A cold rolling iron-containing waste emulsified oil regeneration system and regeneration method
Through the hydrochloric acid leaching method and ferrous chloride solution decomposition technology, combined with active adsorbents, the problem of regeneration and iron recovery of cold-rolled iron-containing waste emulsified oil has been solved, and high-quality emulsified oil regeneration and efficient iron recovery have been achieved. Reduce resource waste and pollution.
Patent Information
- Application Number
- CN202010845640.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-20
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-08-20
AI Technical Summary
Existing technology cannot effectively solve the problems of recycling and iron recovery of cold-rolled iron-containing waste emulsified oil, resulting in poor regeneration quality and waste of resources.
The hydrochloric acid acid leaching method is used to separate iron and oil, combined with the decomposition of ferrous chloride solution, activated clay and activated carbon are used to adsorb and purify the emulsified oil, and the hydrochloric acid is recovered through the exhaust gas purification device to realize hydrochloric acid recycling.
It achieves high-quality emulsified oil regeneration with high saponification value, good lubrication performance, iron yield as high as 99.5%, and reduces pollutant emissions and resource waste.
Smart Images

Figure CN111925861B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waste emulsified oil recycling and utilization, relates to waste emulsified oil regeneration, and particularly relates to a cold-rolled iron-containing waste emulsified oil regeneration system device and a regeneration method thereof. Background Art
[0002] With the continuous development of my country's scientific and technological level and productivity, the demand for cold-rolled plates in the fields of construction, machinery, automobiles, agricultural production, etc. is increasing, which increases the demand for cold-rolled emulsions. my country's small and medium-sized machinery processing plants use more than 100 tons of emulsions each year, and large cold rolling plants replace hundreds of tons of waste emulsified oil each time. In the process of mechanical processing and production, due to the repeated use of emulsions, the unsaturated fatty acids in the emulsions are oxidized and decomposed by oxygen in the air, and the organic compounds in the emulsifier and the decomposed fatty acids continue to rot and deteriorate under the action of bacteria; in addition, impurities such as dust and metal powder are mixed in, causing corruption and aging, reducing its lubrication and protection properties, thereby generating waste cold-rolled emulsions. Cold-rolled waste emulsified oil is a hazardous waste. If it is directly discharged without treatment, it will cause very serious ecological harm to the natural environment and even threaten human life and health.
[0003] At present, the commonly used methods for treating waste emulsified oil mainly include physical method, physicochemical method, chemical method and biochemical method; the treated waste emulsified oil has problems such as poor regeneration quality and low recovery rate, or the waste emulsified oil is regenerated into combustion oil.
[0004] CN103849453A discloses a method for purifying waste emulsified oil. During pretreatment, the waste emulsified oil is heated to 60-100°C, and then the heated waste emulsified oil is allowed to settle, and then a comprehensive reaction is performed. The comprehensive reaction is firstly high-voltage electrolysis, and then a catalyst 1 and a demulsifier are added; finally, a deep reaction is performed, and the deep reaction is firstly aerated and stirred, and then a catalyst 2 is added. The emulsified oil has a high degree of purification after treatment, but it adds a high-voltage electrolysis step, which is inconvenient to operate, and the added catalyst cannot be recycled after deactivation.
[0005] CN102399617A discloses a waste emulsified oil regeneration process, which first heats and precipitates the waste emulsified oil, then centrifuges it, adds a flocculant, removes the precipitate produced after flocculation, then adds bleaching clay for adsorption, and finally filters the waste emulsified oil with bleaching clay to obtain reusable emulsified oil. It proposes a purification and recovery process of coagulation refining combined with centrifugal separation and bleaching clay adsorption, but it adds centrifugal separation to separate the oil, water and residue in the waste emulsified oil, which increases energy consumption.
[0006] CN101805644A discloses a method for processing liquid fuel oil using waste oil, which comprises the following steps: firstly weighing a certain proportion of metal processing oil, waste emulsified oil and waste lubricating oil, adding cationic surfactant and concentrated sulfuric acid in sequence for demulsification, filtering to remove heavy metals and other impurities, and obtaining a mixed oil; then adding diatomaceous earth to the mixed oil for stirring, adsorption and decolorization, adding isopropanol, standing and stratifying, adding a lightning improver and an antioxidant to the separated oil layer, and obtaining liquid fuel oil. The method realizes full utilization of waste oil, but does not recycle and reuse heavy metals, and changes the purpose of emulsified oil, and fails to realize the recycling and regeneration of resources.
[0007] The existing waste emulsified oil regeneration devices and methods cannot solve the problem of emulsified oil regeneration and recycling or the problem of poor quality of regeneration and recycling. Therefore, how to ensure the recycling of cold-rolled iron-containing waste emulsified oil while ensuring the good quality of the regenerated emulsified oil recycling and recovering the iron has become an urgent problem to be solved. Summary of the invention
[0008] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a cold-rolled iron-containing waste emulsified oil regeneration system device and a regeneration method thereof, which dissolves impurities such as elemental iron and iron oxide wrapped in oil through hydrochloric acid leaching to achieve separation of iron and oil, and utilizes ferrous chloride solution to decompose and recycle hydrochloric acid, so that the regenerated emulsified oil can be recycled and the iron can be recovered.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In the first aspect, the present invention provides a cold-rolled iron-containing waste emulsified oil regeneration system device, which includes an acid leaching unit and a sedimentation unit connected in sequence along the material flow direction, and the outlet of the sedimentation unit is respectively connected to the emulsified oil regeneration unit and the hydrochloric acid preparation unit.
[0011] As a preferred technical solution of the present invention, the acid leaching unit includes an acid leaching device.
[0012] Preferably, the liquid inlet pipe of the acid leaching device is divided into two routes, namely a waste emulsified oil liquid inlet pipeline and a hydrochloric acid liquid inlet pipeline, and both the waste emulsified oil liquid inlet pipeline and the hydrochloric acid liquid inlet pipeline are provided with an electromagnetic flowmeter and a regulating valve.
[0013] Preferably, the regulating valve is electrically connected to an online pH meter, and the online pH meter is used to detect the pH of the solution in the acid leaching device and feedback control the regulating valve to adjust the waste emulsified oil inlet flow rate and the hydrochloric acid inlet flow rate.
[0014] Preferably, the material of the acid leaching device includes enamel, steel lined with rubber or steel lined with plastic.
[0015] The present invention provides an electromagnetic flowmeter and a regulating valve on both the waste emulsified oil inlet pipeline and the hydrochloric acid inlet pipeline, and measures the pH of a solution in an acid leaching device through an online pH meter, thereby adjusting the waste emulsified oil inlet flow rate and the hydrochloric acid inlet flow rate to ensure the pH of a mixed reaction in the acid leaching device.
[0016] As a preferred technical solution of the present invention, the sedimentation unit includes at least one sedimentation device, which is used for oil-water separation. The waste emulsified oil enters the sedimentation device and is stratified to obtain an oil layer and a water layer, wherein the oil layer enters the emulsified oil regeneration unit and the water layer enters the hydrochloric acid preparation unit.
[0017] Preferably, the sedimentation unit comprises at least two sedimentation devices connected in series.
