Solid electrolyte for lithium secondary battery and sulfide compound for the solid electrolyte

By using cubic sulfide-germanite sulfide compounds in lithium secondary batteries and adjusting the molar ratio of Cl and Br, high ionic conductivity and low elastic modulus are achieved, solving the problem of high resistance of all-solid-state batteries. , improving the conductivity and cycle characteristics of the battery.

CN112331910BActive Publication Date: 2024-10-18MITSUI MINING & SMELTING CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202011216513.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-07-02
Publication Date
2024-10-18
Estimated Expiration
2038-07-02

AI Technical Summary

Technical Problem

The development of existing all-solid-state lithium secondary batteries with low resistance is limited. In particular, it is difficult to further reduce battery resistance by increasing ion conductivity.

Method used

A sulfide-based compound with a cubic pyrogermanite crystal structure is used, which is represented by the composition formula Li7-xPS6-xClyBrz. By adjusting the molar ratio of Cl and Br, ensure that the molar ratio of Br relative to Cl is within In the range of 0.1 to 10, high ionic conductivity and low elastic modulus are achieved, and the gaps between active material particles are filled by pressing pressure to increase the contact points and contact area of ​​battery electrodes.

Benefits of technology

It effectively reduces the battery resistance, improves the ion conductivity and cycle characteristics of lithium secondary batteries, and is especially suitable for the solid electrolyte of all-solid lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112331910B_ABST
    Figure CN112331910B_ABST
Patent Text Reader

Abstract

The present invention relates to a solid electrolyte for a lithium secondary battery and a sulfide compound for the solid electrolyte. The present invention provides a sulfide compound for a solid electrolyte for a lithium secondary battery, characterized in that it is a novel sulfide compound having a low elastic modulus while maintaining high ion conductivity, and has a crystal phase of a cubic argyrodite-type crystal structure, and has a composition formula of: Li 7‑ x PS 6‑x Cl y Br z Indicates that x in the above composition formula satisfies x=y+z and 1.0
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of Chinese invention patent application 201880042762.4. The application date of Chinese invention patent application 201880042762.4 is July 2, 2018, and the invention name is solid electrolyte for lithium secondary battery and sulfide compound for the solid electrolyte. Technical Field

[0002] The present invention relates to a solid electrolyte for a lithium secondary battery and a sulfide-based compound that can be suitably used as the solid electrolyte. Background Art

[0003] Lithium secondary batteries are secondary batteries with the following structure: when charging, lithium dissolves from the positive electrode in the form of ions, moves to the negative electrode and is embedded, and when discharging, the lithium ions return from the negative electrode to the positive electrode. Lithium secondary batteries have characteristics such as high energy density and long life, so they are widely used as power sources for home appliances such as cameras, portable electronic devices such as notebook computers and mobile phones, power tools and other electric tools, and recently they are also used in large batteries installed in electric vehicles (EVs) and hybrid electric vehicles (HEVs).

[0004] This lithium secondary battery is composed of a positive electrode, a negative electrode, and an ion conductive layer sandwiched by these two electrodes, and the ion conductive layer is generally made of a separator formed of a porous film such as polyethylene or polypropylene filled with a non-aqueous electrolyte. However, since an organic electrolyte using a flammable organic solvent as a medium is used as an electrolyte, improvements are needed not only in the structure / material for preventing volatilization and leakage, but also in the installation of a safety device for suppressing temperature rise during a short circuit and in the structure / material for preventing a short circuit.

[0005] In contrast, the all-solid-state lithium secondary battery formed by using a solid electrolyte and fully solidifying the battery also has the following characteristics: no flammable organic solvent is used, so the simplification of the safety device can be achieved, and not only the manufacturing cost and productivity can be achieved, but also the high voltage can be achieved by stacking in series in the battery. In addition, in this solid electrolyte, except for Li ions, it will not move, so no side reactions caused by the movement of anions are produced, and the improvement of safety and durability can be expected.

[0006] Solid electrolytes used in such batteries are required to have as high ion conductivity as possible and to be chemically / electrochemically stable, and for example, lithium halide, lithium nitride, lithium oxygen salts, or derivatives thereof are known as candidate materials.

[0007] Patent document 1 discloses a lithium ion conductive sulfide ceramic, which is characterized in that it is a sulfide ceramic with high lithium ion conductivity and decomposition voltage, and has Li2S and P2S5 as main components, and has a composition expressed in mol % of Li2S=82.5~92.5 and P2S5=7.5~17.5, among which it is preferred to have a composition in which the molar ratio is Li2S / P2S5=7 (composition formula: Li7PS6).

[0008] Patent Document 2 discloses a lithium ion conductive material having a chemical formula: Li + (12-n-x) B n+ X 2- (6-x) Y - x (B n+ is at least one selected from P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb and Ta, X 2- is at least one selected from S, Se, and Te, Y - It is a argyrodite-type crystal structure shown by at least one selected from F, Cl, Br, I, CN, OCN, SCN and N3, 0≤x≤2).

[0009] Patent Document 3 discloses a lithium argyrodite as a solid compound that can achieve not only high mobility of lithium ions but also single-layer compatibility. The lithium argyrodite is based on the general formula (I): + (12-n-x) B n+ X 2- (6-x) Y - x , in this formula, B n+ is selected from the group consisting of P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb and Ta, X 2- selected from the group consisting of S, Se and Te, Y - Selected from the group consisting of Cl, Br, I, F, CN, OCN, SCN, N3, 0≤x≤2.

