Heater and image forming device

By using thermistors of lead-free manganese, cobalt, copper and nickel materials such as lead-free, combined with an appropriate amount of ruthenium, the problem of lead pollution is solved, and a heater and image forming device with environmental protection and high-precision temperature control is realized. .

CN111436166BActive Publication Date: 2024-11-22TOSHIBA LIGHTING & TECHNOLOGY CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910794206.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-01-11
Filing Date
2019-08-27
Publication Date
2024-11-22
Estimated Expiration
2039-11-26

AI Technical Summary

Technical Problem

The lead component thermistor in existing heaters causes pollution to the environment, and it is necessary to design an environmentally friendly heater and image forming device.

Method used

Design a heater whose thermistor does not contain lead, uses materials such as manganese, cobalt, copper and nickel, and has a total mass content of between 50% and 70%, and contains 2% to 15% ruthenium for 高精度温度探测和控制。

Benefits of technology

It realizes an environmentally friendly heater and image forming device, which can detect and control temperature with high accuracy, avoid lead contamination, and ensure efficient operation of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111436166B_ABST
    Figure CN111436166B_ABST
Patent Text Reader

Abstract

The present invention provides an environmentally friendly heater and an image forming device. The heater includes a substrate, a resistive heating element, and a thermistor. The substrate has a first surface and a second surface opposite to the first surface. The resistive heating element is disposed on the first surface. The thermistor is disposed on the second surface and does not contain lead.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present invention relate to a heater and an image forming apparatus. Background Art

[0002] For example, a heater is known that is used for toner fixing in a copier or fax machine, printing elimination in a rewritable card reader, etc. The heater generates heat from a resistive heating element formed on one side of a substrate by power supplied from a power supply electrode. In addition, a thermistor is disposed on the other side of the substrate. The power supply is controlled based on the temperature detected by the thermistor, so that the heater is adjusted to an appropriate temperature.

[0003] [Prior art literature]

[0004] [Patent Document]

[0005] Patent Document 1: Japanese Patent Application Publication No. 2003-240647 Summary of the invention

[0006] [Problems to be solved by the invention]

[0007] In such a heater, lead is contained as a component constituting the thermistor, and therefore, an environmentally friendly thermistor design is required.

[0008] An object of the present invention is to provide an environmentally friendly heater and an image forming apparatus.

[0009] [Technical means to solve the problem]

[0010] The heater of the embodiment includes a substrate, a resistance heating element, and a thermistor. The substrate has a first surface and a second surface located opposite to the first surface. The resistance heating element is arranged on the first surface. The thermistor is arranged on the second surface and does not contain lead.

[0011] In the heater, the thermistor contains manganese, cobalt, and one or both of copper and nickel. Moreover, the mass contents of the manganese, cobalt, copper and nickel in the thermistor are in this order from large to small. Moreover, the mass contents of the manganese and cobalt in the thermistor are greater than the mass contents of other components. Moreover, the total mass contents of the manganese, cobalt, copper and nickel in the thermistor is greater than 50 [mass %] and less than 70 [mass %]. Moreover, the thermistor contains ruthenium in an amount of greater than 2 [mass %] and less than 15 [mass %].

[0012] An image forming apparatus according to another embodiment includes the heater for heating a medium and a pressure roller for pressing the medium heated by the heater, and the toner image attached to the medium is fixed by the heater and the pressure roller.

[0013] [Effects of the Invention]

[0014] According to the present invention, an environmentally friendly heater and an image forming apparatus can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a plan view showing the heater according to the embodiment from the first surface side of the substrate.

[0016] Figure 2 This is a plan view showing the heater according to the embodiment from the second surface side of the substrate.

[0017] Figure 3 It is a graph showing the results of the peel test of the thermistor.

[0018] Figure 4 This is a graph showing the relationship between the content [mass %] of ruthenium contained in the thermistor and the sheet resistance value [kg / □].

[0019] Figure 5 This is a cross-sectional view showing a fixing device according to an embodiment using the heater according to the embodiment.

