A method for preparing graphene / copper composite metal interconnection line
Through the preparation method of graphene/copper composite metal interconnection, the problem of increasing resistivity of copper interconnection lines at the nanoscale is solved, and graphene/copper composite metal interconnection lines with low resistivity and high density are achieved, improving the The transmission rate and heat dissipation capabilities of the integrated circuit are enhanced, and the performance of the device is enhanced.
Patent Information
- Application Number
- CN201910732429.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-08-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2039-08-09
AI Technical Summary
At the nanoscale, the increase in resistivity of traditional copper interconnects leads to signal delay and heat dissipation problems, affecting the performance and reliability of integrated circuits.
The preparation method of graphene/copper composite metal interconnection is prepared by mixing copper powder and graphene, ball milling, microwave hot press sintering and thermal isostatic pressing, combined with magnetron sputtering coating technology, a low resistivity is prepared and a high-density copper/graphene target to form graphene/copper composite metal interconnection lines.
It significantly improves the electron transmission speed and heat dissipation ability, reduces the resistivity and thermal conductivity, enhances the transmission rate and tensile strength of the integrated circuit, and reduces the damage to material performance by electron migration.
Smart Images

Figure CN112349667B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic materials and devices, and in particular relates to a method for preparing a graphene / copper composite metal interconnection line. Background Art
[0002] Interconnection is to connect the independent components in the same chip into a circuit module with certain functions. With the development of integrated circuits, the feature size is getting smaller and smaller, while the power supply voltage cannot be reduced proportionally, which causes a significant increase in the current density in the interconnection line. In addition, the increase in the density of integrated circuit devices leads to an increase in the line density and heat generated per unit area of the chip, which increasingly aggravates the severity of interconnection reliability.
[0003] In the submicron and deep submicron stages, compared with gate delay, the delay RC caused by interconnection accounts for an increasing proportion of the total delay. A large number of examples show that when the characteristic length of the device is less than 0.18μm, the signal loss and signal delay of the interconnection account for more than 75% of the total delay and loss. The use of low-resistivity interconnection materials and low-dielectric constant dielectric materials can effectively reduce the delay time RC of the interconnection system, thereby meeting the short size effect of the device. Copper interconnection has many advantages: the resistivity of copper is only 1.67μΩ / cm, which is much smaller than the 2.66μΩ / cm of aluminum. At the same time, it can reduce the thickness of the interconnection layer, and reduce the capacitance by reducing the signal. Copper and low-K dielectric interconnection systems have become the materials selected to reduce the interconnection delay time after the integrated circuit enters the deep submicron stage. Therefore, in modern ULSI integrated circuits, metal interconnection lines mainly use double-layer Damascus copper interconnection technology.
[0004] However, after entering the nanoscale, the copper interconnection process will face many problems, including scale effect and stability effect. At the micron and larger scales, the resistivity of metal copper can be considered a constant at room temperature. This is because the electron mean free path of metal copper is about 45nm at room temperature. When the size is equivalent to the electron mean free path, the electron scattering increases significantly, thereby increasing the resistivity. Then entering the 28nm scale, electron surface scattering and grain boundary scattering will cause the effective resistivity of metal interconnects to continue to increase, which is the so-called scale effect. At the same time, the barrier layer in the copper interconnect further increases the equivalent resistivity. On the other hand, the electromigration phenomenon is becoming more and more significant, especially in interconnect circuits with higher current density. The increase in the resistivity of the interconnect will significantly increase the signal delay in the integrated circuit and increase the IR voltage drop of the power / ground network, thereby seriously affecting the overall performance of the circuit. In addition, due to the increase in the resistivity of the copper interconnect and the introduction of low dielectric materials, the self-heating effect and heat dissipation problems of the interconnect will become more serious. Therefore, the deterioration of the electrical performance and the reduction in reliability of traditional copper interconnects have become a great obstacle to the development of future ultra-large-scale integrated circuits. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a graphene / copper composite metal interconnection line. The graphene / copper composite metal interconnection line of the present invention has high electron transmission capability, low resistivity and strong heat dissipation.