[0010] Patent Document 4 discloses a novel sulfide-based solid electrolyte having a Li7PS6 structural framework and containing a composition formula in which a portion of P is replaced with Si: Li 7+x P 1-y Si y S6 (wherein x is -0.6 to 0.6 and y is 0.1 to 0.6) sulfide-based solid electrolyte.

[0011] Patent Document 5 relates to a cubic crystal structure having a space group of F-43m and having a composition formula of: Li 7- x PS 6-x Ha x A compound represented by (Ha is Cl or Br) is disclosed as a sulfide-based solid electrolyte for a lithium secondary battery that can improve the charge and discharge efficiency and cycle characteristics by improving the lithium ion conductivity and reducing the electron conductivity. The sulfide-based solid electrolyte for a lithium secondary battery is characterized in that x in the aforementioned composition formula is 0.2 to 1.8, and the brightness L* value of the L*a*b* colorimetry system is greater than 60.0.

[0012] Patent document 6 relates to a sulfide-based solid electrolyte compound for lithium secondary batteries having a cubic argyrodite-type crystal structure, as a sulfide-based solid electrolyte compound for lithium secondary batteries that can suppress the amount of hydrogen sulfide produced when in contact with the atmosphere and maintain high conductivity even when placed in dry air. A sulfide-based solid electrolyte compound for lithium secondary batteries is disclosed, characterized in that it is composed of a composition formula: Li 7-x+y PS 6- x Cl x+y In the sulfide-based solid electrolyte compound for a lithium secondary battery shown, x and y in the aforementioned composition formula satisfy 0.05≤y≤0.9 and -3.0x+1.8≤y≤-3.0x+5.7.

[0013] In Non-Patent Document 1, a method for preparing Li6PS5Cl by synthesizing Li6PS5Br in Li6PS5Cl by a mechanochemical method and performing a heat treatment to dissolve Li6PS5Br in Li6PS5Cl is described. 1-x Br x The characteristic evaluation when (0≤x≤1) is reported.

[0014] In Non-Patent Document 2, Li6PS5Cl containing two halogens is prepared by a mechanochemical method followed by a heat treatment. 1-x Br x (0≤x≤1) solid solution, and the relationship between its composition and ionic conductivity is reported.

[0015] Prior art literature

[0016] Patent Literature

[0017] Patent Document 1: Japanese Patent Application Publication No. 2001-250580

[0018] Patent Document 2: Japanese Patent Application Publication No. 2011-96630

[0019] Patent Document 3: Japanese Patent Application No. 2010-540396

[0020] Patent Document 4: Japanese Patent Application Publication No. 2013-137889

[0021] Patent Document 5: WO2015 / 012042

[0022] Patent Document 6: WO2016 / 104702

[0023] Non-patent literature

[0024] Non-patent literature 1: Yosuke Ugawa et al. "Study on the preparation method of argyrodite-type Li6PS5X (X = Cl, Br, I) solid electrolyte and its ion conductivity". Technical seminar of the Ceramic Association in January 2015 [1G18].

[0025] Non-patent document 2: Yosuke Ugawa et al., “Characterization of argyrodite-type Li6PS5Cl1-xBrx solid electrolytes”. Electrochemical Society, March 2015 [2H08]. Summary of the invention

[0026] Problem that the invention aims to solve

[0027] It is expected that the resistance of all-solid-state batteries will be further reduced. To date, in order to achieve further resistance reduction of all-solid-state batteries, the development of solid electrolytes with high ion conductivity is underway. However, it is difficult to further develop the resistance reduction of all-solid-state batteries from this point of view alone, so it is necessary to study and try from other angles.

[0028] Therefore, the inventors conducted research and found that if a solid electrolyte material has high crystallinity but low elastic modulus, the solid electrolyte material can be crushed by applying pressing pressure when the electrode is made, so that the gaps between the active material particles can be filled, and the contact points and contact areas with the active material particles can be increased, thereby reducing the battery resistance.

[0029] Sulfide compounds having a cubic argyrodite-type crystal structure generally have high crystallinity and excellent ion conductivity, but are hard and difficult to crush by the pressing pressure during electrode production.

[0030] Therefore, the present invention relates to a sulfide-based compound having a cubic argyrodite-type crystal structure, and proposes a novel sulfide-based compound having a low elastic modulus while maintaining high ion conductivity.

[0031] Solutions for solving problems

[0032] The present invention provides a sulfide-based compound for a solid electrolyte of a lithium secondary battery, which is characterized by having a crystal phase with a cubic thiargyrite-type crystal structure and having a composition formula: Li 7-x PS 6-x Cl y Br z wherein x in the foregoing composition formula satisfies x = y + z and 1.0 < x ≤ 1.8, and the ratio (z / y) of the molar ratio of Br to the molar ratio of Cl is 0.1 to 10.0.

[0033] Effects of the Invention

[0034] The sulfide-based compound provided by the present invention has a crystal phase with a cubic thiargyrite-type crystal structure and has a composition formula: Li 7-x PS 6-x Cl y Br z In the sulfide-based compound shown, on the basis that the total molar ratio of Cl and Br is greater than 1.0, the ratio of the molar ratio of Br to the molar ratio of Cl is specified within a specified range, whereby a high ionic conductivity can be maintained, a low elastic modulus can be achieved, and the battery resistance can be reduced. For example, when using the foregoing sulfide-based compound provided by the present invention as a solid electrolyte to fabricate an electrode, if a pressing pressure is applied, the solid electrolyte is crushed so as to be able to fill the gaps between the active material particles, and the contact points and contact area with the active material particles can be increased, whereby the battery resistance can be reduced. Therefore, the sulfide-based compound provided by the present invention is particularly suitable for use as a solid electrolyte of a lithium secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 (a) in is a SEM photograph (5000 times) obtained by observing the sulfide-based compound (sample) obtained in Example 4 with a scanning electron microscope (SEM), and (b) is a SEM photograph (5000 times) obtained by granulating the sulfide-based compound (sample) obtained in Example 4 under a pressure of 200 MPa and observing its cross section with a scanning electron microscope.

