Cylindrical body and method for manufacturing the same

By using a Ni-W alloy layer cylindrical body in the contact terminal, etching to form a spiral spring portion, with its end protruding outside the Ni metal layer, solves the problem of conductivity decline and achieves efficient conductivity maintenance and Electrode connection stability.

CN112005121BActive Publication Date: 2024-10-25NIDEC-READ CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980027470.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-04-27
Filing Date
2019-04-10
Publication Date
2024-10-25
Estimated Expiration
2039-04-10

AI Technical Summary

Technical Problem

The conductivity of existing contact terminals tends to decrease after the natural oxide film is formed, requiring frequent gold plating or removal of the oxide film to maintain conductivity.

Method used

A cylindrical body containing a Ni metal layer and a Ni-W alloy layer is used. The end of the Ni-W alloy layer protrudes to the outside of the Ni metal layer through etching to form a spiral spring portion to enhance conductivity and reduce contact with the electrode. area, increasing contact pressure.

Benefits of technology

It is possible to maintain the excellent conductivity of the contact terminal without the need for frequent gold plating or removal of oxide films, thereby enhancing the stability of the contact connection with the electrode and the reliability of conduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112005121B_ABST
    Figure CN112005121B_ABST
Patent Text Reader

Abstract

The present invention provides a cylindrical body having excellent conductivity with a simple structure and a method for manufacturing the same. The present invention is a cylindrical body (2) including a conductive member provided with a spiral spring portion, the cylindrical body having a Ni metal layer (5) and a Ni-W alloy layer (6) containing W, the end portion (62) of the Ni-W alloy layer protruding to the outside of the Ni metal layer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is based on Japanese patent application No. 2018-086082 filed on April 27, 2018, and the contents are incorporated herein by reference. Technical Field

[0002] The present invention relates to a cylindrical body that can be used for inspecting an inspection object and a method for manufacturing the cylindrical body. Background Art

[0003] Previously, after a gold-plated layer, an electroformed Ni layer, and a resist layer were formed on the periphery of an extremely fine core wire, the resist layer was spirally irradiated with laser light to remove the irradiated portion of the resist layer, followed by etching to remove the electroformed Ni layer from the portion where the resist layer was removed, and then the core wire was removed, thereby manufacturing a contact terminal having a spiral spring portion (see, for example, Patent Document 1).

[0004] The contact terminal manufactured in this manner is constructed as follows: when inspecting the inspection object, one end of the contact terminal is crimped to the electrode side according to the restoring force generated by the elastic deformation of the spiral spring portion, and the other end of the contact terminal is applied to the inspection object side, thereby achieving electrical conduction.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 4572303 Summary of the invention

[0008] Furthermore, when a natural oxide film is formed on the electrode at one end of the contact terminal constructed as described above, the conductivity may be reduced. Therefore, it is necessary to plate the electrode with gold to suppress the formation of the natural oxide film, or to regularly remove the natural oxide film formed on the surface of the electrode.

[0009] An object of the present invention is to provide a cylindrical body having excellent conductivity with a simple structure and a method for manufacturing the same.

[0010] A cylindrical body according to an example of the present invention includes a conductive member provided with a spiral spring portion, and includes a Ni metal layer and a Ni—W alloy layer containing W, wherein an end portion of the Ni—W alloy layer protrudes outward from the Ni metal layer.

[0011] Moreover, a method for manufacturing a cylindrical body according to an example of the present invention includes: a gold-plated layer forming step of forming a gold-plated layer on the outer peripheral surface of a core wire; a Ni metal layer forming step of forming a Ni metal layer on the outer peripheral surface of the gold-plated layer; a Ni-W alloy layer forming step of forming a Ni-W alloy layer containing W on the outer peripheral surface of the Ni metal layer; an anti-corrosion layer forming step of forming an anti-corrosion layer on the outer peripheral surface of the Ni-W alloy layer; a spiral groove forming step of forming a spiral groove on the anti-corrosion layer; a metal layer removing step of removing the Ni metal layer and the Ni-W alloy layer located in the forming portion of the spiral groove by etching the anti-corrosion layer as a masking material, and etching the end of the Ni metal layer according to the difference in etching speed between the Ni metal layer and the Ni-W alloy layer so that the end of the Ni-W alloy layer protrudes to the outside of the Ni metal layer; an anti-corrosion layer removing step of removing the anti-corrosion layer; a gold-plated layer removing step of removing the gold-plated layer located in the forming portion of the spiral groove; and a core wire pulling out step of pulling out the core wire.

[0012] Moreover, a method for manufacturing a cylindrical body according to an example of the present invention includes: a gold-plated layer forming step of forming a gold-plated layer on the outer peripheral surface of a core wire; a Ni-W alloy layer forming step of forming a Ni-W alloy layer containing W on the outer peripheral surface of the gold-plated layer; a Ni metal layer forming step of forming a Ni metal layer on the outer peripheral surface of the Ni-W alloy layer; an anti-corrosion layer forming step of forming an anti-corrosion layer on the outer peripheral surface of the Ni metal layer; a spiral groove forming step of forming a spiral groove on the anti-corrosion layer; a metal layer removing step of removing the Ni metal layer and the Ni-W alloy layer located in the forming portion of the spiral groove by etching the anti-corrosion layer as a masking material, and etching the end of the Ni metal layer according to the difference in etching speed between the Ni metal layer and the Ni-W alloy layer so that the end of the Ni-W alloy layer protrudes to the outside of the Ni metal layer; an anti-corrosion layer removing step of removing the anti-corrosion layer; a gold-plated layer removing step of removing the gold-plated layer located in the forming portion of the spiral groove; and a core wire pulling out step of pulling out the core wire. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a front view showing an embodiment of a contact terminal using a cylindrical body of the present invention.

