the average composition. 2 of.
[0059] The low-valence silica may exist in the form of a film, a substrate, or a combination thereof.
[0060] According to one embodiment, the graphene-silica composite may be in the following form: particles including low-valence silica (SiO x , 0 < x < 2) and graphene, particles in which the low-valence silica (SiO x , 0 < x < 2) is completely surrounded by graphene, or a combination thereof. The particles including low-valence silica (SiO x , 0 < x < 2) and graphene, particles in which the low-valence silica (SiO x , 0 < x < 2) is completely surrounded by graphene, or a combination thereof may be interconnected with each other in a substrate containing graphene, such as a graphene substrate.
[0061] According to one embodiment, in the particles including low-valence silica and graphene, particles in which the low-valence silica is completely surrounded by graphene, or a combination thereof, the graphene is interconnected to form the substrate containing graphene.
[0062] According to another embodiment, the graphene-silica composite may be in the form of particles in which silica (SiO 2 ) is partially or completely surrounded by low-valence silica (SiO x , 0 < x < 2).
[0063] The graphene-silica composite may also be referred to as a graphene sphere or a graphene spheroid.
[0064] The graphene-silica composite may have any suitable shape that can exist in the voids inside the electrode. The graphene-silica composite may have a wrinkled (crinkled, crumpled) structure. The wrinkled structure according to the embodiment may be, for example, a wrinkled sphere structure. The structure may vary according to the shape of the silica (SiO 2 ) used as the starting material for forming the graphene-silica composite. For example, when the silica (SiO 2 ) is in the form of spherical particles, the graphene-silica composite may have a wrinkled sphere structure such as a wrinkled ball structure. As another example, when the silica (SiO 2 ) is mesoporous silica, the graphene-silica composite may have a rectangular structure.
[0065] The graphene-silica composite according to an embodiment may have a wrinkled sphere structure. The graphene-silica composite according to an embodiment may have a crumpled-spherical paper ball structure. The reduction product of silica (SiO 2 ) such as low-valence silica (SiO x , 0 < x < 2); or low-valence silica (SiO x , 0 < x < 2) and silica (SiO 2 ) may be distributed in the structure.
[0066] In the graphene-silica composite, the silica may be in the form of: particles, tubes, rods, nanowires, nanobelts, fibers, blocks, or combinations thereof.
[0067] For example, the graphene-silica composite may have a popcorn-like graphene sphere structure, for example, having an appearance of fused spheres to provide a fused sphere structure, a faceted sphere structure, or a wrinkled sphere structure, or combinations thereof. The graphene-silica composite may have a popcorn-like graphene sphere structure, for example, a fused sphere structure, as Figure 2A shown in.
[0068] The amount of graphene contained in the graphene-silica composite may range from 0.001 parts by weight to about 90 parts by weight, for example from about 10 parts by weight to about 80 parts by weight, based on the total weight of 100 parts by weight of the composite. When the amount of graphene is within the above range, the conductivity of the graphene-silica composite is considerably improved. For example, the size of the graphene-silica composite may be about 10 nm to about 300 nm, for example about 50 nm to about 200 nm. The size of the graphene-silica composite represents the average particle diameter in the case where the graphene-silica composite is spherical, and represents the length of the major axis in the case where the graphene-silica composite is not spherical.
[0069] In the graphene-silica composite, the graphene may extend from the silica by 10 nm or less, for example 5 nm or less, for example 3 nm or less, for example 1 nm or less, for example in the range of about 0.0001 nm to about 1 nm, about 0.001 nm to about 0.1 nm, or about 0.01 nm. The graphene-silica composite may include about 1 to about 20 graphene layers, for example about 1 to about 10 graphene layers, and the total thickness of the graphene layers may be about 0.6 nm to about 12 nm, or about 1 nm to about 10 nm.
[0070] The degree of adhesion between silica and graphene can be evaluated by measuring the distance between silica and graphene using a scanning electron microscope. The graphene can extend from the silica a distance of 10 nm or less, such as a distance of 1 nm or less. The graphene can be oriented at an angle of 0 - 90° relative to the long axis of, for example, a low-valence silica of the formula SiO x where 0 < x < 2, silica (SiO 2 ), or a combination thereof. In this regard, the long axis can refer to the Y axis. The graphene-silica composite can include at least 1 to about 20 graphene layers, and the total thickness of the graphene layers can be about 0.6 nm - about 12 nm. The graphene can be oriented at an angle of 0 - 90° relative to the long axis of the silica.
[0071] The graphene-silica composite according to an embodiment can be manufactured according to the following method.
[0072] A reaction gas including a carbon source gas is supplied to a structure including silica (SiO 2 ), and the structure is heat-treated.
[0073] The carbon source gas can include a compound represented by Formula 2 below, or can be a mixed gas including a compound represented by Formula 2 and a compound represented by Formula 1, an oxygen-containing gas represented by Formula 3, or a combination thereof.
[0074] Formula 1
[0075] C n H (2n+2-a) [OH] a
[0076] In Formula 1, n is 1 - 20 and a is 0 or 1.
[0077] Formula 2
[0078] C n H (2n)
[0079] In Formula 2, n is 2 - 6.
[0080] Formula 3
[0081] C x H y O z
[0082] In Formula 3, x is 0 or an integer from 1 - 20, y is 0 or an integer from 1 - 20, and z is 1 or 2. Further, in Formulas 1 and 2, n is independently selected.
[0083] For example, the carbon source gas may include methane, ethylene, propylene, methanol, ethanol, propanol, acetylene, or a combination thereof, and may be, for example, methane. The oxygen-containing gas may be, for example, carbon dioxide (CO 2 ), carbon monoxide (CO), water vapor (H 2 O), or a combination thereof.
[0084] After supplying the reaction gas of the carbon source gas to silicon dioxide (SiO 2 ) and heat-treating the mixture, the resultant may be further subjected to a cooling process using at least one inert gas such as nitrogen, helium, argon, or a combination thereof. In this regard, the cooling process refers to a process in which the temperature is returned to room temperature (i.e., in the range of 20°C - 25°C).
[0085] The carbon source gas may further include an inert gas such as nitrogen, helium, argon, or a combination thereof. The heat treatment may be performed at a temperature of about 700°C - about 1100°C.
[0086] In addition, since graphene is coated on low-valent silicon oxide (SiO 2 ), which is a reduction product of silicon dioxide (SiO x , 0 < x < 2), or a combination of low-valent silicon oxide (SiO x , 0 < x < 2) and silicon dioxide (SiO 2 ) through a gas-phase reaction, a coating film having high crystallinity may be formed. When such a graphene-silica composite is used as a conductive agent, the conductivity of the electrode active material may be increased without structural change.
[0087] Throughout the specification, the porous silicon composite includes a porous core having porous silicon secondary particles and a shell formed on at least one surface of the porous core and including first graphene. In this regard, the porous silicon secondary particles may include a plurality of silicon composite primary particles, and the silicon composite primary particles of the plurality of silicon composite primary particles may include silicon, low-valent silicon oxide (SiO x , 0 < x < 2) on the silicon, and second graphene provided on at least one surface of the low-valent silicon oxide (SiO x , 0 < x < 2).
[0088] The porous silicon composite and a method for manufacturing the same are disclosed in Korean Patent Application Laid-Open No. 10-2018-0031585, the content of which is incorporated herein by reference in its entirety.
[0089] According to another embodiment, there is provided an electrode for a lithium battery including the above-described electrode composite conductive agent.
[0090] For example, the electrode may be a negative electrode.
[0091] The negative electrode may include any suitable negative electrode active material used in lithium batteries such as carbonaceous materials, silicon-based materials, silicon oxides, silicon-based alloys, silicon-carbonaceous material composites, tin, tin-based alloys, tin-carbon composites, metal oxides, porous silicon composites, or combinations thereof.
