Perovskite compositions including mixed solvent systems

By using a mixed solvent system and gentle annealing process in perovskite ink solution, the problem of low crystallinity at low temperatures in perovskite solar cell units is solved, and the deposition and efficiency improvement of high-quality polycrystalline perovskite films are achieved.

CN112166160BActive Publication Date: 2024-11-12THE UNIV OF NORTH CAROLINA AT CHAPEL HILL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980035035.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-04-02
Filing Date
2019-04-01
Publication Date
2024-11-12
Estimated Expiration
2039-04-01

AI Technical Summary

Technical Problem

When existing perovskite solar cell cells crystallize rapidly at low temperatures, they lead to low crystallinity and high defect density, which affects efficiency and stability. It is difficult for conventional volatile organic solvent processes to achieve the deposition of high-quality polycrystalline perovskite films.

Method used

Using a mixed solvent system, combining volatile non-coordinating solvents and non-volatile coordination solvents, the solvent coordination ability and volatility of perovskite ink solution are controlled through rapid evaporation and gentle annealing process to form high-quality polycrystalline perititanium Mineral film.

Benefits of technology

It realizes large-area, compact, pinhole-free polycrystalline perovskite film deposition, improves the efficiency and stability of solar cell units, and is suitable for large-scale industrial manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112166160B_ABST
    Figure CN112166160B_ABST
Patent Text Reader

Abstract

An ink solution is described herein, comprising: a composition of formula (I): ABX3(I), wherein A comprises at least one cation selected from the group consisting of methylammonium, tetramethylammonium, formamidinium, cesium, rubidium, potassium, sodium, butylammonium, phenethylammonium, phenylammonium, and guanidinium; B comprises at least one divalent metal; and X is at least one halide ion; and a mixed solvent system comprising two or more solvents selected from the group consisting of dimethyl sulfoxide, dimethylformamide, γ-butyrolactone, 2-methoxyethanol, and acetonitrile. Also described are methods for producing polycrystalline perovskite films using the ink solution described herein and uses of the films in photovoltaic and photosensitive applications.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Government interests

[0002] This invention was made with Government support under Grant No. N00014-17-1-2619 awarded by the Office of Naval Research. The Government has certain rights in this invention.

[0003] CROSS-REFERENCE TO RELATED APPLICATIONS

[0004] This application claims the benefit of priority to U.S. Provisional Application No. 62 / 651,298, filed on April 2, 2018, which is incorporated herein by reference in its entirety for all purposes. Technical Field

[0005] The presently disclosed subject matter generally relates to perovskite compositions that include mixed solvent systems. The perovskite compositions can be used to make polycrystalline films for use in photovoltaic or photosensitive devices. Background Art

[0006] In recent years, perovskite solar cells have shown rapidly improving power conversion efficiency (PCE) and stability. 1-3 Certified PCE for small installations is already competitive with PCE for other thin-film photovoltaic technologies. 4 However, a challenge before commercialization is to transfer these technologies to the market using high-throughput film deposition techniques for module manufacturing. 5-7 The "high-voltage" future in 2050 will require the installation of 1,780 GW of photovoltaic (PV) capacity per year. 8 In 2017, global installations were only 99.1GW. 9 It requires rapid expansion of PV manufacturing, which can be achieved by perovskite PV due to its low cost and fast solution processing. One gigawatt of power requires more than 6.7 million square meters of solar panels with 18% efficiency. These half-micrometer (μm) thick films need to be deposited quickly to be economically competitive. Therefore, fast and safe deposition of perovskite films is crucial. Deposition under ambient conditions is preferred because the deposition allows easy integration into mature industrial processes and reduces safety issues when flammable solvents are involved. However, from the perspective of material growth kinetics, rapid crystallization at low temperatures generally leads to perovskite films with low crystallinity, high defect density and small grains, which reduces the efficiency and stability of perovskite solar cell units. Therefore, there is a need in the art to mediate the conflict between the low crystallinity induced by rapid deposition and the desire for high efficiency and stability for large grains with high crystallinity. The subject matter described herein solves this problem. Summary of the invention

[0007] In one aspect, the presently disclosed subject matter relates to an ink solution comprising: a composition of formula (I):

[0008] ABX3 (I)

[0009] wherein A comprises at least one cation selected from the group consisting of methylammonium, tetramethylammonium, formamidinium, cesium, rubidium, potassium, sodium, butylammonium, phenethylammonium, phenylammonium, and guanidinium;

[0010] B comprises at least one divalent metal; and

[0011] X is at least one halide ion; and

[0012] A mixed solvent system comprising two or more solvents selected from the group consisting of dimethyl sulfoxide, dimethylformamide, γ-butyrolactone, 2-methoxyethanol and acetonitrile.

[0013] In another aspect, the presently disclosed subject matter relates to a film comprising a polycrystalline perovskite composition of formula (I):

[0014] ABX3 (I)

[0015] wherein A comprises at least one cation selected from the group consisting of methylammonium, tetramethylammonium, formamidinium, cesium, rubidium, potassium, sodium, butylammonium, phenethylammonium, phenylammonium, and guanidinium;

[0016] B comprises at least one divalent metal; and

[0017] X is at least one halide ion;

[0018] wherein the film of the polycrystalline perovskite composition has a macrograin size in the range of about 10 nm to 1 mm, a thickness in the range of about 10 nm to 1 cm, and an area of ​​a compact, pinhole-free, and uniform structure of at least 25 cm 2 .

[0019] In another aspect, the presently disclosed subject matter relates to a solar cell, a solar panel, a light emitting diode, a photodetector, an x-ray detector, a field effect transistor, a memristor, or a synapse comprising a polycrystalline perovskite film fabricated by the methods described herein. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1A Photographs showing PbI2:MAI=1:1 and PbI2 alone dissolved by GBL, 2-ME, ACN, DMSO, and DMF solvents at a nominal molar concentration of 1 M are shown.

[0021] Figure 1BShown are the UV-vis absorption spectra of MAPbI3 solutions prepared from different solvents.

[0022] Figure 1C The vapor pressure and donor number (D) of the five solvents studied are shown. N ) and D of iodide ion N .

[0023] Figure 2A is a photographic image of a MAPbI3 solution prepared by dissolving in ACN / 2-ME and then heating to 80° C. Black perovskite crystals are formed at 80° C.

[0024] Figure 2B is a photographic image of a MAPbI3 solution prepared by dissolving in 2-ME and then heating to 80° C. Black perovskite crystals are formed at 80° C.

[0025] Figure 2C is a photographic image of the reverse temperature crystallization of MAPbI3 in 2-ME solvent at 70 °C.

[0026] Figure 3A Schematic representation of N2 blade-assisted doctor blade coating of perovskite film at 99 mm / s at room temperature using a coordinated tailored ink (inset shows the as-applied ink, the perovskite / intermediate film, and the perovskite film).

[0027] Figure 3B Shown in 15 x 15 cm 2 Freshly coated perovskite film on a flexible substrate.

[0028] Figure 3C It is approximately 10×36cm 2 Photo image of a perovskite submodule. A quarter is placed on edge for scale.

[0029] Figure 3D Schematic diagram illustrating the drying of the ink into a perovskite / intermediate film with annealing at 70°C and complete crystallization of the perovskite film. VNCS: volatile non-coordinating solvent. NVCS: non-volatile coordinating solvent.

[0030] Figure 4A Shown are XRD spectra of as-coated films deposited from DMF, GBL or 2-ME based solution mixtures after N2 knife assisted drying.

[0031] Figure 4B Shown are the XRD spectra of annealed perovskite films prepared with different solvent mixtures.

[0032] Figure 4CShown are the XRD spectra of the as-coated perovskite films from different solvents or solvent mixtures after N2 knife-assisted drying.

[0033] Figure 4D Shown are the XRD spectra of annealed perovskite films prepared with different solvent mixtures.

[0034] Figure 5A SEM images of perovskite films coated by N2 knife-assisted doctor blading using DMF as solvent are shown.

[0035] Figure 5B SEM images of perovskite films coated by N2 knife-assisted doctor blading using GBL as solvent are shown.

[0036] Figure 5C SEM images of perovskite films coated by N2 knife-assisted doctor blading using 2-ME as solvent are shown.

[0037] Figure 5D SEM images of perovskite films coated by N2 blade assisted doctor blading using ACN / 2-ME as solvent are shown.

[0038] Figure 5E shows the SEM image of the perovskite film coated by N2 knife assisted doctor blade with GBL as additive.

[0039] Fig. 5F SEM images of perovskite films prepared with different solvents or solvent mixtures are shown.

[0040] Figure 5G Shown are cross-sectional SEM images of perovskite films prepared with different solvents or solvent mixtures.

[0041] Fig. 6A The allowed coating speeds for obtaining high-quality large-area perovskite films in air-knife-assisted doctor blade coating experiments are shown as a function of different solvents or solvent mixtures.

[0042] Figure 6B Shown are the maximum coating speeds for obtaining high-quality large-area perovskite films when applying different solvents in an N2-blade-assisted doctor blade coating process.

[0043] Fig. 7A The JV curves of small-area perovskite solar cells fabricated using N2-assisted room-temperature doctor blade coating are shown.

[0044] Figure 7B The IV curve of the champion perovskite module is shown.

[0045] Figure 7CThe distribution of the efficiencies of 18 modules manufactured in succession is shown.

[0046] Fig.7D The long-term operational stability of the encapsulated perovskite module loaded at maximum power point under 1 sun-equivalent illumination is shown.

[0047] Fig. 7E The average power conversion efficiency of the perovskite module measured at different temperatures from 25°C to 85°C is shown, where the fitted temperature coefficient is -0.13% / °C. The efficiency of a typical silicon module on the market is also added for reference, which has an efficiency of 17% at 25°C and a temperature coefficient of -0.44% / °C.

[0048] Figure 7F Shown is the efficiency of a perovskite module where one subcell undergoes 58 shading / de-shading cycles. The inset schematically shows how shading is applied on one subcell.

[0049] Fig. 8A Schematic diagram of efficiency uniformity testing on perovskite modules.

[0050] Figure 8B Shown is the efficiency distribution of 16 subcells in a perovskite module.

[0051] Figure 8C The efficiency distribution of 7 positions from one end to the other in a subcell in a perovskite module is shown.

[0052] Fig. 9 The hole area is shown to be 63.7 cm 2 And NREL certification of a perovskite submodule with a stabilized efficiency of 16.4%.

[0053] Fig. 10A Shown are IV scans of the module measured at different temperatures from 25°C to 85°C.

[0054] Fig. 10B The stabilized photocurrent output at the corresponding maximum power point of the module measured at different temperatures from 25°C to 85°C is shown.

[0055] Fig. 10C The open circuit voltage of the module measured at different temperatures is shown, resulting in a fitted temperature coefficient of -0.13% / °C.

[0056] Fig.11A Schematic diagram of applying a mask to one subcell in a perovskite module and then removing the mask.

[0057] Fig. 11Bis the photocurrent output of the module before, during, and after shading. The bias voltage is maintained at 13.2V, which is the maximum power point before shading.

[0058] Fig. 11C Shows Fig. 14B IV curves of the module in before, during and after shading.

[0059] Fig.11D The IV curve of another module during 58 shading / deshading cycles is shown.

[0060] Fig.12 Shown is the reverse bias measured on a single sub-cell from the module at -60 mA bias in the dark after breakdown.

[0061] Fig.13 It is about 360cm to charge the mobile phone 2 Photo of a perovskite submodule. The voltage controller converts the voltage output to about 5V (5.2V, as shown in the number) to meet mobile phone charging standards.

[0062] Fig.14A is a schematic diagram illustrating air knife assisted doctor blade coating of perovskite films.

[0063] Fig. 14B is a photographic image of a freshly applied perovskite film.

[0064] Fig. 14C The drying of the perovskite precursor ink and the crystallization of the perovskite are shown.

[0065] Fig.15A XRD patterns of air knife assisted as-coated perovskite films from DMSO, DMF, GBL, 2-ME / ACN, and 2-ME solvents are shown.

[0066] Fig. 15B SEM images of as-coated perovskite films from 2-ME / CAN and 2-ME / CAN / DMSO with and without air knife assisted drying are shown.

[0067] Fig. 15C XRD spectra of 2-Me / ACN sample without DMSO after annealing (top pattern), 2-ME / ACN sample with DMSO after annealing, and 2-ME / CAN sample with DMSO (center pattern) after air knife assisted doctor blade coating (bottom pattern) are shown. From the bottom pattern, it can be seen that the film is mainly composed of mesophase and minor perovskite phase. After annealing at 70°C for several minutes, the film is converted into a pure perovskite phase with stronger XRD peak intensity than the film without DMSO additive, which indicates improved crystallinity.

[0068] Fig.15D Shown is an SEM image of an as-coated film from a perovskite ink solution using DMSO as solvent and air knife assisted drying.

[0069] Fig.15E Shown is an SEM image of an as-coated film from a perovskite ink solution using DMF as solvent and air knife assisted drying.

[0070] Fig.15F Shown is an SEM image of an as-coated film from a perovskite ink solution using GBL as solvent and air knife assisted drying.

[0071] Figure 15G Shown is an SEM image of an as-coated film from a perovskite ink solution using 2-ME as solvent and air knife assisted drying.

[0072] Fig.15H Shown is an SEM image of an as-coated film from a perovskite ink solution using 2-ME / ACN as solvent and air knife assisted drying.

[0073] Fig.16A The hole area is shown to be 57.2 cm 2 JV curve of the Champion module under one day of illumination. The perovskite film was grown using air knife-assisted blade coating.

