Monoalkylated diamines for epoxy formulations: New hardeners for epoxy systems
By using monoalkylated araliphatic and alicyclic diamines as the main curing agent, the problem of premature increase in viscosity of the epoxy resin system during processing is solved, the working time and pot life are extended, and the mechanical properties of the composite materials are improved. and thermal performance.
Patent Information
- Application Number
- CN202010025500.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-01-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-01-10
AI Technical Summary
The viscosity of existing epoxy resin systems increases prematurely during processing, resulting in difficulty in fiber wetting and loss of mechanical properties. Short working times and high viscosity caused by high-functionality curing agents limit the performance improvement of composite materials.
Monoalkylated araliphatic and cycloaliphatic diamines are used as the primary curing agent to extend working time and reduce viscosity, and are used with primary or secondary amines to enhance performance to form epoxy with longer pot life and low temperature curing characteristics. Resin system.
It achieves significantly extended working time at low temperatures, maintains high mechanical, thermal and chemical properties, reduces viscosity, improves fiber wetting effect, and improves the overall performance of composite materials.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_4
Abstract
Description
Background Art
[0001] Aromatic aliphatic amines and cycloaliphatic amines are commonly used as epoxy curing agents for heat cured structural composite applications. The class of amine used as curing agent is critical to achieving the final properties of the cured product. To achieve full cure, each of the classes of reactive amines, primary or secondary, cures at a specific temperature. This cure temperature determines the final use temperature, which is determined by the T of the cured product. g Indication. Typically, formulating epoxy resins with high functionality curing agents (hardeners) results in short working times, high formulation viscosity, and brittle parts after curing. These negative effects are all caused by the high functionality of the curing agent. It is well known that in step-growth polymerization, the degree of polymerization, X n , and the critical reaction degree (gel point - p c ) is directly related to the functionality of the polymer system: X n =2 / (2-pf 平均 ), where p is the degree of reaction, and f 平均 is the average functionality, and p c =2 / f 平均 Thus, systems with high average functionality will reach high molecular weights and gel at lower degrees of polymerization than those systems with low average functionality. US Patent No. 4,293,682 discloses the use of tetra- and pentafunctional amines as curing agents.
[0002] Although low functionality curing agents will provide longer pot life, they result in a final cured network with low crosslink density and poor thermal and mechanical properties. This inverse relationship between the high functionality monomers required for final part performance and the low functionality monomers required for increased working time requires compromises in formulating epoxy resins. Certain lower functionality materials will not build a strong polymer network for structural applications. Any measures that can be implemented to increase working time without adversely affecting final part performance will be beneficial.
[0003] Epoxy resin systems are used to manufacture various structural parts, including composite materials. Examples of products being evaluated for manufacture by epoxy resin systems include composite pipes, pressure vessels, automotive parts, and windmill blades. The manufacture of such parts includes many requirements for efficient manufacturing, especially when complex manufacturing processes are used. These processes include, but are not limited to, resin infusion, resin transfer molding, filament winding, and large-scale casting. One of the needs in the art is a longer working time for epoxy resin systems to wet the fibers in the thicker parts of the product, because in these parts the fabric layers are very tight under vacuum or pressure and the resin cannot easily penetrate the fabric layers. If the temperature rises during the processing of the product, the viscosity of the alicyclic amine will increase under such conditions, and fiber wetting becomes challenging and results in a loss of mechanical properties in the manufactured parts.
[0004] Furthermore, a premature increase in viscosity during processing may result in a higher shrinkage after curing of the manufactured part. During processing, the shrinkage of the cured epoxy resin due to the increase in viscosity leads to stress accumulation in the composite material. The stress sometimes leads to interlaminar cracking in the article, resulting in a loss of mechanical properties. During the processing of larger parts, the shorter pot life of the formulation causes a faster increase in viscosity and a greater amount of stress will accumulate in the article during processing.
[0005] For the composite material for realizing the upgrade of higher performance, multifunctional resin and curing agent are often used. The multifunctional material usually has a very high initial viscosity. In order to reduce the formulation viscosity, heat is usually used. This approach increases the reactivity, thus causing some processing problems. When the composite material parts become larger and thicker, the formulation viscosity needs to be lower to have the best wetting of reinforcement (such as glass, carbon, Kevlar, natural fiber, etc.).
[0006] Systems for composite processing require that the initial mix viscosity be low enough and the rate of viscosity increase at the impregnation temperature be slow enough to allow the reinforcement fiber preform to be fully wetted by the resin before the resin system becomes too viscous to flow satisfactorily through the fibers and fabric of the substrate. As the size of composite parts increases, the requirements for low initial viscosity and long pot life become more stringent.
[0007] In view of the foregoing, there is a need in the art for improved curing agents for preparing epoxy resin systems that have a longer pot life "working time" of the formulation to reduce material replenishment during processing when compared to prior art resin compositions and that when combined with improved fiber wetting, result in enhanced mechanical properties.
[0008] The dialkylation of isophoronediamine (IPD) is known in the literature (U.S. Pat. No. 7,074,963 B2). The monoalkylated structure of IPD is an intermediate of the dialkylated IPD product. The final composition of the dialkylated IPD reported in U.S. Pat. Nos. 6,403,752 B1 and 7,074,963 B2 does not have any monoalkylated IPD present. In the present invention, monoalkylated IPD and other monoalkylated alicyclic diamines will be used as epoxy curing agents to extend the pot life of IPD, which has not been found in any prior art. In addition, the isomer type of the monoalkylated IPD product in the present invention is different from the monoalkylated IPD suggested in U.S. Pat. No. 7,074,963 B2 for the preparation of the dialkylated product. Non-alkylated (unmodified) IPD obtains a higher T g The dialkylated IPD product does not fully cure with the epoxy resin. The present invention using monoalkylated IPD and other monoalkylated alicyclic diamines maintains a high T g while achieving an excellent balance of pot life. Summary of the invention SUMMARY OF THE INVENTION
[0010] It has been found that monoalkylated aromatic aliphatic and alicyclic diamines can be used as primary curing agents for epoxy resin compositions, which provide sufficient working time during processing (in the resin bath and fiber wetting), which generally improves the mechanical properties of the cured composite product compared to typical alicyclic amine-based curing agents. The main disadvantage of alicyclic amines is that they have a short pot life. Another way to measure pot life in industry is the time for the formulation viscosity to double. This gives a good measure of the working life of the system. By using monoalkylated alicyclic diamines as primary curing agents, a pot life twice that of the alicyclic diamines can be achieved, and sufficient curing is achieved at significantly lower temperatures than current alicyclic amine curing agents. Test results show that the use of monoalkylated alicyclic diamines as primary curing agents maintains good mechanical, thermal and chemical processing properties in cured epoxy compositions, and exceeds the mechanical properties of other alicyclic amines. In addition, formulations containing monoalkylated cycloaliphatic diamines achieve lower viscosity, longer pot life, lower temperature T, and lower hardness compared to cured epoxy compositions using current cycloaliphatic amine curing agents. g The monoalkylated alicyclic diamines can also be used in combination with primary and secondary amines as co-curing agents to further enhance the desired properties. The lower viscosity of the monoalkylated alicyclic diamines aids in fiber wetting. Preliminary results using monoalkylated alicyclic diamines in composite applications (filament wound pipes and fittings, wind blades, high pressure vessels, structural laminates, automotive body parts, aerospace, etc.) are very encouraging.
