Electronic products with embedded porous dielectrics, related semiconductor products and methods of manufacturing the same

By adjusting the porosity of the porous anode oxide or anode hydroxide layer in semiconductor products, the problems of electrical signal transmission speed and impedance matching are solved, achieving efficient electrical signal transmission and increasing integration density.

CN111670495BActive Publication Date: 2024-10-15MURATA MFG CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980009874.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-01-25
Filing Date
2019-01-22
Publication Date
2024-10-15
Estimated Expiration
2039-01-22

AI Technical Summary

Technical Problem

In existing semiconductor products, the speed of electrical signals in transmission lines is difficult to accurately control, and conventional dielectrics are difficult to achieve low enough impedance matching, resulting in efficiency loss and control difficulties.

Method used

By forming a porous anodic oxide or anode hydroxide layer on a silicon substrate, adjusting the porosity to control the apparent dielectric constant and impedance of the medium, achieving the expected speed and impedance matching of electrical signals, and setting different pores in different areas rate porous layer to accommodate different drive frequencies.

Benefits of technology

It achieves precise control of electrical signal speed and impedance matching of electrical transmission lines, improves integration density and adaptability, and reduces the size and required coverage area of ​​electro-optical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111670495B_ABST
    Figure CN111670495B_ABST
Patent Text Reader

Abstract

In an electronic product including a silicon-on-insulator substrate, a porous layer of anodic oxide or anodic hydroxide is formed on a silicon layer of the silicon-on-insulator substrate. A metal layer formed on the porous layer provides at least one electrical transmission line. The speed of an electrical signal in the at least one electrical transmission line can be controlled by appropriate configuration of the porosity of the porous layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of integration, and more particularly, to electronic products, related semiconductor products and methods of manufacturing the same. Background Art

[0002] In recent years, semiconductor products have been developed in which different electronic sub-blocks are integrated on a common substrate to construct functions for electrical signal generation, transmission, conversion, detection, etc. Many advanced chips require coupling electronic functions to additional electronic functions or components on the same substrate or by stacking according to packaging solutions.

[0003] Figure 1 A plan view of an exemplary integrated functional structure 100 arranged on a wafer or substrate Sub is shown. For example, the substrate Sub may be a silicon-on-insulator (SOI) wafer.

[0004] exist Figure 1 In the example shown, the functional structure 100 utilizes an electrical transmission line implemented as a differential SGS coplanar waveguide (CPW). The SGS coplanar waveguide includes a ground line formed by a strip conductor G and two signal lines formed by two corresponding strip conductors S. For simplicity, Figure 1 Not shown are electrical connections for supplying electrical signals to the signal conductors S. The conducting wires of the coplanar waveguide are formed on the dielectric layer Diel.

[0005] In such Figure 1 In the device with the functional structure shown, it is desirable to precisely control the speed at which an electrical signal propagates in an electrical transmission line. 电 ∝V_F∝c / √(ε_eff)(V F is the velocity factor, and ε eff It is the equivalent dielectric constant of an electric wave propagating in an electric transmission line composed of a medium with a dielectric constant of εr inserted between the propagation line (signal line) and the ground loop. The properties of the dielectric have an important influence on the ability to control the speed of the electric signal.

[0006] In addition, in the functional structure 100, it is also desirable to ensure good impedance matching of the electrical transmission line used to propagate the electrical signal. In practice, inappropriate impedance matching may cause a large portion of the electrical wave to be reflected back to the source, resulting in efficiency loss and / or inappropriate control of the functional structure. The impedance Z generally used as a reference is usually Z = 50Ω, and the magnitude of the characteristic impedance of the electrical transmission line is Z ~ √ (L / (C)), where L is the line inductance (Hm -1 ), and C is the line capacitance (Fm -1). However, in practice, it is difficult to achieve sufficiently low impedance to ensure good impedance matching using conventional dielectrics because the minimum dimensions (critical dimensions, CD) achievable with conventional technologies (e.g., co-fired ceramics) are limited to tens of μm for both the line width / space within the plane and for the diameter / pitch of connecting via conductors.

[0007] The present invention has been accomplished in view of the above problems. Summary of the invention

[0008] The present invention provides an electronic product, comprising:

[0009] A silicon-on-insulator substrate comprising a base substrate, an insulating layer on the base substrate, and a silicon layer on the insulating layer;

[0010] forming a porous layer of anodic oxide or anodic hydroxide on the silicon layer; and

[0011] a metal layer formed over the porous layer, the metal layer providing at least one electrical transmission line,

[0012] Wherein the porosity of the porous layer in the region below the metal layer is configured based on a desired speed of an electrical signal in at least one electrical transmission line.

[0013] In the electronic product having the above configuration, the porous layer can be formed to contain a large amount of air / vacuum. In addition, the fraction of air / vacuum in the finished product can be set by controlling the size of the holes formed in the porous layer.

[0014] By appropriately adjusting the ratio of material to air / vacuum present in the porous layer (porosity), a number of beneficial results can be achieved.

[0015] First, by appropriately adjusting the porosity of the porous layer, the apparent dielectric constant ε of the medium can be controlled. eff . For ε eff The control of makes it possible to control the velocity factor V related to the velocity of the electrical signal in the electrical transmission line f Thus, a desired speed of electrical signals in electrical transmission lines can be achieved to meet, for example, specific application requirements.

[0016] Second, the inclusion of air / vacuum in the medium below the conductor of the electrical transmission line may lead to an increase in impedance, especially in the case of large porosity (i.e., large fraction of air / vacuum in the porous layer). However, the increase in impedance (associated with a reduction in coupling capacitance) can be compensated by reducing the critical dimension (CD), for example: compared to the known MLCC (multilayer ceramic capacitor) approach, the line width / spacing rule can be reduced by 2 orders of magnitude (e.g., a minimum CD < 5 μm can be obtained), and this allows the line impedance to be tuned to a lower value. Similarly, the vertical dimension can also be reduced by 2 orders of magnitude compared to MLCC. Therefore, for a given target impedance, the overall size (CD) can be reduced and the integration density can be further increased.