[0074] Fig. 16B The photocurrent at the maximum power output point at a bias of 13.6 V is shown to be about 63.5 mA, resulting in a stable PCE of 15.1%. DETAILED DESCRIPTION

[0075] The subject matter described herein relates to new methods for formulating perovskite ink solutions in the fabrication of polycrystalline perovskite films. Halide perovskites, such as methylammonium lead halides (i.e., (CH3NH3)PbX3), where CH3NH3 corresponds to a methylammonium cation and X is a halogen, are a class of photosensitive materials with solar energy applications, with device efficiencies exceeding 20%. Such materials are distinguished by their ABX3 perovskite crystal structure, where A typically includes an organic or alkaline cation; B typically includes tin or lead; and X is a halide ion or a mixture of halide ions, such as fluoride, chloride, iodide, or bromide.

[0076] One advantage of these materials is that they can be produced and processed from solutions at or near room temperature. Ambient temperature processing and production techniques for these photosensitive materials are relatively inexpensive, which is beneficial for large-scale industrial manufacturing of the photosensitive materials. In conventional manufacturing processes, the precursor perovskite components are mixed in a solvent containing a volatile organic solvent, and the resulting precursor solution is deposited onto a substrate, followed by heating the precursor solution at a temperature sufficient to react and convert the precursor materials into a perovskite composition.

[0077] However, there are several challenges and disadvantages in applying conventional volatile organic solvent processes. Although high solvent volatility enables rapid crystallization at low temperatures, rapid crystallization generally results in poor crystallinity and small grain size, which is detrimental for, for example, the transport and collection of photogenerated carriers in a working solar cell. The processes are also known to produce films characterized by incomplete coverage of the substrate and inconsistent (non-uniform) film thickness. These characteristics have been shown to hinder device performance.

[0078] Several investigations have focused on engineering perovskite precursor solutions by using low or non-volatile solvents as a means of enhancing film quality. However, due to the low volatility, high surface tension, and high viscosity of perovskite inks, these solvents typically require high pressure or high temperature techniques to uniformly apply and quickly dry the inks. It has also been shown that many of these solvents strongly coordinate with ions in the precursor inks, inhibiting perovskite formation at room temperature. Proper control of perovskite crystal growth would enable the production of high-quality polycrystalline perovskite films, thereby enhancing device performance potential.

[0079] The inventive method described herein achieves high-quality polycrystalline perovskite films through solvent engineering of perovskite precursor ink solutions. Compared to conventional methods in which the volatility of the solvent in the precursor ink may hinder the production and overall physical properties of the perovskite film, the inventive method described herein focuses on both the coordination ability and volatility of the solvent in the engineered mixed solvent system. In the mixed solvent system described herein, a mixture of a volatile non-coordinating solvent (VNCS) and a non-volatile coordinating solvent (NVCS) is applied to the ink solution. As will be described in further detail, the coordination ability of the solvent refers to the bonding strength between the solvent and the ionic components of the perovskite ink solution. The mixed solvent system including the volatile non-coordinating solvent evaporates rapidly after being deposited on the substrate. The rapid evaporation of the working solvent allows the formation of smooth perovskite films at high speed and room temperature, but results in small grain sizes. Surprisingly, adding a small amount of non-volatile coordinating solvent to the mixed solvent system improves the perovskite crystallinity. It is believed that the non-volatile coordinating solvent is temporarily retained with the perovskite ink components in the as-coated film in an intermediate phase. Under a mild annealing process, the slower release of the non-volatile coordinating solvent provides more time and lower energy barriers for the perovskite crystalline grains to grow larger in size. Therefore, by applying the perovskite ink solution using the methods described herein, high-quality polycrystalline perovskite films of significantly higher quality and resulting improved photovoltaic properties can be achieved.

[0080] The subject matter of the present disclosure will now be described more fully below. However, benefiting from the teaching presented in the foregoing description, the technical personnel in the field involved in the subject matter of the present disclosure will think of many modifications and other embodiments of the subject matter of the present disclosure set forth herein. Therefore, it should be understood that the subject matter of the present disclosure is not limited to the specific embodiments disclosed, and modifications and other embodiments are intended to be included in the scope of the appended claims. In other words, the subject matter described herein covers all substitutions, modifications and equivalent forms. Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as the meaning generally understood by those of ordinary skill in the art. All publications, patent applications, patents and other references mentioned herein are incorporated herein by reference as a whole. If one or more of the combined documents, patents and similar materials are different from or contradictory to the present application, including but not limited to defined terms, term usage, described technology, etc., the present application shall prevail.

[0081] I. Definitions

[0082] As used herein, "and / or" refers to and encompasses any and all possible combinations of one or more of the associated listed items as well as the lack of a combination when interpreted in the alternative ("or").

[0083] As used herein, when referring to a measurable value such as an amount of a compound or agent of the present subject matter, dosage, time, temperature, etc., the term "about" is meant to encompass variations of ±20%, ±10%, ±5%, ±1%, ±0.5%, or even ±0.1% of the specified amount.

[0084] As used herein, the terms "approximately," "about," "essentially," and "essentially" refer to an amount that is close to a stated amount and still performs a desired function or achieves a desired result. For example, in some embodiments, as the context may indicate, the terms "approximately," "about," and "essentially" may refer to an amount that is less than or equal to within 10% of a stated amount. As used herein, the term "generally" refers to a value, amount, or characteristic that primarily contains or tends toward a particular value, amount, or characteristic.

[0085] As used herein, conditional language used herein, such as, inter alia, "can," "could," "might," "may," "eg," and the like, unless otherwise specifically stated or otherwise understood in the context of use, is generally intended to convey that certain embodiments include certain features, elements, and / or steps, while other embodiments do not include certain features, elements, and / or steps. Thus, such conditional language is generally not intended to imply in any way that features, elements, and / or steps are required for one or more embodiments, or that one or more embodiments necessarily include logic for determining whether such features, elements, and / or steps are included in any particular embodiment or will be performed with or without author input or prompting. The terms "comprising," "including," "having," and the like are synonymous and are used in an open-ended manner and do not exclude other elements, features, actions, operations, and the like. Likewise, the term "or" is used in its inclusive sense (and not in its exclusive sense), so that, for example, when used to connect a list of elements, the term "or" means one, some, or all of the elements in the list.

[0086] As defined herein, "compact" refers to a substantially void-free, densely packed film.

[0087] As defined herein, "pinhole-free" refers to a continuous film and wherein the diameter of any hole in the film is less than the thickness of the film. Specifically, a substantially pinhole-free film is a film having a uniform thickness that does not deviate substantially more than + / - 0.10% from the average film thickness.

[0088] As defined herein, a "homogeneous" structure refers to a film characterized by a non-deviating thickness.

[0089] As used herein, "contacting" means allowing the ink solution to contact the substrate.

[0090] As used herein, "VNCS" refers to a volatile non-coordinating solvent.

[0091] As used herein, "NVCS" refers to nonvolatile coordinating solvent.

[0092] As used herein, "VCS" refers to a volatile coordinating solvent.

[0093] As used herein, "NCNCS" refers to a nonvolatile, non-coordinating solvent.

[0094] As used herein, "2-ME" refers to 2-methoxyethanol.

[0095] As used herein, "DMSO" refers to dimethyl sulfoxide.

[0096] As used herein, "DMF" refers to dimethylformamide.

[0097] As used herein, "GBL" refers to gamma-butyrolactone.

[0098] As used herein, "ACN" refers to acetonitrile.

[0099] As used herein, "Ac - ” or “CH3CO2 - ” refers to acetate ion.

[0100] As used herein, "SCN - ” refers to the thiocyanate ion.

[0101] II. Polycrystalline Perovskite Films

[0102] The polycrystalline perovskite films described herein have a perovskite composition according to the formula: ABX3(I)

[0103] In the above formula (I), A includes at least one cation selected from the group consisting of methylammonium, tetramethylammonium, formamidinium, cesium, rubidium, potassium, sodium, butylammonium, phenethylammonium, phenylammonium and guanidinium.

[0104] In certain embodiments, A may include ammonium, the general formula [NR4] + The organic cation, wherein the R groups can be the same or different groups. Suitable R groups include but are not limited to: methyl, ethyl, propyl, butyl, pentyl or isomers thereof; any alkane, alkene or alkyne C x H y, wherein x=1-20, y=1-42, cyclic, branched or linear; alkyl halide, C x H y X z , x=1-20, y=0-42, z=1-42, X=F, Cl, Br or I; any aromatic group (e.g., phenyl, alkylphenyl, alkoxyphenyl, pyridine, naphthalene); cyclic complexes in which at least one nitrogen is contained within the ring (e.g., pyridine, pyrrole, pyrrolidine, piperidine, tetrahydroquinoline); any sulfur-containing group (e.g., sulfoxide, thiol, alkyl thioether); any nitrogen-containing group (nitroxide, amine); any phosphorus-containing group (phosphate); any boron-containing group (e.g., boric acid); any organic acid (e.g., acetic acid, propionic acid); and its ester or amide derivatives; any amino acid containing α, β, γ and higher derivatives (e.g., glycine, cysteine, proline, glutamic acid, arginine, serine, histidine, 5-ammonium pentanoic acid); any silicon-containing group (e.g., siloxane); and any alkoxy or group, —OC x H y , wherein x = 0-20, y = 1-42. In certain embodiments, A comprises methylammonium, (CH3NH3 + In certain embodiments, A is methylammonium. In certain embodiments, A comprises tetramethylammonium, ((CH3)4N + In certain embodiments, A includes butylammonium, which for n-butylammonium can be represented by (CH3(CH2)3NH3 + ) represents, for tert-butylammonium, ((CH3)3CNH3 + ) or for isobutylammonium, (CH3)2CHCH2NH3 + ) is represented by. In certain embodiments, A includes phenethylammonium, which can be represented by C6H5(CH2)2NH3 + Or from C6H5CH(CH3)NH3 + In certain embodiments, A comprises phenylammonium, C6H5NH3 + .

[0105] In certain embodiments, A may include carbamidinium, with the general formula [R2NCHNR2] + The organic cation, wherein the R groups can be the same or different groups. Suitable R groups include but are not limited to: hydrogen, methyl, ethyl, propyl, butyl, pentyl or isomers thereof; any alkane, alkene or alkyne C x H y , wherein x=1-20, y=1-42, cyclic, branched or linear; alkyl halide, C x H y X z, x = 1-20, y = 0-42, z = 1-42, X = F, Cl, Br or I; any aromatic group (e.g., phenyl, alkylphenyl, alkoxyphenyl, pyridine, naphthalene); cyclic complexes in which at least one nitrogen is contained within the ring (e.g., imidazole, benzimidazole, dihydropyrimidine, (azolidinylidenemethyl)pyrrolidine, triazole); any sulfur-containing group (e.g., sulfoxide, thiol, alkyl thioether); any nitrogen-containing group (nitroxide, amine); any phosphorus-containing group (phosphate); any boron-containing group (e.g., boric acid); any organic acid (acetic acid, propionic acid) and its ester or amide derivatives; any amino acid containing α, β, γ and higher derivatives (e.g., glycine, cysteine, proline, glutamic acid, arginine, serine, histidine, 5-ammonium pentanoic acid); any silicon-containing group (e.g., siloxane); and any alkoxy or group, —OC x H y , wherein x = 0-20, y = 1-42. In certain embodiments, A comprises (H2N═CH—NH2 + ) represents the formamidinium ion.

[0106] In certain embodiments, A may include a guanidinium, with the general formula [(R2N)2C═NR2] + The organic cation, wherein the R groups can be the same or different groups. Suitable R groups include but are not limited to: hydrogen, methyl, ethyl, propyl, butyl, pentyl or isomers thereof; any alkane, alkene or alkyne C x H y , wherein x=1-20, y=1-42, cyclic, branched or linear; alkyl halide, C x H y X z , x=1-20, y=0-42, z=1-42, X=F, Cl, Br or I; any aromatic group (e.g., phenyl, alkylphenyl, alkoxyphenyl, pyridine, naphthalene); cyclic complexes in which at least one nitrogen is contained within the ring (e.g., octahydropyrimido[1,2-a]pyrimidine, pyrimido[1,2-a]pyrimidine, hexahydroimidazo[1,2-a]imidazole, hexahydropyrimidin-2-imine); any sulfur-containing group (e.g., sulfoxide, thiol, alkyl thioethers); any nitrogen-containing group (nitroxyl radical, amine); any phosphorus-containing group (phosphate); any boron-containing group (e.g., boric acid); any organic acid (acetic acid, propionic acid) and its ester or amide derivatives; any amino acid containing α, β, γ and higher derivatives (e.g., glycine, cysteine, proline, glutamic acid, arginine, serine, histidine, 5-ammonium pentanoic acid); any silicon-containing group (e.g., siloxane); and any alkoxy or group, —OC x H y, where x = 0-20, y = 1-42. In some embodiments, A may include (H2N═C—(NH2)2 + ) type of guanidinium ion.

[0107] In certain embodiments, A may include an alkali metal cation, such as Li + 、Na + , K + , Rb + or Cs + .

[0108] In certain embodiments, the perovskite crystal structure composition may be doped with a doping element (eg, by partial substitution of cation A and / or metal B), such as an alkali metal (eg, Li + 、Na + , K + , Rb + or Cs + ), alkaline earth metals (e.g., Mg +2 , Ca +2 , Sr +2 , Ba +2 ) or other divalent metal, such as provided below for B, but different from B (e.g., Sn +2 , Pb 2+ 、Zn +2 、Cd +2 ,Ge +2 、Ni +2 , Pt +2 , Pd +2 , Hg +2 、Si +2 、Ti +2 ), or Group 15 elements such as Sb, Bi, As or P, or other metals such as silver, copper, gallium, indium, thallium, platinum or gold, in amounts generally up to or less than about 1, 5, 10, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 99 or 100 mol % of A or B. A may include a mixture of cations. B may include a mixture of cations.

[0109] The variable B includes at least one divalent (B +2) metal atom. The divalent metal (B) may be, for example, one or more divalent elements from Group 14 of the periodic table (e.g., divalent lead, tin, or germanium), one or more divalent transition metal elements from Groups 3-12 of the periodic table (e.g., divalent titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, palladium, platinum, and cadmium), and / or one or more divalent alkaline earth metal elements (e.g., divalent magnesium, calcium, strontium, and barium). The variable X is independently selected from one or a combination of halogen atoms, wherein the halogen atom (X) may be, for example, a fluoride ion (F - ), chloride ion (Cl - ), bromide ion (Br - ) and / or iodide ion (I - ).