[0018] Preferably, the shell material of the sedimentation device includes PP, PPH or fiberglass, for example, the shell material of the sedimentation device is PP, PPH or fiberglass.
[0019] Preferably, the sedimentation unit further comprises a solution collecting device connected to the sedimentation device, and the water layer solution obtained by stratification in the sedimentation device is collected and stored by the solution collecting device and then enters the hydrochloric acid preparation unit.
[0020] As a preferred technical solution of the present invention, the emulsified oil regeneration unit comprises a purification module and a regeneration module which are sequentially connected along the material flow direction. After the waste emulsified oil flows through the purification module and the regeneration module sequentially, regenerated emulsified oil is obtained.
[0021] Preferably, the purification module comprises at least one adsorption device.
[0022] Preferably, the purification module comprises an activated clay adsorption device and an activated carbon adsorption device which are connected in sequence.
[0023] The present invention does not make any specific requirements or special limitations on the type of the bleaching clay. For example, the type of the bleaching clay is bleaching clay used for lubricating oil purification in oil refining enterprises.
[0024] Preferably, the activated carbon filled in the activated carbon adsorption device includes at least one of coconut shell activated carbon, wood activated carbon or bamboo activated carbon, or a combination of two or more thereof.
[0025] Preferably, the regeneration module comprises an emulsified oil preparation device.
[0026] The present invention realizes oil-water separation through a sedimentation device, and obtains purified emulsified oil using an activated clay adsorption device and an activated carbon adsorption device. Finally, a regenerated emulsified oil product is obtained by adding additives in an emulsified oil preparation device. The obtained emulsified oil product has good lubrication performance and can effectively reduce the friction coefficient between roller gaps.
[0027] As a preferred technical solution of the present invention, the hydrochloric acid preparation unit includes a pyrolysis module and a hydrochloric acid preparation module connected in sequence, the inlet of the pyrolysis module is connected to the sedimentation unit, and the water layer solution of the sedimentation unit flows through the pyrolysis module and the hydrochloric acid preparation module in sequence.
[0028] Preferably, the hydrochloric acid preparation module is also connected to the hydrochloric acid inlet pipeline.
[0029] As a preferred technical solution of the present invention, the pyrolysis module includes a hydrolysis roasting device.
[0030] Preferably, a pre-concentrator is further provided on the connecting pipeline between the sedimentation device and the hydrolysis and roasting device, the gas outlet of the hydrolysis and roasting device is connected to the pre-concentrator, the water layer solution in the sedimentation device flows through the pre-concentrator and the hydrolysis and roasting device in sequence, and the high-temperature gas generated by the hydrolysis and roasting device returns to the pre-concentrator to preheat the water layer solution.
[0031] Preferably, the hydrochloric acid preparation module comprises a hydrochloric acid absorption device.
[0032] In the hydrolysis and roasting device of the present invention, clean fuel is used as a heat source, and the high-temperature gas generated by the hydrolysis and roasting device enters the cyclone separator and the pre-concentration device in sequence. In the pre-concentration device, the solution entering the hydrolysis and roasting device is preheated and concentrated, and dust recovery and comprehensive utilization of heat are achieved in this process.
[0033] As a preferred technical solution of the present invention, the cold-rolled iron-containing waste emulsified oil regeneration system device also includes a tail gas purification unit, and the tail gas purification unit is used to collect and treat the tail gas discharged from the acid leaching unit and the hydrochloric acid preparation unit.
[0034] Preferably, the tail gas purification unit comprises a tail gas purification device connected to the hydrochloric acid absorption device, and an acid mist absorption device connected to the acid leaching unit.
[0035] The acid mist absorption device absorbs and treats the tail gas discharged from the acid leaching unit, and part of the generated hydrochloric acid returns to the acid mist absorption device, and part returns to the acid leaching unit.
[0036] Preferably, the hydrochloric acid produced by the tail gas purification device is returned to the hydrochloric acid absorption device.
[0037] The invention provides a tail gas purification unit, recycles the tail gas containing HCl discharged from the acid leaching unit and the hydrochloric acid preparation unit, purifies the tail gas with water and then discharges it in compliance with the standards, and reuses the purified liquid after reaching a certain concentration, thereby not only reducing the emission of pollutants, but also effectively utilizing the tail gas and reducing the waste of resources.
[0038] In a second aspect, the present invention provides a method for regenerating cold-rolled iron-containing waste emulsified oil using the regeneration system device described in the first aspect, the regeneration method comprising:
[0039] The cold-rolled iron-containing waste emulsified oil is mixed with hydrochloric acid for acid leaching and then settled and separated into oil layer and water layer. The oil layer solution enters the emulsified oil regeneration unit, and after adsorption purification, the emulsified oil additive is added to regenerate the emulsified oil; the water layer solution enters the hydrochloric acid preparation unit to prepare the hydrochloric acid solution.
[0040] The invention utilizes hydrochloric acid leaching to demulsify the waste emulsified oil, thereby realizing separation of iron from oil, and realizes recycling of hydrochloric acid by decomposing a ferrous chloride solution, thereby obtaining an iron oxide product, and recovering iron in the waste emulsified oil without causing harm to the environment.
[0041] As a preferred technical solution of the present invention, the regeneration method specifically comprises:
[0042] (I) cold-rolled iron-containing waste emulsified oil and hydrochloric acid are respectively introduced into an acid leaching device for acid leaching reaction after being measured by an electromagnetic flowmeter. During the reaction, the pH of the solution in the acid leaching device is detected by an online pH meter and a feedback control regulating valve is used to adjust the inlet flow rate of the waste emulsified oil and the inlet flow rate of the hydrochloric acid;
[0043] (II) the solution after the reaction is passed into a sedimentation device for sedimentation treatment, and waste emulsified oil and ferrous chloride solution are obtained by stratification;
[0044] (III) the waste emulsified oil obtained in step (II) enters a purification module for adsorption purification, and then enters a regeneration module, an emulsified oil additive is added to the regeneration module, and emulsified oil is regenerated;
[0045] (IV) The ferrous chloride solution obtained in step (II) is sequentially introduced into a pre-concentrator and a hydrolysis and calcination device for pre-concentration and spray pyrolysis, respectively. After spray pyrolysis, high-temperature HCl gas and iron oxide products are generated. The high-temperature HCl gas returns to the pre-concentrator to preheat and concentrate the ferrous chloride solution entering the hydrolysis and calcination device. The preheated HCl gas enters a hydrochloric acid absorption device to prepare hydrochloric acid.
[0046] As a preferred technical solution of the present invention, in steps (I) and (IV), the concentration of the hydrochloric acid is 18-21wt%, for example, the concentration of the hydrochloric acid is 18wt%, 18.5wt%, 19wt%, 19.5wt%, 20wt%, 20.5wt% or 21wt%.
[0047] Preferably, in step (I), the temperature at the end point of the acid leaching reaction is 75-85°C, for example, the temperature at the end point of the acid leaching reaction is 75°C, 77°C, 79°C, 81°C, 83°C or 85°C.
