A porous zinc electrode, a preparation method thereof and a zinc-air battery comprising the same

By employing a porous zinc electrode and a five-layer air electrode structure in the zinc-air battery, the problems of small zinc sheet contact area and electrolyte leakage in zinc-air batteries are solved, thereby improving the battery's charge capacity and sealing performance and extending battery life.

CN112054161BActive Publication Date: 2024-11-29BEIJING TSINGHUA SOLAR SYST LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202010997125.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-21
Publication Date
2024-11-29
Estimated Expiration
2040-09-21

AI Technical Summary

Technical Problem

Existing zinc-air batteries suffer from problems such as small contact area between zinc sheet and electrolyte, low output current, zinc ion dendrite formation, difficulty in battery sealing, and electrolyte leakage, which affect battery performance and lifespan.

Method used

A porous zinc electrode preparation method is adopted, in which a three-dimensional network structure is formed on the surface of the zinc electrode through electroplating. Combined with a five-layer air electrode design, including a semi-permeable membrane layer, a CO2 adsorption layer, a catalyst layer, a current collection layer and an isolation layer, the pore size and structure are optimized to improve the electrolyte contact area and sealing performance.

Benefits of technology

It increases the charge capacity of the zinc-air battery, enhances the flow and diffusion of the electrolyte, effectively prevents electrolyte leakage, and extends battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112054161B_ABST
    Figure CN112054161B_ABST
Patent Text Reader

Abstract

The present invention provides a porous zinc electrode, a preparation method thereof and a zinc-air battery comprising the same. The preparation method comprises: using a template having a porous structure as a cathode and zinc as an anode, inserting the template into a plating solution containing a ruthenium source, applying a current between the anode and the cathode for electroplating, and depositing a zinc layer on the surface of the template to prepare the porous zinc electrode. The porous zinc electrode provided by the present invention has a three-dimensional network-like porous structure, and has obvious structural advantages compared to conventional porous materials with relatively uniform pore sizes. Using the porous zinc electrode as a metal anode of a zinc-air battery can further increase the charge of the zinc-air battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to a porous zinc electrode, a preparation method thereof and a zinc-air battery comprising the same. Background Art

[0002] With the rapid development of science and technology and the improvement of people's living standards, people's use of battery products has been continuously expanded, and the use of batteries has increased rapidly. At the same time, various new electronic products have become more and more functional, more powerful, and consume more energy, and the requirements for battery varieties and performance are also constantly increasing. However, a large number of lead-acid batteries, lithium-ion batteries and nickel-metal hydride batteries are currently popular in the market, but they either have low specific energy or high prices, which makes it difficult to meet market demand.

[0003] Zinc-air battery is a new type of chemical power source that uses oxygen in the air as the positive active material and metal zinc as the negative active material. Zinc-air battery is a half battery and half fuel cell. First, the negative active material is encapsulated inside the battery like zinc-manganese, lead and other batteries, and has the characteristics of a battery; second, the positive active material comes from the oxygen contained in the air outside the battery, and theoretically has unlimited capacity, which is a typical feature of fuel cells.

[0004] Its advantages are: (1) High specific energy: The specific energy of zinc-air batteries is 4 to 6 times that of lead-acid batteries and 1 time that of lithium-ion batteries. Electric vehicles powered by them can travel up to 400 km, while the same vehicle powered by lead-acid batteries of the same mass generally has a range of no more than 100 km. (2) Simple manufacturing process and low cost: The cost of large quantities is about 300 to 500 yuan / kVAh, which is lower than that of lead-acid batteries. (3) Safe and reliable: Even if there is an open flame, short circuit, puncture, impact, etc., there will be no combustion or explosion. (4) Environmental protection: The positive electrode of the battery uses activated carbon and copper mesh, and the negative electrode uses metallic zinc, without the use of some toxic substances. (5) Recyclable: After the zinc electrode is used up, it can be reused by regeneration and reduction. In addition, the zinc electrode can also be charged mechanically, that is, the used zinc electrode is removed from the battery and placed in a special tank for charging. The zinc-air electrode can be reused many times and can also be made into a directly rechargeable zinc-air battery, referred to as a secondary zinc-air battery. Hunan Fengri Power Electric Co., Ltd. has developed a secondary zinc-air battery with a charging cycle life of more than 100 times. (6) Since the charging of zinc-air batteries mainly involves replacing the plates, the regeneration of the plates can be carried out in a centralized manner. The distribution of plates can be done like a store, without the need to build dedicated charging stations. This not only saves a lot of initial investment, but also brings a lot of convenience to users.

[0005] However, the disadvantages of zinc-air batteries are not obvious, which are as follows: (1) The cost of use is relatively high and the charging process is relatively complicated. Because zinc-air batteries are usually charged mechanically, the zinc electrode must be taken out and charged in a special charging tank. Only professionals can operate it, which brings trouble to use and increases labor costs, resulting in a high added value of actual operating costs. (2) The actual service life is short, only 1 to 2 years. This is not mainly due to the poor electrochemical performance of the battery, but the influence of the battery structure. For example, the battery shell is made of plastic wrapped around the air electrode, not a complete plastic tank, which makes it difficult to seal the battery. Many batteries leak after a certain period of use. Secondly, the zinc-air electrode must be made porous. The porous electrode can absorb oxygen, but it also absorbs some carbon dioxide, causing the electrolyte to carbonate, which greatly reduces the efficiency of the battery. (3) The mass production process is not mature enough. This is mainly due to the manufacture of catalytic membranes and waterproof breathable membranes, which mostly require semi-mechanical operations and some manual factors, resulting in differences in electrode performance. (4) The most difficult problem is the difficulty in sealing the battery. When the zinc-air battery is discharged, it needs a constant supply of oxygen from the air to enter the battery, so the battery is not completely sealed. There are one or more air holes in the battery shell, so the inside and outside of the battery are connected. If the air electrode, especially the waterproof and breathable membrane, is not made well, the battery will easily leak, seriously affecting the performance and quality of the zinc-air battery.

[0006] CN108346844A discloses a metal fuel cell, comprising a plurality of battery cells connected in series in sequence, wherein the battery cells include: a battery housing, an air electrode sheet, a zinc sheet and an electrolyte; the battery housing is a hollow structure, a zinc sheet is arranged inside the battery housing, an air electrode sheet is arranged inside the battery housing, on both sides or one side of the zinc sheet, the side of the air electrode sheet away from the zinc sheet is connected to the outside world, an electrolyte is filled between the air electrode sheet and the zinc sheet, and the air electrode sheet and the zinc sheet are respectively connected to a wire. However, a disadvantage of the zinc sheet material as an anode is that the surface contact area with the electrolyte is small, and the speed at which the zinc sheet generates electrons is low, which affects the output current. Generally, a catalyst of precious metal, liquid metal or other materials is required to increase the output current. Moreover, zinc ions are prone to generate dendrites in an alkaline environment and adhere to the surface of the zinc material, exacerbating the above defects.

