Lithium alloy-based electrodes for electrochemical cells and methods of making the same
Through the combination of lithium-aluminum alloy electrodes and anodized aluminum layers, the problems of energy density and cycle life of lithium-ion batteries at low temperatures are solved, achieving efficient electrochemical performance and low-cost battery design.
Patent Information
- Application Number
- CN202010691014.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-17
- Filing Date
- 2020-07-17
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-07-17
AI Technical Summary
When existing lithium-ion batteries work under extreme weather conditions, especially at low temperatures, it is difficult to meet the needs of high energy density, long driving range and fast charging. At the same time, they avoid the use of expensive metals such as cobalt, and traditional electrodes are prone to volume changes. Causes mechanical degradation and reduces cycle life.
Lithium-aluminum alloy is used as the negative electrode electroactive material, combined with an anodized aluminum layer to form a porous structure and an electrode with a lithium concentration gradient. The layer provides mechanical support and ionic conductivity, reducing electrolyte usage. The electrode does not contain a separate current collector and isolation pieces.
It improves the energy density and Coulomb efficiency of lithium-ion batteries, extends cycle life, reduces electrolyte usage, avoids the use of expensive metals, and maintains good performance under low temperature conditions.
Smart Images

Figure CN112242552B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to lithium alloy-based electrodes, electrochemical cells including the lithium alloy-based electrodes, and methods of making the same. Background Art
[0002] This section provides background information related to the present disclosure which is not necessarily prior art.
[0003] High energy density electrochemical cells, such as lithium-ion batteries, can be used in a variety of consumer products and vehicles, such as hybrid or electric vehicles. As technological advances continue to be achieved in terms of battery power, life, and cost, battery-powered vehicles show promise as a transportation option. One factor that potentially limits the wider acceptance and use of battery-powered vehicles is the potentially limited driving range, especially in the early adoption phase where charging stations are not as ubiquitous as today's gas stations. It is desirable to provide batteries that can provide longer driving ranges and shorter charging times. In addition, battery-powered vehicles are often required to operate in extreme weather conditions, such as operating at low temperatures in northern winter weather.
[0004] In the face of these demands, finding an economical battery chemistry that meets both energy and power requirements has been a challenge. There has long been a need for a battery having a chemistry that avoids or minimizes the use of expensive metals such as cobalt and other precious metals while providing advantageous power delivery, long driving range, and fast charging to enhance widespread use of batteries, especially in vehicles. Summary of the invention
[0005] This section provides a general summary of the disclosure, and is not a comprehensive disclosure of its full scope or all of its features.
[0006] In various aspects, the present disclosure provides a negative electrode, the negative electrode comprising a negative electroactive material and a layer. The negative electroactive material comprises a lithium-aluminum alloy. The layer is directly disposed on at least a portion of the negative electroactive material and coupled to the negative electroactive material. The layer comprises anodic aluminum oxide and has a plurality of pores.
[0007] In one aspect, the negative electrode electroactive material defines a body. The layers include a first layer disposed on a first side of the body and a second layer disposed on a second side of the body opposite the first side of the body.
[0008] In one aspect, the body defines a lithium concentration gradient such that a highest molar lithium concentration is disposed in a region of the body adjacent to the layer.
[0009] In one aspect, the body consists essentially of the lithium-aluminum alloy, lithium, aluminum, and electrolyte.
[0010] In one aspect, the layer has a porosity of greater than or equal to about 20% to less than or equal to about 50%. The body has a porosity of less than or equal to about 15%.
[0011] In one aspect, the layer has a thickness of less than or equal to about 10 microns.At least a portion of the plurality of pores extend continuously through the layer to the negative electrode electroactive material.
[0012] In one aspect, the layer further comprises lithium.
[0013] In various aspects, the present disclosure provides an electrochemical cell. The electrochemical cell includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode includes a positive electrode electroactive material. The negative electrode includes a negative electrode electroactive material and a layer. The negative electrode electroactive material includes a lithium-aluminum alloy. The layer is directly disposed on at least a portion of the negative electrode electroactive material and coupled to the negative electrode electroactive material. The layer includes anodized aluminum. The layer includes a plurality of pores. The layer is electrically insulating. The electrolyte is disposed between the positive electrode and the negative electrode such that a portion of the electrolyte is disposed within the plurality of pores of the layer.
[0014] In one aspect, the layer has a thickness greater than or equal to about 5 microns. The layer is configured to act as a separator. The electrochemical cell does not contain a distinct separator component.
[0015] In one aspect, the electrochemical cell further comprises a polymeric membrane separator disposed between the layers of the positive electrode and the negative electrode. The polymeric membrane separator is ionically-conductive and electrically insulating.
[0016] In one aspect, the electrolyte comprises one of: (i) a salt comprising lithium perchlorate and a non-aqueous solvent; (ii) a salt comprising lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, or a combination of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethanesulfonyl)imide and an aqueous, non-aqueous or mixed solvent; or (iii) a salt comprising lithium hexafluorophosphate and an additive or co-solvent comprising fluoroethylene carbonate.
[0017] In one aspect, the electrochemical cell further comprises a positive electrode current collector electrically connected to the positive electrode. The negative electrode electroactive material of the negative electrode is configured to act as a negative electrode current collector. The electrochemical cell does not contain a separate negative electrode current collector assembly.
[0018] In one aspect, the electrolyte is present in the electrochemical cell at greater than or equal to about 10 wt % to less than or equal to about 12 wt %.
[0019] In various aspects, the present disclosure provides a method for manufacturing a negative electrode. The method includes providing an electrode precursor. The electrode precursor comprises a metal selected from the group consisting of aluminum, magnesium, zinc, tin, indium, any alloy thereof, or any combination thereof. The method further includes anodizing a first surface of the electrode precursor to form a layer. The layer comprises a metal oxide. The method further includes lithiating at least a portion of the metal of the electrode precursor to form a negative electrode electroactive material comprising a lithium-metal alloy. The layer is directly disposed on at least a portion of the negative electrode electroactive material and coupled to the negative electrode electroactive material.
[0020] In one aspect, the metal comprises aluminum.The anodizing promotes the formation of a plurality of pores.
[0021] In one aspect, the layer is a first layer, and the anodizing further comprises anodizing a second surface of the electrode precursor to form a second layer comprising the metal oxide.
[0022] In one aspect, the metal comprises aluminum and the electrode precursor consists essentially of the aluminum.
[0023] In one aspect, the electrode precursor comprises a lithium-metal alloy.
[0024] In one aspect, the method further comprises roughening the first surface of the electrode precursor prior to the anodizing.
[0025] In one aspect, the anodizing comprises a reel-to-reel process. The lithiation comprises a reel-to-reel process.
[0026] Further areas of applicability will become apparent from the description provided herein.The description and specific examples in this summary are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The drawings described herein are for illustrative purposes only of selected embodiments and not all possible implementations, and are not intended to limit the scope of the present disclosure.
[0028] Figure 1is a schematic diagram of an electrochemical cell according to various aspects of the present disclosure;
[0029] Figure 2 is a schematic diagram of a negative electrode according to various aspects of the present disclosure;
[0030] Figure 3 is a schematic diagram of another negative electrode according to various aspects of the present disclosure;
[0031] Figure 4 is a schematic diagram of an electrochemical cell according to various aspects of the present disclosure, the electrochemical cell comprising Figure 2 The negative electrode;
[0032] Figure 5 is a schematic diagram of another electrochemical cell according to various aspects of the present disclosure, the electrochemical cell including a separate separator;
[0033] Figure 6 is a schematic diagram of yet another electrochemical cell according to various aspects of the present disclosure, the electrochemical cell comprising a separate negative electrode current collector;
[0034] Figure 7 A method of manufacturing according to various aspects of the present disclosure Figure 2 A schematic diagram of a method for producing a negative electrode;
[0035] Figures 8A-8B is a scanning electron microscope (SEM) image of a surface of an electrode precursor according to various aspects of the present disclosure;
[0036] Figures 9A-9B is a SEM image of a surface of an electrode according to various aspects of the present disclosure;
[0037] Fig.10 is a graph depicting specific capacities of first, second, and third coin cells according to various aspects of the present disclosure;
[0038] Fig.11 It is a depiction Fig.10 a graph of the cycle efficiency of the first, second and third button cells;
[0039] Fig.12 is a graph depicting the charge capacity and discharge capacity of a button cell battery according to various aspects of the present disclosure; and
[0040] Fig.13 It is a depiction Fig.12 A graph of the Coulombic efficiency of a button cell.
[0041] Corresponding reference numerals indicate corresponding parts throughout the several views of the drawings. DETAILED DESCRIPTION
[0042] Exemplary embodiments are provided so that the present disclosure will be thorough and will fully convey its scope to those skilled in the art. Many specific details, such as examples of specific compositions, components, devices and methods, are set forth to provide a full understanding of the embodiments of the present disclosure. It will be apparent to those skilled in the art that specific details need not be used, that the exemplary embodiments may be embodied in many different forms, and that none of them should be considered to limit the scope of the present disclosure. In some exemplary embodiments, well-known methods, well-known device structures, and well-known technologies are not described in detail.
[0043] The terms used herein are intended only to describe specific exemplary embodiments and are not intended to be limiting. Unless the context clearly indicates otherwise, the singular forms "one", "a kind of" and "the" as used herein may be intended to also include plural forms. The terms "comprise", "include", "contain" and "have" are inclusive, thus illustrating the presence of the described features, elements, compositions, steps, integers, operations and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or their collections. Although the open term "comprise" should be understood as a non-limiting term for describing and claiming the various embodiments described herein, in some aspects, the term may be alternatively understood as a more restrictive and limited term, such as "consisting of" or "consisting essentially of". Thus, for any given embodiment of a narration composition, material, component, element, feature, integer, operation and / or process step, the present disclosure also particularly includes an embodiment consisting of or essentially consisting of such a composition, material, component, element, feature, integer, operation and / or process step. In the case of "consisting of," alternative embodiments exclude any additional compositions, materials, components, elements, features, integers, operations and / or process steps, while in the case of "consisting essentially of," any additional compositions, materials, components, elements, features, integers, operations and / or process steps that materially affect the basic and novel characteristics are excluded from such embodiments, but any compositions, materials, components, elements, features, integers, operations and / or process steps that do not materially affect the basic and novel characteristics may be included in the embodiments.
[0044] Any method steps, processes, and operations described herein are not to be construed as necessarily requiring their performance in the particular order discussed or illustrated, unless specifically identified as a certain order of performance. It is also to be understood that additional or alternative steps may be used unless otherwise stated.