[0048] Preferably, in step (I), the pH value of the acid leaching reaction after adding hydrochloric acid is 2-4, for example, the pH value of the acid leaching reaction after adding hydrochloric acid is 2, 2.2, 2.4, 2.6, 2.8, 3.0, 3.2, 3.4, 3.6, 3.8 or 4.
[0049] Preferably, in step (I), iron powder is added during the acid leaching reaction.
[0050] Preferably, in step (I), the pH at the end point of the acid leaching reaction when the iron powder is added is 5.5-6; for example, the pH at the end point of the acid leaching reaction when the iron powder is added is 5.5, 5.6, 5.7, 5.8, 5.9 or 6.
[0051] Preferably, in step (II), the sedimentation treatment is a two-stage sedimentation.
[0052] Preferably, in step (III), the adsorption purification operation is to sequentially enter an activated clay adsorption device and an activated carbon adsorption device to perform activated clay adsorption and activated carbon adsorption, respectively.
[0053] Preferably, in step (III), the emulsified oil additives include an emulsifier, a rust remover, an extreme pressure agent, a bactericide and a defoaming agent.
[0054] The present invention does not impose any specific requirements or special limitations on the type of emulsifier. For example, the emulsifier may be commercially available emulsifiers such as emulsifier fatty alcohol, polyethylene glycol, and vegetable oil emulsifier.
[0055] The present invention does not impose any specific requirements or special limitations on the type of the rust remover. For example, the type of the rust remover is an inorganic rust inhibitor or a composite rust inhibitor.
[0056] Preferably, in step (IV), the temperature of the spray pyrolysis in the hydrolysis and calcination device is 550-700°C, for example, the temperature of the spray pyrolysis in the hydrolysis and calcination device is 550°C, 570°C, 590°C, 610°C, 630°C, 650°C, 670°C, 680°C, 690°C, or 700°C.
[0057] Preferably, in step (IV), the method of preheating and concentrating the ferrous chloride solution with the high-temperature HCl gas in the preconcentrator is direct contact preheating and concentration.
[0058] Preferably, in step (IV), the temperature of the high-temperature HCl produced after spray pyrolysis is 350-450°C, for example, the temperature of the high-temperature HCl produced after spray pyrolysis is 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, 410°C, 420°C, 430°C, 440°C or 450°C.
[0059] Preferably, in step (IV), the temperature of the preheated HCl is reduced to 85-95°C, for example, the temperature of the preheated HCl is reduced to 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C or 95°C.
[0060] Preferably, the hydrochloric acid prepared in step (IV) is returned to step (I) to undergo an acid leaching reaction with the cold-rolled iron-containing waste emulsified oil.
[0061] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0062] Compared with the prior art, the present invention has the following beneficial effects:
[0063] The invention realizes separation of iron and oil by hydrochloric acid leaching, realizes oil-water separation by sedimentation, obtains purified emulsified oil by adsorption of activated clay and activated carbon, obtains regenerated emulsified oil product by adding additives, and the saponification value of the emulsified oil product is as high as 168 mgKOH / g, which indicates good lubrication performance and can effectively reduce the friction coefficient between roller gaps. The invention also realizes hydrochloric acid circulation by spray pyrolysis of ferrous chloride solution, obtains iron oxide product, recovers iron in waste emulsified oil, and the yield of iron is as high as 99.5%, which has good environmental and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] Figure 1 This is a schematic diagram of the structure of a cold-rolled iron-containing waste emulsified oil regeneration system in a specific embodiment of the present invention;
[0065] Figure 2 This is a flow chart of a method for regenerating cold-rolled iron-containing waste emulsified oil in a specific embodiment of the present invention;
[0066] Among them, 1-acid leaching device; 2-acid mist absorption device; 3-primary sedimentation device; 4-secondary sedimentation device; 5-solution collection device; 6-activated clay adsorption device; 7-activated carbon adsorption device; 8-emulsified oil preparation device; 9-hydrolysis roasting device; 10-pre-concentration device; 11-hydrochloric acid absorption device; 12-exhaust gas purification device; 13-online pH meter. DETAILED DESCRIPTION
[0067] It should be understood that, in the description of the present invention, the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0068] It should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "disposed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0069] It should be understood by those skilled in the art that a cold-rolled iron-containing waste emulsified oil regeneration system device provided by the present invention must include necessary pipelines, conventional valves and general pump equipment for realizing a complete process, but the above content does not belong to the main invention point of the present invention. Those skilled in the art can add layouts on their own based on the process flow and equipment structure selection, and the present invention does not make special requirements and specific limitations on this.
[0070] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0071] In a specific embodiment, the present invention provides a cold-rolled iron-containing waste emulsified oil regeneration system device, which includes an acid leaching unit and a sedimentation unit connected in sequence along the material flow direction, and the outlet of the sedimentation unit is respectively connected to the emulsified oil regeneration unit and the hydrochloric acid preparation unit.
[0072] The acid leaching unit includes an acid leaching device 1 made of enamel, steel lined with rubber or steel lined with plastic; the liquid inlet pipe of the acid leaching device 1 is divided into two routes, namely a waste emulsified oil liquid inlet pipeline and a hydrochloric acid liquid inlet pipeline, and electromagnetic flow meters and regulating valves are provided on the waste emulsified oil liquid inlet pipeline and the hydrochloric acid liquid inlet pipeline, and the regulating valve is electrically connected to an online pH meter 13.
[0073] The sedimentation unit includes at least two sedimentation devices for oil-water separation connected in series, and a solution collecting device 5 connected to the sedimentation device, and the shell material of the sedimentation device includes PP, PPH or fiberglass; after the waste emulsified oil is soaked in acid, it enters the sedimentation device for stratification to obtain an oil layer and a water layer, wherein the oil layer enters the emulsified oil regeneration unit, and the water layer is collected and stored by the solution collecting device 5 and then enters the hydrochloric acid preparation unit.
[0074] The emulsified oil regeneration unit comprises an activated clay adsorption device 6, an activated carbon adsorption device 7 and an emulsified oil preparation device 8 which are sequentially connected along the flow direction of the oil layer solution; the activated carbon filled in the activated carbon adsorption device 7 comprises at least one of coconut shell activated carbon, wood activated carbon or bamboo activated carbon or a combination of two or more thereof;
[0075] The hydrochloric acid preparation unit includes a pre-concentrator 10, a hydrolysis and calcination device 9 and a hydrochloric acid absorption device 11 which are connected in sequence. The water layer solution of the sedimentation unit flows through the pre-concentrator 10 and the hydrolysis and calcination device 9 in sequence. The gas outlet of the hydrolysis and calcination device 9 is connected to the pre-concentrator 10. The water layer solution in the sedimentation device flows through the pre-concentrator 10 and the hydrolysis and calcination device 9 in sequence. The high-temperature gas generated by the hydrolysis and calcination device 9 returns to the pre-concentrator 10 to preheat the water layer solution. The preheated gas enters the hydrochloric acid absorption device 11, and the hydrochloric acid absorption device 11 is connected to the hydrochloric acid inlet pipeline.