[0014] Figure 2 It is a partially cutaway front view showing a specific structure of a cylindrical body constituting a contact terminal.

[0015] Figure 3 It is a process diagram showing a first embodiment of the method for manufacturing a cylindrical body according to the present invention.

[0016] Figure 4 It is a cross-sectional view showing the first stage of the manufacturing process of the cylindrical body.

[0017] Figure 5 It is a cross-sectional view showing the second stage of the manufacturing process of the cylindrical body.

[0018] Figure 6 It is a cross-sectional view showing the third stage of the manufacturing process of the cylindrical body.

[0019] Figure 7 It is a cross-sectional view showing the fourth stage of the manufacturing process of the cylindrical body.

[0020] Figure 8 It is a cross-sectional view showing the fifth stage of the manufacturing process of the cylindrical body.

[0021] Fig. 9 It is a cross-sectional view showing the sixth stage of the manufacturing process of the cylindrical body.

[0022] Fig.10 It is a cross-sectional view showing the seventh stage of the manufacturing process of the cylindrical body.

[0023] Fig.11 It is a cross-sectional view showing the structure of a contact terminal including a cylindrical body and a central conductor.

[0024] Fig.12 It is a cross-sectional view showing the structure of an inspection jig including contact terminals.

[0025] Fig.13 It is a perspective view showing a state in which the end of the cylindrical body and the electrode are facing each other.

[0026] Fig.14 It is a cross-sectional view showing the inspection state of the inspection object.

[0027] Fig.15 It is a cross-sectional view showing a state where the electrode protrudes from the end surface of the base plate.

[0028] Fig.16 It is a process diagram showing a second embodiment of the method for manufacturing a cylindrical body of the present invention.

[0029] Fig.17 This is a perspective view showing a state in which the end of a cylindrical body and an electrode are facing each other according to the second embodiment of the present invention.

[0030] Fig.18 This is a cross-sectional view showing a state where the electrode is sunken further inside the end surface of the base plate.

[0031] [Explanation of Symbols]

[0032] 1.1a: Contact terminal

[0033] 2. 2a: Cylindrical body

[0034] 3: Center conductor

[0035] 4: Gold plating

[0036] 5.5a: Ni metal layer

[0037] 6, 6a: Ni-W alloy layer

[0038] 7: Anti-corrosion layer

[0039] 8: Check the fixture

[0040] 9: Check the object

[0041] 10: Core wire

[0042] 31: Connection

[0043] 51: Spring part of Ni metal layer

[0044] 61: Spring part of Ni-W alloy layer

[0045] 62, 62a: End of Ni-W alloy layer

[0046] 71: Spiral groove of the anti-corrosion layer

[0047] 81: Supporting member

[0048] 81a, 81b, 81c: Support plate

[0049] 83: Base plate

[0050] 84: Wiring

[0051] 85: Electrode

[0052] 91: Checkpoint

[0053] H: Through hole

[0054] Ha: Through hole

[0055] Hb: small track

[0056] K1: Gold plating layer formation step

[0057] K2: Ni metal layer formation step

[0058] K2a: Ni-W alloy layer formation step

[0059] K3: Ni-W alloy layer formation step

[0060] K3a: Ni metal layer formation step

[0061] K4: Resist layer formation step

[0062] K5: Spiral groove forming steps

[0063] K6: Metal layer removal step

[0064] K7: Resist removal step

[0065] K8: Gold plating removal steps

[0066] K9: Steps for pulling out the core wire

[0067] w1, w2: width of the spring part DETAILED DESCRIPTION

[0068] Hereinafter, embodiments of the present invention will be described based on the drawings. In addition, the same reference numerals in the drawings indicate the same configurations, and their descriptions are omitted.

[0069] (First Embodiment)

[0070] Figure 1 is a front view showing an example of the contact terminal 1, Figure 2 It is a partially cutaway front view showing a specific structure of the cylindrical body 2 constituting the contact terminal 1 according to the present invention.

[0071] like Figure 1 As shown, the contact terminal 1 includes a cylindrical body 2 formed of a conductive material in a cylindrical shape or the like, and a central conductor 3 formed of a conductive material in a rod shape having a substantially circular cross section.

[0072] like Figure 2 As shown, the cylindrical body 2 includes: an innermost gold-plated layer 4, a Ni metal layer 5 disposed on its outer peripheral surface and containing nickel (hereinafter referred to as Ni) or a Ni-P alloy containing Ni and a specified amount of phosphorus (hereinafter referred to as P), and a Ni-W alloy layer 6 containing a fixed amount of tungsten (hereinafter referred to as W).