[0017] Third, by appropriately tuning the porosity of the porous layer, the specific layout of the electronics can be adapted to different driver frequencies while maintaining performance.

[0018] In an embodiment, the electronic product further comprises an optical waveguide formed within the silicon layer, and the porosity of the porous layer in a region below the metal layer is configured such that a speed of electrical signals in the at least one electrical transmission line approaches a speed at which optical signals propagate in the optical waveguide.

[0019] In the electronic product according to the embodiment of the present invention, the pores in the porous layer may be tubular in shape. The tubular pores extend toward the underlying silicon layer.

[0020] Typically, the porosity of the porous layer ranges from 50% up to 91%.

[0021] In an embodiment, the porous layer is made of anodized aluminum oxide (AAO).

[0022] In an embodiment, the electronic product further comprises an anodization control device formed in the silicon layer, the anodization control device being configured to control the porosity of the porous layer during manufacturing. The anodization control device is configured so that a voltage drop (anode voltage) occurring across an area being anodized during anodization causes a desired porosity of the area. To control the anodization control device, a metal contact is disposed on a surface above the porous layer, and a conductive path is disposed to interconnect the metal contact to the anodization control device. In an embodiment, the metal contact comprises a through-hole conductor extending through the porous layer.

[0023] In an embodiment, the anodization control device is provided by a diode formed by a p-type region and an n-type region formed in the silicon layer. However, embodiments are not limited to the anodization control device being a diode, and other passive devices (e.g., resistors) integrated into the silicon layer may be used in other embodiments.

[0024] In another embodiment, the electronic product comprises a plurality of anodization control devices, each anodization control device being configured to control the porosity of a corresponding region of the porous layer. In an embodiment, the plurality of anodization control devices are configured to produce regions of different porosities in the porous region. In an embodiment, the porous layer comprises a first porous region having a first porosity and a second porous region having a second porosity.

[0025] According to an embodiment of the present invention, one or more electrical transmission lines of the same or different types may be provided in an electronic product. The one or more electrical transmission lines may include transmission lines of microstrip line type, coplanar waveguide type, differential microstrip line type, etc.

[0026] One or more electrical transmission lines can be constructed on a common substrate of a porous layer with uniform porosity. Alternatively, one or more electrical transmission lines can be arranged on multiple porous regions with different porosities. This makes it possible to arrange electrical transmission lines supporting different signal speed requirements on a common substrate.

[0027] In an embodiment, multiple sets of anodization control devices are provided for corresponding different electrical transmission lines on a common substrate. The properties of each anodization control device are set according to the porosity requirements desired for the porous region associated with the corresponding electrical transmission line. Thus, anodization in different regions can be achieved by applying a common voltage to different anodization control devices (e.g., at the periphery of the substrate / wafer). This facilitates the anodization process.

[0028] The present invention also provides a method for manufacturing an electronic product, the method comprising:

[0029] forming a first p-type region and a first n-type region in a silicon layer of a silicon-on-insulator substrate, the silicon-on-insulator substrate comprising a base substrate, an insulating layer on the base substrate, and a silicon layer on the insulating layer, the first p-type region and the first n-type region forming a first anodized control diode;

[0030] forming a second p-type region and a second n-type region in the silicon layer to form a second anodized control diode;

[0031] forming a metal layer over the silicon layer;

[0032] anodizing the metal layer using the first anodizing control diode and the second anodizing control diode to form a porous layer of an anodic oxide or an anodic hydroxide; and

[0033] A metal layer is formed over the porous layer, the metal layer providing at least one electrical transmission line.

[0034] According to the above method, the porosity achieved in the porous layer below at least one electrical transmission line, and thus the effective dielectric constant, can be controlled in a simple manner by controlling the anodization process for anodizing the metal layer. In an embodiment, the porosity of the porous layer in the region below the metal layer is configured based on the desired speed of the electrical signal in the at least one electrical transmission line.

[0035] In another embodiment, anodizing a metal layer includes: controlling a first anodizing control diode and a second anodizing control diode during anodizing of the metal layer so that a porous layer formed includes a first porous region having a first porosity and a second porous region having a second porosity. In an embodiment, the method includes: applying a common voltage to the first anodizing control diode and the second anodizing control diode to anodize the metal layer to form the porous layer.

[0036] In variations of the above method, the anodization control device is provided by other types of passive devices (eg, resistors).

[0037] The present invention also provides an electro-optical product, comprising:

[0038] A silicon-on-insulator substrate comprising a base substrate, an insulating layer on the base substrate, and a silicon layer on the insulating layer;

[0039] a first pair of adjacent p-type and n-type regions in the silicon layer, the first pair of adjacent p-type and n-type regions defining a first metallurgical junction therebetween, the first metallurgical junction having a boundary along an underlying insulating layer, wherein a depletion region around the first metallurgical junction is a propagation region for an optical signal of the first optical waveguide;

[0040] a confinement layer formed on the silicon layer and encapsulating a propagation region of the first optical waveguide;

[0041] a porous region formed of an anodic oxide or anodic hydroxide located on either side of and bounded by the confinement layer; and

[0042] A patterned metal layer overlying the anodic oxide / hydroxide regions forms a conductor for an electrical transmission line.

[0043] In the electro-optical product having the above configuration, the anodized oxide region / hydroxide region can be formed to contain a large amount of air / vacuum. In addition, the fraction of air / vacuum in the finished product can be set by controlling the size of the pores formed in the anodized oxide region / hydroxide region.

[0044] By properly adjusting the ratio of materials present in the anodic oxide / hydroxide region to air / vacuum, a number of beneficial results can be achieved.

[0045] First, by appropriately adjusting the ratio of material present in the anodic oxide / hydroxide region to air / vacuum, the apparent dielectric constant ε of the medium can be controlled. eff , for example ε eff can be reduced to a velocity factor V related to the velocity of the wave f It can be increased to a point closer to 1, so that the mismatch that would otherwise occur between the speed of the electrical signal and the speed of light in the optical waveguide can be reduced. Increasing the speed of the electrical signal so that it substantially matches the speed of the optical signal eliminates the need to include additional loops in the design, and this enables the integration density (i.e., the footprint required to implement the electro-optical device) to be reduced. Furthermore, even when the speed of the electrical signal is brought closer to the speed of the optical signal without matching the speed of the optical signal, a technical advantage can be obtained because the size of the additional loop required can be reduced.