[0076] The tail gas purification unit includes a tail gas purification device 12 connected to the hydrochloric acid absorption device 11, and an acid mist absorption device 2 connected to the acid leaching unit; the hydrochloric acid produced by the tail gas purification device 12 is divided into two paths, one path returns to the tail gas purification device 12, and the other path returns to the hydrochloric acid absorption device 11; the hydrochloric acid produced by the acid mist absorption device 2 is divided into two paths, one path returns to the acid mist absorption device 2, and the other path is connected to the hydrochloric acid inlet pipeline of the acid leaching unit.
[0077] In another specific embodiment, the present invention provides a method for regenerating cold-rolled iron-containing waste emulsified oil using the above-mentioned regeneration system device, wherein the treated cold-rolled iron-containing waste emulsified oil comes from a domestic company, and its main components are shown in the following table:
[0078] Element Oil water Iron-containing solid impurities Acid insoluble matter Composition / (wt%) 50~70 10~30 5~20 0.1~2
[0079] The regeneration method specifically comprises:
[0080] (I) cold rolled iron-containing waste emulsified oil and hydrochloric acid with a concentration of 18-21wt% are respectively introduced into the acid leaching device 1 for acid leaching reaction after being measured by an electromagnetic flowmeter. During the reaction, the pH of the solution in the acid leaching device 1 is detected by an online pH meter 13 and the regulating valve is feedback-controlled to adjust the inlet flow rate of the waste emulsified oil and the inlet flow rate of the hydrochloric acid. During the acid leaching reaction, the pH at the end point of adding hydrochloric acid is 2-4. During the acid leaching reaction, iron powder is added. The pH at the end point of the acid leaching reaction of the cold rolled iron-containing waste emulsified oil and hydrochloric acid is 5.5-6. The temperature at the end point of the acid leaching reaction is 75-85°C;
[0081] (II) the solution after the reaction is passed into a primary sedimentation device 3 and a secondary sedimentation device 4 for two-stage sedimentation, and waste emulsified oil and ferrous chloride solution are obtained by stratification;
[0082] (III) the waste emulsified oil obtained in step (II) is sequentially introduced into an activated clay adsorption device 6 and an activated carbon adsorption device 7 for activated clay adsorption and activated carbon adsorption, respectively, and then introduced into an emulsified oil preparation device 8, into which an emulsifier, an extreme pressure agent, a rust remover, a bactericide and a defoaming agent are sequentially added to regenerate the emulsified oil;
[0083] (IV) The ferrous chloride solution obtained in step (II) is sequentially introduced into a pre-concentrator 10 and a hydrolysis and calcination device 9 for pre-concentration and spray pyrolysis, respectively. The temperature of the spray pyrolysis reaction is 550-700° C. After the spray pyrolysis, HCl gas and iron oxide products at 350-450° C. are generated. The HCl gas at 350-450° C. is returned to the pre-concentrator 10 to directly contact the ferrous chloride solution entering the hydrolysis and calcination device 9 for preheating and concentration. The temperature of the preheated HCl gas is reduced to 85-95° C. The HCl gas is cooled and then enters the hydrochloric acid absorption device 11 to prepare hydrochloric acid with a concentration of 18-21 wt %. The hydrochloric acid is returned to step (I) to react with the cold-rolled iron-containing waste emulsified oil acid leaching.
[0084] The tail gas discharged from the hydrochloric acid absorption device 11 enters the tail gas purification device 12, and is discharged after being purified to meet the standards. The generated hydrochloric acid reaches a certain concentration and is transported to the hydrochloric acid absorption device 11 for HCl absorption; the tail gas discharged from the acid leaching device 1 enters the acid mist absorption device 2, and is discharged after being purified to meet the standards. The generated hydrochloric acid reaches a certain concentration and is transported to the acid leaching device 1 through the hydrochloric acid inlet pipeline.
[0085] Example 1
[0086] This embodiment provides a cold rolling iron-containing waste emulsified oil regeneration system device, such as Figure 1 As shown, a cold-rolled iron-containing waste emulsified oil regeneration system device is provided in a specific embodiment, wherein the interior of the acid leaching device 1 is made of enamel material; the sedimentation unit includes a primary sedimentation device 3 and a secondary sedimentation device 4 connected in series, and the material of the primary sedimentation device 3 and the material of the secondary sedimentation device 4 are both PP; the activated carbon filled in the activated carbon adsorption device 7 is wood activated carbon.
[0087] This embodiment also provides a method for regenerating cold rolling iron-containing waste emulsified oil using the above-mentioned regeneration system device, such as Figure 2 The specific steps are as follows:
[0088] (I) 1000 kg of cold-rolled iron-containing waste emulsified oil is metered by an electromagnetic flowmeter and introduced into an acid leaching device 1, wherein the cold-rolled iron-containing waste emulsified oil contains 690 kg of oil, 180 kg of iron, and the rest is impurities including water, etc., and then 19.5 wt% hydrochloric acid is metered by an electromagnetic flowmeter and introduced into the acid leaching device 1 for acid leaching reaction. During the reaction, the pH of the solution in the acid leaching device 1 is detected by an online pH meter 13 and the regulating valve is feedback-controlled to adjust the liquid inlet flow rate of the waste emulsified oil and the liquid inlet flow rate of the hydrochloric acid. During the acid leaching reaction, the pH at the end point of adding hydrochloric acid is 3.0. A total of 1220 kg of 19.5 wt% hydrochloric acid is added, and then 0.038 kg of iron powder is added, so that the pH at the end point of the acid leaching reaction between the cold-rolled iron-containing waste emulsified oil and the hydrochloric acid is 5.9, and the end point temperature of the acid leaching reaction is 84°C;
[0089] (II) The reacted solution is sequentially passed into a first settling device and a second settling device for two-stage settling, and the waste emulsified oil and the ferrous chloride solution are obtained by stratification, wherein the oil layer solution of the first settling device 3 is transported to the second settling device 4 for secondary settling separation, and the ferrous chloride solution is transported to the solution collecting device 5, and the total ferrous chloride solution is 1480 kg, and the ferrous chloride concentration is 27.4 wt%;
[0090] (III) the waste emulsified oil obtained in step (II) is sequentially fed into an activated clay adsorption device 6 and an activated carbon adsorption device 7 for activated clay adsorption and activated carbon adsorption, respectively, and then fed into an emulsified oil preparation device 8, into which an emulsifier, an extreme pressure agent, a rust remover, a bactericide and a defoaming agent are sequentially added to regenerate the emulsified oil;
[0091] (IV) The ferrous chloride solution obtained in step (II) is sequentially introduced into a pre-concentrator 10 and a hydrolysis and calcination device 9 for pre-concentration and spray pyrolysis, respectively. The spray pyrolysis reaction temperature is 630°C. After the spray pyrolysis, HCl gas at 400°C and iron oxide products are generated. The HCl gas at 400°C is returned to the pre-concentrator 10 to directly contact the ferrous chloride solution entering the hydrolysis and calcination device 9 for preheating and concentration. The temperature of the preheated HCl gas is reduced to 95°C. After cooling, the HCl gas enters the hydrochloric acid absorption device 11 to prepare 1085 kg of hydrochloric acid with a concentration of 21 wt%. The hydrochloric acid is returned to step (I) to react with the cold-rolled iron-containing waste emulsified oil acid leaching.