[0006] The present invention provides a method for preparing a graphene / copper composite metal interconnect line, comprising the following steps:
[0007] A) mixing copper powder and graphene and then ball milling to obtain a mixed powder; the graphene accounts for 1 to 8% of the mass of the mixed powder;
[0008] B) subjecting the mixed powder to microwave hot pressing sintering under a protective atmosphere, and after the microwave hot pressing sintering is completed, subjecting the obtained blank to hot isostatic pressing to obtain a copper / graphene target;
[0009] The vacuum degree of microwave hot pressing sintering reaches 10 -4 When the temperature is below Pa, the temperature is raised at a rate of 10-20°C / min. After reaching 500-600°C, the temperature is raised to 750-950°C at a rate of 20-30°C / min and kept at this temperature for 0.1-1 hour.
[0010] The pressure of the hot isostatic pressing is 130-180 MPa; the temperature of the hot isostatic pressing is 900-1000° C.; the holding time of the hot isostatic pressing is 1-3 hours;
[0011] C) using the copper / graphene target material to perform magnetron sputtering coating on the surface of the etched silicon substrate to obtain a graphene / copper composite metal interconnect.
[0012] Preferably, the particle size of the copper powder is 1 to 2 μm;
[0013] The particle size of the graphene is 1 to 2 μm.
[0014] Preferably, the rotation speed of the ball mill is 400-600 r / min;
[0015] The ball milling time is 4 to 6 hours;
[0016] The mass ratio of the balls to the materials in the ball mill is 15:1.
[0017] Preferably, the pressure of the microwave hot pressing sintering is 20-50 MPa.
[0018] Preferably, the hot isostatic pressing uses argon as the pressure gas.
[0019] Preferably, the power of the magnetron sputtering is 60 to 100 W;
[0020] The background vacuum of the magnetron sputtering is 3 to 6×10 -4 Pa.
[0021] Preferably, the temperature of the magnetron sputtering is 400-500°C;
[0022] The magnetron sputtering time is 5 to 15 minutes.
[0023] Preferably, the magnetron sputtering uses high-purity Ar gas as the working gas;
[0024] The flow rate of the high-purity Ar gas is 50-200 mL / min.
[0025] Preferably, the growth rate of the film in step C) is
[0026] The invention provides a method for preparing a graphene / copper composite metal interconnection line, comprising the following steps: A) mixing copper powder and graphene and then ball milling to obtain a mixed powder; the graphene accounts for 1 to 8% of the mass of the mixed powder; B) subjecting the mixed powder to microwave hot pressing sintering under a protective atmosphere, and after the microwave hot pressing sintering is completed, hot isostatic pressing is performed on the obtained blank to obtain a copper / graphene target material; the vacuum degree of the microwave hot pressing sintering reaches 10 -4 Pa, start heating, the heating rate is 10-20°C / min, after heating to 500-600°C, then heat to 750-950°C at a rate of 20-30°C / min, and keep warm for 0.1-1 hour; the pressure of the hot isostatic pressing is 130-180MPa; the temperature of the hot isostatic pressing is 900-1000°C; the holding time of the hot isostatic pressing is 1-3 hours; C) use the copper / graphene target to perform magnetron sputtering coating on the surface of the etched silicon substrate to obtain a graphene / copper composite metal interconnect. The present invention mixes graphene with copper powder and prepares copper interconnects by magnetron sputtering, and uses hot isostatic pressing to prepare copper / graphene mixed targets, so that the grain size of the mixed targets is smaller, more uniform, and more compact. After sputtering, it is easier to form a good microscopic conductive channel with the same structure, which can accelerate the transmission capacity and speed of electrons, greatly enhance the heat dissipation capacity of the device, reduce the damage of electron migration to material performance, and at the same time, improve the transmission rate of the integrated circuit. Experimental results show that the resistivity of the graphene / copper composite metal interconnect in the present invention is 1.49×10 -8 Ω·m, tensile strength is 381.2MPa, thermal conductivity is 1.380(Kw·(m·K) -1 ). BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0028] Figure 1 is the resistivity curve of the graphene / copper interconnect in Examples 1 to 5 of the present invention;
[0029] Figure 2 is the tensile performance curve of the graphene / copper interconnect in Examples 1 to 5 of the present invention;
[0030] Figure 3 is the thermal conductivity of the graphene / copper interconnect in Examples 1 to 5 of the present invention. DETAILED DESCRIPTION
[0031] The present invention provides a method for preparing a graphene / copper composite metal interconnect line, comprising the following steps:
[0032] A) mixing copper powder and graphene and then ball milling to obtain a mixed powder; the graphene accounts for 1 to 8% of the mass of the mixed powder;
[0033] B) subjecting the mixed powder to microwave hot pressing sintering under a protective atmosphere, and after the microwave hot pressing sintering is completed, subjecting the obtained blank to hot isostatic pressing to obtain a copper / graphene target;
[0034] The vacuum degree of microwave hot pressing sintering reaches 10 -4 When the temperature is below Pa, the temperature is raised at a rate of 10-20°C / min. After reaching 500-600°C, the temperature is raised to 750-950°C at a rate of 20-30°C / min and kept at this temperature for 0.1-1 hour.
