Photosensitive resin composition, photosensitive dry film and pattern forming method
By introducing silicophene and fluorene skeletons into the photosensitive resin composition, combining phenol compounds and photosensitive agents, the problem of low resolution in the prior art is solved, and a high resolution resin coating and dry film are achieved The formation of the slightest size pattern is suitable for the production of fine size patterns.
Patent Information
- Application Number
- CN201911315425.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-12-19
- Filing Date
- 2019-12-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-12-19
AI Technical Summary
Existing photosensitive silicone compositions have low resolution in highly integrated 3D packages, making it difficult to meet the needs of fine dimensional patterns.
A photosensitive resin composition formed by using a polymer containing a silicophene group and a fluorene skeleton, combined with phenol compounds, photoacid generators, benzotriazoles or imidazole compounds and organic solvents, is prepared by exposure and development technology. resin coating or film.
A high resolution photosensitive resin composition and dry film are realized, and a vertical profile pattern of fine size can be formed, suitable for resin coatings in the form of thick films, and the pattern formation ability on the substrate is improved.
Smart Images

Figure BDA0002325706220000021 
Figure BDA0002325706220000041 
Figure BDA0002325706220000051
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This nonprovisional application claims priority under 35 U.S.C. §119(a) to patent application No. 2018-237135 filed in Japan on December 19, 2018, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The invention relates to a photosensitive resin composition, a photosensitive dry film and a pattern forming method. Background Art
[0004] In the prior art, photosensitive protective films for semiconductor chips and photosensitive insulating films for multilayer printed circuit boards are formed from photosensitive polyimide compositions, photosensitive epoxy resin compositions, photosensitive organosilicon compositions, and the like. As a photosensitive material for protecting such substrates and circuits, Patent Document 1 discloses a photosensitive organosilicon composition based on an organosilicon type polymer containing a silylene structure, which has improved flexibility. This composition has improved film properties but low resolution. Further improvements in resolution must be achieved before the composition can be used in highly integrated 3D packaging.
[0005] Reference List
[0006] Patent Document 1: JP-A 2008-184571 (USP 7,785,766, EP 1953183) Summary of the invention
[0007] The present invention aims to provide a photosensitive resin composition which forms a resin coating or film having improved film properties and which can be easily processed to form fine-scale patterns even in thick film form. Another object is to provide a photosensitive dry film and a pattern forming method using the composition.
[0008] The inventors have found that a photosensitive resin composition comprising the following components has high resolution and is suitable as a resist material for plating: a polymer containing a silphenylene group and a fluorene skeleton and having a crosslinking group or a reactive site capable of a crosslinking reaction in a molecule, a phenol compound having a Mw of 300 to 10,000, a photoacid generator, and a benzotriazole compound and / or an imidazole compound.
[0009] In one aspect, the present invention provides a photosensitive resin composition comprising the following components:
[0010] (A) a polymer comprising a repeating unit having the formula (A1) shown below and at least one type of repeating unit selected from a repeating unit having the formula (A2) shown below and a repeating unit having the formula (A3) shown below,
[0011] (B) a phenol compound having a weight average molecular weight of 300 to 10,000,
[0012] (C) a photoacid generator,
[0013] (D) a benzotriazole compound and / or an imidazole compound, and
[0014] (E) Organic solvent.
[0015]
[0016] Where X 1 and X 2 are each independently hydrogen or a glycidyl group, Y 1 is a C1-C5 straight-chain or branched alkanediyl group, Z 1 It is a C1-C 10 Straight chain alkanediyl groups, C2-C 10 A branched alkanediyl group or a divalent group having the formula (A4):
[0017]
[0018] Where Z 11 and Z 13 Each is independently a C1-C5 straight chain or branched alkanediyl group, Z 12 It is C1-C 30 Divalent hydrocarbon group, a 4 and a 5 are each independently an integer from 1 to 50, R 1 , R 2 , R 3 and R 4 are independently hydrogen or C1-C 10 A monovalent hydrocarbon group, a 1 、a 2 and a 3 Is a number in the following range: 0 1 <1, 0≤a 2 <1, 0≤a 3 <1 and a 1 +a 2 +a 3 =1, x and y are each independently an integer from 1 to 50.
[0019] There is also provided a photosensitive resin coating obtained from the photosensitive resin composition defined above.
[0020] In another aspect, the present invention provides a photosensitive dry film comprising a support film and a photosensitive resin coating thereon.
[0021] In another aspect, the present invention provides a pattern forming method comprising the steps of: (a) applying the photosensitive resin composition defined above to a substrate to form a photosensitive resin coating thereon, (b) exposing the photosensitive resin coating to radiation, and (c) developing the exposed resin coating in an organic solvent.
[0022] In still another aspect, the present invention provides a pattern forming method comprising the steps of: (a') using the photosensitive dry film defined above to form a photosensitive resin coating on a substrate, (b) exposing the photosensitive resin coating to radiation, and (c) developing the exposed resin coating in an organic solvent.
[0023] Advantageous Effects of the Invention
[0024] The photosensitive resin composition and the photosensitive dry film of the present invention have satisfactory properties as photosensitive materials. Films with widely varying thicknesses can be formed from the composition or the dry film. Even fine-scale patterns with vertical profiles can be formed from thick films. DETAILED DESCRIPTION
[0025] The notation (Cn-Cm) used herein means a group containing nm carbon atoms per group. UV stands for ultraviolet radiation and EB stands for electron beam.
[0026] Photosensitive resin composition
[0027] The present invention provides a photosensitive resin composition comprising the following components: (A) a polymer containing a silylene skeleton and a fluorene skeleton and having a crosslinking group or a reactive site capable of undergoing a crosslinking reaction in the molecule, (B) a phenol compound having a weight average molecular weight of 300 to 10,000, (C) a photoacid generator, (D) a benzotriazole compound and / or an imidazole compound, and (E) an organic solvent.
[0028] Component (A)
[0029] Component (A) is a polymer comprising a repeating unit having the formula (A1) and at least one type of repeating unit selected from the repeating unit having the formula (A2) and the repeating unit having the formula (A3).
[0030]
[0031] In formula (A1), X 1 and X 2 Each is independently hydrogen or a glycidyl group.
[0032] In formula (A2), Y 1is a C1-C5 straight chain or branched alkanediyl group. Suitable alkanediyl groups include methylene, ethane-1,1-diyl, ethane-1,2-diyl, propane-1,1-diyl, propane-1,2-diyl, propane-1,3-diyl, propane-2,2-diyl, butane-1,2-diyl, butane-1,3-diyl, butane-1,4-diyl and pentane-1,5-diyl. Preferably, Y 1 It is ethane-1,1-diyl, ethane-1,2-diyl, propane-1,1-diyl, propane-1,2-diyl, or propane-1,3-diyl.
[0033] In formula (A3), Z 1 It is C1-C 10 Straight chain alkanediyl group or C2-C 10 A branched alkanediyl group, a straight chain alkanediyl group optionally contains a hydroxyl group. Alternatively, Z 1 is a divalent group having formula (A4):
[0034]
[0035] Where Z 11 and Z 13 Each is independently a C1-C5 straight chain or branched alkanediyl group, Z 12 It is C1-C 30 Divalent hydrocarbon group, a 4 and a 5 Each independently represents an integer from 1 to 50.
[0036] Z 1 Examples of straight chain alkanediyl groups represented include methylene, ethane-1,2-diyl, propane-1,3-diyl, butane-1,4-diyl, pentane-1,5-diyl, hexane-1,6-diyl, heptane-1,7-diyl, octane-1,8-diyl, nonane-1,9-diyl and decane-1,10-diyl.
[0037] Examples of linear alkanediyl groups containing hydroxy groups include hydroxy-substituted forms of pentane-1,5-diyl, hexane-1,6-diyl, heptane-1,7-diyl, octane-1,8-diyl, nonane-1,9-diyl and decane-1,10-diyl, specifically 2-hydroxypropane-1,3-diyl, 2-hydroxybutane-1,4-diyl and 3-hydroxypropane-1,3-diyl.
[0038] Z 1 C2-C 10 Examples of branched alkanediyl groups include ethane-1,1-diyl, propane-1,2-diyl, propane-2,2-diyl, butane-1,2-diyl and butane-1,3-diyl.
[0039] Examples of the divalent group having the formula (A4) are shown below, but are not limited thereto.
[0040]
[0041] Among them, Z 1 It is preferably selected from ethane-1,1-diyl, ethane-1,2-diyl, propane-1,2-diyl, propane-1,3-diyl, propane-2,2-diyl, butane-1,4-diyl, pentane-1,5-diyl and hexane-1,6-diyl.
[0042] In formulas (A2) and (A3), R 1 , R 2 , R 3 and R 4 are independently hydrogen or C1-C 10 The monovalent hydrocarbon group may be linear, branched or cyclic, and examples thereof include monovalent aliphatic hydrocarbon groups such as C1-C 10 Alkyl groups and monovalent aromatic hydrocarbon groups such as C6-C 10 Aryl and C7-C 10 Aralkyl group.