[0092] The tail gas discharged from the hydrochloric acid absorption device 11 enters the tail gas purification device 12, and is discharged after being purified to meet the standards. The generated hydrochloric acid reaches a certain concentration and is transported to the hydrochloric acid absorption device 11 for HCl absorption; the tail gas discharged from the acid leaching device 1 enters the acid mist absorption device 2, and is discharged after being purified to meet the standards. The generated hydrochloric acid reaches a certain concentration and is transported to the acid leaching device 1 through the hydrochloric acid inlet pipeline.
[0093] By regenerating the cold-rolled iron-containing waste emulsion, 635 kg of emulsified oil was obtained, with an oil yield of 92%. A total of 135 kg of additives were added, and 770 kg of emulsified oil for cold rolling was prepared. 258 kg of iron oxide product was also obtained, of which the content of ferric oxide was 98.9%, and the iron yield reached 99.2%.
[0094] The important indicator of the prepared finished cold rolling emulsified oil is the saponification value of 165 mgKOH / g. The high saponification value indicates good lubrication performance and can effectively reduce the friction coefficient between the roll gaps. For other data, see Table 1.
[0095] Example 2
[0096] This embodiment provides a cold rolling iron-containing waste emulsified oil regeneration system device, such as Figure 1 As shown, a cold-rolled iron-containing waste emulsified oil regeneration system device is provided in a specific embodiment, wherein the interior of the acid leaching device 1 is made of steel-lined rubber material; the sedimentation unit includes a primary sedimentation device 3 and a secondary sedimentation device 4 connected in series, and the material of the primary sedimentation device 3 and the material of the secondary sedimentation device 4 are both glass fiber reinforced plastics; the activated carbon filled in the activated carbon adsorption device 7 is bamboo activated carbon.
[0097] This embodiment also provides a method for regenerating cold rolling iron-containing waste emulsified oil using the above-mentioned regeneration system device, such as Figure 2 The specific steps are as follows:
[0098] (I) 1000 kg of cold-rolled iron-containing waste emulsified oil is metered by an electromagnetic flowmeter and introduced into an acid leaching device 1, wherein the cold-rolled iron-containing waste emulsified oil contains 620 kg of oil, 144 kg of iron, and the rest is impurities including water, etc., and then 21 wt% hydrochloric acid is metered by an electromagnetic flowmeter and introduced into the acid leaching device 1 for acid leaching reaction. During the reaction, the pH of the solution in the acid leaching device 1 is detected by an online pH meter 13 and the regulating valve is feedback-controlled to adjust the liquid inlet flow rate of the waste emulsified oil and the liquid inlet flow rate of the hydrochloric acid. During the acid leaching reaction, the pH at the end point of adding hydrochloric acid is 2.0. A total of 895 kg of 21 wt% hydrochloric acid is added, and then 0.31 kg of iron powder is added, so that the pH at the end point of the acid leaching reaction between the cold-rolled iron-containing waste emulsified oil and the hydrochloric acid is 6.0, and the end point temperature of the acid leaching reaction is 79° C.;
[0099] (II) The reacted solution is sequentially introduced into a first settling device and a second settling device for two-stage settling, and the waste emulsified oil and the ferrous chloride solution are obtained by stratification, wherein the oil layer solution of the first settling device 3 is transported to the second settling device 4 for secondary settling separation, and the ferrous chloride solution is transported to the solution collecting device 5, and the total amount of the ferrous chloride solution is 1213 kg, and the concentration of ferrous chloride is 26.9 wt%;
[0100] (III) the waste emulsified oil obtained in step (II) is sequentially fed into an activated clay adsorption device 6 and an activated carbon adsorption device 7 for activated clay adsorption and activated carbon adsorption, respectively, and then fed into an emulsified oil preparation device 8, into which an emulsifier, an extreme pressure agent, a rust remover, a bactericide and a defoaming agent are sequentially added to regenerate the emulsified oil;
[0101] (IV) The ferrous chloride solution obtained in step (II) is sequentially introduced into a pre-concentrator 10 and a hydrolysis and calcination device 9 for pre-concentration and spray pyrolysis respectively. The spray pyrolysis reaction temperature is 650°C. After the spray pyrolysis, HCl gas at 410°C and iron oxide products are generated. The HCl gas at 410°C is returned to the pre-concentrator 10 to directly contact the ferrous chloride solution entering the hydrolysis and calcination device 9 for preheating and concentration. The temperature of the preheated HCl gas is reduced to 93°C. After cooling, the HCl gas enters the hydrochloric acid absorption device 11 to prepare 820 kg of hydrochloric acid with a concentration of 20.4 wt%. The hydrochloric acid is returned to step (I) to react with the cold-rolled iron-containing waste emulsified oil acid leaching.
[0102] The tail gas discharged from the hydrochloric acid absorption device 11 enters the tail gas purification device 12, and is discharged after being purified to meet the standards. The generated hydrochloric acid reaches a certain concentration and is transported to the hydrochloric acid absorption device 11 for HCl absorption; the tail gas discharged from the acid leaching device 1 enters the acid mist absorption device 2, and is discharged after being purified to meet the standards. The generated hydrochloric acid reaches a certain concentration and is transported to the acid leaching device 1 through the hydrochloric acid inlet pipeline.
[0103] By regenerating the cold-rolled iron-containing waste emulsion, 597 kg of emulsified oil was obtained, with an oil yield of 96.3%. A total of 115 kg of additives were added, and 712 kg of emulsified oil for cold rolling was prepared; 205 kg of iron oxide product was also obtained, of which the content of ferric oxide was 99.5%, and the iron yield reached 99.4%.
[0104] The important indicator of the prepared finished cold rolling emulsified oil is the saponification value of 155 mgKOH / g. The high saponification value indicates good lubrication performance and can effectively reduce the friction coefficient between the roll gaps. For other data, see Table 1.
[0105] Example 3
[0106] This embodiment provides a cold rolling iron-containing waste emulsified oil regeneration system device, such as Figure 1 As shown, a cold-rolled iron-containing waste emulsified oil regeneration system device is provided in a specific embodiment, wherein the interior of the acid leaching device 1 is made of enamel material; the sedimentation unit includes a primary sedimentation device 3 and a secondary sedimentation device 4 connected in series, and the material of the primary sedimentation device 3 and the material of the secondary sedimentation device 4 are both PPH; the activated carbon filled in the activated carbon adsorption device 7 is wooden activated carbon.
