Crosslinked rubber composition

By using high-fiber para-aramid short fibers and organic peroxide crosslinking agents in crosslinked rubber compositions, the problem of insufficient compression and tensile properties is solved, and the longitudinal elastic modulus of high compression energy storage is improved, making it suitable for rubber products such as transmission belts and tires.

CN111902479BActive Publication Date: 2026-11-17BANDO CHEM IND LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN201980021132.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-03-23
Filing Date
2019-03-20
Publication Date
2026-11-17
Estimated Expiration
2039-03-20

AI Technical Summary

Technical Problem

Existing crosslinked rubber compositions have shortcomings in compression and tensile properties, especially in the low longitudinal elastic modulus of compression energy storage, which makes it difficult to meet the requirements of certain applications.

Method used

Para-aramid short fibers with a filament fineness of 2.5 dtex or higher are used as reinforcing materials, and cross-linked rubber compositions are prepared using organic peroxides as cross-linking agents. The orientation and content of the fibers are optimized to improve the longitudinal elastic modulus of compression energy storage. At the same time, other short fibers can be selected to improve the surface friction and wear resistance.

Benefits of technology

It significantly improves the compression and tensile properties of crosslinked rubber compositions, especially the longitudinal modulus of elasticity during compression, making them suitable for rubber products under severe compression deformation conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002694206130000071
    Figure BDA0002694206130000071
Patent Text Reader

Abstract

The present invention provides a crosslinked rubber composition comprising a rubber component and para-aramid short fibers with a fineness of 2.5 dtex or more dispersed in the rubber component.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a crosslinked rubber composition. Background Technology

[0002] In various rubber products, cross-linked rubber compositions containing para-aramid short fibers are used. For example, Patent Document 1 discloses a drive belt using a rubber composition containing para-aramid short fibers. Patent Document 2 discloses a tire using a rubber composition containing para-aramid short fibers. Patent Document 3 discloses a hose using a rubber composition containing para-aramid short fibers.

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 2013-108564

[0006] Patent Document 2: Japanese Patent Application Publication No. 2013-18893

[0007] Patent Document 3: Japanese Patent Application Publication No. 2005-200545 Summary of the Invention

[0008] The present invention is a crosslinked rubber composition, wherein the crosslinked rubber composition contains a rubber component and para-aramid short fibers with a fineness of 2.5 dtex or more dispersed in the aforementioned rubber component. Detailed Implementation

[0009] The implementation method will now be described in detail.

[0010] The crosslinked rubber composition of the embodiment contains a rubber component and para-aramid short fibers with a filament fineness of 2.5 dtex or more. It should be noted that, hereinafter, "para-aramid short fibers with a filament fineness of 2.5 dtex or more" will be referred to as "coarse-diameter aramid short fibers".

[0011] By incorporating para-aramid short fibers into the crosslinked rubber composition, an increase in the tensile storage modulus of elasticity can be predicted; however, an increase in the compressive storage modulus of elasticity is also required. To address this, the crosslinked rubber composition according to the embodiment, by containing para-aramid short fibers with a filament fineness of 2.5 dtex or higher, achieves a higher compressive storage modulus of elasticity. It is presumably because, compared to existing para-aramid short fibers with a filament fineness of 1.7 dtex, the larger diameter para-aramid short fibers with higher filament fineness can suppress fibrillation within the rubber component, effectively exhibiting its fibrous properties.

[0012] Examples of rubber components include ethylene-α-olefin elastomers, chloroprene rubber (CR), chlorosulfonated polyethylene rubber (CSM), hydrogenated acrylonitrile rubber (H-NBR), natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene rubber (SBR), nitrile rubber (NBR), and butyl rubber (IIR). The rubber component preferably includes one or more of these components. For use in transmission belts, it is preferable to include ethylene-α-olefin elastomers, chloroprene rubber (CR), chlorosulfonated polyethylene rubber (CSM), and hydrogenated acrylonitrile rubber (H-NBR), and more preferably, ethylene-α-olefin elastomers.