[0092] For example, the negative electrode active material may include a porous silicon composite and a carbonaceous material. When the porous silicon composite is used as the negative electrode active material, the volume expansion of the negative electrode is suppressed and the conductivity can be improved, thereby improving the rate characteristics. In this regard, the amount of the carbonaceous material may be about 0.001 parts by weight to about 99.999 parts by weight, for example, about 10 parts by weight to about 98 parts by weight, for example, about 20 parts by weight to about 95 parts by weight, for example, about 30 parts by weight to about 92 parts by weight, for example, about 50 parts by weight to about 90 parts by weight, based on 100 parts by weight of the total weight of the porous silicon composite and the carbonaceous material. When the amount of the carbonaceous material is within the above range, a lithium battery with improved charge / discharge rate characteristics, life characteristics, and improved capacity retention can be provided.
[0093] For example, the carbonaceous material may include plate-like graphite, spherical graphite, uneven graphite, or a combination thereof. The carbonaceous material can compensate for the instability of the electrode caused by the high capacity when the porous silicon composite is used alone, and the capacity characteristics and the charge and discharge rate characteristics can be further improved.
[0094] Hereinafter, a method of preparing an electrode for a lithium battery according to an embodiment will be further described.
[0095] First, an electrode active material, a carbonaceous conductive material, and a graphene-silica composite are dry mixed to obtain a mixture. The dry mixing is performed in a mixer so that the graphene-silica composite is uniformly dispersed in the mixture together with the electrode active material and the carbonaceous conductive material without aggregation. Without such a dry mixing process, the graphene-silica composite may aggregate, and therefore the mixing and dispersion of the graphene-silica composite with other components may not be satisfactory.
[0096] In dry mixing, for example, a Nobilta mixer or a Thinky mixer may be used as the mixer, and the rotation speed of the mixer may be in the range of about 100 rpm to about 800 rpm, for example, 300 rpm. The mixing time varies depending on the rotation speed, etc., and may be, for example, in the range of about 10 minutes to about 100 minutes.
[0097] When the electrode is a negative electrode, a negative electrode active material is used as the electrode active material, and examples of the negative electrode active material may include carbonaceous materials, silicon, silicon oxide, silicon-based alloys, silicon-carbonaceous material composites, tin, tin-based alloys, tin-carbon composites, metal oxides, or combinations thereof. For example, the negative electrode active material may be a mixture of the porous silicon composite and the carbonaceous material.
[0098] Next, a binder and a solvent are added to the dry-mixed mixture and mixed with the dry-mixed mixture to prepare an electrode active material composition. In addition, the graphene-silicon composite is selected to be about 20 parts by weight or less, based on 100 parts by weight of the total weight of the carbonaceous conductive material and the graphene-silicon composite. In this regard, the total weight of the carbonaceous conductive material and the graphene-silicon composite refers to the total weight of the composite conductive agent.
[0099] The amount of the composite conductive agent in the electrode may be, for example, about 0.1 to about 10 parts by weight, about 0.5 to about 8 parts by weight, or about 1 to about 5 parts by weight based on 100 parts by weight of the total weight of the electrode.
[0100] The binder may be a binder suitable for preparing an electrode of a lithium battery. Examples of the binder include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), styrene butadiene rubber polymer, polyacrylic acid, polyamide imide, polyimide, or a combination thereof.
[0101] The solvent may be N-methylpyrrolidone, acetone, water, etc. However, the solvent is not limited thereto and may be any suitable solvent available in the art.
[0102] Figure 2B A porous silicon composite according to an embodiment is described.
[0103] Reference Figure 2B , the porous silicon composite 310 includes a core 31 including a porous silicon secondary particle and a shell 32 formed on the core 31 and including a first graphene 310 a .
[0104] The porous silicon secondary particles include aggregates of a plurality of silicon composite primary particles, and the silicon composite primary particles of the plurality of silicon composite primary particles may include silicon 311 and second graphene 310b disposed on the silicon 311. Since the second graphene 310b forms a shell on the surface of the silicon oxide of the silicon composite primary particles, and the first graphene 310a forms a shell 32 on the surface of the core 31 of the silicon composite secondary particles, the porous silicon composite 310 has a double core / shell structure. Such a double core / shell structure can prevent volume expansion and penetration of the electrolyte solution, thereby reducing or preventing side reactions occurring between the electrolyte solution and the electrode active material.
[0105] Low-valent silicon oxide (SiO x , O < x < 2) may be further disposed on the silicon 311. The second graphene 310b may be located on the low-valent silicon oxide (SiO x , 0 < x < 2). Although Figure 2B the silicon 311 shown in has a flaky shape or a needle-like shape, the silicon 311 may also have a spherical particle shape.
[0106] The second graphene 310b of the core 31 may have the same or different layers as the first graphene 310a of the shell 32. According to an embodiment, the first graphene 310a of the shell 32 may have a higher density than the density of the second graphene 310b of the core 31. According to an embodiment, the second graphene 310b may have about 1 layer - about 30 layers, such as about 5 layers - about 15 layers, particularly about 10 layers in the core, and the first graphene 310a may have about 1 layer - about 50 layers, such as about 20 layers - about 30 layers in the shell 32.
[0107] According to an embodiment, an outer layer having a higher density than the density of the core 31 may be present. Although the thickness of the outer layer is not limited, the outer layer may have a thickness of, for example, about 20 nm - about 60 nm.
[0108] The core 31 and the shell 32 may further include graphite.
[0109] In the porous silicon composite, the core may have a diameter of about 3 μm - about 10 μm, and the shell may have a thickness of about 10 nm - about 5,000 nm (about 0.01 μm - about 5 μm), such as about 10 nm - about 1,000 nm. The ratio of the diameter of the core of the porous silicon composite to the thickness of the shell (carbonaceous coating film) may be about 1:0.001 - about 1:1.67, such as 1:0.001, 1:1.67, 1:0.0033, or 1:0.5.
[0110] In the porous silicon composite, the total amount of the first graphene and the second graphene may be about 0.1 parts by weight to about 2,000 parts by weight, such as about 0.1 parts by weight to about 300 parts by weight, such as about 0.1 parts by weight to about 90 parts by weight, particularly about 5 parts by weight to about 30 parts by weight, based on 100 parts by weight of the silicon. When the total amount of the first graphene and the second graphene is within the above range, an improved effect of suppressing the volume expansion of silicon and improved conductivity can be obtained.
[0111] In the composite primary particle, the second graphene may extend from low-valence silicon oxide (SiO x , 0 < x < 2) a distance of about 10 nm or less, such as about 1 nm or less, such as about 0.00001 nm to about 1 nm, including at least one graphene layer, such as about 1 to about 30 graphene layers, having a total thickness of about 0.3 nm to about 50 nm, such as about 0.6 nm to about 50 nm, such as about 1 nm to about 30 nm, and being oriented at an angle of 0 - 90° with respect to the long axis of the silicon. In this regard, the long axis may be the Y axis.
[0112] In the porous silicon composite, the first graphene may extend from the low-valence silicon oxide (SiO x , 0 < x < 2) a distance of about 1,000 nm or less, such as about 500 nm or less, such as about 10 nm or less, such as about 1 nm or less, such as about 0.00001 nm to about 1 nm, including at least one graphene layer, such as about 1 to about 30 graphene layers, having a total thickness of about 0.6 nm to about 50 nm, such as about 1 nm to about 50 nm, and may be oriented at an angle of 0 - 90° with respect to the long axis of the silicon. The low-valence silicon oxide (SiO x , 0 < x < 2) located on the silicon may have a thickness of about 30 μm or less, such as about 10 nm.
[0113] The porous silicon clusters can be regarded as secondary particles.