[0036] Figure 2 (a) in is a SEM photograph (5000 times) obtained by observing the sulfide-based compound (sample) obtained in Comparative Example 1 with a scanning electron microscope (SEM), and (b) is a SEM photograph (5000 times) obtained by granulating the sulfide-based compound (sample) obtained in Comparative Example 1 under a pressure of 200 MPa and observing its cross section with a scanning electron microscope. DETAILED DESCRIPTION OF THE INVENTION

[0037] The embodiments of the present invention will be described in detail below, but the scope of the present invention is not limited to the embodiments described below.

[0038] <The present solid electrolyte>

[0039] The sulfide-based solid electrolyte of one example of the present embodiment (referred to as "the present solid electrolyte") contains a crystal phase having a cubic argyrodite-type crystal structure and has a composition formula (1): Li 7-x PS 6-x Cl y Br z A solid electrolyte for a lithium secondary battery comprising a sulfide-based compound represented by (x=y+z) (referred to as "the present sulfide-based compound").

[0040] <The present sulfide compound>

[0041] The sulfide compound has a cubic argyrodite crystal structure and is composed of the following formula (1): Li 7-x PS 6-x Cl y Br z The compounds shown.

[0042] Whether or not the crystal phase has a cubic argyrodite type crystal structure can be confirmed by, for example, analyzing using an X-ray diffraction method (XRD, Cu ray source) as described later.

[0043] In the above composition formula (1), the total molar ratio x (=y+z) of Cl and Br preferably satisfies 1.0 <x≤1.8。

[0044] When the total molar ratio x (=y+z) of Cl and Br is greater than 1.0 and less than 1.8, the ion conductivity can be further improved, which is preferred. In particular, when x is less than 1.8, the generation of heterogeneous phases can be controlled, and the decrease in ion conductivity can be suppressed.

[0045] From such a viewpoint, x in the composition formula (1) is preferably greater than 1.0 and 1.8 or less, more preferably 1.1 or more and 1.7 or less, and particularly preferably 1.2 or more and 1.6 or less.

[0046] In the above composition formula (1), the ratio (z / y) of the molar ratio of Br to the molar ratio of Cl is preferably 0.1-10.

[0047] When the ratio (z / y) of the molar ratio of Br to the molar ratio of Cl is 0.1 or more, the solid electrolyte has a low elastic modulus and is therefore preferred. On the other hand, when the (z / y) is 10 or less, the ion conductivity is high and is therefore preferred.

[0048] From such a viewpoint, the ratio of the molar ratio of Br to the molar ratio of Cl (z / y) is preferably 0.1 to 10, more preferably 0.2 or more or 5 or less, and particularly preferably 0.3 or more or 3 or less.

[0049] In the above composition formula (1), y representing the molar ratio of Cl preferably satisfies 0.3≤y≤1.5.

[0050] When the molar ratio y of Cl is 0.3 or more, the ion conductivity can be further improved compared with less than 0.3, which is preferred. On the other hand, when it is 1.5 or less, the elastic modulus can be maintained at a low level, which is preferred.

[0051] From such a viewpoint, y in the composition formula (1) is preferably 0.3 to 1.5, more preferably 0.4 or more and 1.2 or less, and particularly preferably 0.6 or more and 1.0 or less.

[0052] In the above composition formula (1), z representing the molar ratio of Br preferably satisfies 0.3≤z≤1.5.

[0053] When the molar ratio z of Br is 0.3 or more, the elastic modulus can be further reduced, which is preferred. On the other hand, when it is 1.5 or less, the ion conductivity can be maintained, which is preferred.

[0054] In addition, since the Br compound has a lower melting point than the Cl compound, the addition of the Br compound increases the reactivity and makes it easier to synthesize the sulfide-based compound.

[0055] From such a viewpoint, z in the composition formula (1) is preferably 0.3 to 1.5, more preferably 0.4 or more and 1.2 or less, and particularly preferably 0.6 or more and 1.0 or less.

[0056] The present solid electrolyte only needs to contain the present sulfide-based compound, and therefore may contain other materials and components.

[0057] Therefore, the present solid electrolyte may be the present solid electrolyte formed as follows: comprising a single phase, wherein the single phase is composed of a crystalline phase of a cubic argyrodite-type crystal structure; formed by a mixed phase of a crystalline phase containing a cubic argyrodite-type crystal structure and a crystalline phase represented by LiCl; formed by a mixed phase of a crystalline phase containing a cubic argyrodite-type crystal structure and a crystalline phase represented by LiBr; formed by a mixed phase of a crystalline phase containing a cubic argyrodite-type crystal structure, a crystalline phase represented by LiCl, and a crystalline phase represented by LiBr.

[0058] It should be noted that the mixed phase containing a crystalline phase of a cubic argyrodite type crystal structure and a crystalline phase represented by LiCl and / or LiBr includes, in addition to the mixed phase of a crystalline phase of a cubic argyrodite type crystal structure and a crystalline phase represented by LiCl and / or LiBr, a case where it contains crystalline phases other than these.