[0107] This embodiment also provides a method for regenerating cold rolling iron-containing waste emulsified oil using the above-mentioned regeneration system device, such as Figure 2 The specific steps are as follows:
[0108] (I) 1000 kg of cold-rolled iron-containing waste emulsified oil is metered by an electromagnetic flowmeter and introduced into an acid leaching device 1, wherein the cold-rolled iron-containing waste emulsified oil contains 550 kg of oil, 125 kg of iron, and the rest are impurities. Then, hydrochloric acid with a concentration of 18 wt% is metered by an electromagnetic flowmeter and introduced into the acid leaching device 1 for acid leaching reaction. During the reaction, the pH of the solution in the acid leaching device 1 is detected by an online pH meter 13, and the regulating valve is feedback-controlled to adjust the liquid inlet flow rate of the waste emulsified oil and the liquid inlet flow rate of the hydrochloric acid. During the acid leaching reaction, the pH at the end point of adding hydrochloric acid is 2.0. A total of 906 kg of 18 wt% hydrochloric acid is added, and then 0.004 kg of iron powder is added, so that the pH at the end point of the acid leaching reaction between the cold-rolled iron-containing waste emulsified oil and the hydrochloric acid is 5.5, and the end point temperature of the acid leaching reaction is 75°C;
[0109] (II) The reacted solution is sequentially introduced into a first settling device and a second settling device for two-stage settling, and the waste emulsified oil and the ferrous chloride solution are obtained by stratification, wherein the oil layer solution of the first settling device 3 is transported to the second settling device 4 for secondary settling separation, and the ferrous chloride solution is transported to the solution collecting device 5, the total amount of the ferrous chloride solution is 1350 kg, and the concentration of ferrous chloride is 20.9 wt%;
[0110] (III) the waste emulsified oil obtained in step (II) is sequentially fed into an activated clay adsorption device 6 and an activated carbon adsorption device 7 for activated clay adsorption and activated carbon adsorption, respectively, and then fed into an emulsified oil preparation device 8, into which an emulsifier, an extreme pressure agent, a rust remover, a bactericide and a defoaming agent are sequentially added to regenerate the emulsified oil;
[0111] (IV) The ferrous chloride solution obtained in step (II) is sequentially introduced into a pre-concentrator 10 and a hydrolysis and calcination device 9 for pre-concentration and spray pyrolysis, respectively. The temperature of the spray pyrolysis reaction is 700°C. After the spray pyrolysis, HCl gas at 420°C and iron oxide products are generated. The HCl gas at 420°C is returned to the pre-concentrator 10 to directly contact the ferrous chloride solution entering the hydrolysis and calcination device 9 for preheating and concentration. The temperature of the preheated HCl gas is reduced to 87°C. After cooling, the HCl gas enters the hydrochloric acid absorption device 11 to prepare 795 kg of hydrochloric acid with a concentration of 19 wt%. The hydrochloric acid is returned to step (I) to react with the cold-rolled iron-containing waste emulsified oil acid leaching.
[0112] The tail gas discharged from the hydrochloric acid absorption device 11 enters the tail gas purification device 12, and is discharged after being purified to meet the standards. The generated hydrochloric acid reaches a certain concentration and is transported to the hydrochloric acid absorption device 11 for HCl absorption; the tail gas discharged from the acid leaching device 1 enters the acid mist absorption device 2, and is discharged after being purified to meet the standards. The generated hydrochloric acid reaches a certain concentration and is transported to the acid leaching device 1 through the hydrochloric acid inlet pipeline.
[0113] By regenerating the cold-rolled iron-containing waste emulsion, 535 kg of emulsified oil was obtained, with an oil yield of 97.3%. A total of 96 kg of additives were added to prepare 631 kg of emulsified oil for cold rolling. 179 kg of iron oxide product was also obtained, of which the content of ferric oxide was 98.2%, and the iron yield reached 98.4%.
[0114] The important indicator of the prepared finished cold rolling emulsified oil is the saponification value of 161 mgKOH / g. The high saponification value indicates good lubrication performance and can effectively reduce the friction coefficient between the roll gaps. For other data, see Table 1.
[0115] Example 4
[0116] The present embodiment provides a cold-rolled iron-containing waste emulsified oil regeneration system device, based on a cold-rolled iron-containing waste emulsified oil regeneration system device provided in a specific implementation manner, wherein the interior of the acid leaching device 1 is made of steel-lined plastic material; the sedimentation unit includes a first-stage sedimentation device 3, a second-stage sedimentation device 4 and a third-stage sedimentation device connected in series, and the material of the first-stage sedimentation device 3, the material of the second-stage sedimentation device 4 and the third-stage sedimentation device are all PPH; the activated carbon filled in the activated carbon adsorption device 7 is coconut shell activated carbon.
[0117] This embodiment also provides a method for regenerating cold rolling iron-containing waste emulsified oil using the above-mentioned regeneration system device, and the specific operation steps are as follows:
[0118] (I) 1000 kg of cold-rolled iron-containing waste emulsified oil is metered by an electromagnetic flowmeter and introduced into an acid leaching device 1, wherein the cold-rolled iron-containing waste emulsified oil contains 500 kg of oil, 200 kg of iron, and the rest is impurities including water, etc., and then 19 wt% hydrochloric acid is metered by an electromagnetic flowmeter and introduced into the acid leaching device 1 for acid leaching reaction. During the reaction, the pH of the solution in the acid leaching device 1 is detected by an online pH meter 13 and the regulating valve is feedback-controlled to adjust the liquid inlet flow rate of the waste emulsified oil and the liquid inlet flow rate of the hydrochloric acid. During the acid leaching reaction, the pH at the end point of adding hydrochloric acid is 4.0. A total of 1380 kg of 19 wt% hydrochloric acid is added, and then 0.01 kg of iron powder is added, so that the pH at the end point of the acid leaching reaction between the cold-rolled iron-containing waste emulsified oil and the hydrochloric acid is 5.7, and the end point temperature of the acid leaching reaction is 82°C;
[0119] (II) The reacted solution is sequentially passed into the first settling device and the second settling device for three-stage settling, and the waste emulsified oil and the ferrous chloride solution are obtained by stratification, wherein the oil layer solution of the first settling device 3 is transported to the second settling device 4 for secondary settling separation, and the oil layer solution of the second settling device 4 is transported to the third settling device for three-stage settling separation, and the ferrous chloride solution is transported to the solution collecting device 5, the total amount of the ferrous chloride solution is 1800 kg, and the concentration of ferrous chloride is 25.2 wt%;
[0120] (III) the waste emulsified oil obtained in step (II) is sequentially fed into an activated clay adsorption device 6 and an activated carbon adsorption device 7 for activated clay adsorption and activated carbon adsorption, respectively, and then fed into an emulsified oil preparation device 8, into which an emulsifier, an extreme pressure agent, a rust remover, a bactericide and a defoaming agent are sequentially added to regenerate the emulsified oil;
[0121] (IV) The ferrous chloride solution obtained in step (II) is sequentially introduced into a pre-concentrator 10 and a hydrolysis and calcination device 9 for pre-concentration and spray pyrolysis, respectively. The spray pyrolysis reaction temperature is 700°C. After the spray pyrolysis, HCl gas at 450°C and iron oxide products are generated. The HCl gas at 450°C is returned to the pre-concentrator 10 to directly contact the ferrous chloride solution entering the hydrolysis and calcination device 9 for preheating and concentration. The temperature of the preheated HCl gas is reduced to 90°C. After cooling, the HCl gas enters the hydrochloric acid absorption device 11 to prepare 1300 kg of hydrochloric acid with a concentration of 20 wt%. The hydrochloric acid is returned to step (I) to react with the cold-rolled iron-containing waste emulsified oil acid leaching.
