Processing product manufacturing method and adhesive laminate

By using thermally expandable adhesive sheets and laminates of adhesive sheets, and separating them by heating at the thermal expansion initiation temperature, the problems of cumbersome operation and low productivity of processed objects in electronic component manufacturing are solved, and efficient separation and transfer of processed products are achieved.

CN111837219BActive Publication Date: 2024-11-01LINTEC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980018435.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-03-20
Filing Date
2019-03-04
Publication Date
2024-11-01
Estimated Expiration
2039-03-04

AI Technical Summary

Technical Problem

In the manufacturing process of electronic components, etc., when using adhesive sheets to temporarily fix the workpiece for cutting and grinding, the operation is cumbersome and the productivity is low, making it difficult to efficiently separate and transfer the workpiece.

Method used

By employing thermally expandable adhesive sheets and laminates thereof, and heating the adhesive sheets above the thermal expansion initiation temperature of the thermally expandable particles, the adhesive sheets are separated at the interface, thereby enabling easy separation and transfer of the processed object and simplifying the operation process.

Benefits of technology

It enables efficient separation and transfer of processed materials, simplifies the operation process, and improves production efficiency and product productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111837219B_ABST
    Figure CN111837219B_ABST
Patent Text Reader

Abstract

The present invention provides a method for manufacturing a processed product, which is a method for manufacturing a processed product using an adhesive laminate, wherein the adhesive laminate comprises a heat-expandable adhesive sheet (I) and an adhesive sheet (II), wherein the heat-expandable adhesive sheet (I) has a substrate (Y1) and an adhesive layer (X1), and contains heat-expandable particles in any layer, and the adhesive sheet (II) has a substrate (Y2) and an adhesive layer (X2), and the adhesive laminate is formed by directly laminating the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II), and the method for manufacturing a processed product sequentially comprises: steps (1) of adhering the surface of the adhesive layer (X1) of the adhesive laminate to a support, and adhering a processing object to the adhesive layer (X1) The surface of the adhesive layer (X2) of the adhesive laminate; step (2) performing one or more processing on the processing object; step (3) separating the adhesive laminate at the interface P between the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) while maintaining the state of adhering the processing object to the surface of the adhesive layer (X2) of the adhesive laminate by heating at a temperature above the thermal expansion starting temperature (t) of the heat-expandable particles; and further performing step (4) in step (2) or after step (3), wherein the surface of the processing object opposite to the adhesive surface of the adhesive layer (X2) is subjected to at least one of cutting and grinding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a processed product subjected to at least one of cutting and grinding, and an adhesive laminate used in the production method. Background Art

[0002] Pressure-sensitive adhesive sheets are used not only for semi-permanent fixing of components but also for temporary fixing of target components during processing and inspection of building materials, interior materials, electronic parts, and the like.

[0003] Such a PSA sheet for temporary fixing is required to have both adhesiveness during use and releasability after use.

[0004] For example, Patent Document 1 discloses a heat-peelable pressure-sensitive adhesive sheet for temporary fixing when cutting electronic components, wherein a heat-expandable pressure-sensitive adhesive layer containing heat-expandable microspheres is provided on at least one surface of a substrate.

[0005] In this heat-peelable pressure-sensitive adhesive sheet, the maximum particle size of the heat-expandable microspheres is adjusted relative to the thickness of the heat-expandable pressure-sensitive adhesive layer, and the center line average roughness of the surface of the heat-expandable pressure-sensitive adhesive layer before heating is adjusted to 0.4 μm or less.

[0006] Patent document 1 records the following purport: the heat-peelable adhesive sheet can ensure the contact area with the adherend when the electronic component is cut, so that the adhesiveness that can prevent the chip from flying and other poor bonding situations can be exerted; on the other hand, after use, the heat-expandable microspheres are heated to expand and the contact area with the adherend is reduced, thereby making it easy to peel off.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent No. 3594853 Summary of the invention

[0010] Problems to be solved by the invention

[0011] In the processing step using the adhesive sheet described in Patent Document 1, an object to be processed (hereinafter also referred to as "processing object") is temporarily fixed using the adhesive sheet, and after a given processing is performed on the processing object, the processing object is separated from the adhesive sheet.

[0012] However, in particular, in the production of electronic components and the like, a plurality of processing steps including at least one of a step of cutting and a step of grinding the object to be processed are often required.

[0013] Therefore, for example, after the object temporarily fixed to the adhesive sheet has been subjected to at least one of a cutting process and a grinding process, the object is sometimes separated from the adhesive sheet and the separated object is attached to a new adhesive sheet for the next process.

[0014] In addition, after a processing step other than a cutting step and a grinding step is performed on an object temporarily fixed to an adhesive sheet, the object is sometimes separated from the adhesive sheet, and the separated object is attached to a new adhesive sheet, and at least one of the cutting step and the grinding step is performed on the object.

[0015] However, when manufacturing a product through the above-mentioned steps, not only the operation becomes complicated, but also the productivity of the product is reduced. Therefore, it is desired to establish a method that can suppress the complicatedness of the operation and improve the productivity of the product.

[0016] The object of the present invention is to provide a method for manufacturing a processed product that has been subjected to at least one of cutting and grinding, and an adhesive laminate for manufacturing a processed product that has been subjected to at least one of cutting and grinding. The manufacturing method is as follows: after fixing an object to be processed to a support and subjecting the object to processing to processing, the object to be processed can be easily separated from the support with a small force, and the object to be processed after being separated from the support can be provided for processing in the next step in a state in which the object to be processed is adhered to an adhesive sheet, and the object to be processed can be subjected to at least one of cutting and grinding at least at any time before and after the object to be processed is separated from the support.

[0017] Solution to the problem

[0018] The present inventors have found that the above-mentioned problems can be solved by using the following adhesive laminate to produce a processed product subjected to at least one of cutting and grinding, wherein the adhesive laminate comprises a heat-expandable adhesive sheet (I), and an adhesive sheet (II), wherein the heat-expandable adhesive sheet (I) has a substrate and an adhesive layer and includes a layer containing heat-expandable particles in any layer, and the adhesive sheet (II) has a substrate and an adhesive layer, and the adhesive laminate is formed by directly laminating the substrates of the adhesive sheet (I) and the adhesive sheet (II).

[0019] That is, the present invention relates to the following [1] to

[17] .

[0020] [1] A method for producing a processed product, the method comprising using an adhesive laminate to produce a processed product subjected to at least one of cutting and grinding.

[0021] The adhesive laminate comprises a heat-expandable adhesive sheet (I), and an adhesive sheet (II), wherein the heat-expandable adhesive sheet (I) comprises a substrate (Y1) and an adhesive layer (X1), and contains heat-expandable particles having a thermal expansion starting temperature (t) in any layer, and the adhesive sheet (II) comprises a substrate (Y2) and an adhesive layer (X2), and the adhesive laminate is formed by directly laminating the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II),

[0022] The method for producing the processed product comprises the following steps (1) to (3) in sequence:

[0023] Step (1): a step of laminating the surface of the adhesive layer (X1) of the adhesive laminate to a support, and laminating an object to be processed to the surface of the adhesive layer (X2) of the adhesive laminate;

[0024] Step (2): a step of performing one or more processes on the object to be processed;

[0025] Step (3): a step of separating the adhesive laminate at an interface P between the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) while maintaining the state where the object to be processed is adhered to the surface of the adhesive layer (X2) of the adhesive laminate by heating at a temperature not lower than the thermal expansion starting temperature (t) of the thermally expandable particles,

[0026] The method for producing the processed product further comprises the following step (4):

[0027] Step (4): a step of performing at least one of cutting and grinding on the surface of the object to be processed which is opposite to the surface to which the adhesive layer (X2) is attached,

[0028] The step (4) is carried out in at least any one of the following (X) and (Y),

[0029] (X): one or more of the above-mentioned processes is carried out in the above-mentioned step (2),

[0030] (Y): carried out after the above step (3).

[0031] [2] The production method described in [1] above, wherein the thermal expansion starting temperature (t) of the thermally expandable particles is 60 to 270°C.

[0032] [3] The production method according to [1] or [2], wherein the substrate (Y1) of the pressure-sensitive adhesive sheet (I) has a heat-expandable substrate layer (Y1-1) containing the heat-expandable particles.

[0033] [4] The production method according to [3] above, wherein the substrate (Y1) of the pressure-sensitive adhesive sheet (I) comprises a heat-expandable substrate layer (Y1-1) and a non-heat-expandable substrate layer (Y1-2).

[0034] [5] The production method described in [3] or [4] above, wherein the heat-expandable substrate layer (Y1-1) of the substrate (Y1) of the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) are directly laminated together.

[0035] [6] The production method described in any one of [3] to [5] above, wherein

[0036] The pressure-sensitive adhesive sheet (I) has a structure in which a substrate (Y1) is sandwiched between a first pressure-sensitive adhesive layer (X11) and a second pressure-sensitive adhesive layer (X12).

[0037] It has a structure in which the first adhesive layer (X11) of the adhesive sheet (I) and the base material (Y2) of the adhesive sheet (II) are directly laminated,

[0038] The surface of the second pressure-sensitive adhesive layer (X12) of the pressure-sensitive adhesive sheet (I) is the surface to be bonded to the support.

[0039] [7] The production method described in [1] or [2] above, wherein:

[0040] The first adhesive layer (X11) is a heat-expandable adhesive layer containing the heat-expandable particles.

[0041] The second adhesive layer (X12) is a non-heat-expandable adhesive layer.

[0042] It has a structure in which the first adhesive layer (X11) of the adhesive sheet (I) and the base material (Y2) of the adhesive sheet (II) are directly laminated,

[0043] The surface of the second pressure-sensitive adhesive layer (X12) of the pressure-sensitive adhesive sheet (I) is the surface to be bonded to the support.

[0044] [8] The production method according to [6] or [7], wherein the surface of the substrate (Y1) on which the first pressure-sensitive adhesive layer (X11) is laminated is a surface subjected to an adhesion-facilitating treatment.

[0045] [9] The production method according to any one of [1] to [8] above, wherein the surface of the substrate (Y2) on the side on which the pressure-sensitive adhesive sheet (I) is laminated is a surface subjected to a release treatment.

[0046]

[10] The production method according to any one of [1] to [9] above, wherein the pressure-sensitive adhesive sheet (II) has an intermediate layer (Z2) between the substrate (Y2) and the pressure-sensitive adhesive layer (X2).

[0047]

[11] The production method according to any one of [1] to

[10] above, wherein the pressure-sensitive adhesive layer (X2) of the pressure-sensitive adhesive sheet (II) is an energy-beam-curable pressure-sensitive adhesive layer.

[0048]

[12] The production method according to any one of [1] to

[11] above, wherein the pressure-sensitive adhesive sheet (II) satisfies at least one of the following requirements (α) to (γ).

[0049] Requirement (α): The Young's modulus of the base material (Y2) is 1.0 MPa or more;

[0050] Requirement (β): The thickness of the substrate (Y2) is 5 μm or more;

[0051] Requirement (γ): The storage elastic modulus G′ (23° C.) of the pressure-sensitive adhesive layer (X2) is 0.1 MPa or more.

[0052]

[13] The manufacturing method according to any one of [1] to

[12] above, wherein the object to be processed is a semiconductor wafer,

[0053] The one or more processes in the step (2) include the following step (2-A),

[0054] Step (2-A): a step of forming a modified region serving as a division starting point on the semiconductor wafer,

[0055] The step (4) is the following step (4-A),

[0056] Step (4-A): a step of grinding the surface of the semiconductor wafer opposite to the surface to be bonded to the adhesive layer (X2).

[0057] The step (4-A) is carried out in at least any one of the following (XA) or (YA),

[0058] (XA): one or more of the above-mentioned processes are performed after the above-mentioned step (2-A),

[0059] (YA): carried out after the step (3).

[0060]

[14] The production method described in any one of [1] to

[12] above, wherein

[0061] The object to be processed is a semiconductor chip,

[0062] The one or more processing steps in step (2) include the following step (2-B),

[0063] Step (2-B): a step of covering the semiconductor chip and the peripheral portion of the semiconductor chip in the bonding surface of the adhesive layer (X2) with a sealing material, and curing the sealing material to obtain a cured sealed body in which the semiconductor chip is sealed with the cured sealing material,

[0064] The step (4) is carried out in at least one of the following (XB) and (YB),

[0065] (XB): one or more of the above-mentioned processes are performed after the above-mentioned step (2-B),

[0066] (YB): carried out after the step (3).

[0067]

[15] The production method described in any one of [1] to

[12] above, wherein:

[0068] The object to be processed is a semiconductor wafer having a modified region as a division starting point,

[0069] The step (4) is the following step (4-A),

[0070] Step (4-A): a step of grinding the surface of the semiconductor wafer opposite to the bonding surface of the pressure-sensitive adhesive layer (X2).

[0071]

[16] The production method described in any one of [1] to

[12] above, wherein:

[0072] The object to be processed is a semiconductor wafer having a cut groove as a starting point for division,

[0073] The step (1) is the following step (1-C), the step (4) is the following step (4-C),

[0074] Step (1-C): a step of attaching the surface of the adhesive layer (X1) of the adhesive laminate to a support, and attaching the surface of the semiconductor wafer having the cut groove to the surface of the adhesive layer (X2) of the adhesive laminate,

[0075] Step (4-C): a step of grinding the surface of the semiconductor wafer opposite to the surface to be bonded to the adhesive layer (X2).

[0076]

[17] An adhesive laminate for use in manufacturing a processed product subjected to at least one of cutting and grinding,

[0077] The adhesive laminate comprises a heat-expandable adhesive sheet (I) and an adhesive sheet (II), wherein the heat-expandable adhesive sheet (I) has a substrate (Y1) and an adhesive layer (X1) and contains heat-expandable particles in any layer, and the adhesive sheet (II) has a substrate (Y2) and an adhesive layer (X2), and the adhesive laminate is formed by directly laminating the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II).

[0078] Effects of the Invention

[0079] According to the present invention, a method for manufacturing a processed product that has been subjected to at least one of cutting and grinding, and an adhesive laminate for manufacturing a processed product that has been subjected to at least one of cutting and grinding, can be provided. The manufacturing method is as follows: after fixing an object to be processed to a support and subjecting the object to processing to processing, the object to be processed can be easily separated from the support with a small force, and the object to be processed after being separated from the support can be provided for processing in the next step in a state in which the object to be processed is adhered to an adhesive sheet, and the object to be processed can be subjected to at least one of cutting and grinding at least at any time before and after the object to be processed is separated from the support. BRIEF DESCRIPTION OF THE DRAWINGS

[0080] Figure 1 1 is a schematic cross-sectional view of the pressure-sensitive adhesive laminate showing the structure of the pressure-sensitive adhesive laminate of the first embodiment used in the production method of the present invention.

[0081] Figure 2 1 is a schematic cross-sectional view of a pressure-sensitive adhesive laminate showing the structure of the pressure-sensitive adhesive laminate of the second embodiment used in the production method of the present invention.

[0082] Figure 3 1 is a schematic cross-sectional view of a pressure-sensitive adhesive laminate showing the structure of the pressure-sensitive adhesive laminate of the third embodiment used in the production method of the present invention.

[0083] Figure 4 This is a schematic diagram showing an example of the production method of the present invention.

[0084] Figure 5 This is a schematic diagram showing another example of the production method of the present invention.

[0085] Explanation of symbols

[0086] 1a, 1b, 1c, 1d, 2 Adhesive laminate

[0087] (I) Adhesive sheet

[0088] (X1) Adhesive layer

[0089] (X11) 1st adhesive layer

[0090] (X12) Second adhesive layer

[0091] (Y1) Base material

[0092] (Y1-1) Heat-expandable base material layer

[0093] (Y1-2) Non-thermal expansion base material layer

[0094] (II) Adhesive sheet

[0095] (X2) Adhesive layer

[0096] (Z2) Middle layer

[0097] (Y2) Base material

[0098] 50 Support

[0099] 60, 70 Processing object

[0100] 61 Curing seal

[0101] 61a Monolithic solidification of the cured seal

[0102] 71 Modified area

[0103] 72 Gap DETAILED DESCRIPTION

[0104] In this specification, whether a "layer" is a "non-heat-expandable layer" or a "heat-expandable layer" is determined in the following manner.

[0105] The layer as a target is heated for 3 minutes at the expansion starting temperature (t) of the heat-expandable particles contained in the layer containing heat-expandable particles. When the volume change rate calculated according to the following formula is less than 5%, the layer is judged to be a "non-heat-expandable layer", and when it is 5% or more, the layer is judged to be a "heat-expandable layer".

[0106] Volume change rate (%) = {(volume of the layer after heat treatment - volume of the layer before heat treatment) / volume of the layer before heat treatment} × 100

[0107] In addition, the layer which does not contain heat-expandable particles is a "non-heat-expandable layer".

[0108] In the present specification, the "active ingredient" refers to the ingredients contained in the target composition excluding the diluent solvent.

[0109] In this specification, the weight average molecular weight (Mw) refers to a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene, and specifically, a value measured according to the method described in Examples.

[0110] In this specification, for example, "(meth)acrylic acid" means both "acrylic acid" and "methacrylic acid", and the same applies to other similar terms.

[0111] In this specification, for a preferred numerical range (e.g., a range of content, etc.), the lower limit and upper limit values ​​described in a stepwise manner can be independently combined. For example, according to a description such as "preferably 10 to 90, more preferably 30 to 60", "preferable lower limit (10)" and "more preferably upper limit (60)" can be combined to obtain "10 to 60".

[0112] [Processing product manufacturing method]

[0113] The method for producing a processed product of the present invention is a method for producing a processed product subjected to at least one of cutting and grinding using an adhesive laminate.

[0114] The adhesive laminate comprises a heat-expandable adhesive sheet (I), and an adhesive sheet (II), wherein the heat-expandable adhesive sheet (I) comprises a substrate (Y1) and an adhesive layer (X1), and contains heat-expandable particles having a thermal expansion starting temperature (t) in any layer, and the adhesive sheet (II) comprises a substrate (Y2) and an adhesive layer (X2), and the adhesive laminate is formed by directly laminating the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II),

[0115] The method for producing the processed product comprises the following steps (1) to (3) in sequence:

[0116] Step (1): a step of laminating the surface of the adhesive layer (X1) of the adhesive laminate to a support, and laminating an object to be processed to the surface of the adhesive layer (X2) of the adhesive laminate;

[0117] Step (2): a step of performing one or more processes on the object to be processed;

[0118] Step (3): a step of separating the adhesive laminate at an interface P between the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) while maintaining the state where the object to be processed is adhered to the surface of the adhesive layer (X2) of the adhesive laminate by heating at a temperature not lower than the thermal expansion starting temperature (t) of the thermally expandable particles,

[0119] The method for producing the processed product further comprises the following step (4):

[0120] Step (4): a step of performing at least one of cutting and grinding on the surface of the object to be processed which is opposite to the surface to which the adhesive layer (X2) is attached,

[0121] The step (4) is carried out in at least any one of the following (X) and (Y),

[0122] (X): one or more of the above-mentioned processes is carried out in the above-mentioned step (2),

[0123] (Y): carried out after the above step (3).

[0124] Hereinafter, the pressure-sensitive adhesive laminate used in the production method of the present invention will be described, and then each production step including steps (1) to (4) will be described.

[0125] [Structure of Adhesive Laminated Body]

[0126] The adhesive laminate used in the production method of the present invention comprises a heat-expandable adhesive sheet (I) and an adhesive sheet (II), wherein the heat-expandable adhesive sheet (I) has a substrate (Y1) and an adhesive layer (X1), and any layer contains heat-expandable particles, and the adhesive sheet (II) has a substrate (Y2) and an adhesive layer (X2). The adhesive laminate is formed by directly laminating the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II), and is used to fix the object to be processed to a support when a given process is performed on the object to be processed.

[0127] In this specification, the given processing refers to the processing of step (2) in the manufacturing method of the present invention. It should be noted that in the present invention, as one of the one or more processing in step (2), step (4) is sometimes implemented. Therefore, the given processing may also include step (4) in the manufacturing method of the present invention.

[0128] In the adhesive laminate used by the manufacturing method of the present invention, the surface of the adhesive layer (X1) of the adhesive sheet (I) is a side of the pasting support. When the adhesive sheet (I) has the first adhesive layer (X11) and the second adhesive layer (X12), the surface of the second adhesive layer (X12) is a side of the pasting support, and the surface of the first adhesive layer (X11) is a side stacked on the substrate (Y2) side of the adhesive sheet (II). In addition, the surface of the adhesive layer (X2) of the adhesive sheet (II) is a side of the pasting processing object.

[0129] Therefore, the adhesive laminate used in the manufacturing method of the present invention can be separated at the interface P between the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) by heat treatment at a temperature higher than the expansion starting temperature (t) of the heat-expandable particles. In the following description, this heat treatment is also referred to as "separation heat treatment".

[0130] Figures 1 to 3Schematic cross-sectional views respectively show the structures of the pressure-sensitive adhesive laminated bodies of the first embodiment, the second embodiment, and the third embodiment used in the production method of the present invention.

[0131] <Adhesive laminate of the first aspect>

[0132] Examples of the first embodiment of the adhesive laminate used in the production method of the present invention include: Figure 1 (a) and (b) show pressure-sensitive adhesive laminates 1a and 1b.

[0133] The adhesive laminates 1a and 1b have the following structure: they include an adhesive sheet (I) and an adhesive sheet (II), wherein the adhesive sheet (I) has a substrate (Y1) and an adhesive layer (X1), and the adhesive sheet (II) has a substrate (Y2) and an adhesive layer (X2), and the substrate (Y1) of the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) are directly laminated together.

[0134] In the pressure-sensitive adhesive laminate used in the production method of the present invention, any layer of the pressure-sensitive adhesive sheet (I) is a layer containing heat-expandable particles so that separation at the interface P can be achieved by heat treatment for separation.