[0073] In the portion other than the two ends of the cylindrical body 2, the spiral spring portion 51 and the spring portion 61 that expand and contract in the axial direction of the cylindrical body 2 are formed on the Ni metal layer 5 and the Ni-W alloy layer 6, respectively, over a predetermined length. In addition, in the above-described embodiment, as described later, the width dimension w1 of the spring portion 51 formed on the Ni metal layer 5 is formed to be smaller than the width dimension w2 of the spring portion 61 formed on the Ni-W alloy layer 6.

[0074] The end 62 of the Ni-W alloy layer 6 protrudes a certain distance outward from the end surfaces of the gold plated layer 4 and the Ni metal layer 5. The protrusion amount of the end 62 of the Ni-W alloy layer 6 is preferably 1 μm or more and 0.5 times the outer diameter of the cylindrical body 2 or less.

[0075] Figure 3 1 is a step diagram showing a first embodiment of a method for manufacturing a cylindrical body 2 of the present invention. Figures 4 to 102 is a cross-sectional view showing the first to seventh stages of the manufacturing process of the cylindrical body 2. Fig.11 is a cross-sectional view showing the structure of the contact terminal 1 including the cylindrical body 2 and the central conductor 3. Fig.12 is a cross-sectional view showing the structure of the inspection jig 8 including the contact terminal 1, Fig.13 2 is a perspective view showing a state where the end portion 62 of the cylindrical body 2 and the electrode 85 are facing each other. Fig.14 is a cross-sectional view showing the inspection state of the inspection object 9, Fig.15 It is a cross-sectional view showing a state where the electrode 85 protrudes from the end surface of the base plate 83 .

[0076] like Figure 3 As shown, the manufacturing method of the cylindrical body 2 of the present invention comprises: a gold-plated layer forming step K1, forming a gold-plated layer 4 on the outer peripheral surface of the core wire 10 described later; a Ni metal layer forming step K2, forming a Ni metal layer 5 on the outer peripheral surface of the gold-plated layer 4; a Ni-W alloy layer forming step K3, forming a Ni-W alloy layer 6 containing W on the outer peripheral surface of the Ni metal layer 5; an anti-corrosion layer forming step K4, forming an anti-corrosion layer 7 on the outer peripheral surface of the Ni-W alloy layer 6; a spiral groove forming step K5, forming a spiral groove 71 on the anti-corrosion layer 7; a metal layer removing step K4. Step K6, removing the Ni metal layer 5 and the Ni-W alloy layer 6 located in the formation portion of the spiral groove 71 by etching the anti-etching layer 7 as a masking material, and making the end 62 of the Ni-W alloy layer 6 protrude to the outside of the Ni metal layer 5 according to the difference in etching speed between the Ni metal layer 5 and the Ni-W alloy layer 6; anti-etching layer removal step K7, removing the anti-etching layer 7; gold-plated layer removal step K8, removing the gold-plated layer 4 located in the formation portion of the spiral groove 71 of the anti-etching layer 7; and core wire pulling out step K9, pulling out the core wire 10.

[0077] In the gold plating layer forming step K1, on the surface of the core wire 10 including a steel wire such as stainless steel or aluminum alloy or a wire made of a synthetic resin such as nylon resin or polyethylene resin, a Figure 4 As shown, a gold plating layer 4 having a thickness of about 0.2 μm to 1 μm is formed. In addition, the core wire 10 can use a core wire having an extremely fine outer diameter of 5 μm or more, for example, about 30 μm. Moreover, when a wire made of synthetic resin is used as the core wire 10, it is preferable to form the gold plating layer 4 by electroless plating.

[0078] Next, in the Ni metal layer forming step K2, the outer peripheral surface of the gold plating layer 4 is electroformed using an electroforming device (not shown). Figure 5 As shown, a Ni metal layer 5 made of Ni or a Ni-P alloy containing 0.5 wt % to 10 wt % of P is formed on the outer peripheral surface of the gold plated layer 4. The thickness of the Ni metal layer 5 is set to about 4 μm to 15 μm.

[0079] Furthermore, in the Ni-W alloy layer forming step K3, the outer peripheral surface of the Ni metal layer 5 is subjected to electroforming treatment using an electroforming device outside the figure, thereby Figure 6 As shown, a Ni—W alloy layer 6 is formed, which is made of a Ni—W alloy containing, for example, 10 wt % to 90 wt % of W. The thickness of the Ni—W alloy layer 6 is set to about 2 μm to 8 μm, and is formed thinner than the Ni metal layer 5 .

[0080] Furthermore, in the resist layer forming step K4, the core wire 10 formed with the gold plating layer 4, the Ni metal layer 5 and the Ni-W alloy layer 6 is immersed in a photoresist tank containing a photoresist solution for a predetermined time. Figure 7 As shown, the anti-corrosion layer 7 is formed on the outer peripheral surface of the Ni—W alloy layer 6 .

[0081] Next, in the spiral groove forming step K5, the core wire 10 is rotated at a fixed speed and a laser irradiation device (not shown) is moved in the axial direction of the core wire 10 while irradiating the core wire 10 with laser light, thereby Figure 8 As shown, a spiral groove 71 is formed in the resist layer 7.