[0114] The average particle diameter D50 of the porous silicon secondary particles may be about 200 nm to about 50 μm, such as about 1 μm to about 30 μm, such as about 2 μm to about 25 μm, such as about 3 μm to about 20 μm, such as about 3 μm to about 10 μm, such as about 1 μm to about 15 μm, particularly about 7 μm to about 11 μm. The particle diameter D10 of the porous silicon secondary particles may be about 0.001 μm to about 10 μm, such as about 0.005 μm to about 5 μm, such as about 0.01 μm to about 1 μm. Additionally, the particle diameter D90 of the porous silicon secondary particles may be about 10 μm to about 60 μm, such as about 12 μm to about 28 μm, such as about 14 μm to about 26 μm. Additionally, the porous silicon secondary particles may have about 0.1 m2 / g-about 100m 2 / g, for example, about 1m 2 / g-about 30m 2 / g, for example, about 1m 2 / g-about 10m 2 / g, for example, about 1m 2 / g-about 5m 2 In addition, the porous silicon secondary particles may have a density of about 0.1 g / cc to about 2.8 g / cc, such as about 0.1 g / cc to about 2.57 g / cc, such as about 0.5 g / cc to 2 g / cc, such as about 1.1 g / cc to about 1.2 g / cc, such as about 1.18 g / cc.
[0115] The surface of the porous silicon composite may further include a carbonaceous coating film. Although the initial efficiency is reduced by using the carbonaceous coating film, a lithium battery with improved life characteristics can be prepared. The carbonaceous coating film includes amorphous carbon that promotes the migration of lithium. The carbonaceous coating film may cover the surface area of the porous silicon composite in whole or in part. The coverage of the carbonaceous coating film may be about 10% to about 99%, for example, about 20% to about 95%, for example, about 40% to about 90%, based on the surface area of the porous silicon composite.
[0116] The ratio of the diameter of the porous silicon composite to the thickness of the carbonaceous coating film is about 1:1 to about 1:50, for example, about 1:1 to about 1:40.
[0117] The carbonaceous coating film may have a thickness of about 1 nm to about 5,000 nm, for example, about 10 nm to about 2,000 nm.The carbonaceous coating film includes a carbonaceous material.
[0118] In the carbonaceous coating film, the amorphous carbon may include pitch carbon, soft carbon, hard carbon, mesophase pitch carbonization product, sintered coke, carbon fiber, or a combination thereof. The carbonaceous coating film may be a nonporous continuous coating film and may have a thickness of about 1 nm to about 5000 nm.
[0119] The carbonaceous coating film may further include crystalline carbon. The crystalline carbon may more effectively buffer the volume expansion of the porous silicon composite. The crystalline carbon may include natural graphite, artificial graphite, graphene, fullerene, carbon nanotube, or a combination thereof.
[0120] The carbonaceous coating film may have a single-layer structure including amorphous carbon and crystalline carbon. The carbonaceous coating film may also have a double-layer structure including a first carbonaceous coating film including amorphous carbon and a second carbonaceous coating film including crystalline carbon.
[0121] The silicon constituting the porous silicon composite may have a variety of shapes such as needle-shaped particles, spherical particles, nanowires, nanobelts, rods, or combinations thereof. The silicon may have an average particle diameter of about 10 nm to about 30 μm, such as about 20 nm to about 150 nm, such as about 40 to about 100 nm. When the silicon is in the form of needle-shaped particles, each needle-shaped particle may have a length of about 100 nm to about 160 nm, such as about 108 nm to about 125 nm, and a thickness of about 10 nm to about 100 nm, such as about 20 nm to about 50 nm, particularly 40 nm.
[0122] Each of the first graphene and the second graphene may be a polycyclic aromatic molecule formed by a plurality of carbon atoms covalently bonded to each other, and the covalently bonded carbon atoms constitute a 6-membered ring as a basic repeating unit, but the graphene may further include a 5-membered and / or 7-membered carbon ring. As a result, the graphene as a covalently bonded carbon atom (having sp 2 The graphene may be formed as a single layer. However, a plurality of graphene layers may be stacked to form a multilayer structure. For example, the graphene may have 1 layer to 100 layers, 2 layers to 100 layers, or 3 layers to 50 layers.
[0123] The first graphene and the second graphene may each have a structure of a nanosheet, a layer (film), or a scale. The term "nanosheet" refers to an irregular structure of graphene formed on silicon oxide, and the term "layer" refers to a continuous, uniform film of graphene formed on silicon oxide.
[0124] The second graphene may cover the surface of the silicon in whole or in part. When the subvalent silicon oxide is located on silicon, the second graphene may cover the surface of the subvalent silicon oxide in whole or in part. For example, the coverage of the second graphene on the silicon or subvalent silicon oxide may be about 10%-about 99%, such as about 20%-about 95%, such as about 40%-about 90%, based on the surface area of the silicon or subvalent silicon oxide. In addition, the first graphene may cover the surface of the porous silicon secondary particles in whole or in part. For example, the coverage of the first graphene may be about 10%-about 99%, such as about 20%-about 95%, such as about 40%-about 90%, based on the surface area of the porous silicon secondary particles.
[0125] The porous silicon composite according to an embodiment may have a spherical shape and a sphericity of, for example, 0.9 or less, for example, about 0.7 to about 0.9, for example, about 0.85 to about 0.9.
[0126] The first graphene and the second graphene can be any suitable carbonaceous material in the form of flakes, respectively. Examples of the carbonaceous material include graphene, graphite, carbon fiber, graphite carbon, graphene oxide, or a combination thereof.
[0127] In the porous silicon composite according to the embodiment, the size of the graphene can be from about 10 nm to about 100 nm. In this regard, the size refers to the diameter or the length of the major axis.
[0128] In the porous silicon composite, the amounts of the first graphene and the second graphene can be from about 0.1 parts by weight to about 2,000 parts by weight, such as from about 0.1 parts by weight to about 300 parts by weight, such as from about 0.1 parts by weight to about 90 parts by weight, particularly from about 5 parts by weight to about 30 parts by weight, based on 100 parts by weight of silicon. When the amounts of the first graphene and the second graphene are each within the above range, the first graphene and the second graphene can have an improved effect on suppressing volume expansion and improved electrical conductivity. The first graphene and the second graphene can be, for example, graphene flakes.
[0129] In the porous silicon secondary particle according to the embodiment, the first graphene is in the form of graphene flakes, and the graphene flakes extend from the low-valence silicon oxide (SiO x , O<x<2) a distance of 1,000 nm or less, such as 500 nm or less, such as 10 nm or less, such as 1 nm or less, such as from about 0.00001 nm to about 1 nm, including at least one graphene layer, such as from about 1 graphene layer to about 30 graphene layers, having a total thickness of about 0.6 nm to about 50 nm, such as about 1 nm to about 50 nm, and are oriented at an angle of 0° - 90°, such as 10° - 80°, such as 20° - 70° with respect to the major axis (e.g., the Y-axis) of the silicon.
[0130] In the silicon composite primary particle, the second graphene is in the form of graphene flakes, and the graphene flakes extend from the low-valence silicon oxide (SiO x , 0<x<2) a distance of about 10 nm or less, such as about 5 nm or less, such as about 3 nm or less, such as about 1 nm or less, including graphene layers, having a total thickness of about 1,000 nm or less, such as from about 0.3 nm to about 1,000 nm, such as from about 0.3 nm to about 50 nm, such as about 0.6 nm to about 50 nm, such as about 1 nm to about 30 nm, and are oriented at an angle of 0° - 90°, such as 10° - 80°, such as 20° - 70° with respect to the major axis (e.g., the Y-axis) of the silicon. In this regard, the major axis refers to the Y-axis.