[0110] In certain embodiments, the crystalline perovskite composition of formula (I) is selected from the group consisting of cesium lead iodide (CsPbI3), methylammonium tin iodide (CH3NH3SnI3), cesium tin iodide (CsSnI3), methylammonium lead iodide (CH3NH3PbI3), cesium lead bromide (CsPbBr3), methylammonium tin bromide (CH3NH3SnBr3), cesium tin bromide (CsSnBr3), methylammonium lead bromide (CH3NH3PbBr3), formamidinium tin bromide (CHNH2NH2SnBr3), formamidinium lead bromide (CHNH2NH2PbBr3), formamidinium tin iodide (CHNH2NH2SnI3), and formamidinium lead iodide (CHNH2NH2PbI3). In certain embodiments, the crystalline perovskite composition of formula (I) is methylammonium tin iodide (CH3NH3SnI3) or methylammonium lead iodide (CH3NH3PbI3). In certain embodiments, the crystalline perovskite composition of formula (I) is methylammonium lead iodide (CH3NH3PbI3).

[0111] In certain embodiments, the film thickness of the polycrystalline perovskite film described herein is in the range of about 10nm to about 1cm. In certain embodiments, the thickness of the polycrystalline perovskite film is about 300nm to about 1000nm. In certain embodiments, the thickness of the polycrystalline perovskite film is in the range of about 80nm to about 300nm. In certain embodiments, the thickness of the polycrystalline perovskite film is in the range of about 0.1mm to about 50mm. In certain embodiments, the thickness of the polycrystalline perovskite film is in the range of about 100nm to about 1000nm. In certain embodiments, the film thickness of the perovskite film is about, at least, higher than, up to or less than, for example, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm (1μm), 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm or 10μm.

[0112] The polycrystalline perovskite films described herein have an average grain size of about 10 nm to about 1 mm. In certain embodiments, the average grain size of the crystalline perovskite film is about, at least, or greater than 0.01 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 120 μm, 150 μm, 180 μm, 200 μm, 220 μm, 250 μm, 280 μm, 300 μm, 350 μm, 400 μm, 450 μm, 500 μm, 550 μm, 600 μm, 650 μm, 700 μm, 800 μm, 850 μm, 900 μm, 1000 μm, or the average grain size is within a range defined by any two of the aforementioned exemplary values. It is generally known in the art that large grain sizes are suitable for films in photosensitive or photovoltaic applications.

[0113] In some embodiments, the polycrystalline perovskite film can also be obtained with an area of ​​at least 25 cm 2 In some embodiments, the perovskite film produced has an area of ​​at least 15 cm 2 、17cm 2 , 20cm 2 、22cm 2 、25cm 2 、27cm 2 、30cm 2 、35cm 2 、40cm 2 、45cm 2 , 50cm 2 、55cm 2 、60cm 2 、75cm 2 、80cm 2 、85cm 2 , 100cm 2 、125cm 2 、150cm 2 , 200cm 2 、225cm 2 、250cm 2 、275cm 2 、300cm 2 、325cm 2 or 350cm 2 .

[0114] III. Ink Solution

[0115] In another aspect, the subject matter described herein relates to an ink solution. In certain embodiments, the ink solution includes a compound of formula BX'2, wherein B is at least one divalent metal and X' is a monovalent anion; a compound of formula AX, wherein A is at least one monovalent cation selected from the group consisting of methylammonium, tetramethylammonium, formamidinium, guanidinium, cesium, rubidium, potassium, sodium, butylammonium, phenethylammonium, and phenylammonium; and X is selected from the group consisting of halides, acetate (CH3CO2 - ) and thiocyanate (SCN - ); and a mixed solvent system comprising two or more solvents selected from the group consisting of dimethyl sulfoxide, dimethylformamide, γ-butyrolactone, 2-methoxyethanol and acetonitrile.

[0116] In certain embodiments, the ink solution comprises a compound of formula BX'2, wherein the at least one divalent metal (B) is selected from the group consisting of lead, tin, cadmium, germanium, zinc, nickel, platinum, palladium, mercury, titanium, and silicon. In certain embodiments, the ink solution comprises a compound of formula BX'2, wherein the at least one divalent metal (B) is lead or tin. In certain embodiments, the ink solution comprises a compound of formula BX'2, wherein the divalent metal (B) comprises lead. In certain embodiments, the ink solution comprises a compound of formula BX'2, wherein the divalent metal (B) is lead. In certain embodiments, the ink solution comprises a compound of formula BX'2, further comprising (B) being partially substituted with a metal selected from the group consisting of lithium, sodium, potassium, cesium, rubidium, magnesium, calcium, strontium, barium, antimony, bismuth, arsenic, phosphorus, gallium, indium, thallium, molybdenum, gold, silver, copper, and combinations thereof. In certain embodiments, the ink solution includes a compound of formula BX'2, further comprising (B) partially substituted with a metal selected from the group consisting of lithium, sodium, potassium, cesium, rubidium, antimony, bismuth, arsenic, phosphorus, gallium, indium, thallium, molybdenum, gold, silver, copper, and combinations thereof. The partially substituted dopant element at the B site may be present in an amount up to or less than about 1, 5, 10, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 99, or 100 mol % of B.

[0117] In the compound of formula BX'2, the monovalent anion X' can be any anionic species, including halide species X. In certain embodiments, the monovalent anion (X') is a halide. In addition to halide species, some examples of anionic species X' include formate, acetate, propionate, carbonate, nitrate, sulfate, thiosulfate, oxalate, triflate, cyanate, thiocyanate, acetylacetonate, and 2-ethylhexanoate. Some examples of compounds of formula BX'2 include the following: lead (II) fluoride, (PbF2); lead (II) chloride, (PbCl2); lead (II) bromide, (PbBr2); lead (II) iodide, (PbI2); lead (II) acetate, (Pb(CH3CO2)2) or (PbAc2); lead (II) carbonate, (PbCO3); lead (II) nitrate, (Pb(NO3)2); lead (II) sulfate, (PbSO4); lead (II) oxalate, (PbC2O4); lead (II) trifluoromethanesulfonate, (C2F6O6PbS2); lead (II) thiocyanate, (Pb(SCN)2); lead (II) acetylacetonate, (Pb(C5H7O2)2); lead (II) 2-ethylhexanoate, (C 16 H 30 O4Pb); tin(II) fluoride, (S n F2); Tin(II) chloride, (S n Cl2); tin(II) bromide, (S n Br2); Tin(II) iodide, (S n I2); tin(II) acetate, (Sn(CH3CO2)2) or (SnAc2); tin(II) carbonate, (SnCO3); tin(II) nitrate, (Sn(NO3)2); tin(II) sulfate, (SnSO4); tin(II) oxalate, (SnC2O4); tin(II) trifluoromethanesulfonate, (C2F6O6SnS2); tin(II) thiocyanate, (Sn(SCN)2); tin(II) acetylacetonate, (Sn(C5H7O2)2); tin(II) 2-ethylhexanoate, (C 16 H 30O4Sn); Germanium (II) chloride, (GeCl2); Germanium (II) bromide, (GeBr2); Germanium (II) iodide, (GeI2); Titanium (II) chloride, (TiCl2); Titanium (II) bromide, (TiBr2); Titanium (II) iodide, (TiI2); Titanium (II) acetate, (Ti(CH3CO2)2); Magnesium fluoride, (MgF2); Magnesium chloride, (MgCl2); Magnesium bromide, (MgBr2); Magnesium iodide, (MgI2); Magnesium acetate, (Mg(CH3CO2)2); Magnesium sulfate, (MgSO4); Calcium fluoride, (CaF2); Calcium chloride, (CaCl2); Calcium bromide, (CaBr2); Calcium iodide, (CaI2); Calcium acetate, (Ca(CH3CO2)2); Calcium sulfate (CaS O4); cadmium (II) chloride (CdCl2); cadmium (II) bromide (CdBr2); cadmium (II) iodide (CdI2); zinc (II) chloride (ZnCl2); zinc (II) bromide (ZnBr2); zinc (II) iodide (ZnI2); platinum (II) chloride (PtCl2); platinum (II) bromide (PtBr2); platinum (II) iodide (PtI2); nickel (II) chloride (NiCl2); nickel (II) bromide (NiBr2); nickel (II) iodide (NiI2); palladium (II) chloride (PdCl2); palladium (II) bromide (PdBr2); palladium (II) iodide (PdI2); mercury (II) chloride (HgCl2); mercury (II) bromide (HgBr2); and mercury (II) iodide (HgI2).

[0118] In certain embodiments, formula BX'2 is selected from the group consisting of: PbI2, PbBr2, PbCl2, SnI2, SnBr2, and SnCl2. In certain embodiments, formula BX'2 is PbI2 or SnI2. In certain embodiments, the compound of formula BX'2 is PbI2.

[0119] In formula AX, the cationic species A is at least one monovalent cation selected from the group consisting of methylammonium, tetramethylammonium, formamidinium, guanidinium, cesium, rubidium, potassium, sodium, butylammonium, phenethylammonium and phenylammonium; and X is selected from the group consisting of halide, acetate (CH3CO2 - ) and thiocyanate (SCN -). In certain embodiments, X is a halide. Several non-limiting examples of compounds of formula AX include methylammonium fluoride, methylammonium chloride, methylammonium bromide, methylammonium iodide, tetramethylammonium fluoride, tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium iodide, formamidinium chloride, formamidinium bromide, formamidinium iodide, guanidinium fluoride, guanidinium chloride, guanidinium bromide, guanidinium iodide, cesium iodide, cesium bromide, cesium chloride, butylammonium iodide, butylammonium bromide, butylammonium chloride, phenethylammonium iodide, phenethylammonium bromide, phenethylammonium chloride, phenylammonium iodide, phenylammonium bromide, and phenylammonium chloride. In certain embodiments, the compound of formula AX is selected from the group consisting of: methylammonium iodide, methylammonium bromide, methylammonium chloride, formamidinium iodide, formamidinium bromide, formamidinium chloride, cesium iodide, cesium bromide, cesium chloride, butylammonium iodide, butylammonium bromide, butylammonium chloride, phenethylammonium iodide, phenethylammonium bromide, phenethylammonium chloride, phenylammonium iodide, phenylammonium bromide, and phenylammonium chloride. In certain embodiments, the compound of formula AX is selected from the group consisting of: methylammonium iodide, cesium iodide, formamidinium iodide, butylammonium iodide, phenethylammonium iodide, methylammonium bromide, cesium bromide, formamidinium bromide, butylammonium bromide, and phenethylammonium iodide. In certain embodiments, the compound of formula AX is methylammonium iodide. In certain embodiments, the ink solution includes a compound of formula AX, further comprising (A) partially substituted with a metal selected from the group consisting of lithium, magnesium, calcium, strontium, barium, and combinations thereof. The partially substituted dopant element at the A site may be present in an amount up to or less than about 1, 5, 10, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 99, or 100 mol % of A.

[0120] In certain embodiments, BX'2 is PbI2 and AX is methylammonium iodide.

[0121] In the ink solution, BX'2 and AX in the precursor are generally present in a molar ratio of M:X of about 1:3. In the case where X' is a halide (X) (which corresponds to BX'2 being BX2), a molar ratio of B:X of about 1:3 can be provided by a molar ratio of BX2:AX of 1:1. In the case where X' is a non-halide (e.g., acetate), a molar ratio of B:X of about 1:3 can be provided by a molar ratio of BX'2:AX of about 1:3.

[0122] In certain embodiments, the relative amount of ABX3 to BX'2 and AX is about 99: 1. In certain embodiments, the relative amount of ABX3 to BX'2 and AX is about 80:20, about 70:30, about 50:50, about 30:70, about 20:80, or about 1:99.

[0123] The ink solution disclosed herein includes a mixed solvent system comprising two or more solvents. In certain embodiments, the mixed solvent system includes two or more solvents selected from the group consisting of: dimethyl sulfoxide, dimethylformamide, 2-methoxyethanol, acetonitrile, methanol, propanol, butanol, tetrahydrofuran, pyridine, alkylpyridine, pyrrolidine, chlorobenzene, dichlorobenzene, dichloromethane, 1-methoxypropane-2-ol, 2-methoxy-1-methylethyl acetate, 2-butoxyethanol, 2-butoxyethyl acetate, 2-(propoxy)ethanol, 3-ethoxypropionic acid ethyl ester, glycol ether, dimethylacetamide, acetone, N,N-dimethylpropylene urea and chloroform. In certain embodiments, the mixed solvent system includes two or more solvents selected from the group consisting of: dimethyl sulfoxide, dimethylformamide, γ-butyrolactone, 2-methoxyethanol and acetonitrile. In certain embodiments, the mixed solvent system includes three or more solvents.

[0124] Two or more solvents constituting a mixed solvent system can be classified as coordinating or non-coordinating solvents. On the one hand, the coordinating ability of a solvent can refer to its strength as a Lewis base. As defined herein, a Lewis base is a compound or ionic substance that can provide an electron pair to an acceptor compound. A Lewis acid is a substance that can accept a pair of non-bonded electrons. On the one hand, a "coordinating solvent" is a strong Lewis base, and a "non-coordinating solvent" is a weak Lewis base.