[0135] The adhesive laminate used in the manufacturing method of the present invention is subjected to a heat treatment for separation, and the heat-expandable particles expand, thereby generating irregularities on the surface of the layer containing the heat-expandable particles. As a result, the contact area between the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) is reduced.

[0136] As a result, after the object to be processed is adhered to the surface of the adhesive layer (X2) of the adhesive sheet (II) and subjected to a given processing, it is separated at the interface P between the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II), thereby obtaining the object to be processed in a state of being adhered to the adhesive sheet (II) and subjected to a given processing.

[0137] Therefore, according to the manufacturing method of the present invention, the processing object can be fixed to the support body by the above-mentioned adhesive laminate to implement a given processing, and the processing object that has been subjected to the given processing can be easily separated from the support body with a small force. Moreover, the processing object separated from the support body can be directly provided to the next step in a state of being attached to the adhesive sheet (II).

[0138] Therefore, it is no longer necessary to perform an operation of attaching the separated object to be processed, which has been subjected to a predetermined process, to a new pressure-sensitive adhesive sheet, thereby improving operability and product productivity.

[0139] In the first aspect of the present invention, it is preferred that the substrate (Y1) is Figure 1The pressure-sensitive adhesive laminates 1a and 1b shown have a heat-expandable base material layer (Y1-1) containing heat-expandable particles.

[0140] It should be noted that the substrate (Y1) can be Figure 1 The adhesive laminate 1a shown in (a) has a single-layer structure of only a heat-expandable substrate layer (Y1-1) containing heat-expandable particles. Figure 1 Like the pressure-sensitive adhesive laminate 1b shown in (b), the pressure-sensitive adhesive laminate has a multilayer structure of a heat-expandable base layer (Y1-1) and a non-heat-expandable base layer (Y1-2).

[0141] Figure 1 The adhesive laminate 1a shown in (a) is subjected to separation heat treatment to expand the heat-expandable particles contained in the heat-expandable substrate layer (Y1-1) constituting the substrate (Y1), thereby generating irregularities on the surface of the substrate (Y1) on the side of the adhesive sheet (II), and reducing the contact area between the substrate (Y1) and the substrate (Y2) of the adhesive sheet (II).

[0142] On the other hand, since the adhesive layer (X1) of the adhesive laminate 1a is attached to the support, it is not easy to form unevenness on the surface of the adhesive layer (X1) side of the substrate (Y1). Thus, unevenness can be efficiently formed on the surface of the substrate (Y1) in contact with the adhesive sheet (II).

[0143] As a result, the pressure-sensitive adhesive laminate 1a can be easily separated with a slight force at the interface P between the substrate (Y1) of the pressure-sensitive adhesive sheet (I) and the substrate (Y2) of the pressure-sensitive adhesive sheet (II).

[0144] In addition, by forming the adhesive layer (X1) of the adhesive laminate 1a from an adhesive composition having improved adhesive strength to a support, it is also possible to design the laminate so that separation at the interface P can be facilitated.

[0145] in addition, Figure 1 The adhesive laminate 1b shown in (b) is subjected to separation heat treatment to expand the heat-expandable particles contained in the heat-expandable substrate layer (Y1-1) constituting the substrate (Y1), thereby generating irregularities on the surface of the substrate (Y1) on the adhesive sheet (II) side, and reducing the contact area between the substrate (Y1) and the substrate (Y2) of the adhesive sheet (II).

[0146] On the other hand, the non-heat-expandable substrate layer (Y1-2) constituting the substrate (Y1) has a small degree of expansion caused by heat treatment, so it is not easy to form unevenness on the surface of the adhesive layer (X1) side of the substrate (Y1). Thus, unevenness can be efficiently formed on the surface of the adhesive sheet (II) side of the substrate (Y1).

[0147] As a result, the pressure-sensitive adhesive laminate 1 b can be easily separated with a slight force at the interface P between the substrate ( Y1 ) of the pressure-sensitive adhesive sheet (I) and the substrate ( Y2 ) of the pressure-sensitive adhesive sheet (II).

[0148] As in the case of the pressure-sensitive adhesive laminate 1a, the pressure-sensitive adhesive layer (X1) of the pressure-sensitive adhesive laminate 1b may be designed to be more easily separable at the interface P by forming the pressure-sensitive adhesive layer (X1) of the pressure-sensitive adhesive laminate 1b from a pressure-sensitive adhesive composition having improved adhesive strength to a support.

[0149] From the above viewpoints, in the first embodiment of the present invention, Figure 1 As in the pressure-sensitive adhesive laminate 1b shown in (b), the substrate (Y1) preferably has a heat-expandable substrate layer (Y1-1) on one surface side and a non-heat-expandable substrate layer (Y1-2) on the other surface side.

[0150] In addition, in the first embodiment of the present invention, from the viewpoint of making an adhesive laminate that can be easily separated at the interface P with a small force, it is preferred that the adhesive laminates 1a, 1b have a structure in which the heat-expandable substrate layer (Y1-1) of the substrate (Y1) possessed by the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) are directly laminated.

[0151] <Adhesive laminate of the second embodiment>

[0152] Examples of the second embodiment of the adhesive laminate used in the production method of the present invention include: Figure 2 (a) and (b) are adhesive laminates 1c and 1d.

[0153] The adhesive laminates 1c and 1d have a structure in which the first adhesive layer (X11) of the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) are directly laminated, and the adhesive sheet (I) has a structure in which the first adhesive layer (X11) and the second adhesive layer (X12) sandwich the substrate (Y1).

[0154] In addition, in the pressure-sensitive adhesive laminates 1c and 1d, the surface of the second pressure-sensitive adhesive layer (X12) is the surface to be bonded to the support.

[0155] In the second embodiment of the present invention, Figure 2 As in the pressure-sensitive adhesive laminates 1c and 1d shown in the figure, the substrate (Y1) preferably has a heat-expandable substrate layer (Y1-1) containing heat-expandable particles.

[0156] It should be noted that the substrate (Y1) can be Figure 2 The adhesive laminate 1c shown in (a) has a single-layer structure of only a heat-expandable substrate layer (Y1-1) containing heat-expandable particles. Figure 2 Like the pressure-sensitive adhesive laminate 1d shown in (b), the pressure-sensitive adhesive laminate has a multilayer structure of a heat-expandable base layer (Y1-1) and a non-heat-expandable base layer (Y1-2).

[0157] In addition, when the substrate (Y1) has a multilayer structure having a heat-expandable substrate layer (Y1-1) and a non-heat-expandable substrate layer (Y1-2), it is preferred that the heat-expandable substrate layer (Y1-1) is arranged on the adhesive sheet (II) side and the non-heat-expandable substrate layer (Y1-2) is arranged on the second adhesive layer (X12) side.

[0158] Figure 2 The adhesive laminate 1c shown in (a) is separated by heat treatment to expand the heat-expandable particles in the heat-expandable substrate layer (Y1-1) constituting the substrate (Y1), and the surface of the first adhesive layer (X11) of the substrate (Y1) is uneven. In addition, due to the unevenness generated on the surface of the substrate (Y1), the first adhesive layer (X11) is lifted up, and unevenness is also formed on the surface of the adhesive sheet (II) of the first adhesive layer (X11). Thus, the contact area between the first adhesive layer (X11) and the substrate (Y2) of the adhesive sheet (II) is reduced.

[0159] On the other hand, since the second adhesive layer (X12) is attached to the support, it is not easy to form unevenness on the surface of the second adhesive layer (X12) side of the substrate (Y1). Therefore, unevenness can be efficiently formed on the surface of the first adhesive layer (X11) side of the substrate (Y1), and unevenness can be efficiently formed on the surface of the adhesive sheet (II) side of the first adhesive layer (X11).

[0160] As a result, the pressure-sensitive adhesive laminate 1c can be easily separated with a slight force at the interface P between the first pressure-sensitive adhesive layer (X11) of the pressure-sensitive adhesive sheet (I) and the substrate (Y2) of the pressure-sensitive adhesive sheet (II).

[0161] It should be noted that by forming the second adhesive layer (X12) of the adhesive laminate 1c from an adhesive composition having improved adhesive strength to a support, it is also possible to design the laminate so that separation at the interface P can be facilitated.

[0162] in addition, Figure 2 The adhesive laminate 1d shown in (b) is separated by heat treatment to expand the heat-expandable particles contained in the heat-expandable substrate layer (Y1-1) constituting the substrate (Y1), and the surface of the first adhesive layer (X11) on the substrate (Y1) is uneven. In addition, due to the unevenness generated on the surface of the substrate (Y1), the first adhesive layer (X11) is also lifted up, and unevenness is also formed on the surface of the adhesive sheet (II) on the first adhesive layer (X11). Thus, the contact area between the first adhesive layer (X11) and the substrate (Y2) of the adhesive sheet (II) is reduced.

[0163] On the other hand, the non-heat-expandable substrate layer (Y1-2) constituting the substrate (Y1) has a small degree of expansion caused by heat treatment, so it is not easy to form unevenness on the surface of the second adhesive layer (X12) side of the substrate (Y1). Thus, unevenness can be efficiently formed on the surface of the first adhesive layer (X11) side of the substrate (Y1).

[0164] As a result, the pressure-sensitive adhesive laminate 1d can be easily separated with a slight force at the interface P between the substrate (Y1) of the pressure-sensitive adhesive sheet (I) and the substrate (Y2) of the pressure-sensitive adhesive sheet (II).

[0165] As in the case of the adhesive laminate 1c, the second adhesive layer (X12) of the adhesive laminate 1d may be formed from an adhesive composition having improved adhesiveness to a support, so that separation at the interface P can be facilitated.

[0166] Here, in the second embodiment of the present invention, from the viewpoint of making an adhesive laminate that can be easily separated at the interface P with a smaller force, the adhesive laminates 1c and 1d are preferably a structure in which the heat-expandable substrate layer (Y1-1) of the substrate (Y1) of the adhesive sheet (I) and the first adhesive layer (X11) are directly laminated. In this case, it is more preferred to further laminate the first adhesive layer (X11) and the substrate (Y2) of the resin film forming sheet (II) directly.

[0167] <Adhesive laminate of the third embodiment>

[0168] The first embodiment of the pressure-sensitive adhesive laminates 1a and 1b and the second embodiment of the pressure-sensitive adhesive laminates 1c and 1d used in the production method of the present invention all include a layer containing heat-expandable particles as one of the layers constituting the substrate (Y1).

[0169] On the other hand, the third embodiment of the adhesive laminate used in the manufacturing method of the present invention may be a structure in which the above-mentioned heat-expandable adhesive layer containing heat-expandable particles is provided on the surface on the interface P side of the substrate (Y1) of the adhesive sheet (I), and a non-heat-expandable adhesive layer is provided on the other surface of the substrate (Y1).

[0170] As such a method, for example, Figure 3The adhesive laminate 2 shown has the following structure: the adhesive sheet (I) has a structure in which the substrate (Y1) is sandwiched by the first adhesive layer (X11) and the second adhesive layer (X12), the first adhesive layer (X11) is a heat-expandable adhesive layer containing heat-expandable particles, the second adhesive layer (X12) is a non-heat-expandable adhesive layer, and the first adhesive layer (X11) of the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) are directly laminated together.

[0171] In addition, in the above-mentioned structure of the adhesive laminate 2, the surface of the second adhesive layer (X12) is the surface to be attached to the support.

[0172] In the above-mentioned structure of the pressure-sensitive adhesive laminate 2, the substrate (Y1) is preferably a non-thermally expandable substrate.

[0173] exist Figure 3 In the adhesive laminate 2 shown, the heat treatment for separation produces irregularities on the surface of the heat-expandable adhesive layer as the first adhesive layer (X11), and the contact area between the first adhesive layer (X11) and the base material (Y2) of the adhesive sheet (II) is reduced.

[0174] On the other hand, since the surface of the substrate (Y1) side of the first adhesive layer (X11) is laminated with the substrate (Y1) as a non-thermal expandable substrate, it is not easy to produce unevenness. Therefore, unevenness can be efficiently formed on the surface of the adhesive sheet (II) side of the first adhesive layer (X11).

[0175] As a result, the pressure-sensitive adhesive laminate 2 can be easily separated with a slight force at the interface P between the first pressure-sensitive adhesive layer (X11) of the pressure-sensitive adhesive sheet (I) and the substrate (Y2) of the pressure-sensitive adhesive sheet (II).

[0176] <Structure of Adhesive Laminated Body Having Release Material>

[0177] The adhesive laminate of one embodiment used in the manufacturing method of the present invention may be a structure in which a release material is further laminated on one or both of the surface of the adhesive layer (X1) to be attached to the support and the surface of the adhesive layer (X2) to be attached to the object.

[0178] In addition, for example, Figure 1 The adhesive laminates 1a and 1b shown in (a) and (b) may be laminates in which a release material having release treatment applied to both sides is laminated on one of the adhesive surfaces of the adhesive layer (X1) and the adhesive layer (X2) and rolled into a roll. Figure 2 The adhesive laminates 1c, 1d, and Figure 3The adhesive laminate 2 shown may also be in a rolled-up structure.

[0179] [Various physical properties of adhesive laminate]

[0180] The pressure-sensitive adhesive laminate of one embodiment used in the production method of the present invention can be easily separated with a small force at the interface P between the pressure-sensitive adhesive sheet (I) and the substrate (Y2) of the pressure-sensitive adhesive sheet (II) by heat treatment at a temperature not lower than the expansion starting temperature (t) of the heat-expandable particles.

[0181] Here, in the adhesive laminate of one embodiment of the present invention, the peeling force (F1) when separation is carried out at the interface P by heat treatment at a temperature above the expansion starting temperature (t) of the heat-expandable particles is generally 0 to 2000 mN / 25 mm, preferably 0 to 1000 mN / 25 mm, more preferably 0 to 150 mN / 25 mm, further preferably 0 to 100 mN / 25 mm, and further preferably 0 to 50 mN / 25 mm.

[0182] In addition, when the peel force (F1) is 0 mN / 25 mm, even if the peel force is measured by the method described in the Examples, it may be impossible to measure the peel force because the peel force is too small.

[0183] Furthermore, from the viewpoint of sufficiently fixing the object to be processed before heat treatment without adversely affecting the processing operation, the interlayer adhesion between the pressure-sensitive adhesive sheet (I) and the substrate (Y2) of the pressure-sensitive adhesive sheet (II) is preferably high.

[0184] From the above viewpoints, in the adhesive laminate of one mode used in the manufacturing method of the present invention, the peeling force (F0) when separating at the interface P before heat treatment is preferably 100 mN / 25 mm or more, more preferably 300 mN / 25 mm or more, further preferably 500 mN / 25 mm or more, and preferably 50000 mN / 25 mm or less.

[0185] In one embodiment of the adhesive laminate used in the manufacturing method of the present invention, the peel force (F0) is greater than the peel force (F1). Specifically, the ratio of the peel force (F1) to the peel force (F0) [(F1) / (F0)] is preferably 0 to 0.9, more preferably 0 to 0.8, further preferably 0 to 0.5, and further preferably 0 to 0.2.

[0186] In addition, as a temperature condition when measuring peeling force (F1), it is sufficient as long as it is the expansion starting temperature (t) or more and is the temperature at which the heat-expandable particle expands.

[0187] The temperature condition for measuring the peel force (F0) may be any temperature lower than the expansion starting temperature (t), which is basically room temperature (23°C).

[0188] However, more specific measurement conditions and methods of the peel force (F1) and the peel force (F0) are based on the methods described in Examples.

[0189] In one embodiment of the adhesive laminate used in the manufacturing method of the present invention, the adhesive strength of the adhesive layer (X1) (the first adhesive layer (X11) and the second adhesive layer (X12)) possessed by the adhesive sheet (I) at room temperature (23°C) and the adhesive strength of the adhesive layer (X2) possessed by the adhesive sheet (II) are preferably 0.1 to 10.0 N / 25 mm, more preferably 0.2 to 8.0 N / 25 mm, further preferably 0.4 to 6.0 N / 25 mm, and further preferably 0.5 to 4.0 N / 25 mm.

[0190] When the adhesive sheet (I) has a first adhesive layer (X11) and a second adhesive layer (X12), the adhesive forces of the first adhesive layer (X11) and the second adhesive layer (X12) are preferably within the above-mentioned ranges, respectively. From the viewpoint of improving the adhesion to the support and making it easier to separate together at the interface P, it is more preferred that the adhesive force of the second adhesive layer (X12) adhered to the support is higher than the adhesive force of the first adhesive layer (X11).

[0191] The substrate (Y1) of the pressure-sensitive adhesive sheet (I) and the substrate (Y2) of the pressure-sensitive adhesive sheet (II) are non-adhesive substrates.

[0192] In the present invention, whether or not a substrate is non-adhesive is determined by determining that a substrate is a “non-adhesive substrate” if the probe tack value measured on the surface of the substrate in accordance with JIS Z0237:1991 is less than 50 mN / 5 mmφ.

[0193] The probe viscosity values ​​of the surfaces of the substrate (Y1) possessed by the adhesive sheet (I) and the substrate (Y2) possessed by the adhesive sheet (II) used in one embodiment of the present invention are respectively and independently lower than 50 mN / 5 mmφ, preferably lower than 30 mN / 5 mmφ, more preferably lower than 10 mN / 5 mmφ, and further preferably lower than 5 mN / 5 mmφ.

[0194] In addition, in this specification, the specific method of measuring the probe viscosity value of the surface of the heat-expandable substrate is based on the method described in the Examples.

[0195] Hereinafter, each layer constituting the pressure-sensitive adhesive laminate of the present invention will be described.

[0196] [Structure of Adhesive Sheet (I)]

[0197] The adhesive sheet (I) possessed by the adhesive laminate used in the production method of the present invention is a heat-expandable adhesive sheet, which has a substrate (Y1) and an adhesive layer (X1), and contains heat-expandable particles in any layer in a manner that allows separation at the interface with the substrate (Y2) of the adhesive sheet (II) by heat treatment for separation.

[0198] In one embodiment of the present invention, the thermal expansion starting temperature (t) of the thermally expandable particles is preferably 60 to 270°C.

[0199] As the pressure-sensitive adhesive sheet (I) used in one embodiment of the present invention, the following embodiments are preferred.

[0200] · The pressure-sensitive adhesive sheet (I) of the first embodiment: a pressure-sensitive adhesive sheet (I) having a heat-expandable substrate layer (Y1-1) containing heat-expandable particles as a substrate (Y1).

[0201] ·A second embodiment of the adhesive sheet (I): an adhesive sheet (I) having a first adhesive layer (X11) and a second adhesive layer (X12) on both sides of a substrate (Y1), wherein the first adhesive layer (X11) is a heat-expandable adhesive layer containing heat-expandable particles, and the second adhesive layer (X12) is a non-heat-expandable adhesive layer.

[0202] A pressure-sensitive adhesive sheet (I) in which the substrate (Y1) is a non-heat-expandable substrate.

[0203] Hereinafter, the first and second aspects of the pressure-sensitive adhesive sheet (I) used in one aspect of the present invention will be described.

[0204] <PSA Sheet of First Aspect (I)>

[0205] As the first embodiment of the pressure-sensitive adhesive sheet (I), there can be mentioned the following Figures 1-2 The substrate (Y1) shown here is a PSA sheet having a heat-expandable substrate layer (Y1-1) containing heat-expandable particles.

[0206] In the first embodiment of the PSA sheet (I), the PSA layer (X1) is preferably a non-thermally expandable PSA layer from the viewpoint that the PSA sheet (I) and the substrate (Y2) of the PSA sheet (II) can be easily separated together with a small force at the interface P.

[0207] Specifically, in Figure 1 In the adhesive sheet (I) of the adhesive laminated bodies 1a and 1b shown in FIG. 1 , the adhesive layer (X1) is preferably a non-thermally expandable adhesive layer. Figure 2In the PSA sheet (I) included in the PSA laminates 1c and 1d shown above, it is preferred that any one of the first PSA layer (X11) and the second PSA layer (X12) is a non-thermally expandable PSA layer.

[0208] The thickness of the substrate (Y1) before the heat treatment for separation in the first embodiment of the pressure-sensitive adhesive sheet (I) is preferably 10 to 1000 μm, more preferably 20 to 700 μm, further preferably 25 to 500 μm, and further preferably 30 to 300 μm.

[0209] The thickness of the PSA layer (X1) before the heat treatment for separation in the PSA sheet (I) of the first embodiment is preferably 1 to 60 μm, more preferably 2 to 50 μm, further preferably 3 to 40 μm, and further preferably 5 to 30 μm.

[0210] It should be noted that, in this specification, for example, Figure 2 When the adhesive sheet (I) has a plurality of adhesive layers as shown in FIG. 1 , the above-mentioned “thickness of the adhesive layer (X1)” refers to the thickness of each adhesive layer (in Figure 2 Here, it refers to the thickness of each of the adhesive layers (X11) and (X12)).

[0211] In addition, in this specification, the thickness of each layer constituting the pressure-sensitive adhesive laminate is a value measured by the method described in the Examples.

[0212] In the first embodiment of the adhesive sheet (I), the thickness ratio [(Y1-1) / (X1)] of the heat-expandable substrate layer (Y1-1) to the adhesive layer (X1) before the heat treatment for separation is preferably 1000 or less, more preferably 200 or less, further preferably 60 or less, and further preferably 30 or less.

[0213] When the thickness ratio is 1000 or less, a pressure-sensitive adhesive laminate can be easily separated with a slight force at the interface P between the pressure-sensitive adhesive sheet (I) and the substrate (Y2) of the pressure-sensitive adhesive sheet (II) by heat treatment.

[0214] The thickness ratio is preferably 0.2 or more, more preferably 0.5 or more, further preferably 1.0 or more, and further preferably 5.0 or more.