[0043] Suitable for C1-C 10 Alkyl groups include methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, cyclobutyl, n-pentyl, cyclopentyl, n-hexyl, cyclohexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, norbornyl and adamantyl. Suitable aryl groups include phenyl, 2-methylphenyl, 3-methylphenyl, 4-methylphenyl, 2-ethylphenyl, 3-ethylphenyl, 4-ethylphenyl and dimethylphenyl. Suitable aralkyl groups include benzyl and phenethyl. Wherein, R 1 , R 2 , R 3 and R 4 Preferred are hydrogen or methyl.
[0044] In formulas (A1) to (A3), a 1 、a 2 and a 3 Is a number in the following range: 0 1 <1, 0≤a 2 <1, 0≤a 3 <1 and a 1 +a 2 +a 3 =1; preferably in the following range: 0.20≤a 1 ≤0.95、0≤a 2 ≤0.80、0≤a 3 ≤0.80 and a 1 +a 2 +a 3 =1; more preferably in the following range: 0.30≤a 1 ≤0.95、0≤a 2 ≤0.70、0≤a 3 ≤0.70 and a 1 +a 2 +a 3 =1.
[0045] In formulae (A2) and (A3), x and y are each independently an integer of 1 to 50, preferably 2 to 40, more preferably 3 to 30.
[0046] The polymer as component (A) should preferably have a weight average molecular weight (Mw) of 3,000 to 80,000, more preferably 5,000 to 50,000. As long as the Mw is within this range, even thick polymer films have sufficient resolution. Throughout the disclosure, Mw is measured by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as eluent against polystyrene standards.
[0047] The polymer can be prepared by combining a compound having formula (1), a compound having formula (2), and at least one of a compound having formula (3) and a compound having formula (4), and performing addition polymerization in the presence of a metal catalyst. In particular, these compounds are simply referred to as compounds (1), (2), (3) and (4).
[0048]
[0049] Where X 1 , X 2 , Y 1 , Z 1 , R 1 To R 4 , x and y are as defined above.
[0050] Examples of the metal catalyst used herein include simple platinum group metals such as platinum (including platinum black), rhodium and palladium; platinum chlorides, chloroplatinic acid and chloroplatinates such as H2PtCl4·xH2O, H2PtCl6·xH2O, NaHPtCl6·xH2O, KHPtCl6·xH2O, Na2PtCl6·xH2O, K2PtCl4·xH2O, PtCl4·xH2O, PtCl2 and Na2HPtCl4·xH2O, wherein x is preferably an integer from 0 to 6, more preferably 0 or 6; alcohol-modified chloroplatinic acid as described in USP 3,220,972; as described in USP 3,159,601, USP 3,159,662 and USP 3,775,452; supported catalysts comprising platinum group metals such as platinum black and palladium on alumina, silica and carbon supports; rhodium-olefin complexes; chlorotris(triphenylphosphine)rhodium (known as Wilkinson's catalyst); and complexes of platinum chloride, chloroplatinic acid and chloroplatinates with vinyl-containing siloxanes, particularly vinyl-containing cyclosiloxanes.
[0051] The catalyst is used in a catalytic amount, preferably 0.001 to 0.1% by weight of a platinum group metal based on the total weight of compounds (1) to (4).
[0052] In the polymerization reaction, a solvent may be used if necessary. Suitable solvents are hydrocarbon solvents such as toluene and xylene. The polymerization temperature is preferably in the range of 40 to 150° C., more preferably 60 to 120° C., within which the catalyst is not deactivated and the polymerization can be completed in a short time. The polymerization time varies with the type and amount of the starting compound. It is preferably from about 0.5 to about 100 hours, more preferably from about 0.5 to about 30 hours, to prevent moisture from entering the polymerization system. After the reaction is completed, the solvent (if used) is distilled off, and a polymer is obtained.
[0053] The reaction process is not particularly limited. A preferred process is by first mixing compound (2) with at least one of compounds (3) and (4), heating, adding a metal catalyst to the mixture, and then adding compound (1) dropwise over 0.1 to 5 hours.
[0054] In the polymerization reaction, the starting compounds are preferably combined in such amounts that the molar ratio of the hydrosilyl groups on compound (1) to the total alkenyl groups on compounds (2), (3) and (4) may be in the range of 0.67-1.67, more preferably 0.83-1.25.
[0055] The Mw of the polymer may be controlled using a molecular weight control agent such as a monoallyl compound (eg, o-allylphenol), a monohydrogen silane (eg, triethylhydrogen silane), or a monohydrogen siloxane.
[0056] Component (B)
[0057] Component (B) is a phenolic compound having a Mw of 300 to 10,000. The phenolic compound is a compound having at least one phenolic hydroxyl group, typically a novolac resin. The novolac resin can be prepared by a condensation reaction of phenol or cresol with an aldehyde or ketone in the presence of an acid catalyst. Suitable acid catalysts include hydrochloric acid, formic acid and oxalic acid. Suitable phenols and cresols include phenol, o-cresol, m-cresol, p-cresol, o-ethylphenol, m-ethylphenol, 2,3-xylenol, 2,5-xylenol and 3,5-xylenol. Suitable aldehydes and ketones include formaldehyde, benzaldehyde, acetaldehyde and acetone.
[0058] In addition to the novolac resin, component (B) may be further selected from polyhydroxystyrene, bisphenols, trisphenols, polyphenols, and compounds having the following formulae (B1), (B2), and (B3).
[0059]
[0060] In formula (B1), j is 1 or 2, m, p and r are each independently an integer of 0 to 3, q is an integer of 1 to 3, and n is an integer of 1 to 4, satisfying 1≤m+n+p≤6 and 1≤q+r≤5.
[0061] In formula (B2), k is an integer of 2 or 3, and q and r are as defined above.
[0062] In formula (B3), s and t are each independently an integer from 0 to 3, satisfying 0≤s+t≤4. 11 To R 16 are each independently hydrogen, methyl, or a group having the following formula (B4), provided that R 11 To R 13 At least one and R 14 To R 16 At least one of the groups is a group having the formula (B4), wherein u is an integer from 1 to 3.
[0063]
[0064] In formula (B4), u and v are each independently an integer from 0 to 3, satisfying 0≤u+v≤4.
[0065] The amount of component (B) is preferably 0.2 to 50 parts by weight, more preferably 0.5 to 40 parts by weight, even more preferably 0.8 to 30 parts by weight per 100 parts by weight of component (A).
[0066] Component (C)
[0067] Component (C) is a photoacid generator, and there is no particular limitation on the photoacid generator as long as it decomposes to generate an acid when exposed to high-energy radiation. Examples of high-energy radiation include UV, deep UV and EB, especially g-line, h-line, i-line, KrF excimer laser, ArF excimer laser, EB and synchrotron radiation.
[0068] Suitable PAGs include Salts (such as sulfonium and iodine salts), sulfonyldiazomethane derivatives, N-sulfonyloxyimide PAGs, benzoin sulfonate PAGs, pyrogallol trisulfonate PAGs, nitrobenzyl sulfonate PAGs, sulfone PAGs, O-arylsulfonyl oxime compounds or O-alkylsulfonyl oxime compounds (oxime sulfonate) PAGs.
[0069] Sulfonium salts are salts of sulfonium cations and sulfonate anions. Exemplary sulfonium cations include triphenylsulfonium, (4-tert-butoxyphenyl)diphenylsulfonium, bis(4-tert-butoxyphenyl)phenylsulfonium, tris(4-tert-butoxyphenyl)sulfonium, (3-tert-butoxyphenyl)diphenylsulfonium, bis(3-tert-butoxyphenyl)phenylsulfonium, tris(3-tert-butoxyphenyl)sulfonium, (3,4-di-tert-butoxyphenyl)diphenylsulfonium, bis(3,4-di-tert-butoxyphenyl)phenylsulfonium, tris(3,4-di-tert-butoxyphenyl)sulfonium, diphenyl(4-tert-butoxyphenyl)sulfonium,
[0063] The invention also includes 2-(4-tert-butoxyphenyl)sulfonium, 4-(tert-butoxyphenyl)bis(4-dimethylaminophenyl)sulfonium, 4-(tert-butoxyphenyl)bis(4-dimethylaminophenyl)sulfonium, 4-(tert-butoxyphenyl)bis(4-dimethylaminophenyl)sulfonium, 4-(tert-butoxyphenyl)bis(4-dimethylaminophenyl)sulfonium, 4-(tert-butoxyphenyl)bis(4-dimethylaminophenyl)sulfonium, 4-(tert-butoxyphenyl)bis(4-dimethylaminophenyl)sulfonium, 4-(tert-butoxyphenyl)bis(4-dimethylaminophenyl)sulfonium, 4-(tert-naphthyl)sulfonium, 4-hydroxyphenyldimethylsulfonium, 4-methoxyphenyldimethylsulfonium, 4-(tert-methyl ...butoxyphenyl)bis(4-dimethylaminophenyl) Exemplary sulfonate anions include trifluoromethanesulfonate, nonafluorobutanesulfonate, heptadecafluorooctanesulfonate, 2,2,2-trifluoroethanesulfonate, pentafluorobenzenesulfonate, 4-(trifluoromethyl)benzenesulfonate, 4-fluorobenzenesulfonate, toluenesulfonate, benzenesulfonate, 4-(4-toluenesulfonyloxy)benzenesulfonate, naphthalenesulfonate, camphorsulfonate, octanesulfonate, dodecylbenzenesulfonate, butanesulfonate and methanesulfonate. Further, salts of sulfonium cations with phosphoric acid, antimonic acid, alkylphosphoric acid and fluoroalkylphosphoric acid (i.e., partial hydrogen substitution on the alkyl moiety with fluorine) are included.