[0059] In addition, examples of the other materials include other solid electrolyte materials, Li2S, Li3PS4, Li4P2S6, etc. However, the present invention is not limited to these.

[0060] However, the present solid electrolyte preferably uses the present sulfide-based compound as the main material, and preferably the present sulfide-based compound accounts for more than 50 mass %, more than 80 mass %, or more than 90 mass % (including 100 mass %) of the entire solid electrolyte, and it is particularly ideal that it is composed only of the present sulfide-based compound.

[0061] Furthermore, the present solid electrolyte may contain, in addition to the above-mentioned other materials, inevitable impurities in an amount that has little adverse effect on the effects of the present invention, for example, less than 5% by mass, particularly less than 3% by mass.

[0062] (Particle size)

[0063] The solid electrolyte is preferably in the form of powdered particles, and the average particle size (D50) of the solid electrolyte, that is, the average particle size (D50) determined by laser diffraction scattering particle size distribution measurement, is preferably 0.1 μm to 10 μm.

[0064] When D50 is 0.1 μm or more, there will be no increase in resistance due to the increase in the surface of the solid electrolyte particles, and there will be no difficulty in mixing with the active material, so it is preferred. On the other hand, when D50 is 10 μm or less, the solid electrolyte becomes easy to enter the gap between the active materials, and the contact point and contact area become larger, so it is preferred.

[0065] From such a viewpoint, the average particle size (D50) of the present solid electrolyte is preferably 0.1 μm to 10 μm, more preferably 0.3 μm or more and 7 μm or less, and particularly preferably 0.5 μm or more and 5 μm or less.

[0066] The average particle size (D50) of the solid electrolyte is preferably 1 to 100% of the average particle size (D50) of the positive electrode active material or the average particle size (D50) of the negative electrode active material.

[0067] When the average particle size (D50) of the solid electrolyte is 1% or more of the average particle size (D50) of the positive electrode active material or the average particle size (D50) of the negative electrode active material, it is possible to fill the active material gaps without gaps, so it is preferred. On the other hand, when it is less than 100%, the active material ratio in the electrode becomes high, which is preferred from the perspective of high energy density of the battery.

[0068] From the above viewpoint, the average particle size (D50) of the present solid electrolyte is preferably 1 to 100% of the average particle size (D50) of the positive electrode active material or the average particle size (D50) of the negative electrode active material, wherein it is further preferably 3% or more or 50% or less, and particularly preferably 5% or more or 30% or less.

[0069] (Elastic modulus)

[0070] The Young's modulus of the present solid electrolyte is preferably 1 GPa to 30 GPa.

[0071] When the Young's modulus of the present solid electrolyte is 1 GPa or more, it is not easy to aggregate and is easy to manufacture, so it is preferred. On the other hand, when the Young's modulus of the present solid electrolyte is 30 GPa or less, it will be crushed at the interface with the active material to increase the contact area, so it is preferred.

[0072] From such a viewpoint, the Young's modulus of the present solid electrolyte is preferably 1 GPa to 30 GPa, more preferably 5 GPa or more and 28 GPa or less, and particularly preferably 10 GPa or more and 25 GPa or less.

[0073] When the Young's modulus of the present solid electrolyte is adjusted to the above range, it is preferred to perform a heat treatment at 450 to 600° C. (material temperature), particularly 450 to 500° C., while flowing hydrogen sulfide (H 2 S) gas.

[0074] (Ionic conductivity)

[0075] Sulfide-based solid electrolytes are known to have excellent ion conductivity and are more likely to form a good contact state with active materials at room temperature than oxides, which can reduce interface resistance. Among them, the present solid electrolyte can maintain ion conductivity and achieve a low elastic modulus.

[0076] (Manufacturing method)

[0077] Next, an example of a method for producing the present sulfide-based compound and / or the present solid electrolyte will be described. However, the production method described here is only an example and is not limited to this method.

[0078] The present sulfide-based compound and / or the present solid electrolyte can be obtained, for example, by mixing and calcining lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder, lithium chloride (LiCl) powder and lithium bromide (LiBr) powder.

[0079] As a method for mixing the raw materials, for example, pulverization and mixing using a ball mill, a bead mill, a homogenizer, or the like is preferred.

[0080] At this time, regarding the pulverization and mixing, if the crystallinity of the raw material powder is reduced or the raw material powder is made amorphous or the raw material mixed powder is homogenized by very strong mechanical pulverization and mixing such as mechanical alloying, the bond between the cation and sulfur is cut off, sulfur defects are generated during calcination, and electronic conductivity is exhibited. Therefore, it is ideal to pulverize and mix to a degree that can maintain the crystallinity of the raw material powder.

[0081] After mixing as described above, the mixture is dried as necessary, and then calcined in an inert atmosphere or under a flow of hydrogen sulfide gas (H2S), and crushed and pulverized as necessary, and classified to obtain the mixture.

[0082] The present sulfide-based compound crystallizes from about 200°C, and can therefore be synthesized even at relatively low calcination temperatures. Therefore, by calcining at 350°C or higher in an inert atmosphere or under the flow of hydrogen sulfide gas (H2S), the present sulfide-based compound having a chemical composition with substantially no sulfur deficiency can be produced.

[0083] Among them, when hydrogen sulfide gas is used during calcination, sulfur gas generated by decomposition of hydrogen sulfide during calcination can increase the sulfur partial pressure near the calcined sample, so sulfur defects are less likely to be generated even at high calcination temperatures, and electronic conductivity can be reduced. Therefore, when calcining in an atmosphere containing hydrogen sulfide gas, the calcination temperature is preferably set to 350 to 650°C, particularly preferably 450°C or higher or 600°C or lower, and particularly preferably 500°C or lower.