[0215] In the first embodiment of the pressure-sensitive adhesive sheet (I), the substrate (Y1) may be Figure 1 As shown in (a), it may be composed of only the heat-expandable base material layer (Y1-1), or as shown in Figure 1 As shown in (b), the heat-expandable substrate layer (Y1-1) is provided on the adhesive layer (II) side, and the non-heat-expandable substrate layer (Y1-2) is provided on the adhesive layer (X1) side.

[0216] In the first embodiment of the pressure-sensitive adhesive sheet (I), the thickness ratio [(Y1-1) / (Y1-2)] of the heat-expandable substrate layer (Y1-1) to the non-heat-expandable substrate layer (Y1-2) before the heat treatment for separation is preferably 0.02 to 200, more preferably 0.03 to 150, and even more preferably 0.05 to 100.

[0217] <Second Embodiment of Pressure-Sensitive Adhesive Sheet (I)>

[0218] Examples of the second embodiment of the PSA sheet (I) include: Figure 3 As shown in the figure, the adhesive sheet has a first adhesive layer (X11) and a second adhesive layer (X12) on both sides of the substrate (Y1), wherein the first adhesive layer (X11) is a heat-expandable adhesive layer containing heat-expandable particles, and the second adhesive layer (X12) is a non-heat-expandable adhesive layer.

[0219] In the pressure-sensitive adhesive sheet (I) of the second embodiment, the first pressure-sensitive adhesive layer (X11) which is a thermally expandable pressure-sensitive adhesive layer is in direct contact with the base material (Y2) of the pressure-sensitive adhesive sheet (II).

[0220] In the pressure-sensitive adhesive sheet (I) of the second embodiment, the substrate (Y1) is preferably a non-thermally expandable substrate layer.

[0221] In the second embodiment of the adhesive sheet (I), the thickness ratio [(X11) / (X12)] of the first adhesive layer (X11) and the second adhesive layer (X12) before the heat treatment for separation is preferably 0.1 to 80, more preferably 0.3 to 50, and further preferably 0.5 to 15, and the first adhesive layer (X11) is a thermally expandable adhesive layer, and the second adhesive layer (X12) is a non-thermally expandable adhesive layer.

[0222] In addition, in the second embodiment of the adhesive sheet (I), the thickness ratio of the first adhesive layer (X11) to the substrate (Y1) before the heat treatment for separation [(X11) / (Y1)] is preferably 0.05 to 20, more preferably 0.1 to 10, and further preferably 0.2 to 3, and the first adhesive layer (X11) is a thermally expandable adhesive layer.

[0223] Hereinafter, the heat-expandable particles contained in any layer constituting the adhesive sheet (I) will be described, and on this basis, the heat-expandable substrate layer (Y1-1), the non-heat-expandable substrate layer (Y1-2), and the adhesive layer (X1) constituting the substrate (Y1) will be described in detail.

[0224] <Thermal expansion particles>

[0225] The heat-expandable particles used in the present invention may be particles that expand when heated, and are preferably particles whose expansion starting temperature (t) is adjusted to 60 to 270° C. The expansion starting temperature (t) can be appropriately selected depending on the application of the pressure-sensitive adhesive laminate.

[0226] For example, in the manufacturing method of the present invention, in the case where the adhesive laminate is not exposed to a high temperature environment in the process (1) and the process (2) (for example, the case where a modified region as a starting point for segmentation is formed inside a semiconductor wafer, etc.), the expansion starting temperature of the heat-expandable particles is preferably as low as possible within the above-mentioned temperature range. Thus, the heating energy required when separating the adhesive sheet (I) from the adhesive sheet (II) is reduced, and the manufacturing cost of the cut and / or ground material can be reduced. In addition, the adhesive sheet (I) can be separated from the adhesive sheet (II) without applying excessive thermal processing to the object to be processed.

[0227] In this specification, the expansion starting temperature (t) of the heat-expandable particles is a value measured based on the following method.

[0228] (Method for measuring expansion starting temperature (t) of heat-expandable particles)

[0229] 0.5 mg of heat-expandable particles to be measured were placed in an aluminum cup having a diameter of 6.0 mm (inner diameter of 5.65 mm) and a depth of 4.8 mm, and an aluminum lid (diameter of 5.6 mm, thickness of 0.1 mm) was placed thereon to prepare a sample.

[0230] Using a dynamic viscoelasticity measuring device, a force of 0.01 N was applied to the sample from the upper part of the aluminum cover using an indenter, and the height of the sample was measured in this state. Then, a force of 0.01 N was applied using an indenter, and in this state, the sample was heated from 20°C to 300°C at a heating rate of 10°C / min, and the displacement of the indenter in the vertical direction was measured, and the displacement start temperature in the positive direction was taken as the expansion start temperature (t).

[0231] As the heat-expandable particles, microcapsule foaming agents composed of an outer shell composed of a thermoplastic resin and an inner component encapsulated in the outer shell and vaporized when heated to a predetermined temperature are preferred.

[0232] Examples of the thermoplastic resin constituting the outer shell of the microcapsule foaming agent include vinylidene chloride-acrylonitrile copolymer, polyvinyl alcohol, polyvinyl butyral, polymethyl methacrylate, polyacrylonitrile, polyvinylidene chloride, and polysulfone.

[0233] Examples of the inner component contained in the outer shell include propane, butane, pentane, hexane, heptane, octane, nonane, decane, isobutane, isopentane, isohexane, isoheptane, isooctane, isononane, isodecane, cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, cyclooctane, neopentane, dodecane, isododecane, cyclotridecane, hexylcyclohexane, tridecane, tetradecane, pentadecane, hexadecane, heptadecane, octadecane, nonadecane, Isotridecane, 4-methyldodecane, isotetradecane, isopentadecane, isohexadecane, 2,2,4,4,6,8,8-heptamethylnonane, isoheptadecane, isooctadecane, isononadecane, 2,6,10,14-tetramethylpentadecane, cyclotridecane, heptylcyclohexane, n-octylcyclohexane, cyclopentadecane, nonylcyclohexane, decylcyclohexane, pentadecylcyclohexane, hexadecylcyclohexane, heptadecane, octadecylcyclohexane, etc.

[0234] These internal components may be used alone or in combination of two or more.

[0235] The expansion starting temperature (t) of the heat-expandable particles can be adjusted by appropriately selecting the type of the contained components.

[0236] The average particle size of the heat-expandable particles used in one embodiment of the present invention before expansion at 23° C. is preferably 3 to 100 μm, more preferably 4 to 70 μm, further preferably 6 to 60 μm, and further preferably 10 to 50 μm.

[0237] It should be noted that the average particle size of the heat-expandable particles before expansion refers to the volume median particle size (D 50 ) is a particle size at which the cumulative volume frequency calculated from the smaller particle size among the heat-expandable particles before expansion is equivalent to 50% in the particle distribution of the heat-expandable particles before expansion measured using a laser diffraction particle size distribution measuring apparatus (e.g., manufactured by Malvern, product name "Mastersizer 3000").

[0238] The 90% particle size (D ) of the heat-expandable particles before expansion at 23° C. used in one embodiment of the present invention is 90 ), preferably 10 to 150 μm, more preferably 20 to 100 μm, further preferably 25 to 90 μm, and further preferably 30 to 80 μm.

[0239] It should be noted that the 90% particle size (D 90) is a particle size corresponding to 90% of the cumulative volume frequency calculated from the smaller particle size among the heat-expandable particles before expansion in the particle distribution of the heat-expandable particles before expansion measured using a laser diffraction particle size distribution measuring apparatus (e.g., manufactured by Malvern, product name "Mastersizer 3000").

[0240] The heat-expandable particles used in one embodiment of the present invention preferably have a maximum volume expansion ratio of 1.5 to 100 times, more preferably 2 to 80 times, further preferably 2.5 to 60 times, and further preferably 3 to 40 times when heated to a temperature higher than the expansion starting temperature (t).

[0241] <Thermal expandable base material layer (Y1-1)>

[0242] In the pressure-sensitive adhesive laminate of one embodiment of the present invention, when the substrate (Y1) of the pressure-sensitive adhesive sheet (I) has a heat-expandable substrate layer (Y1-1) containing heat-expandable particles, the heat-expandable substrate layer (Y1-1) preferably satisfies the following requirement (1).

[0243] Requirement (1): At the expansion starting temperature (t) of the heat-expandable particles, the storage modulus E'(t) of the heat-expandable base layer (Y1-1) is 1.0×10 7 Below Pa.

[0244] In addition, in this specification, the storage modulus E' of the heat-expandable base layer (Y1-1) at a given temperature is a value measured by the method described in the Examples.

[0245] The requirement (1) can be considered to be an index showing the rigidity of the heat-expandable base material layer (Y1-1) immediately before the heat-expandable particles expand.

[0246] Before the heat-expandable particles expand, the storage modulus E' of the heat-expandable substrate layer (Y1-1) decreases with increasing temperature. However, around the expansion start temperature (t) of the heat-expandable particles, the heat-expandable particles begin to expand, thereby suppressing the decrease in the storage modulus E' of the heat-expandable substrate layer (Y1-1).

[0247] On the other hand, in order to easily separate the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) at the interface P with a small force, it is necessary to easily form projections and depressions on the surface of the side laminated with the substrate (Y2) of the adhesive sheet (I) by heating to a temperature above the expansion starting temperature (t).

[0248] That is, in the heat-expandable substrate layer (Y1-1) satisfying the above requirement (1), the heat-expandable particles expand at the expansion starting temperature (t) and grow sufficiently large, and are likely to form irregularities on the surface of the adhesive sheet (I) on the side laminated with the substrate (Y2) of the adhesive sheet (II).

[0249] As a result, a pressure-sensitive adhesive laminate can be prepared that can be easily separated with a slight force at the interface P between the pressure-sensitive adhesive sheet (I) and the substrate (Y2) of the pressure-sensitive adhesive sheet (II).

[0250] From the above viewpoints, the storage elastic modulus E'(t) defined in the requirement (1) of the heat expandable substrate layer (Y1-1) used in the present invention is preferably 9.0×10 6 Pa or less, more preferably 8.0×10 6 Pa or less, more preferably 6.0×10 6 Pa or less, more preferably 4.0×10 6 Below Pa.

[0251] In addition, from the viewpoint of suppressing the flow of the heat-expandable particles after expansion, improving the shape retention of the concavo-convex shapes formed on the surface of the adhesive sheet (I) on the side laminated with the substrate (Y2) of the adhesive sheet (II), and enabling easier separation at the interface P with a small force, the storage modulus E'(t) defined in the requirement (1) of the heat-expandable substrate layer (Y1-1) is preferably 1.0×10 3 Pa or more, more preferably 1.0×10 4 Pa or more, more preferably 1.0×10 5 Pa or above.

[0252] From the viewpoint of producing a heat-expandable substrate layer (Y1-1) satisfying the above requirement (1), the content of the heat-expandable particles in the heat-expandable substrate layer (Y1-1) is preferably 1 to 40 mass %, more preferably 5 to 35 mass %, further preferably 10 to 30 mass %, and further preferably 15 to 25 mass %, relative to the total mass (100 mass %) of the heat-expandable substrate layer (Y1-1).

[0253] It should be noted that from the viewpoint of improving the interlayer adhesion with other layers stacked on the heat-expandable substrate layer (Y1-1), the surface of the heat-expandable substrate layer (Y1-1) may be subjected to surface treatment using an oxidation method, a convexo-relief method, or the like, an adhesion-facilitating treatment, or a primer treatment.

[0254] Examples of the oxidation method include corona discharge treatment, plasma discharge treatment, chromic acid treatment (wet method), hot air treatment, ozone, and ultraviolet irradiation treatment. Examples of the roughening method include sandblasting and solvent treatment.

[0255] The heat-expandable base layer (Y1-1) is preferably formed from a resin composition (y) containing a resin and heat-expandable particles.

[0256] In addition, the resin composition (y) may contain a substrate additive as needed within a range not impairing the effects of the present invention.

[0257] Examples of the additive for the substrate include ultraviolet absorbers, light stabilizers, antioxidants, antistatic agents, lubricants, antiblocking agents, colorants, and the like.

[0258] In addition, these additives for substrates may be used alone or in combination of two or more.

[0259] When these additives for base materials are contained, the content of each additive for base materials is preferably 0.0001 to 20 parts by mass, more preferably 0.001 to 10 parts by mass, based on 100 parts by mass of the resin.

[0260] The heat-expandable particles contained in the resin composition (y) as a material for forming the heat-expandable substrate layer (Y1-1) are as described above.

[0261] The content of the heat expandable particles is preferably 1 to 40% by mass, more preferably 5 to 35% by mass, further preferably 10 to 30% by mass, and further preferably 15 to 25% by mass, based on the total amount (100% by mass) of the active ingredients of the resin composition (y).

[0262] The resin contained in the resin composition (y), which is a material for forming the heat-expandable base layer (Y1-1), may be a non-adhesive resin or an adhesive resin.

[0263] That is, even if the resin contained in the resin composition (y) is an adhesive resin, as long as the adhesive resin undergoes a polymerization reaction with a polymerizable compound during the process of forming the heat-expandable substrate layer (Y1-1) from the resin composition (y), the obtained resin is a non-adhesive resin, and the heat-expandable substrate layer (Y1-1) containing the resin is non-adhesive.

[0264] The weight average molecular weight (Mw) of the resin contained in the resin composition (y) is preferably 1,000 to 1,000,000, more preferably 1,000 to 700,000, and even more preferably 1,000 to 500,000.

[0265] When the resin is a copolymer having two or more structural units, the form of the copolymer is not particularly limited, and may be any of a block copolymer, a random copolymer, and a graft copolymer.

[0266] The content of the resin is preferably 50 to 99 mass %, more preferably 60 to 95 mass %, further preferably 65 to 90 mass %, and further preferably 70 to 85 mass % based on the total amount (100 mass %) of the active ingredients of the resin composition (y).

[0267] From the viewpoint of forming the heat expandable substrate layer (Y1-1) satisfying the requirement (1), the resin contained in the resin composition (y) preferably contains at least one selected from acrylic urethane resins and olefin resins.

[0268] Moreover, as said acrylic urethane resin, the following resin (U1) is preferable.

[0269] An acrylic urethane resin (U1) obtained by polymerizing a urethane prepolymer (UP) and a vinyl compound containing (meth)acrylate.

[0270] (Acrylic urethane resin (U1))

[0271] Examples of the urethane prepolymer (UP) forming the main chain of the acrylic urethane resin (U1) include reaction products of polyols and polyisocyanates.

[0272] In addition, the urethane prepolymer (UP) is preferably obtained by further subjecting the urethane prepolymer to a chain extension reaction using a chain extender.

[0273] Examples of the polyol used as a raw material of the urethane prepolymer (UP) include alkylene polyols, ether polyols, ester polyols, ester amide polyols, ester / ether polyols, and carbonate polyols.

[0274] These polyols may be used alone or in combination of two or more.

[0275] The polyol used in one embodiment of the present invention is preferably a diol, more preferably an ester diol, an alkylene diol, and a carbonate diol, and even more preferably an ester diol and a carbonate diol.

[0276] Examples of the ester-type diol include polycondensates formed by one or more of the following diols and one or more of the following dicarboxylic acids and their anhydrides: the diols are selected from alkanediols such as 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, and 1,6-hexanediol; alkylene glycols such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; and the like; the diols are selected from The carboxylic acid is selected from phthalic acid, isophthalic acid, terephthalic acid, naphthalene dicarboxylic acid, 4,4-biphenyl dicarboxylic acid, diphenylmethane-4,4'-dicarboxylic acid, succinic acid, adipic acid, azelaic acid, sebacic acid, chlorobridgeic acid, maleic acid, fumaric acid, itaconic acid, cyclohexane-1,3-dicarboxylic acid, cyclohexane-1,4-dicarboxylic acid, hexahydrophthalic acid, hexahydroisophthalic acid, hexahydroterephthalic acid, methylhexahydrophthalic acid, and the like.

[0277] Specific examples include polyethylene adipate diol, polybutylene adipate diol, polyhexamethylene adipate diol, polyhexamethylene isophthalate diol, polyneopentyl adipate diol, polyethylene propylene adipate diol, polyethylene butylene adipate diol, polyhexamethylene adipate diol, polyethylene diethylene adipate diol, poly(tetramethylene ether) adipate diol, poly(3-methylpentane adipate) diol, polyethylene azelaic acid diol, polyethylene sebacate diol, polybutylene azelaic acid diol, polybutylene sebacate diol, and polyneopentyl terephthalate diol.

[0278] Examples of the alkylene glycol include alkanediols such as 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, and 1,6-hexanediol; alkylene glycols such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; polyalkylene glycols such as polyethylene glycol, polypropylene glycol, and polybutylene glycol; polyoxyalkylene glycols such as polytetramethylene glycol; and the like.

[0279] Examples of the carbonate diol include 1,4-butylene glycol carbonate, 1,5-pentanediol carbonate, 1,6-hexanediol carbonate, 1,2-propylene glycol carbonate, 1,3-propylene glycol carbonate, 2,2-dimethylpropylene glycol carbonate, 1,7-heptanediol carbonate, 1,8-octanediol carbonate, and 1,4-cyclohexanediol carbonate.

[0280] Examples of the polyisocyanate as a raw material of the urethane prepolymer (UP) include aromatic polyisocyanates, aliphatic polyisocyanates, and alicyclic polyisocyanates.

[0281] These polyisocyanates may be used alone or in combination of two or more.

[0282] Furthermore, these polyisocyanates may be trimethylolpropane addition-type modified products, biuret-type modified products obtained by reacting with water, or isocyanurate-type modified products containing an isocyanurate ring.

[0283] Among them, the polyisocyanate used in one embodiment of the present invention is preferably a diisocyanate, and more preferably at least one selected from 4,4′-diphenylmethane diisocyanate (MDI), 2,4-toluene diisocyanate (2,4-TDI), 2,6-toluene diisocyanate (2,6-TDI), hexamethylene diisocyanate (HMDI), and alicyclic diisocyanates.

[0284] Examples of the alicyclic diisocyanate include 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (isophorone diisocyanate, IPDI), 1,3-cyclopentane diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, and methyl-2,6-cyclohexane diisocyanate, and isophorone diisocyanate (IPDI) is preferred.

[0285] In one embodiment of the present invention, the urethane prepolymer (UP) forming the main chain of the acrylic urethane resin (U1) is a reaction product of a diol and a diisocyanate, and is preferably a linear urethane prepolymer having ethylenically unsaturated groups at both ends.

[0286] Examples of a method for introducing ethylenically unsaturated groups into both terminals of the linear urethane prepolymer include a method of reacting the terminal NCO groups of the linear urethane prepolymer formed by reacting a diol with a diisocyanate compound with a hydroxyalkyl (meth)acrylate.

[0287] Examples of the hydroxyalkyl (meth)acrylate include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.

[0288] The vinyl compound forming the branched chain of the acrylic urethane resin (U1) contains at least (meth)acrylate.

[0289] As the (meth)acrylate, at least one selected from the group consisting of alkyl (meth)acrylates and hydroxyalkyl (meth)acrylates is preferred, and a combination of an alkyl (meth)acrylate and a hydroxyalkyl (meth)acrylate is more preferred.

[0290] When an alkyl (meth)acrylate and a hydroxyalkyl (meth)acrylate are used in combination, the mixing ratio of the hydroxyalkyl (meth)acrylate is preferably 0.1 to 100 parts by mass, more preferably 0.5 to 30 parts by mass, further preferably 1.0 to 20 parts by mass, and further preferably 1.5 to 10 parts by mass, relative to 100 parts by mass of the alkyl (meth)acrylate.

[0291] The number of carbon atoms of the alkyl group of the alkyl (meth)acrylate is preferably 1 to 24, more preferably 1 to 12, further preferably 1 to 8, and further preferably 1 to 3.

[0292] Examples of the hydroxyalkyl (meth)acrylate include the same compounds as those mentioned above for use in introducing ethylenically unsaturated groups into both terminals of the linear urethane prepolymer.

[0293] As vinyl compounds other than (meth)acrylates, there can be listed, for example: aromatic hydrocarbon vinyl compounds such as styrene, α-methylstyrene, vinyl toluene, etc.; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, etc.; monomers containing polar groups such as vinyl acetate, vinyl propionate, (meth)acrylonitrile, N-vinyl pyrrolidone, (meth)acrylic acid, maleic acid, fumaric acid, itaconic acid, (meth)acrylamide, etc.; and the like.

[0294] These vinyl compounds may be used alone or in combination of two or more.

[0295] The content of the (meth)acrylate in the vinyl compound is preferably 40 to 100 mass %, more preferably 65 to 100 mass %, further preferably 80 to 100 mass %, and further preferably 90 to 100 mass %, based on the total amount (100 mass %) of the vinyl compound.

[0296] The total content of the alkyl (meth)acrylate and the hydroxyalkyl (meth)acrylate in the vinyl compound is preferably 40 to 100% by mass, more preferably 65 to 100% by mass, further preferably 80 to 100% by mass, and further preferably 90 to 100% by mass, based on the total amount (100% by mass) of the vinyl compound.

[0297] The acrylic urethane resin (U1) used in one embodiment of the present invention can be obtained by mixing a urethane prepolymer (UP) and a vinyl compound containing a (meth)acrylate, and polymerizing the two.

[0298] In the polymerization, it is preferred to further add a radical initiator.

[0299] In the acrylic urethane resin (U1) used in one embodiment of the present invention, the content ratio [(u11) / (u12)] of the structural unit (u11) derived from the urethane prepolymer (UP) to the structural unit (u12) derived from the vinyl compound is preferably 10 / 90 to 80 / 20, more preferably 20 / 80 to 70 / 30, further preferably 30 / 70 to 60 / 40, and further preferably 35 / 65 to 55 / 45 in terms of mass ratio.

[0300] (Olefin resin)

[0301] As the resin contained in the resin composition (y), a suitable olefin-based resin is a polymer having at least a structural unit derived from an olefin monomer.