[0070] iodine Salt is iodine A salt of a cation and a sulfonate anion. Exemplary iodine Cations include aryl iodides Cations such as diphenyl iodide Bis(4-tert-butylphenyl)iodide 4-tert-Butyloxyphenylphenyl iodide and 4-methoxyphenylphenyl iodide Exemplary sulfonate anions include trifluoromethanesulfonate, nonafluorobutanesulfonate, heptadecafluorooctanesulfonate, 2,2,2-trifluoroethanesulfonate, pentafluorobenzenesulfonate, 4-(trifluoromethyl)benzenesulfonate, 4-fluorobenzenesulfonate, toluenesulfonate, benzenesulfonate, 4-(4-toluenesulfonyloxy)benzenesulfonate, naphthalenesulfonate, camphorsulfonate, octanesulfonate, dodecylbenzenesulfonate, butanesulfonate, and methanesulfonate. Combinations of the foregoing examples are included. Salt.
[0071] Exemplary sulfonyldiazomethane compounds include bissulfonyldiazomethane compounds and sulfonylcarbonyldiazomethane compounds such as bis(ethylsulfonyl)diazomethane, bis(1-methylpropylsulfonyl)diazomethane, bis(2-methylpropylsulfonyl)diazomethane, bis(1,1-dimethylethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, bis(perfluoroisopropylsulfonyl)diazomethane, bis(phenylsulfonyl)diazomethane, bis(4-[4-(2-methylpropylsulfonyl)diazomethane) and bis(1,1-dimethylethylsulfonyl)diazomethane. 4-Methylbenzenesulfonyl)diazomethane, bis(2,4-dimethylbenzenesulfonyl)diazomethane, bis(2-naphthylsulfonyl)diazomethane, 4-methylbenzenesulfonylbenzoyldiazomethane, tert-butylcarbonyl-4-methylbenzenesulfonyldiazomethane, 2-naphthylsulfonylbenzoyldiazomethane, 4-methylbenzenesulfonyl-2-naphthoyldiazomethane, methylsulfonylbenzoyldiazomethane and tert-butyloxycarbonyl-4-methylbenzenesulfonyldiazomethane.
[0072] Suitable N-sulfonyloxy imide PAGs include imide compounds in which the hydrogen bonded to nitrogen is replaced with a sulfonyloxy group. Suitable imide compounds include succinimide, naphthalene dicarboxylic acid imide, phthalimide, cyclohexyl dicarboxylic acid imide, 5-norbornene-2,3-dicarboxylic acid imide and 7-oxabicyclo [2.2.1] -5-heptene-2,3-dicarboxylic acid imide. Suitable sulfonyloxy groups include trifluoromethanesulfonyloxy, nonafluorobutanesulfonyloxy, heptadecafluorooctanesulfonyloxy, 2,2,2-trifluoroethanesulfonyloxy, pentafluorobenzenesulfonyloxy, 4-trifluoromethylbenzenesulfonyloxy, 4-fluorobenzenesulfonyloxy, toluenesulfonyloxy, benzenesulfonyloxy, naphthalenesulfonyloxy, camphorsulfonyloxy, octanesulfonyloxy, dodecylbenzenesulfonyloxy, butanesulfonyloxy and methanesulfonyloxy.
[0073] Benzoin sulfonate PAGs include benzoin toluene sulfonate, benzoin methane sulfonate, and benzoin butane sulfonate.
[0074] Pyrogallol trisulfonate PAGs include pyrogallol, phloroglucinol, catechol, resorcinol and hydroquinone, wherein all hydroxyl groups are substituted with sulfonyloxy groups, such as trifluoromethanesulfonyloxy, nonafluorobutanesulfonyloxy, heptadecafluorooctanesulfonyloxy, 2,2,2-trifluoroethanesulfonyloxy, pentafluorobenzenesulfonyloxy, 4-trifluoromethylbenzenesulfonyloxy, 4-fluorobenzenesulfonyloxy, toluenesulfonyloxy, benzenesulfonyloxy, naphthalenesulfonyloxy, camphorsulfonyloxy, octanesulfonyloxy, dodecylbenzenesulfonyloxy, butanesulfonyloxy or methanesulfonyloxy.
[0075] Nitrobenzyl sulfonate PAGs include esters of nitrobenzyl alcohols and sulfonates, such as 2,4-dinitrobenzyl sulfonate, 2-nitrobenzyl sulfonate, and 2,6-dinitrobenzyl sulfonate. Suitable sulfonic acids include trifluoromethanesulfonic acid, nonafluorobutanesulfonic acid, heptadecafluorooctanesulfonic acid, 2,2,2-trifluoroethanesulfonic acid, pentafluorobenzenesulfonic acid, 4-trifluoromethylbenzenesulfonic acid, 4-fluorobenzenesulfonic acid, toluenesulfonic acid, benzenesulfonic acid, naphthalenesulfonic acid, camphorsulfonic acid, octanesulfonic acid, dodecylbenzenesulfonic acid, butanesulfonic acid, and methanesulfonic acid. Also useful are similar nitrobenzyl sulfonate compounds in which the nitro group is substituted with a trifluoromethyl group.
[0076] Sulfone PAGs include bis(phenylsulfonyl)methane, bis(4-methylphenylsulfonyl)methane, bis(2-naphthylsulfonyl)methane, 2,2-bis(phenylsulfonyl)propane, 2,2-bis(4-methylphenylsulfonyl)propane, 2,2-bis(2-naphthylsulfonyl)propane, 2-methyl-2-(p-toluenesulfonyl)propiophenone, 2-cyclohexylcarbonyl-2-(p-toluenesulfonyl)propane, and 2,4-dimethyl-2-(p-toluenesulfonyl)pentan-3-one.
[0077] Suitable O-arylsulfonyl oxime compounds and O-alkylsulfonyl oxime compounds (or oxime sulfonates) PAGs include photoacid generators in the form of oxime derivatives, oxime sulfonates having a long conjugated system separated by thiophene or cyclohexadiene, oxime sulfonates having electron withdrawing groups such as trifluoromethyl introduced to improve stability, oxime sulfonates using phenylacetonitrile or substituted acetonitrile derivatives, and bis-oxime sulfonates.
[0078] Glyoxime derivatives PAG include bis-O-(p-toluenesulfonyl)-α-dimethylglyoxime, bis-O-(p-toluenesulfonyl)-α-diphenylglyoxime, bis-O-(p-toluenesulfonyl)-α-dicyclohexylglyoxime, bis-O-(p-toluenesulfonyl)-2,3-pentanedione dioxime (pentanedionedioxime), bis-O-(n-butanesulfonyl)- )-α-dimethylglyoxime, bis-O-(n-butanesulfonyl)-α-diphenylglyoxime, bis-O-(n-butanesulfonyl)-α-dicyclohexylglyoxime, bis-O-(methanesulfonyl)-α-dimethylglyoxime, bis-O-(trifluoromethanesulfonyl)-α-dimethylglyoxime, bis-O-(2,2,2-trifluoroethanesulfonyl)-α-dimethylglyoxime, bis-O-( 10-camphorsulfonyl)-α-dimethylglyoxime, bis-O-(benzenesulfonyl)-α-dimethylglyoxime, bis-O-(4-fluorobenzenesulfonyl)-α-dimethylglyoxime, bis-O-(4-trifluoromethylbenzenesulfonyl)-α-dimethylglyoxime, bis-O-(xylenesulfonyl)-α-dimethylglyoxime, bis-O-(trifluoromethanesulfonyl)cyclohexanedione dioxime (nio cyclohexanedione dioxime, bis-O-(2,2,2-trifluoroethanesulfonyl)cyclohexanedione dioxime, bis-O-(10-camphorsulfonyl)cyclohexanedione dioxime, bis-O-(benzenesulfonyl)cyclohexanedione dioxime, bis-O-(4-fluorobenzenesulfonyl)cyclohexanedione dioxime, bis-O-(4-(trifluoromethyl)benzenesulfonyl)cyclohexanedione dioxime and bis-O-(xylenesulfonyl)cyclohexanedione dioxime.