[0131] The low-valence silicon oxide (SiO x, (0 < x < 2) may have a thickness of about 30 μm or less, such as about 10 μm or less, such as about 1 nm - about 100 nm, such as about 10 nm. The low-valent silicon oxide may cover all or part of the surface of the silicon. The coverage rate of the low-valent silicon oxide may be about 10% - about 99%, such as about 20% - about 95%, such as about 40% - about 90%, based on the surface area of the silicon.
[0132] The lithium battery according to an embodiment includes the electrode. The electrode may be a negative electrode. The negative electrode may be prepared according to the above method.
[0133] Next, a positive electrode is prepared according to the following process.
[0134] The positive electrode active material, a conductive agent, a binder, and a solvent are mixed to prepare a positive electrode active material composition. The positive electrode active material composition is directly coated on a metal current collector and dried to prepare a positive electrode plate. Alternatively, the positive electrode active material composition may be cast on a separate carrier, and the film separated from the carrier is laminated on a metal current collector to prepare a positive electrode plate.
[0135] The positive electrode active material may include at least one selected from the following: lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate oxide, and lithium manganese oxide. However, the positive electrode active material is not limited thereto, and any suitable positive electrode active material used in the art may also be used.
[0136] For example, the positive electrode active material may be any suitable lithium-containing metal oxide used in the art, without limitation. For example, a composite oxide of lithium and at least one selected from cobalt, manganese, nickel, and any combination thereof may be used, particularly, a compound represented by any of the following formulas: Li a A 1-b B’ b D 2 (where 0.90 ≤ a ≤ 1 and 0 ≤ b ≤ 0.5); Li a E 1-b B’ b O 2-c D c (where 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, and 0 ≤ c ≤ 0.05); LiE 2-b B’ b O 4-c D c (where 0 ≤ b ≤ 0.5 and 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B’ c D α(where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤2); Li a Ni 1-b-c Co b B' c O 2-α F' α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b- c Co b B' c O 2-α F' 2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Mn b B' c D α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤2); Li a Ni 1-b-c Mn b B' c O 2-α F' α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Mn b B' c O 2-α F' 2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni b E c G d O 2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, and 0.001≤d≤0.1); Li a Ni b Co c Mn d G e O 2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, and 0.001≤e≤0.1); Li a NeG b O 2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li aCoG b O 2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a MnG b O 2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a Mn 2 G b O 4 (where 0.90≤a≤1 and 0.001≤b≤0.1); QO 2 ;QS 2 ;LiQS 2 ; V 2 O 5 ;LiV 2 O 5 ;LiI'O 2 ;LiNiVO 4 ;Li (3-f) J 2 (PO 4 ) 3 (where 0≤f≤2); Li (3-f) Fe 2 (PO 4 ) 3 (where 0≤f≤2); and LiFePO 4 .
[0137] In the above formula, A is nickel (Ni), cobalt (Co), manganese (Mn), or any combination thereof; B' is aluminum (Al), nickel (Ni), cobalt (Co), manganese (Mn), chromium (Cr), iron (Fe), magnesium (Mg), strontium (Sr), vanadium (V), rare earth elements, or any combination thereof; D is oxygen (O), fluorine (F), sulfur (S), phosphorus (P), or any combination thereof; E is cobalt (Co), manganese (Mn), or any combination thereof; F' is fluorine (F), sulfur (S), phosphorus (P), or any combination thereof ; G is aluminum (Al), chromium (Cr), manganese (Mn), iron (Fe), magnesium (Mg), lanthanum (La), cerium (Ce), strontium (Sr), vanadium (V), or any combination thereof; Q is titanium (Ti), molybdenum (Mo), manganese (Mn), or any combination thereof; I' is chromium (Cr), vanadium (V), iron (Fe), scandium (Sc), yttrium (Y), or any combination thereof; and J is vanadium (V), chromium (Cr), manganese (Mn), cobalt (Co), nickel (Ni), copper (Cu), or any combination thereof.
[0138] The compounds listed above may have a coating layer on their surface. Alternatively, a mixture of a compound without a coating layer and a compound with a coating layer may be used, the compound being selected from the compounds listed above. The coating layer may include a compound of a coating element, such as an oxide, hydroxide, oxyhydroxide, oxycarbonate, or hydroxycarbonate of the coating element. The compound constituting the coating layer may be amorphous or crystalline. Examples of the coating elements contained in the coating layer may be Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or any mixture thereof. The coating layer may be formed on a compound used as the positive active material by using the coating element via any method such as spraying and impregnation that does not adversely affect the physical properties of the positive active material. The method is clear to those skilled in the art, and therefore its detailed description will be omitted.
[0139] For example, the positive electrode active material may be LiNiO 2 、LiCoO 2 、LiMn x O 2x (where x = 1 or 2), LiNi 1- x Mn x O 2 (where 0 <x<1)、LiNi 1-x-y Co x Mn y O 2 (where 0≤x≤0.5 and 0≤y≤0.5), LiFeO 2 、V 2 O 5 , TiS, MoS, etc.
[0140] The conductive agent, binder, and solvent of the positive active material composition may be the same as those of the negative active material composition. In addition, a plasticizer may be further added to the positive active material composition and / or the negative active material composition to form pores in the electrode.
[0141] The amounts of the positive electrode active material, the conductive agent, the binder, and the solvent may be at the same levels as those used in a lithium battery. Depending on the purpose and structure of the lithium battery, at least one of the conductive agent, the binder, and the solvent may be omitted.
[0142] Subsequently, a separator to be inserted between the positive electrode and the negative electrode is prepared. The separator may be any suitable separator used in the art. Any suitable separator having low resistance to the migration of ions in the electrolyte and excellent electrolyte retention capacity may be used. For example, glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or any combination thereof, each of which may be a nonwoven or woven fabric, may be used. For example, a windable separator including polyethylene, polypropylene, etc. may be used in a lithium ion battery, and a separator having excellent electrolyte retention capacity may be used in a lithium ion polymer battery. For example, the separator may be prepared according to the following method.
[0143] A polymer resin, a filler and a solvent are mixed to prepare a separator composition. The separator composition may be directly coated on an electrode and dried to form a separator. Alternatively, the separator composition may be cast on a support and dried, and a separator film separated from the support may be laminated on the electrode to prepare a separator.
[0144] The polymer resin used to prepare the separator is not particularly limited and may be any suitable material used as a binder for an electrode plate. For example, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or any suitable mixture thereof may be used.
[0145] The separator may include a ceramic component to improve the performance of the separator as a membrane. For example, in the preparation of the separator, the separator may be coated with an oxide or may include ceramic particles.
[0146] Subsequently, an electrolyte is prepared. For example, the electrolyte may be an organic electrolyte solution. In addition, the electrolyte may be a solid. For example, the electrolyte may be boron oxide, lithium oxynitride, etc. However, the electrolyte is not limited thereto and any suitable material that can be used as a solid electrolyte in the art may also be used. The solid electrolyte may be formed on the negative electrode by sputtering, etc.
[0147] For example, the organic electrolyte solution may be prepared by dissolving a lithium salt in an organic solvent.
[0148] The organic solvent may be any suitable organic solvent used in the art. For example, the organic solvent may include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, cyclopentane, ethylene dichloride, chlorobenzene, nitrobenzene, glycol ether, dimethyl ether, or any mixture thereof.
[0149] The lithium salt may be any suitable lithium salt used in the art. For example, the lithium salt may be LiPF 6 , LiBF 4 、LiSbF 6 、LiAsF 6 、LiClO 4 、LiCF 3 SO 3 、Li(CF 3 SO 2 ) 2 N、Li(FSO 2 ) 2 N, LiC 4 F 9 SO 3 、LiAlO 2 、LiAlCl 4 、LiN(C x F 2x+1 SO 2 )(C y F 2y+1 SO 2 )(wherein x and y are natural numbers), LiCl, LiI, or any mixture thereof.