[0007] CN208272078U discloses a zinc-air battery, including: a battery shell, a first current collector, a zinc paste, a diaphragm, an air electrode, a positive pole ear, a negative pole ear, a first rivet and a second rivet, the battery shell includes a positive pole shell and a negative pole shell, and a hollow window is arranged on the shell surface of the positive pole shell; the first current collector is arranged on the negative pole shell, the zinc paste is arranged on the first current collector, the diaphragm is arranged on the zinc paste, the air electrode is arranged on the diaphragm, and the positive pole shell is arranged on the air electrode; the first rivet passes through the through hole on the negative pole shell and is connected to the first current collector; the negative pole ear is connected to the nail cap of the first rivet; the second rivet passes through the hollow window and is connected to the air electrode; the positive pole ear is connected to the nail cap of the second rivet. The powdered zinc powder mixed with the electrolyte is in a paste state, which may cause leakage problems.

[0008] CN203721850U discloses a pole piece moving zinc-air battery device, which mainly includes an unwinding mechanism, an anode plate, a transmission mechanism, a cathode plate, a battery tank, a winding mechanism and a box body. The anode plate adopts a sheet structure, including an anode current collector and zinc paste, and the zinc paste is applied to the anode current collector during production; the transmission mechanism is a V-shaped structure, which is composed of a designed number of transmission shafts installed on the bottom surface of the box body; the cathode plate is molded by mold injection molding to form a V-shaped structure corresponding to the transmission mechanism, the lower side of the cathode plate is in contact with the electrolyte in the battery tank, and the waterproof and breathable layer allows the upper side of the cathode plate to directly contact the air, and the positive electrode ear is led out from the carbon plate at the contact surface between the cathode plate and the box cover of the box body to form a positive electrode output end; the battery tank is placed in the center of the transmission mechanism on both sides, and the electrolyte of the electrochemical reaction is contained in the battery tank; the negative electrode ear is led out at one end of the conductive bracket of the winding mechanism to form a negative electrode output end. But obviously, this scheme cannot ensure a high contact area while preventing electrolyte leakage.

[0009] As can be seen from the above, although zinc-air batteries have many advantages, their disadvantages are not obvious. On the one hand, the use of zinc sheets as anodes results in a smaller contact surface with the electrolyte, and the speed at which the zinc sheets generate electrons is low, which affects the output current. Generally, precious metals, liquid metals or other material catalysts are required to increase the output current. In addition, zinc ions are prone to generate dendrites in an alkaline environment and adhere to the surface of the zinc material, exacerbating the above defects. On the other hand, zinc paste is formed by mixing zinc powder and electrolyte as the anode. When the negative electrode of the battery is replaced, the battery cover and the shell are separated and cannot be well sealed. The electrolyte flowing in the battery is prone to leakage, causing a short circuit in the battery, which greatly reduces the battery life. Therefore, it is urgent to redesign the zinc electrode of the existing zinc-air battery to increase the contact area while avoiding electrolyte leakage. Summary of the invention

[0010] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a porous zinc electrode, a preparation method thereof and a zinc-air battery comprising the same. The porous zinc electrode provided by the present invention has a three-dimensional network-like porous structure, which has obvious structural advantages over traditional porous materials with relatively uniform pore sizes. By using it as the metal anode of a zinc-air battery, the charge capacity of the zinc-air battery can be further increased.

[0011] To achieve this object, the present invention adopts the following technical solutions:

[0012] In a first aspect, the present invention provides a method for preparing a porous zinc electrode, the preparation method comprising:

[0013] A template with a porous structure is used as a cathode and zinc is used as an anode, which is inserted into a plating solution containing a ruthenium source. A current is applied between the anode and the cathode for electroplating, and a zinc layer is deposited on the surface of the template to prepare the porous zinc electrode.

[0014] After adding ruthenium source to the electroplating solution, the ruthenium source will also be deposited on the cathode under the action of the electric field to become metallic ruthenium, and metallic ruthenium is a good hydrogen evolution catalyst, so that the precipitation potential of hydrogen on the ruthenium surface is lower than the precipitation potential of zinc, so hydrogen will be continuously precipitated in the place where ruthenium is precipitated, and zinc will continue to be deposited in the place where ruthenium is not deposited, so that after a certain period of electroplating, a zinc film with a three-dimensional porous structure is formed. Compared with traditional porous materials with relatively uniform pore sizes, the zinc electrode provided by the present invention has a larger difference in pore size, and there is a skeleton structure in which large pores and small pores overlap each other, which has obvious structural advantages. As the metal anode of the zinc-air battery, it can further increase the charge of the zinc-air battery.

[0015] As a preferred technical solution of the present invention, the electroplating solution is prepared by the following method:

[0016] The ruthenium source, the zinc source and the electrolyte are added with water and stirred to obtain the electroplating solution after they are completely dissolved.

[0017] Preferably, the ruthenium source comprises ruthenium chloride and / or ruthenium sulfate.

[0018] Preferably, the concentration of ruthenium chloride is 3-5 mg / L, for example, it can be 3.0 mg / L, 3.2 mg / L, 3.4 mg / L, 3.6 mg / L, 3.8 mg / L, 4.0 mg / L, 4.2 mg / L, 4.4 mg / L, 4.6 mg / L, 4.8 mg / L or 5.0 mg / L, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the concentration of ruthenium sulfate is 3-5 mg / L, for example, it can be 3.0 mg / L, 3.2 mg / L, 3.4 mg / L, 3.6 mg / L, 3.8 mg / L, 4.0 mg / L, 4.2 mg / L, 4.4 mg / L, 4.6 mg / L, 4.8 mg / L or 5.0 mg / L, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the ruthenium source includes ruthenium chloride and ruthenium sulfate, and the concentration ratio of ruthenium chloride to ruthenium sulfate is (0.56-0.89):1, for example, it can be 0.56:1, 0.6:1, 0.65:1, 0.7:1, 0.75:1, 0.8:1, 0.85:1 or 0.89:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] The present invention adds a small amount of ruthenium to the electroplating solution to prevent ruthenium from being precipitated on the cathode surface over a large area after excessive ruthenium ions are added, causing hydrogen to be precipitated on the entire cathode surface, making it difficult to obtain a porous structure. A small amount of ruthenium ions are used, which will only be dispersed and deposited on the cathode surface, and hydrogen will be precipitated in the deposited part, and a zinc layer will be deposited in the non-deposited part. In this way, due to the unevenness of the deposition, a porous structure is formed. When the area of ​​the dispersed deposited ruthenium layer is large, more hydrogen is precipitated accordingly, and the corresponding pore size is larger. Conversely, the pore size is smaller, thereby obtaining a network skeleton structure in which large pores and small pores overlap each other. The large pores are conducive to the circulation and diffusion of the electrolyte, and the small pores are conducive to increasing the contact area with the electrolyte. Therefore, compared with the traditional porous material with relatively uniform pore size, it has obvious structural advantages. As a metal anode of a zinc-air battery, the charge of the zinc-air battery can be further increased. At the same time, the study found that by adjusting the composition and concentration ratio of the ruthenium source, the ratio of the number of large pores and small pores can be further controlled. The present invention specifically limits the concentration ratio of ruthenium chloride to ruthenium sulfate to (0.56-0.89):1. Within this range, the ratio of the number of large pores to small pores is relatively balanced, and there will not be too many large pores or too many small pores. If it is below the lower limit of the range, there will be too many small pores. Due to the small number of large pores, the electrolyte cannot better penetrate into the metal anode of the zinc-air battery; conversely, if it is above the upper limit of the range, there will be too many large pores. Due to the lack of small pores, the electrolyte cannot better contact with the metal anode of the zinc-air battery, and the contact area will be affected accordingly.