[0082] Then, in the metal layer removal step K6, the core wire 10 with the anti-corrosion layer 7 formed on the periphery is immersed in an acidic electrolytic polishing solution, and the anti-corrosion layer 7 remaining on the periphery of the Ni-W alloy layer 6 is etched as a masking material, thereby removing the Ni metal layer 5 and the Ni-W alloy layer 6 located in the formation portion of the spiral groove 71. As a result, Fig. 9 As shown, the spring portion 51 and the spring portion 61 extending in a spiral shape along the spiral groove 71 of the resist layer 7 are formed on the Ni metal layer 5 and the Ni—W alloy layer 6 , respectively.

[0083] According to the manufacturing method, the following cylindrical body 2 can be easily manufactured, that is, the Ni-W alloy layer 6 is arranged on the outer peripheral surface side of the Ni metal layer 5, the end 62 of the Ni-W alloy layer 6 protrudes to the outside of the Ni metal layer 5, and has excellent conductivity.

[0084] That is, the Ni-W alloy layer 6 containing a fixed amount of W has better corrosion resistance than the Ni metal layer 5, and thus the etching rate of the Ni-W alloy layer 6 tends to be slower than that of the Ni metal layer 5. Therefore, even if the time of immersion in the electrolytic polishing solution is the same, the end of the Ni metal layer 5 is more etched than the end 62 of the Ni-W alloy layer 6, and thus, the end 62 of the Ni-W alloy layer 6 protrudes to the outside of the Ni metal layer 5.

[0085] Moreover, similarly, the Ni metal layer 5 located at the portion where the spiral groove 71 is formed is etched more significantly than the Ni-W alloy layer 6, so that the width dimension w1 of the spring portion 51 formed in the Ni metal layer 5 is smaller than the width dimension w2 of the spring portion 61 formed in the Ni-W alloy layer 6 (refer to Figure 2 ).

[0086] Next, in the resist removal step K7, the resist layer 7 is dissolved and removed using a resist removal solution or the like, and in the gold plating removal step K8, the gold plating layer 4 located at the portion where the spiral groove 71 is formed is removed by ultrasonic cleaning or the like (see Fig.10 ).

[0087] In the core wire extraction step K9, the core wire 10 is pulled to reduce its outer diameter, and the core wire 10 is peeled off from the gold plating layer 4 and extracted. Figure 2 As shown, a cylindrical body 2 having a Ni metal layer 5 provided on the inner peripheral surface with a gold plated layer 4 and a Ni—W alloy layer 6 provided on the outer peripheral surface side thereof is manufactured.

[0088] On the other hand, the center conductor 3 includes a rod-shaped body with a circular cross section having an outer diameter that can be inserted into the cylindrical body 2, and a connecting portion 31 with a narrowed front end is formed at one end of the center conductor 3. In addition, when the main body of the center conductor 3 is inserted into the cylindrical body 2 and the front end of the center conductor 3 including the connecting portion 31 protrudes out of the cylindrical body 2 by a predetermined distance, as shown in FIG. Fig.11 As shown, the cylindrical body 2 and the central conductor 3 are integrally connected by caulking, welding, press-fitting, or other methods, thereby manufacturing the contact terminal 1 including the cylindrical body 2 and the central conductor 3.

[0089] The contact terminal 1 manufactured as described above is Fig.12 As shown, the inspection jig 8 is supported by a support member 81 and a base plate 83 constituting an inspection jig 8. The inspection jig 8 is used, for example, to inspect an inspection object 9, which includes a glass epoxy substrate, a flexible substrate, a ceramic multilayer wiring substrate, an electrode plate for a liquid crystal display or a plasma display, a transparent conductive plate for a touch screen, a packaging substrate or a film carrier for a semiconductor package, or a semiconductor substrate such as a semiconductor wafer or a semiconductor element.

[0090] The support member 81 is formed by stacking, for example, plate-shaped support plates 81a, 81b, and 81c, and a plurality of through holes H are formed to penetrate the support plates 81a, 81b, and 81c.

[0091] The support plate 81b and the support plate 81c each have an insertion hole Ha including an opening hole of a predetermined diameter. In addition, in the support plate 81a, a small-diameter portion Hb including a through hole having a smaller diameter than the insertion hole Ha is formed at a portion facing the inspection point 91 of the substrate or the like as the inspection object 9. The small-diameter portion Hb of the support plate 81a is connected to the insertion hole Ha of the support plate 81b and the support plate 81c, thereby forming a through hole H that serves as a setting portion of the contact terminal 1.

[0092] In addition, the support member 81 is not limited to the example in which the support plates 81a, 81b, and 81c are stacked in a plate-like manner, and for example, a through hole H including a small diameter portion Hb and an insertion hole portion Ha may be provided in an integral member. Furthermore, instead of the example in which the support plates 81b and 81c of the support member 81 are stacked on each other, a configuration may be provided in which the support plates 81b and 81c are spaced apart from each other and connected by, for example, a support column or the like.

[0093] A base plate 83 made of, for example, an insulating resin material is disposed on one end side of the support plate 81c. The opening of the through hole H, that is, the end surface of the insertion hole Ha, is blocked by the base plate 83. A wiring 84 is installed in the base plate 83 at a position facing the through hole H so as to penetrate the base plate 83. Fig.13 As shown, the electrode 85 including the end surface of the wiring 84 is arranged to face the cylindrical body 2 of the contact terminal 1 .