[0045] When a part, element or layer is referred to as being "on," "engaged," "connected," or "coupled" to another element or layer, it may be directly on, engaged, connected, or coupled to another part, element or layer, or there may be intermediate elements or layers. Conversely, when an element is referred to as being directly on, "directly engaged," "directly connected," or "directly coupled" to another element or layer, there may be no intermediate elements or layers. Other words used to describe the relationship between elements should be interpreted in a similar manner (e.g., "between" vs. "directly between," "adjacent" vs. "directly adjacent," etc.). As used herein, the term "and / or" includes any and all combinations of one or more of the associated enumerated items.
[0046] Although the terms first, second, third, etc. can be used to describe various steps, elements, components, regions, layers and / or sections in this article, these steps, elements, components, regions, layers and / or sections should not be limited by these terms unless otherwise specified. These terms can only be used to distinguish a step, element, component, region, layer or section from another step, element, component, region, layer or section. Unless clearly stated in the context, terms such as "first", "second" and other numerical terms do not imply order or sequence when used in this article. Therefore, the first step, element, component, region, layer or section discussed below can be referred to as the second step, element, component, region, layer or section without departing from the teaching of exemplary embodiments.
[0047] For ease of description, spatial or temporal relative terms may be used herein, such as "before", "after", "inside", "outside", "below", "beneath", "lower", "upper", etc. to describe the relationship of one element or feature relative to other elements or features shown in the figures. Spatial or temporal relative terms may be intended to include different orientations of a device or system in use or operation in addition to the orientation shown in the figures.
[0048] Throughout this disclosure, numerical values represent approximate measured values or range limits to include slight deviations from given values and embodiments with roughly listed values and embodiments with exactly listed values.Except in the examples provided at the end of the detailed description part, all numerical values of parameters (such as amounts or conditions) in this specification (including the appended claims) should be understood to be modified by the term "about" in all cases, regardless of whether "about" actually appears before the numerical value. "About" means that the numerical value allows certain slight imprecision (some close to the exact value; roughly or reasonably close to the value; almost). If the imprecision provided by "about" is not understood in this art with this common meaning, then "about" used herein at least refers to the variation that may be caused by the common method of measuring and using such parameters.For example, "about" can include less than or equal to 5%, optionally less than or equal to 4%, optionally less than or equal to 3%, optionally less than or equal to 2%, optionally less than or equal to 1%, optionally less than or equal to 0.5% and optionally less than or equal to 0.1% variation in some aspects.
[0049] Additionally, disclosure of ranges includes disclosure of all values within the entire range and further subdivided ranges, including endpoints and subranges given within those ranges.
[0050] Example embodiments will now be described more fully with reference to the accompanying drawings.
[0051] The present technology relates to a rechargeable lithium-ion battery that can be used in vehicle applications. However, the present technology can also be used in other electrochemical devices that circulate lithium ions, such as handheld electronic devices. A rechargeable lithium-ion battery that can exhibit high energy density, low capacity fade, and high coulombic efficiency is provided.
[0052] General electrochemical cell function, structure and composition
[0053] A typical electrochemical cell includes a first electrode, such as a positive electrode or cathode, a second electrode, such as a negative electrode or anode, an electrolyte, and a separator. Typically, in a lithium-ion battery pack, the electrochemical cells are electrically connected in a stack to increase the total output. Lithium-ion electrochemical cells work by reversibly transferring lithium ions between a negative electrode and a positive electrode. A separator and an electrolyte are disposed between the negative electrode and the positive electrode. The electrolyte is suitable for conducting lithium ions and may be in the form of a liquid, gel, or solid. Lithium ions move from the positive electrode to the negative electrode during battery charging and move in the opposite direction when the battery is discharged.
[0054] Each of the negative and positive electrodes within the stack is typically electrically connected to a current collector (e.g., a metal such as copper for the negative electrode and aluminum for the positive electrode). During use of the battery, the current collectors associated with the two electrodes are connected by an external circuit that allows current generated by the electrons to pass between the negative and positive electrodes to compensate for the transport of lithium ions.
[0055] The electrodes are typically incorporated into various commercial battery designs, such as prismatic shaped cells, wound cylindrical cells, button cells, pouch cells, or other suitable battery shapes. The battery may include a single electrode structure of each polarity or a stacked structure having a plurality of positive and negative electrodes assembled in parallel and / or series electrical connection. In particular, the battery may include a stack of alternating positive and negative electrodes with separators disposed therebetween. Although the positive electrode electroactive material can be used in batteries for one-time or single-charge use, the resulting battery typically has the cycle performance required for secondary battery use based on multiple cycles of the battery.
[0056] Figure 1 An exemplary schematic diagram of a lithium-ion battery 20 is shown in FIG. The lithium-ion battery 20 includes a negative electrode 22, a positive electrode 24, and a porous separator 26 (e.g., a microporous or nanoporous polymer separator) disposed between the negative electrode 22 and the positive electrode 24. An electrolyte 30 is disposed between the negative electrode 22 and the positive electrode 24 and in the pores of the porous separator 26. The electrolyte 30 may also be present in the negative electrode 22 and the positive electrode 24, such as in the pores.
[0057] The negative electrode current collector 32 may be arranged at or near the negative electrode 22. The positive electrode current collector 34 may be arranged at or near the positive electrode 24. Although not shown, the negative electrode current collector 32 and the positive electrode current collector 34 may be coated on one or both sides, as known in the art. In some aspects, the current collectors may be coated with an electroactive material / electrode layer on both sides. The negative electrode current collector 32 and the positive electrode current collector 34 collect free electrons and move the free electrons to and from the external circuit 40, respectively. The interruptible external circuit 40 includes a load device 42 connecting the negative electrode 22 (through the negative electrode current collector 32) and the positive electrode 24 (through the positive electrode current collector 34).
[0058] The porous separator 26 works as both an electrical insulator and a mechanical support. More specifically, the porous separator 26 is disposed between the negative electrode 22 and the positive electrode 24 to prevent or reduce physical contact and thus prevent or reduce the occurrence of a short circuit. In addition to providing a physical barrier between the two electrodes 22, 24, the porous separator 26 can also provide a path of least resistance for the internal passage of lithium ions (and associated anions) during lithium ion cycling to facilitate the operation of the lithium ion battery 20.
[0059] The lithium-ion battery 20 can generate current during discharge through a reversible electrochemical reaction that occurs when an external circuit 40 is closed (to electrically connect the negative electrode 22 and the positive electrode 24) when the negative electrode 22 contains a relatively large amount of cyclable lithium. The chemical potential difference between the positive electrode 24 and the negative electrode 22 drives the electrons generated by the oxidation of lithium (e.g., intercalated / alloyed / plated lithium) at the negative electrode 22 to flow to the positive electrode 24 through the external circuit 40. Lithium ions, which are also generated at the negative electrode, are simultaneously transferred through the electrolyte 30 and the porous separator 26 to flow to the positive electrode 24. The electrons flow through the external circuit 40 and the lithium ions migrate through the porous separator 26 in the electrolyte 30 to be intercalated / alloyed / plated into the positive electroactive material of the positive electrode 24. The current through the external circuit 40 can be controlled and directed through the load device 42 until the lithium in the negative electrode 22 is depleted and the capacity of the lithium-ion battery 20 is reduced.
[0060] The lithium ion battery 20 can be charged or recharged at any time by connecting an external power source (e.g., a charging device) to the lithium ion battery 20 to reverse the electrochemical reactions that occur during battery discharge. The connection of the external power source to the lithium ion battery 20 forces the lithium ions at the positive electrode 24 to move back to the negative electrode 22. The electrons, which flow back to the negative electrode 22 through the external circuit 40, and the lithium ions, which are carried by the electrolyte 30 through the separator 26, move back to the negative electrode 22, where they recombine and replenish lithium for consumption during the next battery discharge cycle. In this way, each discharge and charge event is considered a cycle in which lithium ions circulate between the positive electrode 24 and the negative electrode 22.
[0061] The external power source that can be used to charge the lithium-ion battery 20 can vary depending on the size, structure, and specific end use of the lithium-ion battery 20. Some notable and exemplary external power sources include, but are not limited to, an AC power source, such as an AC wall outlet or a motor vehicle alternator. A converter can be used to change from AC to DC to charge the battery 20.
[0062] In many lithium-ion battery configurations, each of the negative electrode current collector 32, the negative electrode 22, the separator 26, the positive electrode 24, and the positive electrode current collector 34 is prepared as a relatively thin layer (e.g., a thickness ranging from a few microns to 1 mm or less) and assembled in layers connected in an electrical series and / or parallel arrangement to provide a suitable electrical energy and power package. In addition, the lithium-ion battery 20 may include various other components, although not shown here, these components are known to those skilled in the art. For example, as a non-limiting example, the lithium-ion battery 20 may include a casing, a gasket, an end cap, a tab, a battery terminal, and any other conventional components or materials that may be located within the battery 20, including between or around the negative electrode 22, the positive electrode 24, and / or the separator 26. As described above, the size and shape of the lithium-ion battery 20 may vary depending on the specific application for which it is designed. Battery-driven vehicles and handheld consumer electronic devices are two examples in which the lithium-ion battery 20 will most likely be designed to different sizes, capacities, and power output specifications. The lithium-ion battery 20 may also be connected in series or in parallel with other similar lithium-ion cells or batteries to produce a greater voltage output, energy, and / or power required by the load device 42 .
[0063] Thus, the lithium-ion battery 20 can generate current to a load device 42 that can be operatively connected to an external circuit 40. Although the load device 42 can be any number of known electrically driven devices, some specific examples of power consuming load devices include, as non-limiting examples, electric motors for hybrid or all-electric vehicles, laptop computers, tablet computers, mobile phones, and cordless power tools or appliances. The load device 42 can also be a power generation device that charges the lithium-ion battery 20 to store energy. In certain other variations, the electrochemical cell can be a supercapacitor, such as a lithium-ion-based supercapacitor.
[0064] Electrolytes
[0065] Any suitable electrolyte 30 capable of conducting lithium ions between the negative electrode 22 and the positive electrode 24, whether in solid, liquid or gel form, can be used in the lithium ion battery 20. In certain aspects, the electrolyte 30 can be a non-aqueous liquid electrolyte solution comprising a lithium salt dissolved in an organic solvent or an organic solvent mixture. Many conventional non-aqueous liquid electrolyte 30 solutions can be used in the lithium ion battery 20. In certain variations, the electrolyte 30 can include an aqueous solvent (i.e., a water-based solvent) or a mixed solvent (e.g., an organic solvent comprising at least 1% by weight water).