[0035] The pressure of the hot isostatic pressing is 130-180 MPa; the temperature of the hot isostatic pressing is 900-1000° C.; the holding time of the hot isostatic pressing is 1-3 hours;
[0036] C) using the copper / graphene target material to perform magnetron sputtering coating on the surface of the etched silicon substrate to obtain a graphene / copper composite metal interconnect.
[0037] The present invention preferably weighs high-purity copper powder and graphene respectively according to a proportion, mixes them and places them in a ball mill for ball milling, and uses high-purity Ar gas as a protective gas during the ball milling process to prevent oxidation of the copper powder, thereby obtaining a mixed powder.
[0038] In the present invention, the purity of the high-purity copper powder is preferably 99.9999%, the shape of the high-purity copper powder is preferably spherical, and the particle size of the high-purity copper powder is preferably 1-2 μm; the purity of the graphene is preferably 99.95%, and the particle size of the graphene is preferably 1-2 μm, more preferably 1.5 μm. The graphene accounts for 1-8% of the mass of the mixed powder, specifically, 1%, 3%, 5%, 7% or 8%.
[0039] The material of the ball milling balls is preferably zirconia, and the mass ratio of the ball materials is preferably 15:1; the rotation speed of the ball mill is preferably 400-600 r / min, more preferably 500-550 r / min; the ball milling time is preferably 4-6 hours, more preferably 5 hours.
[0040] After obtaining the mixed powder, the present invention places the mixed powder in a hot pressing sintering mold, and then places the hot pressing sintering mold in a hot pressing sintering furnace. The whole process needs to be carried out in an argon protective atmosphere. The hot pressing sintering method is preferably microwave hot pressing sintering. After the sintering starts, the sintering furnace is vacuumed. When the vacuum degree reaches 10 -4 Pa, start heating, the heating rate is 10-20℃ / min, preferably 15℃ / min, after heating to 500-600℃, then heat to 750-950℃, preferably 800-900℃, at a rate of 20-30℃ / min, preferably 25℃ / min, and keep warm for 0.1-1 hour, preferably 0.5-0.8 hour. The pressure applied to the powder during the whole sintering process is preferably 20-50MPa, more preferably 30-40MPa.
[0041] After the hot pressing sintering is completed, the sintered green body is taken out and hot isostatic pressing is performed to obtain a copper / graphene target. The hot isostatic pressing preferably uses argon as the pressure gas, and the pressure of the hot isostatic pressing is preferably 130-180MPa, more preferably 140-170MPa, and most preferably 150-160MPa; the temperature of the hot isostatic pressing is preferably 900-1000°C, more preferably 950°C; the holding time of the hot isostatic pressing is preferably 1-3 hours, more preferably 2 hours.
[0042] After hot isostatic pressing, the grain size of the obtained copper / graphene target is about 15μm and the density is as high as 98.3%.
