Preparation method of fluorine-modified nickel oxide / tin oxide composite sensor device and its product and application

Fluorine-modified nickel oxide/tin oxide composite sensor devices were prepared by hydrothermal and template methods, which solved the problems of insufficient selectivity and sensitivity of existing formaldehyde oxide gas sensors and achieved high-sensitivity detection of formaldehyde with a detection limit of 0.3-0.5 ppm.

CN112098463BActive Publication Date: 2024-10-22SHANGHAI NAT ENG RES CENT FORNANOTECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010837422.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-19
Publication Date
2024-10-22
Estimated Expiration
2040-08-19

AI Technical Summary

Technical Problem

Existing formaldehyde oxide gas sensors lack selectivity and sensitivity, and their recovery-response characteristics need improvement. There is an urgent need to develop adsorbents with stronger formaldehyde adsorption capacity to enhance sensor performance.

Method used

Hollow nickel oxide/tin oxide composite spherical particles were prepared using a hydrothermal method and a template method. These particles were then mixed with fluorine-containing organic compounds to form a fluorine-containing composite at high temperature. The metastable carbon-fluorine bond formed by fluorine and carbon in formaldehyde was utilized to improve the detection sensitivity of formaldehyde.

Benefits of technology

By preparing fluorine-modified nickel oxide/tin oxide composite sensor devices, the detection sensitivity for formaldehyde was significantly improved, with a detection limit of 0.3-0.5 ppm. The preparation process was simplified and no complex post-processing was required.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112098463B_ABST
    Figure CN112098463B_ABST
Patent Text Reader

Abstract

The present invention discloses a preparation method of a fluorine-modified nickel oxide / tin oxide composite sensor device, its product and application. First, hollow composite spherical particles are prepared by hydrothermal method and template method, and then mixed with fluorine organic matter. At high temperature, the released fluorine free radicals react with the matrix to form a fluorine-containing composite. Fluorine and carbon in formaldehyde easily form metastable carbon-fluorine bonds, which greatly improves the sensitivity of formaldehyde detection. The present invention has the advantages of simple preparation method, low reaction temperature, and fluorine-containing microporous hollow spheres can be obtained without complicated subsequent treatment conditions. The composite powder prepared by the invention can be used for the detection of formaldehyde gas in the air.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of inorganic non-metallic materials, and specifically relates to a preparation method of a fluorine-modified nickel oxide / tin oxide composite sensor device, a product and an application thereof, and a method for improving the sensitivity of formaldehyde testing. Background Art

[0002] There are many studies on formaldehyde oxide gas sensors, and their sensitivity and recovery-response characteristics have reached a certain level, but their selectivity is not high. The composite doping method can be used to improve their selectivity. In addition, the proper use of the resistance-temperature characteristics of the sensor can improve the selectivity of the formaldehyde gas oxide sensor. Surface bonding modification, reducing material particles, increasing specific surface area and improving the preparation process of gas-sensitive materials can improve the quality of gas-sensitive materials, which can further improve the sensitivity and response-recovery characteristics of gas-sensitive elements. The selectivity and sensitivity of formaldehyde gas sensors need further research, and the recovery-response characteristics also need to be further improved. It is urgent to develop new adsorbents with stronger formaldehyde adsorption capacity to improve the performance of the sensor. Summary of the invention

[0003] In order to overcome the deficiencies of the prior art, the present invention aims to provide a method for preparing a fluorine-modified nickel oxide / tin oxide composite sensor device.

[0004] Another object of the present invention is to provide a fluorine-modified nickel oxide / tin oxide composite sensor device product prepared by the above method.

[0005] Another object of the present invention is to provide an application of the above product.

[0006] The object of the present invention is achieved by the following scheme: a method for preparing a fluorine-modified nickel oxide / tin oxide composite sensor device, characterized in that hollow composite spherical particles are first prepared by a hydrothermal method and a template method, and then mixed with a fluorine organic matter, and at a high temperature, the released fluorine free radicals react with the matrix to form a fluorine-containing composite, and the fluorine and carbon in formaldehyde easily form a metastable carbon-fluorine bond, which greatly improves the sensitivity of formaldehyde detection, and comprises the following steps:

[0007] (1) dissolving an organic template in an organic solvent, and adding nickel and tin precursors and a precipitant hexamethylenetetramine after the organic template is completely dissolved, wherein the molar ratio of the nickel precursor, the tin precursor, the organic template and the organic solvent is (0.1-0.3):(0.1-0.3):(0.05-0.2):(2-4), and stirring at room temperature for 4 hours to obtain a precursor solution;

[0008] (2) placing the precursor solution in a reaction vessel and reacting at 100° C.-200° C. for 20-48 hours;

[0009] (3) The temperature of the reactor was lowered to room temperature, and the suspension was centrifugally washed with alcohol and water for 8-10 times respectively. After drying in an oven at 80° C. for 24 hours, the suspension was placed in a muffle furnace and calcined at 400-800° C. for 5 hours to obtain microporous hollow nickel oxide / tin oxide balls. The microporous hollow balls were placed in alcohol or water for standby use;

[0010] (4) Grind and mix the composite powder and the fluorine-containing organic matter, put them into a corundum crucible, heat them to 400°C in an atmosphere furnace for 2 hours, cool them down, take them out and grind them for later use;

[0011] (5) Clean the alumina ceramic tube with deionized water and acetone, and dry it for later use;

[0012] (6) evenly applying the suspension of fluorine-containing nickel oxide / tin oxide microporous hollow spheres on the alumina ceramic tube in step (5) to encapsulate the ceramic tube;

[0013] (7) Electrically ageing at 200-300°C for 5-10 days to produce a gas sensor device.