[0125] In another aspect, the coordination ability of a solvent can refer to how well it coordinates or bonds to a metal ion. In certain embodiments described herein, the coordination ability of a solvent is related to its ability to bind to Pb 2+ or Sn 2+ In certain embodiments, the coordinating solvent exhibits a degree of coordination or bonding with Pb 2+ or Sn 2+ In certain embodiments, the non-coordinating solvent exhibits strong bonding with Pb 2+ or Sn 2+ Weak bonding of donors. N) is generally used to quantify the coordination ability of a solvent. The donor number is defined as the negative enthalpy of forming a 1:1 adduct between a Lewis base and a standard Lewis acid SbCl5 (antimony pentachloride) in a dilute solution of a non-coordinating solvent 1,2-dichloroethane with a donor number of zero. The donor number is generally reported in units of kcal / mol. In certain embodiments, the donor number of a coordinating solvent is at least 20 kcal / mol. In certain embodiments, the donor number of a coordinating solvent is in the range of 20 kcal / mol to 25 kcal / mol. In certain embodiments, the donor number of a coordinating solvent is greater than 25 kcal / mol. In certain embodiments, the donor number of a non-coordinating solvent is less than 20 kcal / mol. For example, the donor number of acetonitrile is 14.1 kcal / mol. Therefore, acetonitrile is classified as a non-coordinating solvent. The donor number of dimethyl sulfoxide is 29.8 kcal / mol, and is referred to herein as a coordinating solvent.

[0126] In certain embodiments, the mixed solvent system comprises two or more solvents selected from the group consisting of: a volatile coordinating solvent, a non-volatile coordinating solvent, a volatile non-coordinating solvent, and a non-volatile non-coordinating solvent. In certain embodiments, the mixed solvent system comprises two volatile non-coordinating solvents. In certain embodiments, the mixed solvent system comprises three or more solvents selected from the group consisting of: a volatile coordinating solvent, a non-volatile coordinating solvent, a volatile non-coordinating solvent, and a non-volatile non-coordinating solvent. In certain embodiments, the mixed solvent system is a ternary solvent system comprising two volatile non-coordinating solvents and a non-volatile coordinating solvent. In certain embodiments, the mixed solvent system is a ternary solvent system comprising two volatile non-coordinating solvents and a volatile coordinating solvent.

[0127] In certain embodiments, ink solutions, arrays containing ink solutions, and methods use an ink solution comprising about 58.8% by volume of a volatile non-coordinating solvent, about 39.2% by volume of a second volatile non-coordinating solvent, and about 2% by volume of a coordinating solvent. In certain embodiments, the percentage of the coordinating solvent is about 0.01-10.0% by volume, about 0.01-5% by volume, about 0.01-1% by volume, about 0.1-5% by volume, about 0.5-4% by volume, about 1.0-3% by volume, or about 2-2.5% by volume. The coordinating solvent can be a volatile or non-volatile solvent. In certain embodiments, the coordinating solvent is a non-volatile solvent. In certain embodiments, the coordinating solvent is dimethyl sulfoxide.

[0128] In certain embodiments, a mixed solvent system comprising two volatile non-coordinating solvents can be mixed in a volume ratio in the range of about 1:100 to 100:1. In certain embodiments, the two volatile non-coordinating solvents are acetonitrile and 2-methoxyethanol. In certain embodiments, the solvent solution comprises a volume ratio of acetonitrile to 2-methoxyethanol of 2:1. In certain embodiments, the volume ratio of acetonitrile to 2-methoxyethanol is 3:2. In certain embodiments, the ratio is about 4:3, 1:1, 1:2, 2:3 or 3:4. In certain embodiments, the volume ratio of acetonitrile to 2-methoxyethanol is about 1:100 to about 100:1.

[0129] In certain embodiments, the mixed solvent system is a ternary mixed solvent system including two volatile non-coordinating solvents and a coordinating solvent, the solvent system including 95 to 99.9% by volume of a mixture of any volume ratio of two volatile non-coordinating solvents ranging from 1:100 to 100:1 and 0.1 to 5% by volume of a coordinating solvent. The coordinating solvent can be volatile or non-volatile. In certain embodiments, the two volatile non-coordinating solvents are acetonitrile and 2-methoxyethanol, and a coordinating solvent is dimethyl sulfoxide. In certain embodiments, the mixed solvent system includes about 95-99.9% by volume of acetonitrile and 2-methoxyethanol and about 0.1-5% by volume of dimethyl sulfoxide. In certain embodiments, the mixed solvent system includes about 97% by volume of acetonitrile and 2-methoxyethanol and about 3% by volume of dimethyl sulfoxide. In certain embodiments, the mixed solvent system includes about 97.5% by volume of acetonitrile and 2-methoxyethanol and about 2.5% by volume of dimethyl sulfoxide. In certain embodiments, the mixed solvent system includes about 98 volume % acetonitrile and 2-methoxyethanol and about 2 volume % dimethyl sulfoxide.

[0130] In certain embodiments, the ink solution may also contain additives. Non-limiting examples of additives include L-α-phosphatidylcholine, methylammonium chloride, and methylammonium hypophosphite. These additives may be added to the precursor solution at a molar percentage ranging from 0.01% to about 1.5% relative to the ABX3 composition. In certain embodiments, the molar percentage is about 0.025%, about 0.5%, about 0.8%, or about 1.0% relative to the ABX3 composition.

[0131] In certain embodiments, the vapor pressure of the ink solution is in the range of about 5 kPa to 100 kPa. In certain embodiments, the vapor pressure of the ink solution is in the range of about 2 kPa to 80 kPa, about 5 kPa to 70 kPa, about 10 kPa to 60 kPa, about 15 kPa to 50 kPa, about 20 kPa to 40 kPa, about 25 kPa to 40 kPa, about 5 kPa to 15 kPa, about 7 kPa to 10 kPa, about 10 kPa to 20 kPa, or about 8 kPa to 9 kPa.

[0132] IV. Methods

[0133] In certain embodiments, the subject matter disclosed herein relates to a method for producing a polycrystalline perovskite film using the above-mentioned ink solution. In certain embodiments, the method includes: contacting the ink solution onto a substrate using a rapid coating process to form a film, wherein the rapid coating process is selected from the group consisting of: doctor blade coating, slot coating, shear coating, gravure coating, brush coating, syringe coating, and screen printing.

[0134] The use of a rapid coating process is advantageous due to the increased scalability, simplicity, and cost-effectiveness of roll-to-roll production of perovskite devices. In addition, the rapid coating process also provides advantages due to high-throughput deposition, high material usage, and application on flexible substrates. Specifically, due to significantly higher carrier mobility in blade-coated films, perovskite films and devices manufactured using rapid coating processes (such as doctor blade coating) can advantageously have long carrier diffusion lengths (e.g., up to 3 μm thick). Such doctor-blade deposition can be used for large-area perovskite cells manufactured in high-volume roll-to-roll production.

[0135] In some embodiments, a device for contacting the ink solution to the substrate is used in a rapid coating process. In a blade coating process, a "blade coater" may be used. As used herein, "blade coater" is synonymous with "blade". In some embodiments, a blade coating technique is used to facilitate the formation of a polycrystalline perovskite film during the manufacturing process.

[0136] In certain embodiments, the method for producing a polycrystalline perovskite film using a rapid coating process may be performed at a temperature between about 25° C. and about 250° C. In certain embodiments, the method is performed at about room temperature (about 25° C.).

[0137] In certain embodiments of the rapid coating process, the substrate is moving and the device is stationary. In certain embodiments, the device is a scraper. In certain aspects, the substrate moves at a rate of about 2 mm / s relative to the device. In certain aspects, the substrate moves at a rate of about 20 mm / s relative to the device. In certain aspects, the substrate moves at a rate of about 40 mm / s relative to the device. In certain aspects, the substrate moves at a rate of about 99 mm / s relative to the device. In certain aspects, the substrate is stationary and the device moves relative to the substrate. In certain aspects, the device moves at a rate of about 2 mm / s relative to the substrate. In certain aspects, the device moves at a rate of about 20 mm / s relative to the substrate. In certain aspects, the device moves at a rate of about 40 mm / s relative to the substrate. In certain aspects, the device moves at a rate of about 99 mm / s relative to the substrate.

[0138] In certain embodiments, the rapid coating process described herein is performed at about 2 mm / s to about 15,000 mm / s. In certain embodiments, the rapid coating process described herein is performed at about 2 mm / s to about 10,000 mm / s. In certain embodiments, the rapid coating process described herein is performed at about 2 mm / s to about 99 mm / s. In some embodiments, the rapid coating process is performed at least at or about 2 mm / s, 20 mm / s, 40 mm / s, 60 mm / s, 80 mm / s, 99 mm / s, 150 mm / s, 275 mm / s, 500 mm / s, 700 mm / s, 800 mm / s, 900 mm / s, 1000 mm / s, 2000 mm / s, 3000 mm / s, 4000 mm / s, 5000 mm / s, 6000 mm / s, 7000 mm / s, 8000 mm / s, 9000 mm / s, 10,000 mm / s, 11,000 mm / s, 12,000 mm / s, 13,000 mm / s, 14,000 mm / s or 15,000 mm / s.

[0139] In certain embodiments, the distance between the devices used to contact the ink solution onto the substrate in the rapid coating process is between about 10 μm and 1 cm. In certain embodiments, the distance between the device and the substrate is between about 150 and about 350 μm. In certain embodiments, the distance between the device and the substrate is between about 200 and about 300 μm. In certain embodiments, the distance between the device and the substrate is about 200 μm, 225 μm, about 250 μm, about 275 μm, or about 300 μm.

[0140] In certain embodiments, the method for producing a polycrystalline perovskite film described herein further includes knife-assisted drying. Knife drying includes applying a high-speed, low-pressure gas to an ink solution to form a perovskite film on a substrate. The advantage of knife drying in a polycrystalline perovskite film production process is that it helps to produce a uniform and smooth film. As used herein, "air knife", "N2 knife" or "air doctor" may be used to describe a device that performs knife-assisted drying in a perovskite film production process. The knife may have a gas manifold with multiple nozzles that direct a high-speed flow of air or other gas to the perovskite ink on the substrate. The gas used for the knife-assisted drying process may be air, nitrogen, argon, helium, oxygen, neon, hydrogen, and combinations thereof.

[0141] In some embodiments, knife-assisted drying is performed at a temperature of about 25° C. to about 250° C. In some embodiments, knife-assisted drying is performed at room temperature (about 25° C.) In some embodiments, knife-assisted drying is performed at a temperature of about 50° C. to about 100° C.

[0142] In certain embodiments, knife-assisted drying is performed at a pressure in the range of about 0 psi to 500 psi. In certain embodiments, knife-assisted drying is performed at a pressure in the range of about 5 psi to 400 psi, about 20 psi to 300 psi, about 50 psi to 200 psi, about 100 psi to 150 psi, about 5 psi to 25 psi, about 5 psi to 20 psi, about 10 psi to 20 psi, about 10 psi to 19 psi, about 12 psi to 18 psi, about 12-16 psi, or about 13-16 psi. In certain embodiments, knife-assisted drying is performed at a pressure in the range of about 14 psi, about 15 psi, about 16 psi, about 17 psi, about 18 psi, or about 19 psi.

[0143] In some embodiments, the knife is angled with the device and substrate for the rapid coating process to produce a unidirectional airflow on the just coated film, thereby enhancing the uniformity of the blow molding. In some embodiments, the knife is at an angle of 0°, 5°, 10°, 15°, 20°, 25°, 30°, 35°, 40°, 45°, 50°, 55°, 60°, 65°, 70°, 75°, 80°, 90°, 100°, 120°, 150°, 155°, 170°, or 180° with the device or substrate.

[0144] In certain embodiments, after flash coating and / or knife-assisted drying, the film produced from the ink solution (when on a substrate) may be subjected to annealing. The film is annealed at a temperature of at least or above 30°C for a period of time effective to convert the perovskite precursor components in the ink solution into a film of a crystalline halide perovskite within the scope of formula (I) above. In certain embodiments, the annealing employs a temperature of about, at least, above, up to, or less than 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, or 200°C, or a temperature within a range defined by any two of the foregoing values. In various embodiments, annealing may be performed in the range of, for example, 30-200°C, 50-150°C, 30-180°C, 30-150°C, 30-140°C, 30-130°C, 30-120°C, 30-110°C, or 30-100°C.

[0145] Annealing can be performed for a period of time, such as in the range of about 0 seconds to 400 minutes, about 5 seconds to 30 seconds, about 5 minutes to about 10 minutes, about 10 minutes to 20 minutes, or about 20 minutes to 30 minutes. Annealing can be performed for a period of time, such as at least 5 seconds, 10 seconds, 20 seconds, 30 seconds, 1 minute, 5 minutes, 10 minutes, 20 minutes, 30 minutes, 60 minutes, 90 minutes, 120 minutes, 180 minutes, 240 minutes, or 360 minutes.

[0146] In certain embodiments, the methods described herein produce polycrystalline perovskite films having a film thickness in the range of about 10 nm to about 1 cm. In certain embodiments, the methods described herein produce polycrystalline perovskite films having a film thickness in the range of about 300 nm to about 1000 nm. In certain embodiments, the methods described herein produce polycrystalline perovskite films having a film thickness in the range of about 80 nm to about 300 nm. In certain embodiments, the methods described herein produce polycrystalline perovskite films having a film thickness in the range of about 0.1 mm to about 50 mm. In certain embodiments, the methods described herein produce polycrystalline perovskite films having a film thickness in the range of about 100 nm to about 1000 nm. In certain embodiments, the methods described herein produce polycrystalline perovskite films having a film thickness in a range of about, at least, above, up to, or less than, for example, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1000 nm (1 μm), 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, or 10 μm.

[0147] The methods described herein produce polycrystalline perovskite films with an average grain size of about 10 nm to about 1 mm. In certain embodiments, the methods described herein produce polycrystalline perovskite films with an average grain size of about, at least, or above 0.01 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 120 μm, 150 μm, 180 μm, 200 μm, 220 μm, 250 μm, 280 μm, 300 μm, 350 μm, 400 μm, 450 μm, 500 μm, 550 μm, 600 μm, 650 μm, 700 μm, 800 μm, 850 μm, 900 μm, 1000 μm, or a polycrystalline perovskite film with an average grain size within a range defined by any two of the aforementioned exemplary values. It is generally known in the art that large grain sizes are suitable for films in photosensitive or photovoltaic applications.