[0079] Photoacid generators in the form of oxime sulfonates having a long conjugated system separated by thiophene or cyclohexadiene include (5-(p-toluenesulfonyl)oxyimino-5H-thiophen-2-ylidene)benzyl acetonitrile, (5-(10-camphorsulfonyl)oxyimino-5H-thiophen-2-ylidene)benzyl acetonitrile, (5-n-octanesulfonyloxyimino-5H-thiophen-2-ylidene)benzyl acetonitrile, (5-(p-toluenesulfonyl)oxyimino-5H-thiophen-2-ylidene) (2-methylphenyl) )acetonitrile, (5-(10-camphorsulfonyl)oxyimino-5H-thiophen-2-ylidene)(2-methylphenyl)acetonitrile, (5-n-octanesulfonyloxyimino-5H-thiophen-2-ylidene)(2-methylphenyl)acetonitrile, (5-(4-(p-toluenesulfonyloxy)benzenesulfonyl)oxyimino-5H-thiophen-2-ylidene)benzeneacetonitrile and (5-(2,5-bis(p-toluenesulfonyloxy)benzenesulfonyl)oxyimino-5H-thiophen-2-ylidene)benzeneacetonitrile.
[0080] Suitable oxime sulfonates having an electron withdrawing group such as a trifluoromethyl group introduced to improve stability include 2,2,2-trifluoro-1-phenylethanone O-(methylsulfonyl)oxime, 2,2,2-trifluoro-1-phenylethanone O-(10-camphorsulfonyl)oxime, 2,2,2-trifluoro-1-phenylethanone O-(4-methoxyphenylsulfonyl)oxime, 2,2,2-trifluoro-1-phenylethanone O-(1-naphthylsulfonyl)oxime, 2,2,2-trifluoro-1-phenylethanone O-(2-naphthylsulfonyl)oxime, 2,2,2-trifluoro-1-phenylethanone O-(2,4,6-trimethylbenzenesulfonyl)oxime, 2,2,2-trifluoro-1-(4-methylphenyl)ethanone O-(10-camphorsulfonyl)oxime, 2,2,2-trifluoro-1-phenylethanone O-(4-methoxyphenyl)ethanone Trifluoro-1-(4-methylphenyl)ethanone O-(methylsulfonyl)oxime, 2,2,2-trifluoro-1-(2-methylphenyl)ethanone O-(10-camphorsulfonyl)oxime, 2,2,2-trifluoro-1-(2,4-dimethylphenyl)ethanone O-(10-camphorsulfonyl)oxime, 2,2,2-trifluoro-1-(2,4-dimethylphenyl)ethanone O- (1-Naphthylsulfonyl) oxime, 2,2,2-trifluoro-1-(2,4-dimethylphenyl)ethanone O-(2-naphthylsulfonyl) oxime, 2,2,2-trifluoro-1-(2,4,6-trimethylphenyl)ethanone O-(10-camphorsulfonyl) oxime, 2,2,2-trifluoro-1-(2,4,6-trimethylphenyl)ethanone O-(1-naphthylsulfonyl) Oxime, 2,2,2-trifluoro-1-(2,4,6-trimethylphenyl)ethanone O-(2-naphthylsulfonyl)oxime, 2,2,2-trifluoro-1-(4-methoxyphenyl)ethanone O-(methylsulfonyl)oxime, 2,2,2-trifluoro-1-(4-methylthiophenyl)ethanone O-(methylsulfonyl)oxime, 2,2,2-trifluoro-1-(3,4-dimethoxyphenyl)ethanone O-(methylsulfonyl)oxime, 2,2,2-trifluoro-1-(4-methoxyphenyl)ethanone O-(4-methylbenzenesulfonyl)oxime, 2,2,2-trifluoro-1-(4-methoxyphenyl)ethanone O-(4-methoxybenzenesulfonyl)oxime, 2,2,2-trifluoro-1-(4-methoxyphenyl)ethanone O-(4-dodecylbenzenesulfonyl) Oxime, 2,2,2-trifluoro-1-(4-methoxyphenyl)ethanone O-(octylsulfonyl)oxime, 2,2,2-trifluoro-1-(4-thiomethylphenyl)ethanone O-(4-methoxybenzenesulfonyl)oxime, 2,2,2-trifluoro-1-(4-thiomethylphenyl)ethanone O-(4-dodecylbenzenesulfonyl)oxime, 2,2,2-trifluoro-1-(4-thiomethylphenyl)ethanone O-(4-dodecylbenzenesulfonyl)oxime -(4-thiomethylphenyl)ethanone O-(octylsulfonyl)oxime, 2,2,2-trifluoro-1-(4-thiomethylphenyl)ethanone O-(2-naphthylsulfonyl)oxime, 2,2,2-trifluoro-1-(2-methylphenyl)ethanone O-(methylsulfonyl)oxime, 2,2,2-trifluoro-1-(4-methylphenyl)ethanone O-(benzenesulfonyl)oxime, 2,2,2-Trifluoro-1-(4-chlorophenyl)ethanone O-(benzenesulfonyl)oxime, 2,2,3,3,4,4,4-heptafluoro-1-phenylbutanone O-(10-camphorsulfonyl)oxime, 2,2,2-trifluoro-1-(1-naphthyl)ethanone O-(methylsulfonyl)oxime, 2,2,2-trifluoro-1-(2-naphthyl)ethanone O-(methylsulfonyl)oxime, 2,2,2-Trifluoro-1-(4-benzylphenyl)ethanone O-(methylsulfonyl)oxime, 2,2,2-trifluoro-1-(4-(phenyl-1,4-dioxa-butan-1-yl)phenyl)ethanone O-(methylsulfonyl)oxime, 2,2,2-trifluoro-1-(1-naphthyl)ethanone O-(propylsulfonyl)oxime, 2,2,2-trifluoro-1-(2-naphthyl)ethanone 2,2,2-Trifluoro-1-(4-methylsulfonylphenyl)ethanone O-(propylsulfonyl)oxime, 2,2,2-trifluoro-1-(4-methylsulfonylphenyl)ethanone O-(propylsulfonyl)oxime, 2,2,2-trifluoro-1-(4-methylsulfonyloxyphenyl)ethanone O-(propylsulfonyl)oxime, 2,2,2-trifluoro-1-(4-methylsulfonyloxyphenyl)ethanone O-(propylsulfonyl)oxime, Fluoro-1-(4-methylcarbonyloxyphenyl)ethanone O-(propylsulfonyl)oxime, 2,2,2-trifluoro-1-(6H,7H-5,8-dioxonaphth-2-yl)ethanone O-(propylsulfonyl)oxime, 2,2,2-trifluoro-1-(4-methoxycarbonylmethoxyphenyl)ethanone O-(propylsulfonyl)oxime, 2,2,2-Trifluoro-1-(4-(3-(4-(2,2,2-trifluoro-1-(trifluoromethanesulfonyloxyimino)ethyl)phenoxy)propoxy)phenyl)ethanone O-(trifluoromethanesulfonyl)oxime, 2,2,2-trifluoro-1-(4-benzyloxyphenyl)ethanone O-(propylsulfonyl)oxime, 2,2,2-trifluoro-1-(2-thiophenyl)ethanone O-(propylsulfonate)oxime, 2,2,2-trifluoro-1-(1-dioxathiophen-2-yl)ethanone O-(propylsulfonate)oxime, 2,2,2-trifluoro-1-(4-(3-(4-(2,2,2-trifluoro-1-(trifluoromethanesulfonyloxyimino)ethyl)phenoxy)propoxy)phenyl)ethanone O-(trifluoromethanesulfonyl) 2,2,2-trifluoro-1-(4-(3-(4-(2,2,2-trifluoro-1-(1-propanesulfonyloxyimino)ethyl)phenoxy)propoxy)phenyl)ethanone O-(propylsulfonyl)oxime, 2,2,2-trifluoro-1-(4-(3-(4-(2,2,2-trifluoro-1-(1-butanesulfonyloxyimino)ethyl)phenoxy)propoxy)phenyl)ethanone O-(butylsulfonyl)oxime, 2,2,2-trifluoro-1-(4-(3-(4-(2,2,2-trifluoro-1-(4-(4-methylphenylsulfonyloxy)phenylsulfonyloxyimino)ethyl)phenoxy)propoxy)phenyl)ethanone O-(4-(4-methylphenylsulfonyloxy)benzenesulfonyl)oxime and 2,2,2-trifluoro-1-(4-(3-(4-(2,2,2-trifluoro-1-(4-(4-methylphenylsulfonyloxy)phenylsulfonyloxyimino)ethyl)phenoxy)propoxy)phenyl)ethanone O-(4-(4-methylphenylsulfonyloxy)benzenesulfonyl)oxime and 2,2,2-trifluoro-1-(4-(3-(4-(2,2,2-trifluoro-1-(4-(4-methylphenylsulfonyloxy)phenylsulfonyl)2-Trifluoro-1-(4-(3-(4-(2,2,2-trifluoro-1-((2,5-bis(4-methylphenylsulfonyloxy)benzenesulfonyloxy)phenylsulfonyloxyimino)ethyl)phenoxy)propoxy)phenyl)ethanone O-((2,5-bis(4-methylphenylsulfonyloxy)benzenesulfonyloxy)benzenesulfonyl)oxime.