[0046] Second, the inclusion of air / vacuum in the dielectric beneath the conductor of the electrical transmission line may result in an increase in impedance, especially when the porosity is large (i.e., the fraction of air / vacuum in the anodic oxide / hydroxide region is large). However, as described above, the increase in impedance (associated with a reduction in coupling capacitance) can be compensated by reducing the critical dimension (CD).

[0047] Third, by appropriately tuning the porosity of the anodic oxide / hydroxide regions, specific layouts of electro-optical devices can be tailored to different driver frequencies while maintaining performance.

[0048] In an electro-optical product according to an embodiment of the present invention, a conductive path may interconnect a metal layer forming a conductor of an electrical transmission line with a first pair of p-type and n-type regions defining a first metallurgical junction, and the conductive path may include a first via conductor extending through the anode oxide / hydroxide region.

[0049] In an electro-optical product according to an embodiment of the present invention, n may be provided in the silicon layer. + Type region and p + type area, and n + Type region and p + The first through-hole conductor may connect the metal layer defining the first signal conductor of the electrical transmission line to the n-type region in the silicon layer. + The second via conductor may interconnect the metal layer defining the ground conductor of the electrical transmission line with the p-type region in the silicon layer. + The p-type region (and thereby the p-type region defining the first PN junction) is interconnected.

[0050] The sizes of the first and second via conductors and the spacing between the first and second via conductors may be configured to match the impedance of the vias to the characteristic impedance of the electrical transmission line.

[0051] It is simple to control the size and spacing of the via conductors, for example by using a photolithography process.Thus, by setting the size and spacing of the via conductors in such a way that the impedance of the vias matches the characteristic impedance of the electrical transmission line, impedance matching can be achieved in a simple manner.

[0052] In an electro-optical product according to an embodiment of the present invention, a second pair of adjacent p-type and n-type regions may be provided in the silicon layer above the insulating layer, the second pair of adjacent p-type and n-type regions defining a second metallurgical junction therebetween, and a second n-type region in contact with the first n-type region may be provided in the silicon layer. + The depletion region around the second metallurgical junction can be configured as a propagation region of the optical signal of the second optical waveguide. The patterned metal layer can include a second signal conductor. The third through-hole conductor can connect the metal layer defining the second signal conductor to the second n type region in the silicon layer. + The first signal conductor and the second signal conductor can be configured to propagate complementary signals. In this way, the electrical transmission line, the first optical waveguide and the second optical waveguide can be configured to form an electro-optical modulator.

[0053] Multiple electro-optic modulators with anodic oxide / hydroxide regions of different porosity can be constructed on a common substrate. This allows optical waveguides with different optical path lengths to be arranged on a common substrate (taking into account that the optical signal length is related to the wavelength of the optical signal propagating in the optical waveguide).

[0054] In an electro-optical product according to embodiments of the present invention, the electro-optic modulator may include sub-regions of anodic oxide / hydroxide having different porosities along the optical path.

[0055] In an electro-optical product according to an embodiment of the present invention, an anodized control diode may be provided which is electrically connected to the p-type diode in the silicon layer. + Type area and n + The anodizing control diodes make it possible to control the porosity achieved in the anodic oxide / hydroxide regions during manufacturing. Furthermore, if multiple sets of anodizing control diodes are provided for respective different electrical transmission lines on a common substrate, the properties of the anodizing control diodes of each set can be set differently from one another depending on the requirements for the porosity desired for the anodic oxide / hydroxide regions associated with each electrical transmission line, and anodization in different regions can also be achieved by applying a common voltage to the different anodizing control diodes (e.g., at the periphery of the substrate / wafer).

[0056] The porous anodic oxide / hydroxide region may be made of anodized aluminum.

[0057] The present invention also provides a method for manufacturing an electro-optical product, the method comprising:

[0058] forming a first pair of adjacent p-type and n-type regions in a silicon layer of a silicon-on-insulator substrate, the silicon-on-insulator substrate comprising a base substrate, an insulating layer on the base substrate, and a silicon layer on the insulating layer, the first pair of adjacent p-type and n-type regions defining a first metallurgical junction therebetween, the first metallurgical junction having a boundary along an underlying insulating layer;

[0059] forming a confinement layer over the silicon layer, the confinement layer encapsulating a depletion region around the first metallurgical junction, thereby configuring the depletion region as a propagation region for an optical signal of the first optical waveguide;

[0060] forming a metal layer over the silicon layer;

[0061] anodizing the metal layer to form a porous layer of anodic oxide or anodic hydroxide; forming an opening in the anodic oxide / hydroxide layer facing the optical waveguide; and

[0062] Metal conductors for electrical transmission lines are formed over the anodic oxide / hydroxide regions on either side of the opening.

[0063] According to the above method, the porosity achieved in the dielectric beneath the conductor of the electrical transmission line, and thus the effective dielectric constant, can be controlled in a simple manner by controlling the anodization process anodizing the metal layer.

[0064] The present invention also provides a semiconductor product, comprising:

[0065] A silicon-on-insulator substrate comprising a base substrate, an insulating layer on the base substrate, and a silicon layer on the insulating layer;

[0066] a first pair of adjacent p-type and n-type regions in the silicon layer, the first pair of adjacent p-type and n-type regions defining a first metallurgical junction therebetween, the first metallurgical junction having a boundary along an underlying insulating layer, wherein a depletion region around the first metallurgical junction is configured as a propagation region for an optical signal of a first optical waveguide;

[0067] a confinement layer formed on the silicon layer and encapsulating the first optical waveguide; and

[0068] A porous region, formed from the anodic oxide or anodic hydroxide, is located on either side of the confining layer and is bounded by the confining layer.

[0069] The above-mentioned semiconductor product may be an intermediate product formed during the manufacture of the electro-optical product according to the invention.