[0150] like Fig.13 As shown in , the lithium battery 121 includes a positive electrode 123, a negative electrode 122, and a separator 124. The positive electrode 123, the negative electrode 122, and the separator 124 may be wound or folded and then contained in a battery case 125. Then, the battery case 125 may be filled with an organic electrolyte solution and sealed with a cap assembly 126 to complete the manufacture of the lithium battery 121. The battery case 125 may be cylindrical, rectangular, or thin-film. For example, the lithium battery 121 may be a thin-film battery. The lithium battery may be a lithium-ion battery.
[0151] The separator 124 can be inserted between the positive electrode 123 and the negative electrode 122 to form a battery assembly. Multiple such battery assemblies can be stacked in a dual-cell battery structure and impregnated with an organic electrolyte solution. The resulting battery assembly can be placed in a bag and sealed to complete the manufacture of a lithium-ion polymer battery.
[0152] In addition, multiple such battery assemblies can be stacked to form a battery pack, which can be used in any device that requires high capacity and high output, such as a laptop computer, a smartphone, and an electric vehicle.
[0153] The lithium battery can be suitable for use as a power source for an electric vehicle (EV) due to its improved high-rate characteristics and life characteristics. For example, the lithium battery can be suitable for a hybrid vehicle such as a plug-in hybrid electric vehicle (PHEV). For example, the lithium battery is suitable for a long-life electric vehicle with fast charging characteristics.
[0154] Hereinafter, the present disclosure will be described in more detail based on the following examples and comparative examples. However, the following examples are only provided to illustrate the present disclosure, and the scope of the present disclosure is not limited thereto.
[0155] Examples
[0156] Preparation Example 1: Preparation of a porous silicon composite
[0157] 25 parts by weight of plate-like and needle-like silicon, 10 parts by weight of stearic acid, and 65 parts by weight of isopropyl alcohol were mixed to prepare a composition. The composition was spray-dried and then dried to obtain porous silicon secondary particles having an average particle diameter of about 4.5 μm. A low-valent silicon oxide (SiO x , 0 < x < 2) film (having a thickness of about 0.1 nm - about 10 nm) was formed on the surface of the silicon. The spray drying was carried out using a spray dryer (model: MMSD Micro Mist Spray Dryers, Fujisaki Electric). In an N 2 atmosphere, isopropyl alcohol was dried by adjusting the size and pressure of the nozzle and the temperature of the powder spray atmosphere (about 200 °C). The size of the nozzle was controlled to be about 150 μm, and the pressure of the nozzle was adjusted to be about 0.58 MPa. The porous silicon secondary particles were loaded into a reactor. The reactor was purged with nitrogen, and then a gas mixture of CH 4 and CO 2 as a reaction gas (CH 4 :CO 2=80:20) flows into the reactor to form an atmosphere of the gas. The pressure generated by the flow of the gas in the reactor is 1atm. Under the atmosphere of the gas, the internal temperature of the reactor is raised to 1000°C (at a rate of about 23°C / minute), and then heat-treated at the temperature for 1 hour while the gas is continuously supplied to the reactor. Then, the resultant is kept for about 3 hours. Then, the supply of the gas is stopped, the reactor is cooled to room temperature (25°C), and nitrogen is purged in the reactor to obtain a porous silicon composite. At this point, the porous silicon composite is in the form of a cluster.
[0158] In the porous silicon composite, a total amount of the first graphene and the second graphene is about 25 parts by weight based on 100 parts by weight of the total weight of the porous silicon composite.
[0159] Preparation Example 2: Preparation of Graphene-Silica Composite (Graphene Spheres)
[0160] The calcined SiO 2 The particles (having an average particle diameter of about 20 nm to about 30 nm) are loaded in a reactor and CH 4 The internal temperature of the reactor was increased to 1000° C. over 30 minutes while being supplied into the reactor at a rate of about 300 sccm at 1 atm.
[0161] Then, heat treatment was performed at the temperature for 7 hours. Then, while the reactor was purged with nitrogen, the temperature of the reactor was adjusted to room temperature (20-25° C.) to obtain a graphene-silica composite.
[0162] Example 1: Preparation of negative electrode and full unit cell
[0163] The porous silicon composite (SCN) prepared according to Preparation Example 1, artificial graphite (CG1, having a particle diameter of 11.7 μm and a particle diameter of 1.4 μm) and 2 / g specific surface area), flake graphite as a carbonaceous conductive material (SFG6, Timcal, AG, with a particle diameter of 4 μm and a specific surface area of 17 m 2 / g specific surface area), and the graphene-silica composite (GB, having a particle diameter of 50 nm and a specific surface area of 200 m 2 The mixture was dry-blended in a mixer at about 1500 rpm for about 3 minutes to obtain a mixture.
[0164] Polyvinyl alcohol as a binder and water were added to the mixture and mixed at 25° C. for 40 minutes to obtain a negative electrode active material slurry. The mixing ratio of each component in the negative electrode active material slurry is shown in Table 1 below.
[0165] The negative electrode active material slurry was coated on a copper (Cu) foil using a doctor blade to form a film having a thickness of 20 μm. The film was vacuum dried at 130° C. for 3 hours and roll-pressed to prepare a negative electrode.
[0166] Use LiNi 0.6 Co 0.2 Mn 0.2 O 2 、LiNi 0.6 Co 0.2 Al 0.2 O 2 The positive electrode is prepared by mixing a positive electrode active material slurry obtained by mixing LiNi 200,0 ... 0.6 Co 0.2 Mn 0.2 O 2 、LiNi 0.6 Co 0.2 Al 0.2 O 2 The mixing weight ratio of Super P and polyvinylidene fluoride as a binder is 75.2:18.8:3:3.
[0167] A full unit cell was prepared using the negative electrode and the positive electrode. The positive electrode active material slurry was coated on an aluminum (Al) foil using a doctor blade to form a film having a thickness of 40 μm. The film was vacuum dried at 120° C. for 2 hours and roll-pressed to prepare a positive electrode.
[0168] A polypropylene film (Celgard 3510) was used as a separator, and a 1.15 M LiPF was dissolved in a mixed solvent of EC, EMC, and DMC (mixed in a volume ratio of 2:4:4). 6 Here, EC is ethylene carbonate, EMC is ethyl methyl carbonate, and DMC is dimethyl carbonate.
[0169] Table 1
[0170]
[0171]
[0172] In Table 1, the amount of the composite conductive agent is calculated based on 100 parts by weight of the total weight of the active material and the conductive agent, and the amount of GB is calculated based on 100 parts by weight of the total weight of the composite conductive agent (total weight of SFG6+GB).
[0173] Examples 2, 3, and 3a: Preparation of negative electrodes and full-cell batteries
[0174] Full-cell batteries were prepared in the same manner as in Example 1, except that the composition of the negative active material slurry was changed as shown in Table 1.
[0175] Comparative Example 1: Preparation of negative electrode and full unit cell
[0176] A full-cell was prepared in the same manner as in Example 1, except as follows: a negative electrode was prepared according to the following procedure.
[0177] The porous silicon composite (SCN) prepared according to Preparation Example 1, artificial graphite (CG1), flake graphite (SFG6, Timcal, AG, with a particle diameter of 4 μm) as a carbonaceous conductive material, polyvinyl alcohol (PVA) as a binder, and water were mixed at 25° C. for 40 minutes to prepare a negative electrode active material slurry. The mixing ratio of each component in the negative electrode active material slurry is shown in Table 2 below. The negative electrode active material slurry was coated on a Cu foil using a doctor blade to form a film with a thickness of 20 μm. The film was vacuum dried at 130° C. for 3 hours and rolled to prepare a negative electrode.