[0043] After obtaining the copper / graphene target material, the present invention places the copper / graphene target material in a magnetron sputtering chamber and performs magnetron sputtering coating on the surface of the silicon substrate.
[0044] The silicon substrate in the present invention refers to a silicon (001) substrate that is to be coated after etching. The surface of the silicon substrate has etched silicon grooves for growing the copper / graphene film in the present invention. The present invention preferably places the silicon substrate in deionized water for ultrasonic cleaning to obtain a clean and pollution-free silicon substrate.
[0045] The resistivity of the deionized water is preferably 1.8×10 5 Ωm; the frequency of the ultrasonic wave is preferably 50 KHz, and the time of the ultrasonic cleaning is preferably 10 min.
[0046] In the present invention, the magnetron sputtering is preferably radio frequency magnetron sputtering, and the power of the magnetron sputtering is preferably 60 to 100 W, more preferably 70 to 90 W, and most preferably 80 W; the background vacuum degree in the magnetron sputtering chamber is preferably 3 to 6×10 -4 Pa, more preferably 4 to 5×10 -4 Pa; the temperature of the magnetron sputtering is preferably 400-500°C, more preferably 450°C; the time of the magnetron sputtering is preferably 5-15min, more preferably 10min; the growth rate of the film during the magnetron sputtering is preferably More preferably The magnetron sputtering uses high-purity argon as a working gas, and the flow rate of the high-purity argon is preferably 50 to 200 mL / min, and more preferably 100 to 150 mL / min.
[0047] The thickness of the graphene / copper composite metal interconnection line obtained by magnetron sputtering is 5 to 15 nm, which is 30% thinner than the conventional copper film thickness and 20% narrower in line width.
[0048] The method for preparing the graphene / copper composite metal interconnection line of the present invention can be applied in integrated circuits to meet the process requirements of continuously reducing the feature size of integrated circuits.
[0049] The invention provides a method for preparing a graphene / copper composite metal interconnection line, comprising the following steps: A) mixing copper powder and graphene and then ball milling to obtain a mixed powder; the graphene accounts for 1 to 8% of the mass of the mixed powder; B) subjecting the mixed powder to microwave hot pressing sintering under a protective atmosphere, and after the microwave hot pressing sintering is completed, hot isostatic pressing is performed on the obtained blank to obtain a copper / graphene target material; the vacuum degree of the microwave hot pressing sintering reaches 10 -4Pa, start heating, the heating rate is 10-20°C / min, after heating to 500-600°C, then heat to 750-950°C at a rate of 20-30°C / min, and keep warm for 0.1-1 hour; the pressure of the hot isostatic pressing is 130-180MPa; the temperature of the hot isostatic pressing is 900-1000°C; the holding time of the hot isostatic pressing is 1-3 hours; C) use the copper / graphene target to perform magnetron sputtering coating on the surface of the etched silicon substrate to obtain a graphene / copper composite metal interconnect. The present invention mixes graphene with copper powder and prepares copper interconnects by magnetron sputtering, and uses hot isostatic pressing to prepare copper / graphene mixed targets, so that the grain size of the mixed targets is smaller, more uniform, and more compact. After sputtering, it is easier to form a good microscopic conductive channel with the same structure, which can accelerate the transmission capacity and speed of electrons, greatly enhance the heat dissipation capacity of the device, reduce the damage of electron migration to material performance, and at the same time, improve the transmission rate of the integrated circuit. Experimental results show that the resistivity of the graphene / copper composite metal interconnect in the present invention is 1.49×10 -8 Ω·m, tensile strength is 381.2MPa, thermal conductivity is 1.380(Kw·(m·K) -1 ).
[0050] In order to further illustrate the present invention, a method for preparing a graphene / copper composite metal interconnect provided by the present invention is described in detail below in conjunction with an embodiment, but it should not be construed as limiting the scope of protection of the present invention.
[0051] Example 1
[0052] The etched silicon (001) substrate to be coated is placed in deionized water, wherein the resistivity of the deionized water is 1.8×105Ωm, and the silicon substrate is placed in ultrasonic waves with a frequency of 50KHz for 10 minutes to remove impurities on the surface of the substrate and obtain a clean and pollution-free silicon substrate.