[0094] When inspecting an inspection object 9 including a substrate, for example, Fig.14 As shown, one end of the contact terminal 1 supported by the support member 81, specifically, the end 62 of the Ni-W alloy layer 6 constituting the cylindrical body 2 abuts against the electrode 85 provided on the base plate 83. Furthermore, the other end of the contact terminal 1, specifically, the connection portion 31 of the central conductor 3 abuts against the inspection point 91 provided on the wiring pattern (pattern) or solder bump (bump) of the inspection object 9.

[0095] Then, the spring portion of the cylindrical body 2, specifically, the spring portion 51 of the Ni metal layer 5 and the spring portion 61 of the Ni-W alloy layer 6, is compressed and elastically deformed according to the pressure acting on the contact terminal 1. As a result, due to the restoring force of the cylindrical body 2, one end portion thereof is pressed against the electrode 85, and the base end portion of the contact terminal 1 is electrically connected to the electrode 85. Furthermore, the connecting portion 31 of the central conductor 3 is elastically pressed against the inspection point 91, and the front end portion of the contact terminal 1 is electrically connected to the inspection point 91.

[0096] Thus, the contact terminal 1 includes a cylindrical body 2, which includes a conductive member provided with a spiral spring portion 51 and a spring portion 61. The cylindrical body 2 has a Ni metal layer 5 and a Ni-W alloy layer 6 containing W. The end 62 of the Ni-W alloy layer 6 is provided in a manner protruding toward the outside of the Ni metal layer 5. Thus, the contact terminal 1 has the advantage of obtaining excellent conductivity with a simple structure.

[0097] That is, compared with the case where both the Ni metal layer 5 and the Ni-W alloy layer 6 constituting the cylindrical body 2 are in contact with the electrode 85, the contact area between the cylindrical body 2 and the electrode 85 can be greatly reduced, and the contact pressure between the two can be fully increased. In addition, the Ni-W alloy layer 6 containing a fixed amount of W has a characteristic of significantly higher hardness than the Ni metal layer 5, etc., so when a natural oxide film is formed on the surface of the electrode 85, the natural oxide film can be pierced to increase the reliability of the conductive connection between the contact terminal 1 and the electrode 85.

[0098] Therefore, there is no need to perform gold plating on the electrode 85 to suppress the formation of a natural oxide film or to periodically remove the natural oxide film formed on the surface of the electrode 85 as in the prior art. The inspection object 9 can be properly inspected while the contact terminal 1 and the electrode 85 are conductively connected.

[0099] For example, by setting the content of W constituting the Ni-W alloy layer 6 to 10 wt % or more, the hardness of the Ni-W alloy layer 6 can be effectively improved. Furthermore, by setting the content of W in the Ni-W alloy layer 6 to less than 90 wt %, the strength of the Ni-W alloy layer 6 can be sufficiently maintained.

[0100] If the content of tungsten is high, the resistance value of the Ni-W alloy layer 6 increases, so the content of W in the Ni-W alloy layer 6 is more preferably 10 wt% to 70 wt%. In addition, the higher the content of tungsten, the greater the difference in etching amount between Ni or Ni alloy and Ni-W, so the content of W in the Ni-W alloy layer 6 is more preferably 30 wt% to 70 wt%.

[0101] The W content in the Ni-W alloy layer 6 is measured by energy dispersive X-ray spectroscopy (EDX) on the surface of the Ni-W alloy layer 6. The measurement method is to set a predetermined point of the Ni-W alloy layer 6 and calculate it by averaging multiple points. The predetermined point is not particularly limited, for example, it can be set to a predetermined point at equal intervals in the length direction of the Ni-W alloy layer 6. Moreover, as Figure 1As shown, one or more points may be set from each of the spring portion 61 and the two cylindrical portions formed by sandwiching the spring portion 61. Specifically, the surface is measured by EDX with the Ni-W alloy layer 6 exposed. Fig.17 In the contact terminal 1a, the surface of the exposed part of the Ni-W alloy layer 6a near the end 62a or the surface of the Ni-W alloy layer 6a exposed by peeling off the Ni metal layer 5a can be measured. Before the measurement, the surface of the object is cleaned with ethanol. The measurement can be performed using, for example, a device combining a scanning electron microscope (Scanning Electron Microscope, SEM) and EDX. The electron beam is set to 15kV, 80μA. Regarding the W content, 5 points are measured in the length direction (tube axis direction) and the average value is calculated.

[0102] Moreover, as shown in the first embodiment, according to the structure in which the Ni-W alloy layer 6 is arranged on the outer peripheral surface side of the Ni metal layer 5, the Ni-W alloy layer 6 at the end 62 abutting against the electrode 85 is effectively reinforced by the Ni metal layer 5 arranged on the inner peripheral surface side of the Ni-W alloy layer 6, thereby fully maintaining the strength and elasticity of the cylindrical body 2.

[0103] Furthermore, the Ni metal layer 5 has a higher conductivity than the Ni-W alloy layer 6, so that most of the current passing through the contact terminal 1 flows through the Ni metal layer 5 except for the end of the cylindrical body 2. Therefore, by setting the cylindrical body 2 to have a multilayer structure including the Ni metal layer 5 and the Ni-W alloy layer 6, there is an advantage that the resistance increase of the contact terminal 1 can be effectively suppressed. In particular, as shown in the above embodiment, when the thickness of the Ni-W alloy layer 6 is formed to be thinner than the Ni metal layer 5, the resistance increase of the contact terminal 1 can be more effectively suppressed.