[0122] The tail gas discharged from the hydrochloric acid absorption device 11 enters the tail gas purification device 12, and is discharged after being purified to meet the standards. The generated hydrochloric acid reaches a certain concentration and is transported to the hydrochloric acid absorption device 11 for HCl absorption; the tail gas discharged from the acid leaching device 1 enters the acid mist absorption device 2, and is discharged after being purified to meet the standards. The generated hydrochloric acid reaches a certain concentration and is transported to the acid leaching device 1 through the hydrochloric acid inlet pipeline.
[0123] By regenerating the cold-rolled iron-containing waste emulsion, 490 kg of emulsified oil was obtained, with an oil yield of 98.0%. A total of 120 kg of additives were added to prepare 610 kg of emulsified oil for cold rolling. 285 kg of iron oxide product was also obtained, of which the content of ferric oxide was 99.0%, and the iron yield reached 98.7%.
[0124] The important indicator of the prepared finished cold rolling emulsified oil is the saponification value of 168 mgKOH / g. The high saponification value indicates good lubrication performance and can effectively reduce the friction coefficient between the roll gaps. For other data, see Table 1.
[0125] Example 5
[0126] The present embodiment provides a cold-rolled iron-containing waste emulsified oil regeneration system device, based on a cold-rolled iron-containing waste emulsified oil regeneration system device provided in a specific implementation manner, wherein the interior of the acid leaching device 1 is made of steel-lined rubber material; the sedimentation unit includes a first-level sedimentation device 3, a second-level sedimentation device 4, a third-level sedimentation device and a fourth-level sedimentation device connected in series, and the material of the first-level sedimentation device 3, the material of the second-level sedimentation device 4, the third-level sedimentation device and the fourth-level sedimentation device are all PPH; the activated carbon filled in the activated carbon adsorption device 7 is a combination of coconut shell activated carbon and wood activated carbon.
[0127] This embodiment also provides a method for regenerating cold rolling iron-containing waste emulsified oil using the above-mentioned regeneration system device, and the specific operation steps are as follows:
[0128] (I) 1000 kg of cold-rolled iron-containing waste emulsified oil is metered by an electromagnetic flowmeter and introduced into an acid leaching device 1, wherein the cold-rolled iron-containing waste emulsified oil contains 700 kg of oil, 50 kg of iron, and the rest is water and other impurities. Then, hydrochloric acid with a concentration of 20 wt% is metered by an electromagnetic flowmeter and introduced into the acid leaching device 1 for acid leaching reaction. During the reaction, the pH of the solution in the acid leaching device 1 is detected by an online pH meter 13, and the regulating valve is feedback-controlled to adjust the liquid inlet flow rate of the waste emulsified oil and the liquid inlet flow rate of the hydrochloric acid. During the acid leaching reaction, the pH at the end point of adding hydrochloric acid is 2.0. A total of 330 kg of 20 wt% hydrochloric acid is added, and then 0.09 kg of iron powder is added, so that the pH at the end point of the acid leaching reaction between the cold-rolled iron-containing waste emulsified oil and the hydrochloric acid is 6.0, and the end point temperature of the acid leaching reaction is 85°C;
[0129] (II) The reacted solution is sequentially passed into the first settling device and the second settling device for three-stage settling, and the waste emulsified oil and the ferrous chloride solution are obtained by stratification, wherein the oil layer solution of the first settling device 3 is transported to the second settling device 4 for secondary settling separation, the oil layer solution of the second settling device 4 is transported to the third settling device for tertiary settling separation, the oil layer solution of the third settling device is transported to the fourth settling device for four-stage settling separation, and the ferrous chloride solution is transported to the solution collecting device 5, the total amount of ferrous chloride solution is 438 kg, and the concentration of ferrous chloride is 25.9 wt%;
[0130] (III) the waste emulsified oil obtained in step (II) is sequentially fed into an activated clay adsorption device 6 and an activated carbon adsorption device 7 for activated clay adsorption and activated carbon adsorption, respectively, and then fed into an emulsified oil preparation device 8, into which an emulsifier, an extreme pressure agent, a rust remover, a bactericide and a defoaming agent are sequentially added to regenerate the emulsified oil;
[0131] (IV) The ferrous chloride solution obtained in step (II) is sequentially introduced into a pre-concentrator 10 and a hydrolysis and calcination device 9 for pre-concentration and spray pyrolysis respectively. The spray pyrolysis reaction temperature is 550°C. After the spray pyrolysis, HCl gas at 350°C and iron oxide products are generated. The HCl gas at 350°C is returned to the pre-concentrator 10 to directly contact the ferrous chloride solution entering the hydrolysis and calcination device 9 for preheating and concentration. The temperature of the preheated HCl gas is reduced to 85°C. After cooling, the HCl gas enters the hydrochloric acid absorption device 11 to prepare 366 kg of hydrochloric acid with a concentration of 18 wt%. The hydrochloric acid is returned to step (I) to react with the cold-rolled iron-containing waste emulsified oil acid leaching.
[0132] The tail gas discharged from the hydrochloric acid absorption device 11 enters the tail gas purification device 12, and is discharged after being purified to meet the standards. The generated hydrochloric acid reaches a certain concentration and is transported to the hydrochloric acid absorption device 11 for HCl absorption; the tail gas discharged from the acid leaching device 1 enters the acid mist absorption device 2, and is discharged after being purified to meet the standards. The generated hydrochloric acid reaches a certain concentration and is transported to the acid leaching device 1 through the hydrochloric acid inlet pipeline.
[0133] By regenerating the cold-rolled iron-containing waste emulsion, 689 kg of emulsified oil was obtained, with an oil yield of 98.4%. A total of 80 kg of additives were added to prepare 769 kg of emulsified oil for cold rolling. 71 kg of iron oxide product was also obtained, of which the content of ferric oxide was 99%, and the iron yield reached 98.0%.
[0134] The important indicator of the prepared finished cold rolling emulsified oil is the saponification value of 165 mgKOH / g. The high saponification value indicates good lubrication performance and can effectively reduce the friction coefficient between the roll gaps. For other data, see Table 1.