[0302] The olefin monomer is preferably an α-olefin having 2 to 8 carbon atoms, and specific examples thereof include ethylene, propylene, butene, isobutylene, and 1-hexene.

[0303] Among them, ethylene and propylene are preferred.

[0304] Specific examples of olefin resins include ultra-low density polyethylene (VLDPE, density: 880 kg / m 3 Above and below 910kg / m 3 ), low-density polyethylene (LDPE, density: 910kg / m 3 Above and below 915kg / m 3 ), medium density polyethylene (MDPE, density: 915kg / m 3 Above and below 942kg / m 3 ), high-density polyethylene (HDPE, density: 942kg / m 3 The present invention relates to polyethylene resins such as polyethylene (PE) and polyethylene glycol (PEG); polyethylene resins such as linear low-density polyethylene (LDPE); polypropylene resin (PP); polybutene resin (PB); ethylene-propylene copolymer; olefin elastomer (TPO); poly (4-methyl-1-pentene) (PMP); ethylene-vinyl acetate copolymer (EVA); ethylene-vinyl alcohol copolymer (EVOH); olefin terpolymers such as ethylene-propylene-(5-ethylidene-2-norbornene); and the like.

[0305] In one embodiment of the present invention, the olefin-based resin may be a modified olefin-based resin further subjected to one or more modifications selected from the group consisting of acid modification, hydroxy modification, and acryloyl modification.

[0306] For example, examples of the acid-modified olefin resin obtained by acid-modifying an olefin resin include a modified polymer obtained by graft-polymerizing an unsaturated carboxylic acid or an anhydride thereof onto the above-mentioned unmodified olefin resin.

[0307] Examples of the unsaturated carboxylic acid or anhydride thereof include maleic acid, fumaric acid, itaconic acid, citraconic acid, glutaconic acid, tetrahydrophthalic acid, aconitic acid, (meth)acrylic acid, maleic anhydride, itaconic anhydride, glutaconic anhydride, citraconic anhydride, aconitic anhydride, nadic anhydride, and tetrahydrophthalic anhydride.

[0308] In addition, the unsaturated carboxylic acid or its anhydride may be used alone or in combination of two or more.

[0309] Examples of the acrylic-modified olefinic resin obtained by subjecting an olefinic resin to acrylic modification include a modified polymer obtained by graft-polymerizing an alkyl (meth)acrylate as a side chain onto the above-mentioned unmodified olefinic resin as a main chain.

[0310] The number of carbon atoms of the alkyl group of the alkyl (meth)acrylate is preferably 1-20, more preferably 1-16, and even more preferably 1-12.

[0311] Examples of the alkyl (meth)acrylate include the same compounds as those which can be selected as the monomer (a1′) described later.

[0312] Examples of the hydroxy-modified olefinic resin obtained by modifying an olefinic resin with a hydroxy group include a modified polymer obtained by graft-polymerizing a hydroxy-containing compound onto the above-mentioned unmodified olefinic resin as a main chain.

[0313] Examples of the hydroxyl-containing compounds include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and unsaturated alcohols such as vinyl alcohol and allyl alcohol.

[0314] (Resins other than acrylic urethane resins and olefin resins)

[0315] In one embodiment of the present invention, the resin composition (y) may contain a resin other than the acrylic urethane resin and the olefin resin within a range not impairing the effects of the present invention.

[0316] Examples of such resins include vinyl resins such as polyvinyl chloride, polyvinylidene chloride, and polyvinyl alcohol; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polystyrene; acrylonitrile-butadiene-styrene copolymer; cellulose triacetate; polycarbonate; polyurethane that is not an acrylic urethane resin; polysulfone; polyetheretherketone; polyethersulfone; polyphenylene sulfide; polyimide resins such as polyetherimide and polyimide; polyamide resins; acrylic resins; fluororesins, etc.

[0317] Among them, from the viewpoint of forming the heat expandable substrate layer (Y1-1) satisfying the above requirements (1) and (2), the content of resins other than the acrylic urethane resin and the olefin resin in the resin composition (y) is preferably small.

[0318] The content of resins other than acrylic urethane resins and olefin resins is preferably less than 30 parts by mass, more preferably less than 20 parts by mass, further preferably less than 10 parts by mass, further preferably less than 5 parts by mass, and further preferably less than 1 part by mass, relative to 100 parts by mass of the total amount of resins contained in the resin composition (y).

[0319] (Solvent-free resin composition (y1))

[0320] As one embodiment of the resin composition (y) used in one embodiment of the present invention, there can be mentioned a solvent-free resin composition (y1), which is formulated with an oligomer having a weight average molecular weight (Mw) of 50,000 or less and having an ethylenically unsaturated group, an energy line polymerizable monomer, and the above-mentioned thermally expandable particles, and is not formulated with a solvent.

[0321] Although no solvent is added to the solvent-free resin composition (y1), the energy ray polymerizable monomer contributes to improving the plasticity of the oligomer.

[0322] By irradiating the coating film formed of the solvent-free resin composition (y1) with energy rays, the heat-expandable base layer (Y1-1) satisfying the above requirement (1) can be easily formed.

[0323] In addition, the type, shape, and blending amount (content) of the heat-expandable particles blended in the solvent-free resin composition (y1) are as described above.

[0324] The weight average molecular weight (Mw) of the oligomer contained in the solvent-free resin composition (y1) is 50,000 or less, preferably 1,000 to 50,000, more preferably 2,000 to 40,000, further preferably 3,000 to 35,000, and further preferably 4,000 to 30,000.

[0325] The oligomer may be any oligomer having a weight average molecular weight of 50,000 or less and having an ethylenically unsaturated group among the resins contained in the resin composition (y), and is preferably the urethane prepolymer (UP).

[0326] In addition, as this oligomer, a modified olefin resin having an ethylenically unsaturated group may also be used.

[0327] The total content of the above-mentioned oligomers and energy ray-polymerizable monomers in the solvent-free resin composition (y1) is preferably 50 to 99 mass %, more preferably 60 to 95 mass %, further preferably 65 to 90 mass %, and further preferably 70 to 85 mass %, relative to the total amount (100 mass %) of the solvent-free resin composition (y1).

[0328] As energy line polymerizable monomers, for example, there can be listed: alicyclic polymerizable compounds such as isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, cyclohexyl (meth)acrylate, adamantyl (meth)acrylate, and tricyclodecyl acrylate; aromatic polymerizable compounds such as phenyl hydroxypropyl acrylate, benzyl acrylate, and phenol ethylene oxide modified acrylate; heterocyclic polymerizable compounds such as tetrahydrofurfuryl (meth)acrylate, morpholine acrylate, N-vinyl pyrrolidone, and N-vinyl caprolactam, etc.

[0329] These energy ray-polymerizable monomers may be used alone or in combination of two or more.

[0330] In the solvent-free resin composition (y1), the content ratio of the oligomer to the energy ray polymerizable monomer [oligomer / energy ray polymerizable monomer] is preferably 20 / 80 to 90 / 10, more preferably 30 / 70 to 85 / 15, and further preferably 35 / 65 to 80 / 20 in terms of mass ratio.

[0331] In one embodiment of the present invention, the solvent-free resin composition (y1) preferably further contains a photopolymerization initiator.

[0332] By containing a photopolymerization initiator, the curing reaction can be sufficiently advanced even by irradiation with energy rays of relatively low energy.

[0333] Examples of the photopolymerization initiator include 1-hydroxycyclohexyl phenyl ketone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzyl phenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, bibenzyl, diacetyl, and 8-chloroanthraquinone.

[0334] These photopolymerization initiators may be used alone or in combination of two or more.

[0335] The amount of the photopolymerization initiator to be added is preferably 0.01 to 5 parts by mass, more preferably 0.01 to 4 parts by mass, and even more preferably 0.02 to 3 parts by mass, based on the total amount (100 parts by mass) of the oligomer and the energy ray-polymerizable monomer.

[0336] <Non-thermal expansion base material layer (Y1-2)>

[0337] Examples of the material for forming the non-heat-expandable substrate layer (Y1-2) constituting the substrate (Y1) include paper substrates, resins, and metals, and the material can be appropriately selected depending on the application of the pressure-sensitive adhesive laminate of one embodiment of the present invention.

[0338] Examples of the paper constituting the paper substrate include thin paper, mid-grade paper, fully-pulped paper, impregnated paper, coated paper, coated paper, sulphate paper, and glassine paper.

[0339] Examples of the resin include polyolefin resins such as polyethylene and polypropylene; vinyl resins such as polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol copolymer; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polystyrene; acrylonitrile-butadiene-styrene copolymer; cellulose triacetate; polycarbonate; urethane resins such as polyurethane and acrylic modified polyurethane; polymethylpentene; polysulfone; polyetheretherketone; polyethersulfone; polyphenylene sulfide; polyimide resins such as polyetherimide and polyimide; polyamide resins; acrylic resins; fluororesins, etc.

[0340] Examples of the metal include aluminum, tin, chromium, and titanium.

[0341] These forming materials may be composed of one kind or two or more kinds may be used in combination.

[0342] Examples of the non-heat-expandable substrate layer (Y1-2) formed by combining two or more forming materials include a substrate layer formed by laminating a paper substrate with a thermoplastic resin such as polyethylene, and a substrate layer formed by forming a metal film on the surface of a resin film or sheet containing a resin.

[0343] Examples of the method for forming the metal layer include a method of depositing the metal by PVD such as vacuum deposition, sputtering, or ion plating, and a method of attaching a metal foil made of the metal using a common adhesive.

[0344] It should be noted that, from the viewpoint of improving the interlayer adhesion with other layers stacked on the non-heat-expandable substrate layer (Y1-2), when the non-heat-expandable substrate layer (Y1-2) contains a resin, the surface of the non-heat-expandable substrate layer (Y1-2) can be subjected to surface treatment using an oxidation method, a convexo-relief method, or a primer treatment in the same manner as the above-mentioned heat-expandable substrate layer (Y1-1).

[0345] When the non-heat-expandable substrate layer (Y1-2) contains a resin, the substrate additive described above that can be contained in the resin composition (y) may be contained together with the resin.

[0346] The non-heat-expandable base material layer (Y1-2) is a non-heat-expandable layer determined by the above-mentioned method.

[0347] Therefore, the volume change rate (%) of the non-heat-expandable substrate layer (Y1-2) calculated according to the above formula is less than 5%, preferably less than 2%, more preferably less than 1%, further preferably less than 0.1%, and further preferably less than 0.01%.

[0348] In addition, as long as the volume change rate is within the above range, the non-thermally expandable substrate layer (Y1-2) may also contain heat-expandable particles. For example, by selecting the resin contained in the non-thermally expandable substrate layer (Y1-2), even if heat-expandable particles are contained, the volume change rate may be adjusted to the above range.

[0349] However, the smaller the content of the heat-expandable particles in the non-heat-expandable base layer (Y1-2), the better.

[0350] As a specific content of heat-expandable particles, relative to the total mass (100 mass%) of the non-heat-expandable substrate layer (Y1-2), it is usually less than 3 mass%, preferably less than 1 mass%, more preferably less than 0.1 mass%, further preferably less than 0.01 mass%, and further preferably less than 0.001 mass%. It is further preferred that the non-heat-expandable substrate layer (Y1-2) does not contain heat-expandable particles.

[0351] <Adhesive layer (X1)>

[0352] The PSA layer (X1) included in the PSA sheet (I) used in the first aspect of the present invention can be formed from a PSA composition (x1) containing a PSA resin.

[0353] The adhesive composition (x1) may contain adhesive additives such as a crosslinking agent, a tackifier, a polymerizable compound, and a polymerization initiator, as needed.

[0354] Hereinafter, each component contained in the adhesive composition (x1) is demonstrated.

[0355] In addition, when the adhesive sheet (I) has a first adhesive layer (X11) and a second adhesive layer (X12), the first adhesive layer (X11) and the second adhesive layer (X12) may be formed from an adhesive composition (x1) containing the following components.

[0356] (Adhesive resin)

[0357] The adhesive resin used in one embodiment of the present invention may be any polymer as long as the resin alone has adhesiveness and has a weight average molecular weight (Mw) of 10,000 or more.

[0358] The weight average molecular weight (Mw) of the adhesive resin used in one embodiment of the present invention is preferably 10,000 to 2,000,000, more preferably 20,000 to 1,500,000, and even more preferably 30,000 to 1,000,000 from the viewpoint of improving adhesive strength.

[0359] Specific examples of the adhesive resin include acrylic resins, urethane resins, rubber resins such as polyisobutylene resins, polyester resins, olefin resins, silicone resins, and polyvinyl ether resins.

[0360] These adhesive resins may be used alone or in combination of two or more.

[0361] When the adhesive resin is a copolymer having two or more structural units, the form of the copolymer is not particularly limited, and may be any of a block copolymer, a random copolymer, and a graft copolymer.

[0362] The adhesive resin used in one embodiment of the present invention may be an energy ray-curable adhesive resin in which a polymerizable functional group is introduced into a side chain of the above-mentioned adhesive resin.

[0363] Examples of the polymerizable functional group include a (meth)acryloyl group and a vinyl group.

[0364] In addition, examples of the energy rays include ultraviolet rays and electron beams, and ultraviolet rays are preferred.

[0365] In one embodiment of the present invention, from the viewpoint of exhibiting excellent adhesive strength, the adhesive resin preferably includes an acrylic resin.

[0366] It should be noted that when using an adhesive sheet (I) having a first adhesive layer (X11) and a second adhesive layer (X12), by including an acrylic resin in the first adhesive layer (X11) in contact with the resin film forming sheet (II), it is possible to easily form irregularities on the surface of the first adhesive layer.

[0367] The content of the acrylic resin in the adhesive resin is preferably 30 to 100% by mass, more preferably 50 to 100% by mass, further preferably 70 to 100% by mass, and further preferably 85 to 100% by mass, relative to the total amount (100% by mass) of the adhesive resin contained in the adhesive composition (x1) or the adhesive layer (X1).

[0368] (Acrylic resin)

[0369] In one embodiment of the present invention, examples of acrylic resins that can be used as adhesive resins include polymers containing structural units derived from (meth)acrylic acid alkyl esters having a linear or branched alkyl group, polymers containing structural units derived from (meth)acrylic acid esters having a cyclic structure, and the like.

[0370] The weight average molecular weight (Mw) of the acrylic resin is preferably 100,000 to 1.5 million, more preferably 200,000 to 1.3 million, further preferably 350,000 to 1.2 million, and further preferably 500,000 to 1.1 million.

[0371] The acrylic resin used in one embodiment of the present invention is more preferably an acrylic copolymer (A1) having a structural unit (a1) derived from a (meth)acrylic acid alkyl ester (a1') (hereinafter also referred to as "monomer (a1')") and a structural unit (a2) derived from a functional group-containing monomer (a2') (hereinafter also referred to as "monomer (a2')").

[0372] The number of carbon atoms of the alkyl group of the monomer (a1′) is preferably 1 to 24, more preferably 1 to 12, further preferably 2 to 10, and further preferably 4 to 8 from the viewpoint of improving adhesive properties.

[0373] It should be noted that the alkyl group contained in the monomer (a1′) may be a linear alkyl group or a branched alkyl group.

[0374] Examples of the monomer (a1′) include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, and stearyl (meth)acrylate.

[0375] These monomers (a1') may be used alone or in combination of two or more.

[0376] As the monomer (a1′), butyl (meth)acrylate and 2-ethylhexyl (meth)acrylate are preferred.

[0377] The content of the structural unit (a1) is preferably 50 to 99.9% by mass, more preferably 60 to 99.0% by mass, further preferably 70 to 97.0% by mass, and further preferably 80 to 95.0% by mass, based on all structural units (100% by mass) of the acrylic copolymer (A1).

[0378] Examples of the functional group possessed by the monomer (a2′) include a hydroxyl group, a carboxyl group, an amino group, and an epoxy group.

[0379] That is, examples of the monomer (a2′) include a hydroxyl group-containing monomer, a carboxyl group-containing monomer, an amino group-containing monomer, and an epoxy group-containing monomer.

[0380] These monomers (a2') may be used alone or in combination of two or more.

[0381] Among them, as the monomer (a2′), a hydroxyl group-containing monomer and a carboxyl group-containing monomer are preferred.

[0382] Examples of the hydroxyl group-containing monomer include the same monomers as those described above for the hydroxyl group-containing compound.

[0383] Examples of the carboxyl group-containing monomer include ethylenically unsaturated monocarboxylic acids such as (meth)acrylic acid and crotonic acid; ethylenically unsaturated dicarboxylic acids such as fumaric acid, itaconic acid, maleic acid, and citraconic acid and their anhydrides; 2-(acryloyloxy)ethyl succinate; and 2-carboxyethyl (meth)acrylate.

[0384] The content of the structural unit (a2) is preferably 0.1 to 40% by mass, more preferably 0.5 to 35% by mass, further preferably 1.0 to 30% by mass, and further preferably 3.0 to 25% by mass, based on all structural units (100% by mass) of the acrylic copolymer (A1).

[0385] The acrylic copolymer (A1) may further have a structural unit (a3) ​​derived from another monomer (a3') other than the monomers (a1') and (a2').

[0386] In the acrylic copolymer (A1), the content of the structural units (a1) and (a2) is preferably 70 to 100% by mass, more preferably 80 to 100% by mass, further preferably 90 to 100% by mass, and further preferably 95 to 100% by mass, relative to all the structural units (100% by mass) of the acrylic copolymer (A1).

[0387] Examples of the monomer (a3') include olefins such as ethylene, propylene, and isobutylene; halogenated olefins such as vinyl chloride and vinylidene chloride; diene monomers such as butadiene, isoprene, and chloroprene; (meth)acrylates having a cyclic structure such as cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, and acylide (meth)acrylate; styrene, α-methylstyrene, vinyltoluene, vinyl formate, vinyl acetate, acrylonitrile, (meth)acrylamide, (meth)acrylonitrile, (meth)acryloylmorpholine, and N-vinylpyrrolidone.

[0388] The acrylic copolymer (A1) may be an energy ray-curable acrylic copolymer in which a polymerizable functional group is introduced into the main chain and / or the side chain.

[0389] The polymerizable functional group and the energy line are as described above.

[0390] It should be noted that the polymerizable functional group can be introduced by reacting an acrylic copolymer having the above-mentioned structural units (a1) and (a2) with a polymerizable compound (Xa) having a substituent capable of bonding to the functional group possessed by the structural unit (a2) of the acrylic copolymer and a polymerizable functional group.

[0391] Examples of the polymerizable compound (Xa) include (meth)acryloyloxyethyl isocyanate, m-isopropenyl-α,α-dimethylbenzyl isocyanate, (meth)acryloyl isocyanate, allyl isocyanate, glycidyl (meth)acrylate, and (meth)acrylic acid.

[0392] (Crosslinking agent)

[0393] In one embodiment of the present invention, when the pressure-sensitive adhesive composition (x1) contains a pressure-sensitive adhesive resin having a functional group such as the acrylic copolymer (A1), it is preferred that the pressure-sensitive adhesive composition (x1) further contains a cross-linking agent.

[0394] The crosslinking agent is a substance that reacts with the adhesive resin having a functional group and crosslinks the adhesive resins with the functional group serving as a crosslinking starting point.

[0395] Examples of the crosslinking agent include isocyanate crosslinking agents, epoxy crosslinking agents, aziridine crosslinking agents, and metal chelate crosslinking agents.

[0396] These cross-linking agents may be used alone or in combination of two or more.

[0397] Among these crosslinking agents, isocyanate crosslinking agents are preferred from the viewpoints of improving cohesive force to enhance adhesive force and from the viewpoint of easy availability.

[0398] The content of the crosslinking agent can be appropriately adjusted by the number of functional groups of the adhesive resin, and is preferably 0.01 to 10 parts by mass, more preferably 0.03 to 7 parts by mass, and even more preferably 0.05 to 5 parts by mass based on 100 parts by mass of the adhesive resin having functional groups.

[0399] (Thickener)

[0400] In one embodiment of the present invention, the pressure-sensitive adhesive composition (x1) preferably further contains a tackifier from the viewpoint of further improving the adhesive strength.

[0401] In this specification, the "tackifier" refers to a component that assists in improving the adhesive strength of the above-mentioned adhesive resin, and is an oligomer having a weight average molecular weight (Mw) of less than 10,000, and is distinguished from the above-mentioned adhesive resin.

[0402] The weight average molecular weight (Mw) of the tackifier is preferably 400 to 10,000, more preferably 500 to 8,000, and even more preferably 800 to 5,000.

[0403] Examples of the tackifier include rosin-based resins, terpene-based resins, styrene-based resins, C5-based petroleum resins obtained by copolymerizing C5 fractions such as pentene, isoprene, piperylene, and 1,3-pentadiene produced by thermal cracking of naphtha, C9-based petroleum resins obtained by copolymerizing C9 fractions such as indene and vinyltoluene produced by thermal cracking of naphtha, and hydrogenated resins obtained by hydrogenating these.

[0404] The softening point of the tackifier is preferably 60 to 170°C, more preferably 65 to 160°C, and even more preferably 70 to 150°C.

[0405] In addition, in this specification, the "softening point" of a tackifier means the value measured according to JIS K 2531.

[0406] The tackifier may be used alone or in combination of two or more tackifiers having different softening points and structures.

[0407] When two or more tackifiers are used, it is preferred that the weighted average of the softening points of these tackifiers be within the above range.

[0408] The content of the tackifier is preferably 0.01 to 65 mass %, more preferably 0.05 to 55 mass %, further preferably 0.1 to 50 mass %, further preferably 0.5 to 45 mass %, and further preferably 1.0 to 40 mass %, relative to the total amount (100 mass %) of the active ingredients of the adhesive composition (x1) or the total mass (100 mass %) of the adhesive layer (X1).