[0013] Examples of ethylene-α-olefin elastomers include ethylene propylene diene monomer (hereinafter referred to as "EPDM"), ethylene propylene copolymer (EPM), ethylene butene copolymer (EBM), and ethylene octene copolymer (EOM). Ethylene-α-olefin elastomers preferably contain one or more of these elastomers, and from a general viewpoint, EPDM is more preferably included.

[0014] The para-aramid short fibers constituting the coarse-diameter aromatic polyamide short fibers may include poly(p-phenylene terephthalamide) short fibers (PPTA short fibers), or copolymerized p-phenylene-3,4'-oxydiphenylene terephthalamide short fibers, or both. From the viewpoint of obtaining a high compressive energy storage longitudinal elastic modulus, it is preferable that the para-aramid short fibers constituting the coarse-diameter aromatic polyamide short fibers include at least poly(p-phenylene terephthalamide) short fibers (PPTA short fibers).

[0015] Coarse-diameter aromatic polyamide short fibers are dispersed in the rubber component. From the viewpoint of obtaining a high compressive energy storage longitudinal modulus, the coarse-diameter aromatic polyamide short fibers can be oriented in one direction. From the viewpoint of obtaining a high compressive energy storage longitudinal modulus, the content (C1) of coarse-diameter aromatic polyamide short fibers in the crosslinked rubber composition of the embodiment is preferably 1 part by mass or more and 18 parts by mass or less, more preferably 3 parts by mass or more and 15 parts by mass or less, and even more preferably 5 parts by mass or more and 12 parts by mass or less, relative to 100 parts by mass of the rubber component.

[0016] The fineness (D1) of the coarse-diameter aramid staple fiber is 2.5 dtex or more, and from the viewpoint of obtaining a high compressive energy storage longitudinal modulus, it is preferably 2.7 dtex or more, more preferably 3.0 dtex or more, even more preferably 3.3 dtex or more, and preferably 5.0 dtex or less. From the viewpoint of obtaining a high compressive energy storage longitudinal modulus, the fiber length (L1) of the coarse-diameter aramid staple fiber is preferably 0.5 mm or more and 10 mm or less, more preferably 1 mm or more and 5 mm or less, and even more preferably 2 mm or more and 4 mm or less.

[0017] From the viewpoint of improving the surface's resistance to friction and wear, the crosslinked rubber composition of the embodiment may further contain short fibers other than coarse-diameter aromatic polyamide short fibers dispersed in the rubber component. Examples of short fibers other than coarse-diameter aromatic polyamide short fibers include, for example, nylon short fibers, vinylon short fibers, polyester short fibers, cellulose short fibers such as cotton, meta-aromatic polyamide short fibers, and para-aromatic polyamide short fibers with a filament fineness of less than 2.5 dtex. It is preferable that the short fibers other than coarse-diameter aromatic polyamide short fibers include one or more of these short fibers. From the viewpoint of improving the surface's resistance to friction and wear, it is preferable to include short fibers other than para-aromatic polyamide short fibers, and more preferably, nylon short fibers.

[0018] From the viewpoint of improving the surface's resistance to friction and wear, the content (C2) of short fibers other than coarse-diameter aromatic polyamide short fibers in the crosslinked rubber composition of the embodiment, relative to 100 parts by mass of the rubber component, is preferably 5 parts by mass or more and 30 parts by mass or less, more preferably 10 parts by mass or more and 20 parts by mass or less. From the viewpoint of improving the surface's resistance to friction and wear, the content (C2) of short fibers other than coarse-diameter aromatic polyamide short fibers in the crosslinked rubber composition of the preferred embodiment is greater than the content (C1) of coarse-diameter aromatic polyamide short fibers. From the viewpoint of improving the surface's resistance to friction and wear, the ratio (C2 / C1) of the content (C2) of short fibers other than coarse-diameter aromatic polyamide short fibers to the content (C1) of coarse-diameter aromatic polyamide short fibers is preferably 1.1 or more and 2.5 or less, more preferably 1.5 or more and 2.0 or less.