[0020] Figure 6 This is a cross-sectional view showing an image forming apparatus according to an embodiment using the heater according to the embodiment.

[0021] [Explanation of Symbols]

[0022] 1: Heater

[0023] 11: Substrate

[0024] 12: Resistance heating element

[0025] 13: First conductor

[0026] 14: Power supply electrode

[0027] 15, 18: Coating layer

[0028] 16: Thermistor

[0029] 17: Second conductor DETAILED DESCRIPTION

[0030] The heater 1 of the embodiment described below includes a substrate 11, a resistance heating element 12, and a thermistor 16. The substrate 11 has a first surface 11a and a second surface 11b located opposite to the first surface 11a. The resistance heating element 12 is arranged on the first surface 11a. The thermistor 16 is arranged on the second surface 11b and does not contain lead.

[0031] Furthermore, the thermistor 16 of the embodiment described below contains manganese, cobalt, and one or both of copper and nickel.

[0032] Furthermore, in the thermistor 16 of the embodiment described below, the mass contents of one or both of the manganese, the cobalt, the copper, and the nickel are arranged in this order from large to small.

[0033] Furthermore, the mass contents of the manganese and the cobalt in the thermistor 16 of the embodiment described below are larger than the mass contents of other components.

[0034] In addition, the total mass content of the manganese, the cobalt, the copper, and the nickel in the thermistor 16 of the embodiment described below is 50 [mass %] or more and 70 [mass %] or less.

[0035] Furthermore, the thermistor 16 of the embodiment described below contains 2 [mass %] or more and 15 [mass %] or less of ruthenium.

[0036] Moreover, the copier 100 as an image forming device of the embodiment described below includes the heater 1 for heating the medium; and the pressure roller 203 for pressurizing the medium heated by the heater, and the toner image attached to the medium is fixed by the heater 1 and the pressure roller 203.

[0037] [Implementation Method]

[0038] A heater according to an embodiment will be described with reference to the drawings. Figure 1 This is a plan view showing the heater according to the embodiment from the first surface side of the substrate. Figure 2 1 is a plan view showing the heater of the embodiment from the second surface side of the substrate. Figure 1 , Figure 2 In order to facilitate the understanding of the description, a three-dimensional orthogonal coordinate system including the Z axis is shown in the figure, in which the first surface side of the substrate is set as the positive direction and the second surface side is set as the negative direction.

[0039] The heater 1 of the embodiment is mounted on electronic equipment and mainly heats a medium such as paper passing through. Figure 1 As shown in FIG. 1 , the heater 1 includes a substrate 11, a resistance heating element 12, a first conductor 13, a power supply electrode 14, and a coating layer 15. Figure 2 As shown, the heater 1 includes a plurality of thermistors 16 , a second conductor 17 , and a coating layer 18 .

[0040] The substrate 11 has heat resistance and insulation properties, and in the present embodiment, is formed into a long rectangular shape. The substrate 11 is, for example, a flat plate containing ceramics such as aluminum oxide or aluminum nitride, glass ceramics, or a heat-resistant composite material. The substrate 11 has a thickness corresponding to the space in which the heater 1 can be installed, for example, about 0.5 [mm] to about 1.0 [mm]. Moreover, the shape of the substrate 11 is not limited to this as long as it has a length direction (X-axis direction) and a width direction (Y-axis direction) intersecting the length direction, and a concave portion, a convex portion, a notch, etc. can also be formed on the periphery.

[0041] The resistance heating element 12 is electrically connected to the first conductor 13, and is arranged on the first surface 11a in the thickness direction (Z-axis direction) of the substrate 11. The resistance heating element 12 generates heat by being energized. The resistance heating element 12 is, for example, a heating element pattern formed by a heating element paste of a silver-palladium system, a graphite system, a ruthenium oxide system, or the like. In the present embodiment, the resistance heating element 12 is arranged along the X-axis direction. The resistance heating element 12a and the resistance heating element 12b included in the resistance heating element 12 are arranged separately in the Y-axis direction. The resistance heating elements 12a and the resistance heating elements 12b are respectively arranged in strips along the length direction in a manner such that the length in the width direction of the heater 1 is fixed.