[0066] Suitable lithium salts generally have inert anions. Non-limiting examples of lithium salts that can be dissolved in an organic solvent to form a non-aqueous liquid electrolyte solution include lithium hexafluorophosphate (LiPF6); lithium perchlorate (LiClO4); lithium tetrachloroaluminate (LiAlCl4); lithium iodide (LiI); lithium bromide (LiBr); lithium thiocyanate (LiSCN); lithium tetrafluoroborate (LiBF4); lithium difluorooxalatoborate (LiBF2(C2O4))(LiODFB); lithium tetraphenylborate (LiB(C6H5)4); lithium bis-(oxalate)borate (LiB(C2O4)2)(LiBOB); lithium tetrafluorooxalatophosphate ... tetrafluorooxalatophosphate)(LiPF4(C2O4))(LiFOP); lithium nitrate (LiNO3); lithium hexafluoroarsenate (LiAsF6); lithium trifluoromethanesulfonate (LiCF3SO3); lithium bis(trifluoromethanesulfonimide) (LITFSI)(LiN(CF3SO2)2); lithium fluorosulfonyl imide (LiN(FSO2)2)(LIFSI); and combinations thereof. In certain variations, the electrolyte 30 may include a 1M concentration of the lithium salt.
[0067] These lithium salts can be dissolved in various organic solvents, such as organic ethers or organic carbonates, as examples. Organic ethers can include dimethyl ether, glycol dimethyl ether (ethylene glycol dimethyl ether or dimethoxyethane (DME, such as 1,2-dimethoxyethane)), diethylene glycol dimethyl ether (diethylene glycol dimethyl ether or bis (2-methoxyethyl) ether), triethylene glycol dimethyl ether (tri (ethylene glycol) dimethyl ether), other chain structure ethers, such as 1,2-diethoxyethane, ethoxymethoxyethane, 1,3-dimethoxypropane (DMP), cyclic ethers, such as tetrahydrofuran, 2-methyltetrahydrofuran, and combinations thereof. In some variations, the organic ether compound is selected from tetrahydrofuran, 2-methyltetrahydrofuran, dioxolane, dimethoxyethane (DME), diethylene glycol dimethyl ether (diethylene glycol dimethyl ether), triethylene glycol dimethyl ether (tri(ethylene glycol) dimethyl ether), 1,3-dimethoxypropane (DMP), and combinations thereof. Carbonate-based solvents may include various alkyl carbonates, such as cyclic carbonates (e.g., ethylene carbonate, propylene carbonate, butylene carbonate) and non-cyclic carbonates (e.g., dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate (EMC)). Ether-based solvents include cyclic ethers (e.g., tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane) and chain structure ethers (e.g., 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane).
[0068] In various embodiments, in addition to those described above, suitable solvents may be selected from propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, dimethyl sulfoxide, acetonitrile, nitromethane, and mixtures thereof.
[0069] When the electrolyte is a solid electrolyte, it may include a composition selected from the group consisting of LiTi2(PO4)3, LiGe2(PO4)3, Li7La3Zr2O 12 ,Li3xLa 2 / 3 -xTiO3, Li3PO4, Li3N, Li4GeS4, Li 10 GeP2S 12 , Li2S-P2S5, Li6PS5Cl, Li6PS5Br, Li6PS5I, Li3OCl, Li 2.99 Ba 0.005 ClO, or any combination thereof.
[0070] Porous separator
[0071] In certain variations, the porous separator 26 may include a microporous polymer separator comprising a polyolefin, including those prepared from homopolymers (derived from a single monomer component) or heteropolymers (derived from more than one monomer component), which may be linear or branched. In certain aspects, the polyolefin may be polyethylene (PE), polypropylene (PP), or a blend of PE and PP, or a multilayer structured porous film of PE and / or PP. Commercially available polyolefin porous separator 26 membranes include CELGARD ® available from Celgard LLC. ® 2500 (single-layer polypropylene spacer) and CELGARD ® 2340 (three-layer polypropylene / polyethylene / polypropylene separator).
[0072] When the porous separator 26 is a microporous polymer separator, it can be a single layer or a multi-layer laminate. For example, in one embodiment, a single layer of the polyolefin can form the entire microporous polymer separator 26. In other aspects, the separator 26 can be a fibrous membrane having a large number of pores extending between opposing surfaces and can have a thickness of, for example, less than 1 mm. However, as another example, multiple discrete layers of the same or different polyolefins can be assembled to form the microporous polymer separator 26. Instead of or in addition to the polyolefin, the microporous polymer separator 26 can also include other polymers, such as, but not limited to, polyethylene terephthalate (PET), polyvinylidene fluoride (PVdF), polyamide (nylon), polyurethane, polycarbonate, polyester, polyetheretherketone (PEEK), polyethersulfone (PES), polyimide (PI), polyamide-imide, polyether, polyoxymethylene (e.g., acetal), polybutylene terephthalate, polyethylene naphthalate (polyethylenenaphthena te), polybutylene, polymethylpentene, polyolefin copolymers, acrylonitrile-butadiene-styrene copolymers (ABS), polystyrene copolymers, polymethyl methacrylate (PMMA), polysiloxane polymers such as polydimethylsiloxane (PDMS), polybenzimidazole (PBI), polybenzoxazole (PBO), polyphenylenes, polyaryletherketone, polyperfluorocyclobutanes, polyvinylidene fluoride copolymers such as PVdF-hexafluoropropylene or (PVdF-HFP), and polyvinylidene fluoride terpolymers, polyvinyl fluoride, liquid crystal polymers such as VECTRAN TM (Hoechst AG, Germany) and ZENITE® (DuPont, Wilmington, DE)), polyaramides, polyphenylene ethers, cellulosic materials, mesoporous silica, or combinations thereof.
[0073] In addition, the porous separator 26 can be mixed with a ceramic material or its surface can be coated with a ceramic material. For example, the ceramic coating can include aluminum oxide (Al2O3), silicon dioxide (SiO2), or a combination thereof. Various conventionally available polymers and commercial products for forming the separator 26 are contemplated, as well as many manufacturing methods that can be used to produce such microporous polymer separators 26.
[0074] Solid electrolyte
[0075] In various aspects, the porous separator 26 and the electrolyte 30 can be replaced with a solid electrolyte (SSE) that acts as both an electrolyte and a separator. The SSE can be disposed between the positive electrode and the negative electrode. The SSE promotes the transport of lithium ions while mechanically separating the negative electrode 22 and the positive electrode 24 and providing electrical insulation between the negative electrode 22 and the positive electrode 24. As non-limiting examples, the SSE may include LiTi2(PO4)3, LiGe2(PO4)3, Li7La3Zr2O 12 ,Li3xLa 2 / 3 -xTiO3, Li3PO4, Li3N, Li4GeS4, Li 10 GeP2S 12 , Li2S-P2S5, Li6PS5Cl, Li6PS5Br, Li6PS5I, Li3OCl, Li 2.99 Ba 0.005 ClO, or a combination thereof.
[0076] Positive electrode
[0077] The positive electrode 24 may be formed of or include a lithium-based active material that is capable of undergoing lithium insertion and extraction, alloying and alloy degradation, or plating and stripping while serving as a positive terminal of the lithium-ion battery 20. The positive electrode 24 may include a positive electroactive material. The positive electroactive material may include one or more transition metal cations, such as manganese (Mn), nickel (Ni), cobalt (Co), chromium (Cr), iron (Fe), vanadium (V), and combinations thereof. However, in certain variations, the positive electrode 24 is substantially free of selected metal cations, such as nickel (Ni) and cobalt (Co).
[0078] Two exemplary common classes of known electroactive materials that can be used to form the positive electrode 24 are lithium transition metal oxides having a layered structure and lithium transition metal oxides having a spinel phase. For example, in some cases, the positive electrode 24 may include a spinel-type transition metal oxide, such as lithium manganese oxide (Li (1+x) Mn (2-x) O4), where x is usually <0.15, including LiMn2O4 (LMO) and lithium manganese nickel oxide LiMn 1.5 Ni 0.5 In other cases, the positive electrode 24 may include a layered material such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium nickel manganese cobalt oxide (Li(Ni x Mn y Co z)O2), where 0≤x≤1, 0≤y≤1, 0≤z≤1 and x + y + z = 1, including LiMn 0.33 Ni 0.33 Co 0.33 O2, lithium nickel cobalt metal oxide (LiNi (1-x-y) Co x M y O2), where 0<x<1, 0<y<1 and M can be Al, Mn, etc. Other known lithium-transition metal compounds can also be used, such as lithium iron phosphate (LiFePO4) or lithium iron fluoride phosphate (Li2FePO4F). In some aspects, the positive electrode 24 can include an electroactive material containing manganese, such as lithium manganese oxide (Li (1+x) Mn (2-x) O4), mixed lithium manganese nickel oxide (LiMn (2-x) Ni x O4) where 0≤x≤1 and / or lithium manganese nickel cobalt oxide (e.g. LiMn 0.33 Ni 0.33 Co 0.33 In lithium-sulfur batteries, the positive electrode can have elemental sulfur or a sulfur-containing active material as active material.
[0079] The positive electrode electroactive material may be a powder composition. The positive electrode electroactive material may be mixed with an optional conductive material (e.g., conductive particles) and a polymer binder. The binder may both hold the positive electrode electroactive material together and provide ionic conductivity to the positive electrode 24. The polymer binder may include polyvinylidene fluoride (PVdF), poly(vinylidene chloride) (PVC), poly((dichloro-1,4-phenylene)ethylene)), carboxymethyl cellulose (CMC), nitrile rubber (NBR), fluorinated polyurethane, fluorinated epoxide, fluorinated acrylic resin, copolymer of halogenated hydrocarbon polymers, epoxide, ethylene propylene diene terpolymer rubber (EPDM), hexafluoropropylene (HFP), ethylene acrylic acid copolymer (EAA), ethylene vinyl acetate copolymer (EVA), EAA / EVA copolymer, PVDF / HFP copolymer, polyvinylidene fluoride (PVdF), lithium polyacrylate (LiPAA), sodium polyacrylate (NaPAA), sodium alginate, lithium alginate, or a combination thereof.