[0019] From the viewpoint of improving the surface's resistance to friction and wear, the filament fineness (D2) of short fibers other than coarse-diameter aramid short fibers is preferably 3.0 dtex or more and 10 dtex or less, more preferably 5.0 dtex or more and 8.0 dtex or less. From the viewpoint of improving the surface's resistance to friction and wear, it is preferable that the filament fineness (D2) of short fibers other than coarse-diameter aramid short fibers is greater than the filament fineness (D1) of coarse-diameter aramid short fibers. From the viewpoint of improving the surface's resistance to friction and wear, the ratio (D2 / D1) of the filament fineness (D2) of short fibers other than coarse-diameter aramid short fibers to the filament fineness (D1) of coarse-diameter aramid short fibers is preferably 1.1 or more and 3.5 or less, more preferably 2.0 or more and 3.0 or less.

[0020] From the viewpoint of improving the surface's resistance to friction and wear, the fiber length (L2) of the short fibers other than the coarse-diameter aramid short fibers is preferably 0.5 mm or more and 10 mm or less, more preferably 1 mm or more and 5 mm or less, and even more preferably 2 mm or more and 4 mm or less. From the viewpoint of improving the surface's resistance to friction and wear, the ratio (L2 / L1) of the fiber length (L2) of the short fibers other than the coarse-diameter aramid short fibers to the fiber length (L1) of the coarse-diameter aramid short fibers is preferably 0.50 or more and 1.5 or less, more preferably 0.80 or more and 1.2 or less. From the viewpoint of improving the surface's resistance to friction and wear, it is preferable that the fiber length (L2) of the short fibers other than the coarse-diameter aramid short fibers is the same as the fiber length (L1) of the coarse-diameter aramid short fibers.

[0021] The rubber component of the crosslinked rubber composition of the embodiment is crosslinked. The rubber component can be crosslinked using an organic peroxide as a crosslinking agent, or it can be crosslinked using sulfur as a crosslinking agent. Furthermore, it can be crosslinked using both organic peroxide and sulfur as crosslinking agents. From the viewpoint of obtaining a high compressive energy storage longitudinal elastic modulus, it is preferable to crosslink using at least an organic peroxide as a crosslinking agent.

[0022] Examples of organic peroxides used as crosslinking agents include dicumyl peroxide, 1,3-bis(tert-butylperoxyisopropyl)benzene, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane. The organic peroxide preferably contains one or more of these peroxides, and from the viewpoint of obtaining a high compressive energy storage longitudinal modulus, dicumyl peroxide is preferred. From the viewpoint of obtaining a high compressive energy storage longitudinal modulus, the amount of organic peroxide in the uncrosslinked rubber composition before crosslinking is preferably 1 part by mass and 7 parts by mass or less, more preferably 2 parts by mass and 5 parts by mass or less, relative to 100 parts by mass of the rubber component.

[0023] For the crosslinked rubber composition of the embodiments, from the viewpoint of obtaining a high compressive energy storage longitudinal modulus, the rubber component can also be crosslinked by means of a co-crosslinking agent. Examples of co-crosslinking agents include: N,N'-m-phenylene bismaleimide, trimethylolpropane trimethacrylate, ethylene glycol dimethacrylate, triallyl isocyanurate, liquid polybutadiene, etc. It is preferable to use one or more of these crosslinking agents, and from the viewpoint of obtaining a high compressive energy storage longitudinal modulus, N,N'-m-phenylene bismaleimide is more preferably used. From the viewpoint of obtaining a high compressive energy storage longitudinal modulus, the amount of co-crosslinking agent in the uncrosslinked rubber composition before crosslinking is preferably 0.5 parts by mass or more and 7 parts by mass or less, more preferably 2 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the rubber component.

[0024] In addition, the crosslinked rubber composition of the embodiments may, as needed, contain reinforcing materials such as carbon black or silica, functional fillers, softeners, vulcanization accelerators, vulcanization accelerators, processing aids, anti-aging agents, and other rubber compounds.

[0025] The crosslinked rubber composition of the embodiment can be obtained as follows: An uncrosslinked rubber composition is prepared by mixing a rubber component with a rubber complex containing coarse-diameter aromatic polyamide short fibers and a crosslinking agent using a rubber mixer; the rubber component is then crosslinked by heating and pressurizing the mixture using a processing method appropriate to the rubber product, thereby obtaining a crosslinked rubber composition. Examples of rubber mixers include, for example, closed kneaders or Banbury mixers, and open roller mixers.