[0042] The first conductor 13 supplies power to the resistive heating element 12, and is disposed on the first surface 11a of the substrate 11. The first conductor 13 is, for example, a conductor pattern formed on the first surface 11a using a conductor paste such as a silver (Ag) system. The first conductor 13 in the present embodiment is electrically connected to the resistive heating element 12 in the X-axis direction, which is the length direction of the heater 1 (substrate 11). The conductor 13a and the conductor 13b included in the first conductor 13 are separated from the conductor 13c in the X-axis direction, and the resistive heating element 12a and the resistive heating element 12b are respectively arranged between them. The conductor 13a is formed along the length direction of the resistive heating element 12a, and the end on one side is electrically connected to the electrode 14a, and the end on the other side is electrically connected to the end on one side of the resistive heating element 12a. The conductor 13b is formed along the length direction of the resistive heating element 12b, and the end on one side is electrically connected to the electrode 14b, and the end on the other side is electrically connected to the end on one side of the resistive heating element 12b. The conductor 13 c is electrically connected to the other ends of the resistance heating element 12 a and the resistance heating element 12 b , respectively. That is, the first conductor 13 is electrically connected along the longitudinal direction of the resistance heating element 12 .

[0043] The power supply electrode 14 is electrically connected to the first conductor 13 and is disposed on the first surface 11a of the substrate 11. Figure 1 As shown, the pair of electrodes 14a and 14b included in the power supply electrode 14 are arranged at the end of the substrate 11 in the X-axis direction. The pair of electrodes 14a and 14b are electrically connected to the conductors 13a and 13b, respectively, and are electrically connected to the conductors 13a and 13b. Figure 1 In the embodiment, a pair of electrodes 14a and 14b are arranged at the end of one side of the substrate 11, but the pair of electrodes 14a and 14b may be arranged at both ends, or at the end of the other side. Furthermore, a pair of electrodes 14a and 14b are usually formed integrally with the conductors 13a and 13b on the first surface 11a of the substrate 11, respectively, but a pair of electrodes 14a and 14b may be formed separately from the conductors 13a and 13b, respectively. Furthermore, a pair of electrodes 14a and 14b are arranged on the first surface 11a of the substrate 11 on which the conductors 13a and 13b are arranged, but the pair of electrodes 14a and 14b may be arranged on the second surface 11b on the opposite side of the surface on which the conductors 13a and 13b are arranged. In this case, the pair of electrodes 14a and 14b are electrically connected to the conductors 13a and 13b, respectively, via through holes formed in the substrate 11.

[0044] The coating layer 15 is a protective layer that covers the resistive heating element 12 and the first conductor 13 disposed on the first surface 11a of the substrate 11. In the present embodiment, the coating layer 15 is formed in a strip shape. The coating layer 15 is as follows: by covering the resistive heating element 12 and the first conductor 13, the resistive heating element 12 and the first conductor 13 are prevented from being directly exposed to the atmosphere, and the resistive heating element 12 and the first conductor 13 are inhibited from being damaged or broken due to external interference (e.g., mechanical interference, chemical interference, electrical interference).

[0045] The thermistor 16 is a temperature detection element for detecting the temperature of the substrate 11. Figure 2 As shown, the thermistor 16 is arranged at multiple positions of the second surface 11b of the substrate 11 in the length direction of the substrate 11. That is, the thermistor 16 is arranged at the center and both end sides of the substrate 11 in the length direction of the substrate 11. In this way, in the heater 1, the temperatures of multiple positions in the length direction of the substrate 11 are detected respectively by multiple thermistors 16. The thermistor 16 is a printed thermistor directly arranged on the second surface 11b of the substrate 11. Therefore, compared with the so-called chip thermistor, the temperature perception is fast and has excellent temperature control responsiveness. Moreover, the thermistor 16 has a high degree of freedom in size or configuration compared with the chip thermistor. Moreover, the specific characteristics or composition of the thermistor 16 will be described later.