[0053] Weigh high-purity copper powder (particle size of about 1 to 2 microns, purity of 99.9999%, spherical) and graphene (particle size of 1.5 microns. Purity of 99.95%) according to the mass ratio, where graphene accounts for 1% of the mass of the mixed powder. Put the mixed powder into a ball mill, the ball milling balls are zirconium oxide, the ball-to-material mass ratio is 15:1, and high-purity Ar2 is used as a protective gas to prevent oxidation of the copper powder. The speed of the ball mill is 500r / min, and the ball milling time is 4h.
[0054] The mixed powder is placed in a hot pressing sintering mold in a glove box filled with argon, and the hot pressing sintering mold containing the mixed powder is placed in a hot pressing sintering furnace. The whole process needs to be carried out in an argon protective atmosphere. The sintering method adopts microwave sintering, and vacuum pressure is applied in the sintering furnace. When the vacuum degree reaches 10 -4 Pa, the temperature starts to rise at a rate of 15°C / min. After reaching 500°C, it is raised to 750-950°C at a rate of 25°C / min. The sintering time is 0.5h. During the entire sintering process, the pressure applied to the powder is 30MPa. After the hot pressing sintering is completed, the blank is taken out for hot isostatic pressing. The hot isostatic pressing uses argon as the pressure gas. The hot isostatic pressing process is: pressure 150MPa, temperature 950°C, and insulation time 2 hours to obtain a Φ50 copper-based target. The grain size of the target is about 15 microns, and the density is 98.3%.
[0055] The copper / graphene target prepared above was processed into a 4-inch round target with a purity of (above 99.995%), and a SY500w RF magnetron sputtering instrument was used for magnetron sputtering. RF magnetron sputtering technology was used, the sputtering power was 80W, and the background vacuum in the sputtering chamber was 5×10 -4 Pa, the working gas is high-purity Ar gas, the Ar gas flow rate is 100 ml / min, and the film growth rate is The sputtering time is 15 minutes, and a 15nm copper / graphene film can be grown in the etched silicon groove, which is the graphene / copper composite metal interconnect. Before the film is formally sputtered, a 10-minute pre-sputtering is performed to remove pollutants on the target surface.
[0056] The resistivity and tensile strength of the graphene / copper interconnect in this embodiment were tested. The results showed that the resistivity was 1.68×10 -8 Ω·m, and the tensile strength is 294.8MPa.
[0057] Example 2
[0058] The graphene / copper composite metal interconnect was prepared according to the preparation method in Example 1, except that in this example, the graphene accounted for 3% of the mass of the mixed powder.
[0059] The resistivity and tensile strength of the graphene / copper interconnect in this embodiment were tested. The results showed that the resistivity was 1.61×10 -8 Ω·m, and the tensile strength is 327.4MPa.
[0060] Example 3
[0061] The graphene / copper composite metal interconnect was prepared according to the preparation method in Example 1, except that in this example, the graphene accounted for 5% of the mass of the mixed powder.
[0062] The resistivity and tensile strength of the graphene / copper interconnect in this embodiment were tested. The results showed that the resistivity was 1.53×10 -8 Ω·m, and the tensile strength is 381.2MPa.
[0063] Example 4
[0064] The graphene / copper composite metal interconnect was prepared according to the preparation method in Example 1, except that in this example, the graphene accounted for 7% of the mass of the mixed powder.
[0065] The resistivity and tensile strength of the graphene / copper interconnect in this embodiment were tested. The results showed that the resistivity was 1.45×10 -8 Ω·m, and the tensile strength is 368.2MPa.
[0066] Example 5
[0067] The graphene / copper composite metal interconnect was prepared according to the preparation method in Example 1, except that in this example, the graphene accounted for 8% of the mass of the mixed powder.
[0068] The resistivity and tensile strength of the graphene / copper interconnect in this embodiment were tested. The results showed that the resistivity was 1.38×10 -8 Ω·m, and the tensile strength is 320MPa.