[0011] One aspect of the present invention is an epoxy resin system comprising an epoxy resin and a monoalkylated diamine of formula (I):
[0012]
[0013] Wherein Z is selected from cyclohexyl, C1-C 10 Alkyl-substituted cyclohexyl, phenyl, C1-C 10 Alkyl-substituted phenyl, methylenebis(cyclohexyl) and C1-C 10 Alkyl substituted methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is C1-C 10 The monoalkyl diamine includes a monoalkylated alicyclic diamine or a monoalkylated aromatic aliphatic diamine, which is selected from the group consisting of monoalkylated IPD, monoalkylated PACM, monoalkylated DMPACM, monoalkylated MXDA, monoalkylated cyclohexyl diamine and monoalkylated methylcyclohexyl diamine. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 The viscosity distribution curves of the epoxy resin composition containing non-alkylated IPD and the epoxy resin composition containing mono-alkylated IPD (AIPD) at 40°C are shown.
[0015] definition
[0016] The following definitions and abbreviations are provided to assist those skilled in the art in understanding the detailed description of the present invention.
[0017] IPD——isophorone diamine
[0018] PACM——4,4'-methylenebis(cyclohexylamine)
[0019] MXDA——m-xylenediamine
[0020] DMPACM——2,2'-dimethyl-4,4'-methylenebis(cyclohexylamine)
[0021] Hydrogenated TDA——Methylcyclohexyldiamine
[0022] CHONE——cyclohexanone
[0023] MEK - Methyl Ethyl Ketone
[0024] ISO: Isophorone DETAILED DESCRIPTION OF THE INVENTION
[0026] The epoxy resin system of the present invention comprises an epoxy resin and a monoalkylated diamine of formula (I):
[0027]
[0028] Wherein Z is selected from cyclohexyl, C1-C 10 Alkyl-substituted cyclohexyl, phenyl, C1-C 10 Alkyl-substituted phenyl, methylenebis(cyclohexyl) and C1-C 10 Alkyl substituted methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is C1-C 10 alkyl.
[0029] The monoalkylated diamines can preferably be obtained by reaction of the corresponding diamines with acetone, methyl ethyl ketone, cyclohexanone, isophorone or aliphatic aldehydes such as acetaldehyde and subsequent hydrogenation, or by reaction of the diamines with alkyl halides. Thus, Y can preferably be a cyclohexyl group, a sec-butyl group, a trimethylcyclohexyl group or an isopropyl group, which are derived from the respective ketones, aldehydes and alkyl halides.
[0030] In a preferred embodiment of the present invention, the monoalkylated diamine is represented by the following structure:
[0031]
[0032] wherein each of R1, R2, R3, R4, R5 and R6 is H, CH3 or a C2-C4 alkyl group, wherein n is 0 or 1, and wherein A is H and B is C1-C 10 Alkyl, or B is H and A is C1-C 10 The monoalkylated diamine can preferably be obtained by reaction of the diamine with acetone, methyl ethyl ketone, cyclohexanone, isophorone or an aliphatic aldehyde (such as acetaldehyde) and subsequent hydrogenation, or by reaction of the diamine with an alkyl halide. Thus, A or B can preferably be a cyclohexyl group, a sec-butyl group, a trimethylcyclohexyl group or an isopropyl group, which is derived from the respective ketone, aldehyde and alkyl halide.
[0033] In a preferred embodiment of structure (II), the monoalkylated diamine is selected from the monoalkylated isophorone diamine represented by the following structure:
[0034]
[0035] Where A is C1-C 10 alkyl;
[0036] Monoalkylated isophoronediamine represented by the structure:
[0037]
[0038] Where B is C1-C 10 alkyl;
[0039] Monoalkylated methylcyclohexyldiamine represented by the following structure:
[0040]
[0041] Where A is C1-C 10 alkyl;
[0042] Monoalkylated methylcyclohexyldiamine represented by the following structure:
[0043]
[0044] Where B is C1-C 10 Alkyl; and
[0045] Monoalkylated cyclohexyl diamine represented by the following structure:
[0046]
[0047] Where A is C1-C 10 alkyl.
[0048] In another preferred embodiment of the present invention, the monoalkylated diamine is represented by the following structure:
[0049]
[0050] wherein each of R1 and R2 is H or CH3, and wherein A is C1-C 10 The monoalkylated diamines can preferably be obtained by reaction of the diamines with acetone, methyl ethyl ketone, cyclohexanone, isophorone or aliphatic aldehydes (such as acetaldehyde) and subsequent hydrogenation, or by reaction of the diamines with alkyl halides. Thus, A is preferably a cyclohexyl group, a sec-butyl group, a trimethylcyclohexyl group or an isopropyl group, which are derived from the respective ketones, aldehydes and alkyl halides.
[0051] In another preferred embodiment of Structure (VIII), the monoalkylated diamine is selected from the group consisting of monoalkylated 4,4'-methylenebis(cyclohexylamine) represented by the following structure:
[0052]
[0053] Where A is C1-C 10 Alkyl; and
[0054] Monoalkylated 2,2'-dimethyl-4,4'-methylenebis(cyclohexylamine) represented by the following structure:
[0055]
[0056] Where A is C1-C 10 alkyl.
[0057] In another preferred embodiment of the present invention, the monoalkylated diamine is represented by the following structure:
[0058]
[0059] wherein X is a phenyl or cyclohexyl group, and wherein A is a C1-C 10 The monoalkylated diamine can preferably be obtained by reaction of the diamine with acetone, methyl ethyl ketone, cyclohexanone, isophorone or an aliphatic aldehyde (such as acetaldehyde) and subsequent hydrogenation, or by reaction of the diamine with an alkyl halide. Thus, A can preferably be a cyclohexyl group, a sec-butyl group, a trimethylcyclohexyl group or an isopropyl group, which are derived from the respective ketones, aldehydes and alkyl halides.