[0148] In certain embodiments, the methods described herein produce a method capable of obtaining a crystalline solid matrix having an area of ​​at least 25 cm 2 In certain embodiments, the methods described herein produce polycrystalline perovskite films with a compact, pinhole-free, and uniform structure. 2 、17cm 2 , 20cm 2 、22cm 2 、25cm 2 、27cm 2 、30cm 2 、35cm 2 、40cm 2 、45cm 2 , 50cm 2 、55cm 2 、60cm 2 、75cm 2 、80cm 2 、85cm 2 , 100cm 2 、125cm 2 、150cm 2 , 200cm 2 、225cm 2 、250cm 2 、275cm 2 、300cm 2 、325cm 2 or 350cm 2 polycrystalline perovskite film.

[0149] V. Device

[0150] The polycrystalline perovskite films described herein can be used in a variety of photosensitive and photovoltaic applications. The perovskite films can be integrated into, for example, photoluminescent devices, photoelectrochemical devices, thermoelectric devices, and photocatalytic devices. Some non-limiting examples of applications for which polycrystalline perovskite films can be applied include solar cells, solar panels, solar modules, light emitting diodes, lasers, photodetectors, x-ray detectors, batteries, hybrid PV cells, field effect transistors, memristors, or synapses.

[0151] In certain embodiments, polycrystalline perovskite films can be used in active layers of various device architectures. In addition, polycrystalline perovskite films can provide one or more functions of any one or more components of the active layer (e.g., charge transport materials, mesoporous materials, photosensitive materials, and / or interface materials). In some embodiments, the same perovskite film can provide multiple such functions, but in other embodiments, multiple perovskite films can be included in a device, each perovskite film providing one or more such functions.

[0152] In some embodiments, a polycrystalline perovskite film as described herein is applied to a device. In some embodiments, the device may include a first electrode, a second electrode, and an active layer including the polycrystalline perovskite film, the active layer being at least partially disposed between the first electrode and the second electrode. In some embodiments, the first electrode may be one of an anode and a cathode, and the second electrode may be the other of the anode and the cathode.

[0153] The active layer according to some embodiments may include any one or more active layer components, including any one or more of the following: charge transport materials; liquid electrolytes; mesoporous materials; photosensitive materials (e.g., dyes, silicon, cadmium telluride, cadmium sulfide, cadmium selenide, copper indium gallium selenide, gallium arsenide, germanium indium phosphide, semiconductor polymers, other photosensitive materials); and interface materials. Any one or more of these active layer components may include one or more perovskite films. In some embodiments, some or all of the active layer components may be arranged in a sublayer as a whole or in part. For example, the active layer may include any one or more of the following: an interface layer including an interface material; a mesoporous layer including a mesoporous material; and a charge transport layer including a charge transport material. In some embodiments, a photosensitive material such as a dye may be coated on any one or more of these layers, or otherwise disposed on any one or more of these layers. In some embodiments, any one or more layers may be coated with a liquid electrolyte. Further, the interface layer may be included between any two or more other layers in the active layer and / or between the layer and the coating (such as between the dye and the mesoporous layer) and / or between the two coatings (such as between the liquid electrolyte and the dye) and / or between the active layer components and the electrode. References to layers herein may include the final arrangement (e.g., substantially discrete portions of each material that can be defined separately within the device), and / or references to layers may mean the arrangement during the construction of the device, although one or more materials may be subsequently mixed in each layer. In some embodiments, the layer may be discrete and include substantially continuous materials. In other embodiments, the layers may be substantially intermixed (such as in the case of, for example, BHJ, hybrid, and some DSSC cells). In some embodiments, the device may include a mixture of these two layers. In any case, any two or more layers of any kind may be arranged adjacent to each other (and / or intermixed with each other) in certain embodiments in a manner to obtain a high contact surface area. In certain embodiments, a layer comprising a perovskite film may be arranged adjacent to one or more other layers in order to obtain a high contact surface area (e.g., in the case where the perovskite film exhibits low charge mobility). In other embodiments, a high contact surface area may not be necessary (eg, where the perovskite film exhibits high charge mobility).

[0154] The device according to some embodiments may optionally include one or more substrates. In some embodiments, either or both of the first electrode and the second electrode may be coated or otherwise disposed on a substrate so that the electrode is substantially disposed between the substrate and the active layer. In various embodiments, the material of the composition of the device (e.g., substrate, electrode, active layer and / or active layer component) may be rigid or flexible in whole or in part. In some embodiments, the electrode may serve as a substrate, thereby eliminating the need for a separate substrate. In certain embodiments, the component is flexible. In certain embodiments, the rapid coating process described herein is used to coat the electrode, substrate, active layer and / or active layer component.

[0155] The ink solution can be deposited by any process known in the art for depositing liquid films. As described above, some examples of film deposition processes include blade coating, slot coating, shear coating, gravure coating, brush coating, syringe coating, and screen printing. In certain embodiments, blade coating is used. The substrate on which the precursor solution is placed can be any useful substrate known in the art, including functional substrates and sacrificial substrates. The substrate can be any substrate that is non-reactive with the precursor ink components, appropriately robust to withstand potential annealing, and suitable for integration into a photosensitive device. The choice of functional substrate depends on the end-use application. In some embodiments, the substrate is inorganic, such as silicon (Si), metal (e.g., Al, Co, Ni, Cu, Ti, Zn, Pt, Au, Ru, Mo, W, Ta or Rh, stainless steel, metal alloys, or combinations thereof), metal oxides (e.g., glass or ceramic materials, such as indium tin oxide doped with F), metal nitrides (e.g., TaN), metal carbides, metal silicides, or metal borides. In other embodiments, the substrate is organic, such as a rigid or flexible heat-resistant plastic or polymer film, or a combination thereof, or a multilayer composite thereof. Some of these substrates, such as molybdenum-coated glass and flexible plastic or polymer films, are particularly suitable for photovoltaic applications. Photovoltaic substrates can be, for example, absorber layers, emitter layers, or transmitter layers useful in photovoltaic devices. Depending on the end use of the perovskite film, the substrate can be porous or non-porous.

[0156] The electrode may be an anode or a cathode. In some embodiments, one electrode may serve as a cathode and the other electrode may serve as an anode. The electrode may be composed of any conductive material. Suitable electrode materials may include any one or more of: indium tin oxide or tin-doped indium oxide (ITO); fluorine-doped tin oxide (FTO); cadmium oxide (CdO); zinc indium tin oxide (ZITO); zinc aluminum oxide (AZO); aluminum (Al); gold (Au); copper (Cu); chromium (Chromium); calcium (Ca); magnesium (Mg); titanium (Ti); steel; carbon (and its allotropes); and combinations thereof.

[0157] Devices employing the polycrystalline perovskite films described herein may include mesoporous materials. The mesoporous material may comprise any pore-containing material. In some embodiments, the diameter of the pores may range from about 1 nm to about 100 nm; in other embodiments, the pore size may range from about 2 nm to about 50 nm. Suitable mesoporous materials include any one or more of the following: any interface material and / or mesoporous material discussed elsewhere herein; aluminum (Al); bismuth (Bi); indium (In); molybdenum (Mo); niobium (Nb); nickel (Ni); silicon (Si); titanium (Ti); vanadium (V); zinc (Zn); zirconium (Zr); oxides of any one or more of the foregoing metals (e.g., aluminum oxide, ceria, titanium dioxide, zinc oxide, zirconium oxide, etc.); sulfides of any one or more of the foregoing metals; nitrides of any one or more of the foregoing metals; and combinations thereof.

[0158] The photosensitive material may include any photosensitive compound, such as silicon (in some cases, single crystal silicon), cadmium telluride, cadmium sulfide, cadmium selenide, copper indium gallium selenide, gallium arsenide, germanium indium phosphide, one or more semiconductor polymers and any one or more of their combinations. In some embodiments, the photosensitive material may alternatively or additionally include a dye (e.g., N719, N3, other ruthenium-based dyes). In some embodiments, the dye (of whatever composition) may be coated on another layer (e.g., a mesoporous layer and / or an interface layer). The device according to various embodiments may include one, two, three or more photosensitive compounds. In some embodiments including multiple dyes or other photosensitive materials, each of the two or more dyes or other photosensitive materials may be separated by one or more interface layers. In some embodiments, multiple dyes and / or photosensitive compounds may be at least partially mixed with each other.

[0159] The charge transport material (e.g., the charge transport material of the charge transport layer) may comprise a solid charge transport material (i.e., a solid electrolyte colloquially labeled), or the charge transport material may comprise a liquid electrolyte and / or an ionic liquid. Any of a liquid electrolyte, an ionic liquid, and a solid charge transport material may be referred to as a charge transport material. As used herein, a "charge transport material" refers to any material (solid, liquid, or otherwise) that is capable of collecting charge carriers and / or transporting charge carriers. For example, in a PV device according to some embodiments, the charge transport material may be capable of transporting charge carriers to an electrode. The charge carriers may include holes (the transport of holes may cause the charge transport material to be just as appropriately labeled a "hole transport material") and electrons. Holes may be transported toward the anode, and electrons may be transported toward the cathode, depending on the placement of the charge transport material relative to the cathode or anode in the PV or other device. Suitable examples of charge transport materials according to some embodiments may include any one or more of the following: perovskite materials; I - / I3 - ; Co complexes; polythiophenes (e.g., poly(3-hexylthiophene) and its derivatives or P3HT); carbazole-based copolymers, such as polyheptadecanylcarbazole, dithienylbenzothiadiazole and its derivatives (e.g., PCDTBT); other copolymers, such as polycyclopentadienyldithiophene-benzothiadiazole and its derivatives (e.g., PCPDTBT); poly(triarylamine) compounds and their derivatives (e.g., PTAA); spirobifluorene; fullerenes and / or fullerene derivatives (e.g., C60, PCBM); and combinations thereof. In certain embodiments, the charge transport material may include any material (solid or liquid) that is capable of collecting charge carriers (electrons or holes) and / or capable of transporting charge carriers. The charge transport material of some embodiments may therefore be an n- or p-type active and / or semiconducting material. The charge transport material may be positioned close to one of the electrodes of the device. It may be positioned adjacent to the electrode in some embodiments, but in other embodiments, an interface layer may be positioned between the charge transport material and the electrode. In certain embodiments, the type of charge transport material can be selected based on the electrode to which it is close. For example, if the charge transport material collects and / or transports holes, it can be close to the anode in order to transport holes to the anode. However, the charge transport material can alternatively be placed close to the cathode and be selected or constructed so as to transport electrons to the cathode.

[0160] Devices according to various embodiments may optionally include an interface layer between any two other layers and / or materials, but devices according to some embodiments need not contain any interface layer. Thus, for example, a device may contain zero, one, two, three, four, five or more interface layers. The interface layer may include a thin coating interface layer (e.g., including aluminum oxide and / or other metal oxide particles, and / or a titanium dioxide / metal oxide bilayer, and / or other compounds based on a thin coating interface layer). The interface layer according to some embodiments may include any suitable material for enhancing charge transport and / or collection between two layers or materials; it may also help prevent or reduce the likelihood of charge recombination once the charge has been transferred from one of the materials adjacent to the interface layer. Suitable interface materials may include any one or more of the following: any mesoporous material and / or interface material discussed elsewhere herein; Al; Bi; In; Mo; Ni; Platinum (Pt); Si; Ti; V; Nb; Zn; Zr, oxides of any of the foregoing metals (e.g., aluminum oxide, silicon dioxide, titanium dioxide); sulfides of any of the foregoing metals; nitrides of any of the foregoing metals; functionalized or non-functionalized alkylsilyl groups; graphite; graphene; fullerenes; carbon nanotubes; and combinations thereof (including, in some embodiments, bilayers of combined materials). In some embodiments, the interface layer may include a perovskite film.

[0161] In certain embodiments, the subject matter described herein relates to a perovskite solar cell unit. In certain embodiments, the perovskite solar cell unit includes a substrate; a first transmission layer, the first transmission layer disposed on the substrate; a perovskite film as described herein, the perovskite film disposed on the first transmission layer; a second transmission layer, the second transmission layer disposed on the film; and a conductive electrode, the conductive electrode disposed on the second transmission layer.

[0162] The power conversion efficiency (PCE) of the solar cell units described herein ranges from about 13% to about 24%. In certain embodiments, the PCE is at least 14%, 15%, 16%, 17%, 18%, 19%, 20%, or 21%. In certain embodiments, the PCE is 21.3%.

[0163] In certain embodiments, the crystalline perovskite film as described herein is applied in a solar module. In certain embodiments, the module exhibits a PCE of at least 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, or 21%. In certain embodiments, the module exhibits a PCE of about 15.9%, about 15.8%, or about 16.4%.

[0164] In certain embodiments, modules including a crystalline perovskite film as described herein exhibit a temperature coefficient (β) of about -0.08%, -0.09%, -0.10%, -0.11%, -0.12%, -0.13%, -0.14%, -0.15%, -0.16%, -0.17%, -0.18%, -0.19%, or about -0.20% / °C. PCE As described herein, the temperature coefficient of a module can be obtained by measuring its efficiency over a temperature range of 25°C to 85°C under AM 1.5 G.

[0165] The subject matter described herein relates to the following embodiments:

[0166] 1. An ink solution comprising: a composition of formula (I):

[0167] ABX3 (I)

[0168] wherein A comprises at least one cation selected from the group consisting of methylammonium, tetramethylammonium, formamidinium, cesium, rubidium, potassium, sodium, butylammonium, phenethylammonium, phenylammonium, and guanidinium;

[0169] B comprises at least one divalent metal; and

[0170] X is at least one halide ion; and

[0171] A mixed solvent system comprising two or more solvents selected from the group consisting of dimethyl sulfoxide, dimethylformamide, γ-butyrolactone, 2-methoxyethanol and acetonitrile.