[0178] Table 2
[0179]
[0180]
[0181] In Table 2, the amount of the conductive agent is calculated based on 100 parts by weight of the total weight of the negative active material and the conductive agent, and the amount of GB is calculated based on 100 parts by weight of the total weight of the conductive agent.
[0182] Comparative Example 2: Preparation of negative electrode and full unit cell
[0183] A full-cell battery was prepared in the same manner as in Comparative Example 1, except that the composition of the negative active material slurry was changed as shown in Table 2.
[0184] Comparative Example 1a: Preparation of negative electrode and full cell
[0185] A full-cell battery was prepared in the same manner as in Comparative Example 1, except that the composition of the negative active material slurry was changed as shown in Table 2.
[0186] Example 4: Preparation of negative electrode and coin half-cell
[0187] The porous silicon composite (SCN) prepared according to Preparation Example 1, artificial graphite (CG1, having a particle diameter of 11.7 μm and a particle diameter of 1.4 μm) and 2 / g specific surface area), flake graphite as a carbonaceous conductive material (SFG6, Timcal, AG, with a particle diameter of 4 μm and a specific surface area of 17 m 2 / g specific surface area), and graphene-silica composite (GB, with a particle diameter of 50nm and a specific surface area of 100m 2 The mixture was dry-blended in a mixer at about 1500 rpm for about 3 minutes to obtain a mixture.
[0188] Binder polyvinyl alcohol and water were added to the dry-mixed mixture and mixed at 25° C. for 40 minutes to obtain a negative active material slurry. The mixing ratio of each component in the negative active material slurry was as shown in Table 1 above.
[0189] The negative electrode active material slurry was coated on a Cu foil using a doctor blade to form a film having a thickness of 20 μm. The film was vacuum dried at 130° C. for 3 hours and roll-pressed to prepare a negative electrode.
[0190] A coin half-unit cell was prepared using the negative electrode and lithium metal as a counter electrode.
[0191] A polypropylene film (Celgard 3510) was used as a separator, and a 1.0 M LiPF was dissolved in a mixed solvent of ethylene carbonate (EC), diethyl carbonate (DEC), and fluoroethylene carbonate (FEC) (mixed in a volume ratio of 5:70:25). 6 The prepared electrolyte
[0192] Examples 5 and 6: Preparation of negative electrode and coin half-cell
[0193] Coin half cells were prepared in the same manner as in Example 4, except that the negative electrodes prepared according to Examples 2 and 3, respectively, were used.
[0194] Example 6a: Preparation of negative electrode and coin half-cell
[0195] A coin half cell was prepared in the same manner as in Example 4, except that the negative electrode prepared according to Example 3a was used.
[0196] Comparative Examples 3 and 4: Preparation of Negative Electrode and Coin Half Cell
[0197] Coin half-unit cells were prepared in the same manner as in Example 4, except that the negative electrodes prepared according to Comparative Examples 1 and 2, respectively, were used.
[0198] Comparative Example 3a: Preparation of negative electrode and coin half-cell
[0199] A coin half cell was prepared in the same manner as in Example 4, except that the negative electrode prepared according to Comparative Example 1a was used.
[0200] Evaluation Example 1: Electron Microscope Analysis
[0201] The negative electrodes of the full-unit cells prepared according to Example 1 and Comparative Example 1 were analyzed by scanning electron microscopy (SEM) and energy dispersive spectroscopy (EDS). Nova NanoSem 450S, (FEI) was used as a scanning electron microscope.
[0202] The electron microscope analysis results of the negative electrodes of the full-cell batteries according to Example 1 and Comparative Example 1 are shown in Figure 3A and 4 middle. Figure 3A The region indicated by the arrow in FIG. 8 is a region where the graphene-silica composite is observed.
[0203] like Figure 3A and 4 As shown in , it was confirmed that, unlike the negative electrode according to Comparative Example 1, in the negative electrode according to Example 1, spherical particles of the graphene-silica composite having a size of several tens of nanometers were uniformly dispersed around the active material and the carbonaceous conductive material.
[0204] Evaluation Example 2: EDS surface scanning analysis
[0205] EDS surface scanning analysis was performed on the negative electrode of the full unit cell prepared according to Example 1. Nova NanoSem 450S EDS manufactured by FEI was used as an analyzer for the EDS surface scanning analysis.
[0206] The EDS analysis results of the negative electrode of the full-cell battery according to Example 1 are shown in Figure 3B middle.
[0207] like Figure 3B As shown in , silicon was detected in the porous silicon composite region, and it was confirmed that the silicon of the graphene-silica composite was dispersed throughout the negative electrode.
[0208] Evaluation Example 3: Charging and Discharging Characteristics of Coin Full-Cell Battery
[0209] The charge and discharge characteristics of the coin full-cell batteries respectively prepared according to Examples 1 to 3 and Comparative Examples 1 and 2 were evaluated according to the following method. The charge and discharge were repeated 200 cycles.
[0210] Charging and discharging conditions (charging: 1.0C / cutoff: 4.2V-0.01C, discharging: 1.0C / cutoff: 2.5V)
[0211] The lithium battery was charged with a constant current at a C-rate of 0.1C at 25°C until the voltage reached 4.2V (relative to Li), and then the charging process was terminated at a C-rate of 0.01C while maintaining a voltage of 4.2V in a constant voltage mode. Subsequently, the lithium battery was discharged with a constant current at a C-rate of 0.1C until the voltage reached 2.5V (relative to Li) (1st cycle, formation cycle).
[0212] The lithium battery that has undergone the first cycle is charged with a constant current at a C-rate of 0.2C at 25°C until the voltage reaches 4.2V (relative to Li), and then the charging process is terminated at a C-rate of 0.01C while maintaining a voltage of 4.2V in a constant voltage mode. Subsequently, the lithium battery is discharged at a current rate of 0.2C until the voltage reaches 2.5V (relative to Li) (second cycle).
[0213] The lithium battery that has undergone the second cycle is charged with a constant current at a C-rate of 1.0C at 25°C until the voltage reaches 4.2V (relative to Li), and then the charging process is terminated at a C-rate of 0.01C while maintaining a voltage of 4.2V in a constant voltage mode. Subsequently, the lithium battery is discharged with a constant current at a C-rate of 1.0C until the voltage reaches 2.5V (relative to Li) (the third cycle). This charge / discharge cycle is repeated 200 times under the same conditions until the 203rd cycle.
[0214] The lithium battery was allowed to rest for 10 minutes after each charge / discharge cycle.
[0215] The capacity retention rate of the coin full-cell battery is defined by Equation 1 below.
[0216] Equation 1
[0217] Capacity retention rate [%] = [discharge capacity at the 203rd cycle / discharge capacity at the 3rd cycle] × 100%
[0218] Some of the charge / discharge test results are shown in Fig.10 and Table 3 below.
[0219] Table 3
[0220]
[0221]
[0222] like Fig.10 As shown in Table 3, it was confirmed that the coin full-cell batteries prepared according to Examples 1, 2, 3, and 3a had improved capacity retention ratios compared to those according to Comparative Examples 1 and 2.
[0223] Evaluation Example 4: Charging and Discharging Characteristics of Coin Half Cells
[0224] The charge and discharge characteristics of the coin half-cell batteries prepared according to Examples 4 to 6 and Comparative Examples 3, 4, and 3a, respectively, were evaluated according to the following methods.
[0225] The lithium battery was charged with a constant current at a C-rate of 0.1C at 25°C until the voltage reached 0.01V (relative to Li), and then the charging process was terminated at a C-rate of 0.01C while maintaining a voltage of 0.01V in a constant voltage mode. Subsequently, the lithium battery was discharged with a constant current at a C-rate of 0.1C until the voltage reached 1.5V (relative to Li) (1st cycle, formation cycle).