[0060] In a preferred embodiment of structure (XI), the monoalkylated diamine is selected from the monoalkylated meta-xylenediamine represented by the following structure:
[0061]
[0062] Where A is C1-C 10 Alkyl; and
[0063] Monoalkylated 1,3-bisaminomethylcyclohexane represented by the following structure:
[0064]
[0065] Where A is C1-C 10 alkyl.
[0066] The epoxy resin system may comprise one or more epoxy resins. Preferably, the epoxy resin system comprises only one epoxy resin. Likewise, the epoxy resin system may comprise one or more compounds of formula (I). Preferably, the epoxy resin system comprises only one compound of formula (I).
[0067] In one embodiment, the epoxy resin system comprises 1 to 99 wt. % of the monoalkylated diamine, based on the total weight of the curing agent. Preferably, the epoxy resin system comprises at least 20 wt. %, more preferably at least 40 wt. %, even more preferably at least 60 wt. % and particularly preferably at least 80 wt. % of the monoalkylated diamine, based on the total weight of the curing agent.
[0068] Preferably, the epoxy resin system comprises 20-100 wt % of the monoalkylated diamine, 0-50 wt % of the non-alkylated diamine and 0-30 wt % of the dialkylated diamine, based on the total weight of the curing agent.
[0069] Another aspect of the present invention is a method for preparing an epoxy resin system, which method comprises combining an epoxy resin with a monoalkylated diamine of formula (I) and optionally other components,
[0070]
[0071] wherein Z is selected from cyclohexyl, C1-C4 alkyl-substituted cyclohexyl, phenyl, C1-C4 alkyl-substituted phenyl, methylenebis(cyclohexyl) and C1-C4 alkyl-substituted methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is C1-C 10 alkyl.
[0072] The weight ratio of the epoxy resin to the monoalkylated diamine is preferably 1:0.05-1:0.95. In another preferred embodiment, the weight ratio is 1:0.3-1:0.6.
[0073] The epoxy resin system may preferably further comprise a second amine. The second amine is selected from primary amines and secondary amines. The second amine preferably comprises one or more amine compounds selected from the following: polyetheramines, polyetherpolyamines, saturated aliphatic cyclic diamines, linear aliphatic amines, alicyclic amines, polyalicyclic amines and aromatic amines.
[0074] Preferably, the polyetheramine may have the following formula: H2NCH(CH3)CH2-[OCH2CH(CH3)] X NH2, and x is 2 to 70. Preferably, the second amine may comprise a mixture of 4,4'-methylenebiscyclohexylamine, isophoronediamine, 1,2-diaminocyclohexane, 4,4'-methylenebis(2-methylcyclohexylamine), 1,3-bisaminomethylcyclohexane and polyetheramine: H2NCH(CH3)CH2[OCH2CH(CH3)] 2.5 NH2.
[0075] Preferably, modified amine compounds such as Mannich bases, polyamide compounds, amine-epoxy adducts, and combinations thereof may be used as co-curing agents for use with the monoalkylated diamine compounds as described herein.
[0076] Preferably, the epoxy resin may include polyglycidyl ethers of compounds selected from aliphatic diols, alicyclic diols, triols, polyols, polyglycols, and combinations thereof. The epoxy resin system may further include polyacrylates or polymethacrylates of polyols.
[0077] Reference Figure 1, the viscosity distribution curve of the epoxy resin composition containing the non-alkylated product (IPD) at 40°C was compared with the viscosity distribution curve of the epoxy resin composition containing the mono-alkylated product. The time (minutes) of reactivity of the composition increased significantly with the alkylation chemistry.
[0078] The epoxy resin may consist of a single resin, or it may be a mixture of epoxy resins that are compatible with each other. The epoxy resin may include, but is not limited to, difunctional epoxy resins, such as bisphenol A and bisphenol F resins. Multifunctional epoxy resins as used herein describe compounds containing two or more 1,2-epoxy groups per molecule. This type of epoxy compound is well known to those skilled in the art and is described in the following literature: Y. Tanaka, "Synthesis and Characteristics of Epoxides", in Epoxy Resins Chemistry and Technology (Marcel Dekker, 1988), edited by CA May, which is incorporated herein by reference in its entirety.
[0079] One class of epoxy resins suitable for use is the glycidyl ethers of polyhydric phenols, including the glycidyl ethers of dihydric phenols. Preferred are the glycidyl ethers of resorcinol, hydroquinone, bis(4-hydroxy-3,5-difluorophenyl)-methane, 1,1-bis-(4-hydroxyphenyl)-ethane, 2,2-bis-(4-hydroxy-3-methylphenyl)-propane, 2,2-bis-(4-hydroxy-3,5-dichlorophenyl)-propane, 2,2-bis-(4-hydroxyphenyl)-propane (commercially known as bisphenol A), bis-(4-hydroxyphenyl)-methane (commercially known as bisphenol F, and which may contain varying amounts of 2-hydroxyphenyl isomers), and the like, or any combination thereof. Additionally, in the present disclosure, upgraded dihydric phenols of formula (XIV) are also preferred:
[0080]
[0081] wherein m is 0 to 25, and R is a divalent hydrocarbon radical of a dihydric phenol such as those listed above.
[0082] The material according to formula (XIV) can be prepared by polymerizing a mixture of a dihydric phenol and epichlorohydrin, or by advancing a mixture of a diglycidyl ether of a dihydric phenol and the dihydric phenol. Although in any given molecule, the value of m is an integer, the material is invariably a mixture that can be characterized by an average value of m, which is not necessarily an integer. In one aspect of the present disclosure, a polymer material having an average value of m between 0 and about 7 can be used. In other embodiments, the epoxy resin can be a polyglycidyl amine derived from one or more of 2,2'-methylenedianiline, 4,4'-methylenedianiline, meta-xylene diphenylamine, hydantoin, and isocyanate.
[0083] The epoxy resin may preferably be a cycloaliphatic (cycloaliphatic) epoxide. Particularly preferred cycloaliphatic epoxides are diepoxides of cycloaliphatic esters of dicarboxylic acids, in particular bis(3,4-epoxycyclohexylmethyl)oxalate, bis(3,4-epoxycyclohexylmethyl)adipate, bis(3,4-epoxycyclohexylmethyl)adipate, 3,4-Epoxy-6-methylcyclohexylmethyl)ester, vinylcyclohexene diepoxide; Olefin diepoxides; bis(3,4-epoxycyclohexylmethyl)pimelate; dicyclopentadiene diepoxide; and other suitable alicyclic epoxides. Other suitable diepoxides of alicyclic esters of dicarboxylic acids are described, for example, in patent application publication WO 2009 / 089145 A1, which is incorporated herein by reference in its entirety.