[0409] (Photopolymerization Initiator)

[0410] In one embodiment of the present invention, when the adhesive composition (x1) contains an energy ray-curable adhesive resin as the adhesive resin, it is preferred that the adhesive composition (x1) further contains a photopolymerization initiator.

[0411] By preparing an adhesive composition containing an energy ray-curable adhesive resin and a photopolymerization initiator, the adhesive layer formed from the adhesive composition can fully undergo a curing reaction even when irradiated with energy rays of relatively low energy, thereby adjusting the adhesive strength to a desired range.

[0412] In addition, as a photoinitiator used for one aspect of this invention, the same initiator as the initiator mix|blended in the said solvent-free resin composition (y1) is mentioned.

[0413] The content of the photopolymerization initiator is preferably 0.01 to 10 parts by mass, more preferably 0.03 to 5 parts by mass, and even more preferably 0.05 to 2 parts by mass, based on 100 parts by mass of the energy ray-curable adhesive resin.

[0414] (Additives for adhesives)

[0415] In one embodiment of the present invention, the adhesive composition (x1) may contain adhesive additives commonly used in adhesives in addition to the above-mentioned additives, within a range not impairing the effects of the present invention.

[0416] Examples of such adhesive additives include antioxidants, softeners (plasticizers), rust preventives, pigments, dyes, reaction inhibitors, reaction accelerators (catalysts), and ultraviolet absorbers.

[0417] In addition, these adhesive additives may be used individually or in combination of 2 or more types.

[0418] When these adhesive additives are contained, the content of each adhesive additive is preferably 0.0001 to 20 parts by mass, more preferably 0.001 to 10 parts by mass, based on 100 parts by mass of the adhesive resin.

[0419] It should be noted that when using Figure 3 In the case of the above-mentioned second embodiment of the adhesive sheet (I) such as the adhesive laminate 2 shown, the first adhesive layer (X11) as the thermally expandable adhesive layer is formed from a thermally expandable adhesive composition (x11) further containing thermally expandable particles.

[0420] The heat-expandable particles are as described above.

[0421] The content of the heat-expandable particles is preferably 1 to 70% by mass, more preferably 2 to 60% by mass, further preferably 3 to 50% by mass, and further preferably 5 to 40% by mass, relative to the total amount (100% by mass) of the active ingredients of the heat-expandable adhesive composition (x11) or the total mass (100% by mass) of the heat-expandable adhesive layer.

[0422] On the other hand, when the pressure-sensitive adhesive layer (X1) is a non-heat-expandable pressure-sensitive adhesive layer, it is preferred to minimize the content of heat-expandable particles in the non-heat-expandable pressure-sensitive adhesive composition as a material for forming the non-heat-expandable pressure-sensitive adhesive layer.

[0423] The content of the heat-expandable particles is preferably less than 1% by mass, more preferably less than 0.1% by mass, further preferably less than 0.01% by mass, and further preferably less than 0.001% by mass, relative to the total amount (100% by mass) of the active ingredients of the non-heat-expandable adhesive composition or the total mass (100% by mass) of the non-heat-expandable adhesive layer. It is further preferred that the non-heat-expandable adhesive composition or the non-heat-expandable adhesive layer does not contain heat-expandable particles.

[0424] It should be noted that when using Figure 2 In the case of a pressure-sensitive adhesive sheet (I) having a first pressure-sensitive adhesive layer (X11) and a second pressure-sensitive adhesive layer (X12) as the pressure-sensitive adhesive laminates 1c and 1d shown in the drawings, the shear modulus G'(23) of the first pressure-sensitive adhesive layer (X11) as the pressure-sensitive adhesive layer is preferably 1.0×10 8 Pa or less, more preferably 5.0×10 7 Pa or less, more preferably 1.0×10 7 Below Pa.

[0425] If the shear modulus G'(23) of the first adhesive layer (X11) as a non-heat-expandable adhesive layer is 1.0×10 8Pa or less, for example, when making Figure 2 In the case of the structures of the adhesive laminated bodies 1c and 1d shown in the drawings, the expansion of the heat-expandable particles in the heat-expandable substrate layer (Y1-1) by the separation heat treatment easily forms unevenness on the surface of the first adhesive layer (X11) in contact with the adhesive sheet (II). As a result, an adhesive laminated body that can be easily separated at the interface P of the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) with a slight force can be produced.

[0426] It should be noted that the shear modulus G'(23) of the first adhesive layer (X11) as a non-heat-expandable adhesive layer at 23°C is preferably 1.0×10 4 Pa or more, more preferably 5.0×10 4 Pa or more, more preferably 1.0×10 5 Pa or above.

[0427] In addition, in this specification, the shear modulus G'(23) of the adhesive layer refers to the value measured by the method described in the Examples.

[0428] [Structure of Adhesive Sheet (II)]

[0429] The PSA sheet (II) of the PSA laminate used in the production method of the present invention comprises a substrate (Y2) and a PSA layer (X2), and the substrate (Y2) and the PSA sheet (I) are directly laminated together.

[0430] It should be noted that from the perspective of improving the interlayer adhesion between the substrate (Y2) and the adhesive layer (X2), the surface of the laminated adhesive layer side of the substrate (Y2) can be subjected to the above-mentioned surface treatment using the oxidation method, embossing method, etc., the easy-adhesion treatment, or the primer treatment.

[0431] In addition, in the adhesive laminate used in one embodiment of the present invention, from the viewpoint of suppressing the adhesion of residues of the adhesive layer (X2) to the cut and / or ground material, from the viewpoint of excellent followability to a processing object with large surface irregularities such as a semiconductor chip with bumps, and from the viewpoint of excellent temporal stability of the adhesive force of the adhesive layer (X2), the adhesive sheet (II) preferably has an intermediate layer (Z2) between the substrate (Y2) and the adhesive layer (X2).

[0432] In addition, for example, the surface of the substrate (Y2) on the adhesive layer (X2) side may be subjected to antistatic treatment. In the case of having an intermediate layer (Z2), the surface of the substrate (Y2) on the intermediate layer (Z2) side may be subjected to antistatic treatment.

[0433] From the viewpoint of being able to be easily separated with a slight force at the interface P with the pressure-sensitive adhesive sheet (I), the substrate (Y2) is preferably a non-thermally expandable substrate.

[0434] Furthermore, from the viewpoint of maintaining good adhesion to the adherend before and after the above-mentioned heat treatment, the pressure-sensitive adhesive layer (X2) is preferably a non-thermally expandable pressure-sensitive adhesive layer.

[0435] In addition, the intermediate layer (Z2) is preferably also a non-thermally expandable layer.

[0436] Therefore, the volume change rate (%) of the substrate (Y2), the adhesive layer (X2), and the intermediate layer (Z2) calculated according to the above formula is independently less than 5%, preferably less than 2%, more preferably less than 1%, further preferably less than 0.1%, and further preferably less than 0.01%. It should be noted that it is further preferred that the substrate (Y2), the adhesive layer (X2), and the intermediate layer (Z2) do not contain heat-expandable particles.

[0437] Hereinafter, the substrate (Y2), the adhesive layer (X2), and the intermediate layer (Z2) will be described.

[0438] <Base material (Y2)>

[0439] Examples of the material for forming the base material (Y2) include the same materials as those for forming the above-mentioned non-thermally expandable base material layer (Y1-2).

[0440] It should be noted that the substrate (Y2) preferably contains a resin, and more preferably a resin layer containing a resin is formed on at least the surface of the substrate (Y2) on the side laminated with the adhesive sheet (I), and further preferably the substrate (Y2) is a resin film or a resin sheet.

[0441] In addition, among the resin films or resin sheets, from the viewpoint of being able to stably maintain the properties of the processing object even when the processing object is ground to an extremely thin layer in the grinding of the processing object in step (4), preferably, a polyethylene film, a polypropylene film, an ethylene-vinyl acetate copolymer (EVA) film, or a polyethylene terephthalate film is used, and an ethylene-vinyl acetate copolymer (EVA) film is more preferred.

[0442] It should be noted that the above-mentioned resin film or resin sheet may contain a known filler, a colorant, an antistatic agent, an antioxidant, an organic lubricant, a catalyst, and the like.

[0443] The resin film or resin sheet may be transparent, or may be colored or have metal deposited thereon as desired.

[0444] In addition, from the viewpoint of being able to easily separate together at the interface P with a slight force after the heat treatment for separation, the surface of the substrate (Y2) laminated on the side of the pressure-sensitive adhesive sheet (I) may be subjected to a release treatment.

[0445] In addition, from the viewpoint of preventing the object to be processed from being misaligned when being attached to the adhesive layer (X2) and preventing the object from being excessively sunk into the adhesive layer (X2) when being attached, the storage modulus E'(23) of the substrate (Y2) at 23°C is preferably 1.0×10 6 Pa or above.

[0446] It should be noted that as long as the volume change rate of the substrate (Y2) is within the above range, it may contain heat-expandable particles. From the above viewpoint, the smaller the content of heat-expandable particles in the substrate (Y2), the better.

[0447] The content of the heat-expandable particles in the substrate (Y2) is generally less than 3% by mass, preferably less than 1% by mass, more preferably less than 0.1% by mass, further preferably less than 0.01% by mass, and still further preferably less than 0.001% by mass, relative to the total mass (100% by mass) of the substrate (Y2). It is further preferred that the substrate (Y2) does not contain heat-expandable particles.

[0448] The thickness of the substrate (Y2) is preferably 5 to 500 μm, more preferably 15 to 300 μm, and even more preferably 20 to 200 μm.

[0449] When the thickness of the substrate (Y2) is 5 μm or more, the deformation resistance (dimensional stability) at high temperature can be easily improved. On the other hand, when the thickness of the substrate is 500 μm or less, when the object to be processed by the adhesive sheet (II) is subjected to at least one of cutting and grinding, the deformation of the adhesive sheet (II) caused by vibration can be suppressed, so that the processing accuracy such as film thickness accuracy can be easily improved.

[0450] <Adhesive layer (X2)>

[0451] The adhesive layer (X2) of the resin film-forming sheet (II) can be formed using the above-mentioned adhesive composition (x1), and its preferred components and preferred ranges of the content of each component are the same as those of the adhesive composition (x1).

[0452] Here, in one embodiment of the present invention, the adhesive layer (X2) is preferably a layer formed by an adhesive composition comprising an energy ray-curable adhesive resin having a polymerizable functional group introduced into the side chain as an adhesive resin, and more preferably a layer formed by an adhesive composition comprising an energy ray-curable acrylic polymer (B) (hereinafter also referred to as "acrylic polymer (B)" or "(B) component").

[0453] The adhesive layer (X2) formed from the adhesive composition has excellent adhesive strength sufficient to hold the object to be processed before irradiation with energy rays, but the adhesive strength decreases after irradiation with energy rays, so that the processed object can be easily separated from the adhesive sheet (II).

[0454] The content of component (B) in the adhesive composition is preferably 70% by mass or more, more preferably 80% by mass or more, and further preferably 90% by mass or more, relative to the total amount (100% by mass) of the adhesive composition, and is preferably 99.9% by mass or less, more preferably 99.0% by mass or less, and further preferably 98.0% by mass or less.

[0455] From the viewpoint of having good adhesion and good followability for processing objects with large surface unevenness differences such as semiconductor chips with bumps, the thickness of the adhesive layer (X2) is preferably 1 to 100 μm, more preferably 1 to 75 μm, and further preferably 1 to 50 μm.

[0456] When the adhesive composition as a material forming the adhesive layer (X2) contains an energy ray-curable adhesive resin such as an energy ray-curable acrylic polymer (B), it preferably further contains a crosslinking agent and a photopolymerization initiator.

[0457] Examples of the crosslinking agent include the same crosslinking agents as those blended in the above-mentioned acrylic resin. The content range is also as described above. From the viewpoint of increasing the gel fraction of the adhesive layer (X2) and suppressing the generation of adhesive residue on the processed product when the processed product is separated, the content is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 1.0 to 10 parts by mass relative to 100 parts by mass of the adhesive resin having a functional group.

[0458] Examples of the photopolymerization initiator include the same ones as those blended in the above-mentioned solvent-free resin composition (y1), and the range of the content thereof is also as described above.

[0459] Furthermore, other additives may be contained.

[0460] Hereinafter, the energy ray-curable acrylic polymer (B) contained in the pressure-sensitive adhesive composition will be described.

[0461] (Component (B): energy ray-curable acrylic polymer (B))

[0462] The energy ray-curable acrylic polymer (B) used in one embodiment of the present invention is an acrylic copolymer in which a polymerizable functional group is introduced into a side chain and / or a main chain of a non-energy ray-curable acrylic polymer.

[0463] Examples of the non-energy ray-curable acrylic polymer include acrylic polymers having a structural unit derived from an alkyl (meth)acrylate having a linear or branched alkyl group and acrylic polymers having a structural unit derived from a (meth)acrylate having a cyclic structure.

[0464] The polymerizable functional group is as described above, but is preferably a (meth)acryloyl group from the viewpoint of ease of introduction into the non-energy ray-curable acrylic polymer.

[0465] The weight average molecular weight (Mw) of the component (B) is preferably 100,000 to 1,500,000, more preferably 200,000 to 1,200,000, further preferably 250,000 to 1,000,000, further preferably 300,000 to 900,000, and further preferably 350,000 to 800,000.

[0466] From the viewpoint of producing a pressure-sensitive adhesive sheet whose adhesive force can be effectively reduced by irradiation with energy rays, the component (B) preferably comprises an acrylic copolymer (B0) and an energy-ray-curable acrylic copolymer (B1) obtained by reacting with a polymerizable compound (Xb), wherein the acrylic copolymer (B0) has a structural unit (b1) and a structural unit (b2), wherein the structural unit (b1) is derived from a (meth)acrylic acid alkyl ester (b1') having an alkyl group having 1 to 18 carbon atoms (hereinafter also referred to as "monomer (b1')") and the structural unit (b2) is derived from a functional group-containing monomer (b2') (hereinafter also referred to as "monomer (b2')"), and more preferably the energy-ray-curable acrylic copolymer (B1).

[0467] The copolymerization method of the acrylic copolymers (B0) and (B1) is not particularly limited, and the copolymers may be block copolymers, random copolymers, or graft copolymers.

[0468] The content of the acrylic copolymer (B1) is preferably 70 to 100 mass %, more preferably 80 to 100 mass %, further preferably 90 to 100 mass %, and even more preferably 100 mass %, relative to the total amount (100 mass %) of the component (B) contained in the pressure-sensitive adhesive composition.

[0469] The number of carbon atoms of the alkyl group contained in the monomer (b1′) is preferably 1 to 18, more preferably 1 to 12, further preferably 1 to 8, and further preferably 1 to 6.

[0470] Examples of the monomer (b1′) include the monomers exemplified as the above-mentioned monomer (a1′), preferably butyl (meth)acrylate or 2-ethylhexyl (meth)acrylate, and more preferably butyl (meth)acrylate.

[0471] From the viewpoint of improving the adhesive strength of the formed pressure-sensitive adhesive layer, the content of the structural unit (b1) in the acrylic copolymer (B0) is preferably 50 to 99.5% by mass, more preferably 60 to 99% by mass, further preferably 70 to 98% by mass, and further preferably 80 to 96% by mass, relative to all structural units (100% by mass) of the acrylic copolymer (B0).

[0472] The monomer (b2') includes those exemplified as the above-mentioned monomer (a2'), preferably one or more selected from hydroxyl-containing monomers, carboxyl-containing monomers, and epoxy-containing monomers, more preferably hydroxyl-containing monomers, and further preferably 2-hydroxyethyl (meth)acrylate.

[0473] The content of the structural unit (b2) in the acrylic copolymer (B0) is preferably 0.5 to 40% by mass, more preferably 1 to 30% by mass, further preferably 2 to 25% by mass, and further preferably 3 to 15% by mass, relative to all structural units (100% by mass) of the acrylic copolymer (B0).

[0474] When the content of the structural unit (b2) is 0.5% by mass or more, the content of the structural unit (b2) having a functional group having a reaction point with the polymerizable compound (Xb) can be sufficiently ensured, and a highly curable adhesive layer (X2) can be formed by irradiation with energy rays. Therefore, when the cut and / or ground material is peeled off from the adhesive layer (X2), it is possible to peel off while preventing the generation of residues of the adhesive layer (X2) on the cut and / or ground material.

[0475] When the content of the structural unit (b2) is 40% by mass or less, a sufficient pot life can be ensured when the adhesive layer (X2) is formed by applying a solution of the adhesive composition.

[0476] The polymerizable compound (Xb) refers to a compound having a substituent (hereinafter also referred to as a "reactive functional group") capable of bonding to a functional group in the structural unit (b2) of the acrylic copolymer (B0) and a polymerizable functional group.

[0477] The acrylic copolymer (B0) may have a structural unit (b3) derived from another monomer (b3') other than the above-mentioned monomers (b1') and (b2').

[0478] As other monomers (b3'), those exemplified as the above-mentioned monomers (a3') can be mentioned.

[0479] The content of the structural unit (b3) in the acrylic copolymer (B0) is preferably 0 to 20% by mass, more preferably 0 to 10% by mass, further preferably 0 to 5% by mass, and further preferably 0 to 1% by mass, relative to all structural units (100% by mass) of the acrylic copolymer (B0).

[0480] In addition, the above-mentioned monomers (b1') to (b3') can be used alone or in combination of two or more.

[0481] The energy ray-curable acrylic copolymer (B1) can be obtained by reacting the acrylic copolymer (B0) having the structural units (b1) and (b2) with a polymerizable compound (Xb).

[0482] Examples of the polymerizable compound (Xb) include those exemplified as the above-mentioned polymerizable compound (Xa), and among them, a compound having a reactive functional group and having 1 to 5 polymerizable functional groups per molecule is preferred.

[0483] Examples of the reactive substituent include an isocyanate group, a carboxyl group, and an epoxy group, and an isocyanate group is preferred.

[0484] Examples of the polymerizable functional group include a (meth)acryloyl group and a vinyl group as described above, and a (meth)acryloyl group is preferred.

[0485] As a specific polymerizable compound (Xb), (meth)acryloyloxyethyl isocyanate is preferred.

[0486] In addition, the polymerizable compound (Xb) can be used individually or in combination of 2 or more types.

[0487] In the acrylic copolymer (B1), regarding the relationship between the number of functional groups possessed by the acrylic copolymer (B0) and the amount of the polymerizable compound (Xb) blended, from the viewpoint of obtaining a pressure-sensitive adhesive sheet having a moderate adhesive strength before energy ray irradiation and whose adhesive strength can be effectively reduced after energy ray irradiation, the α value calculated by the following formula (1) is preferably 0.5 to 50, more preferably 1.0 to 40, further preferably 1.2 to 35, and further preferably 1.5 to 30.

[0488] In addition, the said α value corresponds to the number of polymerizable functional groups which the acrylic copolymer (B1) has.

[0489] Formula (1): α = [P B 〕×〔Q B 〕×〔R B 〕 / 100

[0490] (In formula (1), [P B 〕 represents the content of the structural unit (b2) relative to 100 parts by mass of all the structural units of the acrylic copolymer (B0), 〔Q B 〕 represents the equivalent weight of the polymerizable compound (Xb) relative to 100 equivalent weights of the functional groups derived from the functional group-containing monomer in the acrylic copolymer (B0), and 〔R B 〕 represents the number of polymerizable functional groups possessed by the polymerizable compound (Xb).

[0491] <Middle layer (Z2)>

[0492] In one embodiment of the present invention, the intermediate layer (Z2) is formed of an intermediate layer-forming composition (z2) containing a non-energy ray-curable acrylic polymer (C) and an energy ray-curable acrylic polymer (D).

[0493] By providing the intermediate layer (Z2), an adhesive sheet (II) having excellent followability for a processing object with large surface irregularities, such as a semiconductor wafer with bumps, can be produced. Therefore, when the processing object to which the adhesive sheet (II) is adhered is subjected to at least one of cutting and grinding, it is possible to prevent cutting chips, grinding chips, cutting water, and grinding water from penetrating into the surface of the processing object to which the adhesive sheet (II) is adhered, while suppressing damage to the processing object.

[0494] It should be noted that the intermediate layer (Z2) may or may not have adhesive properties.

[0495] The thickness of the intermediate layer (Z2) can be appropriately selected according to the degree of concavity and convexity of the processing object. For example, when the processing object is a semiconductor wafer or a semiconductor chip, it can be appropriately selected according to the height of the bumps possessed by the semiconductor wafer or the semiconductor chip. It is preferably 10 to 800 μm, more preferably 15 to 600 μm, and further preferably 20 to 400 μm.

[0496] When the thickness of the intermediate layer (Z2) is 10 μm or more, the followability to the workpiece with large unevenness can be improved. On the other hand, when the thickness of the intermediate layer is 800 μm or less, deformation of the pressure-sensitive adhesive sheet (II) can be easily suppressed.

[0497] From the viewpoints of achieving good adhesion between the intermediate layer (Z2) and the adhesive layer (X2) of the adhesive sheet (II) after irradiation with energy rays, suppressing the breakage of the adhesive layer (X2) when the cut and / or ground material is peeled off from the adhesive sheet (II), and generating residues of the adhesive layer (X2) on the surface of the cut and / or ground material, the intermediate layer forming layer composition (z2) forming the material serving as the intermediate layer (Z2) preferably contains a non-energy ray-curable acrylic polymer (C) (hereinafter also referred to as "acrylic polymer (C)" or "component (C)") and an energy ray-curable acrylic polymer (D) having a weight average molecular weight of 50,000 to 250,000 (hereinafter also referred to as "acrylic polymer (D)" or "component (D)").

[0498] In addition, from the viewpoint of further improving the adhesion between the intermediate layer (Z2) and the adhesive layer (X2) after irradiation with energy rays, the content of the component (D) in the intermediate layer forming composition (z2) relative to 100 parts by mass of the component (C) is preferably 25 parts by mass or more, more preferably 30 parts by mass or more, further preferably 37 parts by mass or more, and further preferably 40 parts by mass or more.