[0084] On the other hand, when calcining in an inert atmosphere, unlike the case of hydrogen sulfide gas, the sulfur partial pressure near the calcined sample cannot be increased during calcination, so sulfur defects are easily generated at high calcination temperatures, and the electronic conductivity becomes high. Therefore, when calcining in an inert atmosphere, the calcination temperature is preferably set to 350 to 500°C, particularly preferably 350°C or higher or 450°C or lower, and particularly preferably 400°C or higher or 450°C or lower.

[0085] It should be noted that the raw material powder is usually allowed to react completely to eliminate the unreacted phase, so it is preferred to calcine at 450°C or above while circulating hydrogen sulfide gas. However, when using a raw material powder with a small particle size and high reactivity, the reaction is promoted even at a low temperature, so calcination can be performed in an inert atmosphere.

[0086] Furthermore, the above raw materials are extremely unstable in the air and react with moisture to decompose, generate hydrogen sulfide gas, or oxidize. Therefore, it is preferred to place the raw materials in a furnace and calcine them in a glove box replaced with an inert gas atmosphere.

[0087] By manufacturing in this way, the generation of sulfur defects can be suppressed and the electronic conductivity can be reduced. Therefore, when the present sulfide-based compound is used as a solid electrolyte to produce an all-solid-state lithium secondary battery, the charge and discharge characteristics and cycle characteristics as battery characteristics can be improved.

[0088] In the method for manufacturing the present sulfide-based compound and / or the present solid electrolyte, when the Young's modulus of the present sulfide-based compound and / or the present solid electrolyte is adjusted to less than 30 GPa, it is preferred to mix a lithium (Li)-containing compound, a phosphorus (P)-containing compound, a sulfur (S)-containing compound, a chlorine-containing compound and a bromine-containing compound, dry them as needed, then calcine them at 450 to 600°C (material temperature), especially 450 to 500°C (material temperature) under the circulation of hydrogen sulfide gas (H2S), and crush and classify them as needed.

[0089] Examples of the compound containing lithium (Li) include lithium compounds such as lithium sulfide (Li 2 S), lithium oxide (Li 2 O), and lithium carbonate (Li 2 CO 3 ), and lithium metal alone.

[0090] Examples of the compound containing phosphorus (P) include phosphorus sulfides such as phosphorus trisulfide (P2S3) and phosphorus pentasulfide (P2S5), phosphorus compounds such as sodium phosphate (Na3PO4), and simple phosphorus.

[0091] Examples of the compound containing sulfur (S) include the above-mentioned lithium sulfide and phosphorus sulfide.

[0092] As chlorine-containing compounds, for example, LiCl, PCl3, PCl5, POCl3, P2Cl4, SCl2, S2Cl2, NaCl, BCl3 and the like can be cited.

[0093] Examples of bromine-containing compounds include LiBr, PBr 3 , POBr 3 , S 2 Br 2 , NaBr, and BBr 3 .

[0094] Among them, a combination of lithium sulfide, phosphorus sulfide, lithium chloride and lithium bromide is preferred.

[0095] In this production method, the raw materials are preferably mixed by pulverizing and mixing using a ball mill, a bead mill, a homogenizer, or the like, rather than a mixing method that applies a strong mechanical stress using a planetary ball mill or the like.

[0096] Furthermore, the above raw materials are extremely unstable in the air and react with moisture to decompose, generate hydrogen sulfide gas, or oxidize. Therefore, it is preferred to place the raw materials in a furnace and calcine them in a glove box replaced with an inert gas atmosphere.

[0097] <Application of the present solid electrolyte>

[0098] The present solid electrolyte can be used as a solid electrolyte layer of an all-solid-state lithium secondary battery, a solid electrolyte mixed in a positive electrode / negative electrode composite material, and the like.

[0099] For example, an all-solid-state lithium secondary battery can be constructed by forming a positive electrode, a negative electrode, and a layer containing the above-mentioned solid electrolyte between the positive electrode and the negative electrode.

[0100] In this case, the present solid electrolyte has excellent water resistance and oxidation resistance, and its characteristics are rarely deteriorated even when handled in dry air, so that, for example, the assembly operation of the all-solid lithium secondary battery can be performed in a dry room or the like.

[0101] Here, the layer containing the solid electrolyte can be prepared, for example, by the following methods: dripping a slurry formed by a solid electrolyte, a binder and a solvent onto a substrate and scraping it with a scraper or the like; making the substrate contact with the slurry and then cutting it with an air knife; forming a coating by screen printing or the like, and then removing the solvent by heating and drying, etc. Alternatively, the solid electrolyte powder can be made into a pressed powder by pressing or the like, and then processed appropriately.

[0102] As the positive electrode material, the positive electrode material used as the positive electrode active material of the lithium secondary battery can be suitably used. As the positive electrode active material, for example, spinel-type lithium transition metal oxides, lithium transition metal oxides with a layered structure, or olivine, or a mixture of two or more thereof can be listed.

[0103] As the negative electrode material, a negative electrode material used as a negative electrode active material for a lithium secondary battery can be preferably used.