[0084] Other particularly preferred alicyclic epoxides are 3,3-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate; 3,3-epoxy-1-methylcyclohexanecarboxylate; 6-methyl-3,4-epoxycyclohexylmethyl 6-methyl-3,4-epoxycyclohexanecarboxylate; and 3,4-epoxy-2-methylcyclohexyl-methyl 3,4-epoxy-3-methylcyclohexanecarboxylate. Other suitable 3,4-epoxycyclohexanecarboxylate 3,4-epoxycyclohexylmethyl esters are described, for example, in U.S. Pat. No. 2,890,194, which is incorporated herein by reference in its entirety. In other embodiments, the epoxy resin may include a polyol polyglycidyl ether derived from polyethylene glycol, polypropylene glycol, or polytetrahydrofuran, or a combination thereof.
[0085] In another aspect, epoxy novolac resins as glycidyl ethers of novolac resins can be used as multifunctional epoxy resins according to the present disclosure. In yet another aspect, the at least one multifunctional epoxy resin is diglycidyl ether of bisphenol A (DGEBA), upgraded or higher molecular weight variants of DGEBA, diglycidyl ether of bisphenol F, epoxy novolac resins, or any combination thereof. Higher molecular weight variants or derivatives of DGEBA are prepared by an upgraded process, wherein excess DGEBA reacts with bisphenol A to produce epoxy-terminated products. The epoxide equivalent weight (EEW) of these products ranges from about 450 to 3000 or higher. Since these products are solid at room temperature, they are often referred to as solid epoxy resins.
[0086] DGEBA or upgraded DGEBA resins are often used in structural formulations due to their combination of low cost and high process performance properties. Commercial grades of DGEBA with an EEW ranging from about 174 to about 250 and more generally about 185 to about 195 are readily available. At these low molecular weights, the epoxy resin is a liquid and is often referred to as a liquid epoxy resin. It is understood by those skilled in the art that most grades of liquid epoxy resins are lightly polymerized because pure DGEBA has an EEW of 174. Resins with an EEW between 250 and 450, which are also typically prepared by the upgrading process, are referred to as semi-solid epoxy resins because they are a mixture of solid and liquid at room temperature. Multifunctional resins with an EEW of about 160 to about 750 based on solids are available in the present disclosure. On the other hand, the multifunctional epoxy resin has an EEW in the range of about 170 to about 250.
[0087] Depending on the end-use application, it may be beneficial to reduce the viscosity of the composition of the present disclosure by modifying the epoxy resin. The epoxy resin comprising at least one multifunctional epoxy resin may further comprise a monofunctional epoxide. Preferred examples of monoepoxides include, but are not limited to, styrene oxide, cyclohexene oxide, and glycidyl ethers of phenol, cresol, tert-butylphenol, other alkylphenols, butanol, 2-ethylhexanol, C4 to C 14 Alcohols and the like, or combinations thereof. The multifunctional epoxy resin may also be present in a solution or emulsion, wherein the diluent is water, an organic solvent, or a mixture thereof.
[0088] Curing agent
[0089] As described above, the curing agent is a monoalkylated diamine of formula (I). The curing agent may further comprise a second amine. The second amine may consist of a single amine or a mixture of amines. The amine in the second amine is a primary or secondary amine.
[0090] In some applications, the following are suitable as the second amine: polyether diamine, saturated aliphatic cyclic diamine, linear aliphatic amine, alicyclic diamine, polyalicyclic amine, aromatic amine and combinations thereof. The weight ratio of the epoxy resin to the monoalkylated diamine and the second amine is preferably 1:0.95:0.05. In another embodiment, the weight ratio is preferably 1:0.05:0.95. The polyamine can be preferably selected from one or more of the following: aliphatic polyamines, such as diethylenetriamine (DETA), triethylenetetramine (TETA), tetraethylenepentamine (TEPA), pentaethylenehexamine (PEHA), hexamethylenediamine (HMDA), N-(2-aminoethyl)-1,3-propylenediamine (N3-amine), N,N'-1,2-ethanediylbis-1,3-propylenediamine (N4-amine) or dipropylenetriamine; aromatic aliphatic polyamines, such as m-xylene diamine (mXDA) or p-xylene diamine; alicyclic polyamines, such as 1,3-bisaminomethylcyclohexane (1,3-BAC), isophoronediamine (IPDA), 4,4'-methylenebiscyclohexylamine (PACM), 1,2-diaminocyclohexane or 4,4'-methylenebis(2-methylcyclohexylamine); aromatic polyamines such as m-phenylenediamine, diaminodiphenylmethane (DDM) or diaminodiphenylsulfone (DDS); heterocyclic polyamines such as N-aminoethylpiperazine (NAEP) or 3,9-bis(3-aminopropyl)2,4,8,10-tetraoxaspiro(5,5)undecane; polyalkoxy polyamines, wherein the alkoxy groups may be oxyethylene, oxypropylene, oxy-1,2-butylene, oxy-1,4-butylene or copolymers thereof, such as 4,7-dioxadecane-1,10-diamine, 1-propylamine, 3,3'-(oxybis(2,1-ethanediyloxy))bis(diaminopropylated diethylene glycol) ( 1922A), poly(oxy(methyl-1,2-ethanediyl)), α-(2-aminomethylethyl)ω-(2-aminomethylethoxy) ( D 230, D-400), triethylene glycol diamine and oligomers ( XTJ-504, XTJ-512), poly(oxy(methyl-1,2-ethanediyl)), α,α'-(oxydi-2,1-ethanediyl)bis(ω-(aminomethylethoxy))( XTJ-511), bis(3-aminopropyl) polytetrahydrofuran 350, bis(3-aminopropyl) polytetrahydrofuran 750, poly(oxy(methyl-1,2-ethanediyl)), α-hydrogen-ω-(2-aminomethylethoxy) ether and 2-ethyl-2-(hydroxymethyl)-1,3-propanediol (3:1) ( T-403), and diaminopropyl dipropylene glycol. is a registered trademark of HuntsmanPetrochemical LLC.
[0091] Particularly suitable polyamines include isophoronediamine (IPD), 4,4'-methylenebiscyclohexylamine (PACM), 3,3'-dimethyl PACM ( 2049), N-aminoethylpiperazine (NAEP), 4,7-dioxadecane-1,10-diamine, 1-propylamine, 3,3'-(oxybis(2,1-ethanediyloxy))bis-( 1922A), poly(oxy(methyl-1,2-ethanediyl)),α-(2-aminomethylethyl)ω-(2-aminomethylethoxy))( D230, D-400), poly(propylene glycol) bis(2-aminopropyl ether), triethylene glycol diamine ( XTJ-504) and poly(oxy(methyl-1,2-ethanediyl))α,α'-(oxy(di-2,1-ethanediyl))bis(ω-(aminomethylethoxy))( XTJ-511) or a mixture thereof. is a registered trademark of EvonikDegussa GmbH.