[0046] The second conductor 17 is a strip-shaped thermistor conductor serving as a plurality of conductors for supplying power to the plurality of thermistors 16, respectively. Figure 2As shown, the second conductor 17 has a connection portion 17a connected to the thermistor 16, a linear conductive portion 17b extending along the length direction (X-axis direction) of the substrate 11, and an electrode portion 17c connected to a terminal member (not shown) for supplying power. Furthermore, the second conductor 17 electrically connects the thermistors 16 to each other.

[0047] The connecting portion 17a has a portion extending in the width direction (Y-axis direction) of the substrate 11, and is connected to one end of the conductive portion 17b. By extending the connecting portion 17a in this way, the position of the conductive portion 17b relative to the width direction of the substrate 11 is adjusted. The conductive portion 17b extends along the length direction (X-axis direction) of the substrate 11 to the end of the substrate 11. A plurality of conductive portions 17b are arranged at intervals in the width direction of the substrate 11.

[0048] The electrode portion 17c is formed at the other end of the conductive portion 17b extending to the end in the longitudinal direction (X-axis direction) of the substrate 11. The electrode portion 17c is arranged at intervals in the longitudinal direction of the substrate 11 at the end in the longitudinal direction of the substrate 11. The electrode portion 17c is connected to a terminal member (not shown) connected to a power supply unit (not shown) of an electronic device such as an image forming apparatus, thereby supplying power to the thermistor 16 via the terminal member.

[0049] The coating layer 18 is a protective layer that covers the thermistor 16 and the second conductor 17 provided on the second surface 11b of the substrate 11. The material of the coating layer 18 can be the same as that of the coating layer 15. In the present embodiment, the coating layer 18 is formed in a strip shape so as to cover the entire width direction (Y-axis direction) of the substrate 11. In addition, both ends of the second conductor 17 in the length direction (X-axis direction) of the substrate 11 where the coating layer 18 is not provided are electrode portions 17c.

[0050] The number and arrangement of the resistance heating element 12 or thermistor 16 of the heater 1, and the structures of the first conductor 13, the second conductor 17, etc. are not limited to the following. Figure 1 , Figure 2 The structure shown in FIG. 1 may be changed according to the application or performance of the heater 1 .

[0051] In the heater 1 of the embodiment, the sheet resistance value of the thermistor 16 disposed on the second surface 11b of the substrate 11 can be set to 100 [kΩ / □] to 10000 [kΩ / □]. The resistance value of the thermistor 16 is usually a high value above the [kΩ / □] level, but if it is set to the range of the sheet resistance value, for example, the measurement accuracy of the resistance value can be measured without affecting the measurement, and the thermistor performance is good. In addition, the B constant of the thermistor 16 can be set to less than -2700 [K]. Here, the "B constant" is a physical property value indicating the sensitivity of the thermistor 16 relative to temperature changes. Since the thermistor 16 has such a physical property value, the temperature of the substrate 11 can be detected with high accuracy.

[0052] Moreover, the thermistor 16 of the embodiment does not contain lead (Pb). Therefore, a heater 1 including the thermistor 16 that takes environmental considerations into account can be provided. Here, the so-called "does not contain lead" means that the thermistor 16 arranged on the second surface 11b is cut in the thickness direction of the substrate 11, and the lead content measured by the electron probe micro analyzer (Electron Probe Micro Analyzer, EPMA) JXA-8200 (manufactured by JEOL Ltd.) is below the detection limit. Moreover, the content and mass content of each component in the thermistor 16 described later can also be measured in the same way as the lead content.

[0053] The thermistor 16 of the embodiment contains manganese, cobalt, and one or both of copper and nickel, and does not contain lead. Therefore, the heater 1 including the thermistor 16 that is environmentally friendly and can detect the temperature of the substrate 11 with high accuracy can be provided.