[0080] The loading of the positive electrode electroactive material in the binder can be large, for example greater than about 80 wt %. For example, the binder can be greater than or equal to about 1 wt % to less than or equal to about 20 wt %, optionally greater than or equal to about 1 wt % to less than or equal to about 10 wt %, optionally greater than or equal to about 1 wt % to less than or equal to about 8 wt %, optionally greater than or equal to about 1 wt % to less than or equal to about 6 wt %, optionally greater than or equal to about 1 wt % to less than or equal to about 7 wt %, optionally greater than or equal to about 1 wt % to less than or equal to about 5 wt %, or optionally greater than or equal to about 1 wt % to less than or equal to about 3 wt % of the binder.
[0081] The conductive material may include graphite, other carbon-based materials, conductive metals, or conductive polymer particles. As a non-limiting example, the carbon-based material may include KETCHEN TM Black, DENKA TM Conductive metal particles may include particles of nickel, gold, silver, copper, aluminum, etc. Examples of conductive polymers include polyaniline, polythiophene, polyacetylene, polypyrrole, etc. In some aspects, a mixture of conductive materials may be used.
[0082] In certain variations, the positive electrode 24 includes the conductive material in an amount of less than or equal to about 15 wt %, optionally less than or equal to about 10 wt %, or optionally greater than or equal to about 0.5 wt % to less than or equal to about 8 wt %. Although the supplemental conductive composition may be described as a powder, these materials lose their powder characteristics after incorporation into the electrode, wherein the associated particles of the supplemental conductive material become components of the resulting electrode structure.
[0083] Negative electrode
[0084] The negative electrode 22 may include a negative electrode electroactive material as a lithium host material capable of serving as a negative terminal of the lithium ion battery 20. Common negative electrode electroactive materials include lithium insertion materials or alloy host materials. These materials may include carbon-based materials such as lithium-graphite intercalation compounds, lithium-silicon compounds, lithium-tin alloys, or lithium titanate Li. 4+x Ti5O 12 , where 0≤x≤3, such as Li4Ti5O 12 (LTO).
[0085] In certain aspects, the negative electrode 22 may comprise lithium, and in certain variations may comprise metallic lithium and a lithium ion battery 20. The negative electrode 22 may be a lithium metal electrode (LME). The lithium ion battery 20 may be a lithium metal battery or cell. Metallic lithium used in the negative electrode of a rechargeable battery has various potential advantages, including having the highest theoretical capacity and the lowest electrochemical potential. Therefore, a battery incorporating a lithium metal anode may have a higher energy density that may potentially double the storage capacity, allowing the battery to be half the size but still last the same amount of time as other lithium ion batteries.
[0086] In certain variations, the negative electrode 22 may optionally include a conductive material, and one or more polymer binder materials to structurally hold the lithium material together. For example, in one embodiment, the negative electrode 22 may include an active material containing lithium metal particles mixed with a binder material selected from: polyvinylidene fluoride (PVdF), ethylene propylene diene monomer (EPDM) rubber, carboxymethyl cellulose (CMC), nitrile rubber (NBR), lithium polyacrylate (LiPAA), sodium polyacrylate (NaPAA), sodium alginate, lithium alginate, or a combination thereof. Suitable additional conductive materials may include carbon-based materials or conductive polymers. As an example, the carbon-based material may include KETCHEN TM Black, DENKA TM The negative electrode 22 may include particles of lithium black, acetylene black, carbon black, etc. Examples of conductive polymers include polyaniline, polythiophene, polyacetylene, polypyrrole, etc. In some aspects, a mixture of conductive materials may be used. The negative electrode 22 may include about 50-100 wt % of an electroactive material (e.g., lithium particles or lithium foil), optionally greater than or equal to about 30 wt % of a conductive material, and the remainder of a binder.
[0087] Electrode manufacturing
[0088] In various aspects, the negative electrode 22 and the positive electrode 24 can be made by mixing the corresponding electroactive materials with a polymer binder compound, a non-aqueous solvent, optionally a plasticizer, and optionally conductive particles if necessary into a slurry. The slurry can be mixed or stirred and then applied thinly to a substrate by a scraper. The substrate can be a removable substrate, or alternatively, it can be a functional substrate, such as a current collector (e.g., a metal grid or mesh layer) attached to one side of the electrode film. In one variation, heat or radiation can be applied to evaporate the solvent from the electrode film, leaving a solid residue. The electrode film can be further consolidated, where heat and pressure are applied to the film to sinter and calender it. In other variations, the film can be dried at a moderate temperature to form a self-supporting film. If the substrate is removable, it is then removed from the electrode film, and the electrode film is then further laminated to the current collector. For either type of substrate, the remaining plasticizer can be extracted before being incorporated into the battery cell. In various aspects, solid electrodes can be formed according to alternative manufacturing methods.
[0089] Optional electrode surface coating
[0090] In certain variations, the prefabricated negative electrode 22 and the positive electrode 24 formed by casting the above-mentioned active material slurry can be directly coated by a vapor phase coating formation process to form a conformal inorganic-organic composite surface coating, as further described below. Thus, one or more exposed areas of the prefabricated negative electrode containing the electroactive material can be coated to minimize or prevent the reaction of the electrode material with the components within the electrochemical cell to minimize or prevent the formation of lithium metal dendrites on the surface of the negative electrode material when incorporated into the electrochemical cell. In other variations, multiple particles containing electroactive materials such as lithium metal can be coated with an inorganic-organic composite surface coating. Then, as described above, the coated electroactive particles can be used in an active material slurry to form a negative electrode.
[0091] Current collector
[0092] The negative electrode 22 and the positive electrode 24 are typically connected to a corresponding negative electrode current collector 32 and a positive electrode current collector 34 to facilitate the flow of electrons between the electrodes and an external circuit 40. The current collectors 32, 34 are conductive and may include metals such as metal foil, metal grids or meshes, or expanded metals. Expanded metal current collectors refer to metal grids with a greater thickness so that a greater amount of electrode material is placed within the metal grid. As non-limiting examples, conductive materials include copper, nickel, aluminum, stainless steel, titanium, alloys thereof, or combinations thereof.
[0093] The positive electrode current collector 34 may be formed of aluminum or any other suitable conductive material known to those skilled in the art. The negative electrode current collector 32 may be formed of copper or any other suitable conductive material known to those skilled in the art. Negative electrode current collectors typically do not contain aluminum because aluminum reacts with lithium, causing large volume expansion and contraction. Drastic volume changes may result in cracking and / or pulverization of the current collector.
[0094] Electrochemical Cells
[0095] In one example, negative electrode 22 includes lithiated aluminum as the negative electrode electroactive material, and positive electrode 24 includes NMC-622 as the positive electrode electroactive material. Electrolyte 30 may be present in negative electrode 22, positive electrode 24, and separator 26. Negative electrode current collector 32 includes copper and positive electrode current collector 34 includes aluminum. The volume and weight percentages of the various components / components are shown in Table 1 below.
[0096] Table 1
[0097] Components Volume Percent Weight Percent Negative electrode 22 21 20 Positive electrode 24 18 39 Isolation member 26 5 2 Electrolyte 30 26 18 Negative electrode current collector 32 1 6 Positive electrode current collector 34 2 2
[0098] Lithium alloy based electrodes
[0099] In various aspects, the present disclosure provides a lithium alloy-based electrode and an electrochemical cell comprising the lithium alloy-based electrode. In some aspects, the electrode may contain a lithium-aluminum alloy as a negative electrode electroactive material, as described below. The electrode includes a negative electrode electroactive material defining a body and a layer disposed on at least one side of the body. The negative electrode electroactive material includes a lithium-metal alloy-based electroactive material, such as a lithium-aluminum alloy. The layer contains a porous metal oxide, such as anodized aluminum. The layer can be electrically insulating. The present disclosure also provides a method for manufacturing a lithium metal alloy-based electrode in various aspects. In some aspects, the layer can be formed during anodization, and the alloy can be formed by pre-lithiation of a metal foil.
[0100] The body of the electrode can be conductive and act as a current collector. Therefore, the electrochemical cell including the lithium metal-based electrode can be free of a separate current collector assembly (e.g., copper foil). In addition, the body can have a low porosity compared to other electroactive materials. The low porosity is conducive to reducing the electrolyte in the electrochemical cell. Compared to an electrochemical cell with a higher porosity electrode connected to a separate current collector assembly, the reduction of electrolyte and the elimination of the current collector lead to an increase in weight and / or volume energy density.
[0101] The pores of the layer can allow fluid communication between the electrolyte and the body, thereby facilitating ion transport. In addition, the layer can be electrically insulating. Therefore, in some aspects, the layer can be used as a separator. The electrochemical cell including the lithium metal-based electrode can be free of a separate separator assembly.
[0102] During the cycle of an electrochemical cell including certain metal-based negative electrodes (e.g., aluminum-based negative electrodes), alloying of lithium with the metal results in large volume expansion and contraction in the electrode. As a result, such a battery may be subject to rupture and / or crushing that may result in a reduced battery cycle life. In some variations, the layer may provide mechanical support to the body during the cycle to reduce or prevent mechanical degradation due to volume changes. In addition, in some aspects, the body may include a lithium gradient formed during pre-lithiation. Due to the gradient, a portion of the body may contain a reduced lithium content or be substantially free of lithium to produce an area with higher strength. The above characteristics may result in an increase in cycle life compared to other electrochemical cells that undergo drastic volume changes.
[0103] Finally, the pre-lithiation process produces lithium storage in the electrode. More particularly, the pre-lithiation produces a stoichiometric excess of lithium within the electrode. The lithium storage can compensate for lithium loss during cycling. Therefore, an electrochemical cell including the pre-lithiated lithium metal alloy-based electrode can have reduced capacity loss compared to a cell that is not pre-lithiated.
[0104] Reference Figure 2 , an electrode 60 according to various aspects of the present disclosure is provided. The electrode 60 includes a body 62 and a layer 64. The body 62 contains an electroactive material, such as a negative electrode electroactive material, which itself can be conductive. Therefore, in addition to promoting electrochemical activity, the body 62 can also act as a current collector. The layer 64 provides mechanical support to the body 62 to reduce or prevent crushing of the body during the cycle of the electrochemical cell including the electrode 60. In addition, the layer 64 can be ionically conductive and electrically insulating. In some aspects, the layer 64 can act as a separator.