[0135] Table 1
[0136]
[0137] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for regenerating cold-rolled iron-containing waste emulsified oil, characterized in that: A cold-rolled iron-containing waste emulsified oil regeneration system device is used to regenerate the cold-rolled iron-containing waste emulsified oil. The cold-rolled iron-containing waste emulsified oil regeneration system device includes an acid leaching unit and a sedimentation unit connected in sequence along the material flow direction, and the outlet of the sedimentation unit is respectively connected to the emulsified oil regeneration unit and the hydrochloric acid preparation unit; the hydrochloric acid preparation unit includes a pyrolysis module and a hydrochloric acid preparation module connected in sequence, the inlet of the pyrolysis module is connected to the sedimentation unit, and the water layer solution of the sedimentation unit flows through the pyrolysis module and the hydrochloric acid preparation module in sequence; the pyrolysis module includes a hydrolysis and roasting device, and a pre-concentration device is further provided on the connecting pipeline between the sedimentation unit and the hydrolysis and roasting device, the gas outlet of the hydrolysis and roasting device is connected to the pre-concentration device, the water layer solution in the sedimentation unit flows through the pre-concentration device and the hydrolysis and roasting device in sequence, and the high-temperature gas generated by the hydrolysis and roasting device returns to the pre-concentration device to preheat the water layer solution; the hydrochloric acid preparation module includes a hydrochloric acid absorption device; The cold-rolled iron-containing waste emulsified oil regeneration system device also includes a tail gas purification unit, which is used to collect and treat the tail gas discharged from the acid leaching unit and the hydrochloric acid preparation unit. The tail gas purification unit includes a tail gas purification device connected to the hydrochloric acid absorption device, and an acid mist absorption device connected to the acid leaching unit. The hydrochloric acid produced by the tail gas purification device is divided into two paths, one path returns to the tail gas purification device, and the other path returns to the hydrochloric acid absorption device; the hydrochloric acid produced by the acid mist absorption device is divided into two paths, one path returns to the acid mist absorption device, and the other path is connected to the hydrochloric acid inlet pipeline of the acid leaching unit; The regeneration method comprises: The cold-rolled iron-containing waste emulsified oil is mixed with hydrochloric acid for acid leaching, and then precipitated and separated to obtain an oil layer and a water layer, wherein the sedimentation treatment is a two-stage sedimentation; wherein the oil layer solution enters the emulsified oil regeneration unit, and after adsorption purification, an emulsified oil additive is added to regenerate the emulsified oil; the water layer solution enters the hydrochloric acid preparation unit to prepare a hydrochloric acid solution, and the prepared hydrochloric acid solution is returned to the acid leaching process to react with the cold-rolled iron-containing waste emulsified oil for acid leaching; The temperature at the end point of the acid leaching reaction is 75-85° C., the pH at the end point of the acid leaching reaction when hydrochloric acid is added is 2-4, iron powder is added during the acid leaching reaction, and the pH at the end point of the acid leaching reaction when iron powder is added is 5.5-6.
2. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 1, characterized in that: The acid leaching unit comprises an acid leaching device.
3. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 2, characterized in that: The liquid inlet pipe of the acid leaching device is divided into two routes, namely a waste emulsified oil liquid inlet pipeline and a hydrochloric acid liquid inlet pipeline. Both the waste emulsified oil liquid inlet pipeline and the hydrochloric acid liquid inlet pipeline are provided with an electromagnetic flowmeter and a regulating valve.
4. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 3, characterized in that: The regulating valve is electrically connected to an online pH meter, which is used to detect the pH of the solution in the acid leaching device and feedback control the regulating valve to adjust the waste emulsified oil inlet flow rate and the hydrochloric acid inlet flow rate.
5. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 2, characterized in that: The lining material of the acid leaching device includes enamel, steel lining rubber or steel lining plastic.
6. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 1, characterized in that: The sedimentation unit comprises two sedimentation devices in series, the sedimentation device is used for oil-water separation, the waste emulsified oil enters the sedimentation device for stratification to obtain an oil layer and a water layer, wherein the oil layer enters the emulsified oil regeneration unit, and the water layer enters the hydrochloric acid preparation unit.
7. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 6, characterized in that: The shell material of the sedimentation device includes PP, PPH or glass fiber reinforced plastic.
8. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 6, characterized in that: The sedimentation unit also includes a solution collecting device connected to the sedimentation device. The water layer solution obtained by stratification in the sedimentation device is collected and stored by the solution collecting device and then enters the hydrochloric acid preparation unit.
9. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 1, characterized in that: The emulsified oil regeneration unit comprises a purification module and a regeneration module which are sequentially connected along the material flow direction. After the waste emulsified oil flows through the purification module and the regeneration module in sequence, regenerated emulsified oil is obtained.
10. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 9, characterized in that: The purification module comprises at least one adsorption device.
11. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 10, characterized in that: The purification module comprises an activated clay adsorption device and an activated carbon adsorption device which are connected in sequence.
12. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 11, characterized in that: The activated carbon filled in the activated carbon adsorption device includes at least one of coconut shell activated carbon, wood activated carbon or bamboo activated carbon, or a combination of two or more thereof.
13. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 9, characterized in that: The regeneration module comprises an emulsified oil preparation device.
14. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 1, characterized in that: The hydrochloric acid preparation module is also connected to the hydrochloric acid liquid inlet pipeline.
15. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 1, characterized in that: The regeneration method specifically comprises: (I) After being measured by an electromagnetic flowmeter, the cold-rolled iron-containing waste emulsified oil and hydrochloric acid are respectively introduced into an acid leaching device for acid leaching reaction. During the reaction, the pH of the solution in the acid leaching device is detected by an online pH meter and a feedback control regulating valve is used to adjust the inlet flow rate of the waste emulsified oil and the inlet flow rate of the hydrochloric acid; (II) the solution after the reaction is passed into a sedimentation device for sedimentation treatment, and waste emulsified oil and ferrous chloride solution are obtained by stratification; (III) the waste emulsified oil obtained in step (II) enters a purification module for adsorption purification, and then enters a regeneration module, an emulsified oil additive is added to the regeneration module, and emulsified oil is regenerated; (IV) The ferrous chloride solution obtained in step (II) is sequentially introduced into a pre-concentrator and a hydrolysis and calcination device for pre-concentration and spray pyrolysis, respectively. After spray pyrolysis, high-temperature HCl gas and iron oxide products are generated. The high-temperature HCl gas returns to the pre-concentrator to preheat and concentrate the ferrous chloride solution entering the hydrolysis and calcination device. The preheated HCl gas enters the hydrochloric acid absorption device to prepare hydrochloric acid.
16. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 15, characterized in that: In steps (I) and (IV), the concentration of the hydrochloric acid is 18-21 wt%.
17. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 15, characterized in that: In step (III), the adsorption purification operation is to sequentially enter the activated clay adsorption device and the activated carbon adsorption device to perform activated clay adsorption and activated carbon adsorption respectively.
18. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 15, characterized in that: In step (III), the emulsified oil additives include emulsifiers, rust removers, extreme pressure agents, bactericides and defoamers.
19. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 15, characterized in that: In step (IV), the temperature of the spray pyrolysis in the hydrolysis roasting device is 550-700°C.
20. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 15, characterized in that: In step (IV), the method of preheating and concentrating the ferrous chloride solution by high-temperature HCl gas in the preconcentrator is direct contact preheating and concentration.
21. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 15, characterized in that: In step (IV), the temperature of the high-temperature HCl generated after the spray pyrolysis is 350-450°C.
22. The method for regenerating cold-rolled iron-containing waste emulsified oil according to claim 15, characterized in that: In step (IV), the temperature of the preheated HCl is reduced to 85-95°C.
Citation Information
Patent Citations
Method for processing liquid fuel oil by using waste oil
CN101805644A
Waste emulsified oil regenerating process
CN102399617A
Purification method of waste emulsified oil
CN103849453A
Rolled oil sludge purifying method
CN104004581A
Treatment method of ferrous waste hydrochloric acid
CN104828995A