[0104] For example, since the present solid electrolyte is electrochemically stable, it can also be used at a low potential (about 0.1 V vs Li) comparable to that of lithium metal. + / Li) is charged and discharged by artificial graphite, natural graphite, and carbon-based materials such as difficult graphitization carbon (hard carbon) as the negative electrode active material of the lithium secondary battery. Therefore, by using this solid electrolyte as the electrolyte of the lithium secondary battery and using carbon-based materials as the negative electrode active material, the energy density of the all-solid-state lithium secondary battery can be greatly improved. Therefore, it is possible to constitute a lithium secondary battery having, for example, this solid electrolyte and a negative electrode active material containing carbon such as artificial graphite, natural graphite, and difficult graphitization carbon (hard carbon).

[0105] In addition, silicon active materials, which are promising high-capacity negative electrode materials, can also be used as negative electrode active materials for lithium secondary batteries.

[0106] In all-solid-state batteries, it is believed that the silicon active material greatly expands and contracts during repeated charge and discharge, and therefore it is extremely difficult to maintain contact with the solid electrolyte.

[0107] If the present solid electrolyte is used as an electrolyte for a lithium-ion all-solid-state battery, since the present solid electrolyte has a low Young's modulus, i.e., a low elastic modulus, it can deform following the expansion and contraction of the silicon active material, and the effect of improving the cycle characteristics can be expected. Therefore, for example, a lithium secondary battery having the present solid electrolyte and a silicon-based negative electrode active material can be constructed.

[0108] <Method for producing a lithium secondary battery electrode using the present solid electrolyte>

[0109] For example, the present solid electrolyte, the negative electrode active material, and other materials such as a conductive aid and a binder as necessary are mixed and compressed to form into a predetermined shape such as a plate, thereby producing a negative electrode.

[0110] Alternatively, for example, the present solid electrolyte, the positive electrode active material, and other materials such as a conductive additive and a binder as required may be mixed and compressed to form into a predetermined shape such as a plate, thereby producing a positive electrode.

[0111] <Explanation of terms>

[0112] In the present invention, "solid electrolyte" refers to a material that can maintain a solid state and allow ions, such as Li + All matter that moves.

[0113] In the present invention, the term "lithium secondary battery" broadly includes a secondary battery that is charged and discharged by transferring lithium ions between a positive electrode and a negative electrode.

[0114] In the present invention, when described as "X to Y" (X and Y are arbitrary numbers), unless otherwise specified, it includes not only the meaning of "X or more and Y or less" but also the meaning of "preferably greater than X" or "preferably less than Y".

[0115] In addition, in the case of being described as "X or more" (X is any number) or "Y or less" (Y is any number), it includes the intention of "preferably greater than X" or "preferably less than Y".

[0116] Examples

[0117] Hereinafter, the present invention will be described based on examples. However, the present invention is not limited to these for interpretation.

[0118] <Examples 1 to 5 / Comparative Examples 1 to 3>

[0119] In such a manner as to achieve the raw material composition (mol%) shown in Table 1, lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder, lithium chloride (LiCl) powder, and lithium bromide (LiBr) powder were used, and each component was weighed so that the total amount became 75 g, and pulverized and mixed for 6 hours using a ball mill to prepare a mixed powder. This mixed powder was filled into a carbon container, and while flowing hydrogen sulfide gas (H2S, purity 100%) at 1.0 L / minute in a tubular electric furnace, it was heated at a temperature increase / decrease rate of 200 °C / hour and calcined at 500 °C for 4 hours. Then, the sample was crushed with a mortar and sized with a sieve having a mesh size of 53 μm to obtain a powdery sample (sulfide-based compound as a solid electrolyte).

[0120] At this time, all of the above weighing, mixing, setting in the electric furnace, taking out from the electric furnace, crushing, and sizing operations were carried out inside a glove box replaced with sufficiently dried Ar gas (dew point -60 °C or lower).

[0121] <Example 6>

[0122] The flowing gas was changed to argon, and the calcination temperature was changed to 450 °C. Otherwise, the operation was the same as above to obtain a powdery sample (sulfide-based compound). The raw material composition is shown in Table 1.

[0123] <Determination of composition>

[0124] Regarding the samples (sulfide-based compounds) obtained in the examples / comparative examples, the composition was determined by ICP emission spectrometry, and the values of x, y, z, and (z / y) in the composition formula: Li 7-x PS 6-x Cl y Br z are shown in Table 1.

[0125] <X-ray diffraction>

[0126] The powdery samples (solid electrolytes) obtained in the examples / comparative examples were analyzed by X-ray diffraction method (XRD, Cu ray source) to determine the generated phase.

[0127] The samples obtained in Examples 1 to 5 were single phases composed of a crystalline phase with a cubic thiogermanate crystal structure, and high crystallinity was confirmed.

[0128] <Measurement of average particle size>

[0129] For the powdery samples (solid electrolytes) obtained in the Examples / Comparative Examples, using an automatic sample feeder (manufactured by Nikkiso Co., Ltd., "Microtorac SDC") of a laser diffraction particle size distribution measuring device, the sample (powder) was put into a non-aqueous solvent, the flow rate was set to 40%, after irradiating ultrasonic waves of 40 W for 360 seconds, the particle size distribution was measured using a laser diffraction particle size distribution measuring machine "MT3000II" manufactured by Nikkiso Co., Ltd., and the average particle size (D50) was measured based on the obtained volume-based particle size distribution graph.

[0130] It should be noted that the non-water-soluble solvent during measurement passed through a 60-μm filter, the refractive index of the solvent was set to 1.50, the particle permeability condition was set to permeable, the refractive index of the particles was set to 1.59, the shape was set to non-spherical, the measurement range was set to 0.133 to 704.0 μm, the measurement time was set to 30 seconds, and the average value of two measurements was used as D50.