[0105] The body 62 and the layer 64 are coupled to each other. More particularly, the body 62 and the layer 64 are integrally formed. The layer 64 is in direct contact with the body 62. The electrode 60 may include a first side 66 and a second side 68 opposite to the first side 66. The layer 64 may extend along at least a portion of the first side 66. In some aspects, the layer 64 may extend substantially along the entire first side 66 of the electrode 60. In some aspects, the body 62 may be a monolithic, substantially planar structure with a length and width significantly greater than a thickness. In various aspects, the body 62 may be described as an electroactive material layer and the layer 64 may be described as a support layer.
[0106] The body 62 includes an electroactive material. The electroactive material may be a negative electroactive material. Thus, as described above, the electrode 60 may be referred to as a negative electrode 60. Figure 7 As will be discussed in more detail in the method of FIG. 6A , the negative electrode electroactive material may be pre-lithiated. Pre-lithiation increases the lithium storage in the body 62. The increased lithium storage compensates for lithium loss during cycling of the electrochemical cell including the negative electrode 60, thereby reducing the magnitude of capacity loss during cycling (see, e.g., FIG. 6B ). Fig.10 and the accompanying text).
[0107] The negative electrode electroactive material comprises a lithium-metal alloy. The negative electrode electroactive material may comprise a lithium-metal alloy, lithium and the metal. The metal may be selected from aluminum, magnesium, zinc, tin, indium, any alloy thereof, or any combination thereof. Thus, the negative electrode electroactive material may comprise a lithium-aluminum alloy, a lithium-magnesium alloy, a lithium-zinc alloy, a lithium-tin alloy, a lithium-indium alloy, any other alloy thereof, or any combination thereof.
[0108] In some aspects, the metal includes aluminum. The negative electrode electroactive material may include a lithium-aluminum alloy. The negative electrode electroactive material may also include lithium and / or aluminum. In some aspects, the negative electrode electroactive material may consist essentially of lithium, aluminum, and their alloys (including any potential impurities). In a further aspect, the negative electrode electroactive material may consist essentially of a lithium-aluminum alloy and aluminum (and any potential impurities), so that substantially all of the lithium has been alloyed with the aluminum. In a further aspect, the negative electrode electroactive material may consist essentially of the lithium-aluminum alloy (and any potential impurities). In various aspects, the molar ratio of aluminum to lithium may be greater than or equal to about 1:10, optionally greater than or equal to 1:1, or optionally greater than or equal to about 10:1. A higher aluminum to lithium ratio results in a greater portion of the lithium, such as substantially all of the lithium, being alloyed with the aluminum rather than plated onto the aluminum. Thus, in certain aspects, the molar ratio of aluminum to lithium can be greater than or equal to about 1:1, optionally greater than or equal to about 2:1, optionally greater than or equal to about 3:1, optionally greater than or equal to about 4:1, optionally greater than or equal to about 5:1, optionally greater than or equal to about 6:1, optionally greater than or equal to about 7:1, optionally greater than or equal to about 8:1, optionally greater than or equal to about 9:1, or optionally greater than or equal to about 10:1.
[0109] The body 62 may have a concentration gradient between the first side 66 and the second side 68. More specifically, the body 62 may include a first molar concentration of lithium adjacent to the first side 66 and a second molar concentration of lithium on the second side 68. The first molar concentration may be greater than the second molar concentration. The molar concentration of lithium may decrease between the first side 66 and the second side 68, as indicated by arrow 70.
[0110] In some aspects, the second molar concentration can be about zero. Thus, the first portion 72 of the body 62 can contain lithium, while the second portion 74 of the body is substantially free of lithium. The first portion 72 can participate in electrochemical activity. The second portion 74 can have a higher strength than the first portion 72. Thus, the second portion 74 can be referred to as a "high strength region". Thus, the concentration gradient can provide a balance between electrochemical activity and mechanical strength. In certain other aspects, both the first portion 72 and the second portion 74 can contain lithium.
[0111] In various aspects, the body 62 has a relatively low porosity compared to other negative electrode electroactive materials (e.g., graphite). The body 62 may have a porosity of greater than or equal to 0% by volume to less than or equal to about 15% by volume, optionally less than or equal to about 10% by volume, optionally less than or equal to about 8% by volume, optionally less than or equal to about 5% by volume, optionally less than or equal to about 4% by volume, optionally less than or equal to about 3% by volume, optionally less than or equal to about 2% by volume, or optionally less than or equal to about 1% by volume. In some aspects, the body 62 may be substantially non-porous.
[0112] Certain electroactive materials, such as aluminum or lithium-aluminum alloys, may be susceptible to cracking and ultimately pulverization due to large volume changes in body 62 during cycling of an electrochemical cell including electrode 60. Cracking and pulverization may result in reduced electrochemical cell cycle life. Pre-lithiated electrode 60 may reduce or prevent cracking and / or pulverization caused by volume changes. In various aspects, layer 64 may provide mechanical support to body 62 to further reduce or prevent cracking and / or pulverization of body 62 during cycling of an electrochemical cell including electrode 60.
[0113] Layer 64 comprises a metal oxide. The metal of the metal oxide is the same as the metal of the lithium-metal alloy. Thus, layer 62 may comprise aluminum oxide (Al2O3), magnesium oxide (MgO), zinc oxide (ZnO), tin oxide (SnO2), indium oxide (In2O3), or a combination thereof. As an example, the aluminum oxide may be an anodic aluminum oxide, such as an anodic nanoporous aluminum oxide. Layer 64 may be ionically conductive and electrically insulating. Thus, in certain aspects, layer 64 may act as a separator, as described below in conjunction with Figure 4 Will be described in more detail.
[0114] In some aspects, layer 64 comprises lithium after pre-lithiation. Thus, layer 64 may comprise a lithium-metal oxide. The metal of the lithium-metal oxide is the same as the metal of the lithium-metal alloy. In one example, the lithium-metal oxide is lithium aluminate (LiAlO2). Layer 64 may be ionically conductive and electrically insulating. In addition, layer 64 may serve as an artificial solid electrolyte interface (SEI) and reduce or prevent electrolyte decomposition.
[0115] Layer 64 may be porous. The pores of layer 64 (see, e.g. Fig. 9B The pores 314 of the layer 64 can facilitate ion transport by providing a path for the electrolyte to contact the body 62. Thus, at least a portion of the pores can extend continuously through the layer 64 to the body 62. In certain aspects, the high porosity can provide a large surface area for the layer 64. The large surface area can facilitate efficient ion transport through the layer 64 between the electrolyte and the body 62.
[0116] In certain aspects, the porosity of layer 64 can be greater than or equal to about 20% by volume to less than or equal to about 70% by volume (e.g., greater than or equal to about 20% by volume to less than or equal to about 30% by volume, greater than or equal to about 30% by volume to less than or equal to about 40% by volume, greater than or equal to about 40% by volume to less than or equal to about 50% by volume, greater than or equal to about 50% by volume to less than or equal to about 60% by volume, greater than or equal to about 60% by volume to less than or equal to about 70% by volume). In certain aspects, the porosity can optionally be greater than or equal to about 25% by volume to less than or equal to about 60% by volume, optionally greater than or equal to about 30% by volume to less than or equal to about 50% by volume, or optionally greater than or equal to about 35% by volume to less than or equal to about 45% by volume. The porosity can be optimized to provide a balance between mechanical strength (favoring lower porosity) and ion transport (favoring higher porosity).
[0117] In certain aspects, the pores of layer 64 can have a size of greater than or equal to about 75 angstroms to less than or equal to about 330 angstroms, optionally greater than or equal to about 100 angstroms to less than or equal to about 300 angstroms, optionally greater than or equal to about 100 angstroms to less than or equal to about 250 angstroms, or optionally greater than or equal to about 125 angstroms to less than or equal to about 225 angstroms. Layer 64 can have a density of greater than or equal to about 0.5 g / cm 3 To less than or equal to about 3.95 g / cm 3 , optionally greater than or equal to about 1 g / cm 3 To less than or equal to about 3g / cm 3 , or optionally greater than or equal to about 2.25 g / cm 3 To less than or equal to about 2.4g / cm 3 (For example, about 2.32 g / cm 3) density. The areal weight of layer 64 may be greater than or equal to about 2.4 mg / cm 3 to less than or equal to about 4.18 mg / cm 3 The roughness of layer 64 may be greater than or equal to about 1 micron to less than or equal to about 4 microns, optionally greater than or equal to about 1.5 microns to less than or equal to about 3 microns, greater than or equal to about 2.1 microns to less than or equal to about 2.3 microns, or optionally about 2.2 microns.
[0118] Layer 64 can define a thickness 80 of less than or equal to about 10 microns, optionally less than or equal to about 8 microns, optionally less than or equal to about 5 microns, or optionally less than or equal to about 3 microns. In one example, thickness 80 is greater than or equal to about 5 microns to less than or equal to about 10 microns. In another example, thickness 80 is greater than or equal to about 2 microns to less than or equal to about 5 microns.
[0119] In various aspects, the electrode 60 can be substantially free of separate binder materials and separate conductive materials (other than the negative electrode electroactive material), such as the above combination Figure 1 Those described. Thus, the body 62 may consist essentially of the electroactive material and the electrolyte disposed in the pores of the body 62. The electrode 60 may consist essentially of the electroactive material, the dielectric, and the layer. In certain aspects, the body 62 is substantially non-porous and the body 62 consists essentially of the electroactive material. Eliminating separate binders and conductive components may contribute to an increase in energy density.
[0120] Reference Figure 3 , another electrode 110 according to various aspects of the present disclosure is provided. The electrode 110 includes a body 112, a first layer 114, and a second layer 116. The first layer 114 can be disposed on a first side 118 of the electrode 110. The second layer 116 can be disposed on a second side 120 of the electrode 110 opposite to the first side 118. In some examples, the electrode 110 is a negative electrode disposed between two positive electrodes.
[0121] Unless otherwise specified, the body 112 may be similar to Figure 2The main body 62 of the electrode 60. In various aspects, the main body 62 can have a molar concentration gradient. More specifically, as shown by arrow 124, the molar lithium concentration can decrease toward the center plane 122 of the electrode 110. In some aspects, the main body 112 can include a first and a second portion 126, 128 containing lithium disposed adjacent to the first and second layers 114, 116, respectively. The main body 112 can further include a third portion 130 that is substantially free of lithium, the third portion 130 being disposed between the first and second portions 126, 128 and including the center plane 122. The third portion 130 can be referred to as a "high-strength region". In certain other aspects, the first, second and third portions 126, 128, 130 all contain lithium.