[0022] Preferably, the zinc source comprises zinc salt and / or zinc oxide.

[0023] Preferably, the concentration of zinc oxide is 25-70 g / L, for example, 25 g / L, 30 g / L, 35 g / L, 40 g / L, 45 g / L, 50 g / L, 55 g / L, 60 g / L, 65 g / L or 70 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] Preferably, the zinc salt comprises zinc sulfate and / or zinc chloride.

[0025] Preferably, the concentration of zinc sulfate is 15-30 g / L, for example, it can be 15 g / L, 16 g / L, 17 g / L, 18 g / L, 19 g / L, 20 g / L, 21 g / L, 22 g / L, 23 g / L, 24 g / L, 25 g / L, 26 g / L, 27 g / L, 28 g / L, 29 g / L or 30 g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0026] Preferably, the concentration of zinc chloride is 25-40 g / L, for example, it can be 25 g / L, 26 g / L, 27 g / L, 28 g / L, 29 g / L, 30 g / L, 31 g / L, 32 g / L, 33 g / L, 34 g / L, 35 g / L, 36 g / L, 37 g / L, 38 g / L, 39 g / L or 40 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the metal salt comprises one or a combination of at least two of iron salt, sodium salt, potassium salt or copper salt.

[0028] Preferably, the iron salt comprises ferrous sulfate and / or ferrous chloride.

[0029] Preferably, the concentration of ferrous sulfate is 20-30 g / L, for example, it can be 20 g / L, 21 g / L, 22 g / L, 23 g / L, 24 g / L, 25 g / L, 26 g / L, 27 g / L, 28 g / L, 29 g / L or 30 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, the concentration of ferrous chloride is 20-30 g / L, for example, 20 g / L, 21 g / L, 22 g / L, 23 g / L, 24 g / L, 25 g / L, 26 g / L, 27 g / L, 28 g / L, 29 g / L or 30 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the sodium salt comprises sodium sulfate and / or sodium chloride.

[0032] Preferably, the concentration of sodium sulfate is 25-35 g / L, for example, it can be 25 g / L, 26 g / L, 27 g / L, 28 g / L, 29 g / L, 30 g / L, 31 g / L, 32 g / L, 33 g / L, 34 g / L or 35 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the concentration of sodium chloride is 25-35 g / L, for example, it can be 25 g / L, 26 g / L, 27 g / L, 28 g / L, 29 g / L, 30 g / L, 31 g / L, 32 g / L, 33 g / L, 34 g / L or 35 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the potassium salt comprises potassium sulfate and / or potassium chloride.

[0035] Preferably, the concentration of potassium sulfate is 15-25 g / L, for example, it can be 15 g / L, 16 g / L, 17 g / L, 18 g / L, 19 g / L, 20 g / L, 21 g / L, 22 g / L, 23 g / L, 24 g / L or 25 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] Preferably, the concentration of potassium chloride is 15-25 g / L, for example, it can be 15 g / L, 16 g / L, 17 g / L, 18 g / L, 19 g / L, 20 g / L, 21 g / L, 22 g / L, 23 g / L, 24 g / L or 25 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] Preferably, the copper salt comprises copper sulfate and / or copper chloride.

[0038] Preferably, the concentration of copper sulfate is 5-20 g / L, for example, it can be 5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L, 10 g / L, 11 g / L, 12 g / L, 13 g / L, 14 g / L, 15 g / L, 16 g / L, 17 g / L, 18 g / L, 19 g / L or 20 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] Preferably, the concentration of cupric chloride is 5 to 20 g / L, for example, 5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L, 10 g / L, 11 g / L, 12 g / L, 13 g / L, 14 g / L, 15 g / L, 16 g / L, 17 g / L, 18 g / L, 19 g / L or 20 g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0040] Preferably, the pH value of the electroplating solution is 2 to 6, for example, 2, 3, 4, 5 or 6, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0041] As a preferred technical solution of the present invention, the template is porous iron with a three-dimensional network structure or porous carbon with a three-dimensional network structure.

[0042] Preferably, the anode and cathode are immersed in a plating solution containing a ruthenium source for a period of time before electroplating.

[0043] Preferably, the soaking time is 5 to 10 minutes, for example, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] As a preferred technical solution of the present invention, the electroplating process adopts a constant current method, a constant voltage method or a pulse method;

[0045] Preferably, the current density of the constant current method is 100-200A / m 2 , for example, it can be 100A / m 2 , 110A / m 2 , 120A / m 2 , 130A / m 2 , 140A / m 2 , 150A / m 2 、160A / m 2 、170A / m 2 、180A / m 2 、190A / m 2 or 200A / m 2 , but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] Preferably, the voltage of the constant voltage method is 0.5-5V, for example, it can be 0.5V, 1V, 1.5V, 2V, 2.5V, 3V, 3.5V, 4V, 4.5V or 5V, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0047] Preferably, the average current density of the pulse method is 100 to 500 A / m 2 , for example, it can be 100A / m 2 , 150A / m 2 , 200A / m 2 , 250A / m 2 、300A / m 2 、350A / m 2 , 400A / m 2 , 450A / m 2 or 500A / m 2 , but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] Preferably, the duty cycle of the pulse method is 10-20%, for example, it can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] Preferably, the electroplating time is 5 to 8 hours, for example, it can be 5.0 hours, 5.5 hours, 6.0 hours, 6.5 hours, 7.0 hours, 7.5 hours or 8.0 hours, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0050] Preferably, the electroplating temperature is 30-50°C, for example, it can be 30°C, 32°C, 34°C, 36°C, 38°C, 40°C, 42°C, 44°C, 46°C, 48°C or 50°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0051] In the present invention, by adjusting the electroplating process parameters and the special ratio of the electroplating solution, the aperture of the macropores and the micropores can be regulated. The present invention needs to specifically limit the current density, electroplating time and electroplating temperature during the electroplating process. Specifically:

[0052] (1) With regard to the current density, when the current density exceeds the upper limit specified in the present application, the hydrogen evolution reaction is too intense, and the generated hydrogen bubbles are larger, thereby causing the pore size of the macropores and the small pores to be too large, and the small pores lose the function of increasing the contact area; on the contrary, when the current density is lower than the specified lower limit, the generated hydrogen is insufficient and the hydrogen bubbles are small, the porosity does not meet the standard, and the pore size of the macropores is too small. In the zinc-air battery, the electrolyte cannot smoothly enter the metal anode;

[0053] (2) Regarding the electroplating time, when the time limit specified in the present application is exceeded, the hydrogen evolution current density will also increase, resulting in an excessively large hydrogen yield, causing the pore size of the macropores and the micropores to be too large, and the micropores lose the function of increasing the contact area. On the contrary, when the time limit is lower than the specified lower limit, the hydrogen evolution current density will be too small, the hydrogen generated will be insufficient, the porosity will not meet the standard, and the macropore size will be too small. In the zinc-air battery, the electrolyte cannot smoothly enter the metal anode.