[0070] The present invention also provides a method for manufacturing a semiconductor product, the method comprising:

[0071] forming a first pair of adjacent p-type and n-type regions in a silicon layer of a silicon-on-insulator substrate, the silicon-on-insulator substrate comprising a base substrate, an insulating layer on the base substrate, and a silicon layer on the insulating layer, the first pair of adjacent p-type and n-type regions defining a first metallurgical junction therebetween, the first metallurgical junction having a boundary along an underlying insulating layer;

[0072] forming a confinement layer over the silicon layer, the confinement layer encapsulating a depletion region around the first metallurgical junction, thereby configuring the depletion region as a propagation region for an optical signal of the first optical waveguide;

[0073] forming a metal layer over the silicon layer;

[0074] anodizing the metal layer to form a porous layer of anodic oxide or anodic hydroxide; and

[0075] Openings are formed in the anodic oxide / hydroxide layer facing the optical waveguide. BRIEF DESCRIPTION OF THE DRAWINGS

[0076] Further features and advantages of the invention will become apparent from the following description of certain embodiments of the invention given by way of example only and not by way of limitation, with reference to the accompanying drawings, in which:

[0077] Figure 1 is a plan view of an example integrated semiconductor structure;

[0078] Figure 2A An example electronic product according to an embodiment of the present invention is shown;

[0079] Figure 2B An example electronic product according to another embodiment of the present invention is shown;

[0080] Figure 2C An example electronic product according to another embodiment of the present invention is shown;

[0081] FIG. 3A to FIG. 3C Porous anodic oxide / hydroxide materials with different porosity values ​​are shown, where:

[0082] Figure 3A shows a porosity of 11%,

[0083] Figure 3B shows a porosity of 54%, and

[0084] Figure 3C A porosity of 91% is shown;

[0085] Figure 4is a graph showing how the speed of an electrical signal is affected by the porosity of a porous anodic oxide / hydroxide layer;

[0086] Figure 5 is a graph showing how the characteristic impedance of an electrical transmission line is affected by the porosity of a porous anodic oxide / hydroxide layer;

[0087] Fig. 6A and Figure 6B showing a substrate having different regions with porous dielectrics including different degrees of porosity;

[0088] 7A to 7D The structure of the pores formed in anodized aluminum is shown, where:

[0089] Fig. 7A This is a close-up 3D schematic diagram of a portion of the porous AAO layer.

[0090] Figure 7B Indicates that Fig. 7A A cross section of a part of

[0091] Figure 7C is a high-resolution TEM image of a porous AAO layer observed from the side, and

[0092] Fig.7D is a high-resolution TEM image of a porous AAO layer observed from above;

[0093] Figure 8 An electro-optical product according to an embodiment of the present invention is shown in cross section;

[0094] Fig. 9 is a diagram showing a variant embodiment including an anodized control diode; and

[0095] FIG. 10A to FIG. 10H Shows the manufacturing Figure 8 The stages in an example method of an electro-optical product. DETAILED DESCRIPTION

[0096] Figure 2A 1 shows a top view and a cross-sectional view of an example electronic product 300A according to an embodiment. (Similarly, the following Figure 2B and Figure 2C A top view and a cross-sectional view of the electronic product are also shown. Figure 2A As shown, the electronic product 300A includes a silicon-on-insulator (SOI) substrate formed of a silicon base substrate 302, an insulating layer 304 formed on the base substrate 302, and a thin silicon layer 306 formed on the insulating layer 304. In an embodiment, the insulating layer 304 is a buried oxide layer made of SiO2, and the thin silicon layer 306 is a relatively low-doped (e.g., 1×1017 a / cm 3 A p-type silicon layer doped with a concentration of .

[0097] Regions 308a and 308b having a specified doping type and level are formed in the thin silicon layer 306. In an embodiment, region 308b is a relatively lightly n-type doped region, and region 308a is a relatively lightly p-type doped region. A PN diode is formed by regions 308a and 308b. In an embodiment, as shown in FIG. Figure 2A As shown, region 308a is formed as a square / rectangular ring surrounding region 308b, which may also be square / rectangular.

[0098] A porous layer 310 is formed on the silicon layer 306. In an embodiment, the porous layer 310 is made of an anodic oxide or an anodic hydroxide. For example, the porous layer 310 can be made of anodized aluminum oxide (AAO). In an embodiment, the porous layer 310 is formed by anodizing a metal layer by performing an anodizing process in an electrolyte. In this anodizing process, an oxide or hydroxide is formed on the surface of the metal layer, and the electrolyte dissolves the oxide or hydroxide layer along a preferred direction determined by the electric field (i.e., generally perpendicular to the surface). As the electrolyte dissolves the oxide / hydroxide layer, new oxide / hydroxide is formed on the metal surface that becomes exposed. As a result, the metal layer is gradually transformed into a porous layer 310 of anodized oxide or hydroxide having tubular pores extending substantially vertically from the top surface, each pore being separated from adjacent pores by the wall of the oxide or hydroxide. The resulting porous layer 310 has cylindrical pores distributed according to a hexagonal pattern (see FIG. 3A to FIG. 3C and 7A to 7D ). The porous layer 310 can be formed in a desired portion of the metal layer by ensuring that other portions of the metal layer are masked before anodization is performed. Figure 2A As shown, non-anodized areas of the masked metal layer remain on either side of the porous layer 310 (adjacent to element 312).

[0099] FIG. 3A to FIG. 3C Some geometries obtained by this method are shown. Figure 3A The case where the ratio of pore diameter to pore spacing is 33% is shown, resulting in a porosity of 11%, where porosity is the ratio of the volume of pores in the porous layer 310 to the volume of the porous layer 310 . Figure 3B The case where the ratio of pore diameter to pore spacing is 66% is shown, corresponding to a porosity of 54%. Figure 3C The case where the ratio of pore diameter to pore spacing is 87% (the actual maximum) is shown, and this gives a porosity of 91%.

[0100] return Figure 2AA conductive path 312, such as a via conductor, extends through the porous layer 310 to interconnect a metal contact 316 formed on the surface above the porous layer 10 with the n-type region 308b of the PN diode. This allows control of the PN diode provided by regions 308a and 308b.