[0104] Furthermore, if Fig.15 As shown, when the electrode 85 including the end surface of the wiring 84 protrudes from the end surface of the base plate 83, or when the electrode 85 and the end surface of the base plate 83 are formed on the same surface, the Ni-W alloy layer 6 is arranged on the outer peripheral surface side of the Ni metal layer 5, thereby setting the contact range between the end 62 of the Ni-W alloy layer 6 and the electrode 85 to a large range. As a result, there is an advantage that the conductivity of the cylindrical body 2 and the electrode 85 can be well maintained, and the formation of a dent on the electrode 85 can be effectively suppressed.

[0105] In addition, the Ni metal layer 5 including the Ni-P alloy containing 0.5 wt% to 10 wt% of P has the property of not being easily plastically deformed even at a high temperature of 150° C. or higher. Therefore, by forming the Ni metal layer 5 with the Ni-P alloy containing 0.5 wt% to 10 wt% of P, the strength and elasticity of the cylindrical body 2 can be further improved.

[0106] Furthermore, when the protrusion amount of the end portion 62 of the Ni-W alloy layer 6 is set to be 1 μm or more as described above, the contact between the Ni metal layer 5 and the electrode 85 can be suppressed, and the end portion 62 of the Ni-W alloy layer 6 can be brought into contact with the electrode 85. Furthermore, by setting the protrusion amount of the end portion 62 of the Ni-W alloy layer 6 to be 0.5 times or less of the outer diameter of the cylindrical body 2 as described above, there is an advantage that the increase in the resistance of the cylindrical body 2 can be reduced, and when the end portion 62 of the Ni-W alloy layer 6 is brought into contact with the electrode 85, the concern about the end portion 62 of the Ni-W alloy layer 6 being damaged can be reduced.

[0107] in addition, Figure 3 In the manufacturing method of the cylindrical body shown, the following structure can be set, that is, the gold plating layer forming step K1 and the gold plating layer removing step K8 are omitted, the Ni metal layer 5 is formed on the outer peripheral surface of the core wire 10 by electroforming, and the gold plating layer 4 located on the inner peripheral surface of the Ni metal layer 5 is omitted.

[0108] (Second Embodiment)

[0109] Fig.16 1 is a step diagram showing a method for manufacturing a cylindrical body according to a second embodiment of the present invention. Fig.17 2 is a perspective view showing the structure of a contact terminal 1a using a cylindrical body 2a according to a second embodiment of the present invention. Fig.18 It is a cross-sectional view showing a state where the electrode 85 is sunken further inside the end surface of the base plate 83 .

[0110] The manufacturing method of the cylindrical body of the second embodiment comprises: a gold-plated layer forming step K1, forming a gold-plated layer 4 on the outer peripheral surface of the core wire; a Ni-W alloy layer forming step K2a, forming a Ni-W alloy layer 6a containing W on the outer peripheral surface of the gold-plated layer 4; a Ni metal layer forming step K3a, forming a Ni metal layer 5a on the outer peripheral surface of the Ni-W alloy layer 6a; an anti-corrosion layer forming step K4, forming an anti-corrosion layer on the outer peripheral surface of the Ni metal layer 5a; a spiral groove forming step K5, forming a spiral groove in the anti-corrosion layer; a metal layer removal step K3a, forming a Ni metal layer 5a on the outer peripheral surface of the Ni-W alloy layer 6a; a metal layer removal step K4, forming a metal layer 5a on the outer peripheral surface of the Ni metal layer 5a; a metal layer removal step K5, forming a metal layer 5a on the outer peripheral surface of the Ni metal layer 5a; a metal layer removal step K6, forming a metal layer 5a on the outer peripheral surface of the Ni metal layer 5a; a metal layer 5a removal step K7, forming a metal layer 5a on the outer peripheral surface of the Ni metal layer 5a; a metal layer 5a removal step K8, forming a metal layer 5a on the outer peripheral surface of the Ni metal layer 5a; a metal layer 5a removal step K9, forming a metal layer 5a on the outer peripheral surface of the Ni metal layer 5a; a metal layer 5a removal step K10, forming a metal layer 5a on the outer peripheral surface of the Ni metal layer 5a; a metal layer 5a removal step K11, forming a metal layer 5a on the outer peripheral surface of the Ni metal layer 5a; a metal layer 5a removal step K12, forming a metal layer 5a on the outer peripheral surface of the Ni metal layer 5a; a metal layer 5a removal step K13, forming a metal layer 5a on the outer peripheral surface of In addition to step K6, the Ni metal layer 5a and the Ni-W alloy layer 6a located in the forming part of the spiral groove are removed by etching the anti-etching layer as a masking material, and the end of the Ni-W alloy layer 6a is made to protrude to the outside of the Ni metal layer 5a according to the difference in etching speed between the Ni metal layer 5a and the Ni-W alloy layer 6a; the anti-etching layer removal step K7, removing the anti-etching layer; the gold-plated layer removal step K8, removing the gold-plated layer 4 located in the forming part of the spiral groove; and the core wire pulling out step K9, pulling out the core wire.