[0069] The mechanical properties and resistivity data of the graphene / copper interconnects in Examples 1 to 5 were plotted, and the results are as follows: Figures 1-2 As shown, Figure 1 is the resistivity curve of the graphene / copper interconnect in Examples 1 to 5 of the present invention; Figure 2 This is the tensile performance curve of the graphene / copper interconnect in Examples 1 to 5 of the present invention.
[0070] Depend on Figure 1 It can be seen that with the addition of different contents of graphene, the resistivity of the copper / graphene film continues to decrease. When the graphene addition amount is 5wt%, the alloy film has the lowest resistivity of 1.49×10 -8 Ω·m, but as the graphene content continues to increase, the resistivity tends to increase. This shows that graphene doping will optimize the conductivity of metal interconnects. As the amount of graphene doping increases, the film resistivity reaches the optimal value. If it continues to be added, too much graphene in the alloy will cause interface scattering, surface scattering, etc., which will lead to a decrease in conductivity and an increase in resistivity.
[0071] Depend on Figure 2It can be seen that with the addition of graphene, the tensile strength gradually increases. This is because graphene has good ductility, and the tensile strength of the alloy after mixing is greatly improved. However, excessive graphene will cause the density of the alloy to decrease during the sintering process, which will lead to a decrease in tensile strength.
[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
[0073] Figure 3 It can be seen that with the addition of graphene, the thermal conductivity of the material is greatly improved. This is because graphene has good ductility and the heat transfer after mixing is greatly improved. However, when the addition amount of graphene reaches 5%, the thermal conductivity is 1.380 (Kw·(m·K)-1). After that, with the increase of graphene content, the thermal conductivity does not increase significantly. This is because after the excess graphene, the density of the alloy is reduced, thereby affecting the thermal conductivity of the alloy.
Claims
1. A method for preparing a graphene / copper composite metal interconnect, comprising the following steps: A) mixing copper powder and graphene and then ball milling to obtain a mixed powder; the graphene accounts for 1 to 8% of the mass of the mixed powder; B) subjecting the mixed powder to microwave hot pressing sintering under a protective atmosphere, and after the microwave hot pressing sintering is completed, subjecting the obtained blank to hot isostatic pressing to obtain a copper / graphene target; The vacuum degree of microwave hot pressing sintering reaches 10 -4 When the temperature is below Pa, the temperature is raised at a rate of 10-20°C / min. After reaching 500-600°C, the temperature is raised to 750-950°C at a rate of 20-30°C / min and kept at this temperature for 0.1-1 hour. The pressure of the hot isostatic pressing is 130-180 MPa; the temperature of the hot isostatic pressing is 900-1000° C.; the holding time of the hot isostatic pressing is 1-3 hours; C) using the copper / graphene target material to perform magnetron sputtering coating on the surface of the etched silicon substrate to obtain a graphene / copper composite metal interconnect with a thickness of 5 to 15 nm; The power of the magnetron sputtering is 60-100W; the background vacuum of the magnetron sputtering is 3-6×10 -4 Pa; the temperature of the magnetron sputtering is 400-500° C.; the time of the magnetron sputtering is 5-15 min.
2. The preparation method according to claim 1, characterized in that: The particle size of the copper powder is 1 to 2 μm; The particle size of the graphene is 1 to 2 μm.
3. The preparation method according to claim 1, characterized in that: The rotation speed of the ball mill is 400-600 r / min; The ball milling time is 4 to 6 hours; The mass ratio of the balls to the materials in the ball mill is 15:
1.
4. The preparation method according to claim 1, characterized in that: The pressure of the microwave hot pressing sintering is 20-50 MPa.
5. The preparation method according to claim 1, characterized in that: The hot isostatic pressing uses argon as the pressure gas.
6. The preparation method according to claim 1, characterized in that: The magnetron sputtering uses high-purity Ar gas as the working gas; The flow rate of the high-purity Ar gas is 50-200 mL / min.
7. The preparation method according to claim 1, characterized in that: The growth rate of the film in step C) is