[0122] The first and second layers 114, 116 can be substantially identical. Each of the first and second layers 114, 116 can be similar to Figure 2 The layer 64 of the electrode 60. When the electrode 110 is in an electrochemical cell or battery stack, it can be disposed between two positive electrodes. Each of the layers 114, 116 can be disposed between the body 112 and the corresponding positive electrode.
[0123] Reference Figure 4 , an electrochemical cell 140 according to various aspects of the present disclosure is provided. The electrochemical cell 140 includes Figure 2 Electrode 60 of the negative electrode 60 serves as a negative electrode. The electrochemical cell 140 further includes a positive electrode 142, a positive electrode current collector 144, and an electrolyte 146. The electrochemical cell 140 is electrically connected to an external circuit 148 through the positive electrode current collector 144 and the body 62 of the negative electrode 60.
[0124] The body 62 of the negative electrode 60 is conductive. In various aspects, the body 62 acts as a current collector within the electrochemical cell 140. The metal of the electrode 60, such as aluminum, can be used as a current collector because the layer 64 provides sufficient mechanical support to reduce or prevent cracking and crushing. Therefore, the body 62 can be electrically connected to the external circuit 148 directly or through a terminal (not shown). Therefore, the electrochemical cell 140 can be free of a separate negative current collector.
[0125] As above combined Figure 1 As described above, electrochemical cells typically include a current collector associated with each respective electrode. Such current collectors increase the overall weight and volume of the battery and may therefore reduce energy density. Certain negative electrode electroactive materials, such as those comprising aluminum, are significantly lighter in weight than copper. For example, the negative electrode 60 may include a current collector having a density greater than or equal to about 1 g / cm 3 To less than or equal to about 2.7g / cm 3Thus, eliminating the copper negative electrode current collector and replacing it with the negative electrode electroactive material of body 62 can result in a significant reduction in the weight of the electrochemical cell. Thus, compared to having a separate separator, such as a separate copper separator (see, e.g., Figure 1 Electrochemical cell 140 may have an improved gravimetric energy density compared to an electrochemical cell having a negative electrode current collector 32 .
[0126] In some aspects, layer 64 can act as a separator and eliminate the need for a separate separator in electrochemical cell 14. Layer 64 can be electrically insulating. Layer 64 can be porous so that it is configured to allow ions to be transported through it. For example, when thickness 80 is greater than or equal to about 5 microns, layer 64 can act as a separator. Therefore, electrochemical cell 140 can be free of a separate separator, such as a microporous polymer separator or a ceramic separator.
[0127] Electrolyte 146 may be present between positive electrode 142 and negative electrode 60. Electrolyte 146 may also be present in the pores of positive electrode 142, pores of layer 64, and pores of body 62, if pores are present. In one example, in a typical electrochemical cell, for example Figure 1 In the lithium-ion battery 20 of the embodiment of the present invention, about one-third of the electrolyte is present in the porous negative electrode. In contrast, the body 62 of the electrode 60 can have a relatively low porosity compared to other negative electrode electroactive materials (e.g., graphite). Therefore, the body 62 can be referred to as dense. The low porosity of the body 62 can contribute to the reduction in the amount of electrolyte 146 used compared to electrochemical cells with other negative electrode electroactive materials. Generally, due to the low porosity of the body 62, the electrochemical cell 140 has an increased weight energy density and an increased volume energy density compared to electrochemical cells with more porous negative electrodes.
[0128] In one example, the electrochemical cell 140 may include electrolyte 146 in an amount of greater than or equal to about 6 wt % to less than or equal to about 16 wt %, greater than or equal to about 8 wt % to less than or equal to about 14 wt %, or optionally greater than or equal to about 10 wt % to less than or equal to about 12 wt %. In another example, to achieve a capacity of about 600 mAh, the electrochemical cell 140 may include an aluminum-lithium alloy as a negative electrode electroactive material and NMC as a positive electrode electroactive material. The electrochemical cell 140 includes about 1.5 grams of electrolyte 146. A reference electrochemical cell (which may be similar to Figure 1 The lithium-ion battery 20) includes graphite as the negative electrode electroactive material and NMC as the positive electrode electroactive material. The reference electrochemical cell contains about 2 grams of electrolyte.
[0129] The positive electrode 142 may include a positive electroactive material, such as a combination of the above Figure 1In some variations, the positive electrode electroactive material may be selected from, for example, lithium nickel manganese cobalt oxide (NMC), lithium nickel cobalt aluminum oxide (NCA), LiFePO4, LiCoO2, LiMnO2, LiMn 1.5 Ni 0.5 O2 or a combination thereof. In some examples, the positive electrode electroactive material may include NMC-622 (LiNi 0.6 Co 0.2 Mn 0.2 O2). The positive electrode 142 can be electrically connected to a positive electrode current collector 144. In some aspects, the positive electrode current collector 144 is disposed at an intermediate position within the positive electrode 142, such as the center of the positive electrode 142. In some optional aspects, the positive electrode current collector 142 can be disposed on an outer side 150 of the positive electrode 142.
[0130] The electrolyte 146 may include a combination of Figure 1 Any composition discussed above for electrolyte 30. In certain variations, electrolyte 146 is substantially free of ethylene carbonate (EC). Thus, electrochemical cell 140 including electrolyte 146 may operate well at lower temperatures, such as those temperatures less than or equal to 20°C.
[0131] Certain combinations of lithium salts and solvents in the electrolyte 146 can contribute to the high coulombic efficiency of the electrochemical cell 140. In one example, the electrolyte 146 includes (i) a salt including lithium perchlorate (LiClO4) and (ii) a non-aqueous solvent (e.g., dimethyl carbonate). In another example, the electrolyte 146 includes (i) a salt including lithium bis(fluorosulfonyl)imide (LiFSI) (F2LiNO4S2), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) (LiC2F6NO4S2), or a combination of LiFSI and LiTFSI and (ii) an aqueous solvent (e.g., water), a non-aqueous solvent (e.g., dimethyl carbonate), or a mixed solvent (e.g., 50 wt% water and 50 wt% dimethyl carbonate). In yet another example, the electrolyte 146 includes (i) a salt including lithium hexafluorophosphate (LiPF6) and (ii) fluoroethylene carbonate (FEC) (C3H3FO3). FEC may be present as an additive or a co-solvent. The solvent may include other organic solvents (e.g., dimethyl carbonate (DMC) (C3H6O3), diethyl carbonate (DEC) (C5H 10 O3)).
[0132] Reference Figure 5, another electrochemical cell 160 according to various aspects of the present disclosure is provided. The electrochemical cell 160 may include a negative electrode 162, a positive electrode 164, a positive electrode current collector 166, an electrolyte 168, and a separator 170. The positive electrode 164 and the positive electrode current collector 166 may be similar to Figure 4 The negative electrode 162 includes a main body 172 and a layer 174. Unless otherwise specified, the main body 172 and the layer 174 may be similar to Figure 2 The body 62 and layer 64 of the negative electrode 60. The electrochemical cell 160 is connected to an external circuit 176. More specifically, the external circuit 176 is electrically connected to the body 172 and the positive electrode current collector 166.
[0133] The separator 170 may be a microporous polymer separator, such as the one described above. Figure 1 In some aspects, separator 170 can be substantially free of ceramic material. Separator 170 can be disposed within electrolyte 146 between negative electrode 162 and positive electrode 164. In some aspects, electrochemical cell 160 can include separator 170 when layer 174 is less than or equal to about 5 microns, optionally less than or equal to about 4 microns, optionally less than or equal to about 3 microns, or optionally less than or equal to about 2 microns. Electrolyte 168 can be similar to Figure 4 of electrolyte 146.
[0134] Reference Figure 6 , yet another electrochemical cell 190 according to various aspects of the present disclosure is provided. The electrochemical cell 190 includes a negative electrode 192, a negative electrode current collector 194, a positive electrode 196, a positive electrode current collector 198, and an electrolyte 200. The positive electrode 196 and the positive electrode current collector 198 may be similar to Figure 4 The positive electrode 164 and the positive electrode current collector 166 of the embodiment of the present invention are provided. The electrolyte 200 may be similar to Figure 4 of electrolyte 146.
[0135] Negative electrode 192 includes body 202 and layer 204. Unless otherwise specified, body 202 and layer 204 may be similar to Figure 2 The body 62 and layer 64 of the electrode 60. However, Figure 2 Unlike the electrode 60 of the main body 202, the negative electrode 192 is electrically connected to a separate negative electrode current collector 194. In some aspects, the negative electrode current collector 194 may include aluminum, lithium-aluminum alloy, magnesium, zinc, indium, gallium, or any combination thereof. The aluminum may have a different form or treatment than the metal (e.g., aluminum) of the main body 202. The negative electrode current collector 194 may be disposed at an intermediate position within the negative electrode 192, such as the center of the negative electrode 192. In some optional variations, the negative electrode current collector 194 may be disposed on the outer side 206 of the negative electrode 192 (similar to Figure 2The electrochemical cell 190 is electrically connected to an external circuit 208 via a negative electrode current collector 194 and a positive electrode current collector 198.
[0136] In various aspects, the present disclosure provides methods of making lithium-metal alloy electrodes and methods of making electrochemical cells including the lithium-metal alloy electrodes. Figure 2 However, those skilled in the art will appreciate that the methods described herein can be similarly applied to other electrodes and electrochemical cells according to various aspects of the present disclosure.
[0137] Reference Figure 7 , the method includes providing a first electrode precursor 220. In some aspects, the first electrode precursor 220 can be a foil. The first electrode precursor 220 can have a substantially planar shape. The first electrode precursor can extend between a first surface 222 and a second surface 224 opposite the first surface 222.
[0138] The first electrode precursor 220 includes a metal. In certain aspects, the first electrode precursor 220 can consist essentially of the metal. The first electrode precursor 220 can include the metal at greater than or equal to about 95 wt %, optionally greater than or equal to about 96 wt %, optionally greater than or equal to about 97 wt %, optionally greater than or equal to about 98 wt %, or optionally greater than or equal to about 99 wt %.
[0139] The metal may be selected from aluminum, magnesium, zinc, tin, indium, any alloy thereof, or any combination thereof. The first electrode precursor 220 may further comprise lithium, for example in the form of a lithium-metal alloy. Thus, as an example, the first electrode precursor 220 may comprise a lithium-aluminum alloy, a lithium-magnesium alloy, a lithium-zinc alloy, a lithium-tin alloy, or any combination thereof. In some aspects, the metal comprises aluminum. In one example, the first electrode precursor 220 consists essentially of aluminum. In another example, the first electrode precursor 220 comprises a lithium-aluminum alloy. The first electrode precursor 220 may consist essentially of the lithium-aluminum alloy.