[0226] The lithium battery having undergone the first cycle was charged with a constant current at a C-rate of 0.1C at 25°C until the voltage reached 0.01V (relative to Li) and discharged with a constant current at a C-rate of 0.1C until the voltage reached 1.5V (relative to Li) (0.1C charge rate characteristic evaluation cycle).
[0227] The lithium battery that had undergone a 0.1C charge rate characteristic evaluation cycle was charged with a constant current at a C-rate of 0.2C at 25°C until the voltage reached 0.01 V (relative to Li) and discharged with a constant current at a C-rate of 0.2C until the voltage reached 1.5 V (relative to Li) (0.2C charge rate characteristic evaluation cycle).
[0228] The lithium battery that had undergone a 0.2C charge rate characteristic evaluation cycle was charged with a constant current at a C-rate of 0.5C at 25°C until the voltage reached 0.01 V (relative to Li) and discharged with a constant current at a C-rate of 0.2C until the voltage reached 1.5 V (relative to Li) (0.5C charge rate characteristic evaluation cycle).
[0229] The lithium battery that had undergone a 0.5C charge rate characteristic evaluation cycle was charged with a constant current at a C-rate of 1.0C at 25°C until the voltage reached 0.01 V (relative to Li) and discharged with a constant current at a C-rate of 0.2C until the voltage reached 1.5 V (relative to Li) (1.0C charge rate characteristic evaluation cycle).
[0230] The lithium battery that had undergone a 1.0C charge rate characteristic evaluation cycle was charged with a constant current at a C-rate of 2.0C at 25°C until the voltage reached 0.01 V (relative to Li) and discharged with a constant current at a C-rate of 0.2C until the voltage reached 1.5 V (relative to Li) (2.0C charge rate characteristic evaluation cycle).
[0231] The lithium battery that had undergone a 2.0C charge rate characteristic evaluation cycle was charged with a constant current at a C-rate of 3.0C at 25°C until the voltage reached 0.01 V (relative to Li) and discharged with a constant current at a C-rate of 0.2C until the voltage reached 1.5 V (relative to Li) (3.0C charge rate characteristic evaluation cycle).
[0232] The lithium battery that has undergone the first cycle is charged with a constant current at a C-rate of 0.2C at 25°C until the voltage reaches 0.01V (relative to Li), and then the charging process is terminated at a C-rate of 0.01C while maintaining a voltage of 0.01V in a constant voltage mode. Subsequently, the lithium battery is discharged with a constant current at a C-rate of 0.2C until the voltage reaches 1.5V (relative to Li) (0.2C discharge rate characteristic evaluation cycle)
[0233] The lithium battery that had undergone a 0.2C discharge rate characteristic evaluation cycle was charged with a constant current at a C-rate of 0.2C at 25°C until the voltage reached 0.01V (relative to Li), and then the charging process was terminated at a C-rate of 0.01C while maintaining a voltage of 0.01V in a constant voltage mode. Subsequently, the lithium battery was discharged with a constant current at a C-rate of 0.5C until the voltage reached 1.5V (relative to Li) (0.5C discharge rate characteristic evaluation cycle).
[0234] The lithium battery that had undergone a 0.5C discharge rate characteristic evaluation cycle was charged with a constant current at a C-rate of 0.2C at 25°C until the voltage reached 0.01V (relative to Li), and then the charging process was terminated at a C-rate of 0.01C while maintaining a voltage of 0.01V in a constant voltage mode. Subsequently, the lithium battery was discharged with a constant current at a C-rate of 1.0C until the voltage reached 1.5V (relative to Li) (1.0C discharge rate characteristic evaluation cycle).
[0235] The lithium battery that had undergone a 1C discharge rate characteristic evaluation cycle was charged with a constant current at a C-rate of 0.2C at 25°C until the voltage reached 0.01V (relative to Li), and then the charging process was terminated at a C-rate of 0.01C while maintaining a voltage of 0.01V in a constant voltage mode. Subsequently, the lithium battery was discharged with a constant current at a C-rate of 2.0C until the voltage reached 1.5V (relative to Li) (2.0C discharge rate characteristic evaluation cycle).
[0236] The lithium battery that had undergone a 1C discharge rate characteristic evaluation cycle was charged with a constant current at a C-rate of 0.2C at 25°C until the voltage reached 0.01V (relative to Li), and then the charging process was terminated at a C-rate of 0.01C while maintaining a voltage of 0.01V in a constant voltage mode. Subsequently, the lithium battery was discharged with a constant current at a C-rate of 3.0C until the voltage reached 1.5V (relative to Li) (3.0C discharge rate characteristic evaluation cycle).
[0237] The lithium battery was allowed to rest for 10 minutes after each charge / discharge cycle.
[0238] The initial efficiency is defined by Equation 2 below.
[0239] Equation 2
[0240] Initial efficiency (%) = [discharge capacity at the first cycle / charge capacity at the first cycle] × 100%
[0241] During the charge and discharge test, the rate characteristics of the coin half-cell batteries prepared according to Example 4, Comparative Example 3, and Comparative Example 4 were shown in Figures 6A to 6D In addition, the rate characteristics of the coin half-cell batteries prepared according to Examples 4, 5 and 6a and Comparative Example 3 are shown in Fig.11A , 11B , and 12. Fig. 11B To have Fig.11A Magnified view of the dotted area.
[0242] The initial efficiencies are shown in Table 4 below.
[0243] Table 4
[0244] Example Initial efficiency (%) Example 4 89.7 Example 5 88.6 Example 6 89.9 Example 6a 87.9 Comparative Example 3 89.3 Comparative Example 4 88.4 Comparative Example 3a 87.1
[0245] Reference Figures 6A to 6D It was confirmed that the coin half-cell battery according to Example 4 had improved charge and discharge rate characteristics compared with the coin half-cell batteries prepared according to Comparative Examples 3 and 4. In addition, as shown in Table 4, the coin half-cell batteries according to Examples 4 to 6 and 6a had increased initial efficiencies compared with the coin half-cell battery according to Comparative Example 4. Moreover, as shown in Table 4, Fig.11A , 11B As shown in , and 12, the coin half-cell batteries according to Examples 4, 5, and 6a have improved charge and discharge high rate characteristics compared to the coin half-cell battery according to Comparative Example 3.
[0246] Evaluation Example 5: SEM analysis after charging and discharging
[0247] The charge and discharge characteristics of the coin full-cell batteries prepared according to Example 1, Comparative Example 1, and Comparative Example 2, respectively, were evaluated in the same manner as in Evaluation Example 3 to observe the cross-section of the negative electrode using a scanning electron microscope before the charge and discharge test and after 200 charge and discharge cycles.
[0248] Fig. 7A and 7B Cross sections of the negative electrode of the coin full-cell cell prepared according to Example 1 before the charge and discharge cycles and after repeating the charge and discharge cycles 200 times are respectively shown.
[0249] Fig. 8A and 8B Cross sections of the negative electrode of the coin full-cell cell prepared according to Comparative Example 1 before the charge and discharge cycles and after repeating the charge and discharge cycles 200 times are respectively shown. Fig.9A and 9B Cross sections of the negative electrode of the coin full-cell cell prepared according to Comparative Example 2 before the charge and discharge cycles and after repeating the charge and discharge cycles 200 times are respectively shown.
[0250] It was confirmed that the negative electrode according to Example 1 had less voids and less expansion after repeating 200 charge and discharge cycles compared to the negative electrodes according to Comparative Examples 1 and 2. Such results indicate that by adding the graphene-silica composite to the negative electrode according to Example 1, the adhesion between the structural components of the negative electrode is increased to form a surface-to-surface conductive path, and a conductive network is formed, thereby improving the adhesion strength. As a result, the voids in the negative electrode are reduced and electrical short circuits are prevented during cycling. As described above, the negative electrode according to Example 1, which is structurally stable after charging and discharging and includes a negative electrode active material, can be used to prepare a battery with low expansion and excellent durability.