[0054] (3) Regarding the electroplating temperature, when the temperature exceeds the upper limit specified in the present application, the hydrogen evolution current density will also increase, resulting in an excessively large hydrogen yield and a larger bubble volume, causing the pore size of the large and small pores to be too large, and the small pores lose the function of increasing the contact area. Conversely, when the temperature is lower than the lower limit specified, the hydrogen evolution current density will be too small, the hydrogen generated will be insufficient and the hydrogen bubbles will be small, the porosity will not meet the standard and the pore size of the large pores will be too small. In the zinc-air battery, the electrolyte cannot smoothly enter the metal anode.

[0055] The present invention coordinates the ratio of the electrolyte and the electroplating process to control the number and diameter of macropores and small pores, thereby obtaining a porous zinc electrode with a suitable number and diameter of macropores and small pores, thereby increasing the contact area between the electrolyte and the metal anode while ensuring smooth infiltration of the electrolyte into the metal anode.

[0056] As a preferred technical solution of the present invention, the preparation method further comprises:

[0057] After the electroplating is completed, the template with the zinc layer deposited thereon is rinsed and dried in sequence to obtain the porous zinc electrode.

[0058] Preferably, the cleaning process is carried out under ultrasonic conditions.

[0059] Preferably, the ultrasonic power is 40-50kHz, for example, it can be 40kHz, 41kHz, 42kHz, 43kHz, 44kHz, 45kHz, 46kHz, 47kHz, 48kHz, 49kHz or 50kHz, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0060] Preferably, the cleaning time is 10 to 20 minutes, for example, it can be 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, 15 minutes, 16 minutes, 17 minutes, 18 minutes, 19 minutes or 20 minutes, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0061] Preferably, the drying temperature is 60-70°C, for example, it can be 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C or 70°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0062] Preferably, the drying time is 2 to 4 hours, for example, it can be 2.0 hours, 2.2 hours, 2.4 hours, 2.6 hours, 2.8 hours, 3.0 hours, 3.2 hours, 3.4 hours, 3.6 hours, 3.8 hours or 4.0 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0063] In a second aspect, the present invention provides a porous zinc electrode prepared by the preparation method described in the first aspect, wherein the porous zinc electrode has a three-dimensional network structure.

[0064] As a preferred technical solution of the present invention, the porosity of the porous zinc electrode is 70-80%, for example, it can be 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79% or 80%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0065] Preferably, the pore size of the zinc electrode is 500-2000 μm, for example, it can be 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, 1000 μm, 1100 μm, 1200 μm, 1300 μm, 1400 μm, 1500 μm, 1600 μm, 1700 μm, 1800 μm, 1900 μm or 2000 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0066] In a third aspect, the present invention provides a zinc-air battery, comprising a shell with an open end, a through hole being provided on a side wall of the shell, an air cathode being circumferentially arranged near an inner wall of the shell, an air intake cavity being formed between the air cathode and the shell, and external air entering the air intake cavity through the through hole.

[0067] A metal anode is inserted axially into the central area inside the shell, and an electrolyte is injected into the annular cavity formed between the air cathode and the metal anode. The metal anode is the porous zinc electrode described in the second aspect.

[0068] As a preferred technical solution of the present invention, the air cathode comprises a semi-permeable membrane layer, a CO2 adsorption layer, a catalyst layer, a current collecting layer and an isolation layer which are sequentially stacked from the outside to the inside.

[0069] The zinc-air battery provided by the present invention effectively solves the problem of electrolyte leakage by providing an air electrode with a five-layer structure. Specifically:

[0070] (1) The first layer is a semipermeable membrane layer. The pore size of the semipermeable membrane layer is larger than that of air molecules, so the free flow of air can be guaranteed. At the same time, due to the large surface tension of water and the pore size of the semipermeable membrane layer being smaller than that of water droplets, the electrolyte is blocked from seeping out, and the infiltration of water molecules from the external environment can also be effectively prevented.

[0071] (2) The second layer is a carbon dioxide adsorption layer, which is used to absorb carbon dioxide in the air, effectively avoiding the carbonation of the electrolyte;

[0072] (3) The third layer is the catalyst layer. The catalyst layer is a redox bifunctional catalyst coated on the surface of the current collecting layer. The bifunctional characteristics of the catalyst can carry out oxygen reduction reaction and OH - Oxidation reaction;

[0073] (4) The fourth layer is the current collector layer, which is a profiled thin-walled structure. The profiled thin-walled structure forms multiple parallel air flow channels between the current collector layer and the catalyst layer, greatly increasing the catalytic reaction area and catalytic reaction time between the catalyst and the air, thereby increasing the reaction rate;

[0074] (5) The fifth layer is the isolation layer, which has a certain degree of hydrophobicity, which can further prevent the leakage of electrolyte, while not affecting the air entering the battery to participate in the reaction.

[0075] Preferably, the semipermeable membrane is made of polytetrafluoroethylene membrane, PVDF hydrophobic ultrafiltration membrane or polyester breathable membrane.

[0076] Preferably, the pore size of the semipermeable membrane layer is 0.01-0.1 nm, for example, it can be 0.01 nm, 0.02 nm, 0.03 nm, 0.04 nm, 0.05 nm, 0.06 nm, 0.07 nm, 0.08 nm, 0.09 nm or 0.1 nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0077] Preferably, the CO2 adsorption layer is made of porous carbon material.

[0078] Preferably, the pore size of the porous carbon material is 0.2 to 200 nm, for example, it can be 0.2 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm or 200 nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0079] Preferably, the current collecting layer is a special-shaped thin-walled structure.

[0080] Preferably, the contact area between the current collecting layer and the catalyst layer is 30-40%, for example, it can be 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% or 40%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0081] Preferably, the current collecting layer is a curved sheet structure, a wavy curved surface structure, a continuous concave-convex structure or a sawtooth special-shaped structure.

[0082] Preferably, the material of the current collecting layer is foamed nickel, foamed copper or foamed stainless steel.

[0083] Preferably, the pore size of the current collecting layer is 1 to 10 μm, for example, it can be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0084] Preferably, the material of the isolation layer is polypropylene, polyethylene or polyvinyl chloride.

[0085] Preferably, the pore size of the isolation layer is 0.1 to 100 nm, for example, it can be 0.1 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0086] As a preferred technical solution of the present invention, a fixing part is arranged in the air intake cavity, and the fixing part is used to support and fix the air anode.

[0087] Preferably, the fixing member is a spring, and two ends of the spring are respectively fixed to the inner wall of the shell and the outer wall of the semipermeable membrane layer.

[0088] Preferably, the zinc-air battery further comprises an end cover located at the opening of the shell, and the end cover is used to seal the opening of the shell.

[0089] Preferably, an annular groove is provided on the inner surface of the end cover, and the annular groove is used to fix the air cathode. The annular groove is opposite to the annular end surface of the air cathode, and one end of the air cathode close to the opening of the shell is inserted into the annular groove.

[0090] The present invention fixes the air cathode by arranging a spring and an annular groove, wherein the spring mainly plays a protective role and is used to support the air cathode in the radial direction, and has a buffering effect on the air cathode when it is hit by the outside or subjected to external forces during transportation; the annular groove plays a more fixing role and is used to fix the air cathode in the axial direction to prevent the displacement of the air cathode and cause leakage of the electrolyte.