[0499] In addition, in one embodiment of the present invention, from the viewpoint of suppressing the seepage of a portion of the intermediate layer (Z2) from the end of the adhesive sheet (II), the content of the component (D) in the intermediate layer forming composition (z2) relative to 100 parts by mass of the component (C) is preferably 150 parts by mass or less, more preferably 140 parts by mass or less, and further preferably 130 parts by mass or less.

[0500] Relative to the total amount (100 mass %) of the intermediate layer forming composition (z2), the total content of the (C) component and the (D) component in the intermediate layer forming composition (z2) is preferably 70 mass % or more, more preferably 80 mass % or more, further preferably 90 mass % or more, and is preferably 99.9 mass % or less, more preferably 99.0 mass % or less, further preferably 98.0 mass % or less.

[0501] The intermediate layer forming composition (z2) preferably contains a photopolymerization initiator and a crosslinking agent in addition to the above-mentioned components (C) and (D).

[0502] Examples of the crosslinking agent include the same crosslinking agents as those blended in the above-mentioned acrylic resin, and the range of the content thereof is also as described above.

[0503] Examples of the photopolymerization initiator include the same ones as those blended in the above-mentioned solvent-free resin composition (y1), and the range of the content thereof is also as described above.

[0504] Furthermore, other additives may be contained.

[0505] Hereinafter, the non-energy ray-curable acrylic polymer (C) and the energy ray-curable acrylic polymer (D) contained in the intermediate layer forming composition (z2) will be described.

[0506] (Component (C): non-energy ray-curable acrylic polymer (C))

[0507] Examples of the non-energy ray-curable acrylic polymer (C) include polymers having a structural unit derived from an alkyl (meth)acrylate having a linear or branched alkyl group and polymers having a structural unit derived from a (meth)acrylate having a cyclic structure.

[0508] The weight average molecular weight (Mw) of the component (C) is preferably 300,000 to 1,500,000, more preferably 350,000 to 1,300,000, further preferably 400,000 to 1,200,000, further preferably 400,000 to 1,100,000, and further preferably 450,000 to 900,000.

[0509] As the component (C), from the viewpoint of compatibility with the component (D), it is preferred that the component (C) comprises an acrylate copolymer (C1) having a structural unit (c1) derived from an alkyl (meth)acrylate (c1') having an alkyl group having 1 to 18 carbon atoms (hereinafter also referred to as "monomer (c1')") and a structural unit (c2) derived from a functional group-containing monomer (c2') (hereinafter also referred to as "monomer (c2')"), and more preferably an acrylic copolymer (C1).

[0510] The copolymerization method of the acrylic copolymer (C1) is not particularly limited, and the acrylic copolymer (C1) may be a block copolymer, a random copolymer, or a graft copolymer.

[0511] The content of the acrylic copolymer (C1) is preferably 70 to 100 mass %, more preferably 80 to 100 mass %, further preferably 90 to 100 mass %, and even more preferably 100 mass %, relative to the total amount (100 mass %) of the component (C) contained in the intermediate layer-forming composition (z2).

[0512] The number of carbon atoms of the alkyl group of the monomer (c1′) is more preferably 4 to 12, further preferably 4 to 8, and even more preferably 4 to 6 from the viewpoint of compatibility with the component (D).

[0513] Examples of the monomer (c1′) include the same monomers as those mentioned above for the monomer (a1′).

[0514] Among them, butyl (meth)acrylate and 2-ethylhexyl (meth)acrylate are preferred, and butyl (meth)acrylate is more preferred.

[0515] The content of the structural unit (c1) in the acrylic copolymer (C1) is preferably 50 to 99.5% by mass, more preferably 60 to 99% by mass, further preferably 70 to 95% by mass, and further preferably 80 to 93% by mass, relative to all structural units (100% by mass) of the acrylic copolymer (C1).

[0516] When the content of the structural unit (c1) is 50% by mass or more, the PSA sheet can be made to have good followability to an object having a large difference in irregularities, which is preferred.

[0517] Moreover, when the content of the structural unit (c1) is 99.5 mass % or less, the content of the structural unit (c2) can be sufficiently ensured, and the compatibility with the component (D) can be improved, which is preferred.

[0518] The acrylic copolymer (C1) preferably has a structural unit (c11) as the structural unit (c1), wherein the structural unit (c11) is derived from an alkyl (meth)acrylate having an alkyl group having 4 or more carbon atoms (preferably 4 to 12, more preferably 4 to 8, and even more preferably 4 to 6).

[0519] The content ratio of the structural unit (c11) in the structural unit (c1) is preferably 60 mass% or more, more preferably 70 mass% or more, further preferably 80 mass% or more, further preferably 85 mass% or more, and is preferably 100 mass% or less, relative to the total amount (100 mass%) of the structural unit (c1) possessed by the acrylic copolymer (C1).

[0520] Examples of the functional group possessed by the monomer (c2′) include the same functional groups as those possessed by the above-mentioned monomer (a2′).

[0521] As specific monomers (c2'), the same ones as those mentioned above for the monomers (a2') can be mentioned.

[0522] Among them, at least one monomer selected from the group consisting of a hydroxyl group-containing monomer, a carboxyl group-containing monomer, and an epoxy group-containing monomer is preferred, and a carboxyl group-containing monomer is more preferred.

[0523] Specific examples of the hydroxyl group-containing monomer, the carboxyl group-containing monomer, and the epoxy group-containing monomer are the same as those described above for the monomer (a2′).

[0524] The content of the structural unit (c2) in the acrylic copolymer (C1) is preferably 0.5 to 50 mass %, more preferably 1 to 40 mass %, further preferably 5 to 30 mass %, and further preferably 7 to 20 mass %, relative to all structural units (100 mass %) of the acrylic copolymer (C1).

[0525] When the content of the structural unit (c2) is 0.5% by mass or more, the compatibility with the component (D) can be improved, which is preferred.

[0526] In addition, when the content of the structural unit (c2) is 50% by mass or less, the PSA sheet can be made to have good followability to an adherend having large differences in irregularities, which is preferred.

[0527] The acrylic copolymer (C1) may have a structural unit (c3) derived from another monomer (c3') other than the above-mentioned monomers (c1') and (c2').

[0528] As other monomers (c3'), the same ones as the above-mentioned monomers (a3') can be mentioned.

[0529] The content of the structural unit (c3) in the acrylic copolymer (C1) is preferably 0 to 30 mass %, more preferably 0 to 20 mass %, further preferably 0 to 10 mass %, and even more preferably 0 to 5 mass %, relative to all structural units (100 mass %) of the acrylic copolymer (C1).

[0530] In addition, the above-mentioned monomers (c1') to (c3') can be used alone or in combination of two or more.

[0531] (Component (D): energy ray-curable acrylic polymer (D))

[0532] The energy ray-curable acrylic polymer (D) is an acrylic polymer obtained by introducing a polymerizable functional group into a non-energy ray-curable acrylic polymer.

[0533] In addition, the said polymerizable functional group is introduced into the main chain and / or the side chain of the non-energy-ray-curable acrylic polymer.

[0534] It can be considered that by containing (D) component in the middle layer, when irradiating energy line, (D) component reacts with (B) component in adhesive layer (X2) and bonds, and the adhesion between the middle layer (Z2) and adhesive layer (X2) of adhesive sheet (II) is improved. In addition, it can be considered that adhesive layer (X2) and middle layer (Z2) become firm, and residual glue can be suppressed. Therefore, when peeling off cuttings and / or grindings from adhesive sheet (II), the residue of adhesive layer (X2) can be suppressed.

[0535] Examples of the non-energy ray-curable acrylic polymer include acrylic polymers having a structural unit derived from an alkyl (meth)acrylate having a linear or branched alkyl group and acrylic polymers having a structural unit derived from a (meth)acrylate having a cyclic structure.

[0536] The polymerizable functional group may be any group containing an energy ray polymerizable carbon-carbon double bond, and examples thereof include a (meth)acryloyl group and a vinyl group. From the viewpoint of facilitating introduction of an energy ray polymerizable group, a (meth)acryloyl group is preferred.

[0537] The energy ray-polymerizable group may be bonded to the main chain or side chain of the non-energy ray-curable acrylic polymer via an alkylene group, an alkyleneoxy group, a polyalkyleneoxy group, or the like.

[0538] The weight average molecular weight (Mw) of the component (D) is preferably 50,000 to 250,000, more preferably 60,000 to 220,000, further preferably 70,000 to 200,000, further preferably 80,000 to 180,000, and further preferably 85,000 to 150,000.

[0539] When the Mw of (D) component is less than 50,000, the stability of the adhesive sheet obtained over time deteriorates. That is, when the adhesive sheet is kept for a long period, a part of (D) component is transferred into the adhesive layer, and the adhesive force of the adhesive sheet becomes unstable, and the adhesive layer (X2) is easily over-cured after irradiating the energy line. As a result, for the adhesive sheet, in the case of using after long-term storage or in the case of long-term placement under the state of pasting the processing object, the adhesion of the intermediate layer (Z2) after irradiating the energy line and the adhesive layer (X2) becomes insufficient, therefore, when peeling the adhesive sheet, sometimes the adhesive layer (X2) breaks, and the residue of the adhesive layer (X2) is attached to the cutting object and / or the grinding object.

[0540] On the other hand, when the Mw of component (D) exceeds 250,000, the adhesion between the intermediate layer (Z2) and the adhesive layer (X2) after irradiation with energy rays is likely to deteriorate, and when the cut / ground material is peeled off from the adhesive sheet (II), the adhesive layer (X2) sometimes breaks and the residue of the adhesive layer (X2) adheres to the cut and / or ground material.

[0541] As the component (D), from the viewpoint of producing a pressure-sensitive adhesive sheet having excellent temporal stability and from the viewpoint of producing a pressure-sensitive adhesive sheet having improved adhesion between the formed intermediate layer (Z2) and the pressure-sensitive adhesive layer (X2) after irradiation with energy rays, it is preferred that the component (D) comprises an acrylic copolymer (D0) and an energy-ray-curable acrylic copolymer (D1) obtained by reacting with a polymerizable compound (Xd), wherein the acrylic copolymer (D0) has a structural unit (d1) and a structural unit (d2), wherein the structural unit (d1) is derived from a (meth)acrylic acid alkyl ester (d1') having an alkyl group having 1 to 18 carbon atoms (hereinafter also referred to as "monomer (d1')"), and the structural unit (d2) is derived from a functional group-containing monomer (d2') (hereinafter also referred to as "monomer (d2')"), and more preferably the energy-ray-curable acrylic copolymer (D1).

[0542] It should be noted that the copolymerization method of the acrylic copolymers (D0) and (D1) is not particularly limited, and they may be any of a block copolymer, a random copolymer, and a graft copolymer.

[0543] The content of the acrylic copolymer (D1) is preferably 70 to 100 mass %, more preferably 80 to 100 mass %, further preferably 90 to 100 mass %, and even more preferably 100 mass %, relative to the total amount (100 mass %) of the component (D) contained in the intermediate layer-forming composition (z2).

[0544] The number of carbon atoms of the alkyl group contained in the monomer (d1′) is more preferably 4 to 12, further preferably 4 to 8, and further preferably 4 to 6.

[0545] Examples of the monomer (d1′) include those exemplified as the above-mentioned monomer (a1′).

[0546] Among them, butyl (meth)acrylate or 2-ethylhexyl (meth)acrylate is preferred, and butyl (meth)acrylate is more preferred.

[0547] The content of the structural unit (d1) in the acrylic copolymer (D0) is preferably 50 to 99% by mass, more preferably 55 to 95% by mass, further preferably 60 to 90% by mass, and further preferably 65 to 85% by mass, relative to all structural units (100% by mass) of the acrylic copolymer (D0).

[0548] When the content of the structural unit (d1) is 50% by mass or more, the shape of the intermediate layer (Z2) to be formed can be sufficiently maintained, which is preferred.

[0549] In addition, when the content of the structural unit (d1) is less than 99 mass %, the content of the structural unit (d2) having a functional group that becomes a reaction site with the polymerizable compound (Xd) can be sufficiently ensured, and the adhesion between the formed intermediate layer (Z2) and the adhesive layer (X2) after irradiation with energy rays can be improved, so it is preferred.

[0550] The monomer (d2') includes those exemplified as the above-mentioned monomer (a2'), preferably one or more selected from a hydroxyl group-containing monomer, a carboxyl group-containing monomer, and an epoxy group-containing monomer, more preferably a hydroxyl group-containing monomer, further preferably (meth)acrylate hydroxyacrylate, and further preferably 2-hydroxyethyl (meth)acrylate.

[0551] The content of the structural unit (d2) in the acrylic copolymer (D0) is preferably 1 to 50% by mass, more preferably 5 to 45% by mass, further preferably 10 to 40% by mass, and further preferably 15 to 35% by mass, relative to all structural units (100% by mass) of the acrylic copolymer (D0).

[0552] When the content of the structural unit (d2) is 1 mass % or more, sufficient reaction sites with the polymerizable compound (Xd) can be ensured to improve the adhesion between the formed intermediate layer (Z2) and the adhesive layer (X2) after irradiation with energy rays, which is preferred.

[0553] In addition, when the content of the structural unit (d2) is 50% by mass or less, the shape of the intermediate layer (Z2) to be formed can be sufficiently maintained, which is preferred.

[0554] The acrylic copolymer (D0) may have a structural unit (b3) derived from another monomer (d3') other than the above-mentioned monomers (d1') and (d2').

[0555] Examples of the other monomer (d3') include those exemplified as the above-mentioned monomer (a3').

[0556] The content of the structural unit (d3) in the acrylic copolymer (D0) is preferably 0 to 30 mass %, more preferably 0 to 20 mass %, further preferably 0 to 10 mass %, and even more preferably 0 to 5 mass %, relative to all structural units (100 mass %) of the acrylic copolymer (D0).

[0557] In addition, the above-mentioned monomers (d1') to (d3') can be used alone or in combination of two or more.

[0558] The energy ray-curable acrylic copolymer (D1) is a compound obtained by reacting a functional group in the structural unit (d2) of the acrylic copolymer (D0) with a polymerizable compound (Xd) to introduce a polymerizable functional group of the polymerizable compound (Xd) into at least one of the main chain and the side chain of the acrylic copolymer (D0).

[0559] The polymerizable compound (Xd) is not particularly limited as long as it is a compound having a polymerizable functional group and a reactive functional group.

[0560] Among the polymerizable compounds (Xd), preferred are compounds having the above-mentioned reactive substituent and having 1 to 5 polymerizable functional groups per molecule.

[0561] Examples of the reactive substituent include an isocyanate group, a carboxyl group, and an epoxy group, and an isocyanate group is preferred.

[0562] As the polymerizable functional group, there can be mentioned a (meth)acryloyl group, a vinyl group, etc., as described above, and a (meth)acryloyl group is preferred.

[0563] Specific examples of the polymerizable compound (Xd) include the same ones as those mentioned above for the polymerizable compound (Xb).

[0564] The polymerizable compound (Xd) can be used alone or in combination of two or more.

[0565] Among them, (meth)acryloyloxyethyl isocyanate is preferred from the viewpoint of a compound having a suitable isocyanate group as the reactive substituent and an appropriate distance between the acrylic copolymer (D0) and the energy ray polymerizable group.

[0566] In the acrylic copolymer (D1), regarding the relationship between the number of functional groups possessed by the acrylic copolymer (D0) and the amount of the polymerizable compound (Xd), from the viewpoint of improving the adhesion between the formed intermediate layer (Z2) and the adhesive layer (X2) after irradiation with energy rays, the β value calculated according to the following formula (2) is preferably 1 to 50, more preferably 2 to 40, further preferably 3 to 35, and further preferably 5 to 30.

[0567] In addition, the said β value corresponds to the number of energy-beam polymerizable groups which the acrylic copolymer (D1) has.

[0568] Formula (2): β = [P d 〕×〔Q d 〕×〔R d 〕 / 100

[0569] (In formula (2), [Pd 〕 represents the content of the structural unit (d2) relative to 100 parts by mass of all the structural units of the acrylic copolymer (D0), 〔Q d 〕 represents the equivalent weight of the polymerizable compound (Xd) relative to 100 equivalent weights of the functional groups derived from the functional group-containing monomer possessed by the acrylic copolymer (D0), and 〔R d 〕 represents the number of polymerizable functional groups possessed by the polymerizable compound (Xd).

[0570] (Other additives contained in the intermediate layer forming composition)

[0571] The intermediate layer forming composition (z2) may contain other additives within a range not impairing the effects of the present invention.

[0572] Examples of other additives include antioxidants, softeners (plasticizers), fillers, rust preventives, pigments, dyes, and thickeners.

[0573] When these additives are contained, the content of each additive is preferably 0.01 to 6 parts by mass, more preferably 0.01 to 2 parts by mass, based on 100 parts by mass of the component (A).

[0574] <Peeling material>

[0575] The pressure-sensitive adhesive laminate of one embodiment of the present invention may further include a release material laminated on the surface of the pressure-sensitive adhesive layers (X1) and (X2) to be attached to the object to be processed.

[0576] As the release material, a release sheet subjected to double-sided release treatment, a release sheet subjected to single-sided release treatment, or the like can be used. Examples of the release material include a release material obtained by coating a release agent on a release material substrate.

[0577] Examples of the release material substrate include paper such as fully pulped paper, glassine paper, and kraft paper; plastic films such as polyester resin films such as polyethylene terephthalate resin, polybutylene terephthalate resin, and polyethylene naphthalate resin; and olefin resin films such as polypropylene resin and polyethylene resin.

[0578] Examples of the release agent include silicone-based resins, olefin-based resins, isoprene-based resins, butadiene-based resins and other rubber-based elastomers, long-chain alkyl-based resins, alkyd-based resins, and fluororesins.

[0579] The thickness of the release material is not particularly limited, but is preferably 10 to 200 μm, more preferably 25 to 170 μm, and even more preferably 35 to 80 μm.

[0580] <Physical properties of adhesive sheet (II)>

[0581] In one embodiment of the present invention, from the viewpoint of making it easier to perform cutting and grinding in step (4), the adhesive sheet (II) preferably satisfies one or more of the following requirements (α) to (γ), more preferably satisfies any two of the following requirements (α) to (γ), and even more preferably satisfies all of the requirements (α) to (γ).

[0582] Requirement (α): The Young's modulus of the base material (Y2) is 1.0 MPa or more.

[0583] Requirement (β): The thickness of the substrate (Y2) is 5 μm or more.

[0584] Requirement (γ): The storage modulus G′ (23° C.) of the pressure-sensitive adhesive layer (X2) is 0.10 MPa or more.

[0585] From the viewpoint of facilitating cutting and grinding in step (4), the Young's modulus of the substrate (Y2) specified in requirement (α) is preferably 1.0 to 1000 MPa, more preferably 1.5 to 800 MPa, and even more preferably 2.0 to 500 MPa.

[0586] From the viewpoint of facilitating cutting and grinding in step (4), the thickness of the substrate (Y2) specified in requirement (β) is preferably 5 to 250 μm, more preferably 10 to 230 μm, and even more preferably 20 to 210 μm.

[0587] From the viewpoint of facilitating cutting and grinding in step (4), the storage elastic modulus G' (23°C) of the adhesive layer (X2) specified in requirement (γ) is preferably 0.10 to 1 MPa, more preferably 0.12 to 0.9 MPa, and even more preferably 0.14 to 0.8 MPa.

[0588] [Each step of the method for manufacturing a processed product]

[0589] Next, each step of the method for producing a processed product of the present invention will be described in detail.

[0590] The method for producing a processed product of the present invention is a method for producing a processed product subjected to at least one of cutting and grinding using an adhesive laminate.

[0591] The adhesive laminate comprises a heat-expandable adhesive sheet (I), and an adhesive sheet (II), wherein the heat-expandable adhesive sheet (I) comprises a substrate (Y1) and an adhesive layer (X1), and contains heat-expandable particles having a thermal expansion starting temperature (t) in any layer, and the adhesive sheet (II) comprises a substrate (Y2) and an adhesive layer (X2), and the adhesive laminate is formed by directly laminating the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II),

[0592] The method for producing the processed product comprises the following steps (1) to (3) in sequence:

[0593] Step (1): a step of laminating the surface of the adhesive layer (X1) of the adhesive laminate to a support, and laminating an object to be processed to the surface of the adhesive layer (X2) of the adhesive laminate;

[0594] Step (2): a step of performing one or more processes on the object to be processed;

[0595] Step (3): a step of separating the adhesive laminate at an interface P between the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) while maintaining the state where the object to be processed is attached to the surface of the adhesive layer (X2) of the adhesive laminate by heating at a temperature not lower than the thermal expansion starting temperature (t) of the thermally expandable particles,

[0596] The method for producing the processed product further comprises the following step (4):

[0597] Step (4): a step of performing at least one of cutting and grinding on the surface of the object to be processed which is opposite to the surface to which the adhesive layer (X2) is attached,

[0598] The step (4) is carried out in at least any one of the following (X) and (Y),

[0599] (X): implemented in the step (2) as one or more of the above-mentioned processes,

[0600] (Y): carried out after the above step (3).

[0601] In the manufacturing method of the present invention, the above-mentioned adhesive laminate is used. Specifically, the surface of the adhesive layer (X1) of the adhesive sheet (I) of the adhesive laminate is pasted on a support, and the object to be processed is pasted on the surface of the adhesive layer (X2) of the adhesive sheet (II) of the adhesive laminate and used. Therefore, a given processing can be implemented under the state that the object to be processed is fixed to the support. And, after implementing the given processing, the adhesive sheet (II) pasted with the object to be processed that has implemented the given processing can be easily separated from the adhesive sheet (I) together with a small force. That is, the adhesive sheet (II) pasted with the object to be processed that has implemented the given processing can be easily separated from the support. Therefore, the object to be processed that has implemented the given processing can be supplied to the next process without being pasted on a new adhesive sheet.