[0092] Additional amines suitable for forming the second amine are polyamines comprising at least one or more polyfunctional amines of structure (XV).
[0093]
[0094] wherein R1 is CH2CH2CH2NH2; R2, R3 and R4 are independently H or CH2CH2CH2NH2; and X is CH2CH2 or CH2CH2CH2. In one embodiment, R2 and R3 are not H at the same time.
[0095] Optional additives
[0096] The epoxy system formulation for the composite material may optionally include additives such as, but not limited to, non-reactive plasticizer(s), filler(s), processing aid(s), stabilizers, degassing agents, viscosity modifier(s), UV absorbers, flame retardants and / or impact modifiers.
[0097] The optional acrylate or methacrylate ester of the polyol is blended with the epoxy resin in a weight ratio of 0 to up to about 100 parts of ester per 100 parts of epoxy resin. In another embodiment, the acrylate or methacrylate ester of the polyol is blended with the epoxy resin in a weight ratio of about 5 to about 100 parts of ester per 100 parts of epoxy resin.
[0098] Nanomaterials / fillers may be included. The term "nanomaterial" includes, but is not limited to, multi-walled carbon or boron nitride nanotubes, single-walled carbon, carbon or boron nitride nanoparticles, carbon or boron nitride nanofibers, carbon or boron nitride nanorope, carbon or boron nitride nanobelts, nanoclays; nanoclays containing small tubes; delaminated inorganic clay materials; talc; carbon black; cellulose fibers; silica; and alumina.
[0099] The epoxy resin system of the invention can preferably be prepared by a process for preparing an epoxy resin system, wherein an epoxy resin is combined with a monoalkylated diamine of the formula (I) and optionally further components:
[0100]
[0101] wherein Z is selected from cyclohexyl, C1-C4 alkyl-substituted cyclohexyl, phenyl, C1-C4 alkyl-substituted phenyl, methylenebis(cyclohexyl) and C1-C4 alkyl-substituted methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is C1-C 10 alkyl.
[0102] The curable epoxy resin compositions and cured products described herein can be used as structural and electrical laminates, coatings, castings, structural components (particularly for the aerospace industry), and as circuit boards and the like for the electronics industry, among other applications. The curable epoxy resin compositions disclosed herein can also be used in electrical varnishes, encapsulants, semiconductors, general molding powders, filament wound pipes and fittings, filament wound pressure vessels, low and high pressure pipes and fittings, low and high pressure vessels, storage tanks, wind turbine blades, automotive structural components, aerospace structural components, oil and gas buoyancy modules, drilling rigs, well plugs, cured in place pipe (CIPP), structural bonding adhesives and laminates, composite linings, pump linings, corrosion resistant coatings, and other suitable epoxy-containing products.
[0103] The curable epoxy resin composition can be used to form a composite material based on a reinforced fiber substrate. The reinforced fiber substrate may preferably be one or more layers of glass fiber material. Contacting the reinforced fiber substrate with the epoxy resin system may preferably include an application method selected from the following: manual lamination, infusion method, filament winding, pultrusion, resin transfer molding, fiber pre-impregnation method and combinations thereof.
[0104] Preferred fiber substrates include organic or inorganic fibers, natural fibers or synthetic fibers, and may be in the form of woven or non-crimp fabrics, nonwoven webs or mats, and in the form of fiber strands (rovings) or staple fibers formed from continuous or discontinuous fibers, such as glass fibers, carbon fibers, carbon nanotubes, nanocomposite fibers, polyaramid fibers, such as those sold under the trade name Those sold, poly(p-phenylenebenzobis(2- azole) fibers, such as those sold under the trade name Ultra-high molecular weight polyethylene fibers, such as those sold under the trade name Those sold are, high and low density polyethylene fibers, polypropylene fibers, nylon fibers, cellulose fibers, natural fibers, biodegradable fibers, and combinations thereof.
[0105] Preferably, these fibers (woven or non-woven) can be coated with a solvent or solvent-free epoxy resin mixture by standard impregnation methods, particularly for filament winding (FW), pultrusion, sheet molding compound, bulk molding compound autoclave molding, resin infusion, vacuum assisted resin transfer molding (VARTM), resin transfer molding (RTM), wet / hand layup, vacuum bagging, resin impregnation, prepreg processing, fiber impregnation, compression molding (CM), brushing, spraying or dipping, casting, injection molding, or combinations thereof.
[0106] The present disclosure also includes manufactured products, which include amine-epoxy compositions as described above. Such products may include, but are not limited to, adhesives, coatings, primers, sealants, curing compounds, building products, flooring products, composite products, laminates, potting compounds, grouts, fillers, cementitious grouts or self-leveling flooring materials. Additional components or additives may be used with the compositions of the present disclosure to prepare manufactured products. In addition, such coatings, primers, sealants, curing compounds or grouts may be applied to metal or cementitious substrates.
[0107] The invention also relates to the use of monoalkylated diamines of the formula (I) as hardeners for epoxy resins.
[0108]
[0109] wherein Z is selected from cyclohexyl, phenyl and methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is C1-C 10 Alkyl, or their preferred embodiments as described before. DETAILED DESCRIPTION
[0110] Example
[0111] Examples 1-9 are methods for synthesizing the curing agent of the present invention.
[0112] Example 1. Synthesis of sec-butylated isophorone diamine 0.5 / 1.0 molar ratio (MEK:IPD)
[0113] The synthesis of N-sec-butylisophorone diamine is a batch process. 990.3 g of isophorone diamine (5.815 mol) and 209.7 g of 2-butanone (2.908 mol) are fed into a 2-liter autoclave batch reactor along with 7.43 g of a 5% sulfided platinum catalyst on carbon. The reactor is sealed and subsequently purged with nitrogen and then hydrogen to remove any air from the reactor. The reactor is pressurized to 27.2 atm (400 psig) with hydrogen, and the reactor is heated to 120-140° C. When the rate of hydrogen absorption slows, the pressure is increased to 54.4 atm (800 psig). The hydrogenation process continues until the rate of hydrogen absorption drops below 0.0007 MPa / min (0.1 psi / min). The reactor is cooled to ambient temperature and decompressed, and the reaction product is filtered to remove the catalyst. Water is removed using a rotary evaporator operating at a vacuum of 30 mm Hg and a temperature of up to 100° C. The resulting reaction product was sec-butylated isophoronediamine having a composition as determined by gas chromatography shown in the table below and represented by the following structure. Alternatively, the same product was obtained via the same procedure as above using a 5% palladium on carbon catalyst with a small difference in conversion.