[0091] Compared with the prior art, the present invention has the following beneficial effects:

[0092] (1) The porous zinc electrode provided by the present invention has a three-dimensional network-like porous structure, which is composed of large pores and small pores that overlap each other. The large pores are conducive to the circulation and diffusion of the electrolyte, and the small pores are conducive to increasing the contact area with the electrolyte. Therefore, compared with traditional porous materials with relatively uniform pore sizes, it has obvious structural advantages. Using it as the metal anode of the zinc-air battery can further increase the charge capacity of the zinc-air battery.

[0093] (2) The present invention coordinately regulates the number and diameter of macropores and small pores by adjusting the electrolyte ratio and the electroplating process, thereby obtaining a porous zinc electrode with a suitable number and diameter of macropores and small pores, thereby increasing the contact area between the electrolyte and the metal anode while ensuring smooth infiltration of the electrolyte into the metal anode.

[0094] (3) The zinc-air battery provided by the present invention effectively solves the problem of electrolyte leakage by setting up a five-layer air electrode. The pore size of the semipermeable membrane layer is larger than that of air molecules, so the free flow of air can be guaranteed. At the same time, due to the large surface tension of water and the pore size of the semipermeable membrane layer being smaller than that of water droplets, the electrolyte is blocked from seeping out, and the infiltration of water molecules from the external environment can also be effectively prevented. The carbon dioxide adsorption layer is used to absorb carbon dioxide in the air, effectively avoiding the carbonation of the electrolyte. The collector layer with a special-shaped thin-wall structure is adopted, so that a plurality of parallel air flow channels are formed between the collector layer and the catalyst layer, which greatly increases the catalytic reaction area and catalytic reaction time of the catalyst and the air, and increases the reaction rate. Finally, the isolation layer with a certain hydrophobicity is used to further prevent the seepage of the liquid, and at the same time, it does not affect the air entering the battery to participate in the reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0095] Figure 1A schematic diagram of the structure of a zinc-air battery provided in one embodiment of the present invention;

[0096] Among them, 1-housing; 2-air cathode; 21-semipermeable membrane layer; 22-CO2 adsorption layer; 23-catalyst layer; 24-current collecting layer; 25-isolation layer; 3-air inlet cavity; 4-metal anode; 5-electrolyte; 6-end cover; 7-spring. DETAILED DESCRIPTION

[0097] It should be understood that, in the description of the present invention, the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0098] It should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "disposed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.

[0099] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0100] In a specific embodiment, the present invention provides a method for preparing a porous zinc electrode, the preparation method comprising:

[0101] (1) preparing an electroplating solution: adding water to a ruthenium source, a zinc source, an electrolyte and an additive, stirring, and obtaining an electroplating solution after the ruthenium source, a zinc source and an electrolyte and an additive are completely dissolved;

[0102] (2) using a template having a three-dimensional network structure as a cathode and zinc as an anode, inserting it into a plating solution containing a ruthenium source and immersing it for 5 to 10 minutes, then applying a current between the anode and the cathode, and performing electroplating by a constant current method, a constant voltage method or a pulse method;

[0103] (3) Post-treatment: The template with the zinc layer deposited is rinsed and dried in sequence to obtain a porous zinc electrode.

[0104] The porous zinc electrode prepared by the preparation method has a three-dimensional network structure, a porosity of 70-80%, and a pore size of 500-2000 μm.

[0105] In another specific embodiment, the present invention provides a zinc-air battery, wherein the zinc-air battery is Figure 1 As shown, it includes a shell 1 with an open end, a through hole is opened in the side wall of the shell 1, an air cathode 2 is circumferentially arranged near the inner wall of the shell 1, and an air intake cavity 3 is formed between the air cathode 2 and the shell 1, and the outside air enters the air intake cavity 3 through the through hole. A metal anode 4 is inserted axially into the central area inside the shell 1, and an electrolyte 5 is injected into the annular cavity formed between the air cathode 2 and the metal anode 4.

[0106] The air cathode 2 includes a semipermeable membrane layer 21, a CO2 adsorption layer 22, a catalyst layer 23, a current collecting layer 24 and a separation layer 25 which are stacked in sequence from the outside to the inside. Furthermore, the semipermeable membrane is made of a polytetrafluoroethylene membrane, a PVDF hydrophobic ultrafiltration membrane or a polyester breathable membrane, and the pore size of the semipermeable membrane layer 21 is 0.01 to 0.1 nm. The CO2 adsorption layer 22 is made of a porous carbon material, and the pore size of the porous carbon material is 0.2 to 200 nm. The current collecting layer 24 is a profiled thin-walled structure, and the contact area between the current collecting layer 24 and the catalyst layer 23 is 30 to 40%. Specifically, the current collecting layer 24 is a curved sheet structure, a wavy curved surface structure, a continuous concave-convex structure or a sawtooth profiled structure. The material of the current collecting layer 24 is foamed nickel, foamed copper, or foamed stainless steel, and the pore size of the current collecting layer 24 is 1 to 10 μm. The material of the isolation layer 25 is polypropylene, polyethylene or polyvinyl chloride, and the pore size of the isolation layer 25 is 0.1-100 nm.

[0107] A fixing member is provided in the air inlet cavity 3, and the fixing member is used to support and fix the air anode. Specifically, the fixing member is a spring 7, and two ends of the spring 7 are respectively fixed to the inner wall of the housing 1 and the outer wall of the semi-permeable membrane layer 21.

[0108] The zinc-air battery further includes an end cap 6 located at the opening of the shell 1, and the end cap 6 is used to block the opening of the shell 1. An annular groove is provided on the inner surface of the end cap 6, and the annular groove is used to fix the air cathode 2. The annular groove is opposite to the annular end surface of the air cathode 2, and one end of the air cathode 2 close to the opening of the shell 1 is inserted into the annular groove.

[0109] Example 1

[0110] This embodiment provides a method for preparing a porous zinc electrode, the preparation method comprising:

[0111] (1) Preparation of electroplating solution: Add water to ruthenium source, zinc source, electrolyte and additives, stir and completely dissolve to obtain electroplating solution. The ruthenium source is ruthenium chloride, and the concentration of ruthenium chloride is 4.8 mg / L. The zinc source is zinc oxide, and the concentration of zinc oxide is 50 g / L. The electrolytes are ferrous sulfate, sodium sulfate, sodium chloride, potassium chloride and cupric chloride, and the concentration of ferrous sulfate is 20 g / L, the concentration of sodium sulfate is 35 g / L, the concentration of sodium chloride is 25 g / L, the concentration of potassium chloride is 20 g / L, and the concentration of cupric chloride is 15 g / L. The pH of the electroplating solution is 2.

[0112] (2) Using porous iron with a three-dimensional network structure as the cathode and zinc as the anode, the samples were immersed in a plating solution containing a ruthenium source for 5 minutes, and then a current was applied between the anode and the cathode. The constant current method was used for electroplating. The current density of the constant current method was 130 A / m 2 , electroplating at 30°C for 8h, a zinc layer is deposited on the porous iron surface;

[0113] (3) Post-treatment: The porous iron with the zinc layer deposited thereon was rinsed and dried in sequence to obtain a porous zinc electrode, wherein the cleaning process was carried out under 40kHz ultrasonic conditions for 20 minutes, the drying temperature was 60°C, and the drying time was 4 hours. The prepared porous zinc electrode had a three-dimensional network structure, and most of the pores were large, and there were basically no small pores, the porosity was 79.8%, and the average pore size was 1980 μm.