[0131] <Observation of SEM photographs>

[0132] For the sulfide-based compound (sample) obtained in the Examples / Comparative Examples, granulation was carried out by applying a pressure of 200 MPa assuming pressing compression during electrode formation, and the cross-section was observed with a scanning electron microscope (SEM). Based on the obtained SEM photograph (5000 times), it was judged as "〇: good" or "×: poor" according to the following criteria. It should be noted that in the case of non-evaluation, it was recorded as "-".

[0133] 〇: The case where the sulfide-based compound was crushed was observed.

[0134] ×: The case where the sulfide-based compound was not crushed was not observed.

[0135] <Measurement of Young's modulus>

[0136] For the powdery samples (sulfide-based compounds) obtained in the Examples / Comparative Examples, using an atomic force microscope (AFM) (manufactured by Bruker, "Dimension Icon"), force curve measurement was carried out, and the elastic modulus (Young's modulus) was obtained from the obtained force curve.

[0137] In a glove box under an Ar atmosphere, the specimen was spread on a silicon wafer thinly coated with epoxy resin and fixed to be used as a measurement specimen.

[0138] As the measurement conditions, the Ramp mode (force curve measurement mode) was used to measure the force curve of 10 particles per one sample.

[0139] The sample was measured after adjusting the measurement parameters so as to calculate a predetermined value using a known standard sample (glass: elastic modulus 72 GPa).

[0140] The measurement environment was set to an Ar atmosphere (oxygen concentration <0.1 ppm, water concentration <0.1 ppm) at 25° C., and a diamond probe (DNISP-HS) manufactured by Bruker was used as the measurement probe.

[0141] The obtained force curve was fitted using DMTmodel to derive the damped Young's modulus. Based on the relationship between the damped Young's modulus and the Young's modulus of the sample, the Poisson's ratio was set to 0.3 to derive the Young's modulus of the sample.

[0142] Formula 1

[0143]

[0144] In the above formula 1, F: force applied to the cantilever, Fadh: adsorption force, E * : damping Young's modulus, R: cantilever curvature radius, d-d0: distance between cantilever and sample.

[0145] Formula 2

[0146]

[0147] In the above formula 2, E * : Damping Young's modulus, E s : Young's modulus of the sample, v s : Poisson's ratio of the sample.

[0148] It should be noted that when the Young's modulus is measured by a compression test represented by an indentation method, it is difficult to distinguish between the aggregation force of secondary particles formed by the aggregation of primary particles and the original elastic modulus of the primary particles. The ease of disentanglement of the secondary particles is dominant, so it is difficult to measure the actual elastic modulus of the particles.

[0149] On the other hand, when the Young's modulus is measured by the above-mentioned method adopted in the examples of the present invention, the value of the particle surface is calculated, and therefore the original elastic modulus of the particle can be measured.

[0150] <Measurement of ionic conductivity>

[0151] The samples (sulfide compounds) obtained in the examples / comparative examples were uniaxially pressed at a pressure of 200 MPa in a glove box purged with sufficiently dry Ar gas (dew point -60°C or less), and pellets with a diameter of 10 mm and a thickness of 2 to 5 mm were prepared by cold isostatic pressing (CIP) at a pressure of 200 MPa. After carbon paste as an electrode was applied to both the upper and lower surfaces of the pellets, a heat treatment was performed at 180°C for 30 minutes to prepare samples for ion conductivity measurement. The ion conductivity measurement was performed by an AC impedance method at room temperature (25°C).

[0152] <Method for producing and using a lithium secondary battery using the present solid electrolyte compound>

[0153] (Material)

[0154] As the positive electrode active material, LiNi is used as a ternary layered compound. 0.5 Co 0.2 Mn 0.3 O2 (NCM) powder (D50 = 6.7 μm); as the negative electrode active material, graphite (Gr) powder (D50 = 20 μm) was used; as the solid electrolyte powder, the sample obtained in the example / comparative example (sulfide-based compound) was used.

[0155] For the positive electrode composite material powder, the positive electrode active material powder, the solid electrolyte powder and the conductive aid (acetylene black) were mixed in a mortar at a weight ratio of 60:37:3 and uniaxially pressed at 20 MPa to obtain positive electrode composite material pellets.

[0156] The negative electrode composite material powder was prepared by mixing graphite powder and solid electrolyte powder in a mortar at a weight ratio of 64:36.

[0157] The lower opening of a polypropylene cylinder (opening diameter 10.5 mm, height 18 mm) with upper and lower openings was blocked with a positive electrode (SUS), and positive electrode composite material pellets were placed on the positive electrode. A powdered solid electrolyte was placed on it, and uniaxial pressing was performed at 180 MPa to form a positive electrode composite material and a solid electrolyte layer. After placing the negative electrode composite powder on it, it was blocked with a negative electrode (SUS), and uniaxial forming was performed at 550 MPa to produce a mold battery consisting of a three-layer structure of a positive electrode composite material of approximately 100 μm thick, a solid electrolyte layer of approximately 300 μm thick, and a negative electrode composite material of approximately 20 μm thick.

[0158] (Battery Evaluation)

[0159] Using the molded battery produced as described above, resistance measurement and charge and discharge tests were carried out as follows.

[0160] The battery was placed in an environmental tester set at an ambient temperature of 25° C. for charging and discharging the battery, prepared so as to be chargeable and dischargeable, and allowed to stand until the battery temperature reached the ambient temperature.

[0161] Before charging, the AC resistance at 1 kHz was measured, and this value was defined as the AC resistance before charging.