[0081] Suitable oxime sulfonate PAGs using substituted acetonitrile derivatives include α-(p-toluenesulfonyloxyimino)-phenylacetonitrile, α-(p-chlorobenzenesulfonyloxyimino)-phenylacetonitrile, α-(4-nitrobenzenesulfonyloxyimino)-phenylacetonitrile, α-(4-nitro-2-trifluoromethylbenzenesulfonyloxyimino)-phenylacetonitrile, α-(benzenesulfonyloxyimino)-4-chlorobenzeneacetonitrile, α-(benzenesulfonyloxyimino)-2,4-dichlorobenzeneacetonitrile, α-(benzenesulfonyloxyimino)-2,6-dichlorobenzeneacetonitrile, α-(benzenesulfonyloxyimino)-4-methoxybenzeneacetonitrile, α-(2-chlorobenzenesulfonyloxyimino)-4-methoxybenzeneacetonitrile, α-(benzenesulfonyloxyimino)-2-thiopheneacetonitrile, α-(4-dodecylbenzenesulfonyloxyimino)- ] acetonitrile, α-[(4-toluenesulfonyloxyimino)-4-methoxyphenyl]acetonitrile, α-[(dodecylbenzenesulfonyloxyimino)-4-methoxyphenyl]acetonitrile, α-(toluenesulfonyloxyimino)-3-thiopheneacetonitrile, α-(methylsulfonyloxyimino)-1-cyclopentenylacetonitrile, α-(ethylsulfonyloxyimino)-1-cyclopentenylacetonitrile, α-(isopropylsulfonyloxyimino)-1-cyclopentenylacetonitrile, α-(n-butylsulfonyloxyimino)-1-cyclopentenylacetonitrile, α-(ethylsulfonyloxyimino)-1-cyclohexenylacetonitrile, α-(isopropylsulfonyloxyimino)-1-cyclohexenylacetonitrile, and α-(n-butylsulfonyloxyimino)-1-cyclohexenylacetonitrile.
[0082] Suitable bisoxime sulfonate PAGs include bis(α-(p-toluenesulfonyloxy)imino)-p-phenylenediacetonitrile, bis(α-(benzenesulfonyloxy)imino)-p-phenylenediacetonitrile, bis(α-(methanesulfonyloxy)imino)-p-phenylenediacetonitrile, bis(α-(butanesulfonyloxy)imino)-p-phenylenediacetonitrile, bis(α-(10-camphorsulfonyloxy)imino)-p-phenylenediacetonitrile, bis(α-(trifluoromethanesulfonyloxy)imino)-p-phenylenediacetonitrile, bis(α-(4-methoxybenzenesulfonyloxy)imino)-p-phenylenediacetonitrile, phenyldiacetonitrile, bis(α-(p-toluenesulfonyloxy)imino)-meta-phenylenediacetonitrile, bis(α-(benzenesulfonyloxy)imino)-meta-phenylenediacetonitrile, bis(α-(methanesulfonyloxy)imino)-meta-phenylenediacetonitrile, bis(α-(butanesulfonyloxy)imino)-meta-phenylenediacetonitrile, bis(α-(10-camphorsulfonyloxy)imino)-meta-phenylenediacetonitrile, bis(α-(trifluoromethanesulfonyloxy)imino)-meta-phenylenediacetonitrile, and bis(α-(4-methoxybenzenesulfonyloxy)imino)-meta-phenylenediacetonitrile.
[0083] Oxime sulfonates having formula (C1) are also useful PAGs.
[0084]
[0085] Here R 21 is substituted or unsubstituted C1-C 10 A haloalkylsulfonyl or halobenzenesulfonyl group, R 22 It is C1-C 11 a haloalkyl group, and R 23 is a substituted or unsubstituted aryl or heteroaryl group.
[0086] Examples include 2-[2,2,3,3,4,4,5,5-octafluoro-1-(nonafluorobutylsulfonyloxyimino)pentyl]fluorene, 2-[2,2,3,3,4,4-pentafluoro-1-(nonafluorobutylsulfonyloxyimino)butyl]fluorene, 2-[2,2,3,3,4,4,5,5,6,6-decafluoro-1-(nonafluorobutylsulfonyloxyimino)hexyl]fluorene, 2-[2 ,2,3,3,4,4,5,5-octafluoro-1-(nonafluorobutylsulfonyloxyimino)pentyl]-4-biphenyl, 2-[2,2,3,3,4,4-pentafluoro-1-(nonafluorobutylsulfonyloxyimino)butyl]-4-biphenyl and 2-[2,2,3,3,4,4,5,5,6,6-decafluoro-1-(nonafluorobutylsulfonyloxyimino)hexyl]-4-biphenyl.
[0087] Among them, preferred PAGs are sulfonium salts, bissulfonyldiazomethanes, N-sulfonyloxyimides, and sulfonyloxime compounds.
[0088] Although the most suitable anion of the generated acid varies with factors such as the ease of cleavage of the acid-labile groups in the polymer, anions that are nonvolatile and not very diffusible are generally selected. Suitable anions include anions of benzenesulfonic acid, toluenesulfonic acid, 4-(4-toluenesulfonyloxy)benzenesulfonic acid, pentafluorobenzenesulfonic acid, 2,2,2-trifluoroethanesulfonic acid, nonafluorobutanesulfonic acid, heptadecafluorooctanesulfonic acid, and succinic acid. When a highly sensitive reaction is required, phosphate anions and alkylphosphate anions in which some of the hydrogen is replaced by fluorine can be used.
[0089] PAG (C) is preferably added in an amount of 0.2 to 20 parts by weight, more preferably 0.3 to 10 parts by weight per 100 parts by weight of component (A). The amount of PAG within this range ensures practically acceptable sensitivity and pattern profile. PAG can be used alone or in a mixture of two or more. The transmittance of the resin film can be controlled by using a PAG having a low transmittance at the exposure wavelength and adjusting the amount of PAG added.
[0090] Component (D)
[0091] Component (D) is at least one compound selected from benzotriazole compounds and imidazole compounds.
[0092] The benzotriazole compound is typically selected from compounds having formula (D1) and (D2).
[0093]
[0094] In formulas (D1) and (D2), R 31 and R 33 are each independently hydrogen, hydroxy, amino, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted phenyl, a sulfonyl-containing substituent, or -A 1 -A 2 . A 1 It is a carbonyl group, C1-C 12 Alkanediyl, C3-C 12 Cycloalkylene or -A 11 -O-, where A 11 It is C1-C 12 Alkanediyl group. 2 is hydrogen, halogen, cyano, hydroxy, C1-C6 alkoxy, carboxyl, or a dialkylamino group, wherein each alkyl moiety is C1-C6.
[0095] In formulas (D1) and (D2), R 32 and R 34Each is independently hydrogen, halogen, hydroxyl, optionally substituted C1-C6 alkyl, C1-C6 alkoxy, a sulfonyl-containing substituent, or an organic group having formula (D3):
[0096]
[0097] Where R 35 is hydrogen or an optionally substituted C1-C 12 alkyl, and d is 0 or 1.
[0098] Examples of the benzotriazole compound include benzotriazole, 1-hydroxybenzotriazole, 1-methylbenzotriazole, 1-hydroxymethylbenzotriazole, 1-ethylbenzotriazole, 1-(1-hydroxyethyl)benzotriazole, 1-(2-hydroxyethyl)benzotriazole, 1-propylbenzotriazole, 1-(1-hydroxypropyl)benzotriazole, 1-(2-hydroxypropyl)benzotriazole, 1-(3-hydroxypropyl)benzotriazole, 4-hydroxy-1H-benzotriazole, 5-methylbenzotriazole, 1-(1-hydroxyethyl ...1-(1-hydroxypropyl)benzotriazole, 1-(2-hydroxypropyl)benzotriazole, 1-(2-hydroxypropyl)benzotriazole, 1-(3-hydroxypropyl)benzotriazole, 1-(1-hydroxypropyl)benzotriazole, 1-(2-hydroxypropyl)benzotriazole, 1-(2-hydroxypropyl)benzotriazole, 1-(3-hydroxypropyl)benzotriazole, 1-(1-hydroxypropyl)benzotriazole, 1-(2-hydroxypropyl)benzotriazole, 1-(2-hydroxypropyl)benzotriazole, 1-(3-hydroxypropyl)benzotriazole, 1-(1-hydroxypropyl)benzotriazole, 1-(1-hydroxypropyl)benzotriazole, 1-(2-hydroxypropyl)benzotriazole, 1-(2-hydroxypropyl)benzotriazole, 1-(2- 1H-benzotriazole, benzotriazole-5-carboxylic acid, 1-methylbenzotriazole-5-carboxylic acid, 1-ethylbenzotriazole-5-carboxylic acid, 1-tert-butylbenzotriazole-5-carboxylic acid, 1-(2-cyclopentylethyl)benzotriazole-5-carboxylic acid, 1H-benzotriazole-4-sulfonic acid, 1H-benzotriazole-1-acetonitrile, 1H-benzotriazole-1-carboxaldehyde, 2-methyl-2H-benzotriazole and 2-ethyl-2H-benzotriazole.