[0114] This embodiment also provides a zinc-air battery, wherein the metal anode 4 in the zinc-air battery is the zinc electrode prepared as described above, and the basic structure of the zinc-air battery is the same as that of the zinc-air battery provided in the specific embodiment, wherein the specific definition of the material, pore size and structure of each layer in the air cathode 2 is as follows:

[0115] The semi-permeable membrane layer 21 is made of polytetrafluoroethylene membrane with a pore size of 0.01 nm;

[0116] The pore size of the CO2 adsorption layer 22 is 0.2 nm;

[0117] The current collector layer has a wavy curved surface structure, and the contact area with the catalyst layer 23 is 32%; the material of the current collector layer 24 is nickel foam, and the pore size is 1 μm;

[0118] The material of the isolation layer 25 is polypropylene, and the pore size is 0.1 nm.

[0119] Example 2

[0120] This embodiment provides a method for preparing a porous zinc electrode, the preparation method comprising:

[0121] (1) Preparation of electroplating solution: Add water to ruthenium source, zinc source, electrolyte and additives, stir and completely dissolve to obtain electroplating solution. The ruthenium source is ruthenium sulfate, and the concentration of ruthenium sulfate is 4.8 mg / L. The zinc source includes zinc oxide and zinc sulfate, and the concentration of zinc oxide is 25 g / L and the concentration of zinc sulfate is 30 g / L.

[0122] The electrolyte is ferrous chloride, sodium chloride, potassium sulfate, copper sulfate and cupric chloride. The concentration of ferrous chloride is 30g / L, the concentration of sodium chloride is 30g / L, the concentration of potassium sulfate is 18g / L, the concentration of copper sulfate is 16g / L, and the concentration of cupric chloride is 5g / L. The pH of the plating solution is 3;

[0123] (2) Using porous carbon with a three-dimensional network structure as the cathode and zinc as the anode, the porous carbon was immersed in a plating solution containing a ruthenium source for 6 minutes, and then a current was applied between the anode and the cathode. The constant voltage method was used for electroplating. The voltage of the constant voltage method was 1V. The electroplating was performed at 35°C for 7 hours, and a zinc layer was deposited on the surface of the porous carbon.

[0124] (3) Post-treatment: The porous carbon with the zinc layer deposited thereon was rinsed and dried in sequence to obtain a porous zinc electrode, wherein the cleaning process was carried out under 43kHz ultrasonic conditions for 16 minutes, the drying temperature was 63°C, and the drying time was 3.5 hours. The prepared porous zinc electrode had a three-dimensional network structure, and most of the pores were small, and there were basically no large pores, the porosity was 72.3%, and the average pore size was 506 μm.

[0125] This embodiment also provides a zinc-air battery, wherein the metal anode 4 in the zinc-air battery is the zinc electrode prepared as described above, and the basic structure of the zinc-air battery is the same as that of the zinc-air battery provided in the specific embodiment, wherein the specific definition of the material, pore size and structure of each layer in the air cathode 2 is as follows:

[0126] The semi-permeable membrane layer 21 is made of PVDF hydrophobic ultrafiltration membrane with a pore size of 0.03 nm;

[0127] The pore size of the CO2 adsorption layer 22 is 50 nm;

[0128] The current collector layer is a curved sheet structure, and the contact area with the catalyst layer 23 is 35%;

[0129] The material of the current collecting layer 24 is copper foam, and the pore size is 3 μm;

[0130] The material of the isolation layer 25 is polyethylene, and the pore size is 10 nm.

[0131] Example 3

[0132] This embodiment provides a method for preparing a porous zinc electrode, the preparation method comprising:

[0133] (1) Prepare the electroplating solution: add water to the ruthenium source, zinc source, electrolyte and additives, stir and obtain the electroplating solution after they are completely dissolved. The ruthenium sources are ruthenium chloride and ruthenium sulfate, the concentration of ruthenium chloride is 2.8 mg / L, and the concentration of ruthenium sulfate is 4 mg / L. The zinc sources include zinc oxide and zinc chloride, the concentration of zinc oxide is 70 g / L, and the concentration of zinc chloride is 25 g / L. The electrolytes are ferrous chloride, potassium sulfate, potassium chloride, copper sulfate and cupric chloride, the concentration of ferrous chloride is 30 g / L, the concentration of potassium sulfate is 20 g / L, the concentration of potassium chloride is 20 g / L, the concentration of copper sulfate is 5 g / L, and the concentration of copper chloride is 18 g / L. The pH of the electroplating solution is 4;

[0134] (2) Using porous iron with a three-dimensional network structure as the cathode and zinc as the anode, the samples were immersed in a plating solution containing a ruthenium source for 8 minutes, and then a current was applied between the anode and the cathode. The electroplating was performed using a pulse method. The average current density of the pulse method was 300 A / m 2 , the duty cycle of the pulse method was 18%, and the zinc layer was deposited on the porous iron surface after electroplating at 40°C for 6h;

[0135] (3) Post-treatment: The porous iron with the zinc layer deposited thereon was rinsed and dried in sequence to obtain a porous zinc electrode, wherein the cleaning process was carried out under 45kHz ultrasonic conditions for 15 minutes, the drying temperature was 65°C, and the drying time was 3 hours. The prepared porous zinc electrode had a three-dimensional network structure and had both large pores and small pores, the ratio of large pores to small pores was 1:1, the porosity was 76.5%, the average pore size of the large pores was 1850μm, and the average pore size of the small pores was 680μm.

[0136] This embodiment also provides a zinc-air battery, wherein the metal anode 4 in the zinc-air battery is the zinc electrode prepared as described above, and the basic structure of the zinc-air battery is the same as that of the zinc-air battery provided in the specific embodiment, wherein the specific definition of the material, pore size and structure of each layer in the air cathode 2 is as follows:

[0137] The semi-permeable membrane layer 21 is made of a polyester breathable membrane with a pore size of 0.05 nm;

[0138] The pore size of the CO2 adsorption layer 22 is 100 nm;

[0139] The current collector layer has a continuous concave-convex structure, and the contact area with the catalyst layer 23 is 35%;

[0140] The material of the current collecting layer 24 is foam stainless steel, and the pore size is 5 μm;

[0141] The material of the isolation layer 25 is polyvinyl chloride, and the pore size is 50 nm.