[0054] Furthermore, the thermistor 16 of the embodiment has a mass content of one or both of manganese, cobalt, copper and nickel in this order, and does not contain lead. Therefore, the heater 1 including the thermistor 16 that takes the environment into consideration and can detect the temperature of the substrate 11 with high accuracy can be provided.

[0055] Furthermore, the mass contents of manganese and cobalt in the thermistor 16 are greater than the mass contents of other components. Therefore, the heater 1 including the thermistor 16 that is environmentally friendly and can detect the temperature of the substrate 11 with high accuracy can be provided.

[0056] Furthermore, the total mass content of manganese, cobalt, copper, and nickel in the thermistor 16 of the embodiment is 50 [mass %] or more and 70 [mass %] or less. If the total mass content is less than 50 [mass %], there is a case where the B constant exceeds -2700 [K] and the thermistor 16 cannot detect the temperature of the substrate 11 with high accuracy. On the other hand, if the total mass content exceeds 70 [mass %], there is a case where other components contained in the thermistor 16, such as the amount of glass mixed for adhesion with the substrate 11, are small and affect the adhesion strength, or the amount of conductive material controlling the resistance value is small and has an effect of increasing the resistance value.

[0057] Furthermore, the thermistor 16 of the embodiment contains ruthenium in an amount of 2 [mass %] or more and 15 [mass %] or less. If the ruthenium content is less than 2 [mass %] or exceeds 15 [mass %], the sheet resistance value of the thermistor 16 becomes outside the range of 100 [kΩ / □] to 10000 [kΩ / □], and therefore, there is a case where the temperature of the substrate 11 cannot be detected with high accuracy.

[0058] Here, the relationship between the total mass content of manganese, cobalt, and copper and the physical properties of the thermistor 16 is described. The total mass content of manganese, cobalt, and copper was changed to test the physical properties of the thermistor 16, especially the presence or absence of peeling. The test was conducted on the thermistor 16 in which the total mass content of manganese, cobalt, and copper was changed to 60 [mass %], 65 [mass %], 70 [mass %], 75 [mass %], and 80 [mass %]. The presence or absence of pattern peeling when a needle with an epoxy resin adhesive (area φ2mm) attached to one side was bonded to the thermistor 16 and stretched horizontally was visually confirmed. In addition, the result of the peeling test was required to be no pattern peeling.

[0059] The test results are shown in Figure 3 .exist Figure 3 In the example, the case of "no pattern peeling" is expressed as "○", and the case of "pattern peeling" is expressed as "×". Figure 3 It is clear that when the total mass content of manganese, cobalt, and copper is 60 [mass %], 65 [mass %], and 70 [mass %], that is, when the total mass content of manganese, cobalt, and copper is 70 [mass %] or less, there is no pattern peeling, and there is no problem as the thermistor 16. On the other hand, when the total mass content of manganese, cobalt, and copper exceeds 70 [mass %], that is, when the total mass content of manganese, cobalt, and copper is 75 [mass %] and 80 [mass %], there is pattern peeling, and there is a problem as the thermistor 16. Based on the above, it is preferable that the total mass content of manganese, cobalt, and copper is 70 [mass %] or less.

[0060] Furthermore, regarding the thermistor 16 containing manganese, cobalt, and nickel, the thermistor 16 containing manganese, cobalt, copper, and nickel also obtained the same Figure 3 The same results were obtained for thermistor 16 shown in FIG. Based on the above, it is preferable that the total mass content of manganese, cobalt, copper, and nickel is 70 [mass %] or less.

[0061] Next, the relationship between the content [mass %] of ruthenium contained in the thermistor 16 and the sheet resistance value [kΩ / □] was tested. The test results are shown in Figure 4 .exist Figure 4 In the figure, the horizontal axis represents the ruthenium content [mass %], and the vertical axis represents the sheet resistance [kΩ / □]. The sheet resistance [kΩ / □] is the result of measurement at 25°C. Figure 4 It is clear that the ruthenium content at which the sheet resistance value of the thermistor 16 falls within the range of 100 [kΩ / □] to 10000 [kΩ / □] is 2 [mass %] or more and 15 [mass %] or less.