[0099] The imidazole compound is typically selected from compounds having formulae (D4) to (D9).
[0100]
[0101] In formulas (D4) to (D9), R 41 is hydrogen, or a C2-C 20 An alkyl group, wherein the polar functional moiety is selected from hydroxyl, carbonyl, ester, ether, sulfide, carbonate, cyano and acetal. 42 , R 43 and R 44 are independently hydrogen, C1-C 10 Alkyl, C6-C 10 Aryl or C7-C 10 Aralkyl group. 45 , R 47 , R 49 and R 53 Each independently is C1-C 10 Alkanediyl group. 46 and R 48 Each independently is hydrogen, or may contain at least one C1-C 15An alkyl group, wherein the moiety is selected from the group consisting of hydroxy, carbonyl, ester, ether, sulfide, carbonate, cyano and acetal. 50 is a C1-C 15 An alkyl group, wherein the moiety is selected from the group consisting of hydroxy, carbonyl, ester, ether, sulfide, carbonate, cyano and acetal. 51 is (h+1)-valence C2-C 10 Hydrocarbon group. 52 Each independently is hydrogen, or may contain at least one C1-C 15 An alkyl group, wherein the moiety is selected from hydroxyl, carbonyl, ester, ether, sulfide, carbonate, cyano and acetal, or two R 52 The groups may be bonded together to form a ring, and h is 2, 3, 4 or 5.
[0102] Preferred examples of the imidazole compound include imidazole, 2-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-methoxymethylimidazole, N-tert-butoxycarbonylimidazole, 1-(2-cyanoethyl)-2-methylimidazole, 1-(2-hydroxyethyl)imidazole, 1-(carboxymethyl)imidazole and 2-methyl-1-vinylimidazole.
[0103] Component (D) is preferably used in an amount of 0.01 to 10 parts by weight, more preferably 0.02 to 5 parts by weight per 100 parts by weight of component (A). The amount of component (D) within this range ensures pattern formation with practically acceptable sensitivity.
[0104] Component (E)
[0105] There is no particular limitation on the organic solvent as component (E) as long as other components are soluble therein and satisfactory coating properties can be achieved. Suitable organic solvents include cellosolve solvents such as methyl cellosolve, ethyl cellosolve, methyl cellosolve acetate and ethyl cellosolve acetate; propylene glycol solvents such as propylene glycol and dipropylene glycol; propylene glycol alkyl ether solvents such as propylene glycol monomethyl ether (PGME) and propylene glycol monobutyl ether; propylene glycol alkyl ether acetate solvents such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol dimethyl ether and propylene glycol monoethyl ether acetate; ester solvents such as butyl acetate, ethyl acetate, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monomethyl ...methyl ether esters, such as methyl phenyl ether and diethylene glycol dimethyl ether; highly polar solvents such as N,N-dimethylformamide, N-methylpyrrolidone and dimethyl sulfoxide; and mixtures thereof.
[0106] Among these solvents, propylene glycol alkyl ether acetate, alkyl lactate and alkyl ketone are preferred. It should be noted that the alkyl group of propylene glycol alkyl ether acetate preferably has 1-4 carbon atoms, such as methyl, ethyl and propyl, of which methyl and ethyl are particularly preferred. Since propylene glycol alkyl ether acetate includes 1,2- and 1,3-substituted propylene glycol alkyl ether acetate, each includes three isomers depending on the combination of substitution positions, which can be used alone or in combination. Similarly, the alkyl group of alkyl lactate preferably has 1-4 carbon atoms, such as methyl, ethyl and propyl, of which methyl and ethyl are particularly preferred. The alkyl group of alkyl ketone preferably has 1-10 carbon atoms, such as methyl, ethyl, propyl, isobutyl, cyclopentyl and cyclohexyl, of which isobutyl, cyclopentyl and cyclohexyl are particularly preferred.
[0107] The amount of component (E) is preferably 20 to 90% by weight, more preferably 25 to 70% by weight of the composition. The amount of component (E) within this range ensures formation of a film having a uniform thickness and avoids the risk of defects in the film.
[0108] Other components
[0109] In addition to the aforementioned components, the photosensitive resin composition may contain additives such as surfactants. Examples of surfactants include nonionic surfactants, for example, polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether, polyoxyethylene alkyl aryl ethers such as polyoxyethylene octylphenyl ether and polyoxyethylene nonylphenyl ether, polyoxyethylene polyoxypropylene block copolymers, sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, and sorbitan monostearate, polyoxyethylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate, and polyether silicones; fluorine-containing compound surfactants such as EF301, EF303 and EF352 (Tohkem Products Co., Ltd.), F171, F172 and F173 (DIC Corp.), FC-4430, FC-430 and FC-431 (Sumitomo 3M Co.,Ltd.), E1004 (Nissin Chemical Industry Co., Ltd.), AG710, S-381, S-382, SC101, SC102, SC103, SC104, SC105, SC106, KH-10, KH-20, KH-30 and KH-40 (AGC Seimi Chemical Co., Ltd.); organosiloxane polymer KP341, X-70-092 and X-70-093 (Shin-Etsu Chemical Co., Ltd.), acrylic acid or methacrylic acid Polyflow No. 75 and No. 95 (Kyoeisha Ushi Kagaku Kogyo Co., Ltd.). In particular, FC-4430 and X-70-093 are preferred. These surfactants can be used alone or in combination.
[0110] The surfactant is preferably formulated in an amount of up to 5 parts by weight, and more preferably up to 2 parts by weight, per 100 parts by weight of component (A).
[0111] In the resin composition, other optional components may be added, such as a light absorbing substance (e.g., dye) for reducing diffuse reflection from the substrate, a compound having a 1,2-naphthoquinonediazidesulfonyl group in the molecule, a basic compound, a sensitizer, a crosslinking agent, a photobase generator, and an acid multiplier. Such optional components may be added in conventional amounts as long as they do not impair the benefits of the present invention.
[0112] The photosensitive resin composition may be prepared by any conventional method, for example, by dissolving components (A) to (D) and optional components in an organic solvent (E) simultaneously or in any order to form a uniform solution of the photosensitive resin composition. If necessary, the resulting solution may be passed through a filter.
[0113] Pattern forming method using photosensitive resin composition
[0114] Another embodiment of the present invention is a method for forming a pattern using the photosensitive resin composition defined above, the method comprising the steps of: (a) applying the photosensitive resin composition to a substrate to form a photosensitive resin coating thereon, (b) exposing the photosensitive resin coating to radiation, and (c) developing the exposed resin coating in an organic solvent.
[0115] In step (a), a photosensitive resin coating is formed on a substrate using a photosensitive resin composition. Examples of substrates include substrates of Si, SiO2, SiN, SiON, TiN, WSi, BPSG and SOG, metal substrates of Au, Ti, W, Cu, Ni-Fe, Ta, Zn, Co and Pb, and organic anti-reflective coatings.
[0116] When forming the photosensitive resin coating, the photosensitive resin composition is generally applied to the substrate by a suitable coating technique such as spin coating, roller coating, flow coating, dipping, spray coating, knife coating, etc., with such a coating weight that the coating can have a desired thickness. If necessary, the coating is prebaked on a hot plate or in an oven at 60 to 150° C. for 0.5 to 120 minutes, preferably at 80 to 130° C. for 1 to 90 minutes.
[0117] Next, in step (b), the photosensitive resin coating is exposed to radiation. Exposure preferably uses radiation having a wavelength of at least 300 nm, more preferably 300 to 500 nm. Examples of radiation include UV radiation such as g-line and i-line. Suitable exposure doses are about 1 to 5,000 mJ / cm 2 , more preferably about 10 to 4,000 mJ / cm 2 .
[0118] Exposure can be performed through a photomask. The photomask may be, for example, a photomask perforated with a desired pattern. Although the material of the photomask is not particularly limited, a material capable of shielding irradiation within the above wavelength range is preferred. For example, a mask having a light shielding film of chromium is used.
[0119] The next step may be a post-exposure bake (PEB). PEB is generally performed on a hot plate or in an oven at 60 to 150°C for 1 to 90 minutes, preferably at 80 to 130°C for 1 to 60 minutes.
[0120] Exposure or PEB is followed by a step (c) of developing the exposed resin coating in an organic solvent. The organic solvent is preferably selected from alcohols such as isopropyl alcohol (IPA), ketones such as cyclohexanone and glycols such as PGME and PGMEA. Solvents used in the photosensitive resin composition are also useful.