[0162] The battery was charged and discharged with 1 mA set to 1 C. Then, constant current and constant potential charging was performed at 0.1 C to 4.5 V to obtain the initial charge capacity. The AC resistance at 1 kHz was measured in the same manner as before charging, and this value was taken as the resistance value before discharge.

[0163] Then, the battery was discharged at a constant current of 0.1 C to 2.5 V to obtain the initial discharge capacity. The initial charge and discharge efficiency was obtained from the discharge capacity relative to the charge capacity.

[0164] Next, the battery was charged to 4.5 V at 0.2 C with constant current and constant potential, and then discharged to 2.5 V at 5 C with constant current to obtain a discharge capacity of 5 C. The ratio of the discharge capacity of 5 C to the discharge capacity of 0.1 C was calculated to obtain the rate characteristic (5 C capacity retention rate (%)).

[0165] [Table 1]

[0166]

[0167] According to the results of Table 1 and the test results conducted so far, it was confirmed that when only Cl was contained as a halogen, although ionic conductivity could be ensured, the resistance tended to be high due to the high elastic modulus and hardness. On the other hand, it was confirmed that when only Br was contained as a halogen, the elastic modulus was low, the material became soft, and the resistance was low, but the ionic conductivity was reduced, so the rate characteristics tended to be reduced. In this case, the ionic conductivity was 2.0×10 -3 S / cm or more, an AC resistance before charge of 100Ω or less, and a rate characteristic (5C capacity retention rate (%)) of 20% or more are practically preferred, and these values ​​can be used as criteria for determination.

[0168] When Example 3 is compared with Comparative Example 1, it can be confirmed that Example 3 has low battery resistance, that is, is superior to Comparative Example 1, although the ion conductivity is low.

[0169] That is, it is considered that by containing Br as a halogen at a predetermined ratio relative to Cl, it is possible to provide a solid electrolyte that can maintain ion conductivity at a practical level and can exhibit more excellent battery performance with respect to battery resistance.

[0170] In addition, the solid electrolyte of each example was pelletized and its cross section was observed using a scanning electron microscope (SEM). As a result, if the Young's modulus of the sulfide-based compound used as the solid electrolyte is 23 GPa or less, Figure 1 As shown in Example 4, a state in which the solid electrolyte is crushed can be observed. On the other hand, if the Young's modulus of the sulfide-based compound is greater than 30 GPa, Figure 2 As shown in (Comparative Example 1), no crushing of the solid electrolyte was observed.

[0171] According to the results in Table 1 above and the test results conducted so far, it can be seen that the composition formula: Li 7-x PS 6- x Cl y Br z The sulfide-based compound shown can maintain high ion conductivity and achieve low elastic modulus by making the total molar ratio of Cl and Br greater than 1.0 and regulating the ratio of the molar ratio of Br to the molar ratio of Cl within a specified range, thereby reducing battery resistance.

[0172] It can also be seen that when both Cl and Br are contained as halogens, in order to further improve the rate characteristics, it is more preferable to carry out calcination at 450-600°C (material temperature) under the circulation of hydrogen sulfide gas (H2S) in its manufacturing method, thereby further reducing the elastic modulus, that is, Young's modulus.

Claims

1. A sulfide compound for a solid electrolyte of a lithium secondary battery, characterized in that: A crystal phase having a cubic thiogermanate-type crystal structure and represented by the composition formula: Li 7-x PS 6-x Cl y Br z wherein x in the composition formula satisfies x = y + z and 1.0 < x ≤ 1.8, the ratio (z / y) of the molar ratio of Br to the molar ratio of Cl is 0.1 to 10.0, and the Young's modulus is 1 GPa to 30 GPa.

2. The sulfide-based compound according to claim 1, characterized in that In the composition formula, y satisfies 0.3≤y≤1.5, and z satisfies 0.3≤z≤1.

5.

3. A solid electrolyte for lithium secondary battery, characterized in that Contains the sulfide compound according to claim 1 or 2.

4. The solid electrolyte for lithium secondary battery according to claim 3, characterized in that: It includes a single phase composed of a crystal phase of a cubic argyrodite type crystal structure.

5. A method for producing a solid electrolyte, characterized in that: It is a method for manufacturing a solid electrolyte as described in any one of claims 3 to 4, wherein a compound containing lithium (Li), a compound containing phosphorus (P), a compound containing sulfur (S), a chlorine-containing compound and a bromine-containing compound are mixed to obtain a mixture, and the mixture is calcined in a manner such that the temperature of the mixture becomes 450 to 600° C. under the circulation of hydrogen sulfide gas (H2S) to obtain a solid electrolyte.

6. A negative electrode for a lithium secondary battery, characterized in that: The invention comprises the solid electrolyte according to any one of claims 3 to 4 and a negative electrode active material. 7 . The negative electrode for a lithium secondary battery according to claim 6 , comprising a negative electrode active material containing carbon or silicon.

8. A positive electrode for a lithium secondary battery, characterized in that: The invention comprises the solid electrolyte according to any one of claims 3 to 4 and a positive electrode active material. 9 . A lithium secondary battery comprising the solid electrolyte according to claim 3 .

Citation Information

Patent Citations

  • Sulfide ceramics with high lithium ion conductivity and all solid cell using the same

    JP2001250580A

  • Lithium silver sulfide germanium ore

    JP2010540396A

  • Solid-state lithium secondary battery, and method for producing the same

    JP2011096630A

  • Sulfide-based solid electrolyte

    JP2013137889A

  • Sulfide-based solid electrolyte for lithium ion battery

    WO2015012042A1