[0062] As described above, the heater 1 of the embodiment includes a substrate 11, a resistance heating element 12, and a thermistor 16. The substrate 11 has a first surface 11a and a second surface 11b located on the opposite side of the first surface 11a. The resistance heating element 12 is arranged on the first surface 11a. The thermistor 16 is arranged on the second surface 11b and does not contain lead. Therefore, a heater 1 that takes environmental considerations into account can be provided.

[0063] Furthermore, the thermistor 16 of the embodiment contains manganese, cobalt, and one or both of copper and nickel. Therefore, the heater 1 that can detect the temperature of the substrate 11 with high accuracy while taking the environment into consideration can be provided.

[0064] The thermistor 16 of the embodiment has the mass contents of one or both of the manganese, cobalt, copper and nickel in this order. Therefore, the heater 1 can be provided which can detect the temperature of the substrate 11 with high accuracy while taking the environment into consideration.

[0065] Furthermore, the mass contents of the manganese and cobalt in the thermistor 16 of the embodiment are larger than the mass contents of other components. Therefore, the heater 1 which is environmentally friendly and can detect the temperature of the substrate 11 with high accuracy can be provided.

[0066] The total mass content of the manganese, cobalt, copper, and nickel in the thermistor 16 of the embodiment is 50 mass % or more and 70 mass % or less. Therefore, the heater 1 that can detect the temperature of the substrate 11 with high accuracy while taking the environment into consideration can be provided.

[0067] Furthermore, the thermistor 16 of the embodiment contains ruthenium in an amount of 2 [mass %] or more and 15 [mass %] or less. Therefore, the heater 1 which can detect the temperature of the substrate 11 with high accuracy while taking the environment into consideration can be provided.

[0068] [Structure of Fixing Device]

[0069] Next, as an example, a fixing device according to the embodiment using the heater 1 according to the embodiment will be described with reference to the drawings. Figure 5 2 is a cross-sectional view showing a fixing device according to an embodiment using a heater according to an embodiment. Figure 5 As shown in FIG. 2 , the fixing device 200 is provided with a heater 1 at the bottom of a fixing film belt 201 wound around a support 202 in a cylindrical shape. The fixing film belt 201 is formed of a heat-resistant resin material such as polyimide. A pressure roller 203 is arranged at a position facing the heater 1 and the fixing film belt 201. The pressure roller 203 has a heat-resistant elastic material on its surface, such as a silicone resin layer 204, and can rotate around a rotating shaft 205 ( Figure 5 The P direction in the figure rotates.

[0070] In the toner fixing step, the toner image U1 attached to the recording paper (carbon paper) M as a medium is heated and melted by the heater 1 via the fixing film belt 201 at the contact surface between the fixing film belt 201 and the silicone resin layer 204. As a result, at least the surface portion of the toner image U1 exceeds the melting point, softens and melts. Thereafter, at the paper discharge side of the pressure roller 203, the recording paper M is separated from the heater 1 and the fixing film belt 201, and the toner image U2 is naturally radiated and solidified again, thereby fixing the toner image U2 to the recording paper M.

[0071] [Structure of Image Forming Apparatus]

[0072] Finally, an image forming apparatus according to an embodiment including the heater 1 according to the embodiment will be described as an example with reference to the drawings. Figure 6 1 is a cross-sectional view showing an image forming apparatus of the embodiment using the heater of the embodiment. The image forming apparatus of the embodiment is configured as a copier 100. Figure 6 As shown in FIG. 1 , in the copy machine 100, each component including the fixing device 200 is arranged in a housing 101. A document placement table made of a transparent material such as glass is installed on the upper part of the housing 101, and the document M1 to be the object of image information reading is moved back and forth on the document placement table ( Figure 6 Q direction in the figure) to scan the original M1.