[0026] The longitudinal elastic modulus of the crosslinked rubber composition of the embodiment, under compression at 100°C in the grain direction, is preferably 65.0 MPa or more, more preferably 70.0 MPa or more. This longitudinal elastic modulus of compression (E') can be determined based on JIS K 6265:2001.

[0027] The longitudinal elastic modulus of the crosslinked rubber composition of the embodiment, when stretched at 100°C in the grain direction, is preferably 255 MPa or more, more preferably 265 MPa or more. This longitudinal elastic modulus (E') can be measured based on JIS K 6394:2007.

[0028] The ratio of the compressive energy storage longitudinal elastic modulus (E') of the crosslinked rubber composition at 100°C in the texture direction to the tensile energy storage longitudinal elastic modulus (E') at 100°C in the texture direction is preferably 0.260 or more, more preferably 0.270 or more.

[0029] The crosslinked rubber composition of the embodiments can be applied to rubber products such as drive belts, tires, and hoses, and is especially suitable for drive belts that are subjected to severe compression deformation during use.

[0030] Example

[0031] (Cross-linked rubber composition)

[0032] The crosslinked rubber compositions of Examples 1-2 and Comparative Examples were prepared. The composition of each crosslinked rubber composition is shown in Table 1.

[0033] <Example 1>

[0034] The rubber component is EPDM (JSR T7241, manufactured by JSR Corporation). For every 100 parts by weight of this rubber component, the following are added: 45 parts by weight of FEF carbon black (Seast SO, manufactured by Tokai Carbon Co., Ltd.) as a reinforcing material; 10 parts by weight of powdered ultra-high molecular weight polyethylene resin (HI-ZEX MILLION240S, manufactured by Mitsui Chemicals Co., Ltd.) as a functional filler; 10 parts by weight of oil (SUNPAR 2280, manufactured by JAPAN SUN OIL Co., Ltd.) as a softener; 5 parts by weight of zinc oxide (three types of zinc oxide, manufactured by Sakai Chemical Industry Co., Ltd.) as a vulcanization accelerator; 1 part by weight of stearic acid (Lunac, manufactured by Kao Corporation) as a processing aid; 4 parts by weight of co-crosslinking agent (VULNOC PM, manufactured by Ouchi Shinsei Chemical Co., Ltd.); and PEROXYMON as a crosslinking agent. An uncrosslinked rubber composition was prepared by mixing 7 parts by weight of F40 (purity 40% by mass, manufactured by Nippon Oil Co., Ltd.) (active ingredient: 2.8 parts by weight), 18 parts by weight of nylon staple fiber (Reona 66, manufactured by Asahi Kasei Co., Ltd., filament fineness: 6.7 dtex, fiber length: 3 mm), and 10 parts by weight of coarse-diameter PPTA staple fiber (Kevlar, manufactured by Dupont Toray Co., Ltd., fiber length: 3 mm) with a filament fineness of 2.5 dtex. The uncrosslinked rubber composition was then heated and pressurized to prepare a crosslinked rubber composition for compression and tensile tests, which is designated as Example 1.

[0035] <Example 2>

[0036] As the coarse-diameter PPTA short fiber, PPTA short fiber with a filament fineness of 3.3 dtex (manufactured by Kevlar, Dupont Toray Co., Ltd., fiber length: 3 mm) was used. Otherwise, the crosslinked rubber composition for compression and tensile tests was prepared in the same manner as in Example 1, and it was designated as Example 2.

[0037] <Comparative Example>

[0038] PPTA short fibers with a filament fineness of 1.7 dtex (manufactured by Kevlar, Dupont Toray Co., Ltd., fiber length: 3 mm) were used instead of coarse-diameter aramid short fibers. Otherwise, the crosslinked rubber composition for compression and tensile tests was prepared in the same manner as in the examples and was designated as a comparative example.