[0172] 2. The ink solution of embodiment 1, further comprising a compound of BX'2, wherein B is at least one divalent metal and X' is a monovalent anion; a compound of formula AX, wherein A is at least one monovalent cation selected from the group consisting of methylammonium, tetramethylammonium, formamidinium, guanidinium, cesium, rubidium, potassium, sodium, butylammonium, phenethylammonium, and phenylammonium; and X is selected from the group consisting of halides, acetates,

[0173] (CH3CO2 - ) and thiocyanate (SCN - ).

[0174] 3. The ink solution according to embodiment 1 or 2, wherein the relative amount of ABX3 to BX'2 and AX is about 99:1.

[0175] 4. The ink solution of any one of embodiments 1 to 3, wherein the two or more solvents are acetonitrile and 2-methoxyethanol.

[0176] 5. The ink solution according to any one of embodiments 1 to 4, wherein the mixed solvent system comprises one or more coordinating solvents selected from the group consisting of dimethyl sulfoxide and dimethylformamide and one or more solvents selected from the group consisting of γ-butyrolactone, 2-methoxyethanol and acetonitrile.

[0177] 6. The ink solution of any one of embodiments 1 to 5, wherein the coordinating solvent is present in an amount of about 0.01 to 10.0 volume percent.

[0178] 7. The ink solution of any one of embodiments 1 to 6, wherein the coordinating solvent is dimethyl sulfoxide.

[0179] 8. The ink solution according to any one of embodiments 1 to 7, wherein the mixed solvent system is a ternary mixed solvent system comprising acetonitrile, 2-methoxyethanol and dimethyl sulfoxide.

[0180] 9. The ink solution according to any one of embodiments 1 to 8, wherein the ternary mixed solvent system comprises 95-99.9 volume % of acetonitrile and 2-methoxyethanol and 0.1-5 volume % of dimethyl sulfoxide.

[0181] 10. The ink solution of any one of embodiments 1 to 9, wherein the composition of formula (I) is selected from the group consisting of cesium lead iodide (CsPbI3), methylammonium tin iodide (CH3NH3SnI3), cesium tin iodide (CsSnI3), methylammonium lead iodide (CH3NH3PbI3), cesium lead bromide (CsPbBr3), methylammonium tin bromide (CH3NH3SnBr3), cesium tin bromide (CsSnBr3), methylammonium lead bromide (CH3NH3PbBr3), formamidinium tin bromide (CHNH2NH2SnBr3), formamidinium lead bromide (CHNH2NH2PbBr3), formamidinium tin iodide (CHNH2NH2SnI3), and formamidinium lead iodide (CHNH2NH2PbI3).

[0182] 11. The ink solution of any one of embodiments 1 to 10, wherein the composition of formula (I) is methylammonium lead iodide (CH3NH3PbI3).

[0183] 12. The ink solution according to any one of embodiments 1 to 11, wherein the at least one divalent metal (B) is selected from the group consisting of lead, tin, cadmium, germanium, zinc, nickel, platinum, palladium, mercury, titanium and silicon.

[0184] 13. The ink solution of any one of embodiments 1 to 12, wherein the at least one divalent metal (B) is lead or tin.

[0185] 14. The ink solution of any one of embodiments 1 to 13, wherein the divalent metal (B) is lead.

[0186] 15. The ink solution of any one of embodiments 1 to 14, further comprising (B) being partially substituted with a metal selected from the group consisting of lithium, sodium, potassium, cesium, rubidium, magnesium, calcium, strontium, barium, antimony, bismuth, arsenic, phosphorus, gallium, indium, thallium, molybdenum, gold, silver, copper, and combinations thereof.

[0187] 16. The ink solution according to any one of embodiments 1 to 15, wherein the monovalent anion (X') is selected from the group consisting of: halide, acetate (CH3CO2 - ) and thiocyanate

[0188] (SCN - ).

[0189] 17. The ink solution of any one of embodiments 1 to 16, wherein the compound of formula BX'2 is selected from the group consisting of PbI2, PbBr2, PbCl2, Pb(CH3CO2)2, SnI2, SnBr2, SnCl2, and Sn(CH3CO2)2.

[0190] 18. The ink solution of any one of embodiments 1 to 17, wherein the compound of formula BX'2 is PbI2.

[0191] 19. The ink solution of any one of embodiments 1 to 18, wherein the compound of formula AX is selected from the group consisting of methylammonium iodide, methylammonium bromide, methylammonium chloride, formamidinium iodide, formamidinium bromide, formamidinium chloride, cesium iodide, cesium bromide, cesium chloride, butylammonium iodide, butylammonium bromide, butylammonium chloride, phenethylammonium iodide, phenethylammonium bromide, phenethylammonium chloride, phenylammonium iodide, phenylammonium bromide, and phenylammonium chloride.

[0192] 20. The ink solution of any one of embodiments 1 to 19, wherein the compound of formula AX is selected from the group consisting of methylammonium iodide, cesium iodide, formamidinium iodide, butylammonium iodide, phenethylammonium iodide, methylammonium bromide, cesium bromide, formamidinium bromide, butylammonium bromide, and phenethylammonium iodide.

[0193] 21. The ink solution of any one of embodiments 1 to 20, wherein the compound of formula AX is methylammonium iodide.

[0194] 22. The ink solution of any one of embodiments 1 to 21, further comprising (A) partial substitution with a metal selected from the group consisting of lithium, magnesium, calcium, strontium, barium, and combinations thereof.

[0195] 23. The ink solution of any one of embodiments 1 to 22, wherein BX'2 is PbI2 and AX is methylammonium iodide.

[0196] 24. The ink solution of any one of embodiments 1 to 23, having a vapor pressure in the range of about 5 kPa to 100 kPa, for use in a rapid coating process, wherein the rapid coating process is selected from the group consisting of: doctor blade coating, slot die coating, shear coating, gravure coating, brush coating, syringe coating, and screen printing.

[0197] 25. A method for producing a polycrystalline perovskite film using the ink solution according to any one of embodiments 1 to 24, the method comprising:

[0198] The ink solution according to any one of Examples 1 to 24 is contacted onto a substrate to form a film using a rapid coating process, wherein the rapid coating process is selected from the group consisting of doctor blade coating, slot die coating, shear coating, gravure coating, brush coating, syringe coating, and screen printing.

[0199] 26. The method of embodiment 25, wherein the contacting the ink solution onto the substrate using the rapid coating process is performed at about 2 mm / s to about 10,000 mm / s.

[0200] 27. The method of embodiment 25 or 26, wherein the contacting the ink solution onto the substrate using the rapid coating process is performed at about 40 mm / s.

[0201] 28. The method of any one of embodiments 25 to 27, wherein the contacting the ink solution onto the substrate using the rapid coating process is performed at about 99 mm / s.

[0202] 29. The method of any one of embodiments 25 to 28, further comprising annealing the film, wherein a polycrystalline perovskite film having a large grain size of about 10 nm to 1 mm is produced.

[0203] 30. The method of any one of embodiments 25 to 29, wherein the membrane produced has an area of ​​at least 25 cm 2 .

[0204] 31. A film comprising a polycrystalline perovskite composition of formula (I):

[0205] ABX3 (I)

[0206] wherein A comprises at least one cation selected from the group consisting of methylammonium, tetramethylammonium, formamidinium, cesium, rubidium, potassium, sodium, butylammonium, phenethylammonium, phenylammonium, and guanidinium;

[0207] B comprises at least one divalent metal; and

[0208] X is at least one halide ion;

[0209] wherein the film of the polycrystalline perovskite composition has a macro grain size in the range of about 10 nm to 1 mm, a thickness in the range of about 10 nm to 1 cm, and a compact, pinhole-free, and uniform structure of at least 25 cm 2 .

[0210] 32. A film according to embodiment 31, wherein the crystalline perovskite composition of formula (I) is selected from the group consisting of: cesium lead iodide (CsPbI3), methylammonium tin iodide (CH3NH3SnI3), cesium tin iodide (CsSnI3), methylammonium lead iodide (CH3NH3PbI3), cesium lead bromide (CsPbBr3), methylammonium tin bromide (CH3NH3SnBr3), cesium tin bromide (CsSnBr3), methylammonium lead bromide (CH3NH3PbBr3), formamidinium tin bromide (CHNH2NH2SnBr3), formamidinium lead bromide (CHNH2NH2PbBr3), formamidinium tin iodide (CHNH2NH2SnI3), and formamidinium lead iodide (CHNH2NH2PbI3).

[0211] 33. A film according to embodiment 31 or 32, wherein the crystalline perovskite composition of formula (I) is methylammonium lead iodide (CH3NH3PbI3).

[0212] 34. A solar cell, a solar panel, a light emitting diode, a photodetector, an x-ray detector, a field effect transistor, a memristor, or a synapse comprising the polycrystalline perovskite film of any one of embodiments 31 to 33.

[0213] 35. A perovskite solar cell unit comprising:

[0214] substrate;

[0215] a first transmission layer disposed on the substrate;

[0216] The film of any one of embodiments 31 to 33, disposed on the first transmission layer;

[0217] a second transmission layer disposed on the film; and

[0218] A conductive electrode is disposed on the second transmission layer.

[0219] 36. A photovoltaic module comprising a plurality of solar cell units according to embodiment 35, wherein the module exhibits a power conversion efficiency of at least 12%.

[0220] 37. The photovoltaic module of embodiment 36, wherein the module exhibits a power conversion efficiency of at least 13%.

[0221] 38. The photovoltaic module of embodiment 36 or 37, wherein the module exhibits a power conversion efficiency of at least 14%.

[0222] 39. The photovoltaic module of any of embodiments 36 to 38, wherein the module exhibits a power conversion efficiency of at least 15%.

[0223] The following examples are offered by way of illustration and not by way of limitation.

[0224] Examples

[0225] Material

[0226] Unless otherwise noted, all chemicals were purchased from Sigma Aldrich and used without further purification. Methylammonium iodide was purchased from Greatcell Solar. Methylammonium hypophosphite was synthesized according to the procedure demonstrated by Xiao et al. (Energy & Environmental Science 9, 867-872 (2016)).

[0227] Device characteristics

[0228] The JV measurements of the perovskite modules were performed with a Keithley 2400 source meter under simulated AM 1.5G radiation generated by a xenon lamp-based solar simulator (Convex Sol3A, AAA class solar simulator). The light intensity was calibrated using a silicon reference cell (Newport 91150V-KG5). The scan rate of the module was 1V / s and was not pre-adjusted before the measurement. In order to measure the long-term operational stability of the perovskite module, the module was encapsulated, illuminated by a daylight equivalent metal halide lamp and loaded at the maximum power point. In order to measure the module efficiency at elevated temperatures, the encapsulated module was placed on a large hot plate and the temperature of the module was measured with an infrared thermometer. The temperature variation over the hole area of ​​the module was less than 5°C. Scanning electron microscopy (SEM) images were obtained using a Quanta 200FEG environmental scanning electron microscope. X-ray diffraction (XRD) patterns were obtained using a Rigaku sixth-generation MiniFlex X-ray diffractometer.

[0229] Example 1: Solvent engineering for perovskite ink solutions

[0230] First, the coordination ability of dimethyl sulfoxide (DMSO), dimethylformamide (DMF), γ-butyrolactone (GBL), 2-methoxyethanol (2-ME) and acetonitrile (ACN) with MAPbI3 was studied. 10,11 It was found that DMSO and DMF react with Pb 2+ The strong coordination of ions can dissolve PbI2. 12 GBL, 2-ME and ACN cannot dissolve PbI2 unless MAI ( Figure 1A ). It should be understood that only after MAI is dissolved can PbI2 pass through PbI3 - The complex is formed by I - Coordination dissolution to Pb 2+ ions, PbI3 was observed for GBL, 2-ME, and ACN:2-ME solutions - The characteristic absorption peak of the complex at 390 nm ( Figure 1B ). 12,13 In contrast, much weaker PbI3 - Instead of applying ACN alone, a mixed solvent of ACN:2-ME was used, because it is understood that the solubility of MAPbI3 in ACN is much lower than that in other solvents (<0.1 M). The above experiments demonstrate that DMSO and DMF have a significant effect on the absorption of Pb 2+ has strong coordination ability, while GBL, 2-ME and ACN:2-ME have no coordination ability or have much weaker coordination ability. Since ACN:2-ME mixed solvents exhibit "non-coordinating" behavior, ACN is also considered to be a "non-coordinating" solvent. It is further observed that 2-ME or ACN:2-ME solvent mixtures exhibit reverse temperature solubility ( Figure 2A , Figure 2B , Figure 2C ), which was also observed in GBL but not in DMF and DMSO. 14,15 This phenomenon further indicates that GBL, 2-ME or ACN have stronger coordination ability than MAI for Pb 2+ Weaker, allowing MAPbI3 to precipitate from the solvent at elevated temperatures. 16 Select the number of donors D N As a quality factor to describe the solvent effect on Pb 2+ coordination ability. 16 I measured in 1,2-dichloroethane - Ion D N is 28.9 kcal / mol, which is similar to the D of DMF and DMSO. NEquivalent, but much larger than 2-ME, ACN, and GBL, 16-18 This is consistent with the results disclosed in this article. Figure 1C The D values ​​of the five solvents were plotted. N For vapor pressure, the graph shows that 2-ME and ACN can act as VNCSs, while DMSO can act as NVCS.

[0231] Example 2: Using N2 knife to examine the effect of solvent on perovskite crystallinity

[0232] Then, room temperature N2-assisted blade coating of perovskite films using VNCS, NVCS, or a combination of both was investigated. Figure 3A and Figure 3D The films coated with 2-ME or ACN:2-ME (3:2 volume ratio) turned black immediately after coating, showing a pure perovskite phase, as shown by Figure 4A and Figure 4C In contrast, when DMSO or DMF was used as the solvent, the film remained wet and required tens of minutes to dry at room temperature. Due to the strong coordination of DMSO or DMF with the perovskite precursor ink material, these films exhibited strong XRD peaks of the intermediate phase below 10°. It should be noted that the drying of the GBL-based solution was also slow, but due to its low coordination ability to GBL (such as that of 2-ME and ACN), the freshly dried film only exhibited a pure perovskite phase. The SEM image of the obtained perovskite film is shown in Figure 5A , Figure 5B , Figure 5C , Figure 5D and Fig. 5F Compared to films coated using DMSO, DMF, or GBL-based solvents, perovskite films coated using solutions of 2-ME or ACN:2-ME solvents are more compact and uniform, although the perovskite grain size is only a few hundred nanometers. Cross-sectional SEM images of these films ( Figure 5G , top image) shows that these perovskite films have poor physical contact with the PTAA-coated ITO substrate, as evidenced by large gaps between the layers. The formation of the gaps can be explained by early solidification on top of the solution.