[0073] An illumination device 102 having a light irradiation lamp and a reflector is provided at the upper part of the housing 101. The light irradiated from the illumination device 102 is reflected by the surface of the original M1 on the original placement table, and is slit-exposed on the photosensitive drum 104 through the short-focus small-diameter imaging element array 103. The photosensitive drum 104 is rotatable ( Figure 6 The photosensitive drum 104 is provided in the frame 101 in the R direction. In addition, a charger 105 is provided near the photosensitive drum 104 disposed in the frame 101, and the photosensitive drum 104 is also charged by the charger 105. The photosensitive drum 104 is coated with, for example, a zinc oxide photosensitive layer or an organic semiconductor photosensitive layer. An electrostatic image is formed on the charged photosensitive drum 104 by image exposure through the short-focus small-diameter imaging element array 103. The electrostatic image is developed by toner to become a toner image, and the toner contains a resin that is softened and melted by heating of the developer 106.

[0074] The recording paper M accommodated in the cassette 107 is fed to the photosensitive drum 104 by a pair of conveying rollers 109 that rotate synchronously with the feed roller 108 and the toner image on the photosensitive drum 104 and are pressed in the up-down direction. Then, the toner image on the photosensitive drum 104 is transferred to the recording paper M by the transfer discharger 110. Thereafter, the recording paper M that has been conveyed to the downstream side from the photosensitive drum 104 is guided to the fixing device 200 by the conveying guide 111 to be subjected to a heat fixing process (the toner fixing step) and then discharged to the tray 112. Then, after the toner image has been transferred, the residual toner on the photosensitive drum 104 is removed by the cleaner 113.

[0075] In the fixing device 200, the heater 1 is set in a state where the silicone resin layer 204 installed on the periphery of the pressure roller 203 is pressurized. The heater 1 includes a resistance heating element 12 larger than the effective length consistent with the width (length) of the maximum size paper that can be copied by the copier 100, that is, the width (length) of the maximum size paper, in the width direction of the recording paper M orthogonal to the conveying direction of the recording paper M. In addition, the heat generated by the resistance heating element 12 is used to melt the unfixed toner image on the recording paper M conveyed between the heater 1 and the pressure roller 203, so that the copy image of text, symbols, images, etc. appears on the recording paper M.

[0076] Furthermore, the heater 1 of the embodiment is described as an example of being used as a fixing heater of an image forming apparatus such as a copier 100, but the use of the heater 1 is not limited. The heater 1 of the embodiment can also be installed in household electrical appliances, precision machinery for work or experiments, or chemical reaction machines, etc., and used as a heat source for heating or heat preservation.

[0077] The embodiments of the present invention have been described, but the embodiments are only illustrative and are not intended to limit the scope of the invention. The embodiments can be implemented in various other ways, and various omissions, substitutions, and changes can be made without departing from the scope of the invention. The embodiments or their modifications are included in the scope or spirit of the invention, and similarly, are included in the invention described in the claims and their equivalents.

Claims

1. A heater, comprising: A substrate having a first surface and a second surface located opposite to the first surface; A resistance heating element is arranged on the first surface; as well as a thermistor disposed on the second surface, the thermistor containing manganese, cobalt, and copper, and not containing lead and nickel, The thermistor contains ruthenium in an amount of 2 [mass %] or more and 15 [mass %] or less.

2. The heater according to claim 1, wherein The mass contents of the manganese, the cobalt, and the copper in the thermistor are in this order from large to small.

3. The heater according to claim 1, wherein The mass contents of the manganese and the cobalt in the thermistor are greater than the mass contents of other components.

4. The heater according to claim 1, wherein The total mass content of the manganese, the cobalt, and the copper in the thermistor is 50 [mass %] or more and 70 [mass %] or less.

5. The heater according to claim 2, wherein The total mass content of the manganese, the cobalt, and the copper in the thermistor is 50 [mass %] or more and 70 [mass %] or less.

6. The heater according to claim 3, wherein The total mass content of the manganese, the cobalt, and the copper in the thermistor is 50 [mass %] or more and 70 [mass %] or less.