[0142] Example 4

[0143] This embodiment provides a method for preparing a porous zinc electrode, the preparation method comprising:

[0144] (1) Prepare electroplating solution: Add water to ruthenium source, zinc source, electrolyte and additives, stir and obtain electroplating solution after complete dissolution. Among them, the ruthenium source is ruthenium chloride and ruthenium sulfate, the concentration of ruthenium chloride is 2.52 mg / L, and the concentration of ruthenium sulfate is 4.5 mg / L. The zinc source is zinc chloride, and the concentration of zinc chloride is 40 g / L. The electrolytes are ferrous sulfate, ferrous chloride, potassium chloride, cupric sulfate and cupric chloride, the concentration of ferrous sulfate is 20 g / L, the concentration of ferrous chloride is 30 g / L, the concentration of potassium chloride is 15 g / L, the concentration of cupric sulfate is 5 g / L, and the concentration of cupric chloride is 20 g / L. The pH of the electroplating solution is 5;

[0145] (2) Using porous carbon with a three-dimensional network structure as the cathode and zinc as the anode, the samples were immersed in a plating solution containing a ruthenium source for 7 minutes, and then a current was applied between the anode and the cathode. The constant current method was used for electroplating. The current density of the constant current method was 170 A / m 2 , electroplating at 45 °C for 6 h, a zinc layer was deposited on the porous carbon surface;

[0146] (3) Post-treatment: The porous carbon with the zinc layer deposited thereon was rinsed and dried in sequence to obtain a porous zinc electrode, wherein the cleaning process was carried out under ultrasonic conditions of 47 kHz for 13 min, the drying temperature was 67°C, and the drying time was 3.5 h. The prepared porous zinc electrode had a three-dimensional network structure and had both large pores and small pores, the ratio of large pores to small pores was 1:1.3, the porosity was 75.8%, the average pore size of the large pores was 1780 μm, and the average pore size of the small pores was 750 μm.

[0147] This embodiment also provides a zinc-air battery, wherein the metal anode 4 in the zinc-air battery is the zinc electrode prepared as described above, and the basic structure of the zinc-air battery is the same as that of the zinc-air battery provided in the specific embodiment, wherein the specific definition of the material, pore size and structure of each layer in the air cathode 2 is as follows:

[0148] The semi-permeable membrane layer 21 is made of polytetrafluoroethylene membrane with a pore size of 0.07 nm;

[0149] The pore size of the CO2 adsorption layer 22 is 150 nm;

[0150] The current collector layer has a sawtooth-shaped structure, and the contact area with the catalyst layer 23 is 37%;

[0151] The material of the current collecting layer 24 is nickel foam, and the pore size is 6 μm;

[0152] The material of the isolation layer 25 is polypropylene, and the pore size is 70 nm.

[0153] Example 5

[0154] This embodiment provides a method for preparing a porous zinc electrode, the preparation method comprising:

[0155] (1) Prepare electroplating solution: Add water to ruthenium source, zinc source, electrolyte and additives, stir and obtain electroplating solution after complete dissolution. Among them, the ruthenium source is ruthenium chloride and ruthenium sulfate, the concentration of ruthenium chloride is 2.67 mg / L, and the concentration of ruthenium sulfate is 3 mg / L. The zinc source is zinc sulfate and zinc chloride, the concentration of zinc sulfate is 15 g / L, and the concentration of zinc chloride is 30 g / L. The electrolyte is sodium chloride, potassium sulfate, potassium chloride, copper sulfate and copper chloride, the concentration of sodium chloride is 25 g / L, the concentration of potassium sulfate is 15 g / L, the concentration of potassium chloride is 25 g / L, the concentration of copper sulfate is 10 g / L, and the concentration of copper chloride is 10 g / L. The pH of the electroplating solution is 6;

[0156] (2) Using porous iron with a three-dimensional network structure as the cathode and zinc as the anode, the porous iron was immersed in a plating solution containing a ruthenium source for 10 minutes, and then a current was applied between the anode and the cathode. The constant voltage method was used for electroplating. The voltage of the constant voltage method was 3V. The electroplating was performed at 50°C for 5 hours, and a zinc layer was deposited on the surface of the porous iron.

[0157] (3) Post-treatment: The porous iron with the zinc layer deposited thereon was rinsed and dried in sequence to obtain a porous zinc electrode, wherein the cleaning process was carried out under 50kHz ultrasonic conditions for 10 minutes, the drying temperature was 70°C, and the drying time was 2 hours. The prepared porous zinc electrode had a three-dimensional network structure and had both large pores and small pores, the ratio of large pores to small pores was 1.2:1, the porosity was 76.3%, the average pore size of the large pores was 1860μm, and the average pore size of the small pores was 730μm.

[0158] This embodiment also provides a zinc-air battery, wherein the metal anode 4 in the zinc-air battery is the zinc electrode prepared as described above, and the basic structure of the zinc-air battery is the same as that of the zinc-air battery provided in the specific embodiment, wherein the specific definition of the material, pore size and structure of each layer in the air cathode 2 is as follows:

[0159] The semi-permeable membrane layer 21 is made of a polyester breathable membrane with a pore size of 0.1 nm;

[0160] The pore size of the CO2 adsorption layer 22 is 200 nm;

[0161] The current collector layer has a wavy curved surface structure, and the contact area with the catalyst layer 23 is 38%;

[0162] The material of the current collecting layer 24 is copper foam, and the pore size is 10 μm;

[0163] The material of the isolation layer 25 is polypropylene, and the pore size is 100 nm.

[0164] The discharge mass specific capacity of the zinc-air batteries prepared in Examples 1-5 was tested, and the specific testing method was as follows:

[0165] The discharge test was carried out at a constant current density of 1.5A, and the cut-off voltage was set to 0.8V. The discharge mass specific capacity is shown in Table 1.

[0166] The anti-leakage performance of the zinc-air batteries prepared in Examples 1-5 under extreme conditions was tested, and the specific testing method was as follows:

[0167] 50 zinc-air batteries were prepared and placed in a high temperature and high humidity environment of 60°C and 90%RH for 5 weeks. The batteries were observed one by one with the naked eye to see if any leakage occurred. The test results are shown in Table 1.

[0168] Table 1

[0169] Example Discharge mass specific capacity mAh / g Leakage Example 1 273.8 No leakage Example 2 286.4 No leakage Example 3 305.6 No leakage Example 4 302.8 No leakage Example 5 295.2 No leakage

[0170] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a porous zinc electrode, characterized in that: The preparation method comprises: A template with a porous structure is used as a cathode and zinc is used as an anode, which are inserted into an electroplating solution containing a ruthenium source, and a current is applied between the anode and the cathode for electroplating, and a zinc layer is deposited on the surface of the template to prepare the porous zinc electrode; The ruthenium source comprises ruthenium chloride and ruthenium sulfate, and the concentration ratio of ruthenium chloride to ruthenium sulfate is (0.56-0.89):1; The concentration of ruthenium chloride is 3-5 mg / L; The concentration of ruthenium sulfate is 3-5 mg / L.

2. The preparation method according to claim 1, characterized in that: The electroplating solution is prepared by the following method: Add water to the ruthenium source, the zinc source and the electrolyte and stir until they are completely dissolved to obtain the electroplating solution.

3. The preparation method according to claim 2, characterized in that: The zinc source includes zinc salt and / or zinc oxide.

4. The preparation method according to claim 3, characterized in that: The concentration of the zinc oxide is 25-70 g / L.

5. The preparation method according to claim 3, characterized in that: The zinc salt includes zinc sulfate and / or zinc chloride.

6. The preparation method according to claim 5, characterized in that: The concentration of the zinc sulfate is 15-30 g / L.

7. The preparation method according to claim 5, characterized in that: The concentration of the zinc chloride is 25-40 g / L.