[0233] After this, a small amount of NCVS (DMSO) was added to the VNCS hosting solvent. Figure 3A ) and XRD patterns ( Figure 4C), the freshly coated films (within hours after knife coating) exhibited a mixture of mesophase and perovskite phases. After annealing at 70°C for 1 minute, the films containing the mixed composition transformed into a pure perovskite phase. These perovskite films exhibited stronger and sharper XRD peaks than those formed without DMSO, with the full width at half maximum (FWHM) of the (110) peak narrowing from 0.104° to 0.089° ( Figure 4D and 4B ). Fig. 5F The SEM images in further show that these films are compact and their large grain size is 1-2 μm in the lateral direction. Figure 5G The cross-sectional SEM images in (bottom image) show that the addition of DMSO also provides good physical contact between the perovskite film and the underlying substrate. However, replacing DMSO with GBL results in a much smaller grain size ( Figure 5E ), suggesting that it is the coordination ability, rather than the low volatility of DMSO, that improves the perovskite crystallinity. The mesophase formed with the coordinating solvent exhibits a larger lattice constant and more solvent. These properties should allow for faster ion transport and therefore a more efficient ripening process during annealing, resulting in larger grain sizes.

[0234] Example 3: Doctor Blade Coating Speed ​​Study

[0235] Figure 6B The allowed blade coating speeds for forming high-quality perovskite films using different solvents or solvent mixtures using an N2 blade-assisted blade coating method are summarized. The N2 blade was operated at a pressure of less than 20 psi. "High quality" refers to uniform and pinhole-free films for module manufacturing. Pure DMSO as a solvent requires very slow coating speeds, less than 2 mm / s. When 2-ME was used as the main solvent, the coating speed increased to up to 40 mm / s. For ACN:2-ME mixed solvent, the coating speed further increased to 99 mm / s, which is the upper limit speed of the blade coater, in the case of adding ACN in a volume ratio of 3:2. Using the latter mixed solvent, the perovskite film was blade-coated at a speed of 99 mm / s on an area of ​​about 225 cm at room temperature. 2 on a flexible glass substrate. For reference, Figure 3B Shows an area of ​​225cm 2 Photographic image of doctor-bladed MAPbI3 film on flexible Corning glass.

[0236] Example 4: Fabrication of perovskite module using N2 knife-assisted doctor blade-coated perovskite film

[0237] The perovskite module was fabricated using N2 blade-assisted perovskite film coating by doctor blade coating. The device structure is indium tin oxide (ITO) / poly (bis (4-phenyl) (2,4,6-trimethylphenyl) amine (PTAA) / MAPbI3 / fullerene (C 60 ) / bathocuproine (BCP) / metal cathode. The PTAA layer was also doctor blade coated, while the other layers were deposited by thermal evaporation.

[0238] Device fabrication

[0239] The pre-patterned ITO / glass substrate was washed sequentially with detergent, deionized water, isopropanol, and acetone, and dried overnight in an oven at 60°C. The PTAA / toluene solution was doctor-coated on the UV-ozone treated ITO / glass substrate at 20 mm / s, with a coating gap of 200 μm. The perovskite layer was then doctor-coated with a nitrogen knife with air blast at room temperature. The solution composition was about 1.0 M MAPbI3 in a mixture solvent consisting of ACN (60% v / v) / 2-ME (40% v / v) for coating at 99 mm / s. The molar ratio of DMSO to MAPbI3 was about 20%. L-α-phosphatidylcholine, methylammonium chloride, and methylammonium hypophosphite were added to the solution as additives at molar percentages of about 0.025%, about 0.8%, and about 1.0% of MAPbI3, respectively. The doctor blade coater was 200-300 μm. The air knife worked below 20.0 psi. The freshly coated solid film was annealed at 70°C for several minutes and then at 100°C for 5-20 minutes. 60 (30nm), BCP (6nm) thermally evaporated perovskite film. Laser scribing is performed twice before and after electrode deposition to complete module manufacturing. For modules sent for certification, polydimethylsiloxane (PDMS) anti-reflective (AR) coating is applied (see Manzoor et al., Solar Energy Materials and Solar Cells 173, 59-65 (2017)).

[0240] A small-area single cell can achieve a high PCE of 21.3%, where V OC is 1.13V, J SC 23.0mA / cm 2 , and FF is 81.8% ( Fig. 7A ). These values ​​highlight the advantages of the knife coating method disclosed herein. 20 Large-area solar modules are then manufactured. Figure 7B The hole area is shown to be 63.7 cm 2The JV curve of the champion module under one day of irradiation shows very little hysteresis. OC ,I SC , FF and PCE values ​​are summarized in the inset table. Figure 7C Efficiency statistics for 18 modules manufactured in series are summarized. Approximately 90% of the modules have an efficiency of 15%-17%, which demonstrates high reproducibility. 7,21 The device uniformity along the transverse direction (parallel to the blade coater) and coating direction was then investigated, as Fig. 8A , Figure 8B and Figure 8C The results show that the distribution of device efficiency is uniform in both the lateral and coating directions. After this, 5 modules were sent to the National Renewable Energy Laboratory (NREL) for certification. All modules showed a stable efficiency above 15.9%, with the champion efficiency being 16.4% ( Fig. 9 ). It should be noted that certification is performed by stabilizing the module near the maximum power point (MPP) for 1 hour. Fig.7D The long-term operational stability of the encapsulated perovskite module is presented. The module was loaded at the MPP and its PCE was measured regularly. After irradiation for more than 1000 h at 1 sun-equivalent light intensity (without UV filter), the module retained 87% of its peak efficiency of 15.8%.

[0241] Example 5: Temperature coefficient of perovskite module

[0242] Temperature coefficient β PCE It is a parameter that characterizes the module efficiency under actual working conditions where the temperature can rise to more than 50°C. Under AM1.5 G irradiation, the temperature coefficient of the perovskite module measured in the temperature range of 25°C to 85°C is -0.13% / °C ( Fig. 7E ). The efficiency loss mainly comes from V OC , whose same coefficient (β Voc ) is -0.13% / ℃, while FF and I SC Almost unchanged ( Fig. 10A , Fig. 10B and Fig. 10C ). When the temperature drops to 25°C, the efficiency of the module remains the same as before the test, without degradation of the perovskite module. This temperature coefficient is smaller than that of CdTe (-0.28% / °C), CIGS (-0.32% / °C) and c-Si (-0.44% / °C), 22 Because of the large V OC But E. g / qV OC Solar cells with comparable deficits generally have smaller betaVoc . 23 At practical operating temperatures above 55°C, the perovskite module exhibits a low temperature coefficient ( Fig. 7E ) appear to be more efficient than silicon modules.

[0243] Example 6: Shading tolerance of perovskite modules

[0244] The shading effect is another factor that limits the performance of PV modules in practical applications. When subcells are connected in series, the shaded subcell blocks the photocurrent of the entire module. The shaded subcell can be burned by bias generated from other subcells to restore the photocurrent output. The maximum breakdown voltage of silicon solar modules is above 15V, 25,26 And the lower breakdown voltage of CdTe and CIGS solar modules is less than 10 V. These solar modules lose more than 50% of their power after breakdown, even if the shaded area is only about 10%. 25,26 Additionally, the breakdown caused permanent damage to the CdTe and CIGS modules and resulted in a 4%-14% PCE loss after 20 s shading. 27,28 Here, the following extreme case is simulated: one subcell in the module is completely shaded while all other subcells are exposed to one sunlight ( Figure 7F , inset). Breakdown of the shaded subcell was observed during 2–4 min of MPP tracking ( Figures 11A-11C ). After the breakdown, the module recovered its power generation with a small power loss of 6.0 relative %, which is proportional to the nominal area reduction (6.25%). This means that the shaded sub-cell does not negatively affect the remaining sub-cells in the perovskite module. To assess the damage, one module was shaded for 4 minutes. When the shading was removed, the module recovered almost 100% of its original power output, indicating that there was no permanent damage. More than 50 shading / de-shading cycles were performed on the same sub-cell of the module. A slight decrease in PCE from 15.7% to 15.1% was observed after the first 20 cycles, and then the module PCE stabilized in subsequent cycles ( Figure 7F and Figures 11A-11C ). Studies on the reverse bias behavior of single perovskite solar cell cells indicate that ion migration will induce tunneling breakdown. 24 This mechanism is supported by the lack of permanent damage after recovery and the low breakdown voltage of about 0.4 V. Ion migration is a unique property in halide perovskites, which helps explain why perovskite solar modules exhibit good shading tolerance relative to other commercial PV modules.

[0245] Example 7: Perovskite module for charging mobile phones

[0246] Figure 3CAn example of a submodule constructed using a perovskite film produced by the method disclosed herein is shown. One such perovskite submodule is used to charge a mobile phone. Fig.13 As shown, a 360cm2 galvanized sheet with a power generation capacity of 5-6W was manufactured. 2 A submodule that matches the power output of a mobile phone charger (e.g., an iPhone charger).

[0247] Example 8: Using an air knife to examine the effect of solvent on perovskite crystallinity

[0248] In addition to the N2-assisted rapid scraping study, the air knife-assisted study was also conducted ( Fig.14A , Fig. 14B and Fig. 14C ). It was found that when the air humidity in the knife was low, there was a negligible difference between the perovskite films dried using an air knife or with a N2 knife. Fig.15A X-ray diffraction (XRD) patterns of freshly obtained film samples dried with an air knife are shown. Samples coated from DMSO or DMF solvents show few perovskite phase peaks, but strong peaks of the intermediate phase containing coordinated solvent molecules. Other samples generated in GBL, 2-ME, and ACN / 2-ME mixed solvents at a volume ratio of 2:1 exhibit pure perovskite phase.

[0249] Perovskite films coated from DMSO, DMF, or GBL solvents did not exhibit the same complete coverage and high uniformity as those coated with 2-ME or ACN / 2-ME based solutions ( Figure 15D-15H ). Similar to what was observed in studies involving N2 knife-assisted drying, the size of the grains was only a few hundred nanometers due to the short growth duration. As mentioned above, the coordinating solvent can compete with MAI for Pb 2+ ion coordination to suppress perovskite formation. However, the slow release of the coordinating solvent can promote prolonged perovskite crystallization and lead to greater crystallinity. Keeping this in mind, a mixed solvent was prepared using ACN / 2-ME as the main solvent and 2.5% v / v DMS as an additive for the perovskite precursor ink. Fig. 15C As shown, the as-coated film appears brown and reflective, and the XRD pattern shows that the film is primarily composed of an intermediate perovskite phase with some minor perovskite phase also present. After annealing at 70°C for several minutes, the film transforms into a pure perovskite phase with greater XRD peak intensity than the film produced without the DMSO additive, demonstrating enhanced crystallinity ( Fig. 15C ). Fig. 15B The SEM image of (bottom right) shows that the film is smooth and consists of large grains of 1-2 μm.

[0250] Similar to what was demonstrated with N2 knife-assisted doctor blade coating, the rapid removal of volatile solvents with the assistance of an air knife can help produce uniform and compact perovskite films in the doctor blade coating process. Despite the use of ACN and 2-ME as highly volatile solvents, the air knife promotes solvent evaporation and assists the spreading of the perovskite ink on the substrate. Fig. 15B As shown in the SEM image in the upper figure, the perovskite film coated without air knife assistance exhibits large gaps and / or pinholes. Fig. 6A The allowed blade coating speeds for obtaining high quality perovskite films with the assistance of an air knife are summarized as a function of different solvents or solvent compositions. As defined above, "high quality" refers to films that are uniform and pinhole-free for module manufacturing. The air knife was operated at a constant pressure of 20 psi. By adding ACN at a volume ratio of 2:1 ACN to 2-ME, the coating speed was increased to 99 mm / s, which, as mentioned above, is the upper limit of the blade coater.

[0251] Example 9: Characterization of air-knife-assisted doctor blade-coated perovskite films in PV modules

[0252] Fabrication of perovskite modules based on rapid blade coating and air knife coating of perovskite films. The device structure was indium tin oxide (ITO) / poly(bis(4-phenyl)(2,4,6-trimethylphenyl)amine (PTAA) / MAPbI3 / fullerene (C60) / bathocuproine (BCP) / chromium / copper. The pre-patterned ITO / glass substrate was washed sequentially with detergent, deionized water, isopropanol, and acetone, and dried overnight in an oven at 60°C. A 3 mg / ml PTAA / toluene solution was doctor-coated on the UV-ozone treated ITO / glass substrate at 20 mm / s, where the coating gap was 200 μm and the solution volume was 6 μl / cm (6 μl per 1 cm substrate width). The perovskite layer was then coated with an air knife with air blowing at room temperature. The module was coated at 99 mm / s, and the solution composition was 0.9 M in a mixture solution consisting of ACN (65% v / v) / 2-ME (32.5% v / v) / DMSO (2.5% v / v). MAPbI3. The gap was 300 μm and the solution volume was 10 μl / cm. The air knife was operated at 20 psi. The freshly coated solid film was annealed at 70°C for several seconds and then at 100°C for 10 minutes. After that, the perovskite film was thermally evaporated with C60, BCP, Cr and Cu in sequence, where laser scribing was performed twice after BCP deposition and Cu deposition to complete the module fabrication.