[0602] Below, refer to Figure 4 and Figure 5 Each step of the production method of the present invention will be described.

[0603] <Process (1)>

[0604] Figure 4 (a) and Figure 5 (a) is a schematic cross-sectional view showing a state where an object to be processed is attached to a support via a pressure-sensitive adhesive laminate.

[0605] In step (1), if Figure 4 (a) and Figure 5 As shown in (a), the objects 60 and 70 are attached to the support 50 via the adhesive laminate 1a of the first embodiment, and the support, the adhesive laminate, and the objects are stacked in this order.

[0606] It should be noted that in Figure 4 and Figure 5 In the figure, the use of Figure 1 Although the example of the adhesive laminate 1a shown in (a) is shown, when the adhesive laminate of the present invention having another structure is used, the support, the adhesive laminate, and the object to be processed are laminated in this order in the same manner.

[0607] like Figure 4 (a) and Figure 5 As shown in (a), in step (1), the processing objects 60, 70 are adhered to the adhesive layer (X2) of the adhesive sheet (II) possessed by the above-mentioned adhesive laminate, and the adhesive layer (X1) of the adhesive sheet (I) possessed by the above-mentioned adhesive laminate and the support 50 are adhered.

[0608] Examples of the object to be processed and attached to the pressure-sensitive adhesive laminate include semiconductor chips, semiconductor wafers, compound semiconductors, semiconductor packages, electronic components, sapphire substrates, displays, and panel substrates.

[0609] In addition, the object to be processed may be a semiconductor wafer having a cut-in groove formed on the surface, or the side of the cut-in groove formed on the surface may be bonded to the adhesive layer (X2) of the adhesive sheet (II). In addition, the object to be processed may be a semiconductor wafer having a modified region formed in advance inside by laser irradiation. In this case, by grinding in step (4), the object to be processed may be segmented using the cut-in groove or the modified region as the segmentation starting point.

[0610] That is, when the object to be processed is a semiconductor wafer having grooves cut into the surface, step (1) of the manufacturing method according to one embodiment of the present invention is the following step (1-C), and the above-mentioned step (4) is the following step (4-C),

[0611] Step (1-C): a step of laminating the surface of the adhesive layer (X1) of the adhesive laminate to a support, and laminating the surface of the semiconductor wafer having the cut groove to the surface of the adhesive layer (X2) of the adhesive laminate,

[0612] Step (4-C): a step of grinding the surface of the semiconductor wafer opposite to the surface to be bonded to the adhesive layer (X2).

[0613] In addition, when the object to be processed is a semiconductor wafer having a modified region as a division start point, step (4) of the manufacturing method according to one embodiment of the present invention is the following step (4-A),

[0614] Step (4-A): a step of grinding the surface of the semiconductor wafer opposite to the surface to be bonded to the adhesive layer (X2).

[0615] The support body can be used to fix the object to be processed in step (2) to improve the processing accuracy.

[0616] It is preferred that the support is attached to the entire adhesive surface of the adhesive layer (X1) of the adhesive laminate.

[0617] Therefore, the support is preferably in the form of a plate. Figure 4 and Figure 5 As shown, the area of ​​the surface of the support 50 on the side to which the adhesive surface 122a of the adhesive layer (X1) is attached is preferably larger than the area of ​​the adhesive surface 122a of the adhesive layer (X1).

[0618] The material constituting the support body can be appropriately selected according to the type of the object to be processed and the processing to be performed in the step (α-2), taking into consideration the required properties such as mechanical strength and heat resistance.

[0619] Specific materials for constituting the support body include, for example: metal materials such as SUS; non-metallic inorganic materials such as glass and silicon wafers; resin materials such as epoxy resin, ABS resin, acrylic resin, engineering plastics, super engineering plastics, polyimide resin, polyamide-imide resin; composite materials such as glass epoxy resin, etc., among which SUS, glass, and silicon wafers are preferred.

[0620] In addition, examples of engineering plastics include nylon, polycarbonate (PC), and polyethylene terephthalate (PET).

[0621] Examples of super engineering plastics include polyphenylene sulfide (PPS), polyethersulfone (PES), and polyetheretherketone (PEEK).

[0622] The thickness of the support can be appropriately selected in consideration of required properties and the like, and is preferably 20 μm or more and 50 mm or less, and more preferably 60 μm or more and 20 mm or less.

[0623] The temperature conditions in the step (1) may be any temperature lower than the expansion starting temperature (t) of the heat-expandable particles.

[0624] <Process (2)>

[0625] In the step (2), the object to be processed, which has been attached to the adhesive layer (X2) of the adhesive laminate of the present invention in the step (1), is subjected to one or more types of processing.

[0626] The processing performed in step (2) includes, for example: sealing the object to be processed using a resin, forming a modified region on the object to be processed as a starting point for division, circuit formation, etching, plating, sputtering, vapor deposition, protective film formation, lamination using a separately prepared adhesive sheet, etc.

[0627] The processing performed in step (2) may be at least one of cutting and grinding of the object to be processed.

[0628] That is, the processing performed in step (2) may be a processing including at least one of a cutting process and a grinding process of the processing object, or may be a processing not including a cutting process and a grinding process of the processing object.

[0629] The temperature conditions in the step (2) are the same as those in the step (1) and may be lower than the expansion starting temperature (t) of the heat-expandable particles.

[0630] Hereinafter, as step (2), in the case of performing a process of forming a modified region as a division starting point on the object to be processed (process (2-A)), a case of performing a process of sealing the object to be processed using a resin (process (2-B)) will be described as an example.

[0631] (Step (2-A))

[0632] The step (2-A) is a step in which the object to be processed is a semiconductor wafer and a modified region serving as a division start point is formed on the semiconductor wafer.

[0633] Specifically, if Figure 4As shown in (b), the surface of the semiconductor wafer opposite to the bonding surface with the adhesive sheet (II) is used as the laser incident surface, and the laser is irradiated in such a way that the laser light converges inside the semiconductor wafer to form a modified region 71 caused by multiphoton absorption, etc. The modified region 71 functions as a starting point for dividing the semiconductor wafer by grinding in step (4).

[0634] It should be noted that in Figure 4 In the manufacturing example shown, step (4) is performed after step (3), and after step (2-A), grinding in step (4) can be performed as one of the one or more processes in step (2). In this case, the semiconductor wafer after singulation can be provided to the next step in a state where the semiconductor wafer after singulation is attached to the adhesive sheet (II) without being separated from the adhesive sheet (II).

[0635] That is, in a manufacturing method according to one embodiment of the present invention, the object to be processed is a semiconductor wafer, and one or more processes in step (2) include the following step (2-A):

[0636] Step (2-A): a step of forming a modified region serving as a division starting point on the semiconductor wafer.

[0637] Step (4) is the following step (4-A),

[0638] Step (4-A): a step of grinding the surface of the semiconductor wafer opposite to the surface to be bonded to the adhesive layer (X2).

[0639] In the case of (XA) or (YA) below, step (4-A) is carried out,

[0640] (XA): carried out after one or more processing steps (2-A),

[0641] (YA): Implemented after step (3).

[0642] (Process (2-B))

[0643] Process (2-B) is the following process: the object to be processed is a semiconductor chip, the semiconductor chip and the peripheral portion of the semiconductor chip in the bonding surface of the adhesive layer (X2) are covered with a sealing material, the sealing material is cured, and a cured sealed body is obtained in which the semiconductor chip is sealed with the cured sealing material.

[0644] like Figure 5 As shown, when the manufacturing method of the present invention has the step (2-B), in the step (1), the semiconductor chip 60 is used as the object to be processed.

[0645] The semiconductor chip 60 may be a conventionally known chip, and its circuit surface is formed by an integrated circuit composed of circuit elements such as transistors, resistors, and capacitors.

[0646] Then, the circuit surface of the semiconductor chip 60 is preferably placed and covered with the adhesive surface of the adhesive layer (X2) of the adhesive sheet (II). The semiconductor chip can be placed using a known device such as a flip chip bonder or a die bonder.

[0647] The layout of the arrangement of the semiconductor chip 60 , the number of arrangements, and the like can be appropriately determined according to the target package format, production quantity, and the like.

[0648] Here, as a manufacturing method of one embodiment of the present invention, it is preferably applied to the following packaging: such as FOWLP, FOPLP, etc., the semiconductor chip 60 is covered with a sealing material in an area larger than the chip size, and a rewiring layer is formed not only on the circuit surface of the semiconductor chip 60 but also in the surface area of ​​the sealing material.

[0649] Therefore, the semiconductor chip 60 is placed on a portion of the adhesive surface of the adhesive layer (X2), and preferably, a plurality of semiconductor chips 60 are placed on the adhesive surface in a state of being arranged at a certain interval, and more preferably, a plurality of semiconductor chips 60 are placed on the adhesive surface in a state of being arranged at a certain interval and in an array of multiple rows and columns.

[0650] The interval between the semiconductor chips 60 can be appropriately determined according to the target packaging format and the like.

[0651] Then, in step (2-B), the semiconductor chip 60 and the bonding surface of the adhesive layer (X1) of at least the peripheral portion of the semiconductor chip 60 are coated with a sealing material (hereinafter also referred to as the "coating step"), and the sealing material is cured to obtain a cured sealed body 61 (hereinafter also referred to as the "curing step") in which the semiconductor chip 60 is sealed with the cured sealing material.

[0652] By placing the semiconductor chip 60 on a portion of the bonding surface of the adhesive layer (X2), the peripheral portion of the semiconductor chip 60 in the bonding surface of the adhesive layer (X2) is formed.

[0653] That is, the peripheral portion of the semiconductor chip 60 refers to the bonding surface of the adhesive layer ( X2 ) corresponding to the gap between adjacent semiconductor chips 60 among the plurality of semiconductor chips 60 .

[0654] In the encapsulation step of step (2-B), the semiconductor chip 60 and the peripheral portion of the semiconductor chip 60 on the bonding surface of the adhesive layer (X2) are first encapsulated with a sealing material. The sealing material encapsulates the entire exposed surface of the semiconductor chip CP and fills the gaps between the plurality of semiconductor chips CP.

[0655] The sealing material has a function of protecting the semiconductor chip CP and its attached elements from the external environment.

[0656] As the sealing material, any material may be appropriately selected from materials used as semiconductor sealing materials, and examples thereof include sealing materials containing a thermosetting resin and sealing materials containing an energy ray-curable resin.

[0657] The sealing material may be in a solid form such as pellets or sheets at room temperature, or may be in a liquid form such as a composition. From the viewpoint of handling, a sealing material in sheet form is preferred.

[0658] As a method of using a sealing material to cover the semiconductor chip 60 and its peripheral parts, it can be appropriately selected from the methods currently used in the semiconductor sealing process according to the type of sealing material. For example, roller lamination, vacuum pressing, vacuum lamination, spin coating, die coating, transfer molding, compression molding, etc. can be used.

[0659] Then, after the encapsulation step is performed, the sealing material is cured, and a cured sealed body 61 in which the semiconductor chip 60 is sealed with the cured sealing material can be obtained.

[0660] It should be noted that the coating step and the curing step of the step (2-B) are preferably performed under a temperature condition lower than the expansion starting temperature (t) of the heat-expandable particles.

[0661] The coating step and the curing step may be performed separately. When the sealing material is heated in the coating step, the sealing material may be directly cured by the heating, and the coating step and the curing step may be performed simultaneously.

[0662] It should be noted that in Figure 5 In the manufacturing example shown, step (4) is performed after step (3), but step (4) may also be performed after step (2-B) as one of the one or more processes in step (2). In this case, the cured sealant may not be separated from the adhesive sheet (II), but may be provided to the next step in a state where the cured sealant is attached to the adhesive sheet (II).

[0663] That is, in a manufacturing method according to one embodiment of the present invention, the object to be processed is a semiconductor chip, and one or more processes in step (2) include the following step (2-B):

[0664] Step (2-B): a step of covering the semiconductor chip and the peripheral portion of the semiconductor chip in the bonding surface of the adhesive layer (X2) with a sealing material, and curing the sealing material to obtain a cured sealed body in which the semiconductor chip is sealed with the cured sealing material,

[0665] In at least any one of the following (XB) and (YB), step (4) is performed,

[0666] (XB): carried out after the above step (2-B) as one or more of the above processing,

[0667] (YB): carried out after the above step (3).

[0668] <Step (3)>

[0669] In step (3), separation occurs at the interface P between the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) of the adhesive laminate by heat treatment at a temperature not lower than the expansion starting temperature (t) (heat treatment for separation).

[0670] Figure 4 (c) and Figure 5 (c) is a schematic cross-sectional view showing a state of separation at the interface P by heat treatment for separation.

[0671] exist Figure 4 (c) and Figure 5 (c) shows a state where the object to be processed, which has been subjected to a predetermined process, is laminated on the pressure-sensitive adhesive sheet (II) and separated by heat treatment for separation.

[0672] The "temperature above the expansion starting temperature (t)" during the heat treatment for separation in step (3) is preferably above "expansion starting temperature (t) + 10°C" and below "expansion starting temperature (t) + 60°C", and more preferably above "expansion starting temperature (t) + 15°C" and below "expansion starting temperature (t) + 40°C".

[0673] Thus, the adhesive sheet (II) can be separated from the adhesive sheet (I) and from the support in a state where the object to be processed which has been subjected to a given processing in step (2) is stacked (pasted). Therefore, the operation of pasting the separated object to be processed to the adhesive sheet can be omitted and the object can be provided for the next step.

[0674] <Step (4)>

[0675] In the step (4), the surface of the object to be processed, which is opposite to the surface to which the adhesive layer (X2) is attached, is subjected to at least one of cutting and grinding.

[0676] For example, by cutting the object to be processed, the object to be processed can be divided into desired sizes. In addition, by grinding, the object to be processed can be adjusted to a desired thickness. It should be noted that both cutting and grinding can be performed to divide the object to be processed and adjust the thickness.

[0677] In addition, for example Figure 4 As shown in (d), the surface of the semiconductor wafer on the opposite side of the bonding surface with the adhesive sheet (II) in which a modified area serving as a starting point for division is formed by laser irradiation is ground. Thus, after the semiconductor wafer is thinned and in a state that is easy to cut, the processing pressure of a grinding stone or the like is used to make the modified area 71 as a starting point for division to produce a gap 72, so that the semiconductor wafer can be singulated into a given size to form a semiconductor chip.

[0678] In addition, if Figure 5 As shown in (d), by cutting the cured seal 61, a single-piece cured seal 61a obtained by singulating the cured seal 61 into semiconductor chip CP units can be obtained. The cutting method for singulating the cured seal 61 is not particularly limited, and a cutting device such as a dicing saw can be cited.

[0679] Although not shown in the figure, the cured sealing body 61 may be ground to expose the circuit surface of the semiconductor chip.

[0680] It should be noted that other steps may be further included between steps (1) to (4), before step (1), and after step (4). For example, a rewiring formation step may be included.

[0681] In addition, as described above, step (4) may be implemented as one of the one or more processes in step (2), or may be implemented after step (3). In addition, step (4) may be implemented as one of the one or more processes in step (2), and may be implemented after step (3).

[0682] For example, as one of the one or more processes in step (2), the surface of the object opposite to the surface to which the adhesive layer (X2) is attached may be ground, and cutting may be performed after step (3).

[0683] In addition, as one of the one or more processing in step (2), the processing object can be cut only in one direction (for example, the X-axis direction in the XY plane of the processing object) on the surface opposite to the bonding surface of the adhesive layer (X2) to divide the processing object into rectangles, and after step (3), only cutting is performed in other directions (for example, the Y-axis direction in the XY plane of the processing object) to further divide the processing object divided into rectangles (for example, into squares).

[0684] Example

[0685] The present invention is described in more detail by the following examples, but the present invention is not limited to the following examples. It should be noted that the physical property values ​​in the following preparation examples and examples are values ​​measured by the following methods.

[0686] <Weight average molecular weight (Mw)>

[0687] The measurement was performed using a gel permeation chromatography apparatus (manufactured by Tosoh Corporation, product name "HLC-8020") under the following conditions, and the measured value converted into standard polystyrene was used.

[0688] (Measurement conditions)

[0689] ·Chromatographic column: A column made by connecting "TSK guard column HXL-L", "TSK gel G2500HXL", "TSK gelG2000HXL", and "TSK gel G1000HXL" (all manufactured by Tosoh Corporation) in this order

[0690] Column temperature: 40℃

[0691] Elution solvent: tetrahydrofuran

[0692] Flow rate: 1.0mL / min

[0693] <Measurement of thickness of each layer>

[0694] The measurement was performed using a constant pressure thickness gauge manufactured by Teclock (model: "PG-02J", in accordance with the standards: JIS K6783, Z1702, Z1709).

[0695] <Average particle size of heat-expandable particles (D 50 )、90% particle size (D 90 )>

[0696] The particle distribution of the heat-expandable particles before expansion at 23° C. is measured using a laser diffraction particle size distribution measuring apparatus (for example, manufactured by Malvern, product name “Mastersizer 3000”).

[0697] Then, the particle sizes corresponding to the 50% and 90% cumulative volume frequencies calculated from the particle size with the smallest particle size in the particle distribution are respectively taken as the "average particle size (D 50 )” and “90% particle size of heat-expandable particles (D 90 )”.

[0698] <Storage modulus E' of heat-expandable base material layer (Y1-1)>

[0699] The heat-expandable base layer (Y1-1) was formed into a size of 5 mm in length×30 mm in width×200 μm in thickness, and the base from which the release material was removed was used as a test sample.

[0700] The storage modulus E' of the test sample at a given temperature was measured using a dynamic viscoelasticity measuring apparatus (manufactured by TA Instruments, product name "DMAQ800") under the conditions of test start temperature 0°C, test end temperature 300°C, heating rate 3°C / min, vibration frequency 1 Hz, and amplitude 20 μm.

[0701] <Shear modulus G′ of the first adhesive layer (X11), the second adhesive layer (X12), and the adhesive layer (X2)>

[0702] The formed first adhesive layer (X11), second adhesive layer (X12), and adhesive layer (X2) were cut into a circle with a diameter of 8 mm, the release material was removed, and the circles were stacked to a thickness of 3 mm to prepare test samples.

[0703] The shear modulus G' of the test sample at a given temperature was measured by the torsional shear method using a viscoelasticity measuring device (manufactured by Anton Paar, device name "MCR300") under the conditions of test start temperature 0°C, test end temperature 300°C, heating rate 3°C / min, and vibration frequency 1 Hz.

[0704] <Probe viscosity value>

[0705] The substrate to be measured was cut into a square with a side length of 10 mm, and then left to stand for 24 hours in an environment of 23° C. and 50% RH (relative humidity) to prepare a test sample.

[0706] The probe tack value of the test sample surface was measured in an environment of 23° C. and 50% RH (relative humidity) using a tack tester (manufactured by Nippon Tokusakushoku Co., Ltd., product name “NTS-4800”) in accordance with JIS Z0237:1991.

[0707] Specifically, in 1 second, the contact load is 0.98N / cm 2After a stainless steel probe with a diameter of 5 mm was brought into contact with the surface of the test sample under the conditions of , the force required to separate the probe from the surface of the test sample at a speed of 10 mm / sec was measured, and the measured value was taken as the probe viscosity value of the test sample.

[0708] <Measurement of Adhesive Strength of Adhesive Layer Before Separation Heat Treatment>

[0709] A 50 μm-thick PET film (product name: "Cosmoshine A4100" manufactured by Toyobo Co., Ltd.) was laminated on the adhesive surface of the adhesive layer formed on the release film to prepare an adhesive sheet with a substrate.

[0710] Then, the release film was removed, and the adhesive surface of the exposed adhesive layer was attached to a stainless steel plate (SUS304 360 polish) as an adherend, and allowed to stand for 24 hours under an environment of 23°C and 50% RH (relative humidity). Then, the adhesive strength at 23°C was measured under the same environment by a 180° peeling method at a tensile speed of 300 mm / min based on JIS Z0237:2000.

[0711] The details of the adhesive resin, additives, heat-expandable particles, and release material used to form each layer in the following examples are as follows.

[0712] <Adhesive resin>

[0713] Acrylic copolymer (i): an acrylic copolymer having a Mw of 600,000, having structural units derived from raw material monomers consisting of 2-ethylhexyl acrylate (2EHA) / 2-hydroxyethyl acrylate (HEA) = 80.0 / 20.0 (mass ratio).

[0714] Acrylic copolymer (ii): an acrylic copolymer having a Mw of 600,000, having structural units derived from raw material monomers consisting of n-butyl acrylate (BA) / methyl methacrylate (MMA) / 2-hydroxyethyl acrylate (HEA) / acrylic acid = 86.0 / 8.0 / 5.0 / 1.0 (mass ratio).

[0715] <Additives>

[0716] Isocyanate crosslinking agent (i): manufactured by Tosoh Corporation, product name “Coronate L”, solid content concentration: 75% by mass.

[0717] Photopolymerization initiator (i): manufactured by BASF, product name “Irgacure 184”, 1-hydroxycyclohexyl phenyl ketone.

[0718] <Thermal expansion particles>

[0719] Thermally expandable particles (i): Japan Fillite Co., Ltd., product name "Expancel 031DU40", expansion starting temperature (t) = 90°C, average particle size (D 50 )=22μm, 90% particle size (D 90 )=30μm.

[0720] <Peeling material>

[0721] Heavy release film: manufactured by Lintec Corporation, product name "SP-PET382150", a release agent layer formed of a silicone release agent is provided on one side of a polyethylene terephthalate (PET) film, thickness: 38 μm.