[0101] In an embodiment, the PN diode formed by regions 308a and 308b provides an anodization control diode that can be used to control the anodization process that creates the porous layer 310 during the manufacture of the electronic product 300A. More specifically, the anodization control diode can be used to control the porosity of the porous layer 310, which is a function of the pitch P and diameter D of the pores within the porous layer 310 (see Figure 3A ). The spacing P between adjacent pores is related to the voltage applied during the anodization process (and the adjustment of the electrolyte), and the diameter D of the pores can be adjusted by controlling the etching time during the subsequent isotropic etching step. Thus, the ratio of the fraction of air (or vacuum) to the fraction of oxide / hydroxide in the structure can be adjusted (see FIG. 3A to FIG. 3C ), and can be bounded by 真空 <·ε 多孔层 <ε 氧化物 / 氢氧化物(在没有孔的情况下) Adjust the apparent dielectric constant of the medium.

[0102] In another embodiment, the PN diode formed by regions 308a and 308b is replaced with a different type of passive device (eg, a resistor) formed in silicon layer 306. The passive device may be configured as an anodization control device for controlling the porosity of porous layer 310.

[0103] return Figure 2A , a metal layer 314 is formed on the porous layer 310 to provide at least one electrical transmission line. Figure 2A In an embodiment, metal layer 314 includes a single signal (S) conductor line, and insulating layer 304 provides grounding, thereby creating a microstrip line configuration. Connections (not shown) are provided for supplying electrical signals to the conductor line of the microstrip line.

[0104] Using the above-described anodization control features, in an embodiment, the porosity of the porous layer 310 is configured based on the desired speed of the electrical signal in at least one electrical transmission line. The desired speed of the electrical signal may be a speed required to meet the requirements of a particular application. Specifically, to achieve a greater speed of the electrical signal, the porosity of the porous layer 310 is increased to reduce the effective dielectric constant of the medium below the electrical transmission line. Conversely, a lower speed is achieved by reducing the porosity of the porous layer 310 to increase the effective dielectric constant of the medium below the electrical transmission line.

[0105] Figure 4is a graph showing the velocity of an electrical signal in an electrical transmission line on the y-axis as a function of frequency on the x-axis. Figure 4 The fact is shown that by increasing the porosity of the porous layer, the apparent dielectric constant of the medium below the conductor of the electric transmission line decreases, and the speed of the electric signal can be increased. This same effect is also obtained using anodic oxides and hydroxides other than AAO.

[0106] Figure 5 is a graph showing the characteristic impedance of an electrical transmission line on the y-axis as a function of frequency on the x-axis. Figure 5 It is shown how an increase in the porosity of the porous layer 310 made of anodized aluminum causes an increase in the characteristic impedance of the electrical transmission line. As mentioned above, this increase in impedance can be compensated by reducing the critical dimension.

[0107] When using anodic oxides and hydroxides other than anodized aluminum, Figure 5 And the effect shown in Figure 6.

[0108] Typically, the uniformity of the porosity of the porous region depends on the uniformity of the anodizing current supplied to different portions of the metal layer being anodized during the anodizing process. Given the fact that in the context of integrated circuit manufacturing it is desirable / necessary to apply the anodizing voltage at the periphery of the wafer, it is questionable whether a suitable degree of uniformity can be obtained during the anodizing process. However, significantly, suitable uniformity can be achieved when the anodizing voltage is applied from contact regions at the periphery of the wafer for the reasons explained below.

[0109] According to other embodiments, different types of electrical transmission lines may be provided by a metal layer formed on the porous layer 310. For example, Figure 2B In the illustrated embodiment, the metal layer includes a signal conductor line 314 formed between two ground conductor lines 318a and 318b, whereby at least one electrical transmission line includes a GSG coplanar waveguide. Figure 2C In another embodiment shown, the metal layer includes differential signal conductor lines 336a and 336b, whereby at least one electrical transmission line includes a differential microstrip conductor. Figure 2A Insulating layer 304 provides grounding. In other embodiments, multiple electrical transmission lines of the same and / or different types may be provided by a metal layer formed on top of porous layer 310.

[0110] According to other embodiments, the porous layer 310 may include a plurality of porous regions with different porosities. The same electrical transmission line and / or different electrical transmission lines may be formed on the plurality of porous regions. Figure 2CAn example electronic product 300C illustrating this concept is shown in FIG. As shown, the electronic product 300C includes a first porous region 324 and a second porous region 326. The first porous region 324 is characterized by a first porosity, and the second porous region 326 is characterized by a second porosity. The first porosity and the second porosity can be configured to be different or equal.

[0111] For the purpose of independently controlling the anodization of the first porous region and the second porous region, separate anodization control devices and associated conductive paths are provided. Figure 2C In an embodiment of the present invention, silicon layer 306 includes p-type regions 308a and 308c and n-type regions 308b and 308d. P-type region 308a and n-type region 308b provide a first anodized control diode for first porous region 324, and p-type region 308c and n-type region 308d provide a second anodized control diode for second porous region 326. A conductive path 328, such as a through-hole conductor, extends through porous region 324 to interconnect metal contact 332 with n-type region 308b of the first diode to allow control of the first diode. A conductive path 330, such as a through-hole conductor, extends through porous region 326 to interconnect metal contact 334 with n-type region 308d of the second diode to allow control of the second diode.

[0112] exist Figure 2C In an example embodiment of the present invention, the same electrical transmission line, i.e., a differential microstrip guide, extends over both the first porous region 324 and the second porous region 326. However, in other embodiments, the metal layer formed on the porous layer may include a first electrical transmission line and a second electrical transmission line, such that the first porous region 324 is located below the first electrical transmission line and is coupled to ground, the first electrical transmission line, and the second porous region 326 is located below the second electrical transmission line and is coupled to ground, the second electrical transmission line. The first electrical transmission line and the second electrical transmission line may be of the same or different types. For example, the first electrical transmission line and the second electrical transmission line may each include a microstrip line, a coplanar waveguide, or a differential microstrip guide.