[0140] In various aspects, the method may optionally include a surface roughening step at 225. More particularly, the first surface 222 of the first electrode precursor 220 may be roughened to form a second electrode precursor 226 having a roughened first surface 228. As an example, the roughening step 225 may include sandblasting, mechanical grinding, plasma etching, or a combination thereof. The roughened first surface 228 may have a roughness greater than or equal to about 0.6 times, optionally greater than or equal to about 0.8 times, optionally greater than or equal to about 1 times, optionally greater than or equal to about 1.2 times, optionally greater than or equal to about 1.4 times, or optionally greater than or equal to about 1.6 times, of the roughness of the first surface 222. The increase in surface area can reduce the current density of the electrode 60 during use in the electrochemical cell. The reduced current density can contribute to improved cycle stability and extended cycle life.
[0141] At 230, the second electrode precursor 226 is anodized to form a third electrode precursor 232. More specifically, the first roughened surface 228 of the second electrode precursor 226 (or the first surface 222 of the first electrode precursor 220 if the roughening step 225 is omitted) is anodized to form a layer precursor 234. The layer precursor 234 includes a metal oxide containing the metal of the first electrode precursor 220. In certain aspects, the porosity and thickness of the layer precursor 234 can be controlled based on one or more of the operating potential, the current density, the concentration of the anodizing solution, the characteristics of the first electrode precursor 220, and the processing steps.
[0142] In various aspects, such as in large-scale manufacturing operations, a roll-to-roll process may be used to continuously anodize the electrode precursor at step 230. In a roll-to-roll process, the thickness of layer 64 may be controlled at least in part by controlling the winding speed.
[0143] The method may proceed to step 240 or step 250. More specifically, the method may proceed to step 240 to pre-lithiate the third electrode precursor 232 and form the electrode 60. However, in order to form a structure similar to Figure 3
[0043] After forming the electrode 100, the method may optionally continue at step 250 to form a second layer precursor 234'.
[0144] At 250, the second surface 224 is anodized to form an optional third electrode precursor 232'. The optional third electrode precursor 232' may include a layer precursor 234 disposed on the first side 66 and another layer precursor 234' disposed on the second side 68. The method may continue at 270.
[0145] At 240, the third electrode precursor 232 is pre-lithiated to form the electrode 60. In various optional aspects, the pre-lithiation at step 240 can be performed before the anodizing step 230. The surface roughening at step 225 can be performed at any point before the anodizing at step 230. During the pre-lithiation, the lithium alloys with the metal to form a body 62 comprising the lithium-metal alloy. In certain aspects, a portion of the lithium can be disposed in the layer 64. For example, the lithium can be bonded to the metal oxide.
[0146] Pre-lithiation can be performed using a half-cell method, a short-circuit method, or other methods. In the half-cell method, the second electrode precursor 232 is used as an electrode and is combined with a lithium foil as another electrode and as described above. Figure 1 The electrolyte pairing described. A constant current is applied to lithiate the second electrode precursor 232. In the short circuit method, a piece of lithium foil with a controlled thickness is placed on the second electrode precursor 232. One or more drops of electrolyte can be added between the lithium foil and the second electrode precursor 232. A current is applied to drive lithium to move toward the metal of the second electrode precursor 232. In another method, lithium and aluminum can be placed in direct contact, or placed in indirect contact through copper foil. A current is applied to drive lithium to move toward the metal of the second electrode precursor 232. In various aspects, the alloying is substantially uniform. The pre-lithiation process can be controlled to achieve a desired thickness, concentration, concentration gradient, and element distribution within the electrode 60.
[0147] In various aspects, forming the electrode 60 further includes forming a lithium concentration gradient in the body 62. In one example, forming the concentration gradient includes lithiation of the reaction substrate at the interface 260 between the body 62 and the layer 64. The reaction substrate is alloyed to form a lithium-metal alloy at the interface 260, such as Li x Al 1-x In the presence of a continuous supply of electrons at the interface 260, lithium ions (Li + ) can be continuously attracted to the reaction substrate. The lithium-metal alloy formed, such as Li x Al 1-x , further alloying can be performed at the interface 260 to produce the highest lithium molar ratio at the interface 260. The method can further include forming a new lithium-metal alloy phase below each previous phase (each subsequent phase is arranged further away from the interface 260 and closer to the second surface 224). As a non-limiting example, the above process can be controlled by changing the lithiation rate. In some aspects, mass diffusion can promote the formation of the concentration gradient. Mass diffusion can be controlled by various processing parameters, including temperature, pressure and / or aging as non-limiting examples.
[0148] In various aspects, such as in large-scale manufacturing operations, a roll-to-roll process can be used to continuously pre-lithiate an electrode precursor. For example, an electric potential (e.g., about 0.05 volts to about 1.5 volts) is applied between the electrode precursor and a lithium metal counter electrode, both of which are embedded in an electrolyte.
[0149] At 270, the optional second electrode precursor 232' is pre-lithiated to form another electrode 60'. The electrode 60' includes a body 62 and layers 64, 64'. The pre-lithiation at 270 may be similar to the pre-lithiation at 240, except that it may be used to form a similar Figure 3 The lithium concentration gradient of the main body 112 of the electrode 110 is a lithium concentration gradient.
[0150] In various aspects, the method can further include forming an electrochemical cell including the electrode 60 or the electrode 60'. The electrochemical cell can be similar to Figure 4 The electrochemical cell 140. Forming the electrochemical cell may include methods known to those skilled in the art.
[0151] Example 1
[0152] Reference Figures 8A-8B , a second electrode precursor 310 according to various aspects of the present disclosure is provided. The second electrode precursor 310 includes a layer precursor 312. The layer 312 includes anodized aluminum and is substantially free of lithium. The layer defines a plurality of pores 314. At least a portion of the pores 314 extend through the entire thickness of the layer precursor 312 to a body (not shown). A surface 316 of the layer precursor 312 may include a plurality of first average size 320 ( Figure 8B ) of structures 318. The hole 314 can be arranged between the structures 318 and surrounded by the structures 318.
[0153] Reference Figures 9A-9B , an electrode 330 according to various aspects of the present disclosure is provided. The electrode 330 is composed of Figures 8A-8B More specifically, the electrode 330 is formed by pre-lithiation. Figures 8A-8B The second electrode precursor 310 is formed, for example, according to Figure 7 method.
[0154] Electrode 330 includes layer 332 and a body (not shown). Layer 332 is formed from layer precursor 312. Thus, layer 332 includes a plurality of pores 334 formed from the plurality of pores 314 and a plurality of structures 336 formed from the plurality of structures 318. At least a portion of pores 334 extend through the entire thickness of layer 332 into the body. Structures 336 define a second average size 338 ( Fig. 9B ).
[0155] During pre-lithiation, the lithium is not plated onto the surface 316, but rather alloys with the aluminum in the bulk, as shown in FIG. Figures 8A-9B In various aspects, the host may have a capacity of about 4 mAh / cm 2 334 and a thickness greater than about 20 microns. A portion of the lithium may also combine with the anodic aluminum oxide of the layer precursor 312 to form a lithium-metal-oxide, such as lithium aluminate (LiAlO2). Therefore, due to the addition of lithium in the layer 332, the second average size 338 can be larger than the first average size 320. The layer 332 maintains the high surface area of the layer precursor 312 during the pre-lithiation process, as defined by the pores 334 and the structure 336. The high surface area of the layer 332 can advantageously promote contact between the electrolyte and the body (e.g., through the pores 334).
[0156] Example 2
[0157] Three button cells were formed. Each button cell included a positive electrode having NMC-622 as the positive electroactive material and an electrolyte comprising 1M LiPF6 in EC-DEC with 10 wt % FEC. The three button cells did not contain a negative electrode current collector.
[0158] The first button cell includes a first negative electrode. The first negative electrode includes aluminum as a negative electrode electroactive material. The first negative electrode does not contain a metal oxide layer and is not pre-lithiated. Therefore, the first button cell can be referred to as a "first electrode precursor" and can be similar to Figure 7 The first electrode precursor 220. The second button cell includes a second negative electrode.
[0159] The second negative electrode includes a body having aluminum as a negative electrode electroactive material and a layer including anodized aluminum. The second negative electrode is not pre-lithiated. Both the body and the layer are substantially free of lithium. Therefore, the second button cell can be referred to as a "third electrode precursor" and can be similar to Figure 7 A third electrode precursor 232 is provided.
[0160] The third button cell includes a third negative electrode. The third negative electrode includes a body having a lithium-aluminum alloy as a negative electrode electroactive material and a layer including anodized aluminum and lithium. Thus, the third button cell may be similar to Figure 2 Electrode 60.
[0161] The button cell was cycled at a rate of C / 10 for two cycles. Fig.10 The x-axis 410 represents the cycle number, and the y-axis 416 represents the cycle number in mAh / cm 2 The unit is the discharge capacity.
[0162] The discharge capacity of the first button cell is shown at 422. The first button cell has no capacity after 15 cycles, as shown at 424. It is believed that the capacity loss is due to mechanical degradation of the first electrode. Mechanical degradation may occur due to comminution caused by large volume changes when lithium alloys with aluminum during cycling.
[0163] The discharge capacity of the second button cell is shown at 426. The second button cell has capacity throughout at least 60 cycles, as shown at 428. The second button cell discharge capacity 426 indicates that the layer can reduce or prevent mechanical degradation, thereby increasing the cycle life of the second button cell when compared to the first button cell.
[0164] The discharge capacity of the third coin cell is shown at 430. After 60 cycles, as shown at 432, the third coin cell still has a discharge capacity of greater than about 3 mAh / cm 2 The third button cell discharge capacity 430 indicates that pre-lithiation can increase the life of the third button cell compared to the first and second button cells. It is believed that the reduction or prevention of lithium storage and / or mechanical degradation in the third negative electrode contributes to the increase in cycle life compared to the first and second button cells. After about 10 cycles, the third button cell discharge capacity 430 is greater than the first button cell discharge capacity 422 and the second button cell discharge capacity 426. In addition, the third button cell shows almost no capacity loss after about 60 cycles.
[0165] Reference Fig.11 , the x-axis 440 represents the number of cycles, and the y-axis 446 represents the coulombic efficiency. The coulombic efficiency of the first button cell is shown at 448. The first button cell coulombic efficiency 448 jumps between about 30% and about 80%. The coulombic efficiency of the second button cell is shown at 450. The second button cell coulombic efficiency 450 is generally greater than about 90%. The coulombic efficiency of the third button cell is shown at 452. The third button cell coulombic efficiency 452 is almost 100% after 60 cycles. It is believed that pre-lithiation promotes the high third button cell coulombic efficiency 452.