[0014] The template described in step (1) is hexadecyltrimethylammonium bromide (CATB) or amino acid.

[0015] The organic solvent described in step (1) is one of anhydrous ethanol and ethylene glycol.

[0016] The nickel precursor in step (1) is one of nickel chloride and nickel oxalate. And,

[0017] The tin precursor described in step (1) is tin tetrachloride.

[0018] The fluorine organic compound described in step (4) is an organic compound including one of polyvinylidene fluoride, polytetrafluoroethylene and perfluororesin.

[0019] The present invention provides a fluorine-modified nickel oxide / tin oxide composite sensor device, which is prepared according to any of the above methods.

[0020] The invention provides an application of a fluorine-modified nickel oxide / tin oxide composite sensor device for detecting formaldehyde gas in the air.

[0021] The present invention is based on a full understanding of the chemical reaction principle and proposes to enhance gas sensitivity by using fluorine to modify inorganic substances. The present invention has the advantages of simple preparation method, low reaction temperature and can obtain fluorine-containing microporous hollow spheres without complicated subsequent treatment conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the SEM spectrum of the powder sample obtained in Example 1 of the present invention;

[0023] Figure 2 This is the gas-sensitive test curve obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0024] Example 1

[0025] A fluorine-modified nickel oxide / tin oxide composite sensor device is first prepared by a hydrothermal method and a template method to prepare hollow composite spherical particles, which are then mixed with fluorine-containing organic matter. At high temperature, the released fluorine free radicals react with the matrix to form a fluorine-containing composite. Fluorine and carbon in formaldehyde easily form a metastable carbon-fluorine bond, which greatly improves the sensitivity of formaldehyde detection. The preparation is carried out according to the following steps:

[0026] (1) 0.05 mol of the organic template CATB was dissolved in 2 mol of anhydrous ethanol, and after complete dissolution, 0.1 mol of nickel chloride, 0.1 mol of tin chloride and 0.3 mol of a precipitant hexamethylenetetramine were added, and then stirred at room temperature for 4 hours to obtain a precursor solution;

[0027] (2) placing the precursor solution in a reactor and reacting at 100° C. for 48 hours;

[0028] (3) The temperature of the reactor was lowered to room temperature, and the suspension was washed by centrifugation with alcohol and water for 8 times respectively. After drying in an oven at 80° C. for 24 hours, it was placed in a muffle furnace and calcined at 400° C. for 5 hours to obtain microporous hollow nickel oxide / tin oxide balls. The microporous hollow balls were placed in alcohol or water for standby use;

[0029] (4) Grind and mix the composite powder and polytetrafluoroethylene and put them into a corundum crucible. Heat them to 400°C in an atmosphere furnace for 2 hours. Cool them down and take out the suspension of fluorine-containing nickel oxide / tin oxide microporous hollow spheres for standby use. The morphology is as follows: Figure 1 As shown;

[0030] (5) Clean the alumina ceramic tube with deionized water and acetone, and dry it for later use;

[0031] (6) evenly applying the suspension of fluorine-containing nickel oxide / tin oxide microporous hollow spheres on the alumina ceramic tube in step (5) to encapsulate the ceramic tube;

[0032] (7) Electrical aging at 200°C for 10 days to produce a gas sensor device.

[0033] The gas-sensitive test curve obtained in Example 1 is shown in Figure 2 , the sensitivity to formaldehyde can reach 0.5ppm.

[0034] As can be seen from the figure, the fluorine-modified nickel oxide-tin oxide composite material has a very good response to formaldehyde gas, and the detection limit can reach 0.5ppm.

[0035] Example 2

[0036] A fluorine-modified nickel oxide / tin oxide composite sensor device is similar to Example 1 and is prepared according to the following steps:

[0037] (1) Weigh 0.2 mol of amino acid and dissolve it in 4 mol of anhydrous ethanol. After it is completely dissolved, add 0.3 mol of nickel chloride and 0.3 mol of tin chloride, and 0.4 mol of hexamethylenetetramine, and then stir at room temperature for 4 hours to obtain a precursor solution;

[0038] (2) placing the precursor solution in a reactor and reacting at 200°C for 20 hours;

[0039] (3) The temperature of the reactor was lowered to room temperature, and the suspension was centrifugally washed 10 times with alcohol and water respectively. After drying in an oven at 80°C for 24 hours, it was placed in a muffle furnace and calcined at 400°C for 5 hours to obtain microporous hollow nickel oxide / tin oxide balls. The microporous hollow balls were placed in alcohol or water for standby use;