[0111] According to the method for manufacturing a cylindrical body of the second embodiment, the cylindrical body 2a is manufactured as follows, that is, the outer peripheral surface of the gold-plated layer 4 formed in the gold-plated layer forming step K1 is as follows: Fig.17The Ni-W alloy layer 6a is formed as shown, and the Ni metal layer 5a is formed on its outer peripheral surface. The cylindrical body 2a is different from the first embodiment in that the Ni-W alloy layer 6a is arranged on the outer peripheral surface side of the Ni metal layer 5a.

[0112] In this way, when the Ni-W alloy layer 6a is disposed on the inner peripheral surface side of the Ni metal layer 5a, the end 62a of the Ni-W alloy layer 6a is located near the axis of the cylindrical body 2a compared to the cylindrical body 2 of the first embodiment. Therefore, there is an advantage that the end 62a of the Ni-W alloy layer 6a and the electrode 85 can be easily aligned.

[0113] For example, Fig.18 As shown in the figure, when the electrode 85 is sunken to the inner side than the end face of the base plate 83, when a large positional deviation occurs between the axis of the cylindrical body 2 and the axis of the electrode 85, there is a possibility that the Ni-W alloy layer 6a abuts against the end face of the base plate 83 and the electrode 85 cannot be brought into contact with the Ni-W alloy layer 6a. However, when the Ni-W alloy layer 6a is located inside the cylindrical body 2a as in the second embodiment, it is possible to suppress the Ni-W alloy layer 6a from abutting against the end face of the base plate 83 as compared with the case where the Ni-W alloy layer 6a is located outside the cylindrical body 2 as in the first embodiment. Therefore, by disposing the Ni-W alloy layer 6a on the inner peripheral surface side of the Ni metal layer 5a as described above, it is possible to easily perform position alignment for bringing the electrode 85 into contact with the Ni-W alloy layer 6a.

[0114] in addition, Fig.16 In the manufacturing method of the cylindrical body shown, the following structure can be set, that is, the gold plating layer forming step K1 and the gold plating layer removing step K8 are omitted, the Ni-W alloy layer 6a is formed on the outer peripheral surface of the core wire by electroforming, and the gold plating layer 4 located on the inner peripheral surface of the Ni-W alloy layer 6a is omitted.

[0115] Moreover, the cylindrical body 2 and the cylindrical body 2a need not be limited to the example of the component used as the contact terminal, and can be used for various purposes. Moreover, the cylindrical body 2 and the cylindrical body 2a need not be limited to the example of combining the cylindrical body 2 and the cylindrical body 2a with the central conductor 3, and the cylindrical body 2 and the cylindrical body 2a can also be directly used as the contact terminal.

[0116] That is, a cylindrical body according to an example of the present invention includes a conductive member provided with a spiral spring portion, and the cylindrical body has a Ni metal layer and a Ni—W alloy layer containing W, and an end portion of the Ni—W alloy layer protrudes outside the Ni metal layer.

[0117] According to the above configuration, the contact area between the cylindrical body and the electrode is greatly reduced, and the contact pressure between the two can be fully increased. In addition, the Ni-W alloy layer containing a fixed amount of W has a characteristic of significantly higher hardness than the Ni metal layer containing Ni or Ni-P alloy, etc., so even when a natural oxide film is formed on the surface of the electrode, the natural oxide film can be easily pierced to connect the cylindrical body to the electrode.

[0118] Furthermore, it is preferable to adopt a configuration in which the Ni—W alloy layer is disposed on the outer peripheral surface side of the Ni metal layer.

[0119] According to the above configuration, the Ni-W alloy layer at the end portion in contact with the electrode can be effectively reinforced by the Ni metal layer having low resistance. Therefore, the conductivity of the cylindrical body can be well maintained, and the strength and elasticity of the cylindrical body can be fully maintained.

[0120] Furthermore, the Ni—W alloy layer may be disposed on the inner peripheral surface side of the Ni metal layer.

[0121] According to the above configuration, since the end of the Ni—W alloy layer is located near the axis of the cylindrical body, there is an advantage that the end of the Ni—W alloy layer and the electrode can be easily aligned even when the electrode is immersed in the base plate.

[0122] Moreover, a method for manufacturing a cylindrical body according to an example of the present invention includes: a gold-plated layer forming step of forming a gold-plated layer on the outer peripheral surface of a core wire; a Ni metal layer forming step of forming a Ni metal layer on the outer peripheral surface of the gold-plated layer; a Ni-W alloy layer forming step of forming a Ni-W alloy layer containing W on the outer peripheral surface of the Ni metal layer; an anti-corrosion layer forming step of forming an anti-corrosion layer on the outer peripheral surface of the Ni-W alloy layer; a spiral groove forming step of forming a spiral groove on the anti-corrosion layer; a metal layer removing step of removing the Ni metal layer and the Ni-W alloy layer located in the forming portion of the spiral groove by etching the anti-corrosion layer as a masking material, and etching the end of the Ni metal layer according to the difference in etching speed between the Ni metal layer and the Ni-W alloy layer so that the end of the Ni-W alloy layer protrudes to the outside of the Ni metal layer; an anti-corrosion layer removing step of removing the anti-corrosion layer; a gold-plated layer removing step of removing the gold-plated layer located in the forming portion of the spiral groove; and a core wire pulling out step of pulling out the core wire.