[0113] An electronic product such as the example electronic product 300C may be obtained from, for example, Fig. 6A The wafer 50 shown in FIG. 1 is fabricated starting with a wafer 50. As shown, the wafer 50 includes different regions 52, 54, 56 of anodized aluminum oxide (AAO). In region 52, the porosity of the AAO is 90%. In region 54, the porosity of the AAO is 45%. In region 56, the porosity of the AAO is 70%. The remaining portion 58 of the wafer 50 is provided with an AAO layer having a porosity of 11%.

[0114] By realizing specific areas with different porosities on a common substrate, structures with different electrical signal speed requirements can be integrated. Figure 6B Such an integrated structure is shown with respect to a substrate portion 60 having different regions 62, 64, 68 of AAO. In region 62, the porosity of the AAO is 90%. In region 64, the porosity of the AAO is 45%. In region 68, the porosity of the AAO is 11%. Figure 6B In the example shown, the first Mach-Zehnder modulator 72 is formed in the region corresponding to the AAO region 68, and the second Mach-Zehnder modulator 74 is formed in the region corresponding to the AAO regions 62 and 64 (in Figure 6B Only the position of the optical waveguide is shown in FIG. 1 ). Therefore, MZMs 72 and 74 may have different optical path lengths. Moreover, in MZM 74, since the effective dielectric constant changes along the length of the optical waveguide, the electrical velocity achieved changes along the propagation direction. As will be understood by those skilled in the art based on the teachings herein, Figure 6B The illustrated embodiments are not limited to Mach-Zehnder modulators embedded therein and may include any structure using at least one electrical transmission line.

[0115] 7A to 7D The structure of a porous anodized aluminum oxide layer that may be provided in an electronic product or a semiconductor product according to certain embodiments of the present invention is shown. Fig. 7A A cross section of a porous AAO layer is schematically shown in perspective and on a greatly enlarged scale. Figure 7B Indicates that Fig. 7A A cross section of a part of. Figure 7C and Fig.7D TEM high-resolution images of a real porous AAO layer observed from the side and from above, respectively.

[0116] In the following, reference will be made to Figure 8 Electro-optical products utilizing aspects of the present invention according to embodiments are described. The embodiments will be described in the context of an electro-optical product 1 comprising an integrated electro-optical modulator of the Mach-Zehnder type. However, it should be understood that electro-optical products according to the present invention are not limited to electro-optical products comprising Mach-Zehnder electro-optical modulators, and may include other types of electro-optical products, including electrical and optical waveguides associated with each other in various devices. For example, electro-optical products according to embodiments may include, but are not limited to, ring modulators, photodiodes, and the like.

[0117] Figure 8 The electro-optical product 1 shown uses a silicon base substrate 2 ( Fig. 9 2 ), an insulating layer 3 formed on the base substrate 2, and a thin silicon layer 4 formed on the insulating layer 3. In this example, the insulating layer 3 is a buried oxide layer made of SiO2, and the thin silicon layer is a relatively low-doped (for example, 1×10 17 a / cm3 A p-type silicon layer (doped with a concentration of 1000 N) is formed. Regions 4a to 4e of specified doping types and levels are formed in the thin silicon layer. Region 4b is a relatively lightly n-type doped region, and region 4d is a relatively lightly p-type doped region. Region 4c is a very lightly p-type doped region around the metallurgical junction between regions 4b and 4d. A PN or PIN diode is formed by regions 4b and 4d sandwiching region 4c. The metallurgical junction extends downward to the buried oxide layer 3 below.

[0118] Region 4a is a relatively heavily n-doped region, designated here as n + type region, and region 4e is a relatively heavily p-type doped region, designated herein as p + Type area. + Regions 4a and p + Region 4e serves to facilitate electrical connection of the doped regions 4b and 4c of the PIN diode to the conductors of an electrical transmission line (in this example a coplanar waveguide, see below) and to reduce the access impedance to the metallurgical junction.

[0119] The grooves 6a, 6b are formed on either side of the metallurgical junction and are slightly spaced apart from the metallurgical junction. The region 8 between the grooves serves as a propagation region for the optical signal. The region 8 is surrounded by a limiting material 9 disposed above the recessed region and filling the grooves 6a, 6b. The limiting material 9 may be made of the same material as the insulating layer 3 (e.g., SiO2). The limiting material 9 ensures that an appropriate refractive index transition occurs at the boundary surface between the optical path and the limiting material 9, which prevents undesirable optical signal losses caused by parasitic reflections at these boundaries.

[0120] Limit material 9 overlap in n + Regions 4a and p + The limiting material is provided above the edge of the region 4e and adjacent to an adjacent region 10 made of a porous layer of anodic oxide or anodic hydroxide. In this example, the porous region 10 is made of anodized aluminum. An opening 17 is provided through the porous anodic oxide / hydroxide layer 10 above the light path, and the opening 17 is free of anodic oxide / hydroxide to avoid unwanted reflections that might otherwise occur at the interface between the light path and the anodic oxide / hydroxide. The limiting material has a protective portion 19 that extends upwardly and over the edge of the porous anodic oxide / hydroxide layer 10 around the periphery of the opening 17. The protective portion 19 is used to control the porosity of the vertical surface of the region 10 adjacent to the protective portion 19 and prevent the formation of side holes.

[0121] Figure 8 The case where the same material is used in the grooves 6 a , 6 b , for the limiting material 9 above these grooves and for forming the protective portion 19 is shown.

[0122] One end of the through hole passing through the anodic oxide / hydroxide region 10 is provided to contact n + Regions 4a and p + The through-hole electrodes 12a and 12b of the region 4e are connected to each other, and the metal strips 14 and 15 corresponding to the signal line and the ground line of the electric transmission line are in contact with the other ends of the through-hole electrodes 12a and 12b. + The region 4a is electrically connected to the n-type region 4b of the PIN diode, and the ground line 15 of the electrical transmission line is connected via the p + Region 4e is electrically connected to p-type region 4d of the PIN diode.Connections (not shown) are provided for supplying electrical signals to the conductors of the electrical transmission line, and input / output connections (not shown) to the optical waveguide are also provided.