[0040] (4) The composite powder obtained in (3) was ground and mixed with polyvinylidene fluoride and placed in a corundum crucible. The mixture was heated to 400°C in an atmosphere furnace for reaction for 2 hours. The mixture was cooled and ground for standby use. The morphology was similar to that of Figure 1 Same as shown;

[0041] (5) Clean the alumina ceramic tube with deionized water and acetone, and dry it for later use;

[0042] (6) evenly applying a suspension of fluorine-containing nickel oxide / tin oxide microporous hollow spheres on an alumina ceramic tube, and encapsulating the ceramic tube;

[0043] (7) After electrical aging at 300°C for 5 days, the gas sensor device can achieve a formaldehyde sensitivity of 0.3 ppm.

[0044] Example 3

[0045] A fluorine-modified nickel oxide / tin oxide composite sensor device is similar to Example 1 and is prepared according to the following steps:

[0046] (1) 0.1 mol of CATB was weighed and dissolved in 3 mol of ethylene glycol. After the mixture was completely dissolved, 0.2 mol of nickel oxalate and 0.2 mol of tin chloride and 0.3 mol of hexamethylenetetramine were added, and then stirred at room temperature for 4 hours to obtain a precursor solution;

[0047] (2) placing the precursor solution in a reactor and reacting at 150°C for 34 hours;

[0048] (3) The temperature of the reactor was lowered to room temperature, and the suspension was centrifugally washed 10 times with alcohol and water respectively. After drying in an oven at 80°C for 24 hours, it was placed in a muffle furnace and calcined at 600°C for 5 hours to obtain microporous hollow nickel oxide / tin oxide balls. The microporous hollow balls were placed in alcohol or water for standby use; subsequently,

[0049] (4) The composite powder obtained in (3) was ground and mixed with the perfluororesin and placed in a corundum crucible. The mixture was heated to 400°C in an atmosphere furnace for 2 hours. The mixture was cooled and ground for later use. The morphology was similar to that of Figure 1 Same as shown;

[0050] (5) Clean the alumina ceramic tube with deionized water and acetone, and dry it for later use;

[0051] (6) evenly applying a suspension of fluorine-containing nickel oxide / tin oxide microporous hollow spheres on an alumina ceramic tube, and encapsulating the ceramic tube;

[0052] (7) After electrical aging at 250°C for 7 days, the gas sensor device can achieve a formaldehyde sensitivity of 0.4 ppm.

Claims

1. A method for preparing a fluorine-modified nickel oxide / tin oxide composite sensor device, characterized in that First, hollow composite spherical particles are prepared by hydrothermal method and template method, and then mixed with fluorine-containing organic matter. At high temperature, the released fluorine free radicals react with the matrix to form a fluorine-containing composite. Fluorine and carbon in formaldehyde easily form metastable carbon-fluorine bonds, which greatly improves the sensitivity of formaldehyde detection. The process includes the following steps: (1) dissolving an organic template in an organic solvent, and after the organic template is completely dissolved, adding nickel and tin precursors and a precipitant hexamethylenetetramine, wherein the molar ratio of the nickel precursor, the tin precursor, the organic template and the organic solvent is (0.1-0.3):(0.1-0.3):(0.05-0.2):(2-4), and stirring at room temperature for 4 hours to obtain a precursor solution; (2) placing the precursor solution in a reaction vessel and reacting at 100° C.-200° C. for 20-48 hours; (3) The temperature of the reaction kettle was lowered to room temperature, and the suspension was centrifugally washed with alcohol and water for 8-10 times respectively, dried in an oven at 80° C. for 24 hours, and then placed in a muffle furnace and calcined at 400-800° C. for 5 hours to obtain microporous hollow nickel oxide / tin oxide balls, and the microporous hollow balls were placed in alcohol or water for standby use; (4) Grinding and mixing the composite powder and the fluorine-containing organic matter, placing them in a corundum crucible, heating them to 400° C. in an atmosphere furnace for reaction for 2 hours, cooling them down, taking them out and grinding them for later use; (5) Clean the alumina ceramic tube with deionized water and acetone, and dry it for later use; (6) evenly applying the suspension of fluorine-containing nickel oxide / tin oxide microporous hollow spheres on the alumina ceramic tube in step (5) to encapsulate the ceramic tube; (7) Electrically aging at 200-300°C for 5-10 days to produce a gas sensor device; The organic template in step (1) is hexadecyltrimethylammonium bromide (CATB) or amino acid; The organic solvent described in step (1) is one of anhydrous ethanol and ethylene glycol; The nickel precursor described in step (1) is one of nickel chloride and nickel oxalate; In step (1), the tin precursor is tin tetrachloride; The fluorine-containing organic compound in step (4) is one of polyvinylidene fluoride, polytetrafluoroethylene and perfluororesin.

2. A fluorine-modified nickel oxide / tin oxide composite sensor device, characterized in that Prepared according to the method of claim 1.

3. Use of the fluorine-modified nickel oxide / tin oxide composite sensor device according to claim 2 for detecting formaldehyde gas in the air.