8. The preparation method according to claim 2, characterized in that: The electrolyte includes a metal salt.

9. The preparation method according to claim 8, characterized in that: The metal salt includes one or a combination of at least two of iron salt, sodium salt, potassium salt or copper salt.

10. The preparation method according to claim 9, characterized in that: The iron salt includes ferrous sulfate and / or ferrous chloride.

11. The preparation method according to claim 10, characterized in that: The concentration of the ferrous sulfate is 20-30 g / L.

12. The preparation method according to claim 10, characterized in that: The concentration of the ferrous chloride is 20-30 g / L.

13. The preparation method according to claim 9, characterized in that: The sodium salt includes sodium sulfate and / or sodium chloride.

14. The preparation method according to claim 13, characterized in that: The concentration of the sodium sulfate is 25-35 g / L.

15. The preparation method according to claim 13, characterized in that: The concentration of the sodium chloride is 25-35 g / L.

16. The preparation method according to claim 9, characterized in that: The potassium salt includes potassium sulfate and / or potassium chloride.

17. The preparation method according to claim 16, characterized in that: The concentration of potassium sulfate is 15-25 g / L.

18. The preparation method according to claim 16, characterized in that: The concentration of potassium chloride is 15-25 g / L.

19. The preparation method according to claim 9, characterized in that: The copper salt includes copper sulfate and / or copper chloride.

20. The preparation method according to claim 19, characterized in that: The concentration of the copper sulfate is 5-20 g / L.

21. The preparation method according to claim 19, characterized in that: The concentration of the cupric chloride is 5-20 g / L.

22. The preparation method according to claim 1, characterized in that: The pH of the electroplating solution is 2-6.

23. The preparation method according to claim 1, characterized in that: The template is porous iron with a three-dimensional network structure or porous carbon with a three-dimensional network structure.

24. The preparation method according to claim 1, characterized in that: The anode and cathode are inserted into the electroplating solution containing the ruthenium source and immersed for a period of time before electroplating.

25. The preparation method according to claim 24, characterized in that: The soaking time is 5 to 10 minutes.

26. The preparation method according to claim 1, characterized in that: The electroplating process adopts a constant current method, a constant voltage method or a pulse method.

27. The preparation method according to claim 26, characterized in that: The current density of the constant current method is 100~200A / m 2 .

28. The preparation method according to claim 26, characterized in that: The voltage of the constant voltage method is 0.5~5V.

29. The preparation method according to claim 26, characterized in that: The average current density of the pulse method is 100~500A / m 2 .

30. The preparation method according to claim 26, characterized in that: The duty cycle of the pulse method is 10-20%.

31. The preparation method according to claim 26, characterized in that: The electroplating time is 5 to 8 hours.

32. The preparation method according to claim 26, characterized in that: The electroplating temperature is 30-50°C.

33. The preparation method according to claim 1, characterized in that: The preparation method further comprises: After the electroplating is completed, the template with the zinc layer deposited thereon is rinsed and dried in sequence to obtain the porous zinc electrode.

34. The preparation method according to claim 33, characterized in that: The flushing process is carried out under ultrasonic conditions.

35. The preparation method according to claim 34, characterized in that: The ultrasonic power is 40-50kHz.

36. The preparation method according to claim 33, characterized in that: The flushing time is 10 to 20 minutes.

37. The preparation method according to claim 33, characterized in that: The drying temperature is 60-70°C.

38. The preparation method according to claim 33, characterized in that: The drying time is 2 to 4 hours.

39. A porous zinc electrode prepared by the preparation method according to any one of claims 1 to 38, characterized in that: The porous zinc electrode has a three-dimensional network structure.

40. The porous zinc electrode according to claim 39, characterized in that The porosity of the porous zinc electrode is 70-80%.

41. The porous zinc electrode according to claim 39, characterized in that The pore size of the zinc electrode is 500-2000 μm.

42. A zinc-air battery, characterized in that: The zinc-air battery comprises a shell with an open end, a through hole is provided on the side wall of the shell, an air cathode is circumferentially arranged near the inner wall of the shell, an air intake cavity is formed between the air cathode and the shell, and external air enters the air intake cavity through the through hole; A metal anode is inserted axially into the central area inside the shell, and an electrolyte is injected into the annular cavity formed between the air cathode and the metal anode. The metal anode is the porous zinc electrode described in any one of claims 39-41.

43. The zinc-air battery according to claim 42, characterized in that The air cathode comprises a semi-permeable membrane layer, a CO2 adsorption layer, a catalyst layer, a current collecting layer and an isolation layer which are sequentially stacked from the outside to the inside.

44. The zinc-air battery according to claim 43, characterized in that The semipermeable membrane is made of polytetrafluoroethylene membrane, PVDF hydrophobic ultrafiltration membrane or polyester breathable membrane.

45. The zinc-air battery according to claim 43, characterized in that The pore size of the semi-permeable membrane layer is 0.01-0.1 nm.

46. ​​The zinc-air battery according to claim 43, characterized in that The material of the CO2 adsorption layer is porous carbon material.

47. The zinc-air battery according to claim 46, characterized in that The pore size of the porous carbon material is 0.2-200 nm.

48. The zinc-air battery according to claim 43, characterized in that The current collecting layer is a special-shaped thin-wall structure.

49. The zinc-air battery according to claim 43, characterized in that The contact area between the current collecting layer and the catalyst layer is 30-40%.

50. The zinc-air battery according to claim 43, characterized in that The current collecting layer is a curved sheet structure, a wavy curved surface structure, a continuous concave-convex structure or a sawtooth special-shaped structure.

51. The zinc-air battery according to claim 43, characterized in that The material of the current collecting layer is foam nickel, foam copper or foam stainless steel.

52. The zinc-air battery according to claim 43, characterized in that The pore size of the current collecting layer is 1-10 μm.

53. The zinc-air battery according to claim 43, characterized in that The material of the isolation layer is polypropylene, polyethylene or polyvinyl chloride.

54. The zinc-air battery according to claim 43, characterized in that The pore size of the isolation layer is 0.1-100 nm.

55. The zinc-air battery according to claim 42, characterized in that A fixing piece is arranged in the air intake cavity, and the fixing piece is used to support and fix the air anode.

56. The zinc-air battery according to claim 55, characterized in that The fixing member is a spring, and two ends of the spring are respectively fixed to the inner wall of the shell and the outer wall of the semi-permeable membrane layer.

57. The zinc-air battery according to claim 42, characterized in that The zinc-air battery further comprises an end cover located at the opening of the shell, and the end cover is used for sealing the opening of the shell.

58. The zinc-air battery according to claim 57, characterized in that The inner surface of the end cover is provided with an annular groove for fixing the air cathode. The annular groove is opposite to the annular end surface of the air cathode, and one end of the air cathode close to the opening of the shell is inserted into the annular groove.

Citation Information

Patent Citations

  • Metal fuel battery

    CN108346844A

  • Pole piece motion type zinc air battery device

    CN203721850U

  • Empty battery of zinc

    CN208272078U

  • Aluminum-air battery with liquid leakage prevention and environment self-testing

    CN104332675A

  • Air electrode of zinc-air battery

    CN104518223A