[0123] Because the porous regions 10 are formed from anodic oxides or anodic hydroxides, these regions can be formed so that they contain a large and adjustable percentage of air or vacuum. This enables the effective dielectric constant of the medium beneath the conductor of the electrical transmission line to be reduced to a specified value. The reduction in the effective dielectric constant enables the speed of electrical signals in the electrical transmission line to be closer to the speed of optical signals. As will be discussed below, the porosity of the porous regions 10 can be set by appropriately controlling the size and spacing of the pores.

[0124] Now refer to FIG. 10A to FIG. 10H A method of manufacturing an electro-optical product according to an embodiment of the present invention is described.

[0125] According to the manufacturing method of this example, the silicon layer 4 of the silicon-on-insulator (SOI) substrate wafer is doped, preferably to obtain a relatively low level of p-type doping, for example 1×10 17 a / cm 3boron concentration (the SOI wafer includes a p-type silicon layer 4 above an insulating layer 3, where the insulating layer is a buried oxide layer). At least one PIN diode structure is formed in the silicon layer 4 so that the vertical depth of the PN junction extends to the depth of the buried oxide 3. The PIN diode structure is realized by the following operation: dopants of the opposite type are implanted into corresponding regions that define a volume of silicon with very low p-type doping. The implantation process is followed by activation / driving in a processing step (heat treatment) that forms a metallurgical junction with a low doping level on both sides. Alternatively, the desired PIN diode structure can be created by the following operation: consecutive implantation steps are performed to create corresponding highly doped n / p sub-regions (corresponding to the p-type region and the n-type region of the PIN structure) and a low doped n / p sub-region (corresponding to the central part of the PIN diode). In order to reduce the access impedance to the intrinsic region, preferably, contact regions of the P-electrode and the N-electrode of the PIN diode are formed with heavier doping (or even preferably formed as silicide) to form the above-mentioned n + Regions 4a and p + Area 4e.

[0126] The p- and n-doped regions are etched down to form recesses 6a, 6b near the low-doped regions (close to the metallurgical junctions) corresponding to the waveguides for the optical signals. Fig. 10A represents the resulting structure at this stage.

[0127] like Fig. 10B As shown, a material layer 90, in this example silicon oxide, is then deposited on the wafer surface. The material layer 90 is patterned (see Fig. 10C ) to create a confinement material 9 that ensures a proper refractive index transition at the boundary between the light path and the confinement material. The desired patterning can be created by conventional photolithography steps.

[0128] like Fig. 10D As shown, a thick metal film 100 is deposited on top of the structure. The metal film is composed of at least one metal layer that can be anodized. The thick metal film 100 is preferably an aluminum film with a thickness of more than 1 μm and less than 500 μm. However, other metal types may also be used, including, for example, titanium (Ti), tungsten (W) or tantalum (Ta). In this document, the expressions "anodized" and "anodic" refer to oxides or hydroxides formed by a metal layer by anodization in an electrolyte (see below).

[0129] like Fig. 10E As shown, the thick metal film 100 is patterned to form openings 17 near the light path. This is for the purpose of avoiding unwanted reflections at the interface between the metal 100 and the light path. The patterning may be performed by any suitable lithographic process, for example by photolithography and etching.

[0130] Deposit another material having an appropriate refractive index value to coat the surface of the metal layer 100 at the periphery of the opening 17 and form the protective portion 19 (see Fig.10F ). Preferably, the additional material is selected to Fig. 10C The confinement material 9 has the same refractive index.

[0131] The metal layer 100 is anodized by performing an anodizing process in an electrolyte. In the anodizing process, an oxide or hydroxide is formed on the surface of the metal, and the electrolyte dissolves the oxide or hydroxide layer in a preferred direction determined by the electric field (i.e., generally perpendicular to the surface). As the electrolyte dissolves the oxide / hydroxide layer, new oxide / hydroxide is formed on the metal surface that becomes exposed. As a result, the metal layer 100 is gradually transformed into a porous layer 10 of anodized oxide or hydroxide having tubular pores extending substantially vertically from the top surface, each pore being separated from adjacent pores by the wall of the oxide or hydroxide. The porous region 10 is preferably an anodized aluminum region having cylindrical pores distributed according to a hexagonal pattern (see FIG. 3A to FIG. 3C and 7A to 7D ). Figure 10G The resulting structure, which may be considered as an intermediate semiconductor product 21 , is shown.

[0132] A via is etched through the porous region 10 to expose the n + Regions 4a and p + Region 4e, a metal layer is then deposited over the structure and etched by a known photolithography process to form conductors 14, 15 of the electrical transmission line and via conductor 12. As a result, the coplanar waveguide signal (S) and ground (GND) lines are connected to the corresponding n-type and p-type regions (such as ) that define the PN junction used by the optical waveguide. Fig. 10H shown).

[0133] Since the voltage set to the p-type silicon layer (specifically, to the region 4a) during the anodization process is anodic (positive), an n-type silicon layer is formed. + The diodes in the region are forward biased (and therefore non-blocking). As a result, the voltage seen by the thick metal layer 100 is the voltage applied to the p-type silicon layer 4 at the edge of the wafer minus the forward voltage drop of the diode, V F (It is of the order of 0.6V). + For the regions, the contact is ohmic and therefore has no effect on the voltage distribution (considering the low current density involved in the anodic reaction). As a result, the anodic oxide / hydroxide regions formed on the silicon layer 4 have approximately equal porosity, regardless of whether they are formed on regions with p-type polarity or on regions with n-type polarity.

[0134] As described above, because embodiments of the present invention employ regions of anodic oxide / hydroxide whose porosity can be set to a desired value during fabrication, it becomes possible to create different regions with different effective dielectric constants (porosity) on a common substrate (wafer). Fig. 9 In the modified electro-optical product 31 shown, the silicon layer 4 may be formed to have a low-doped p-type, and anodized control diodes 40a, 40b as NP diodes may be arranged at n + Area 4a / p + At the outer edge of region 4e. Anodized control diodes 40a, 40b may be used to enable the creation of regions of different porosity.