[0166] Example 3
[0167] Manufacturing similar to Figure 10-11 For the first part of the test, the button cell was cycled for 8 cycles at C / 10 charge and C / 5 discharge. The first part of the test can be described as a low rate test. For the second part of the test, the button cell was cycled at C / 3.
[0168] Reference Fig.12 , the x-axis 470 represents the cycle number, and the y-axis 472 represents the unit of mAh / cm 2The first portion of the test is shown at 474 and the second portion of the test is shown at 476. The discharge capacity is shown at 480. The button cell exhibits only a minimal drop in capacity between the first and second portions 474, 476 of the test. In addition, the button cell exhibits high rate capability because there is no significant drop in capacity when the rate is changed from C / 10 to C / 5. The ionic conductivity and high surface area of the layer are believed to contribute to the high rate capability.
[0169] Reference Fig.13 , the x-axis 490 represents the number of cycles and the y-axis 492 represents the coulombic efficiency. The first part of the test is indicated by 494 and the second part of the test is indicated by 496. The coulombic efficiency of the button cell is shown at 498. After 32 cycles, the button cell coulombic efficiency 498 is almost 100%.
[0170] The above description of the embodiments has been provided for the purpose of illustration and description. It is not intended to be exhaustive or to limit the present disclosure. Individual elements or features of a particular embodiment are generally not limited to that particular embodiment, but are interchangeable and can be used in selected embodiments when applicable, even if not explicitly shown or described. It can also be changed in many ways. Such changes are not considered to depart from the present disclosure, and all such modifications are intended to be included within the scope of the present disclosure.
[0171] The present disclosure may include the following technical solutions:
[0172] Scheme 1. A negative electrode comprising:
[0173] a negative electrode electroactive material comprising a lithium-aluminum alloy; and
[0174] A layer disposed directly on at least a portion of the negative electrode electroactive material and coupled to the negative electrode electroactive material comprises anodized aluminum oxide and comprises a plurality of pores.
[0175] Option 2. A negative electrode according to Option 1, wherein the negative electrode electroactive material defines a body; and
[0176] The layers include a first layer disposed on a first side of the body and a second layer disposed on a second side of the body opposite to the first side of the body.
[0177] Option 3. A negative electrode according to Option 2, wherein the body defines a lithium concentration gradient such that the highest lithium molar concentration is disposed in a region of the body adjacent to the layer.
[0178] Option 4. A negative electrode according to Option 2, wherein the main body is essentially composed of the lithium-aluminum alloy, lithium, aluminum and electrolyte.
[0179] Scheme 5. The negative electrode according to Scheme 2, wherein
[0180] The layer has a porosity of greater than or equal to about 20% to less than or equal to about 50%; and
[0181] The body has a porosity of less than or equal to about 15%.
[0182] Option 6. The negative electrode according to Option 1, wherein:
[0183] The layer has a thickness of less than or equal to about 10 microns; and
[0184] At least a portion of the plurality of pores extend continuously through the layer to the negative electrode electroactive material.
[0185] Option 7. The negative electrode according to Option 1, wherein the layer further comprises lithium.
[0186] Scheme 8. An electrochemical cell comprising:
[0187] a positive electrode comprising a positive electroactive material;
[0188] A negative electrode comprising
[0189] a negative electrode electroactive material comprising a lithium-aluminum alloy; and
[0190] a layer disposed directly on and coupled to at least a portion of the negative electrode electroactive material, the layer comprising anodized aluminum oxide, comprising a plurality of pores, and being electrically insulating; and
[0191] An electrolyte is disposed between the positive electrode and the negative electrode such that a portion of the electrolyte is disposed within the plurality of pores of the layer.
[0192] Option 9. An electrochemical cell according to Option 8, wherein the layer has a thickness greater than or equal to about 5 microns and is configured to act as a separator such that the electrochemical cell does not contain a separate separator component.
[0193] Option 10. The electrochemical cell according to Option 8, further comprising a polymer membrane separator disposed between the layers of the positive electrode and the negative electrode, the polymer membrane separator being ionically conductive and electrically insulating.
[0194] Option 11. The electrochemical cell according to Option 8, wherein the electrolyte comprises one of the following:
[0195] (i) comprising a salt of lithium perchlorate and a non-aqueous solvent;
[0196] (ii) a salt comprising lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, or a combination of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethanesulfonyl)imide, and an aqueous, non-aqueous or mixed solvent; or
[0197] (iii) A salt comprising lithium hexafluorophosphate and an additive or co-solvent comprising fluoroethylene carbonate.
[0198] Option 12. The electrochemical cell according to Option 8, further comprising a positive electrode current collector electrically connected to the positive electrode, wherein the negative electrode electroactive material of the negative electrode is configured to act as a negative electrode current collector, so that the electrochemical cell does not contain a separate negative electrode current collector component.
[0199] Embodiment 13. The electrochemical cell of Embodiment 12, wherein the electrolyte is present in the electrochemical cell at greater than or equal to about 10 wt % to less than or equal to about 12 wt %.
[0200] Embodiment 14. A method for manufacturing a negative electrode, the method comprising:
[0201] providing an electrode precursor comprising a metal selected from the group consisting of aluminum, magnesium, zinc, tin, indium, any alloy thereof, or any combination thereof;
[0202] anodizing the first surface of the electrode precursor to form a layer, the layer comprising a metal oxide; and
[0203] At least a portion of the metal of the electrode precursor is lithiated to form a negative electroactive material comprising a lithium-metal alloy, the layer being disposed directly on and coupled to at least a portion of the negative electroactive material.
[0204] Option 15. A method according to Option 14, wherein the metal includes aluminum and the anodizing promotes the formation of multiple pores.
[0205] Option 16. A method according to Option 14, wherein the layer is a first layer and the anodizing further comprises anodizing a second surface of the electrode precursor to form a second layer comprising the metal oxide.
[0206] Option 17. A method according to Option 14, wherein the metal includes aluminum and the electrode precursor is essentially composed of the aluminum.
[0207] Option 18. A method according to Option 14, wherein the electrode precursor comprises a lithium-metal alloy.
[0208] Option 19. The method according to Option 14 further includes roughening the first surface of the electrode precursor before the anodizing.
[0209] Option 20. A method according to Option 14, wherein the anodizing comprises a roll-to-roll process and the lithiation comprises a roll-to-roll process.
Claims
1. A negative electrode comprising: a negative electrode electroactive material comprising a lithium-aluminum alloy; and a layer disposed directly on and coupled to at least a portion of the negative electrode electroactive material, the layer comprising anodized aluminum oxide, comprising a plurality of pores, and further comprising lithium; wherein the negative electrode electroactive material defines a body; and The layers include a first layer disposed on a first side of the body and a second layer disposed on a second side of the body opposite to the first side of the body.
2. The negative electrode of claim 1, wherein the body defines a lithium concentration gradient such that a highest lithium molar concentration is disposed in a region of the body adjacent to the layer.
3. The negative electrode of claim 1, wherein the body consists essentially of the lithium-aluminum alloy, lithium, aluminum, and electrolyte.
4. The negative electrode according to claim 1, wherein The layer has a porosity of greater than or equal to 20% to less than or equal to 50%; and The body has a porosity less than or equal to 15%.
5. The negative electrode according to claim 1, wherein: The layer has a thickness less than or equal to 10 microns; and At least a portion of the plurality of pores extend continuously through the layer to the negative electrode electroactive material.
6. An electrochemical cell comprising: a positive electrode comprising a positive electroactive material; A negative electrode comprising a negative electrode electroactive material comprising a lithium-aluminum alloy; and a layer disposed directly on and coupled to at least a portion of the negative electrode electroactive material, the layer comprising anodized aluminum oxide, comprising a plurality of pores, comprising lithium, and being electrically insulating; and an electrolyte disposed between the positive electrode and the negative electrode such that a portion of the electrolyte is disposed within the plurality of pores of the layer; wherein the negative electrode electroactive material defines a body; and The layers include a first layer disposed on a first side of the body and a second layer disposed on a second side of the body opposite to the first side of the body.
7. The electrochemical cell of claim 6, wherein the layer has a thickness greater than or equal to 5 microns and is configured to function as a separator such that the electrochemical cell is free of a separate separator assembly.
8. The electrochemical cell of claim 6, further comprising a polymer membrane separator disposed between the layers of the positive electrode and the negative electrode, the polymer membrane separator being ionically conductive and electrically insulating.
9. The electrochemical cell of claim 6, wherein the electrolyte comprises one of: (i) comprising a salt of lithium perchlorate and a non-aqueous solvent; (ii) a salt comprising lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, or a combination of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethanesulfonyl)imide, and an aqueous, non-aqueous or mixed solvent; or (iii) A salt comprising lithium hexafluorophosphate and an additive or co-solvent comprising fluoroethylene carbonate.
10. The electrochemical cell of claim 6, further comprising a positive electrode current collector electrically connected to the positive electrode, wherein the negative electroactive material of the negative electrode is configured to function as a negative electrode current collector such that the electrochemical cell is free of a separate negative electrode current collector assembly.
11. The electrochemical cell of claim 10, wherein the electrolyte is present in the electrochemical cell at greater than or equal to 10 wt% to less than or equal to 12 wt%.
12. A method for manufacturing a negative electrode, the method comprising: providing an electrode precursor comprising aluminum; anodizing the first surface of the electrode precursor to form a layer, the layer comprising aluminum oxide; and lithiating at least a portion of the aluminum of the electrode precursor to form a negative electrode electroactive material comprising a lithium-aluminum alloy, the layer being disposed directly on and coupled to at least a portion of the negative electrode electroactive material, and the layer further comprising lithium; wherein the anodizing promotes the formation of a plurality of pores; and wherein the layer is a first layer and the anodizing further comprises anodizing a second surface of the electrode precursor to form a second layer comprising the aluminum oxide.
13. The method of claim 12, wherein the electrode precursor consists essentially of the aluminum.
14. The method of claim 12, wherein the electrode precursor comprises a lithium-aluminum alloy.
15. The method of claim 12, further comprising roughening the first surface of the electrode precursor prior to the anodizing.
16. The method of claim 12, wherein the anodizing comprises a roll-to-roll process and the lithiation comprises a roll-to-roll process.