[0039] [Table 1]

[0040]

[0041] (Experimental Methods)

[0042] For each crosslinked rubber composition of Examples 1-2 and the Comparative Examples, cylindrical test pieces with the axial direction aligned with the grain direction were prepared. Based on JISK 6265:2001, using a deflectometer (FT-1200, manufactured by Uejima Manufacturing Co., Ltd.), the compressive storage modulus (E') at 100°C in the grain direction was measured under the conditions of a test temperature of 100°C, a test static load of 250N, a test dynamic load of 250N, and a test frequency of 10Hz. Additionally, elongated test pieces with the length direction aligned with the grain direction were prepared. Based on JISK 6394:2007, using a dynamic viscoelasticity testing machine, the tensile storage modulus (E') at 100°C in the grain direction was measured under the conditions of a test temperature of 100°C, a test dynamic strain of 0.1%, and a test frequency of 10Hz. Then, the ratio of the compressive longitudinal elastic modulus (E') at 100°C in the texture direction to the tensile longitudinal elastic modulus (E') at 100°C in the texture direction is calculated.

[0043] (Experimental Results)

[0044] The test results are shown in Table 1. According to Table 1, compared with the comparative example, Examples 1 and 2 using coarse-diameter PPTA short fibers have higher compressed longitudinal elastic modulus (E') and tensile longitudinal elastic modulus (E') at 100°C in the grain direction. Moreover, the ratio of compressed longitudinal elastic modulus (E') to tensile longitudinal elastic modulus (E') at 100°C in the grain direction is also higher.

[0045] Industrial availability

[0046] This invention is useful in the technical field of crosslinked rubber compositions.

Claims

1. A crosslinked rubber composition, characterized in that, contain: Rubber components, and The filaments dispersed in the rubber component are para-aramid short fibers with a fineness of 2.5 dtex or more and 3.3 dtex or less. The length of the para-aramid short fibers is more than 2 mm and less than 5 mm.

2. The crosslinked rubber composition according to claim 1, wherein, The content of para-aramid short fibers is more than 1 part by mass and less than 18 parts by mass relative to 100 parts by mass of the rubber component.

3. The crosslinked rubber composition according to claim 1 or 2, wherein, It also contains short fibers other than the para-aramid short fibers dispersed in the rubber component.

4. The crosslinked rubber composition according to claim 3, wherein, The content of short fibers other than the para-aramid short fibers is greater than the content of the para-aramid short fibers.

5. The crosslinked rubber composition according to claim 4, wherein, The ratio of the content of short fibers other than the para-aramid short fibers to the content of the para-aramid short fibers is 1.1 or more and 2.5 or less.

6. The crosslinked rubber composition according to claim 3, wherein, The fineness of the filaments of the short fibers other than the para-aramid short fibers is greater than that of the para-aramid short fibers.

7. The crosslinked rubber composition according to claim 6, wherein, The ratio of the fineness of the filament of the short fibers other than the para-aramid short fibers to the fineness of the filament of the para-aramid short fibers is 1.1 or more and 3.5 or less.

8. The crosslinked rubber composition according to claim 3, wherein, The ratio of the fiber length of the short fibers other than the para-aramid short fibers to the fiber length of the para-aramid short fibers is 0.5 or more and 1.5 or less.

9. The crosslinked rubber composition according to claim 1 or 2, wherein, The rubber component contains an ethylene-α-olefin elastomer.

10. The crosslinked rubber composition according to claim 1 or 2, wherein, The rubber component is cross-linked using organic peroxide as a cross-linking agent.

11. The crosslinked rubber composition according to claim 1 or 2, wherein, The rubber component is also cross-linked by means of a co-crosslinking agent.

12. The crosslinked rubber composition according to claim 1 or 2, wherein, The para-aromatic polyamide short fibers comprise poly(p-phenylene terephthalamide) short fibers.

13. The crosslinked rubber composition according to claim 1 or 2, wherein, The ratio of the compressive energy storage longitudinal elastic modulus to the tensile energy storage longitudinal elastic modulus at 100°C in the texture direction is greater than 0.260.

Citation Information

Patent Citations

  • Rubber composition between hose-reinforcing layers and hose using the same

    JP2005200545A

  • Pneumatic tire

    JP2013018893A

  • Transmission belt

    JP2013108564A

  • Short rubber reinforcement fiber, rubber composition containing said short fiber, and power transmission belt