[0121] Development is carried out by conventional means such as dipping, puddle or spraying. If necessary, development is followed by rinsing, rinsing and drying. In this way, a photosensitive resin coating with a desired pattern is obtained. Although the development time is selected depending on the thickness of the photosensitive resin coating, the time is generally 0.1 to 180 minutes, preferably 0.5 to 120 minutes.
[0122] Photosensitive dry film
[0123] Another embodiment of the present invention is a photosensitive dry film comprising a support film and a photosensitive resin coating thereon.
[0124] The dry film is usually made in a clean room with a cleanliness of up to 1,000. The clean room includes an area maintained at a temperature of 5 to 45°C, preferably 15 to 35°C and a humidity of 5 to 90%, preferably 10 to 70%, in which a film coater is arranged. Examples of film coaters include forward roll coaters, reverse roll coaters, notched wheel coaters, pattern coaters, lip coaters, gravure coaters, dip coaters, air knife coaters, capillary coaters, raising and rising, R&R coaters, blade coaters, rod coaters, coaters and extrusion molding machines. By means of a film coater, the photosensitive resin composition is applied to a support film such as a thermoplastic film or a demoulding substrate. The coating speed is preferably 0.05 to 1,000 m / min, more preferably 0.1 to 500 m / min.
[0125] After the resin composition is applied, the coated support is passed through an online dryer or hot air circulation oven preferably at 40 to 130° C. for 1 to 40 minutes, more preferably 50 to 120° C. for 2 to 30 minutes, until the organic solvent and any volatiles are removed. By drying in this way, a photosensitive resin coating or film is formed on the support. Photosensitive dry films can also be constructed by replacing an online dryer with infrared irradiation or a combination of multiple drying methods, such as solvent removal using an online dryer and infrared irradiation simultaneously. If necessary, a protective film (or another demoulding substrate) can be pressure-bonded to the photosensitive resin coating by means of a roller laminator, thereby producing a laminate.
[0126] Preferably, the photosensitive resin coating layer formed on the support film has a thickness of 10 to 700 μm, more preferably 50 to 600 μm, and an organic solvent content of 0 to 15 wt %.
[0127] In one embodiment, a photosensitive resin coating can be continuously formed on a support film to produce a certain length of photosensitive dry film, which is wound in the form of a film roll that is easy to handle. This is also the case when the photosensitive dry film is covered with a protective film.
[0128] The support film and (optional) protective film are not particularly limited as long as the film does not adversely affect the shape of the photosensitive dry film and can be separated from the photosensitive resin coating. The film can be a single polymer film or a multilayer film consisting of multiple polymer layers. Any plastic film can be used, including nylon film, polyethylene (PE) film, polyethylene terephthalate (PET) film, polyethylene naphthalate film, polyphenylene sulfide (PPS) film, polypropylene (PP) film, polystyrene film, polymethylpentene (TPX) film, polycarbonate film, fluororesin film, special polyvinyl alcohol (PVA) film and polyester film treated with a release agent.
[0129] Among them, due to appropriate flexibility, PET and PE films are preferred as protective films. Commercially available films can also be used. Available PET films include E-7301, E-7302 and E-7304 (Toyobo Co., Ltd.). Available PE films include GF-8 (Tamapoly Co., Ltd.), PE FILM OTYPE (Nippa Corp.), Toretec 7332, Toretec 7111 and Toretec 7721 (Toray Advanced Film Co., Ltd.).
[0130] The support film and the protective film each have a thickness of preferably 10 to 150 μm, more preferably 25 to 100 μm, from the viewpoint of consistent film formation and prevention of curling in a roll state wound on a take-up mandrel.
[0131] Pattern forming method using photosensitive dry film
[0132] Still another embodiment of the present invention is a pattern forming method comprising the steps of: (a') using a photosensitive dry film to form a photosensitive resin coating on a substrate, (b) exposing the photosensitive resin coating to radiation, and (c) developing the exposed resin coating in an organic solvent.
[0133] In step (a'), a photosensitive dry film is used to form a photosensitive resin coating on a substrate. The substrate is selected from a plastic film or sheet, a semiconductor substrate of Si, SiO2, SiN, SiON, TiN, WSi, BPSG and SOG, a metal substrate of Au, Ti, W, Cu, Ni-Fe, Ta, Zn, Co and Pb, and an organic substrate such as an organic anti-reflective coating. The substrate may have steps (convex and concave parts) on its surface, which are usually left after forming a circuit or a dielectric resin layer by plating or sputtering. Such steps are preferably in the range of 0 to about 500 μm, more preferably about 3 to 400 μm, and even more preferably about 5 to 300 μm.
[0134] The photosensitive dry film is bonded to the substrate using a suitable laminator such as a vacuum laminator or a roller laminator, after which the support is peeled off so that the photosensitive resin coating is transferred to the substrate. The substrate may have a step structure as mentioned above. In this case, a photosensitive resin coating having an appropriate thickness corresponding to the step height is used so that the photosensitive resin coating can be buried in the step. The photosensitive resin coating can be advantageously applied to a substrate having a step of 0 to 500 μm in magnitude. Prebaking may or may not be performed after the transfer step. When prebaking is performed, the assembly is prebaked on a hot plate or in an oven at 60 to 150° C. for 1 to 90 minutes, preferably at 80 to 130° C. for 1 to 30 minutes.
[0135] Step (a') is followed by steps (b) and (c) in the same manner as in the pattern forming method using the photosensitive resin composition.
[0136] Plating steps
[0137] After the development step, electroplating or electroless plating can be performed to form a metal coating on the substrate with the resin pattern. That is, a metal plating pattern is obtained. The plating step can be any of the standard electroplating or electroless plating methods to deposit the conductor pattern, and then remove the resin (or resist) pattern.
[0138] Suitable electroplating or electroless plating methods include electroplating Cu, electroless Cu, electroplating Ni, electroless Ni and electroplating Au. Can be plated in any known plating bath and under standard conditions. The thickness of the coating is generally 80 to 100% of the thickness of the resist pattern. For example, a 1 μm thick resist pattern is formed on the seed layer of Cu, and thereafter a 0.8 to 1.2 μm thick Cu plating pattern is deposited thereon by electroplating Cu.
[0139] Example
[0140] Examples of the present invention are given below by way of illustration and not by way of limitation. In particular, the weight average molecular weight (Mw) was measured by gel permeation chromatography (GPC) on monodisperse polystyrene standards using a GPC column TSKgel Super HZM-H (Tosoh Corp.) under the following analytical conditions: flow rate 0.6 mL / min, tetrahydrofuran eluent and column temperature 40° C. Parts are by weight (pbw).
[0141] Compounds (M-1) to (M-5) used in Synthesis Examples are shown below.
[0142]
[0143] [1] Synthesis of polymers
[0144] Synthesis Example 1
[0145] Synthesis of Poly-1
[0146] 172.1 g (0.40 mol) of the compound (M-1), 53.9 g (0.10 mol) of the compound (M-2) (having Mw ∼ 500) (NOF Corp. ) and 2,000 g of toluene were charged into a 3-L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser, and heated at 70°C. Thereafter, 1.0 g of chloroplatinic acid toluene solution (platinum concentration 0.5 wt%) was added, and 97.0 g (0.50 mol) of compound (M-3) was added dropwise over 1 hour. The molar ratio of the total amount of hydrosilyl groups to the total amount of alkenyl groups was 1 / 1. At the end of the dropwise addition, the reaction solution was heated at 100°C and matured for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to produce Poly-1. The Mw of Poly-1 was 38,000 and was obtained by 1 H-NMR spectroscopy (Bruker Corp.) identified it as the desired polymer.
[0147] Synthesis Example 2
[0148] Synthesis of Poly-2
[0149] 217.1 g (0.40 mol) of compound (M-4), 53.9 g (0.10 mol) of compound (M-2) (having Mw ∼ 500) (NOF Corp. ) and 2,000 g of toluene were charged into a 3-L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser, and heated at 70°C. Thereafter, 1.0 g of chloroplatinic acid toluene solution (platinum concentration 0.5 wt%) was added, and 97.0 g (0.50 mol) of compound (M-3) was added dropwise over 1 hour. The molar ratio of the total amount of hydrosilyl groups to the total amount of alkenyl groups was 1 / 1. At the end of the dropwise addition, the reaction solution was heated at 100°C and matured for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to produce Poly-2. The Mw of Poly-2 was 40,000 and was obtained by 1 H-NMR spectroscopy (Bruker Corp.) identified it as the desired polymer.