[0253] Fig.16A The hole area is shown to be 57.2 cm 2 The JV curve of the champion module under one day of irradiation shows very little hysteresis. Fig.16A The Voc, Jsc, FF and PCE values ​​are provided in the table in the inset of FIG. Fig. 16B As shown, the stable photocurrent at the maximum power output point at a bias of 13.6 V is about 63.5 mA, resulting in a stable PCE of 15.1%.

[0254] References

[0255] The references listed below and all references cited in the specification are incorporated herein by reference to the extent that they supplement, explain, provide background or teaching of the methods, techniques and / or compositions employed herein. All cited patents and publications mentioned in this application are expressly incorporated herein by reference.

[0256] 1 Christians, J. A. et al., “Tailored interfaces of unencapsulated perovskite solar cells for>1,000hour operational stability,” Nature Energy, 3, 68 (2018).

[0257] 2Hou, Y. et al., “A generic interface to reduce the efficiency-stability-cost gap of perovskite solar cells,” Science 358, 1192-1197 (2017).

[0258] 3Tan, H. et al., “Efficient and stable solution-processed planar perovskite solar cells via contact passivation,” Science, 355, 722-726 (2017).

[0259] 4 Green, MA et al., “Solar cell efficiency tables (version 50)”, Progress in Photovoltaics: Research and Applications, 25, 668-676 (2017).

[0260] 5Li, Z. et al., “Scalable fabrication of perovskite solar cells,” Nature Reviews Materials 3, 18017 (2018).

[0261] 6 Rong, Y. et al., “Challenges for commercializing perovskite solar cells,” Science 361, eaat8235 (2018).

[0262] 7Chen, H. et al., “A solvent-and vacuum-free route to large-area perovskite films for efficient solar modules,” Nature 550, 92 (2017).

[0263] 8Mayer, J. N., Philipps, S., Hussein, N. S., Schlegl, T., and Senkpiel, C., “Current and future cost of photovoltaics,” in Long-term scenarios for market development, system prices and LCOE of utility-scale PV systems, Fraunhofer ISE, 1-82 (2015).

[0264] 9 Schmela, M. “Global Market Outlook for Solar Power”, 2018–2022. SolarPower Europe (2018).

[0265] 10 Hendriks, KH et al., “2-Methoxyethanol as a new solvent for processing methylammonium lead halide perovskite solar cells,” Journal of Materials Chemistry A 5, 2346-2354 (2017).

[0266] 11Noel, NK et al., “A low viscosity, low boiling point, clean solvent system for the rapid crystallisation of highly specular perovskite films,” Energy & Environmental Science, 10, 145-152 (2017).

[0267] 12 Sharenko, A., Mackeen, C., Jewell, L., Bridges, F., and Toney, M. F., “Evolution of Iodoplumbate Complexes in Methylammonium Lead Iodide Perovskite Precursor Solutions,” Chemistry of Materials 29, 1315–1320 (2017).

[0268] 13Stamplecoskie, KG, Manser, JS, and Kamat, PV, “Dual nature of the excited state in organic–inorganic leadhalide perovskites,” Energy & Environmental Science 8, 208–215 (2015).

[0269] 14Saidaminov, MI et al., “High-quality bulk hybrid perovskite single crystals within minutes by inverse temperature crystallization,” Nature Communications 6, 7586 (2015).

[0270] 15Kadro,JM, Nonomura,K., Gachet,D., M. and Hagfeldt, A., “Facile route to freestanding CH 3 NH 3 PbI 3 crystals using inverse solubility”, Scientific reports 5, 11654 (2015).

[0271] 16Hamill Jr, J.C., Schwartz, J., and Loo, Y.-L., “Influence of Solvent Coordination on Hybrid Organic–Inorganic Perovskite Formation,” ACS Energy Letters 3, 92–97 (2017).

[0272] 17Lau, KW et al., “Solvent, electrolyte and solute shape effects on optical electron transfer in mixed-valence ruthenium ammine dimers,” Inorganica Chimica Acta 226, 137-143 (1994).

[0273] 18Linert, W., Jameson, R. F., and Taha, A., “Donor numbers of anions in solution: the use of solvatochromic Lewis acid–base indicators,” Journal of the Chemical Society, Dalton Transactions, 3181–3186 (1993).

[0274] 19Ding, J. et al., “Fully Air-Bladed High-Efficiency Perovskite Photovoltaics,” Joule, https: / / doi.org / 10.1016 / j.joule.2018.1010.1025 (2018).

[0275] 20Shin, SS et al., “Colloidally prepared La-doped BaSnO3 electrodes for efficient, photostable perovskite solar cells,” Science, 356, 167-171 (2017).

[0276] 21Deng, Y. et al., “Surfactant-controlled ink drying enables high-speed deposition of perovskite films for efficient photovoltaic modules,” Nature Energy, 1 (2018).

[0277] 22Fu, F. et al., “High-efficiency inverted semi-transparent planar perovskite solar cells in substrate configuration,” Nature Energy, 2, 16190 (2017).

[0278] 23Dupré, O., Vaillon, R., and Green, M., “Physics of the temperature coefficients of solar cells,” Solar Energy Materials and Solar Cells, 140, 92–100 (2015).

[0279] 24Bowring, A. R., Bertoluzzi, L., O'Regan, B. C., and McGehee, M. D., "Reverse Bias Behavior of Halide Perovskite Solar Cells," Advanced Energy Materials 8, 1702365 (2018).

[0280] 25 Khaing, HH, Liang, YJ, Htay, NNM, and Fan, J., “Characteristics of different solar PV modules under partial shading,” Int J Electr Comput Electron Commun Eng 8, 1328–1332 (2014).

[0281] 26Tzikas, C. et al., “Do thin film PV modules offer an advantage under partial shading conditions?”, 33rd European Photovoltaic Solar Energy Conference and Exhibition (2017).

[0282] 27Silverman, TJ, Deceglie, MG, Deline, C., and Kurtz, S., “In Reliability of Photovoltaic Cells, Modules, Components, and Systems VIII,” 95630F (International Society for Optics and Photonics).

[0283] 28Silverman, T. J., Mansfield, L., Repins, I., and Kurtz, S., “Damage in Monolithic Thin-Film Photovoltaic Modules Due to Partial Shade,” IEEE Journal of Photovoltaics 6, 1333–1338 (2016).

[0284] Efforts have been made to ensure accuracy with respect to numbers used (eg, amounts, temperature, etc.) but some experimental errors and deviations should be accounted for.

[0285] One skilled in the art will recognize many methods and materials similar or equivalent to those described herein, which can be used to practice the subject matter described herein.The present disclosure is in no way limited to the methods and materials described.

[0286] Unless defined otherwise, technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the subject matter belongs and are consistent with Singleton et al. (1994), Dictionary of Microbiology and Molecular Biology, 2nd ed., J. Wiley & Sons, New York, NY; and Janeway, C., Travers, P., Walport, M., Shlomchik (2001), Immunobiology, 5th ed., Garland Publishing, New York.

[0287] Throughout this specification and claims, unless the context requires otherwise, the words "comprise", "comprises", and "comprising" are used in a non-exclusive sense. It should be understood that the embodiments described herein include embodiments that "consist of" and / or "consist of essentially".

[0288] Where a range of values ​​is provided, it is understood that each intervening value (to one-tenth of the unit of the lower limit) between the upper and lower limits of the range is encompassed, as well as any other stated or intervening value in the range, unless the context clearly dictates otherwise. The upper and lower limits of these smaller ranges that may be independently included in the smaller ranges are also encompassed, subject to any specifically excluded limits in the stated ranges. Where the stated range includes one or both of the limits, ranges excluding either or both of those included limits are also encompassed.

[0289] Many modifications and other embodiments set forth herein will occur to those skilled in the art who have the benefit of the teachings presented in the foregoing description and the associated drawings. Therefore, it should be understood that the subject matter should not be limited to the specific embodiments disclosed, and modifications and other embodiments are intended to be included within the scope of the appended claims. Although specific terms are employed herein, they are used in a general and descriptive sense only and not for purposes of limitation.

Claims

1. An ink solution comprising: The composition of formula (I): ABX3(I) wherein A comprises at least one cation selected from the group consisting of methylammonium, tetramethylammonium, formamidinium, cesium, rubidium, potassium, sodium, butylammonium, phenethylammonium, phenylammonium, and guanidinium; B comprises at least one divalent metal; and X is at least one halide ion; and A mixed solvent system; wherein the mixed solvent system comprises a coordinating solvent selected from the group consisting of dimethyl sulfoxide and dimethylformamide and two solvents selected from the group consisting of gamma-butyrolactone, 2-methoxyethanol and acetonitrile; and wherein the coordinating solvent is present in an amount of 0.01 to 5.0 volume %, wherein the macro-grain size of the film obtained by coating the ink solution is in the range of 1-2 μm.

2. The ink solution according to claim 1, wherein the coordinating solvent is dimethyl sulfoxide. 3 . The ink solution according to claim 1 , wherein the mixed solvent system is a ternary mixed solvent system comprising acetonitrile, 2-methoxyethanol and dimethyl sulfoxide.

4. The ink solution according to claim 3, wherein the ternary mixed solvent system comprises 95-99.9 volume % of acetonitrile and 2-methoxyethanol and 0.1-5 volume % of dimethyl sulfoxide.

5. The ink solution according to claim 1, wherein the composition of formula (I) is selected from the group consisting of cesium lead iodide (CsPbI3), methylammonium tin iodide (CH3NH3SnI3), cesium tin iodide (CsSnI3), methylammonium lead iodide (CH3NH3PbI3), cesium lead bromide (CsPbBr3), methylammonium tin bromide (CH3NH3SnBr3), cesium tin bromide (CsSnBr3), methylammonium lead bromide (CH3NH3PbBr3), formamidinium tin bromide (CHNH2NH2SnBr3), formamidinium lead bromide (CHNH2NH2PbBr3), formamidinium tin iodide (CHNH2NH2SnI3), and formamidinium lead iodide (CHNH2NH2PbI3).

6. The ink solution according to claim 5, wherein the composition of formula (I) is methylammonium lead iodide (CH3NH3PbI3).

7. The ink solution according to claim 1, wherein the at least one divalent metal B is selected from the group consisting of lead, tin, cadmium, germanium, zinc, nickel, platinum, palladium, mercury, titanium and silicon.

8. The ink solution according to claim 1, wherein the at least one divalent metal B is lead or tin.

9. The ink solution according to claim 1, wherein the divalent metal B is lead.

10. The ink solution according to any one of claims 1 to 9, further comprising an additive selected from the group consisting of methylammonium chloride, methylammonium hypophosphite and L-α-phosphatidylcholine.

11. The ink solution of claim 10, wherein the additive is present in a mole percentage ranging from 0.01% to 1.5% relative to the ABX3 composition.

12. The ink solution according to claim 3, wherein the mixed solvent system comprises 97.5 volume % of acetonitrile and 2-methoxyethanol and 2.5 volume % of dimethyl sulfoxide.

13. A method for producing a polycrystalline perovskite film using the ink solution according to claim 1, the method comprising: The ink solution according to claim 1 is contacted onto a substrate to form a film using a rapid coating process, wherein the rapid coating process is selected from the group consisting of doctor blade coating, slot coating, shear coating, gravure coating, brush coating, syringe coating and screen printing.

14. The method of claim 13, wherein the contacting the ink solution onto the substrate using the rapid coating process is performed at 2 mm / s to 10,000 mm / s.

15. The method of claim 13, further comprising annealing the film, wherein a polycrystalline perovskite film having a large grain size of 10 nm to 1 mm is produced.

16. The method of claim 13, wherein the polycrystalline perovskite film produced has an area of ​​at least 25 cm 2 .

17. A film obtained by using the ink solution according to claim 1, comprising a polycrystalline perovskite composition of formula (I): ABX3(I) wherein A comprises at least one cation selected from the group consisting of methylammonium, tetramethylammonium, formamidinium, cesium, rubidium, potassium, sodium, butylammonium, phenethylammonium, phenylammonium, and guanidinium; B comprises at least one divalent metal; and X is at least one halide ion; wherein the film of the polycrystalline perovskite composition has a macro-grain size in the range of 1-2 μm, a thickness in the range of 10 nm to 1 cm, and a compact, pinhole-free, and uniform structure of at least 25 cm 2 .

18. A film according to claim 17, wherein the polycrystalline perovskite composition of formula (I) is selected from the group consisting of: cesium lead iodide (CsPbI3), methylammonium tin iodide (CH3NH3SnI3), cesium tin iodide (CsSnI3), methylammonium lead iodide (CH3NH3PbI3), cesium lead bromide (CsPbBr3), methylammonium tin bromide (CH3NH3SnBr3), cesium tin bromide (CsSnBr3), methylammonium lead bromide (CH3NH3PbBr3), formamidinium tin bromide (CHNH2NH2SnBr3), formamidinium lead bromide (CHNH2NH2PbBr3), formamidinium tin iodide (CHNH2NH2SnI3) and formamidinium lead iodide (CHNH2NH2PbI3).

19. The film of claim 17, wherein the polycrystalline perovskite composition of formula (I) is methylammonium lead iodide (CH3NH3PbI3).

20. A solar cell unit comprising the film of claim 17.

21. A solar panel comprising the film of claim 17.

22. A light emitting diode comprising the film according to claim 17.

23. A photodetector comprising the film of claim 17.

24. An x-ray detector comprising the film of claim 17.

25. A field effect transistor comprising the film of claim 17.

26. A memristor comprising the film of claim 17.

27. A synapse comprising the membrane of claim 17.

28. A perovskite solar cell unit comprising: substrate; a first transmission layer disposed on the substrate; The membrane of claim 17, disposed on the first transmission layer; a second transmission layer disposed on the membrane; as well as A conductive electrode is disposed on the second transmission layer.

29. A photovoltaic module comprising a plurality of perovskite solar cell units according to claim 28, wherein the photovoltaic module exhibits a power conversion efficiency of at least 15%.