[0123] According to the above configuration, a cylindrical body having excellent conductivity can be easily manufactured, in which the Ni—W alloy layer is disposed on the outer peripheral surface side of the Ni metal layer and the end of the Ni—W alloy layer protrudes outside the Ni metal layer.

[0124] Moreover, a method for manufacturing a cylindrical body according to an example of the present invention includes: a gold-plated layer forming step of forming a gold-plated layer on the outer peripheral surface of a core wire; a Ni-W alloy layer forming step of forming a Ni-W alloy layer containing W on the outer peripheral surface of the gold-plated layer; a Ni metal layer forming step of forming a Ni metal layer on the outer peripheral surface of the Ni-W alloy layer; an anti-corrosion layer forming step of forming an anti-corrosion layer on the outer peripheral surface of the Ni metal layer; a spiral groove forming step of forming a spiral groove on the anti-corrosion layer; a metal layer removing step of removing the Ni metal layer and the Ni-W alloy layer located in the forming portion of the spiral groove by etching the anti-corrosion layer as a masking material, and etching the end of the Ni metal layer according to the difference in etching speed between the Ni metal layer and the Ni-W alloy layer so that the end of the Ni-W alloy layer protrudes to the outside of the Ni metal layer; an anti-corrosion layer removing step of removing the anti-corrosion layer; a gold-plated layer removing step of removing the gold-plated layer located in the forming portion of the spiral groove; and a core wire pulling out step of pulling out the core wire.

[0125] According to the above-described structure, the cylindrical body includes a Ni-W alloy layer disposed on the inner peripheral surface side of a Ni metal layer, and an end portion of the Ni-W alloy layer protrudes toward the outside of the Ni metal layer, thereby making it easy to manufacture a cylindrical body in which the end portion of the Ni-W alloy layer can be easily aligned with the position of the electrode.

[0126] The cylindrical body of such a structure can easily obtain excellent conductivity with a simple structure. Moreover, according to the manufacturing method of the cylindrical body, a cylindrical body with excellent conductivity can be easily manufactured.

[0127] In addition, the specific embodiments and examples mentioned in the section of the specific embodiments are only for clarifying the technical content of the present invention, and the present invention should not be limited to such specific examples and interpreted in a narrow sense.

Claims

1. A cylindrical body comprising a conductive member provided with a spiral spring portion, The cylindrical body has a Ni metal layer and a Ni-W alloy layer containing W. The end of the Ni-W alloy layer protrudes outward from the Ni metal layer, and The Ni—W alloy layer is formed thinner than the Ni metal layer.

2. The cylindrical body according to claim 1, wherein The Ni—W alloy layer is disposed on the outer peripheral surface side of the Ni metal layer.

3. The cylindrical body according to claim 1, wherein The Ni—W alloy layer is disposed on the inner peripheral surface side of the Ni metal layer.

4. A method for manufacturing a cylindrical body, comprising: a gold-plated layer forming step of forming a gold-plated layer on the outer peripheral surface of the core wire; A Ni metal layer forming step, forming a Ni metal layer on the outer peripheral surface of the gold-plated layer; A Ni-W alloy layer forming step, forming a Ni-W alloy layer containing W on the outer peripheral surface of the Ni metal layer; an anti-corrosion layer forming step, forming an anti-corrosion layer on the outer peripheral surface of the Ni-W alloy layer; a spiral groove forming step of forming a spiral groove in the resist layer; a metal layer removing step, wherein the Ni metal layer and the Ni-W alloy layer located at the formation portion of the spiral groove are removed by etching the anti-etching layer as a masking material, and an end portion of the Ni metal layer is etched according to a difference in etching speed between the Ni metal layer and the Ni-W alloy layer so that the end portion of the Ni-W alloy layer protrudes outward from the Ni metal layer; an anti-corrosion layer removing step, removing the anti-corrosion layer; a gold-plated layer removing step of removing the gold-plated layer at a portion where the spiral groove is formed; as well as A core wire pulling out step, pulling out the core wire, and In the Ni—W alloy layer forming step, the Ni—W alloy layer is formed to be thinner than the Ni metal layer.

5. A method for manufacturing a cylindrical body, comprising: a gold-plated layer forming step of forming a gold-plated layer on the outer peripheral surface of the core wire; A Ni-W alloy layer forming step, forming a Ni-W alloy layer containing W on the outer peripheral surface of the gold-plated layer; A Ni metal layer forming step, forming a Ni metal layer on the outer peripheral surface of the Ni-W alloy layer; an anti-corrosion layer forming step, forming an anti-corrosion layer on the outer peripheral surface of the Ni metal layer; a spiral groove forming step of forming a spiral groove in the resist layer; a metal layer removing step, wherein the Ni metal layer and the Ni-W alloy layer located at the formation portion of the spiral groove are removed by etching the anti-etching layer as a masking material, and an end portion of the Ni metal layer is etched according to a difference in etching speed between the Ni metal layer and the Ni-W alloy layer so that the end portion of the Ni-W alloy layer protrudes outward from the Ni metal layer; an anti-corrosion layer removing step, removing the anti-corrosion layer; a gold-plated layer removing step of removing the gold-plated layer at a portion where the spiral groove is formed; as well as A core wire pulling out step, pulling out the core wire, and In the Ni—W alloy layer forming step, the Ni—W alloy layer is formed to be thinner than the Ni metal layer.