[0114] Example 2. Synthesis of sec-butylated isophorone diamine 1.0 / 1.0 molar ratio (MEK:IPD)
[0115] The synthesis of N-sec-butylisophorone diamine is a batch process. 843.0 g of isophorone diamine (4.950 mol) and 357.0 g of 2-butanone (4.950 mol) are fed into a 2-liter autoclave batch reactor along with 6.32 g of a 5% sulfided platinum catalyst on carbon. The reactor is sealed and subsequently purged with nitrogen and then hydrogen to remove any air from the reactor. The reactor is pressurized to 27.2 atm (400 psig) with hydrogen and the reactor is heated to 120-140° C. When the rate of hydrogen absorption slows, the pressure is increased to 54.4 atm (800 psig). The hydrogenation process continues until the rate of hydrogen absorption drops below 0.0007 MPa / min (0.1 psi / min). The reactor is cooled to ambient temperature and decompressed, and the reaction product is filtered to remove the catalyst. Water is removed using a rotary evaporator operating at a vacuum of 30 mm Hg and a temperature of up to 100° C. The resulting reaction product is sec-butylated isophorone diamine having a composition determined by gas chromatography shown in the table below and represented by the following structure. Alternatively, the same product was obtained via the same procedure as above using a 5% palladium on carbon catalyst with a small difference in conversion. For this case, NMR spectroscopy analysis of the product was performed and the ratio of major monoalkylated IPD to minor monoalkylated IPD was 80:20, while the selectivity of the total monoalkylated IPD was about 90%.
[0116]
[0117] Composition of the product:
[0118]
[0119] Example 3. Synthesis of cyclohexylated isophorone diamine 0.5 / 1.0 molar ratio (CHONE:IPD)
[0120] The synthesis of N-cyclohexylisophorone diamine is a batch process. 465.8 g of isophorone diamine (2.74 mol) and 134.2 g of cyclohexanone (1.37 mol) are fed into a 1 liter autoclave batch reactor along with 7.0 g of a 5% sulfided platinum catalyst on carbon. The reactor is sealed and subsequently purged with nitrogen and then hydrogen to remove any air from the reactor. The reactor is pressurized to 27.2 atm (400 psig) with hydrogen, and the reactor is heated to 120° C. When the rate of hydrogen absorption slows, the pressure is increased to 54.4 atm (800 psig). The hydrogenation process continues until the rate of hydrogen absorption drops below 0.0007 MPa / min (0.1 psi / min). The reactor is cooled to ambient temperature and decompressed, and the reaction product is filtered to remove the catalyst. Water is removed using a rotary evaporator operating at a vacuum of 30 mm Hg and a temperature of up to 100° C. The resulting reaction product was cyclohexylated isophoronediamine having the composition determined by gas chromatography shown in the table below.
[0121] Example 4. Synthesis of Cyclohexylated Isophorone Diamine 1.0 / 1.0 Molar Ratio (CHONE:IPD)
[0122] The synthesis of N-cyclohexylisophorone diamine is a batch process. 348.9 g of isophorone diamine (2.05 mol) and 201.1 g of cyclohexanone (2.05 mol) are fed into a 1 liter autoclave batch reactor along with 5.2 g of a 5% palladium on carbon catalyst. The reactor is sealed and subsequently purged with nitrogen and then hydrogen to remove any air from the reactor. The reactor is pressurized to 27.2 atm (400 psig) with hydrogen, and the reactor is heated to 120° C. When the rate of hydrogen absorption slows, the pressure is increased to 54.4 atm (800 psig). The hydrogenation process continues until the rate of hydrogen absorption drops below 0.0007 MPa / min (0.1 psi / min). The reactor is cooled to ambient temperature and decompressed, and the reaction product is filtered to remove the catalyst. Water is removed using a rotary evaporator operating at a vacuum of 30 mm Hg and a temperature of up to 100° C. The resulting reaction product was cyclohexylated isophoronediamine having the composition determined by gas chromatography shown in the table below.
[0123] Composition of the product:
[0124]
[0125] Example 5. Synthesis of trimethylcyclohexylated isophorone diamine 0.5 / 1.0 molar ratio (isophorone: IPD)
[0126] The synthesis of N-trimethylcyclohexylisophoronediamine is a batch process. 170.8 g of isophoronediamine (1.00 mol) and 69.2 g of isophorone (0.50 mol) are combined with 240 g of tetrahydrofuran and charged into a 1 liter autoclave batch reactor together with 7.2 g of 5% palladium on carbon catalyst. The reactor is sealed and then purged with nitrogen and then hydrogen to remove any air from the reactor. The reactor is pressurized to 27.2 atm (400 psig) with hydrogen, and the reactor is heated to 160° C. When the rate of hydrogen absorption slows, the pressure is increased to 54.4 atm (800 psig). The hydrogenation process continues until the rate of hydrogen absorption drops below 0.0007 MPa / min (0.1 psi / min). The reactor is cooled to ambient temperature and depressurized, and the reaction product is filtered to remove the catalyst. Water and tetrahydrofuran were removed using a rotary evaporator operating at vacuum as low as 30 mm Hg and temperatures up to 100° C. The resulting reaction product was trimethylcyclohexylated isophoronediamine having the composition as determined by gas chromatography shown in the table below.
[0127] Example 6. Synthesis of trimethylcyclohexylated isophorone diamine 1.0 / 1.0 molar ratio (isophorone: IPD)
[0128] The synthesis of N-trimethylcyclohexylisophoronediamine is a batch process. 132.5 g of isophoronediamine (0.78 mol) and 107.5 g of isophorone (0.78 mol) are combined with 240 g of tetrahydrofuran and charged into a 1 liter autoclave batch reactor along with 3.6 g of 5% palladium on carbon catalyst. The reactor is sealed and subsequently purged with nitrogen and then hydrogen to remove any air from the reactor. The reactor is pressurized to 27.2 atm (400 psig) with hydrogen, and the reactor is heated to 160° C. When the rate of hydrogen absorption slows, the pressure is increased to 54.4 atm (800 psig). The hydrogenation process continues until the rate of hydrogen absorption drops below 0.0007 MPa / min (0.1 psi / min). The reactor is cooled to ambient temperature and depressurized, and the reaction product is filtered to remove the catalyst. Water and tetrahydrofuran were removed using a rotary evaporator operating at vacuum as low as 30 mm Hg and temperatures up to 100° C. The resulting reaction product was trimethylcyclohexylated isophoronediamine having the composition as determined by gas chromatography shown in the table below.