[0150] Synthesis Example 3
[0151] Synthesis of Poly-3
[0152] Using 217.1 g (0.40 mol) of compound (M-4), 70.4 g (0.10 mol) of compound (M-5) (NOF Corp. ) and 2,000 g of toluene were charged into a 3-L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser, and heated at 70°C. Thereafter, 1.0 g of a chloroplatinic acid toluene solution (platinum concentration 0.5 wt%) was added, and 97.0 g (0.50 mol) of compound (M-3) was added dropwise over 1 hour. The molar ratio of the total amount of hydrosilyl groups to the total amount of alkenyl groups was 1 / 1. At the end of the dropwise addition, the reaction solution was heated at 100°C and matured for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to produce Poly-3. The Mw of Poly-3 was 35,000 and was obtained by 1 H-NMR spectroscopy (Bruker Corp.) identified it as the desired polymer.
[0153] [2] Preparation of photosensitive resin composition
[0154] Examples 1-1 to 1-11 and Comparative Examples 1-1 to 1-5
[0155] Photosensitive resin compositions 1 to 16 were prepared by mixing a polymer (Poly-1, Poly-2 or Poly-3), a photoacid generator (PAG-1 or PAG-2), a phenol compound (Ph-1, Ph-2 or Ph-3), a benzotriazole compound (BTA-1 or BTA-2), an imidazole compound (4-MI), an organic solvent (cyclopentanone) and optional additives according to the formulation shown in Table 1, and filtering through a membrane filter having a pore size of 1.0 μm. All compositions contained 0.10 pbw of a surfactant KP-341 (Shin-Etsu Chemical Co., Ltd.).
[0156] In Table 1, PAG-1, PAG-2, Ph-1, Ph-2, Ph-3, BTA-1, BTA-2, 4-MI and Nikalac MW-390 are identified as follows.
[0157] PAG-1: PAI-101 (manufactured by Midori Kagaku Co., Ltd., 4-methylphenylsulfonyloxyimino-α-(4-methoxyphenyl)acetonitrile).
[0158] PAG-2: CPI-200K (San-Apro Ltd.)
[0159] Ph-1: EP 6050G (Asahi Yukizai Corp., m-cresol / p-cresol=40 / 60, Mw=2,500-4,000)
[0160] Ph-2: Maruka Lyncur MS-2P (Maruzen Petrochemical Co., Ltd., poly(p-vinylphenol), Mw=5,000)
[0161] Ph-3: Tris P-PA (Honshu Chemical Industry Co., Ltd., α,α-bis(4-hydroxyphenyl)-4-(4-hydroxy-α,α-dimethylbenzyl)ethylbenzene)
[0162] BTA-1, BTA-2, 4-MI:
[0163]
[0164] Nikalac MW-390: Hexamethoxymethyl melamine (Sanwa Chemical Co., Ltd.)
[0165] Table 1
[0166]
[0167]
[0168] [3] Formation of patterns using photosensitive resin compositions and evaluation
[0169] Examples 2-1 to 2-11 and Comparative Examples 2-1 to 2-5
[0170] Each of the photosensitive resin compositions 1 to 16 was spin-coated on an 8-inch silicon wafer on which Cu was deposited by sputtering, and pre-baked on a hot plate at 110° C. for 5 minutes to form a 100 μm thick photosensitive resin coating. The photosensitive resin coating was exposed to i-line by reticle using an i-line stepper (NSR-2205i11D of Nikon Corp.). The resin coating was PEBed at 100° C. for 2 minutes, spray-developed in PGMEA for 15 minutes, and dried to form a pattern.
[0171] The exposure dose, resolution and pattern profile of the pattern were analyzed using a scanning electron microscope (S-4700 from Hitachi High-Technologies Corp.). The optimum dose is the exposure dose when a hole pattern with a size of 50 μm is printed to 50 μm. The resolution is the mask size through which the smallest hole pattern can be resolved at the optimum dose.
[0172] Table 2
[0173]
[0174]
[0175] [4] Preparation and evaluation of photosensitive dry films
[0176] Example 3
[0177] In a clean room with a cleanliness level of 1,000, a humidity of 40-45% and a temperature of 22-26° C., the photosensitive resin composition 7 was applied to a 38 μm thick PET film as a support film by means of a die coater as a film coater. The coated film was passed through a hot air circulation oven (length 4 m) set at 100° C. for more than 5 minutes to form a photosensitive resin coating layer (100 μm thick) on the support film, thereby producing a photosensitive dry film. A 50 μm thick PE film as a protective film was bonded to the surface of the photosensitive resin coating layer under a pressure of 1 MPa, thereby producing a photosensitive dry film with a protective film.
[0178] The protective film was peeled off from the photosensitive dry film with the protective film. The photosensitive resin coating on the support film was tightly bonded to a 200 mm copper substrate at a temperature of 60° C. using a vacuum laminator TEAM-100M (Takatori Corp.) with a vacuum chamber set at 80 Pa vacuum. After restoring the atmospheric pressure, the substrate was taken out of the laminator and the support film was peeled off. This process was repeated three times to form a three-layer photosensitive resin coating.
[0179] The photosensitive resin coating / substrate was then pre-baked on a hot plate at 110°C for 5 minutes. The thickness of the pre-baked photosensitive resin coating was measured by a contact film thickness meter (Mitsutoyo Co., Ltd.) and found to be 300 μm. The photosensitive resin coating was exposed to the i-line by a reticle using an i-line stepper (NSR-2205i11D from Nikon Corp.). The resin coating was PEBed at 100°C for 2 minutes, puddle developed in PGMEA for 45 minutes, rinsed with deionized water, and dried to form a pattern.
[0180] The pattern was observed under SEM S-4700 and it was found that the 2 The exposure dose resolved the hole pattern of 20 μm size as a rectangle.
[0181] Japanese Patent Application No. 2018-237135 is incorporated herein by reference.
[0182] While some preferred embodiments have been described, numerous modifications and variations are possible in light of the above teachings. It should therefore be understood that the invention may be practiced otherwise than as specifically described without departing from the scope of the appended claims.
Claims
1. A photosensitive resin composition comprising: (A) a polymer comprising a repeating unit having the formula (A1) shown below and at least one type of repeating unit selected from a repeating unit having the formula (A2) shown below and a repeating unit having the formula (A3) shown below, (B) a phenol compound having a weight average molecular weight of 300 to 10,000, (C) a photoacid generator, (D) a benzotriazole compound and / or an imidazole compound, and (E) an organic solvent, Where X 1 and X 2 are each independently hydrogen or a glycidyl group, Y 1 is a C1-C5 straight-chain or branched alkanediyl group, Z 1 It is a C1-C 10 Straight chain alkanediyl groups, C2-C 10 A branched alkanediyl group or a divalent group having the formula (A4): Where Z 11 and Z 13 Each is independently a C1-C5 straight chain or branched alkanediyl group, Z 12 It is C1-C 30 A divalent hydrocarbon group, a 4 and a 5 are each independently an integer from 1 to 50, R 1 , R 2 , R 3 and R 4 are independently hydrogen or C1-C 10 A monovalent hydrocarbon group, a 1 、a 2 and a 3 Is a number in the following range: 0 1 <1, 0≤a 2 <1, 0≤a 3 <1 and a 1 +a 2 +a 3 =1, x and y are each independently an integer from 1 to 50, The phenol compound having a weight average molecular weight of 300 to 10,000 is a compound having the following formula (B1), (B2) or (B3), in, j is 1 or 2, m, p and r are each independently an integer from 0 to 3, q is an integer from 1 to 3, and n is an integer from 1 to 4, satisfying 1≤m+n+p≤6 and 1≤q+r≤5, k is an integer of 2 or 3, s and t are each independently an integer from 0 to 3, satisfying 0≤s+t≤4, R 11 To R 16 are each independently hydrogen, methyl, or a group having the following formula (B4), provided that R 11 To R 13 At least one and R 14 To R 16 At least one of them is a group having the formula (B4), wherein u is an integer from 1 to 3, Here, u and v are each independently an integer from 0 to 3, satisfying 0≤u+v≤4.
2. A photosensitive resin coating obtained from the photosensitive resin composition of claim 1.
3. A photosensitive dry film comprising a support film and the photosensitive resin coating of claim 2 thereon.
4. A pattern forming method comprising the following steps: (a) applying the photosensitive resin composition of claim 1 to a substrate to form a photosensitive resin coating thereon, (b) exposing the photosensitive resin coating to radiation, and (c) The exposed resin coating is developed with an organic solvent.
5. A pattern forming method comprising the following steps: (a') using the photosensitive dry film of claim 3 to form a photosensitive resin coating on a substrate, (b) exposing the photosensitive resin coating to radiation, and (c) The exposed resin coating is developed with an organic solvent.
Citation Information
Patent Citations
Silphenylene skeleton-bearing polymer compound, photo-curable resin composition and patterning process, and substrate circuit protective film
JP2008184571A
Photosensitive resin composition, photosensitive dry film, and pattern forming process
JP2020098296A
Semiconductor apparatus, stacked semiconductor apparatus, encapsulated stacked-semiconductor apparatus, and method for manufacturing the same
CN106249542A
Photo-curable resin composition and photo-curable dry film using the same
CN106249547A
Chemically amplified positive resist composition and pattern forming process
CN106444288A