[0722] Light release film: manufactured by Lintec Corporation, product name “SP-PET381031”, a release agent layer formed of a silicone-based release agent is provided on one side of the PET film, thickness: 38 μm.

[0723] [Example 1]

[0724] An adhesive laminate was prepared according to the following steps. Figure 2 In the adhesive laminate 1d shown in (b), a release material is further laminated on the second adhesive layer (X12) of the adhesive sheet (I) and the adhesive layer (X2) of the adhesive sheet (II), and an intermediate layer (Z2) is provided between the substrate (Y2) of the adhesive sheet (II) and the adhesive layer (X2).

[0725] [1] Preparation of adhesive sheet (I)

[0726] (1-1) Formation of the first adhesive layer (X11)

[0727] 5.0 parts by mass (solid content ratio) of the above-mentioned isocyanate crosslinking agent (i) was added to 100 parts by mass of the solid content of the above-mentioned acrylic copolymer (i) as the adhesive resin, and the mixture was diluted with toluene and stirred uniformly to prepare an adhesive composition having a solid content concentration (active ingredient concentration) of 25% by mass.

[0728] Then, the adhesive composition was applied to the surface of the release agent layer of the heavy release film to form a coating film, and the coating film was dried at 100° C. for 60 seconds to form a first adhesive layer (X11) as a non-thermally expandable adhesive layer with a thickness of 5 μm.

[0729] It should be noted that the shear modulus G'(23) of the first adhesive layer (X11) at 23°C is 2.5×10 5 Pa.

[0730] The adhesive force of the first pressure-sensitive adhesive layer (X11) measured by the above method was 0.3 N / 25 mm.

[0731] (1-2) Formation of the Second Adhesive Layer (X12)

[0732] 0.8 parts by mass (solid content ratio) of the above-mentioned isocyanate crosslinking agent (i) was added to 100 parts by mass of the solid content of the above-mentioned acrylic copolymer (ii) as an adhesive resin, diluted with toluene, and uniformly stirred to prepare an adhesive composition having a solid content concentration (active ingredient concentration) of 25% by mass.

[0733] Then, the adhesive composition was applied on the surface of the release agent layer of the light release film to form a coating film, and the coating film was dried at 100° C. for 60 seconds to form a second adhesive layer (X12) having a thickness of 10 μm.

[0734] It should be noted that the shear modulus G'(23) of the second adhesive layer (X12) at 23°C was 9.0×10 4 Pa.

[0735] The adhesive force of the second pressure-sensitive adhesive layer (X12) measured by the above method was 1.0 N / 25 mm.

[0736] (1-3) Preparation of substrate (Y1)

[0737] (1-3-1) Preparation of composition (y1-1)

[0738] An isocyanate-terminated urethane prepolymer was obtained by reacting an ester diol with isophorone diisocyanate (IPDI), and the prepolymer was reacted with 2-hydroxyethyl acrylate to obtain a bifunctional urethane-acrylic oligomer having a weight average molecular weight (Mw) of 5,000.

[0739] Then, 40 mass % (solid content ratio) of isobornyl acrylate (IBXA) and 20 mass % (solid content ratio) of phenylhydroxypropyl acrylate (HPPA) as energy ray polymerizable monomers were added to 40 mass % (solid content ratio) of the above-synthesized acrylic urethane oligomers, and 2.0 mass parts (solid content ratio) of a photopolymerization initiator (i) and 0.2 mass parts (solid content ratio) of a phthalocyanine pigment as an additive were further added to the total amount (100 mass parts) of the acrylic urethane oligomers and the energy ray polymerizable monomers to prepare an energy ray curable composition.

[0740] Then, the heat-expandable particles (i) were blended into the energy ray-curable composition to prepare a solvent-free composition (y1-1) containing no solvent.

[0741] In addition, content of the heat-expandable particle (i) was 20 mass % with respect to the whole amount (100 mass %) of the composition (y1-1).

[0742] (1-3-2) Preparation of substrate (Y1)

[0743] The prepared composition (y1-1) was applied on the surface of a 50 μm thick polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name “Cosmoshine A4300”, probe viscosity value: 0 mN / 5 mmφ) as a non-thermally expandable substrate to form a coating film.

[0744] Then, an ultraviolet irradiation device (manufactured by EYE GRAPHICS, product name "ECS-401GX") and a high-pressure mercury lamp (manufactured by EYE GRAPHICS, product name "H04-L41") were used to irradiate the sample at an illumination of 160 mW / cm 2 , light intensity 500mJ / cm 2 The coating was cured by irradiating ultraviolet rays under the conditions of , and a heat expandable substrate (Y-1) with a thickness of 50 μm was formed. It should be noted that the above-mentioned illuminance and light quantity when irradiating ultraviolet rays are values ​​measured using an illuminance / light energy meter (manufactured by EIT, product name "UV PowerPuck II").

[0745] The PET film as the above-mentioned non-heat-expandable base material corresponds to the non-heat-expandable base material layer (Y1-2).

[0746] It should be noted that, as a sample for measuring the physical properties of the heat-expandable substrate layer (Y1-1), the resin composition was applied to the surface of the release agent layer of the above-mentioned light release film to form a coating film, and the coating film was dried at 100°C for 120 seconds to similarly form a heat-expandable substrate layer (Y1-1) with a thickness of 50 μm.

[0747] Then, the storage modulus and probe viscosity value of the heat-expandable base layer (Y1-1) at each temperature were measured based on the above-mentioned measurement method. The measurement results are as follows.

[0748] Storage modulus at 23°C E'(23) = 5.0 × 10 8 Pa

[0749] Storage modulus at 100°C E'(100) = 4.0 × 10 6 Pa

[0750] Storage modulus at 208°C E'(208) = 4.0 × 10 5 Pa

[0751] Probe viscosity value = 2mN / 5mmφ

[0752] (1-4) Stacking of layers

[0753] The non-heat-expandable substrate layer (Y1-2) of the substrate (Y1) prepared in the above (1-3) is bonded to the second adhesive layer (X12) formed in the above (1-2), and the heat-expandable substrate layer (Y1-1) is bonded to the second adhesive layer (X12) formed in the above (1-2).

[0754] Then, a pressure-sensitive adhesive sheet (I) was prepared by laminating light release film / second pressure-sensitive adhesive layer (X12) / non-heat-expandable substrate layer (Y1-2) / heat-expandable substrate layer (Y1-1) / first pressure-sensitive adhesive layer (X11) / heavy release film in this order.

[0755] [2] Preparation of adhesive sheet (II)

[0756] (2-1) Formation of Adhesive Layer (X2)

[0757] 8 parts by weight of the isocyanate crosslinking agent (i) was added to 100 parts by weight of the solid content of the acrylic copolymer (ii) as the adhesive resin (solid content ratio), diluted with toluene, and stirred uniformly to prepare an adhesive composition having a solid content concentration (active ingredient concentration) of 25% by weight.

[0758] Then, the adhesive composition was applied on the surface of the release agent layer of the heavy release film to form a coating film, and the coating film was dried at 100° C. for 60 seconds to form an adhesive layer (X2) having a thickness of 20 μm.

[0759] The adhesive force of the adhesive layer (X2) measured by the above method was 0.5 N / 25 mm.

[0760] (2-2) Base material (Y2)

[0761] The substrate (Y2) was a polyethylene terephthalate (PET) film having a thickness of 50 μm (manufactured by Toyobo Co., Ltd., product name: “Cosmoshine A4300”, probe viscosity value: 0 mN / 5 mmφ).

[0762] (2-3) Middle layer (Z2)

[0763] (1) Preparation of composition for forming intermediate layer

[0764] 100 parts by mass of the non-energy ray-curable acrylic copolymer C1, 68 parts by mass of the energy ray-curable acrylic copolymer D1, 2.8 parts by mass of a toluene diisocyanate crosslinking agent (trade name: BHS 8515, manufactured by TOYOCHEM), and 2.7 parts by mass of the above-mentioned photopolymerization initiator (i) were added, and the mixture was diluted with ethyl acetate to prepare a solution of a composition for forming an intermediate layer having a solid content concentration (active ingredient concentration) of 35% by mass.

[0765] (2) Preparation of non-energy ray-curable acrylic copolymer C1

[0766] 90 parts by mass of butyl acrylate (BA) and 10 parts by mass of acrylic acid (AAc) were added to an ethyl acetate solvent, and 1.0 parts by mass of azobisisobutyronitrile (AIBN) was added as a polymerization initiator, and solution polymerization was carried out to obtain a non-energy ray-curable acrylic copolymer C1 (Mw: 500,000).

[0767] (3) Preparation of energy-ray-curable acrylic copolymer D1

[0768] 62 parts by mass of butyl acrylate (BA), 10 parts by mass of methyl methacrylate (MMA), and 28 parts by mass of 2-hydroxyethyl acrylate (HEA) were added to an ethyl acetate solvent, and 1.0 parts by mass of azobisisobutyronitrile (AIBN) was added as a polymerization initiator, and solution polymerization was carried out. After a certain period of time, an acrylic copolymer (BA / MMA / HEA=62 / 10 / 28 (mass %)) was obtained.

[0769] Next, 80 equivalents of methacryloyloxyethyl isocyanate were added to the acrylic copolymer with respect to 100 equivalents of the total hydroxyl groups in the added HEA, and the reaction was carried out to obtain an energy ray-curable acrylic copolymer D1 (Mw: 100,000) having an energy ray polymerizable group in the side chain. The β value of the energy ray-curable acrylic copolymer D1 calculated according to the above formula (2) was 22.4.

[0770] (4) Preparation of the middle layer (Z2)

[0771] The solution of the intermediate layer forming composition prepared as described above was applied to the release-treated surface of a release sheet (manufactured by Lintec Co., Ltd., trade name "SP-PET381031", a polyethylene terephthalate film subjected to silicone release treatment, thickness: 38 μm) to form a coating film having a thickness of 45 μm after drying. Next, the coating film was dried at 100° C. for 2 minutes to form an intermediate layer (Z2), thereby producing a release sheet with an intermediate layer.

[0772] It should be noted that, for the release sheet with an intermediate layer, two identical release sheets were prepared, and the intermediate layers of the two release sheets with an intermediate layer were bonded together to obtain a laminated sheet in which the intermediate layer (Z2) with a thickness of 90 μm was sandwiched between the two release sheets.

[0773] (2-4) Stacking of layers

[0774] One of the release sheets in a laminated sheet in which an intermediate layer (Z2) having a thickness of 90 μm was sandwiched between two release sheets was removed, and the base material (Y2) was laminated on the surface of the exposed intermediate layer (Z2).

[0775] In addition, another release sheet is removed, and the adhesive layer (X2) formed in the above (2-1) is adhered to the surface of the exposed intermediate layer (Z2), thereby producing an adhesive sheet (II) in which the substrate (Y2) / intermediate layer (Z2) / adhesive layer (X2) / heavy release film are stacked in sequence.

[0776] [3] Preparation of adhesive laminate

[0777] The heavy release film of the PSA sheet (I) prepared in the above [1] was removed, and the exposed first PSA layer (X11) was bonded to the substrate (Y2) of the PSA sheet (II) to obtain a PSA laminate.

[0778] The adhesive laminate was measured for peeling forces (F0) and (F1) at the interface P between the first adhesive layer (X11) of the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) before and after the heat treatment according to the following method.

[0779] As a result, the peeling force (F0) = 0.5 N / 25 mm, the peeling force (F1) = 0 mN / 25 mm, and the ratio of the peeling force (F1) to the peeling force (F0) [(F1) / (F0)] was zero.

[0780] <Measurement of peel force (F0)>

[0781] The prepared adhesive laminate was left to stand at 23°C and 50% RH (relative humidity) for 24 hours, then the heavy release film of the adhesive sheet (II) of the adhesive laminate was removed and the exposed adhesive layer (X2) was attached to a stainless steel plate (SUS304, 360 polish).

[0782] Next, the end of the stainless steel plate to which the pressure-sensitive adhesive laminate was bonded was fixed to the lower chuck of a universal tensile testing machine (manufactured by ORIENTEC, product name “Tensilon UTM-4-100”).

[0783] In addition, the adhesive sheet (I) of the adhesive laminate is fixed by the upper chuck of the universal tensile tester so that peeling occurs at the interface P between the first adhesive layer (X11) of the adhesive sheet (I) of the adhesive laminate and the substrate (Y2) of the adhesive sheet (II).

[0784] Then, the peeling force measured when peeling was performed at the interface P at a tensile speed of 300 mm / min by a 180° peeling method according to JIS Z0237:2000 under the same environment as above was referred to as “peeling force (F0)”.

[0785] <Measurement of peel force (F1)>

[0786] The heavy release film of the adhesive sheet (II) of the produced adhesive laminate was removed, and the exposed adhesive layer (X2) was attached to a stainless steel plate (SUS304, 360-grade finish).

[0787] Then, the stainless steel plate and the pressure-sensitive adhesive laminate were heated at 240° C. for 3 minutes to expand the heat-expandable particles in the heat-expandable base material layer (Y1-2) of the pressure-sensitive adhesive laminate.

[0788] Then, in the same manner as the above-mentioned measurement of the peel force (F0), the peel force measured when peeling occurs at the interface P between the first adhesive layer (X11) of the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) under the above-mentioned conditions is referred to as the "peel force (F1)".

[0789] It should be noted that in the measurement of the peel force (F1), when an attempt is made to fix the adhesive sheet (I) of the adhesive laminate using the upper chuck of the universal tensile tester, the adhesive sheet (I) is completely separated at the interface P and cannot be fixed. In this case, the measurement is terminated and the peel force (F1) at this time is "0 mN / 25 mm".

[0790] [Example 2]

[0791] A pressure-sensitive adhesive sheet (II) to which a processing object was attached was prepared by the following steps.

[0792] (1) Fixing of semiconductor wafers

[0793] The light release film of the adhesive laminate produced in Example 1 was removed, and the exposed adhesive surface of the second adhesive layer (X12) of the adhesive sheet (I) was attached to a support (glass).

[0794] Then, the circuit surface side surface of the semiconductor wafer having the circuit surface formed with the pattern was bonded to the adhesive layer (X2) of the adhesive sheet (II), and the semiconductor wafer was fixed to the support via the adhesive laminate produced in Example 1.

[0795] (2) Formation of modified regions

[0796] An invisible laser irradiation device (manufactured by Tokyo Seimitsu Co., Ltd., device name "ML300PlusWH") was used to irradiate the semiconductor wafer from the surface opposite to the circuit formation surface, thereby forming a modified region serving as a division starting point inside the semiconductor wafer.

[0797] (3) Separation at interface P

[0798] After the above (2), the adhesive laminate was heat treated for 3 minutes at 120°C, which is higher than the expansion starting temperature (90°C) of the heat-expandable particles. Then, the first adhesive layer (X11) of the adhesive sheet (I) and the interface P of the substrate (Y2) of the adhesive sheet (II) can be easily separated together.

[0799] Then, after separation, a pressure-sensitive adhesive sheet (II) in a state where the semiconductor wafer having the reformed region formed therein was adhered was obtained.

Claims

1. A method for producing a processed product, which is a method for producing a processed product subjected to at least one of cutting and grinding using an adhesive laminate, The adhesive laminate comprises a heat-expandable adhesive sheet (I), and an adhesive sheet (II), wherein the heat-expandable adhesive sheet (I) comprises a substrate (Y1) and an adhesive layer (X1), and contains heat-expandable particles having a thermal expansion starting temperature (t) in any layer, and the adhesive sheet (II) comprises a substrate (Y2) and an adhesive layer (X2). The substrate (Y1) of the pressure-sensitive adhesive sheet (I) comprises a heat-expandable substrate layer (Y1-1) containing the heat-expandable particles. The pressure-sensitive adhesive sheet (I) has a structure in which a substrate (Y1) is sandwiched between a first pressure-sensitive adhesive layer (X11) and a second pressure-sensitive adhesive layer (X12). The adhesive laminate has a structure in which the first adhesive layer (X11) of the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) are directly laminated. The surface of the second adhesive layer (X12) of the adhesive sheet (I) is the surface to be attached to the support. The method for producing the processed product comprises the following steps (1) to (3) in sequence: Step (1): a step of laminating the surface of the adhesive layer (X1) of the adhesive laminate to a support, and laminating an object to be processed to the surface of the adhesive layer (X2) of the adhesive laminate; Step (2): a step of performing one or more processes on the object to be processed; Step (3): a step of separating the adhesive laminate at an interface P between the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) while maintaining the state in which the object to be processed is adhered to the surface of the adhesive layer (X2) of the adhesive laminate by heating at a temperature not lower than the thermal expansion starting temperature (t) of the thermally expandable particles, The method for producing the processed product further comprises the following step (4): Step (4): a step of performing at least one of cutting and grinding on the surface of the object to be processed which is opposite to the surface to which the adhesive layer (X2) is attached, The step (4) is carried out in at least any one of the following (X) and (Y), (X): one or more of the above-mentioned processes is carried out in the above-mentioned step (2), (Y): carried out after the step (3).

2. The manufacturing method according to claim 1, wherein: The thermal expansion starting temperature (t) of the thermally expandable particles is 60 to 270°C.

3. The manufacturing method according to claim 1, wherein: The substrate (Y1) included in the pressure-sensitive adhesive sheet (I) includes a heat-expandable substrate layer (Y1-1) and a non-heat-expandable substrate layer (Y1-2).

4. The manufacturing method according to claim 1 or 2, wherein: The first adhesive layer (X11) is a heat-expandable adhesive layer containing the heat-expandable particles. The second pressure-sensitive adhesive layer (X12) is a non-thermally expandable pressure-sensitive adhesive layer.

5. The manufacturing method according to claim 1 or 2, wherein: The surface of the substrate (Y1) on which the first pressure-sensitive adhesive layer (X11) is laminated is subjected to an adhesion-facilitating treatment.

6. The manufacturing method according to claim 1 or 2, wherein: The surface of the substrate (Y2) on the side on which the pressure-sensitive adhesive sheet (I) is laminated is a release-treated surface.

7. The manufacturing method according to claim 1 or 2, wherein: The pressure-sensitive adhesive sheet (II) has an intermediate layer (Z2) between the substrate (Y2) and the pressure-sensitive adhesive layer (X2).

8. The manufacturing method according to claim 1 or 2, wherein: The pressure-sensitive adhesive layer (X2) of the pressure-sensitive adhesive sheet (II) is an energy-beam-curable pressure-sensitive adhesive layer.

9. The manufacturing method according to claim 1 or 2, wherein: The adhesive sheet (II) satisfies at least one of the following requirements (α) to (γ), Requirement (α): The Young's modulus of the base material (Y2) is 1.0 MPa or more; Requirement (β): The thickness of the substrate (Y2) is 5 μm or more; Requirement (γ): The storage elastic modulus G′ (23° C.) of the pressure-sensitive adhesive layer (X2) is 0.1 MPa or more.

10. The manufacturing method according to claim 1 or 2, wherein: The object to be processed is a semiconductor wafer, The one or more processes in the step (2) include the following step (2-A), Step (2-A): a step of forming a modified region serving as a division starting point on the semiconductor wafer, The step (4) is the following step (4-A), Step (4-A): a step of grinding the surface of the semiconductor wafer opposite to the surface to be bonded to the adhesive layer (X2). The step (4-A) is carried out in the case of (XA) or (YA) below, (XA): one or more of the above-mentioned processes are performed after the above-mentioned step (2-A), (YA): carried out after the step (3).

11. The manufacturing method according to claim 1 or 2, wherein: The object to be processed is a semiconductor chip, The one or more processing steps in step (2) include the following step (2-B), Step (2-B): a step of covering the semiconductor chip and the peripheral portion of the semiconductor chip in the bonding surface of the adhesive layer (X2) with a sealing material, and curing the sealing material to obtain a cured sealed body in which the semiconductor chip is sealed with the cured sealing material, The step (4) is carried out in at least one of the following (XB) and (YB), (XB): one or more of the above-mentioned processes are performed after the above-mentioned step (2-B), (YB): carried out after the step (3).

12. The manufacturing method according to claim 1 or 2, wherein: The object to be processed is a semiconductor wafer having a modified region as a division starting point, The step (4) is the following step (4-A), Step (4-A): a step of grinding the surface of the semiconductor wafer opposite to the surface to be bonded to the adhesive layer (X2).

13. The manufacturing method according to claim 1 or 2, wherein: The object to be processed is a semiconductor wafer having a cut groove as a starting point for division, The step (1) is the following step (1-C), the step (4) is the following step (4-C), Step (1-C): a step of attaching the surface of the adhesive layer (X1) of the adhesive laminate to a support, and attaching the surface of the semiconductor wafer having the cut groove to the surface of the adhesive layer (X2) of the adhesive laminate, Step (4-C): a step of grinding the surface of the semiconductor wafer opposite to the surface to be bonded to the adhesive layer (X2).

14. An adhesive laminate for use in producing a processed product subjected to at least one of cutting and grinding, The adhesive laminate comprises a heat-expandable adhesive sheet (I) and an adhesive sheet (II), wherein the heat-expandable adhesive sheet (I) comprises a substrate (Y1) and an adhesive layer (X1) and contains heat-expandable particles in any layer, and the adhesive sheet (II) comprises a substrate (Y2) and an adhesive layer (X2). The substrate (Y1) of the pressure-sensitive adhesive sheet (I) comprises a heat-expandable substrate layer (Y1-1) containing the heat-expandable particles. The pressure-sensitive adhesive sheet (I) has a structure in which a substrate (Y1) is sandwiched between a first pressure-sensitive adhesive layer (X11) and a second pressure-sensitive adhesive layer (X12). The adhesive laminate has a structure in which the first adhesive layer (X11) of the adhesive sheet (I) and the substrate (Y2) of the adhesive sheet (II) are directly laminated. The surface of the second pressure-sensitive adhesive layer (X12) of the pressure-sensitive adhesive sheet (I) is the surface to be bonded to the support.