[0129] Product composition:
[0130]
[0131] Example 7. Synthesis of sec-butylated 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane 1.0 / 1.0 molar ratio (MEK:DMPACM)
[0132] The synthesis of N-sec-butyl 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane is a batch process. 460.7 g of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane (1.93 mol) and 139.3 g of 2-butanone (1.93 mol) were charged to a 1 liter autoclave batch reactor along with 3.46 g of 5% sulfided platinum on carbon catalyst. The reactor was sealed and subsequently purged with nitrogen and then hydrogen to remove any air from the reactor. The reactor was pressurized to 34.0 atm (500 psig) with hydrogen, and the reactor was heated to 160° C. When the rate of hydrogen absorption slowed, the pressure was increased to 54.4 atm (800 psig). The hydrogenation process continued until the rate of hydrogen absorption dropped below 0.0007 MPa / min (0.1 psi / min). The reactor was cooled to ambient temperature and depressurized, and the reaction product was filtered to remove the catalyst. Water was removed using a rotary evaporator operating at 40 mm Hg vacuum and temperatures up to 100° C. The resulting reaction product was sec-butylated 3,3′-dimethyl-4,4′-diaminodicyclohexylmethane having the composition as determined by gas chromatography shown in the table below and represented by the structure below.
[0133]
[0134] Product composition:
[0135]
[0136] Example 8. Synthesis of sec-butylated meta-xylene diamine 1.0 / 1.0 molar ratio (MEK:MXDA)
[0137] The synthesis of N-sec-butyl-m-xylenediamine is a batch process. 392.3 g of m-xylenediamine (2.88 mol) and 207.7 g of 2-butanone (2.88 mol) are fed into a 1-liter autoclave batch reactor together with 2.94 g of a 5% sulfided platinum catalyst on carbon. The reactor is sealed and subsequently purged with nitrogen and then hydrogen to remove any air from the reactor. The reactor is pressurized to 34.0 atm (500 psig) with hydrogen, and the reactor is heated to 120° C. When the rate of hydrogen absorption slows, the pressure is increased to 54.4 atm (800 psig). The hydrogenation process continues until the rate of hydrogen absorption drops below 0.0007 MPa / min (0.1 psi / min). The reactor is cooled to ambient temperature and decompressed, and the reaction product is filtered to remove the catalyst. Water is removed using a rotary evaporator operated at a 40 mm Hg vacuum and up to 100° C. temperature. The resulting reaction product was sec-butylated meta-xylenediamine having a composition measured by gas chromatography shown in the following table and represented by the following structure.
[0138]
[0139] Composition of the product:
[0140]
[0141] Example 9. Synthesis of sec-butylated 4,4'-diaminodicyclohexylmethane 1.0 / 1.0 molar ratio (MEK:PACM)
[0142] The synthesis of N-sec-butyl 4,4'-diaminodicyclohexylmethane is a batch process. 446.6 g of 4,4'-diaminodicyclohexylmethane (2.13 mol) and 153.4 g of 2-butanone (2.13 mol) were charged to a 1 liter autoclave batch reactor along with 3.40 g of 5% sulfided platinum on carbon catalyst. The reactor was sealed and subsequently purged with nitrogen and then hydrogen to remove any air from the reactor. The reactor was pressurized to 27.2 atm (400 psig) with hydrogen, and the reactor was heated to 140°C. When the rate of hydrogen absorption slowed, the pressure was increased to 54.4 atm (800 psig). The hydrogenation process continued until the rate of hydrogen absorption dropped below 0.0007 MPa / min (0.1 psi / min). The reactor was cooled to ambient temperature and depressurized, and the reaction product was filtered to remove the catalyst. Water was removed using a rotary evaporator operating at 40 mm Hg vacuum and temperatures up to 100° C. The resulting reaction product was sec-butylated 4,4′-diaminodicyclohexylmethane having the composition as determined by gas chromatography shown in the table below and represented by the structure below.
[0143]
[0144] Product composition:
[0145]
[0146] These examples are provided to demonstrate certain aspects of the invention, and they are not intended to limit the scope of the claims appended hereto.
[0147] Example 10. This example describes the preparation of an alkylated IPD curing agent and its testing with epoxy resin.
[0148] Table 1
[0149]
[0150] A comparison between commercial cycloaliphatic amines such as IPD (Formulation 1) and the mono- and di-alkylated products of the present invention (Formulations 2-4) is reported in Table 1. The viscosity of the alkylated isophorone diamine (AIPD) product itself remains very low. It is desirable for the curing agent to have a low viscosity, which helps to reduce the overall epoxy formulation viscosity for composite applications. At 25°C, the gel time of the alkylated isophorone diamine (AIPD) product doubles with an IPD:MEK ratio of (1:0.5) and increases almost five times with an IPD:MEK ratio of (1:1). This is sufficient time and viscosity for uniformly processing larger and thicker composite parts.
[0151] The reactivity of the alkylated isophorone diamine (AIPD) product with epoxy resins maintains physical, thermal and chemical properties that are ideal for composite applications.
[0152] The curing agent was used for mixing with epoxy resin (epoxy equivalent weight (EEW) 180) at varying stoichiometric ratios as shown in Table 1. Liquid Epoxy Resin (LER) (EEW 180) 826 was used as the epoxy resin. is a registered trademark of Hexion Specialty Chemicals, Inc.
[0153] The viscosity of all formulations shown in Table 1 was measured at 25°C and 40°C using a Brookfield Viscometer RV with spindle number 27. 12 grams of the epoxy resin composition was used to measure the viscosity.
[0154] use The gel timer measures the gel time of all formulations shown in Table 1. Sometimes, in the industry, gel time is also equated with pot life. The epoxy resin and curing agent were preheated separately at 25°C. A total of 150 grams of the mixture (epoxy resin and curing agent) were mixed for 3-5 minutes. The 1" diameter disc was immersed in the beaker content mixture and the gel timer was immediately turned on to obtain an accurate reading.
[0155] The results for Formulations 1-4 are reported in Table 1. According to the present disclosure, Formulation 1 was used as a control sample and provided an initial mixed viscosity of about 319 cP. Formulations 2 and 3 produced initial mixed viscosities of about 313 cP and 206 cP, respectively. The lower mixed viscosity enhanced fiber wetting in thick composite sections under pressure due to improved resin penetration between the fabric layers. Formulation 1 provided a T in the range of 140°C-155°C. g , and Formulations 2 and 3 provided T in the range of 130°C-150°C g The alkylated isophorone diamine (AIPD) maintains the T g range, while improving the gel time by 2-5 times that of the control formulation (IPD).
[0156] Table 2
[0157]
[0158] The processing performance results of IPD alkylated with CHONE and isophorone at two different ratios are reported in Table 2 (Formulations 5-8). The viscosity of the alkylated product itself remains very low. It is desirable that the curing agent has a low viscosity, which helps to reduce the overall epoxy formulation viscosity for composite applications. The reactivity of the two alkylated products is significantly slowed. This feature provides sufficient time and viscosity for uniform processing of larger and thicker composite parts.