[0135] The anodized control diodes 40a, 40b can be formed by means of two additional implantation steps. One of these implantation steps implants p-type dopants into the n-type contacts, respectively. + Regions 4a and p + Another of these implantation steps implants n-type dopants into an adjacent small area located towards the outside of the structure.

[0136] Subsequently, during the anodization process, an anode voltage is applied to the silicon layer 4, and the voltage experienced by the thick metal layer 100 corresponds to the voltage of the anode power supply (Vanode) minus the reverse bias voltage (Vz) of the anodization control diodes 40a, 40b described above. As a result, by appropriately adjusting the properties (particularly Vz) of the anodization control diodes 40a, 40b disposed at different locations on the wafer, different voltages can be applied to different locations on a common substrate, thereby producing different levels of porosity at different locations, while still using the common voltage Vanode applied to the silicon layer 4. The properties (e.g., Vz) of the anodization control diodes 40a, 40b can be set as desired by appropriately adjusting the doping of the NP diodes 40a, 40b. In another embodiment, the anodization control diodes 40a, 40b can be designed to be substantially identical, and different anode voltages configured to cause different anodization levels are applied to different locations on the common substrate.

[0137] Additional variants

[0138] Although the present invention has been described above with reference to certain specific embodiments, it should be understood that the present invention is not limited to the particularities of the specific embodiments. Many changes, modifications and developments can be made in the above embodiments within the scope of the appended claims.

Claims

1. An electronic product (1, 300A, 300B, 300C), comprising: A silicon-on-insulator substrate, the silicon-on-insulator substrate comprising a base substrate (2, 302), an insulating layer (3, 304) on the base substrate (2, 302), and a silicon layer (4, 306) on the insulating layer (3, 304); a porous layer (10, 310) of anodic oxide or anodic hydroxide formed on the silicon layer (4, 306); a metal layer (14 / 15, 314) formed on the porous layer (10, 310), the metal layer providing at least one electrical transmission line; as well as an anodization control device formed in the silicon layer (4, 306), the anodization control device being configured to control the porosity of the porous layer (10, 310) in a region below the metal layer (14 / 15, 314), wherein the porous layer (10, 310) comprises a first porous region (324) having a first porosity and a second porous region (326) having a second porosity, and The porosity of the porous layer (10, 310) in a region below the metal layer (14 / 15, 314) is configured based on a desired speed of an electrical signal in the at least one electrical transmission line.

2. The electronic product (1, 300A, 300B, 300C) according to claim 1, wherein: The pores in the porous layer (10, 310) are tubular in shape.

3. The electronic product (1, 300A, 300B, 300C) according to claim 1 or 2, wherein: The porosity of the porous layer (10, 310) in the region below the metal layer (14 / 15, 314) ranges from 50% up to 91%.

4. The electronic product (300A, 300B, 300C) according to claim 1, further comprising: a metal contact (316) located on a surface above the porous layer (310); as well as A conductive path interconnects the metal contact (316) to the anodization control device, wherein the metal contact (316) includes a through-hole conductor (312a) extending through the porous layer (310).

5. The electronic product (300A, 300B, 300C) according to claim 1, wherein: The anodization control device includes a diode or a resistor.

6. The electronic product (300A, 300B, 300C) according to any one of claims 1 to 5, wherein: The metal layer (314) includes a signal conductor line, whereby the at least one electrical transmission line includes a microstrip line.

7. The electronic product (300A, 300B, 300C) according to any one of claims 1 to 5, wherein: The metal layer (314) includes a signal conductor line located between two ground conductor lines, whereby the at least one electrical transmission line includes a coplanar waveguide.

8. The electronic product (300A, 300B, 300C) according to any one of claims 1 to 5, wherein: The metal layer (314) includes differential signal conductor lines, whereby the at least one electrical transmission line includes a differential microstrip conductor.

9. The electronic product (1, 300A, 300B, 300C) according to any one of claims 1 to 8, wherein: The at least one electrical transmission line includes a first electrical transmission line and a second electrical transmission line, and wherein the first electrical transmission line is coupled to ground via the first porous region (324) and the second electrical transmission line is coupled to ground via the second porous region (326).

10. The electronic product (1, 300A, 300B, 300C) according to any one of claims 1 to 9, further comprising: an optical waveguide formed in the silicon layer (4, 304), The porosity of the porous layer (10, 310) in the region below the metal layer (14 / 15, 314) is configured so that the speed of the electrical signal approaches the speed at which the optical signal propagates in the optical waveguide.

11. The electronic product (1, 300A, 300B, 300C) according to any one of claims 1 to 10, wherein: The porous layer (10, 310) includes a region made of anodized aluminum oxide (AAO).

12. A method for manufacturing an electronic product, the method comprising: forming a first p-type region (308a) and a first n-type region (308b) in a silicon layer (306) of a silicon-on-insulator substrate, the silicon-on-insulator substrate comprising a base substrate (302), an insulating layer (304) on the base substrate, and the silicon layer (306) on the insulating layer (304), the first p-type region (308a) and the first n-type region (308b) forming a first anodized control diode; forming a second p-type region (308c) and a second n-type region (308d) in the silicon layer (306), wherein the second p-type region (308c) and the second n-type region (308d) form a second anodized control diode; forming a metal layer on the silicon layer (306); anodizing the metal layer using the first anodizing control diode and the second anodizing control diode to form a porous layer (310) of an anodic oxide or an anodic hydroxide, wherein anodizing the metal layer comprises: controlling the first anodizing control diode and the second anodizing control diode so that the formed porous layer (310) comprises a first porous region (324) having a first porosity and a second porous region (326) having a second porosity; and A metal layer (314) is formed on the porous layer (310), and the metal layer (314) provides at least one electrical transmission line.

13. The method according to claim 12, comprising: A common voltage is applied to the first anodization control diode and the second anodization control diode to anodize the metal layer to form the porous layer (310).

14. The method according to claim 12 or 13, wherein: The porosity of the porous layer (310) in a region below the metal layer (314) is configured based on a desired speed of an electrical signal in the at least one electrical transmission line.