[0251] Evaluation Example 6: Electrolyte Immersion Time
[0252] The time taken for each of the coin half-cells prepared according to Example 4 and Comparative Example 3 to be impregnated with an electrolyte was measured. The electrolyte was prepared by dissolving 1.0 M LiPF in a mixed solvent of ethylene carbonate (EC), diethyl carbonate (DEC), and fluoroethylene carbonate (FEC) (mixed in a volume ratio of 5:70:25). 6 Prepared.
[0253] The results are shown in Table 5 below.
[0254] Table 5
[0255] Example Electrolyte immersion time Example 4 50 seconds Comparative Example 3 1 minute 15 seconds
[0256] As shown in Table 5, the coin half cell according to Example 4 exhibited an electrolyte impregnation time less than that of the coin half cell according to Comparative Example 3. Therefore, it was confirmed that the coin half cell according to Example 4 had better electrolyte impregnation properties and wetting properties than the coin half cell of Comparative Example 3.
[0257] By using the electrode composite conductive agent according to the embodiment, initial efficiency, charge and discharge rate characteristics, and lifespan characteristics of a lithium battery may be improved.
[0258] It should be understood that the embodiments described herein should be considered in a descriptive sense only and not for purposes of limitation. The description of features or aspects in each embodiment should be considered as applicable to other similar features or aspects in other embodiments.
[0259] Although embodiments have been described with reference to the accompanying drawings, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope as defined by the following claims.
Claims
1. An electrode composite conductive agent for a lithium battery, the electrode composite conductive agent include: Carbonaceous conductive materials; and Graphene-silica composite, The graphene-silica composite comprises a substrate comprising graphene, and Silicon oxide of the formula SiO where 0 < x < 2 x Low-valent silicon oxide, or a combination of silicon dioxide and low-valent silicon oxide of the formula SiO where 0 < x < 2 x The amount of the graphene-silica composite is 0.5 parts by weight to 20 parts by weight, based on 100 parts by weight of the total weight of the composite conductive agent. The graphene-silica composite has a specific surface area of 50 m2 / g to 800 m2 / g.
2. The electrode composite conductive agent for lithium battery according to claim 1, wherein The graphene-silica composite is in the form of particles including silicon suboxide and graphene, particles in which silicon suboxide is completely surrounded by graphene, or a combination thereof, and The particles comprising silicon suboxide and graphene, the particles in which silicon suboxide is completely surrounded by graphene, or a combination thereof are interconnected to form the graphene-containing matrix. 3 . The electrode composite conductive agent for a lithium battery according to claim 1 , wherein the silicon dioxide is partially or completely surrounded by the low-valent silicon oxide.
4. The electrode composite conductive agent for a lithium battery as claimed in claim 1, wherein the graphene-silica composite has a size of 50 nanometers to 200 nanometers, wherein the size of the graphene-silica composite represents an average particle diameter in the case where the graphene-silica composite is spherical, and represents the length of the major axis in the case where the graphene-silica composite is not spherical.
5. The electrode composite conductive agent for lithium battery according to claim 1, wherein the carbonaceous conductive material comprises graphene, graphite, carbon black, carbon nanotubes, vapor-grown carbon fibers, or a combination thereof, and The carbonaceous conductive material has a specific surface area of 10 m2 / g to 1000 m2 / g.
6. The electrode composite conductive agent for a lithium battery according to claim 1, wherein the carbonaceous conductive material has a flake shape, a plate shape, a rod shape, or a combination thereof, and The graphene-silica composite has a fused sphere structure, a faceted sphere structure, or a wrinkled sphere structure.
7. An electrode for a lithium battery, the electrode include: Electrode active materials and conductive agents, The conductive agent comprises the composite conductive agent as claimed in any one of claims 1 to 6. 8 . The electrode according to claim 7 , wherein the amount of the composite conductive agent is 0.1 parts by weight to 10 parts by weight based on 100 parts by weight of the total weight of the electrode.
9. The electrode of claim 7, wherein the electrode active material comprises a carbonaceous material, a silicon-based material, tin, a tin-based alloy, a tin-carbon composite, a metal oxide, or a combination thereof. 10 . The electrode of claim 9 , wherein the silicon-based material is silicon oxide, a silicon-based alloy, a silicon-carbonaceous material composite, or a porous silicon composite.
11. The electrode according to claim 10, wherein the porous silicon composite comprises a porous core including a porous silicon secondary particle, and a shell formed on at least one surface of the porous core and including a first graphene, wherein the porous silicon secondary particles include aggregates of a plurality of silicon composite primary particles, and The silicon composite primary particles of the plurality of silicon composite primary particles include silicon, Low-valence silicon oxide of the formula SiO where 0 < x < 2 on the silicon x and A second graphene is formed on at least one surface of the silicon suboxide.
12. The electrode of claim 7, wherein the electrode active material comprises a porous silicon composite and a carbonaceous material.
13. The electrode of claim 12, wherein the carbonaceous material comprises graphene, graphite, fullerene, carbon fiber, carbon nanotube, pitch carbon, or a combination thereof.
14. A method for preparing an electrode for a lithium battery, the method include: dry-mixing an electrode active material, a carbonaceous conductive material, and a graphene-silica composite to obtain a mixture; adding a binder and a solvent to the dry-blended mixture; and mixing the binder and the mixture to obtain an electrode active material composition, The graphene-silica composite comprises a substrate comprising graphene, and Silicon oxide of the formula SiO where 0 < x < 2 x Low-valent silicon oxide, or a combination of silicon dioxide and low-valent silicon oxide of the formula SiO where 0 < x < 2 x and The amount of the graphene-silica composite is 0.5 parts by weight to 20 parts by weight, based on 100 parts by weight of the total weight of the carbonaceous conductive material and the graphene-silica composite constituting the composite conductive agent. The graphene-silica composite has a specific surface area of 50 m2 / g to 800 m2 / g.
15. The method of claim 14, wherein the carbonaceous conductive material has a specific surface area of 10 m2 / g to 1,000 m2 / g.
16. The method of claim 14, wherein the graphene-silica composite is in the form of particles comprising silicon suboxide and graphene, particles in which silicon suboxide is completely surrounded by graphene, or a combination thereof, and The particles comprising silicon suboxide and graphene, the particles in which silicon suboxide is completely surrounded by graphene, or a combination thereof are interconnected with each other in a matrix comprising graphene.
17. The method of claim 14, wherein the electrode active material comprises a carbonaceous material, a silicon-based material, tin, a tin-based alloy, a tin-carbon composite, a metal oxide, or a combination thereof, The carbonaceous material includes graphene, graphite, carbon black, carbon nanotubes, vapor-grown carbon fibers, metal-coated carbon fibers, or a combination thereof.
18. The method of claim 17, wherein the silicon-based material is a silicon oxide, a silicon-based alloy, a silicon-carbonaceous material composite, or a porous silicon composite, The porous silicon composite includes a porous core including porous silicon secondary particles and a shell on at least one surface of the porous core and including a first graphene, wherein the porous silicon secondary particles include aggregates of a plurality of silicon composite primary particles, and The silicon composite primary particles of the plurality of silicon composite primary particles include silicon, a silicon suboxide on the silicon, and a second graphene on at least one surface of the silicon suboxide.
19. The method of claim 14, wherein the carbonaceous conductive material has a flake shape, a plate shape, a rod shape, or a combination thereof, and The graphene-silica composite has a fused sphere structure, a faceted sphere structure, or a wrinkled sphere structure.
20. A lithium battery comprising the electrode according to any one of claims 7 to 13.