[0159] Embodiment 11
[0160] This example describes the testing of cured epoxy resin formulations
[0161] Table 3
[0162] Formulations 1 2 3 4 performance IPD IPD:MEK (1:0.5) IPD:MEK (1:1) Dialkylated IPD LER EEW-180 100 100 100 100 Curing agent Phr 24 30 39 74 Tensile Strength (psi) 8,489 6,910 7,738 Uncured Tensile modulus(ksi) 441 465 474 Uncured % Elongation at break 2.8 1.7 1.9 Uncured Flexural Strength (psi) 15,556 17,595 14,965 Uncured Flexural modulus(ksi) 345 383 397 Uncured Compression strength (psi) 15,167 13,568 11,107 Uncured Compression modulus (psi) 251 296 267 Uncured
[0163] The epoxy resin and amine curing agent shown in Table 3 were mixed manually at 40°C for 3-5 minutes. Entrained air was removed by placing the mixture in a centrifuge for 5 minutes or until the mixture was clarified. The mixture was then poured into a 1 / 8" aluminum mold. The system in the mold was cured at 60°C for 1 hour and at 150°C for 2 hours. The mold was allowed to cool to room temperature, after which the cured sample was taken out. Specimens were prepared from the cast samples according to ASTM methods for mechanical testing: tensile test (ASTM D638), flexural test (ASTM D790), and compression test (ASTM D695). Additional 1"×3"×1 / 8" samples were prepared for chemical resistance testing in different reagents (Table 4).
[0164] Example 12
[0165] This example describes the testing of a cured epoxy resin formulation after chemical impregnation.
[0166] Table 4
[0167]
[0168] *NP – Not Conducted
[0169] Neat cast panels of Formulations 1-3 were prepared using the method described in Example 11. Flexural specimens (1 / 2" x 3" x 1 / 8") were machined according to ASTM D790. The specimens were immersed in different reagents at 40°C for 30 days to understand the retention of flexural modulus before and after immersion. The reagents used were: DI water, methanol, 10% ammonium hydroxide, and 10% nitric acid. The flexural modulus of Formulations 2 and 3 was maintained in most of the reagents.
[0170] Embodiment 13
[0171] This example describes the processing and thermal properties of the alkylation products of various cycloaliphatic amines.
[0172] Table 5
[0173]
[0174] Comparisons between commercial amines such as IPD, MXDA, PACM and DMPACM (Formulations 1, 9, 11, 13) and the monoalkylated products of the present invention (Formulations 3, 10, 12, 14) are reported in Table 5. The viscosity of the alkylated products themselves remains very low. It is desirable for the curing agent to have a low viscosity, which helps to reduce the overall epoxy formulation viscosity for composite applications. The gel time of the alkylated products (Formulations 3, 10, 12 and 14) increases almost five times at 25°C. This is sufficient time and viscosity for uniform processing of larger and thicker composite parts.
Claims
1. An epoxy resin system comprising an epoxy resin and a monoalkylated diamine, wherein the monoalkylated diamine is selected from the monoalkylated isophorone diamine represented by the following structure: (III) Where A is C1-C 10 alkyl.
2. The epoxy resin system of claim 1, wherein the epoxy resin system comprises at least 20 wt% of the monoalkylated diamine, based on the total weight of the curing agent for the epoxy resin.
3. The epoxy resin system of claim 1 or 2, wherein the epoxy resin system further comprises a second amine selected from the group consisting of a primary amine and a secondary amine.
4. The epoxy resin system of claim 3, wherein the second amine component comprises one or more amine compounds selected from the group consisting of polyetheramines, polyetherpolyamines, saturated aliphatic cyclic diamines, linear aliphatic amines, alicyclic amines, polyalicyclic amines, and aromatic amines.
5. The epoxy resin system of claim 1 or 2, wherein the epoxy resin component comprises at least one glycidyl ether selected from the group consisting of glycidyl ethers of resorcinol, hydroquinone, bis-(4-hydroxy-3,5-difluorophenyl)-methane, 1,1-bis-(4-hydroxyphenyl)-ethane, 2,2-bis-(4-hydroxy-3-methylphenyl)-propane, 2,2-bis-(4-hydroxy-3,5-dichlorophenyl)-propane, 2,2-bis-(4-hydroxyphenyl)-propane, bis-(4-hydroxyphenyl)-methane, and any combination thereof.
6. The epoxy resin system of claim 1 or 2, wherein the epoxy resin component comprises at least one dihydric phenol of the following structure: (XIV) wherein m is 0 to 25, and R is a divalent hydrocarbon group.
7. The epoxy resin system of claim 1 or 2, wherein the epoxy resin component comprises at least one selected from the following group of substances: bis(3,4-epoxycyclohexylmethyl)oxalate, bis(3,4-epoxycyclohexylmethyl)adipate, bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, vinylcyclohexene diepoxide; Alkene diepoxide; bis(3,4-epoxycyclohexylmethyl)pimelate; dicyclopentadiene diepoxide; 3,3-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, 3,4-epoxycyclohexanecarboxylate; 3,3-epoxy-1-methylcyclohexanecarboxylate; 6-methyl-3,4-epoxycyclohexylmethyl 6-methyl-3,4-epoxycyclohexanecarboxylate; 3,4-epoxy-2-methylcyclohexyl-methyl 3,4-epoxy-3-methylcyclohexanecarboxylate, and combinations thereof.
8. A process for preparing an epoxy resin system according to any one of claims 1 to 7, wherein an epoxy resin is combined with a monoalkylated diamine as defined in any one of claims 1 to 7 and optionally further components.
9. Use of the epoxy resin system according to any one of claims 1 to 7 for the preparation of structural or electrical laminates, coatings, castings, structural components, circuit boards, electrical varnishes, encapsulants, semiconductors, general molding powders, filament wound pipes and fittings, filament wound pressure vessels, low and high pressure pipes and fittings, low and high pressure vessels, storage tanks, wind turbine blades, automotive structural components, aerospace structural components, oil and gas buoyancy modules, drilling rigs, well plugs, cured in place pipe (CIPP), structural bonding adhesives and laminates, composite linings, pump linings, corrosion resistant coatings or composite materials based on reinforced fiber matrix.
10. Use of a monoalkylated isophoronediamine represented by the following structure as a hardener for epoxy resins: (III) Where A is C1-C 10 alkyl.
Citation Information
Patent Citations
Compositions of epoxides and polycarboxylic acid compounds
US2890194A
Nitrogen containing compounds and compositions
US4293682A
Secondary aliphatic diamines as curing agents for polyurethanes and polyureas prepared using high-pressure impingement mixing
US6403752B1
Preparation of secondary amines
US7074963B2